Methods to improve the photoelectric performance and stability of perovskite solar cells based on interface modification
By introducing a polyguanidine polymer modification layer into perovskite solar cells, the problem of weak interfacial bonding between the electron transport layer and the hole blocking layer was solved, thereby improving photoelectric conversion efficiency and stability.
Patent Information
- Application Number
- CN202611042317.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-14
- Publication Date
- 2026-11-17
AI Technical Summary
In existing perovskite solar cells, the weak bonding force at the interface between the electron transport layer and the hole blocking layer leads to reduced stability of photovoltaic devices.
A polyguanidine polymer modification layer is coated between the electron transport layer and the tin dioxide barrier layer. The guanidine functional groups of the polymer enhance the interfacial forces, thereby forming a modification layer to improve the bonding strength.
This enhances the adhesion of the hole blocking layer to the electron transport layer surface, thereby improving the photoelectric conversion efficiency and stability of the perovskite solar cell.
Smart Images

Figure CN123124642A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of perovskite solar cell technology, and particularly relates to a method for improving the photoelectric performance and stability of perovskite solar cells based on interface modification. Background Technology
[0002] Perovskite solar cells, as an emerging photovoltaic technology, possess advantages such as high photoelectric conversion efficiency, low cost, and ease of large-scale fabrication, driving the certified photoelectric conversion efficiency of small-area perovskite solar cells to jump from 3.8% to 28.0% in just over a decade. This efficiency record for single-junction perovskite photovoltaic devices was achieved by inverted perovskite cells. The basic structure of an inverted perovskite cell, from bottom to top, consists of: a conductive glass substrate, a hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a back electrode. To minimize non-radiative recombination and improve the photoelectric conversion efficiency and operational stability of perovskite photovoltaic devices, a passivation layer and a hole-blocking layer are generally added during the fabrication of inverted perovskite photovoltaic devices. The passivation layer is placed between the perovskite light-absorbing layer and the electron transport layer to passivate perovskite interface defects; the blocking layer is placed between the electron transport layer and the back electrode to prevent the passage of minority carriers. Currently, the electron transport layer material is generally fullerene (C6H2O). 60 [6,6]-phenylC 61 Methyl butyrate (PCBM) and copper hydroxide (BCP) were once commonly used hole-blocking layer materials, but their chemical stability was unsatisfactory, and they were prone to decomposition under thermal stress and certain bias voltages. Inorganic tin dioxide (SnO2), due to its higher chemical stability and suitable electrical conductivity, replaced BCP and was used as the hole-blocking layer between the electron transport layer and the back electrode. However, electron transport layer materials (C... 60 The intermolecular forces between PCBM and SnO2 are weak, causing SnO2 to... 60 The adhesion of PCBM surfaces is relatively weak, especially under stress conditions. The hole blocking layer is prone to separation from the electron transport layer, which reduces the operational stability of photovoltaic devices.
[0003] Therefore, in order to improve the stability of perovskite photovoltaic devices, it is urgent to develop a new technology to enhance the bonding force at the interface between the inorganic hole blocking layer and the organic electron transport layer. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a method for enhancing the interfacial forces between the electron transport layer and hole blocking layer in inverted perovskite photovoltaic cells, based on perovskite solar cell interface modification. The method is characterized by coating the electron transport layer surface with a polyguanidine polymer containing numerous imino structures (—NH—). Both the imino groups and the guanidine groups can react with SnO2 and C. 60PCBM molecules possess strong intermolecular forces, which can act as interfacial bridges, enhancing the hole-blocking layer material SnO2's role in the electron transport layer material C. 60 The adhesion of PCBM to the surface improves the working efficiency and stability of perovskite solar cells.
[0005] This invention is achieved through the following technical solution: I. A method for improving the photoelectric performance and stability of perovskite solar cells based on interface modification: The polyguanidine polymer is applied to the interface between the electron transport layer and the tin dioxide layer of a perovskite solar cell using a coating process to form a modification layer, which is used to strengthen the interlayer bonding force and improve the photoelectric performance and stability of the cell.
[0006] The polyguanidine polymer modification layer is located above the electron transport layer interface and below the tin dioxide layer interface.
[0007] The polyguanidine polymer backbone or side chain contains multiple guanidine functional groups, which can interact with the perovskite electron transport layer and the tin dioxide blocking layer to enhance the adhesion of the hole blocking layer to the surface of the electron transport layer.
[0008] The polyguanidine polymers include one or more of the functional groups of aminoguanidine, monoguanidinium triguanidinium urea, or cytoguanidine.
[0009] II. A type of perovskite solar cell: The perovskite solar cell is obtained by the above method and includes a conductive glass substrate layer, a hole transport layer, a perovskite light absorption layer, a passivation layer, an electron transport layer, a polyguanidine polymer modification layer, a tin dioxide blocking layer, and a metal electrode layer; the modification layer is formed on the interface of the electron transport layer by a spin coating process.
[0010] The thickness of the polyguanidine polymer modification layer ranges from 1 to 10 nm.
[0011] The modified layer is mainly formed by spin-coating or coating with a polyguanidine polymer solution, wherein the concentration of the polyguanidine polymer solution is 0.1~2 mg / mL.
[0012] III. A method for preparing a perovskite solar cell, the method being as follows: 1) Clean the ITO or FTO glass sequentially with deionized water, acetone and ethanol solution using ultrasonic cleaning, dry it with nitrogen, and then treat it in an ultraviolet ozone cleaner for 10~30 min. Assemble the hole transport layer on the surface of the conductive substrate by coating or vapor deposition. 2) Dissolve FAI and PbI2 in N,N-dimethylformamide (DMF) to obtain a perovskite precursor solution with a concentration of 1.0~2.0 mol / L. Spin coat the perovskite precursor solution onto the surface of the hole transport layer using a spin coater at a speed of 2000~5000 r / min. Use ethyl acetate (EA) as the antisolvent. After spin drying for 15~35 seconds, drop the solution onto the center of the spin-coated ITO or FTO glass substrate. Continue spin drying for 3~10 seconds, then place the substrate on a hot plate at 100~150 ℃ and anneal for 5~30 minutes to form a perovskite absorber layer. 3) Assemble PCBMs or C on the substrate prepared in step 2) using coating or vapor deposition methods. 60 Electron transport layer; 4) A layer of polyguanidine polymer is uniformly coated onto the surface of the electron transport layer using spin coating or coating method as a modification layer; 5) Deposit SnO2 as a hole-blocking layer on the modified layer prepared in step 4); 6) Finally, a back electrode is deposited on the surface of the hole blocking layer.
[0013] In step 4), the polyguanidine polymer is dissolved in an alcohol such as isopropanol (IPA), ethanol, or butanol, or a mixture thereof, and the concentration of the polyguanidine polymer in the solution is 0.1~2.5 mg / L.
[0014] Furthermore, in step 2, FAI and PbI2 can be replaced by FAPbI3, MAPbI3, FAPbBr3, MAPbBr3, CsPbI3, CsPbBr3 and mixtures thereof; In step 2), FAI can be replaced by MAI, FABr, MABr, CsI, CsBr or a mixture thereof; In step 2), PbI2 can be replaced by PbBr2, PbCl2, Pb(SCN)2 or a mixture thereof; The DMF in step 2) can be replaced by N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAc), or a mixture thereof. In step 2), EA can be replaced by propyl acetate, diethyl ether, chlorobenzene, anisole, or a mixture thereof.
[0015] In step 5), SnO2 is deposited by methods such as atomic layer deposition (ALD) and vacuum evaporation (PVD).
[0016] The beneficial effects of this invention are as follows: This invention improves the photoelectric performance and stability of batteries by adding polyguanidine polymers to strengthen interlayer bonding.
[0017] This invention utilizes the coordination between the abundant imino groups in polyguanidine polymers and tin ions, as well as the coordination between the guanidine group and PCBM, C 60 The dipole-dipole interaction between the holes strengthens the bonding force between the hole blocking layer and the electron transport layer surface, thereby improving the photoelectric conversion efficiency and stability of perovskite solar cells. Attached Figure Description
[0018] Figure 1 This is a structural diagram of the polyhexamethylene biguanide hydrochloride used in Example 1 of this invention; Figure 2 This is a structural diagram of the polyhexamethylene biguanide molybdate used in Example 2 of this invention; Figure 3 This is a structural diagram of the polyhexamethylene guanidine used in Example 3 of this invention; Figure 4 This is a structural diagram of the device used in the embodiments of the present invention; Figure 5 These are the JV curves of the perovskite solar cells obtained in Example 1 and Comparative Example 1 of this invention; Figure 6 These are the JV curves of the perovskite solar cells obtained in Example 2 and Comparative Example 2 of this invention; Figure 7 These are the JV curves of the perovskite solar cells obtained in Example 3 and Comparative Example 3 of this invention; Figure 8 These are the performance stability test graphs of the perovskite solar cell devices obtained in Embodiment 1 and Comparative Example 1 of this invention. Detailed Implementation
[0019] All technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The singular forms “a,” “described,” and “the” used in this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the term “and / or” as used in this invention refers to and includes any or all possible combinations of one or more of the associated listed items.
[0020] Unless otherwise specified in the embodiments of this invention, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained through conventional technical means or commercially available.
[0021] Specific embodiments of the present invention are as follows: The device structure diagram of a specific embodiment of the present invention is shown below. Figure 4 As shown.
[0022] Example 1 This embodiment describes the fabrication of an inverted perovskite solar cell containing a 0.3 mg / mL polyhexamethylene biguanide hydrochloride modification layer. The specific steps are as follows: Step 1: After the ITO conductive glass was successively cleaned with deionized water, isopropanol, and ethanol solutions, it was dried with nitrogen gas and then treated with an ultraviolet ozone instrument for 30 min. Me-4PACz was ultrasonically dispersed in ethanol to form a 1 mg / L dispersion, which was then spin-coated onto the ITO surface and annealed on a hot plate at 100 °C for 10 min to form a hole transport layer.
[0023] Step 2: Dissolve equimolar amounts of MAI and PbI2 in DMSO to form a perovskite precursor solution with a concentration of 1.5 mol / L. Spin-coat the precursor solution onto the surface of the hole transport layer. Spin coat the substrate at 3400 r / min. After spin-drying for 30 s, add ethyl acetate dropwise to the center of the substrate and continue spin-drying for 10 s. After spin-drying, place the substrate on a hot plate at 100 ℃ for annealing for 15 min to form a perovskite light-absorbing layer.
[0024] Step 3: Dissolve PCBM in chlorobenzene to prepare a solution with a concentration of 20 mg / ml, and then spin-coat the solution onto the substrate at a speed of 3000 r / min for 30 s; Step 4: Weigh 0.3 mg of polyhexamethylene biguanide hydrochloride, with the structural formula shown below. Figure 1 As shown, it was dissolved in 1 ml of IPA, and then a polyhexamethylene biguanide hydrochloride modification layer was spin-coated on the substrate surface at a speed of 3500 r / min; Step 5: Deposit 20 nm SnO2 as a hole-blocking layer using an atomic layer deposition apparatus; Step 6: Place the substrate in a vapor deposition apparatus and vapor deposit 80 nm of silver as the back electrode.
[0025] Example 2 This embodiment uses a modification layer containing a polyhexamethylene biguanide molybdate solution with a mass concentration of 0.5 mg / mL to prepare an inverted perovskite solar cell. The specific steps are as follows: Step 1: After the ITO conductive glass was successively cleaned with deionized water, isopropanol, and ethanol solutions, it was dried with nitrogen gas and then treated with an ultraviolet ozone instrument for 20 min. Me-4PACz was ultrasonically dispersed in ethanol to form a 1 mg / L dispersion, which was then spin-coated onto the ITO surface and annealed on a hot plate at 100 °C for 10 min to form a hole transport layer.
[0026] Step 2: Dissolve equimolar amounts of FAI and PbI2 in DMSO to form a perovskite precursor solution with a concentration of 1.5 mol / L. Spin-coat the precursor solution onto the surface of the hole transport layer. Spin coat the substrate at 4000 r / min. After spin-drying for 35 s, drop chlorobenzene into the center of the substrate and continue spin-drying for 8 s. After spin-drying, place the substrate on a hot plate at 150 ℃ for annealing for 10 min to form a perovskite light-absorbing layer.
[0027] Step 3: Dissolve PCBM in chlorobenzene to prepare a solution with a concentration of 25 mg / ml, and then spin-coat the solution onto the substrate at a speed of 5000 r / min for 25 s; Step 4: Weigh 0.5 mg of polyhexamethylene biguanide molybdate, with the structural formula shown below. Figure 2 As shown, it was dissolved in 1 ml of IPA, and then a polyhexamethylene biguanide molybdate modification layer was spin-coated on the substrate surface at a speed of 4000 r / min; Step 5: Deposit 20 nm SnO2 as a hole-blocking layer using an atomic layer deposition apparatus; Step 6: Place the substrate in a vapor deposition apparatus and vapor deposit 80 nm of copper as the back electrode.
[0028] Example 3 This embodiment uses a precursor solution containing a polyhexamethylene guanidine solution with a mass concentration of 0.6 mg / mL to prepare an inverted perovskite solar cell. The specific steps are as follows: Step 1: After the ITO conductive glass was successively cleaned with deionized water, isopropanol, and ethanol solutions, it was dried with nitrogen gas and then treated with an ultraviolet ozone instrument for 20 min. Me-4PACz was ultrasonically dispersed in ethanol to form a 1 mg / L dispersion, which was then spin-coated onto the ITO surface and annealed on a hot plate at 100 °C for 10 min to form a hole transport layer.
[0029] Step 2, Preparation of perovskite precursor solution I: Weigh 1450 mg of PbI2, 438 mg of FAI, 30 mg of MACl, 39 mg of CsI, and 47 mg of MAI, dissolve them in 1.5 mL of DMF and 0.3 mL of DMSO, stir for 12 h, and then mix to obtain the precursor solution. Spin-coat the precursor solution onto the surface of the hole transport layer using a spin coater at 1000 r / min for 10 s, 5000 r / min for 35 s, and add anisole as an anti-solvent in the last 12 s. Anneal on a hot plate at 100 ℃ for 30 min.
[0030] Step 3: Place the substrate in an evaporator and deposit a 16 nm thick layer of fullerene (C1) onto the substrate surface. 60 ).
[0031] Step 4: Weigh 0.6 mg of polyhexamethylene guanidine, with the structural formula shown below. Figure 3 As shown, the polyhexamethylene guanidine passivation layer with a concentration of 0.6 mg / mL was dissolved in 1 mL of IPA, and then spin-coated onto the substrate surface and annealed at 120 °C for 3 min.
[0032] Step 5: Deposit 20 nm SnO2 as a hole-blocking layer using an atomic layer deposition apparatus; Step 6: Place the substrate in a vapor deposition apparatus and vapor deposit 80 nm of silver as the back electrode.
[0033] Comparative Example 1 The difference between this comparative example and Example 1 is that the polyhexamethylene biguanide hydrochloride modification layer was not spin-coated in step 3.
[0034] Comparative Example 2 The difference between this comparative example and Example 2 is that the polyhexamethylene biguanide molybdate modification layer in step 3 is not present.
[0035] Comparative Example 3 The difference between this comparative example and Example 3 is that the polyhexamethylene guanidine salt modification layer in step 3 is not spin-coated.
[0036] The perovskite solar cells obtained using Examples 1-3 and Comparative Examples 1-3 of the present invention were described below. JV The curve test and stability test, along with the results, are as follows: 1. JV Curve test The aforementioned battery uses silver as the back cell, and during the process... JV During testing, the instrument calibration and assembly method for the formal / reverse perovskite solar cell devices are as follows: First, the Keithley instrument is calibrated using a standard silicon-based solar cell. Then, the prepared cell is placed within it, with the back electrode in contact with the probe in the test cell mold. The positive and negative electrodes of the test cell mold are connected to the positive and negative electrodes of the calibrated Keithley instrument, respectively. A voltage of 1.2 V is applied to the cell for testing. J- V Curve test.
[0037] Figure 5 Examples of inverted perovskite solar cells containing a polyhexamethylene biguanide hydrochloride modified layer (Example 1) and a comparative sample (Comparative Example 1). JV curve, Figure 6 Examples 2 and 2 (comparative examples) are inverted perovskite solar cells containing a polyhexamethylene biguanide molybdate passivation layer. JV curve, Figure 7Examples of trans-perovskite solar cells containing polyhexamethylene guanidine (Example 3) and comparative samples (Comparative Example 3) are provided. JV curve.
[0038] from Figure 5 As can be seen, the photoelectric conversion efficiency of the inverted perovskite solar cell with the addition of a polyhexamethylene biguanide hydrochloride modification layer is the highest at 23.20% (Example 1), with a corresponding current density. J SC , opening pressure V OC The fill factor FF is 24.43 mA / cm². 2 The photoelectric conversion efficiency of Example 1 was 1.144 V and 82.93%. Compared with Comparative Example 1, the photoelectric conversion efficiency was improved by 8.76%.
[0039] from Figure 6 As can be seen, the inverted perovskite solar cell containing a polyhexamethylene biguanide molybdate modified layer (Example 2) has a maximum photoelectric conversion efficiency of 24.02%, corresponding to a current density of J SC , opening pressure V OC The fill factor FF is 25.78 mA / cm². 2 The photoelectric conversion efficiency of Example 2 was 1.132 V and 82.32%. Compared with Comparative Example 2, the photoelectric conversion efficiency was improved by 8.24%.
[0040] from Figure 7 As can be seen, the inverted perovskite solar cell containing the polyhexamethylene guanidine modified layer (Example 3) has a maximum photoelectric conversion efficiency of 24.51%, corresponding to a current density of J SC , opening pressure V OC The fill factor FF is 25.51 mA / cm. 2 The photoelectric conversion efficiency of Example 3 was 1.138V and 84.38%. Compared with Comparative Example 3, the photoelectric conversion efficiency was improved by 11.61%.
[0041] Figure 8 Stability tests were conducted on the inverted perovskite solar cell containing a polyhexamethylene guanidine (PPG) modification layer (Example 3) and a control sample (Comparative Example 3). As can be seen from the figures, the stability of the perovskite solar cell with polymer modification is significantly improved.
[0042] As can be seen from this implementation, the original biguanide hydrochloride is usually used for sterilization. This invention uses it in battery preparation to enhance battery performance and has achieved outstanding results.
[0043] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. It should be noted that, for those skilled in the art, the present invention is intended to cover any variations, uses, or adaptations of this application that follow the general principles of this application and include common knowledge or customary technical means in the art that are not disclosed in this application.
Claims
1. A method for improving the photoelectric performance and stability of perovskite solar cells based on interface modification, characterized in that: The polyguanidine polymer is applied to the interface between the electron transport layer and the tin dioxide layer by a coating process to form a modification layer, which is used to strengthen the interlayer bonding force and improve the photoelectric performance and stability of the battery. The polyguanidine polymer modification layer is located above the electron transport layer and below the tin dioxide layer.
2. The method for improving the photoelectric performance and stability of perovskite solar cells based on interface modification according to claim 1, characterized in that, The main chain or side chain of the polyguanidine polymer contains multiple guanidine functional groups.
3. A method for improving the photoelectric performance and stability of perovskite solar cells based on interface modification according to claim 1 or 2, characterized in that, The polyguanidine polymers include one or more of the functional groups of aminoguanidine, monoguanidinium triguanidinium urea, or cytoguanidine.
4. A perovskite solar cell, characterized in that, The perovskite solar cell is obtained by any one of the methods described in claims 1-3, and includes a conductive glass substrate layer, a hole transport layer, a perovskite light absorption layer, a passivation layer, an electron transport layer, a modification layer, a tin dioxide blocking layer, and a metal electrode layer. The modification layer is formed on the interface of the electron transport layer by a spin coating process.
5. The perovskite solar cell according to claim 4, characterized in that, The thickness of the polyguanidine polymer modification layer ranges from 1 to 10 nm.
6. A perovskite solar cell based on a polymer interface modification layer according to claim 1, characterized in that: The modified layer is mainly formed by spin-coating or coating with a polyguanidine polymer solution, wherein the concentration of the polyguanidine polymer solution is 0.1~2 mg / mL.
7. The method for preparing a perovskite solar cell according to any one of claims 4-6, characterized in that: The method is as follows: 1) Clean the ITO or FTO glass sequentially with deionized water, acetone and ethanol solution using ultrasonic cleaning, dry it with nitrogen, and then treat it in an ultraviolet ozone cleaner. Assemble the hole transport layer on the surface of the conductive substrate by coating or vapor deposition. 2) Dissolve FAI and PbI2 in N,N-dimethylformamide (DMF) to obtain a perovskite precursor solution with a concentration of 1.0~2.0 mol / L. Spin coat the perovskite precursor solution onto the surface of the hole transport layer using a spin coater at a speed of 2000~5000 r / min. Use ethyl acetate (EA) as the antisolvent. After spin drying for 15~35 seconds, drop the solution onto the center of the spin-coated ITO or FTO glass substrate. Continue spin drying for 3~10 seconds, then place the substrate on a hot plate at 100~150 ℃ and anneal for 5~30 minutes to form a perovskite absorber layer. 3) Assemble the electron transport layer on the substrate prepared in step 2) by coating or vapor deposition; 4) A layer of polyguanidine polymer is uniformly coated onto the surface of the electron transport layer using spin coating or coating method as a modification layer; 5) Deposit SnO2 as a hole-blocking layer on the modified layer prepared in step 4); 6) Finally, a back electrode is deposited on the surface of the hole blocking layer.
8. The method for preparing a perovskite solar cell based on a polymer interface modification layer as described in claim 7, characterized in that: In step 4), the polyguanidine polymer is dissolved in an alcohol such as isopropanol (IPA), ethanol, or butanol, or a mixture thereof, and the concentration of the polyguanidine polymer in the solution is 0.1~2.5 mg / L.
9. The method for preparing a perovskite solar cell based on a polymer interface modification layer as described in claim 7, characterized in that: In step 2, FAI and PbI2 can be replaced by FAPbI3, MAPbI3, FAPbBr3, MAPbBr3, CsPbI3, CsPbBr3 and mixtures thereof; In step 2), FAI can be replaced by MAI, FABr, MABr, CsI, CsBr or a mixture thereof; In step 2), PbI2 can be replaced by PbBr2, PbCl2, Pb(SCN)2 or a mixture thereof; The DMF in step 2) can be replaced by N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAc), or a mixture thereof. In step 2), EA can be replaced by propyl acetate, diethyl ether, chlorobenzene, anisole, or a mixture thereof.