Oxide Thin Film Post-processing Apparatus and Method

By using high-purity H2O2 gas to form supercritical CO2 with CO2 and surfactants in the oxide thin film treatment, the problem of low H2O2 concentration was solved, achieving efficient repair of oxygen vacancies and improving the dielectric and electrical properties of oxide thin films.

CN123124779APending Publication Date: 2026-11-17张江国家实验室
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510616554.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing supercritical CO2-dissolved H2O2 co-solution solution has a low H2O2 concentration, resulting in insufficient oxygen vacancy repair capacity and efficiency, which affects the dielectric and electrical properties of oxide films.

Method used

High-purity H2O2 gas is mixed with CO2 and gaseous surfactant to form a supercritical CO2 state, thereby increasing the H2O2 concentration and utilizing its high solubility and diffusivity to treat oxide films and fill oxygen vacancy defects.

Benefits of technology

It effectively regulates oxygen vacancy concentration, improves dielectric properties, reduces leakage current, enhances device electrical performance and stability, and increases reaction rate and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124779A_ABST
    Figure CN123124779A_ABST
Patent Text Reader

Abstract

This invention provides an oxide thin film post-treatment apparatus and method, which can improve the oxygen vacancy repair capability and efficiency in the oxide thin film post-treatment process. It includes: a reaction apparatus containing an oxide thin film to be treated; a carbon dioxide gas supply device supplying carbon dioxide gas to the reaction apparatus; a hydrogen peroxide gas supply device supplying hydrogen peroxide gas to the reaction apparatus; a gaseous surfactant supply device supplying gaseous surfactant to the reaction apparatus; and a control device controlling the pressure and temperature of the reaction apparatus to make the carbon dioxide gas inside the reaction apparatus supercritical, thereby using the supercritical carbon dioxide carrying the hydrogen peroxide gas to perform supercritical oxidation treatment on the oxide thin film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductors, and more particularly to an apparatus and method for post-processing oxide thin films in semiconductor manufacturing processes. Background Technology

[0002] In recent years, with the development of high integration and high speed of semiconductor devices, oxide thin films, represented by hafnium oxide (HfO2) and zirconium oxide (ZrO2), have been widely used as dielectric layers in devices such as capacitors and transistors due to their high dielectric constant, low leakage current, high temperature resistance and corrosion resistance.

[0003] However, oxygen vacancies are widely present in oxide thin film materials. The enrichment of oxygen vacancies leads to an increase in film defects and leakage current, thereby affecting the electrical properties of the film, such as dielectric or ferroelectric properties. Therefore, post-processing of oxide thin films is extremely important in semiconductor manufacturing processes.

[0004] One existing oxygen vacancy thin film post-treatment technology uses supercritical carbon dioxide (CO2) to dissolve a eutectic solution of hydrogen peroxide (H2O2) with high oxidizing activity to treat the surface of metal oxide semiconductor field-effect transistors (MOSFETs), thereby improving the oxygen vacancies in the interface layer (GeO2) and dielectric layer (ZrO2), reducing leakage current, and thus obtaining better dielectric properties.

[0005] Supercritical CO2 refers to a fluid state in which the temperature and pressure of CO2 are higher than its critical temperature (Tc = 31.26℃) and critical pressure (Pc = 72.9 atm, approximately 7.39 MPa), respectively. At this point, the gas-liquid interface disappears, and it has both the fluidity of a liquid and the diffusivity of a gas, thus possessing extremely high solubility.

[0006] In addition, hydrogen peroxide (H2O2) has stronger oxidizing activity than O2. Using H2O2 to treat oxygen vacancies in oxides can fill oxygen vacancy defects more efficiently and avoid surface damage.

[0007] In the above-mentioned post-treatment method for oxygen vacancy films, the surfactant ethanol is mixed with an aqueous solution of H2O2 to form a eutectic solution. This eutectic solution is pumped into supercritical CO2 to form supercritical CO2 carrying a certain amount of H2O2. Then, it is introduced into the sample processing chamber. By controlling the temperature and pressure in the sample processing chamber, the supercritical CO2 carrying H2O2 is made to fully contact the sample. After the highly oxidizing H2O2 molecules come into contact with the sample, they can repair the oxygen vacancy defects of the film, thereby improving the film quality and leakage current performance.

[0008] However, existing techniques for repairing oxygen vacancies in thin films by dissolving H2O2 in a supercritical CO2 solution have the drawback of low H2O2 concentration. The co-solution solution contains only 10% highly oxidizing H2O2, with the majority being water (H2O). This results in the supercritical CO2 carrying a large amount of weakly oxidizing water, which interacts with the sample film, significantly weakening the ability and efficiency of oxygen vacancy repair. Summary of the Invention

[0009] The following provides a brief overview of one or more aspects to offer a basic understanding of them. This overview is not an exhaustive summary of all conceived aspects, nor is it intended to identify key or decisive elements of all aspects, nor to define the scope of any or all aspects. Its sole purpose is to present some concepts of one or more aspects in a simplified form to prepare for the more detailed descriptions that follow.

[0010] To overcome the aforementioned shortcomings, this invention aims to provide an apparatus and method for treating oxide thin films by using supercritical CO2 to adsorb high-purity H2O2 gas molecules to improve oxygen vacancies. This enhances the oxygen vacancy repair capability and efficiency in the post-processing of oxide thin films. Consequently, it effectively controls the concentration of oxygen vacancies in the oxide thin film, repairs interface defects, improves leakage current and dispersion, and enhances the electrical performance, stability, and cycle life of the device.

[0011] According to one aspect of the present invention, an oxide thin film post-processing apparatus is provided, comprising:

[0012] A reaction apparatus containing a thin film of oxide to be treated;

[0013] A carbon dioxide gas supply device that supplies carbon dioxide gas to the reaction apparatus;

[0014] A hydrogen peroxide gas supply device that supplies hydrogen peroxide gas to the reaction apparatus;

[0015] A gaseous surfactant supply device that supplies gaseous surfactant to the reaction apparatus; and

[0016] A control device controls the pressure and temperature of the reaction apparatus to make the carbon dioxide gas inside the reaction apparatus supercritical, and uses the supercritical carbon dioxide carrying the hydrogen peroxide gas to perform supercritical oxidation treatment on the oxide film.

[0017] In one embodiment, the concentration of hydrogen peroxide gas in the mixture of carbon dioxide gas, hydrogen peroxide gas, and gaseous surfactant is 30% or more.

[0018] In one embodiment, the molar ratio of the carbon dioxide gas, the hydrogen peroxide gas, and the gaseous surfactant is (1-1.2):1:1.

[0019] In one embodiment, the hydrogen peroxide gas supply device is a solid hydrogen peroxide source.

[0020] In one embodiment, the purity of the hydrogen peroxide gas is 70% to 98%.

[0021] In one embodiment, during the supercritical oxidation process, the pressure inside the reaction apparatus is 8–20 MPa, and the temperature inside the reaction apparatus is 100°C–180°C.

[0022] In one embodiment, the supercritical oxidation treatment time is 1 to 3 hours.

[0023] In one embodiment, one or more of oxygen, water vapor, ozone, and ammonia are further supplied to the reaction apparatus as additive gases, such that the supercritical carbon dioxide carries the hydrogen peroxide gas and the additive gases to post-treat the oxide film.

[0024] According to another aspect of the present invention, a post-treatment method for oxide thin films is provided, comprising post-treatment of oxide thin films disposed in a reaction apparatus, including:

[0025] A mixture of carbon dioxide gas, hydrogen peroxide gas, and gaseous surfactant gas is introduced into the reaction apparatus;

[0026] The pressure and temperature of the reaction device are controlled to make the carbon dioxide gas supercritical.

[0027] The oxide film is subjected to supercritical oxidation treatment using supercritical carbon dioxide carrying the hydrogen peroxide gas.

[0028] In one embodiment, the concentration of hydrogen peroxide gas in the mixture of carbon dioxide gas, hydrogen peroxide gas, and gaseous surfactant is 30% or more.

[0029] In one embodiment, the molar ratio of the carbon dioxide gas, the hydrogen peroxide gas, and the gaseous surfactant is (1-1.2):1:1.

[0030] According to another aspect of the present invention, a semiconductor device is also provided, comprising an oxide thin film obtained by supercritical oxidation using the above-described oxide thin film post-processing method.

[0031] In one embodiment, the semiconductor device is a capacitor comprising a bottom electrode, a top electrode, and an oxide film sandwiched between the bottom electrode and the top electrode.

[0032] The oxide thin film post-treatment apparatus and method provided by this invention can effectively control the concentration of oxygen vacancies in the oxide thin film without introducing surface damage or interfacial oxide layers, ensuring the high dielectric properties of the oxide and reducing leakage current. Furthermore, the oxide thin film post-treatment apparatus and method of this invention have a much higher concentration of active H2O2 than existing solutions, effectively improving the reaction rate and efficiency. Attached Figure Description

[0033] The above-described features and advantages of the present invention will be better understood after reading the detailed description of the embodiments of this disclosure in conjunction with the following accompanying drawings.

[0034] Figure 1 A structural block diagram of the oxide thin film post-processing apparatus of this embodiment is shown.

[0035] Figures 2(a) and 2(b) show example diagrams of the planar capacitor and capacitor column used as samples in this embodiment.

[0036] Figure 3 A schematic diagram of an embodiment of the oxide thin film post-treatment apparatus for oxygen vacancy treatment using supercritical CO2 mixed with high-purity H2O2 gas is shown.

[0037] Figure 4 A flowchart of the oxide thin film post-processing method of this embodiment is shown.

[0038] Figures 5(a) and 5(b) show schematic diagrams of oxygen vacancy treatment in the oxide thin film post-treatment method of this embodiment.

[0039] Figure 6 This diagram illustrates the change in leakage current density before and after oxygen vacancy treatment using supercritical CO2 mixed with high-purity H2O2 gas in this embodiment.

[0040] For clarity, a brief explanation of the reference numerals in the accompanying drawings is provided below:

[0041] 110 reaction apparatus;

[0042] 120 CO2 gas supply device;

[0043] 130H2O2 gas supply device;

[0044] 140 Gaseous surfactant supply device;

[0045] 150 Control device;

[0046] 301 High-Pressure Reactor;

[0047] 302 Sample Stage;

[0048] 310 CO2 gas cylinder;

[0049] Gas pipelines 311, 312, and 313;

[0050] Valves V1, V2, V3, and V4. Detailed Implementation

[0051] The following description is provided to enable those skilled in the art to implement and use the invention and adapt it to specific application contexts. Various modifications and uses in different applications will be readily apparent to those skilled in the art, and the general principles defined herein are applicable to a wide range of embodiments. Therefore, the invention is not limited to the embodiments given herein, but should be granted the broadest scope consistent with the principles and novel features disclosed herein.

[0052] In the following detailed description, numerous specific details are set forth to provide a more thorough understanding of the invention. However, it will be apparent to those skilled in the art that practice of the invention is not necessarily limited to these specific details. In other words, well-known structures and devices are shown in block diagram form without being depicted in detail to avoid obscuring the invention.

[0053] Readers should note all documents and references submitted concurrently with this specification and open to public inspection, the contents of which are incorporated herein by reference. Unless otherwise expressly stated, all features disclosed in this specification (including any appended claims, abstracts, and drawings) may be replaced by alternative features for the same, equivalent, or similar purposes. Therefore, unless explicitly stated otherwise, each disclosed feature is merely one example of a set of equivalent or similar features.

[0054] Note that, where used, the markings left, right, front, back, top, bottom, front, back, clockwise, and counterclockwise are merely for convenience and do not imply any specific fixed direction. In fact, they are used to reflect the relative position and / or orientation between different parts of an object. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0055] Note that, in practice, "further," "preferably," "even further," and "more preferably" are simply starting points for describing another embodiment based on the foregoing embodiments. The combination of the content following "further," "preferably," "even further," or "more preferably" with the foregoing embodiments constitutes the complete configuration of another embodiment. Any combination of several "further," "preferably," "even further," or "more preferably" settings following the same embodiment can form yet another embodiment.

[0056] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. It should be noted that the aspects described below with reference to the accompanying drawings and specific embodiments are merely exemplary and should not be construed as limiting the scope of protection of the present invention in any way.

[0057] Figure 1 A structural block diagram of the oxide thin film post-processing apparatus according to this embodiment is shown. (Refer to...) Figure 1 The oxide film post-processing device mainly includes a reaction device 110, a CO2 gas supply device 120, an H2O2 gas supply device 130, a gaseous surfactant supply device 140, and a control device 150.

[0058] The reaction apparatus 110 is used to hold the sample to be processed, such as a planar capacitor or a high aspect ratio capacitor column having an oxide thin film as the dielectric layer. Figures 2(a) and 2(b) show example structural diagrams of the planar capacitor and capacitor column used as samples in this embodiment, respectively. The planar capacitor shown in Figure 2(a) is a stacked planar structure consisting of a bottom electrode, a dielectric layer, and a top electrode stacked sequentially from bottom to top. The capacitor column shown in Figure 2(b) is a circular array structure with a high aspect ratio column having a bottom electrode, a dielectric layer, and a top electrode arranged radially from the inside to the outside. However, it is not limited to these; any oxide thin film requiring oxygen vacancy treatment can be post-processed in the reaction apparatus 110.

[0059] The reaction apparatus 110 is connected to a CO2 gas supply device 120, an H2O2 gas supply device 130, and a gaseous surfactant supply device 140, respectively. The CO2 gas supply device 120 supplies CO2 gas to the reaction apparatus 101; for example, it can be a CO2 storage tank. By controlling the temperature and pressure inside the reaction apparatus 101 to be higher than the critical temperature (Tc = 31.26℃) and critical pressure (Pc = 72.9 atm, approximately 7.39 MPa) of CO2, the CO2 gas inside can be made into a supercritical state.

[0060] H2O2 gas supply device 130 can supply H2O2 gas to reaction device 110, for example, by using a commercial solid H2O2 source to provide high-purity (70% to 98%) H2O2 gas.

[0061] The gaseous surfactant supply device 140 supplies gaseous surfactants, such as ethanol and isopropanol, to the reaction device 110 to connect non-polar supercritical CO2 molecules with polar H2O2 molecules, thereby overcoming the incompatibility between the two and stably binding or dispersing them together to achieve interaction and effectively perform their functions.

[0062] The control device 150 controls the reaction device 110, the CO2 gas supply device 120, the H2O2 gas supply device 130, and the gaseous surfactant supply device 140 respectively. For example, it controls the temperature and pressure of the reaction device 110 to achieve the temperature and pressure required for supercriticality. In addition, it controls the on / off connection between the CO2 gas supply device 120, the H2O2 gas supply device 130, the gaseous surfactant supply device 140 and the reaction device 110, as well as the flow rate and proportion of the gas supplied by each supply device 120-140.

[0063] According to the oxide thin film post-processing apparatus of this embodiment, CO2 gas, gaseous surfactant, and highly oxidizing H2O2 gas are introduced into the reaction apparatus 110, and the CO2 gas is made into a supercritical state. By adjusting the concentration of H2O2 gas as an oxidant, a higher concentration of H2O2 molecules than that in the co-solution solution of the prior art can be carried in the supercritical CO2. Through the permeation and diffusion of this supercritical CO2 carrying a high concentration of H2O2 gas molecules into the planar structure or high aspect ratio nanoporous structure of the sample, the high concentration of H2O2 gas molecules can fully interact with the surface of the oxide thin film in the sample, thereby more effectively eliminating unsaturated bonds on the surface, filling oxygen vacancies, regulating the distribution of oxygen vacancies, and repairing interfacial defect states.

[0064] The oxide thin film post-processing apparatus and method of this embodiment will be described below with reference to specific embodiments. In this embodiment, gaseous ethanol is used as the gaseous surfactant, and the sample uses a hafnium-based oxide capacitor pillar device with a high aspect ratio, the capacitor structure of which can be denoted as TiN / Hf. 1-x Zr x O2 / TiN, that is, using TiN as the bottom electrode and top electrode, and Hf 1-x Zr x The hafnium oxide of O2 is used as the dielectric layer. However, this is just an example, and the invention is not limited thereto.

[0065] Figure 3 This diagram illustrates a structural schematic of an embodiment of an oxide thin film post-treatment apparatus that utilizes supercritical CO2 mixed with a high concentration of H2O2 gas for oxygen vacancy treatment.

[0066] To simplify the explanation, Figure 3 The oxide thin film post-processing device 300 shown in this embodiment mainly includes a high-pressure reactor 301, a CO2 gas tank 310, gas pipelines 311, 312, 313, and valves V1, V2, V3, and V4.

[0067] High-pressure reactor 301 (equivalent to Figure 1The "reaction apparatus" (as described) includes a sample stage 302 for holding the sample S to be processed, which is a hafnium-based oxide Hf. 1-x Zr x Capacitor pillar devices using O2 as the dielectric layer material (e.g., the structure shown in Figure 2(b)).

[0068] The temperature and pressure inside the high-pressure reactor 301 can be adjusted by a control device (not shown), which may include a heating device, vacuum equipment, temperature and pressure regulating device (not shown). Additionally, the high-pressure reactor 301 can be connected to the outside via valve V4 for discharging waste gas, waste liquid, etc.

[0069] CO2 cylinder 310 (equivalent to) Figure 1 The “CO2 gas supply device” in the text is used to store CO2 gas and is connected to the high-pressure reactor 301 via gas pipeline 311 and valve V1. The CO2 gas tank 310 and the high-pressure reactor 301 constitute a supercritical CO2 generator.

[0070] Gas line 312 is connected to, for example, a commercial solid H2O2 source (not shown) (equivalent to...) Figure 1 The device (“H2O2 gas supply device”) is connected to the high-pressure reactor 301 via valve V2, and provides stable and high-purity (e.g. 70% to 98%) H2O2 gas to the high-pressure reactor 301.

[0071] Gaseous ethanol is supplied to the high-pressure reactor 301 via gas pipeline 313 and valve V3 to act as a surfactant. Gaseous ethanol can be prepared by heating or evaporating liquid ethanol under reduced pressure (equivalent to...). Figure 1 (The "gaseous surfactant supply device" in the text).

[0072] Here, the flow rate or mixing ratio of CO2 gas, H2O2 gas, and gaseous ethanol introduced into the high-pressure reactor 301 can be controlled by a flow meter (not shown).

[0073] Figure 4 A flowchart is shown of a method for processing a sample using the oxide thin film post-processing apparatus of this embodiment. Although the above method is illustrated and described as a series of actions for the sake of simplicity, it should be understood and appreciated that these methods are not limited to the order of the actions, as some actions may occur in a different order and / or concurrently with other actions from the illustrations and descriptions herein or not illustrated and described herein but which may be understood by those skilled in the art, according to one or more embodiments.

[0074] For the capacitor pillar array structure shown in Figure 2(b), firstly, in step 401, a bottom electrode and a dielectric thin film are sequentially fabricated on the pillars by, for example, atomic layer deposition. In this embodiment, titanium nitride (TiN) is used as the bottom electrode, but TaN, Mo, W, Ru, RuO2, IrOx, WO3, etc., can also be used. The dielectric thin film is made of hafnium-based oxide Hf. 1-x Zr x O2, but it can also be a multilayer film or solid solution of materials such as HfO2, ZrO2, TiO2, SiO2, La2O3, Y2O3, Al2O3, Nb2O5 (NbO, NbO2, Nb2O3).

[0075] Then, in step 402, the dielectric thin film formed in step 401 is subjected to the post-processing described in this embodiment, namely oxygen vacancy treatment.

[0076] Specifically, in step 4021, sample S is placed in high-pressure reactor 301 and sealed. A vacuum device is used to achieve a certain vacuum level inside the high-pressure reactor 301 (e.g., below 1 Pa). Then, valves V1, V2, and V3 are opened, and CO2 gas, H2O2 gas, and gaseous ethanol are introduced into the high-pressure reactor 301 through gas pipelines 311, 312, and 313 respectively, and then sealed. Here, to increase the concentration of H2O2 gas acting on oxygen vacancy treatment and achieve a better effect of filling oxygen vacancies, the molar ratio of CO2 gas, H2O2 gas, and gaseous ethanol in the mixed gas can be set to (1-1.2):1:1, so that the concentration of high-purity H2O2 gas in the mixed gas is above 30%.

[0077] Then, in step 4022, the pressure (8-20 MPa) and temperature (100℃-180℃) inside the high-pressure reactor 301 are controlled to make the CO2 gas become supercritical CO2. At this time, gaseous ethanol acts as a surfactant, with one end connected to polar high-purity H2O2 molecules and the other end connected to non-polar supercritical CO2. Utilizing the high solubility, high diffusivity, and low surface tension of supercritical CO2, supercritical CO2 carrying H2O2 is formed.

[0078] In step 4023, supercritical CO2 carrying H2O2 permeates and diffuses in the high aspect ratio nanoporous structure of sample S. The high concentration of H2O2 molecules it carries can fully interact with the surface of the oxide thin film medium material, fill oxygen vacancies, and eliminate unsaturated bonds on the surface of the medium layer.

[0079] Figures 5(a) and 5(b) illustrate the oxygen vacancy treatment in the oxide thin film post-processing method of this embodiment. Figure 4A schematic diagram of step 4023. In the upper part of Figure 5(a), supercritical CO2 carrying a high concentration of H2O2 gas permeates and diffuses into the pores of each columnar structure of sample S, allowing the high concentration of H2O2 gas molecules to fully contact the surface of the oxide film serving as the dielectric layer in the capacitor column. The lower part of Figure 5(a) shows that sample S, processed in this step, is in Hf x Zr 1-x O2 represents the cross-sectional structure of a capacitor column made of dielectric material (excluding the top electrode). Specifically, a bottom electrode TiN is formed on the inner wall of a column filled with filler in the center, and a dielectric layer Hf is formed around the outer periphery of the bottom electrode TiN. x Zr 1-x O2.

[0080] The upper part of Figure 5(b) schematically represents Hf with a red circle. x Zr 1-x Oxygen vacancies exist on the surface of the O2 dielectric layer, with oxygen atoms missing at certain positions in the Hf-Zr-O lattice. The generation of oxygen vacancies causes changes in local dielectric properties, affecting the overall capacitance performance of the device. However, after treatment with supercritical CO2 carrying H2O2 gas, some oxygen vacancies are oxidized and filled under the action of high-concentration H2O2 (as shown in the lower part of Figure 5(b)).

[0081] Back Figure 4 The processing time in step 4023 can be 1–3 hours to ensure sufficient reaction between the H2O2 gas and the surface of the dielectric film. Afterwards, valve V4 can be opened to discharge the waste gas and waste liquid generated in this step. Thus, the dielectric film that has undergone oxygen vacancy treatment is obtained.

[0082] Finally, in step 403, a top electrode is fabricated on the oxide dielectric layer film after the above treatment by, for example, deposition. In this embodiment, TiN is used as the top electrode, but it can also be TaN, Mo, W, Ru, RuO2, IrOx, WO3, etc.

[0083] pass Figure 4 The processing flow shown can obtain a MIM (Metal-Insulator-MetalCapacitor) capacitor structure with a good interface state.

[0084] Figure 6 This diagram illustrates the change in leakage current density before and after oxygen vacancy treatment using supercritical CO2 mixed with high-purity H2O2 gas, as shown in this embodiment. Figure 6 It can be seen that the leakage current density J of the sample without supercritical CO2-carrying H2O2 gas oxidation treatment at 1V voltage is... leak 3.03x10 -7 A / cm 2The leakage current density J of the treated sample at 1V voltage leak 5.02x10 -8 A / cm 2 This means that the leakage current density has decreased by an order of magnitude.

[0085] Therefore, the oxygen vacancy concentration at the interface is significantly reduced and the interface defect state density is lowered after supercritical CO2 treatment with high-purity H2O2 gas in this embodiment, effectively improving the TiN / Hr ratio. 1-x Zr x The O2 / TiN capacitor structure improves leakage current and phase stability, thereby enhancing the read / write stability and cycle life of the capacitor, as well as reducing the capacitor's refresh rate and power consumption.

[0086] The above embodiments describe a scheme for filling oxygen vacancies through supercritical oxidation by mixing supercritical CO2 with H2O2 gas. However, this is not a limitation. In some embodiments, supercritical CO2 can also be mixed with any one or more of O2, H2O, H2O2, and O3 to fill oxygen vacancies through supercritical oxidation. NH3 gas can also be mixed with supercritical CO2 to fill oxygen vacancies or to passivate the film surface.

[0087] The oxide thin film post-processing apparatus and method of the present invention utilize the dual fluid and gas properties of supercritical CO2 to carry a high concentration of highly active oxidant H2O2 gas onto a planar or high aspect ratio structure. This allows for the control of oxygen vacancy defects in the oxide thin film, improving its interfacial performance and stability with the top electrode, while avoiding surface damage and the formation of an interfacial oxide layer. This ensures the high dielectric properties of the oxide thin film, reduces leakage current, and decreases the equivalent oxide thickness (EOT). Compared to existing co-solution H2O2 solutions, this method provides a higher concentration of highly active oxidizing H2O2, effectively improving the reaction rate and efficiency.

[0088] This invention is applicable to fields such as electronic devices and storage devices, and can improve the performance and reliability of devices, thereby promoting the development of related fields.

[0089] The preceding description is provided to enable any person skilled in the art to practice the various aspects described herein. However, it should be understood that the scope of protection of this invention should be determined by the appended claims and should not be limited to the specific structures and components of the embodiments described above. Various changes and modifications can be made to the embodiments by those skilled in the art within the spirit and scope of this invention, and these changes and modifications also fall within the scope of protection of this invention.

Claims

1. A post-processing apparatus for oxide thin films, characterized in that, include: A reaction apparatus containing a thin film of oxide to be treated; A carbon dioxide gas supply device that supplies carbon dioxide gas to the reaction apparatus; A hydrogen peroxide gas supply device that supplies hydrogen peroxide gas to the reaction apparatus; A gaseous surfactant supply device that supplies gaseous surfactant to the reaction apparatus; and A control device controls the pressure and temperature of the reaction apparatus to make the carbon dioxide gas inside the reaction apparatus supercritical, and uses the supercritical carbon dioxide carrying the hydrogen peroxide gas to perform supercritical oxidation treatment on the oxide film.

2. The oxide thin film post-processing apparatus as described in claim 1, characterized in that, In the mixture of carbon dioxide gas, hydrogen peroxide gas, and gaseous surfactant, the concentration of hydrogen peroxide gas is 30% or more.

3. The oxide thin film post-processing apparatus as described in claim 1 or 2, characterized in that, The molar ratio of the carbon dioxide gas, the hydrogen peroxide gas, and the gaseous surfactant is (1-1.2):1:

1.

4. The oxide thin film post-processing apparatus as described in claim 1 or 2, characterized in that, The hydrogen peroxide gas supply device is a solid hydrogen peroxide source.

5. The oxide thin film post-processing apparatus as described in claim 1 or 2, characterized in that, The purity of the hydrogen peroxide gas is 70% to 98%.

6. The oxide thin film post-processing apparatus as described in claim 1 or 2, characterized in that, During the supercritical oxidation process, the pressure inside the reaction device is 8–20 MPa, and the temperature inside the reaction device is 100°C–180°C.

7. The oxide thin film post-processing apparatus as described in claim 6, characterized in that, The supercritical oxidation treatment time is 1 to 3 hours.

8. The oxide thin film post-processing apparatus as described in claim 1 or 2, characterized in that, The reaction apparatus is further supplied with one or more of oxygen, water vapor, ozone, and ammonia as additive gases, so that the supercritical carbon dioxide carries the hydrogen peroxide gas and the additive gases to perform post-treatment on the oxide film.

9. A method for post-processing oxide thin films, comprising post-processing oxide thin films disposed in a reaction apparatus, characterized in that, include: A mixture of carbon dioxide gas, hydrogen peroxide gas, and gaseous surfactant gas is introduced into the reaction apparatus; The pressure and temperature of the reaction device are controlled to make the carbon dioxide gas supercritical. The oxide film is subjected to supercritical oxidation treatment using supercritical carbon dioxide carrying the hydrogen peroxide gas.

10. The post-processing method for oxide thin films as described in claim 9, characterized in that, In the mixture of carbon dioxide gas, hydrogen peroxide gas, and gaseous surfactant, the concentration of hydrogen peroxide gas is 30% or more.

11. The post-processing method for oxide thin films as described in claim 9 or 10, characterized in that, The molar ratio of the carbon dioxide gas, the hydrogen peroxide gas, and the gaseous surfactant is (1-1.2):1:

1.

12. A semiconductor device, characterized in that, This includes oxide films obtained by supercritical oxidation using the oxide film post-processing method according to any one of claims 9 to 11.

13. The semiconductor device as claimed in claim 12, characterized in that, The semiconductor device is a capacitor comprising a bottom electrode, a top electrode, and an oxide thin film sandwiched between the bottom electrode and the top electrode.