A hafnium oxide ferroelectric storage material and its preparation method
By introducing a dual-mode gradient structure of bulk La3+ substitution and surface Ti3+ interstitial doping into hafnium oxide ferroelectric thin films, combined with TiN bottom electrodes and remote plasma processing, the problems of high polarization intensity and low coercivity, low-temperature process compatibility and oxygen vacancy migration in hafnium oxide ferroelectric thin films were solved, thereby improving durability and electrical performance.
Patent Information
- Application Number
- CN202611330475.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to achieve both high polarization intensity and low coercivity in hafnium oxide ferroelectric thin films while maintaining low-temperature process compatibility and durability, and oxygen vacancy migration leads to fatigue failure.
A dual-mode gradient structure of bulk La3+ substitutional doping and surface Ti3+ interstitial doping is adopted. Combined with the lattice mismatch self-assembly of TiN bottom electrode and remote plasma treatment, low-temperature crystallization and selective reduction are achieved, forming an in-plane compressive stress gradient to suppress oxygen vacancy migration.
It achieves synergistic optimization of high polarization intensity, low coercivity field and durability, reduces write voltage and increases charge storage density, while maintaining CMOS back-end process compatibility.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of inorganic materials technology, specifically relating to a hafnium oxide ferroelectric storage material and its preparation method. Background Technology
[0002] Since its initial report in 2011, hafnium oxide (HfO2)-based ferroelectric thin films have been considered a key candidate material for breaking through the miniaturization limits of traditional perovskite ferroelectric materials (such as PZT and SBT) due to their high compatibility with CMOS processes and the ability to maintain ferroelectricity at nanometer-scale thicknesses. They have shown great application potential in ferroelectric random access memory, ferroelectric field-effect transistors, and neuromorphic computing. Current technologies mainly control the HfO2 ferroelectric phase (orthorhombic PcaO2) through doping modification and fabrication process optimization. 21 The formation and stability of ( ). However, existing technologies still have the following significant shortcomings: Firstly, a single substitutional doping mode struggles to achieve synergistic optimization of polarization intensity and coercivity. For example, CN122003093A discloses a double-aluminum-layer-doped hafnium zirconium oxide ferroelectric thin film. This method prepares HZO thin films via atomic layer deposition and introduces double-aluminum oxide doping, promoting the transformation of tetragonal and monoclinic phases to orthorhombic ferroelectric phases during annealing, thereby improving residual polarization intensity and cycle stability. However, this approach relies solely on Al... 3+ While substitutional doping can stabilize the ferroelectric phase, it does not solve the problem of excessively high write voltage caused by high coercivity (typically >1 MV / cm), which limits low-power applications.
[0003] Secondly, the high crystallization temperature is not compatible with advanced CMOS back-end processes. For example, the hafnium oxide-based ferroelectric gate field-effect transistor disclosed in CN109962112B uses rapid thermal annealing (RTA) technology with annealing temperatures as high as 400-1000℃ and times of 1-60 seconds. Although it can activate doped ions and form a ferroelectric phase, such a high thermal budget far exceeds the <400℃ limit usually required by CMOS back-end processes (BEOL), making it impossible to directly integrate the ferroelectric layer on the wafer with the prepared metal interconnect layer, which seriously restricts the realization of the three-dimensional stacked architecture.
[0004] Third, uncontrolled oxygen vacancy migration easily leads to fatigue failure and degradation of retention properties. While existing doping schemes can partially stabilize the ferroelectric phase, they lack a targeted suppression mechanism for oxygen vacancies (Vö), the core cause of ferroelectric fatigue. Substitutional doping (such as La) 3+ Replacement for Hf 4+ Although charge compensation is introduced, a single doping mode cannot simultaneously achieve the dual effects of electrostatic pinning and energy level shielding of oxygen vacancy migration paths, resulting in device limitations at 10... 9 After each cycle, the polarization intensity decreases significantly and is typically maintained for only 3-5 years.
[0005] In summary, this invention aims to improve the performance of hafnium ferroelectric materials in terms of high polarization intensity, low coercivity, low-temperature processing, and long durability through multi-mechanism coupling. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention constructs a bulk La... 3+ Substitutional doping, surface Ti 3+ The interstitial doped dual-mode gradient structure utilizes the self-assembly of TiN bottom electrode lattice mismatch to induce in-plane compressive stress, and combines it with remote plasma to achieve simultaneous crystallization of ferroelectric phase and surface selective reduction at low temperature. This solves the problems in the prior art where high polarization intensity is inevitably accompanied by high coercivity field, low-temperature process cannot crystallize, and oxygen vacancy migration leads to fatigue failure. While maintaining compatibility with CMOS back-end processes, it achieves improved residual polarization intensity, reduced coercivity field, and improved durability.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention provides a method for preparing hafnium oxide ferroelectric storage material, comprising the following steps: Step A: A TiN bottom electrode is fabricated on a Si(100) substrate using thermal atomic layer deposition; Step B: Spin-coat the Hf / La / Ti precursor solution onto the TiN bottom electrode. Heat-treat each layer immediately after spin-coating. Repeat the spin-coating-heat-treating operation to obtain an amorphous precursor film on the TiN bottom electrode. Step C: Apply a DC self-bias to the substrate and use a remote inductively coupled plasma system to perform low-temperature crystallization treatment on the amorphous precursor film to obtain hafnium oxide ferroelectric storage material.
[0008] This invention involves depositing a hafnium oxide-based ferroelectric thin film on a TiN substrate. An in-plane lattice mismatch exists between the lattice constant of the TiN substrate (α = 4.24 Å) and the orthorhombic HfO2 phase (α = 5.08 Å), inducing in-plane biaxial compressive stress in the HfO2 film. According to elasticity theory, this in-plane biaxial compressive stress (σ < 0) causes the HfO2 lattice to compress in-plane and elongate out-of-plane. The orthorhombic phase (Pca...) 21 The polarization axis of TiN is along the
[001] direction, and the out-of-plane elongation is conducive to the displacement of oxygen atoms along the c-axis, enhancing ion displacement polarization; at the same time, compressive stress helps to suppress the stabilization of the monoclinic phase (the monoclinic phase is more stable under tensile stress), promoting the thermodynamic stability of the orthorhombic phase over a wider temperature range. In addition, the dislocation network of the semi-coherent interface formed between TiN and HfO2 helps to release some stress, making the stress field gradient distribution and avoiding stress concentration at the interface that could lead to film cracking.
[0009] In some embodiments, in step A, the thermal atomic layer deposition temperature is 190–210°C, and the pulse operation of the thermal atomic layer deposition is as follows: sequentially performing tetrakis(dimethylamino)titanium pulse for 0.1–0.3 s, NH3 pulse for 1–3 s, and N2 purging for 8–12 s, for 180–220 cycles.
[0010] The low-temperature thermal atomic layer deposition in step A helps to avoid excessive growth of TiN grains (<20nm), and the resulting fine-grained TiN provides high-density grain boundaries, which can enhance the interfacial bonding energy with HfO2.
[0011] Step B, layer-by-layer spin coating, makes the film thickness controllable. Heat treatment of organic residues forms a porous amorphous structure, providing a channel for the penetration of plasma active particles. Step C, remote plasma, achieves "non-thermal equilibrium" crystallization. High-energy electrons break Hf-O and Ti-O bonds to promote atomic rearrangement, while low-energy ions avoid bombardment damage.
[0012] In some embodiments, step B involves the following steps for preparing the Hf / La / Ti precursor solution: In a glove box, Hf(OC2H5)4 was dissolved in ethylene glycol methyl ether, acetylacetone was added, and the mixture was stirred until completely dissolved to obtain a transparent solution A; La(acac)3 was dissolved in ethylene glycol methyl ether and stirred until completely dissolved to obtain solution B; Ti(OC4H9)4 was mixed with acetylacetone and stirred at room temperature until completely dissolved to obtain solution C; solutions B and C were added to A in sequence, and the mixture was stirred to obtain the Hf / La / Ti precursor solution.
[0013] In some embodiments, the molar ratio of Hf(OC2H5)4, La(acac)3, and Ti(OC4H9)4 is 1:(0.07-0.09):(0.07-0.09).
[0014] In some embodiments, in step B, the spin coating speed is 2600-3200 rpm and the spin coating time is 25-35 s; the heat treatment temperature is 130-160℃ and the heat treatment time is 4-8 min.
[0015] The heat treatment temperature used in this invention is lower than the complete decomposition temperature of the organic precursors (metal alkoxides, acetylacetone salts) (typically >300℃), so that each layer retains a portion of the organic ligands as a molecular spacer layer, thereby inhibiting interlayer atomic diffusion and maintaining the uniformity of the interlayer distribution of La and Ti; combined with a short heat treatment time, it avoids non-uniform nucleation caused by local hot spots.
[0016] The multilayer amorphous stacking obtained by repeated spin coating-heat treatment operation gives the final film a layered amorphous-crystallized structure. During crystallization, each layer nucleates independently, refining the grain size to 10-15 nm. The high volume fraction of grain boundaries of nanocrystals is beneficial for pinning ferroelectric domain walls, improving coercive field uniformity and suppressing fatigue.
[0017] In some implementations, the specific conditions for the remote inductively coupled plasma processing in step C are as follows: The plasma source gas is a mixture of H2 and Ar; the total gas flow rate is 90–100 sccm; the radio frequency power is 280–320 W; the substrate temperature is 230–260℃; the processing time is 25–35 min; the chamber pressure is 10–20 Pa; and the distance between the plasma source and the substrate is 10–20 cm.
[0018] The mixture of H2 and Ar ensures the simultaneous presence of high concentrations of H· radicals and Ar metastable atoms in the plasma. The Ar metastable energy is efficiently transferred to the metal-oxygen bonds on the film surface (Hf-O bond energy ≈ 7.8 eV, Ti-O bond energy ≈ 6.9 eV) through Penning ionization and energy resonance transfer mechanisms, promoting amorphous network breakage and atomic diffusion. H· radicals possess reducing properties (E... o (H + / H2)=0V, but the plasma-state H· has extremely high activity, and can selectively reduce surface Ti. 4+ For Ti 3+ (Ti) 4 + / Ti 3+ The standard electrode potential is +0.1V, and thermodynamically, H· can drive this reduction, while the bulk La... 3+ Because of its extremely low reduction potential (La 3+ (La=-2.37V) remains stable. The substrate temperature provides thermal activation energy, which, in conjunction with plasma energy, makes the crystallization activation energy lower than that of traditional thermal annealing, thus achieving low-temperature crystallization.
[0019] In some embodiments, the volume ratio of H2 to Ar is 1:(8-10).
[0020] H2 plasma reduction treatment reduces the Ti content in the thin film surface region. 4+ Convert to Ti 3+ Interstitial doped state, while bulk Ti retains Ti. 4+ Substitutional or unreduced H· radicals exist in interstitial spaces, forming a dual-mode gradient doping structure: Specifically, the diffusion of H· radicals in the HfO2 film follows Fick's law. Due to the extremely small radius of H·, it can rapidly penetrate to a depth of 3-5 nm, resulting in a high surface concentration of H· that will... 4+ Restore to Ti 3+ Ti3+ The ionic radius (0.067 nm) is greater than that of Ti. 4+ (0.0605nm); low concentrations of H· in the bulk phase are insufficient to reduce Ti. 4+ Ti 4+ Maintain with La 3+ The co-substitutional state. This surface reduction-bulk phase stable gradient distribution creates a low-barrier polarization reversal region on the surface, while the bulk phase maintains a high polarization intensity.
[0021] In some implementations, in step C, the DC self-bias voltage is -50 to -40V.
[0022] A DC self-bias voltage applied to the substrate can establish a weak electric field in the plasma sheath, which has an effect on charged particles H + Ar + Directional acceleration is achieved, but the acceleration energy is below the sputtering threshold of HfO2 (~200 eV), avoiding physical sputtering damage. There is no electric field effect on neutral particles such as H·, but the bias-induced ion bombardment can slightly compress the surface layer, increasing the surface atomic density and promoting preferential nucleation for surface crystallization. Simultaneously, the DC self-bias can prevent high-energy ions (>100 eV) from directly bombarding the film surface, introducing trace defect oxygen vacancies on the surface by reducing ion energy. These oxygen vacancies interact with Ti... 3+ The formation of defect complexes, which generate a pinning effect at the ferroelectric domain walls through effective charges, inhibits long-range migration of the domain walls, thereby improving fatigue resistance.
[0023] In another aspect, the present invention provides a hafnium ferroelectric storage material obtained by the above preparation method, wherein the material has a coexistence structure of orthorhombic phase and rhombohedral phase, wherein the volume fraction of orthorhombic phase is ≥80%.
[0024] Quadrature phase Pca 21 It is the main contributing phase to the ferroelectricity of HfO2, and its spontaneous polarization originates from Hf 4+ The oxygen atoms, deviating from the center of the oxygen octahedron, undergo cooperative displacement along the c-axis, resulting in macroscopic polarization. The rhombohedral phase R3 exhibits antiferroelectric tendency, but it can exist stably in nanocrystals due to surface energy effects. Furthermore, the rhombohedral phase, as a grain boundary phase (volume fraction <20%), encapsulates the orthorhombic phase grains. The difference in its lattice constant (a≈3.6Å) compared to the orthorhombic phase (a≈5.08Å, b≈5.17Å) generates coherent strain at the grain boundaries, further stabilizing the orthorhombic phase. Simultaneously, the high dielectric constant (ε≈30-40) of the rhombohedral phase can form a dielectric buffer layer at the grain boundaries, homogenizing the electric field distribution, suppressing breakdown caused by local electric field concentration, and reducing leakage current density.
[0025] In some embodiments, the structure of the hafnium oxide ferroelectric storage material includes a bulk region and a surface region; the surface region and the bulk region have a continuous compositional gradient transition layer.
[0026] La in the bulk region 3+ It exists in the HfO2 lattice as a substitutional dopant, replacing Hf 4+ Grid position, due to La 3+ Radius greater than Hf 4+ This generates lattice expansion stress, reducing the orthorhombic Pca phase. 21 An energy barrier is formed, stabilizing the ferroelectric phase; the surface region is 3-5 nm from the upper surface, within which Ti... 3+ Ti exists as interstitial doping at the interstitial sites of the HfO2 lattice. 3+ Interstitial doping introduces 3d 1 Electronic states form shallow donor levels within the band gap, shielding the depolarization field of polarization charges and reducing the coercive field. This gradient structure allows polarization reversal to preferentially occur in the low coercive field region on the surface, while the high polarization intensity region in the bulk provides stable charge storage, achieving a synergistic optimization of easy writing and storage.
[0027] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention achieves easy writing and storage through dual-mode gradient doping, resulting in bulk La... 3+ Substitutional doping introduces charge-compensating defects, and its effective charge forms an electrostatic attraction with oxygen vacancies, inhibiting long-range migration of oxygen vacancies; and La 3+ Radius greater than Hf 4+ This generates lattice expansion stress, lowering the energy barrier for orthorhombic phase formation; simultaneously, the surface Ti... 3+ Interstitial doping introduces 3d 1 Electronic states form shallow donor levels in the band gap, providing a mobile electron shielding depolarization field and reducing the polarization reversal barrier. This gradient structure allows polarization reversal to preferentially occur in the low coercive field region on the surface, while the high polarization intensity region in the bulk provides stable charge storage, achieving a reduction in write voltage while maintaining an increase in charge storage density.
[0028] 2. This invention uses TiN bottom electrode lattice mismatch-induced self-assembly compressive stress to replace high-temperature annealing stress engineering. In-plane lattice mismatch introduces in-plane biaxial compressive stress during thin film growth. The compressive stress causes the HfO2 lattice to compress in-plane and elongate out-of-plane. Since the orthorhombic phase polarization axis is along the
[001] direction, the out-of-plane elongation directly enhances the cooperative displacement of oxygen ions along the c-axis and strengthens ion displacement polarization. At the same time, the compressive stress suppresses monoclinic phase stabilization and widens the thermodynamic stability window of the orthorhombic phase. This stress originates from the interfacial chemical bonding of Ti-NO-Hf, without the need for additional annealing or epitaxial substrate, and is compatible with CMOS processes.
[0029] 3. This invention employs remote plasma-assisted low-temperature crystallization. The remote inductively coupled plasma of a H2 and Ar mixed gas can promote the rearrangement of amorphous network atoms and selectively reduce surface Ti. 4+ For Ti3+ Meanwhile, high-energy electrons in the plasma provide crystallization activation energy, while low-energy ions avoid bombardment damage, making the crystallization activation energy lower than that of traditional thermal annealing, thus meeting the strict limit of BEOL < 400℃.
[0030] 4. This invention improves durability by using a multi-pinching mechanism to maintain a dynamic balance in the distribution of oxygen vacancies throughout the cycle, rather than allowing them to continuously accumulate. Firstly, La 3+ The electrostatic binding energy of substitutional defects and Vö is higher than the thermal activation energy of 85℃, thus inhibiting the thermal migration of Vö; secondly, Ti 3+ The shallow donor levels in the gaps provide mobile electrons, shielding the built-in electric field generated by Vö and reducing the drift driving force of Vö; the third aspect is that the high-density nanograin boundaries act as a Vö diffusion trap network, making it difficult for Vö to cross the grain boundaries and enter adjacent grains after being captured by the grain boundaries, thus preventing the formation of conductive filaments.
[0031] 5. Compared with vacuum processes such as ALD and PLD, the solution spin coating method used in this invention does not require expensive vacuum equipment. The molar ratio of the precursor solution can be precisely controlled, and the combination of spin coating and heat treatment processes ensures the uniformity of film thickness.
[0032] 6. This invention enhances overall electrical performance through a multiphase coexistence structure. The orthorhombic phase provides the main ferroelectricity, while the rhombohedral phase exists as a grain boundary phase. The difference in lattice constant between the rhombohedral phase and the orthorhombic phase generates coherent strain at the grain boundaries, further stabilizing the orthorhombic phase. Simultaneously, the high dielectric constant of the rhombohedral phase forms a dielectric buffer layer at the grain boundaries, homogenizing the electric field distribution and suppressing breakdown caused by local electric field concentration. The synergy of the two phases enables the material to possess both high polarization intensity and low leakage current, thereby improving overall electrical performance. Detailed Implementation
[0033] The present invention will be described below with reference to specific implementation schemes. It should be noted that the following embodiments and comparative examples are examples of the present invention and are used only to illustrate the invention, not to limit it. Other combinations and various modifications within the scope of the present invention can be made without departing from its spirit or scope. It is worth noting that, unless otherwise specified, the raw materials used in the following preparation examples and embodiments are all from any commercially available manufacturer.
[0034] Preparation Example 1 The preparation steps of Hf / La / Ti precursor solution A are as follows: In a glove box (Ar atmosphere, H2O < 1 ppm, O2 < 1 ppm), 0.85 mol Hf(OC2H5)4 was dissolved in 800 mL of ethylene glycol methyl ether, and 0.2 mol acetylacetone was added. The mixture was stirred at 60 °C until completely dissolved to obtain a transparent solution A. 0.075 mol La(acac)3 was dissolved in 100 mL of ethylene glycol methyl ether and stirred at 80 °C until completely dissolved to obtain solution B. 0.075 mol Ti(OC4H9)4 was mixed with 0.1 mol acetylacetone and stirred at room temperature until completely dissolved to obtain solution C. Solutions B and C were added to A in sequence and stirred at 60 °C for 4 h to obtain the Hf / La / Ti precursor solution A.
[0035] Preparation Example 2 The preparation steps of Hf / La / Ti precursor solution B are the same as those in preparation example 1, except that 0.9 mol Hf(OC2H5)4, 0.05 mol La(acac)3, and 0.05 mol Ti(OC4H9)4 were used.
[0036] Preparation Example 3 The preparation steps of Hf / La / Ti precursor solution C are the same as those in Preparation Example 1, except that 0.8 mol Hf(OC2H5)4, 0.1 mol La(acac)3, and 0.1 mol Ti(OC4H9)4 were used.
[0037] Preparation Example 4 The preparation steps of the Hf / La precursor solution are as follows: In a glove box (Ar atmosphere, H2O < 1 ppm, O2 < 1 ppm), 0.85 mol Hf(OC2H5)4 was dissolved in 800 mL of ethylene glycol methyl ether, and 0.3 mol acetylacetone was added. The mixture was stirred at 60 °C until completely dissolved to obtain a clear solution A. 0.15 mol La(acac)3 was dissolved in 100 mL of ethylene glycol methyl ether and stirred at 80 °C until completely dissolved to obtain solution B. Solution B was added to A and stirred at 60 °C for 4 h to obtain the Hf / La precursor solution.
[0038] Preparation Example 5 The preparation steps of the Hf / Ti precursor solution are as follows: In a glove box (Ar atmosphere, H2O < 1 ppm, O2 < 1 ppm), 0.85 mol Hf(OC2H5)4 was dissolved in 900 mL of ethylene glycol methyl ether, and 0.1 mol acetylacetone was added. The mixture was stirred at 60 °C until completely dissolved to obtain a transparent solution A. 0.15 mol Ti(OC4H9)4 was mixed with 0.2 mol acetylacetone and stirred at room temperature until completely dissolved to obtain solution B. Solution B was added to A and stirred at 60 °C for 4 h to obtain the Hf / Ti precursor solution.
[0039] Example 1 A method for preparing hafnium oxide ferroelectric storage material includes the following steps: Step A: A TiN bottom electrode was prepared on a Si(100) substrate by thermal atomic layer deposition at a temperature of 200℃. The pulse operation of thermal atomic layer deposition was as follows: a tetrakis(dimethylamino)titanium pulse of 0.1s, an NH3 pulse of 2s, and an N2 purge of 10s were performed sequentially for 200 cycles. Step B: Spin-coat Hf / La / Ti precursor solution A onto the TiN bottom electrode at a spin speed of 3000 rpm for 30 s; heat-treat immediately after each spin coating at a temperature of 150℃ for 6 min. Repeat the spin coating-heat treatment operation 5 times to obtain an amorphous precursor film on the TiN bottom electrode. Step C: Apply a -50V DC self-bias to the substrate and perform low-temperature crystallization treatment on the amorphous precursor film using a remote inductively coupled plasma system. The specific conditions are as follows: the plasma source gas is a mixed gas with a volume ratio of H2:Ar = 1:9; the total gas flow rate is 100 sccm; the radio frequency power is 300 W; the substrate temperature is 250℃; the processing time is 30 min; the chamber pressure is 10 Pa; and the distance between the plasma source and the substrate is 15 cm, thus obtaining hafnium oxide ferroelectric storage material.
[0040] Example 2 A method for preparing hafnium oxide ferroelectric storage material includes the following steps: Step A: A TiN bottom electrode was prepared on a Si(100) substrate by thermal atomic layer deposition at a temperature of 190℃. The pulse operation of thermal atomic layer deposition was as follows: tetrakis(dimethylamino)titanium pulse for 0.3s, NH3 pulse for 3s, and N2 purge for 12s were performed sequentially for 180 cycles. Step B: Spin-coat Hf / La / Ti precursor solution A onto the TiN bottom electrode at a spin speed of 2600 rpm for 25 s; heat-treat immediately after each spin coating at a temperature of 160℃ for 4 min. Repeat the spin coating-heat treatment operation 10 times to obtain an amorphous precursor film on the TiN bottom electrode. Step C: Apply a -40V DC self-bias to the substrate and perform low-temperature crystallization treatment on the amorphous precursor film using a remote inductively coupled plasma system. The specific conditions are as follows: the plasma source gas is a mixed gas with a volume ratio of H2:Ar = 1:8; the total gas flow rate is 100 sccm; the radio frequency power is 320 W; the substrate temperature is 230℃; the processing time is 35 min; the chamber pressure is 10 Pa; and the distance between the plasma source and the substrate is 15 cm, thus obtaining hafnium oxide ferroelectric storage material.
[0041] Example 3 A method for preparing hafnium oxide ferroelectric storage material includes the following steps: Step A: A TiN bottom electrode was prepared on a Si(100) substrate by thermal atomic layer deposition at a temperature of 210℃. The pulse operation of thermal atomic layer deposition was as follows: a tetrakis(dimethylamino)titanium pulse of 0.1s, an NH3 pulse of 1s, and an N2 purge of 8s were performed sequentially for 220 cycles. Step B: Spin-coat Hf / La / Ti precursor solution A onto the TiN bottom electrode at a spin speed of 3200 rpm for 35 s; immediately after each spin coating, heat-treat at a temperature of 130℃ for 8 min. Repeat the spin coating-heat treatment operation 10 times to obtain an amorphous precursor film on the TiN bottom electrode. Step C: Apply a -50V DC self-bias to the substrate and perform low-temperature crystallization treatment on the amorphous precursor film using a remote inductively coupled plasma system. The specific conditions are as follows: the plasma source gas is a mixture of H2:Ar with a volume ratio of 1:10; the total gas flow rate is 100 sccm; the radio frequency power is 280W; the substrate temperature is 260℃; the processing time is 25min; the chamber pressure is 10Pa; and the distance between the plasma source and the substrate is 15cm, thus obtaining hafnium oxide ferroelectric storage material.
[0042] Example 4 This embodiment provides a method for preparing hafnium oxide ferroelectric storage material, which is the same as in embodiment 1, except that Hf / La / Ti precursor solution A is replaced with Hf / La / Ti precursor solution B.
[0043] Example 5 This embodiment provides a method for preparing hafnium oxide ferroelectric storage material, which is the same as in embodiment 1, except that the Hf / La / Ti precursor solution A is replaced with the Hf / La / Ti precursor solution C.
[0044] Example 6 This embodiment provides a method for preparing hafnium oxide ferroelectric storage material, which is the same as in embodiment 1, except that the plasma source gas is a mixed gas with a volume ratio of H2:Ar = 1:1.
[0045] Comparative Example 1 This comparative example provides a method for preparing hafnium oxide ferroelectric storage material, which is the same as in Example 1, except that the Hf / La / Ti precursor solution A is replaced with an Hf / La precursor solution.
[0046] Comparative Example 2 This comparative example provides a method for preparing hafnium oxide ferroelectric storage material, which is the same as in Example 1, except that the Hf / La / Ti precursor solution A is replaced with an Hf / Ti precursor solution.
[0047] Comparative Example 3 This comparative example provides a method for preparing hafnium oxide ferroelectric storage material, which is the same as in Example 1, except that step C is adjusted as follows: Step C: Without plasma treatment or DC self-bias, the amorphous precursor film is annealed at 500°C for 30 min in a N2 atmosphere to obtain hafnium oxide ferroelectric storage material.
[0048] Comparative Example 4 This comparative example provides a method for preparing hafnium oxide ferroelectric storage material, which is the same as in Example 1, except that step C does not apply a DC self-bias voltage and is directly plasma treated.
[0049] Comparative Example 5 This comparative example provides a method for preparing hafnium oxide ferroelectric storage material, which is the same as in Example 1, except that the TiN bottom electrode is replaced with a Pt bottom electrode, and the material is prepared by DC magnetron sputtering with a thickness of 20 nm and a deposition temperature of 200 °C.
[0050] Performance testing The hafnium oxide ferroelectric storage materials provided in the examples and comparative examples were tested as follows, and the results are shown in Table 1: 1. Ferroelectric loop (PE) test: An AixACCT TF Analyzer 3000 ferroelectric testing instrument was used. The test sample was a ferroelectric storage device with a MIM capacitor structure. A bipolar triangular wave voltage with a frequency of 1kHz and a maximum electric field of ±3 MV / cm was applied. The remanent polarization intensity Pr and coercive field Ec were measured. The structure of the MIM capacitor ferroelectric storage device is as follows: Bottom electrode: TiN or Pt (Comparative Example 5), 20 nm thick, deposited on a Si(100) substrate; Ferroelectric layer: Hafnium oxide ferroelectric thin film, 100 nm thick; Top electrode: Tungsten (W), 50 nm thick, fabricated by DC magnetron sputtering, with an area of 100 μm × 100 μm.
[0051] 2. Leakage current density (JE) test: The test sample was tested in the same way as performance test 1. A Keithley 4200-SCS semiconductor parameter analyzer was used to scan the voltage range of 0-±2V (corresponding to an electric field of 0-±2MV / cm), with a step of 0.05V and a delay time of 1s. The leakage current density was recorded.
[0052] 3. Fatigue Test: The test sample was tested in the same manner as in Performance Test 1, using a bipolar square wave pulse (±2V, pulse width 1μs, frequency 1MHz) for 10 cycles. 10 Once, every 10 6 The cycle is interrupted and the Pr value is measured to evaluate the polarization intensity decay rate.
[0053] 4. XRD testing: A Bruker D8 Advance diffractometer was used, with Cu Kα radiation (λ=1.5406 Å) and a scanning range of 2θ=20°. o -60 o Step size 0.02 o Scanning speed 2 o / min, analyze the thin film phase composition (orthorhombic Pca) 21 Monoclinic phase P21 / c, rhombohedral phase R3) and their contents.
[0054] Table 1 Performance Test Results As shown in Table 1, Example 1 exhibits the highest remanent polarization and the lowest coercive field, along with extremely low leakage current density and low attenuation rate. Compared to Example 1, the changes in process conditions in Examples 2 and 3 may have affected TiN grain refinement and organic ligand decomposition, thereby influencing grain size, crystallization quality, and phase distribution.
[0055] Compared to Example 1, the reduction in La doping in Example 4 weakens the lattice expansion stress caused by substitutional doping, reduces the orthorhombic phase stabilization effect, and decreases the ferroelectric phase volume fraction; simultaneously, the reduction in Ti doping reduces the interstitial Ti content on the surface. 3+ Insufficient concentration weakens the depolarization field shielding effect, significantly increasing Ec; it also reduces oxygen vacancy pinning sites, exacerbating oxygen vacancy migration and accumulation during cycling, and degrading fatigue properties. In Example 5, excessive La... 3+ Substitution may lead to excessive lattice distortion, which in turn induces an increase in non-ferroelectric monoclinic or rhombohedral phases; while excessive Ti 4+ It may produce excessively high Ti levels after reduction. 3+ Interstitial concentration, excessive crowding of interstitial atoms leading to lattice stress relaxation, and excess Ti 3+ The shallow donor level provides too many free electrons, increasing the leakage current channel; in addition, excessive doping may also introduce a large number of intrinsic defects, leading to an increase in oxygen vacancy concentration and deterioration of fatigue and retention properties.
[0056] In Example 6, the H· radical concentration far exceeded the requirement, not only affecting the surface Ti 4+ Restore to Ti 3+ It may also penetrate deeper into the relatively part of the body Hf 4+ The reduction process involves the extraction of a large number of oxygen atoms from the lattice, resulting in an extremely high concentration of oxygen vacancies. Although the polarization reversal barrier disappears after severe lattice disruption, leading to a decrease in Ec, the leakage current increases by orders of magnitude, and the material has lost its ferroelectric storage function. Simultaneously, XRD analysis reveals only broadened amorphous inclusions and weak HfO. x Suboxide diffraction peaks make it impossible to accurately calculate grain size and phase content.
[0057] Comparative Example 1 lacks Ti 3+ Interstitial doping results in the absence of shallow donor levels to shield the depolarization field in the film. Polarization reversal requires overcoming the complete Coulomb interaction and the oxygen octahedral distortion barrier, leading to a significant increase in Ec. Although La 3+ Substitution can still stabilize some orthorhombic phases, but without Ti. 3+ The gap pinning and electron shielding reduce the migration resistance of oxygen vacancies under the cyclic electric field, making it easier for Vö to migrate over long distances and accumulate to form conductive channels, thus accelerating fatigue failure.
[0058] Comparative Example 2 lacks La 3+ Substitutional doping causes the orthorhombic phase to lose its primary lattice expansion stress stabilization mechanism, leading to a decrease in the volume fraction of the ferroelectric phase; simultaneously, La 3+ The lack of charge compensation leads to an increase in oxygen vacancy concentration. A large number of oxygen vacancy forms a leakage current conductive channel, and oxygen vacancy migrates and accumulates rapidly under the cyclic electric field, resulting in a decrease in polarization intensity and a continuous increase in leakage current.
[0059] The 500℃ high-temperature annealing used in Comparative Example 3 may cause rapid growth of HfO2 grains, increasing the size of ferroelectric domains within the large grains and consequently increasing the domain wall migration distance, leading to an increase in Ec. Simultaneously, the high temperature induces interfacial diffusion and oxidation of the TiN bottom electrode, releasing interfacial stress and introducing additional interfacial defects, causing a decrease in Pr. Furthermore, high-temperature annealing cannot achieve the desired effect on Ti... 4+ Selective reduction can also cause thermal stress cracks at the Si-TiN interface of the substrate, increasing the number of leakage current channels.
[0060] Comparative Example 4: Without DC self-bias, active particles in the plasma migrate to the film surface solely through thermal diffusion and concentration gradient, resulting in a significant reduction in penetration depth and flux, and a decrease in surface Ti... 4+ Insufficient reduction efficiency, Ti 3+ Uneven interstitial doping distribution prevents the formation of an effective gradient layer; meanwhile, the lack of bias guidance results in a weak electric field in the plasma sheath, a scattered distribution of ion bombardment energy, uneven crystallization on the thin film surface, incomplete crystallization in local areas, and an increase in leakage current paths.
[0061] In Comparative Example 5, the TiN bottom electrode was replaced with a Pt bottom electrode. The lattice mismatch between Pt's lattice constant (a = 3.92 Å) and the orthorhombic HfO2 phase was greater than that with TiN. This excessive mismatch may lead to the formation of high-density mismatched dislocations at the interface, and the stress is completely released near the interface, failing to be effectively transferred to the bulk phase of the HfO2 film. At the same time, there is a lack of chemical bonding between Pt and HfO2 (TiN is bonded through Ti-NO-Hf), resulting in weak interfacial bonding and low stress coupling efficiency. Consequently, there is almost no in-plane compressive stress in the HfO2 film, and monoclinic phase stabilization is dominant, leading to a decrease in Pr and an increase in Ec.
[0062] The embodiments and comparative examples described above do not limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method of preparing a hafnium oxide iron electric memory material, characterized in that, Includes the following steps: Step A: A TiN bottom electrode is fabricated on a Si(100) substrate using thermal atomic layer deposition; Step B: Spin-coat the Hf / La / Ti precursor solution onto the TiN bottom electrode. Heat-treat each layer immediately after spin-coating. Repeat the spin-coating-heat-treating operation to obtain an amorphous precursor film on the TiN bottom electrode. Step C: Apply a DC self-bias to the substrate and use a remote inductively coupled plasma system to perform low-temperature crystallization treatment on the amorphous precursor film to obtain hafnium oxide ferroelectric storage material.
2. The method for preparing hafnium oxide ferroelectric storage material according to claim 1, characterized in that, In step A, the thermal atomic layer deposition temperature is 190–210°C, and the pulse operation of thermal atomic layer deposition is as follows: sequentially perform tetrakis(dimethylamino)titanium pulse for 0.1–0.3 s, NH3 pulse for 1–3 s, and N2 purging for 8–12 s, for 180–220 cycles.
3. The method for preparing hafnium oxide ferroelectric storage material according to claim 1, characterized in that, In step B, the preparation steps of the Hf / La / Ti precursor solution are as follows: In a glove box, Hf(OC2H5)4 was dissolved in ethylene glycol methyl ether, acetylacetone was added, and the mixture was stirred until completely dissolved to obtain a transparent solution A; La(acac)3 was dissolved in ethylene glycol methyl ether and stirred until completely dissolved to obtain solution B; Ti(OC4H9)4 was mixed with acetylacetone and stirred at room temperature until completely dissolved to obtain solution C; solutions B and C were added to A in sequence, and the mixture was stirred to obtain the Hf / La / Ti precursor solution.
4. The method for preparing hafnium oxide ferroelectric storage material according to claim 3, characterized in that, The molar ratio of Hf(OC2H5)4, La(acac)3, and Ti(OC4H9)4 is 1:(0.07~0.09):(0.07~0.09).
5. The method for preparing hafnium oxide ferroelectric storage material according to claim 1, characterized in that, In step B, the spin coating speed is 2600-3200 rpm and the spin coating time is 25-35 s; the heat treatment temperature is 130-160℃ and the heat treatment time is 4-8 min.
6. The method for preparing hafnium oxide ferroelectric storage material according to claim 1, characterized in that, In step C, the specific conditions for the remote inductively coupled plasma processing are as follows: The plasma source gas is a mixture of H2 and Ar; the total gas flow rate is 90–100 sccm; the radio frequency power is 280–320 W; the substrate temperature is 230–260℃; the processing time is 25–35 min; the chamber pressure is 10–20 Pa; and the distance between the plasma source and the substrate is 10–20 cm.
7. The method for preparing hafnium oxide ferroelectric storage material according to claim 6, characterized in that, The volume ratio of H2 to Ar is 1:(8-10).
8. The method for preparing hafnium oxide ferroelectric storage material according to claim 1, characterized in that, In step C, the DC self-bias voltage is -50 to -40V.
9. The hafnium oxide iron-electron memory material of any one of claims 1 to 8, wherein the hafnium oxide iron-electron memory material is prepared by the method of any one of claims 1 to 8. The hafnium oxide ferroelectric storage material has a coexistence structure of orthorhombic and rhombohedral phases, wherein the volume fraction of the orthorhombic phase is ≥80%.
10. The hafnium oxide ferroelectric storage material according to claim 9, characterized in that, The structure of the hafnium oxide ferroelectric storage material includes a bulk region and a surface region; a continuous compositional gradient transition layer exists between the surface region and the bulk region.
Citation Information
Patent Citations
A ferroelectric gate field-effect transistor and its fabrication method
CN109962112B
Double-aluminum-layer-doped hafnium zirconium oxide ferroelectric film material and preparation method and application thereof
CN122003093A