Resin compositions, cured products, prepregs, resin composites, printed circuit boards, and semiconductor devices
By combining isopropylene resin and maleimide compounds to form a high molecular weight resin composition, the demand for low thermal expansion coefficient materials for the diverse applications of electronic devices is addressed, thereby improving the heat resistance and low dielectric properties of printed circuit boards.
Patent Information
- Application Number
- CN202580028821.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-22
- Filing Date
- 2025-04-16
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, the diversification of applications of electronic devices has led to a diversification of material requirements for substrates used to mount semiconductor elements, and in particular, the demand for resin compositions with low thermal expansion rates has not been met.
A resin composition is formed by combining a resin with a specified isopropylene group and a maleimide compound, and a high molecular weight structure is formed by utilizing the Diels-Alder reaction to reduce the thermal expansion coefficient.
It provides a cured material with low thermal expansion coefficient, which improves the heat resistance and low dielectric properties of printed circuit boards, meeting the diverse needs of substrates for semiconductor device mounting.
Smart Images

Figure CN123125250A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to resin compositions, cured products, prepregs, resin composite sheets, printed circuit boards, and semiconductor devices. Background Technology
[0002] In recent years, the integration and miniaturization of semiconductor components used in electronic devices and communication equipment, exemplified by portable terminals, have been accelerating. This has led to a demand for technologies capable of high-density mounting of semiconductor components, and consequently, improvements are needed in printed circuit boards (PCBs), such as substrates for mounting these semiconductor components, which occupy a crucial position in the process.
[0003] On the other hand, the applications of electronic devices and the like are diversifying and continuously expanding. As a result, the various characteristics required for printed circuit boards (PCBs) such as substrates for mounting semiconductor components, the metal foil laminates used in them, and prepregs are becoming more diverse and stringent. To improve PCBs while taking these required characteristics into account, various materials and processing methods have been proposed. One example is the improved development of resin materials constituting prepregs and resin composite sheets. Such materials are described in Patent Documents 1-4.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2022-058409
[0007] Patent Document 2: Japanese Patent Application Publication No. 2021-187893
[0008] Patent Document 3: International Publication No. 2019 / 188189
[0009] Patent Document 4: Japanese Patent Application Publication No. 2018-090728 Summary of the Invention
[0010] The problem the invention aims to solve
[0011] As mentioned above, the applications of electronic devices and the like are diversifying and expanding, requiring new materials for the resins that constitute prepregs and the like. In particular, further material development is needed for resin compositions that can provide cured products with low coefficients of thermal expansion.
[0012] The object of the present invention is to solve the above-mentioned problems, and to provide a resin composition capable of providing a cured product with a low coefficient of thermal expansion, as well as cured products, prepregs, metal foil laminates, resin composites, printed circuit boards, and semiconductor devices.
[0013] Solution for solving the problem
[0014] Based on the above-mentioned issues, the inventors conducted research and found that by combining a resin having a specified isopropylene group and a specified maleimide compound, a resin composition that can provide a cured product with a low coefficient of thermal expansion can be obtained.
[0015] Specifically, the above-mentioned problems were solved through the following solution.
[0016] [1] A resin composition comprising, relative to 10 to 90 parts by weight of resin (A), 90 to 10 parts by weight of maleimide compound (B) of formula (M4).
[0017] The resin (A) is the resin shown in formula (T).
[0018]
[0019] (In formula (T), Ma independently represents hydrocarbon groups with 1 to 12 carbon atoms arbitrarily substituted by halogen atoms, and x represents an integer from 0 to 4. R is a divalent group.)
[0020]
[0021] (In formula (M4), R) 56 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group, R. 57 Each can be used independently to represent a hydrogen atom or a methyl group.
[0022] [2] The resin composition according to [1], wherein R is a group comprising an indane structure.
[0023] [3] The resin composition according to [1] or [2], wherein R is a group comprising the following structure.
[0024]
[0025] (In formula (Tx), n, o, and p are the average number of repeating units. n represents a number greater than 0 and less than 20. o and p each independently represent a number from 0 to 20, satisfying 1.0 ≤ n + o + p ≤ 20.0. Ma each independently represents a hydrocarbon group with 1 to 12 carbon atoms arbitrarily substituted by halogen atoms. x represents an integer from 0 to 4. Structural units (a), (b), and (c) are bonded to structural units (a), (b), and (c) or other groups at the * position, and each structural unit is randomly bonded.)
[0026] [4] According to the resin composition of [3], wherein the parameter α of the resin (A) calculated by formula (α) is 0.20 or more and 1.00 or less, the parameter β calculated by formula (β) is 0.20 or more and 3.00 or less, and the number average molecular weight of the resin (A) is 400 to 3000.
[0027] [Mathematical Expression 1]
[0028]
[0029] (The parentheses in formula (α) indicate) 1 The integral value between the corresponding chemical shift values in H-NMR, the part in parentheses in equation (β) represents 1 (The integral value between the corresponding chemical shift values in H-NMR.)
[0030] [5] The resin composition according to any one of [1] to [4], wherein the compound represented by formula (M4) comprises the following compound.
[0031]
[0032] (In the formula, Me is methyl and Et is ethyl.)
[0033] [6] The resin composition according to any one of [1] to [5], wherein R is a group comprising the following structure,
[0034] The resin (A) has a parameter α calculated by formula (α) of 0.20 or more and 1.00 or less, and a parameter β calculated by formula (β) of 0.20 or more and 3.00 or less. The number-average molecular weight of the resin (A) is 400 to 3000.
[0035] The compound represented by formula (M4) includes the following compounds.
[0036]
[0037] (In formula (Tx), n, o, and p are the average number of repeating units. n represents a number greater than 0 and less than 20. o and p each independently represent a number from 0 to 20, satisfying 1.0 ≤ n + o + p ≤ 20.0. Ma each independently represents a hydrocarbon group with 1 to 12 carbon atoms arbitrarily substituted by halogen atoms. x represents an integer from 0 to 4. Structural units (a), (b), and (c) are bonded to structural units (a), (b), and (c) or other groups at the * position, and each structural unit is randomly bonded.)
[0038] [Mathematical Expression 2]
[0039]
[0040] (The parentheses in formula (α) indicate) 1 The integral value between the corresponding chemical shift values in H-NMR, the part in parentheses in equation (β) represents 1 (The integral value between the corresponding chemical shift values in H-NMR.)
[0041]
[0042] (In the formula, Me is methyl and Et is ethyl.)
[0043] [7] The resin composition according to any one of [1] to [6] further comprises a compound represented by formula (BV).
[0044]
[0045] (In formula (BV), Md independently represents hydrocarbon groups with 1 to 12 carbon atoms. w represents an integer from 0 to 4. r represents an integer from 0 to 6.)
[0046] [8] The resin composition according to any one of [1] to [7] further comprises a filler material.
[0047] [9] The resin composition according to any one of [1] to [8] further comprises at least one selected from the group consisting of ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, flow modifiers, lubricants, defoamers, leveling agents, gloss agents and polymerization inhibitors.
[0048]
[10] The resin composition according to any one of [1] to [9] is for use in printed circuit boards.
[0049] [X] The resin composition according to any one of the above claims, wherein when the resin composition is cured at 200°C, it has the following structure (X).
[0050]
[0051] (In formula (X), R) i R is a group derived from resin (A). m (These are groups derived from the compound represented by formula (M4).)
[0052]
[11] A cured product, which is a cured product of the resin composition described in any one of [1] to
[10] and [X].
[0053]
[12] A prepreg formed from a substrate and a resin composition of any one of [1] to
[10] and [X].
[0054]
[13] A metal foil laminate comprising at least one prepreg as described in
[12] and a metal foil disposed on one or both sides of the prepreg.
[0055]
[14] A resin composite sheet comprising a support and a layer formed of a resin composition as described in any one of [1] to
[10] and [X] disposed on the surface of the support.
[0056]
[15] A printed circuit board comprising an insulating layer and a conductor layer disposed on the surface of the insulating layer,
[0057] The insulating layer comprises a layer formed of a resin composition of any one of [1] to
[10] and [X].
[0058]
[16] A semiconductor device comprising the printed circuit board described in
[15] .
[0059] The effects of the invention
[0060] According to the present invention, resin compositions capable of providing cured products with low coefficients of thermal expansion, as well as cured products, prepregs, metal foil laminates, resin composites, printed circuit boards, and semiconductor devices can be provided. Attached Figure Description
[0061] Figure 1 The image shows the 1H-NMR spectrum of Synthetic Example 1.
[0062] Figure 2 This is a graph showing the peak values of parameters α and β in the 1H-NMR spectrum of the resin obtained in Synthesis Example 1. Detailed Implementation
[0063] Hereinafter, a method for implementing the present invention (hereinafter referred to as "this embodiment") will be described in detail. It should be noted that the following embodiment is an example for illustrating the present invention, and the present invention is not limited to this embodiment.
[0064] It should be noted that in this specification, "~" is used to encompass the values listed before and after it as the lower and upper limits.
[0065] Unless otherwise specified, all physical property values and characteristic values in this manual are set at 23°C.
[0066] In this specification, the description of groups (atomic groups) includes both unsubstituted and substituted groups (atomic groups). For example, "alkyl" includes not only unsubstituted alkyl groups (unsubstituted alkyl groups) but also substituted alkyl groups (substituted alkyl groups). In this specification, the description of unsubstituted and unsubstituted groups is preferably unsubstituted.
[0067] In this specification, relative permittivity refers to the ratio of the dielectric constant of a material to the dielectric constant of vacuum. Additionally, in this specification, relative permittivity is sometimes simply referred to as "dielectric constant". Furthermore, unless otherwise specified, the relative permittivity in this specification refers to the relative permittivity at a frequency of 10 GHz, measured using the cavity resonance perturbation method.
[0068] In this specification, "(meth)acrylic acid" means either or both of acrylic acid and methacrylic acid. "(meth)allyl" means either or both of allyl and methylallyl.
[0069] Unless otherwise specified, the standards shown in this manual are based on January 1, 2024, and the measurement methods may vary depending on the year.
[0070] In this specification, the resin solids component refers to the components other than fillers and solvents, and its main purpose is to include resin (A), maleimide compound (B) as shown in formula (M4), and other thermosetting compounds to be blended as needed, as well as other resin additive components (flame retardants and other additives).
[0071] The resin composition of this embodiment is characterized in that, relative to 10 to 90 parts by mass of resin (A), it comprises 90 to 10 parts by mass of maleimide compound (B) of formula (M4), wherein resin (A) is resin of formula (T).
[0072]
[0073] (In formula (T), Ma independently represents hydrocarbon groups with 1 to 12 carbon atoms arbitrarily substituted by halogen atoms, and x represents an integer from 0 to 4. R is a divalent group.)
[0074]
[0075] (In formula (M4), R) 56 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group, R. 57 Each can be used independently to represent a hydrogen atom or a methyl group.
[0076] By adopting the above configuration, a resin composition capable of providing a cured product with a low coefficient of thermal expansion can be obtained. The inventors conducted research and concluded that the reason for this is as follows: When resin (A) was attempted to cure at 200°C in the absence of a catalyst, a sufficiently cured product could not be obtained. Furthermore, when the maleimide compound (B) shown in formula (M4) was also attempted to cure at 200°C in the absence of a catalyst, a sufficiently cured product could not be obtained. However, when a mixture of resin (A) and the maleimide compound (B) shown in formula (M4) was attempted to cure at 200°C in the absence of a catalyst, a sufficiently cured product was obtained. Furthermore, even when a mixture of resin (A) and the maleimide compound (B) shown in formula (M4) was attempted to cure at 200°C in the presence of an inhibitor for free radical polymerization, a sufficiently cured product was obtained.
[0077] Generally, compounds with vinyl bonds undergo free radical polymerization with maleimide compounds via vinyl addition polymerization. However, based on the experimental results above, it is speculated that the curing of resin (A) with the maleimide compound (B) shown in formula (M4) occurs not only through free radical polymerization but also through other reactions.
[0078] As another possible reaction, it is speculated that the following reaction occurred.
[0079]
[0080] Includes R i0 The compound is resin (A), containing R m0 The compound is maleimide compound (B) as shown in formula (M4). It is presumed that resin (A) and maleimide compound (B) as shown in formula (M4) form a rigid structure through the Diels-Alder reaction as described above.
[0081] R in the above reaction system i R is a group derived from resin (A). m Derived from the group shown in formula (M4). R is obtained by carrying out the Diels-Alder reaction. i and R m Further increase in molecular weight.
[0082] Ma and x have the same meaning as Ma and x in equation (T).
[0083] Hereinafter, embodiments of the present invention will be described in detail, but the following description of the constituent elements is only one example of the embodiments of the present invention and is not limited to these contents.
[0084] <Resin (A)>
[0085] In this embodiment, resin (A) is the resin shown in formula (T).
[0086]
[0087] (In formula (T), Ma independently represents hydrocarbon groups with 1 to 12 carbon atoms arbitrarily substituted by halogen atoms, and x represents an integer from 0 to 4. R is a divalent group.)
[0088] In formula (T), Ma is preferably a hydrocarbon group with 1 to 10 carbon atoms that are optionally substituted with a halogen atom, more preferably a hydrocarbon group with 1 to 5 carbon atoms that are optionally substituted with a halogen atom, and even more preferably a hydrocarbon group with 1 to 3 carbon atoms that are optionally substituted with a halogen atom. Examples of halogen atoms include fluorine, chlorine, and bromine atoms, with fluorine or chlorine atoms being preferred. Ma is preferably a hydrocarbon group with 1 to 12 carbon atoms that are not substituted with a halogen atom. The aforementioned hydrocarbon group is preferably an alkyl group, more preferably a straight-chain alkyl group. Methyl or ethyl groups are particularly preferred for Ma.
[0089] x is preferably an integer from 0 to 3, more preferably an integer from 0 to 2, further preferably 0 or 1, and even more preferably 0.
[0090] In formula (T), R is a divalent group, preferably a group formed by -S-, -O-, C(=O)-NH2-, or a hydrocarbon group, and combinations of two or more of them (these groups may optionally have substituents), more preferably a hydrocarbon group, preferably a group containing an indane structure, and even more preferably a group containing the group shown in formula (Tx).
[0091]
[0092] (In formula (Tx), n, o, and p are the average number of repeating units. n represents a number greater than 0 and less than 20. o and p each independently represent a number from 0 to 20, satisfying 1.0 ≤ n + o + p ≤ 20.0. Ma each independently represents a hydrocarbon group with 1 to 12 carbon atoms arbitrarily substituted by halogen atoms. x represents an integer from 0 to 4. Structural units (a), (b), and (c) are bonded to structural units (a), (b), and (c) or other groups at the * position, and each structural unit is randomly bonded.)
[0093] In formula (Tx), n, o, and p refer to the average number of repeating units in all molecules of the resin.
[0094] In formula (Tx), the sum of n, o, and p is preferably 1.1 ≤ n + o + p, more preferably 1.2 ≤ n + o + p, even more preferably 1.5 ≤ n + o + p, even more preferably 2.0 ≤ n + o + p, even more preferably 2.5 ≤ n + o + p, even more preferably 3.0 ≤ n + o + p, and even more preferably 3.3 ≤ n + o + p. In formula (Tx), the sum of n, o, and p is also preferably n + o + p ≤ 20.0, more preferably n + o + p ≤ 10.0, even more preferably n + o + p ≤ 8.0, even more preferably n + o + p ≤ 7.0, even more preferably n + o + p ≤ 6.4, and can also be n + o + p ≤ 4.0. The sum of n, o, and p can be calculated using the method described in the embodiments described later.
[0095] In formula (Tx), n is preferably 0.2 or more, more preferably 0.6 or more, even more preferably 1.0 or more, even more preferably 1.2 or more, even more preferably 1.6 or more, and may also be 2.2 or more, 2.4 or more. In addition, it is preferably 18.0 or less, more preferably 12.0 or less, even more preferably 9.0 or less, even more preferably 7.0 or less, even more preferably 6.0 or less, and may also be 5.0 or less, 4.0 or less, 3.0 or less.
[0096] In formula (Tx), o is preferably 0 or more, more preferably 0.01 or more, even more preferably 0.03 or more, even more preferably 0.05 or more, even more preferably 0.07 or more, and preferably 10.0 or less, more preferably 5.0 or less, even more preferably 4.0 or less, even more preferably 2.0 or less, even more preferably 1.0 or less, and may also be 0.8 or less, 0.5 or less, 0.3 or less, 0.2 or less, or 0.1 or less.
[0097] In formula (Tx), p is preferably 0 or more, more preferably 0.01 or more, even more preferably 0.1 or more, even more preferably 0.2 or more, even more preferably 0.3 or more, and preferably 18.0 or less, more preferably 10.0 or less, even more preferably 5.0 or less, even more preferably 4.0 or less, even more preferably 3.0 or less, and may also be 2.5 or less, 2.0 or less, 1.0 or less, or 0.5 or less.
[0098] Furthermore, in equation (Tx), n / (n+o+p) is, for example, 0.2 or more, 0.25 or more, 0.3 or more, 0.34 or more, 0.4 or more, 0.45 or more, 0.5 or more, 0.55 or more, 0.6 or more, or 0.7 or more, and is 1.0 or less. Among the structural units (a) to (c) included in equation (Tx), structural unit (a) with the lowest activation energy and the largest change in free energy is preferentially generated.
[0099] When the R part in formula (T) is set to 100 parts by mass, the proportion of the structural unit (i.e., any one of the structural units (a), (b), and (c)) shown in formula (Tx) is preferably 80 parts by mass, more preferably 90 parts by mass or more, even more preferably 95 parts by mass or more, even more preferably 97 parts by mass or more, even more preferably 99 parts by mass or more, and other than 100 parts by mass or less.
[0100] In equation (Tx), Ma and x have the same meaning as Ma and x in equation (T), and the preferred range is also the same.
[0101] The resin shown in formula (T) is further preferably such that the parameter α calculated from formula (α) is 0.20 or more and 1.00 or less, and the parameter β calculated from formula (β) is 0.20 or more and 3.00 or less. By setting the parameters α and β to the above ranges, the resulting cured product tends to have low dielectric properties (Dk and / or Df) and excellent heat resistance.
[0102] [Mathematical Expression 3]
[0103]
[0104] (The parentheses in formula (α) indicate) 1 The integral value between the corresponding chemical shift values in H-NMR, the part in parentheses in equation (β) represents 1 (The integral value between the corresponding chemical shift values in H-NMR.)
[0105] Here, α represents the ratio of structural units with an indane framework (structural unit (a) in formula (Tx)) in the resin shown in formula (T). More specifically, it is speculated that by adjusting the structural units with an indane framework to satisfy the range of the aforementioned parameter α, the resulting resin molecules have high rigidity, which can increase the glass transition temperature. Furthermore, it is speculated that since molecules with high rigidity have lower mobility compared to molecules with low rigidity, the dielectric relaxation time is longer, and Df can be reduced. When synthesizing the resin shown in formula (T), α can be increased by reducing the concentration of raw materials, using highly polar solvents, increasing the amount of catalyst, and increasing the reaction temperature.
[0106] On the other hand, β represents the ratio of terminal double bonds in the resin specified by formula (T). More specifically, it is speculated that the increased number of crosslinking points with the functional groups of the maleimide compound (B) facilitates network formation during thermosetting, resulting in cured products with high glass transition temperature, low thermal expansion coefficient, and low Df. β can be increased by reducing the amount of catalyst, lowering the reaction temperature, and using low-polarity solvents during the synthesis of the resin specified by formula (T).
[0107] More specifically, regarding the resin of Synthetic Example 1 described later, the above-mentioned 2.55ppm to 2.31ppm corresponds to the peak originating from structural unit (a), the above-mentioned 6.24ppm to 5.91ppm corresponds to the peak originating from structural unit (b), the above-mentioned 2.98ppm to 2.55ppm corresponds to the peak originating from structural unit (c), the above-mentioned 5.49ppm to 4.89ppm corresponds to the peak originating from isopropylene group and structural unit (c), the above-mentioned 4.89ppm to 4.45ppm corresponds to the peak originating from structural unit (c), and the above-mentioned 2.31ppm to 1.96ppm corresponds to the peak originating from isopropylene group and structural unit (a).
[0108] More specifically, the H used in the calculation of parameters α and β is recorded in the following structural formula.
[0109]
[0110]
[0111] The above calculations of parameters α and β are used 1 The H-NMR peaks can be assigned according to the H values recorded above as follows.
[0112] • 2.55ppm~2.31ppm: H a1
[0113] • 6.24ppm~5.91ppm: H b1
[0114] • 2.98ppm~2.55ppm: H c1
[0115] • 5.49ppm~4.89ppm: H i2 H i3 and H c2
[0116] • 4.89ppm~4.45ppm: H c3
[0117] • 2.31ppm~1.96ppm: H a2 and H i1
[0118] Based on the above, the formulas for parameters α and β are expressed using the amounts of each hydrogen atom shown below.
[0119] That is, H a1 The more elements there are, that is, the more 5-membered rings there are in the structural unit (a), the larger the parameter α will be.
[0120] Additionally, parameter β is represented by the H in the isopropenyl group. i1The quantity is the denominator, H i2 and H i3 The total amount is expressed as 1.5 times the numerator, in formula form. That is, ideally (H i2 and H i3 (1.5 times the total amount) ÷ (H) i1 The total amount is 1.
[0121] in addition, Figure 2 The term "indicates" refers to the resin obtained in the synthetic example 1 described later. 1 Peak values of parameters α and β in the H-NMR image.
[0122] When synthesizing the resin shown in formula (T), the parameters α and β of the resin shown in formula (T) can be adjusted by increasing the parameters α and β described above. Of course, parameters α and β can also be adjusted by methods other than those described above.
[0123] The parameter α is preferably 0.20 or higher, more preferably 0.25 or higher, even more preferably 0.34 or higher, even more preferably 0.45 or higher, even more preferably 0.50 or higher, even more preferably 0.55 or higher, even more preferably 0.57 or higher, and even more preferably 0.59 or higher, 0.60 or higher, or 0.62 or higher. Depending on the application, it can be 0.65 or higher, 0.70 or higher, 0.75 or higher, or 0.80 or higher. By setting the parameter α to the above-mentioned lower limit value or higher, there is a tendency to further improve the heat resistance of the obtained cured product. Regarding the parameter α, since there is a tendency for the obtained cured product to have low dielectric properties (Dk and / or Df) and excellent heat resistance, the larger the parameter α is, the better. However, depending on the application, it can be 1.00 or lower, 0.95 or lower, 0.90 or lower, 0.85 or lower, 0.82 or lower, 0.80 or lower, 0.77 or lower, 0.75 or lower, 0.74 or lower, 0.70 or lower, or 0.65 or lower.
[0124] The parameter β is preferably 0.20 or higher, more preferably 0.25 or higher, even more preferably 0.30 or higher, even more preferably 0.35 or higher, even more preferably 0.40 or higher, even more preferably 0.43 or higher, even more preferably 0.50 or higher, and may also be 0.60 or higher, 0.65 or higher, 0.70 or higher, 0.77 or higher, 0.80 or higher, 0.90 or higher, or 0.95 or higher. By setting the parameter β to the aforementioned lower limit value or higher, there is a tendency for the heat resistance of the obtained cured product to be improved and the Df value to be lower. The parameter β is preferably 3.00 or lower, more preferably 2.50 or lower, even more preferably 2.00 or lower, even more preferably 1.50 or lower, even more preferably 1.30 or lower, even more preferably 1.20 or lower, even more preferably 1.10 or lower, and may further be 1.00 or lower, 0.95 or lower, 0.90 or lower, 0.85 or lower, 0.83 or lower, or 0.80 or lower. By setting the parameter β below the aforementioned upper limit, there is a tendency to improve the heat resistance of the resulting cured material and reduce Df.
[0125] As an example of raw materials for synthesizing the resin shown in formula (T), m-bis(α-hydroxyisopropyl)benzene, p-bis(α-hydroxyisopropyl)benzene, 1,3-diisopropenylbenzene and 1,4-diisopropenylbenzene, etc., can be used.
[0126] As an example of raw materials for synthesizing the resin shown in formula (T), when m-bis(α-hydroxyisopropyl)benzene and p-bis(α-hydroxyisopropyl)benzene are used, 1,3-diisopropenylbenzene and 1,4-diisopropenylbenzene can be generated in the reaction system through a dehydration reaction. Alternatively, the resin shown in formula (T) can be synthesized directly without separating 1,3-diisopropenylbenzene and 1,4-diisopropenylbenzene. The generated 1,3-diisopropenylbenzene and 1,4-diisopropenylbenzene can also be purified by distillation or the like before use.
[0127] The pressure used when synthesizing the resin shown in formula (T) is preferably atmospheric pressure, but it can also be carried out under reduced or increased pressure.
[0128] Examples of steps involving the removal of solid catalysts from resins of the synthetic formula (T) include filtration and decantation. These steps may be performed individually or in combination, depending on the objective.
[0129] Examples of such equipment include centrifuges, pressure filters, pressure filters, and atmospheric pressure filters. In order to dry the filtered material, there may also be equipment for heating and depressurization.
[0130] Filter aids can also be used in filtration. Examples of filter aids include diatomaceous earth, cellulose, and perlite. These can be used alone or in combination.
[0131] When synthesizing 1,3-diisopropenylbenzene and 1,4-diisopropenylbenzene, which are raw materials for the resin shown in formula (T), it is preferable to introduce an inactive gas such as nitrogen or to introduce an inactive gas such as nitrogen into the liquid in order to carry out the dehydration reaction efficiently.
[0132] The catalyst used in the synthesis of the resin shown in formula (T) can be added in one go or in batches.
[0133] When synthesizing the resin shown in formula (T), the heating rate is preferably 0.2°C / min or more, more preferably 0.4°C / min or more, even more preferably 0.7°C / min or more, and may also be 1.0°C / min or more, 1.5°C / min or more, 2.0°C / min or more, or 2.5°C / min or more. Furthermore, the heating rate is preferably 5°C / min or less, and more preferably 4°C / min or less.
[0134] The material used as the filter material when synthesizing the resin shown in formula (T) is preferably a material that is resistant to aromatic solvents such as toluene.
[0135] Examples of stirring devices used in the synthesis process of the resin shown in formula (T) include mechanical stirring devices, magnetic stirring devices, and ultrasonic stirring devices.
[0136] As a means of temperature control used in the synthesis process of the resin shown in formula (T), a jacketed reaction vessel, a heating or cooling circulation device, an infrared heating device, a microwave heating device, or a combination thereof can be used.
[0137] The number-average molecular weight (Mn) of resin (A) converted from polystyrene using GPC (gel permeation chromatography) (details as described in the examples below) is preferably 400 or more, more preferably 500 or more, further preferably 550 or more, even more preferably 600 or more, and even more preferably 650 or more. By setting the number-average molecular weight to the aforementioned lower limit or above, there is a tendency for the heat resistance of the obtained cured product to be improved and the dielectric constant (Df) to be lower. In addition, the upper limit of the number-average molecular weight (Mn) of resin (A) converted from polystyrene using GPC (gel permeation chromatography) is preferably 3000 or less, more preferably 2500 or less, further preferably 2000 or less, even more preferably 1500 or less, even more preferably 1250 or less, and depending on the application, it can be 1000 or less, or 800 or less. By setting the number-average molecular weight to the aforementioned upper limit or below, there is a tendency for the heat resistance of the obtained cured product to be improved and the relative dielectric constant (Dk) and dielectric loss tangent (Df) to be lower.
[0138] Furthermore, the weight-average molecular weight (Mw) of resin (A) based on GPC-converted polystyrene (details according to the method described in the examples below) is preferably 500 or more, more preferably 800 or more, further preferably 900 or more, and even more preferably 1000 or more. By setting the weight-average molecular weight to the aforementioned lower limit or above, there is a tendency for the heat resistance of the obtained cured product to increase and Df to decrease. The upper limit of the weight-average molecular weight (Mw) of resin (A) based on GPC-converted polystyrene (details according to the method described in the examples below) is preferably 6000 or less, more preferably 5000 or less, further preferably 4000 or less, even more preferably 3000 or less, and even more preferably 2800 or less. Depending on the application, it can be 2500 or less, 2000 or less, or 1500 or less. By setting the weight-average molecular weight to the aforementioned upper limit or below, there is a tendency for the heat resistance of the obtained cured product to increase and the relative permittivity (Dk) and dielectric loss tangent (Df) to decrease.
[0139] The weight-average molecular weight to number-average molecular weight ratio (Mw / Mn) of resin (A) is preferably 1.1 to 3.0. More preferably, the Mw / Mn ratio of resin (A) is 1.2 or higher, even more preferably 1.3 or higher, even more preferably 1.4 or higher, even more preferably 1.5 or higher, and even more preferably 1.6 or higher. Furthermore, the Mw / Mn ratio of resin (A) is more preferably 2.5 or lower, even more preferably 2.4 or lower, and can be 2.3 or lower, 2.0 or lower, or 1.8 or lower.
[0140] The weight-average molecular weight and number-average molecular weight were determined according to the methods described in the examples below.
[0141] In this embodiment, the functional group equivalent (isopropenyl equivalent) of resin (A) is preferably 100 g / eq. or more, more preferably 150 g / eq. or more, even more preferably 200 g / eq. or more, even more preferably 250 g / eq. or more, even more preferably 275 g / eq. or more, even more preferably 300 g / eq. or more, and preferably 7500 eq. or less, more preferably 5000 eq. or less, even more preferably 4000 eq. or less, even more preferably 3000 g / eq. or less, even more preferably 2000 g / eq. or less, even more preferably 1500 g / eq. or less, even more preferably 1000 g / eq. or less, and can further be 800 g / eq. or less, 750 g / eq. or less, 700 g / eq. or less, or 500 g / eq. or less. By setting the functional group equivalent of resin (A) to or above the aforementioned lower limit, the resulting cured product tends to have superior low dielectric properties (Dk and / or Df, especially Df) and superior peel strength. Furthermore, by setting the functional group equivalent of resin (A) to or below the aforementioned upper limit, the resulting cured product tends to have superior low dielectric properties (Dk and / or Df, especially Df), superior heat resistance (especially glass transition temperature), and a further decrease in coefficient of thermal expansion. The functional group equivalent (isopropylene equivalent) of resin (A) is determined according to the method described in the examples described later.
[0142] Relative to 100 parts by weight of the resin solids in the resin composition, the content of resin (A) in the resin composition of this embodiment is preferably 10 parts by weight or more, more preferably 15 parts by weight or more, and even more preferably 20 parts by weight or more. Depending on the application, it can be 25 parts by weight or more, 30 parts by weight or more, or 35 parts by weight or more. By setting the content of resin (A) to the aforementioned lower limit or above, there is a tendency to reduce the Df of the obtained cured product. In addition, the upper limit of the content of resin (A) relative to 100 parts by weight of the resin solids in the resin composition is preferably 90 parts by weight or less, more preferably 85 parts by weight or less, and even more preferably 80 parts by weight or less. Depending on the application, it can be 75 parts by weight or less, 70 parts by weight or less, 65 parts by weight or less, 60 parts by weight or less, 55 parts by weight or less, or 50 parts by weight or less. By setting the content of resin (A) to the aforementioned upper limit or below, there is a tendency to improve the formability of the resin composition and the heat resistance of the obtained cured product.
[0143] The resin composition of this embodiment may contain only one type of resin (A), or it may contain two or more types. When two or more types are contained, the total amount is preferably within the range described above.
[0144] The method for manufacturing resin (A) in this embodiment is not particularly limited, and resins obtained by known manufacturing methods can be used. Furthermore, the raw materials, reaction temperature, type of catalyst, amount of catalyst, reaction solvent, and concentration of raw materials used in the synthesis of resin (A) are not particularly limited, and can be appropriately selected or controlled according to the desired physical properties described above.
[0145] <The maleimide compound (B) represented by formula (M4)>
[0146] The resin composition of this embodiment comprises maleimide compound (B) as shown in formula (M4).
[0147]
[0148] (In formula (M4), R) 56 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group, R. 57 Each can be used independently to represent a hydrogen atom or a methyl group.
[0149] In one example of maleimide compound (B) represented by formula (M4), R 56 Each is independently methyl or ethyl, R 57 It is methyl. The above R 56 More preferably, the two benzene rings are methyl and ethyl, respectively.
[0150] Another example of maleimide compound (B) represented by formula (M4) is R. 56 and R 57 It is a hydrogen atom.
[0151] In this embodiment, the maleimide compound (B) represented by formula (M4) preferably contains the following compound.
[0152]
[0153] In the above formula, Me represents methyl and Et represents ethyl.
[0154] The maleimide compound shown in formula (M4) can be a commercially available product, such as "BMI-70" manufactured by K·I Chemical Industry Co.,LTD. or "BMI-5100" manufactured by Yamato Chemical Industry Co., Ltd.
[0155] Relative to 100 parts by mass of the resin solids in the resin composition, the content of the maleimide compound (B) shown in formula (M4) in the resin composition of this embodiment is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and may also be 20 parts by mass or more. Depending on the application, it may be 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, 45 parts by mass or more, or 50 parts by mass or more. By setting the content of the maleimide compound (B) shown in formula (M4) to the above-mentioned lower limit value or above, there is a tendency to improve the heat resistance of the obtained cured product and reduce Df. In addition, the upper limit value of the content of the maleimide compound (B) shown in formula (M4) relative to 100 parts by mass of the resin solids in the resin composition is preferably 90 parts by mass or less, more preferably 85 parts by mass or less, and even more preferably 80 parts by mass or less. Depending on the application, it may be 70 parts by mass or less or 65 parts by mass or less. By setting the content of the maleimide compound (B) shown in formula (M4) below the above-mentioned upper limit, there is a tendency to improve the formability of the resin composition and to make the thermal expansion coefficient of the resulting cured product lower.
[0156] The resin composition of this embodiment may contain only one maleimide compound (B) of formula (M4), or it may contain two or more. When two or more are contained, the total amount is preferably within the range described above.
[0157] Furthermore, in the resin composition of this embodiment, 10 to 90 parts by weight of resin (A) contain 90 to 10 parts by weight of maleimide compound (B) of formula (M4); preferably 10 to 80 parts by weight of resin (A) contain 90 to 20 parts by weight of maleimide compound (B) of formula (M4); more preferably 20 to 70 parts by weight of resin (A) contain 80 to 30 parts by weight of maleimide compound (B) of formula (M4); and even more preferably 30 to 65 parts by weight of resin (A) contain 70 to 35 parts by weight of maleimide compound (B) of formula (M4).
[0158] In another example of the resin composition of this embodiment, the total amount of resin (A) and maleimide compound (B) shown in (M4) is 90 parts by mass or more, preferably 95 parts by mass or more, more preferably 97 parts by mass or more, and may also be 98 parts by mass or more, relative to 100 parts by mass of the resin solid component contained in the resin composition.
[0159] <Other thermosetting compounds>
[0160] The resin composition of this embodiment may contain other thermosetting compounds besides resin (A) and the maleimide compound shown in formula (M4). Other thermosetting compounds are typically thermosetting resins.
[0161] The types of other thermosetting compounds are not specifically specified, but preferably include at least one of the following groups: other maleimide compounds selected from those other than the maleimide compound shown in formula (M4) (hereinafter referred to as "other maleimide compounds"), aromatic resins having a carbon-carbon double bond at the end, cyanate ester compounds, (meth)allyl compounds, (meth)acrylate compounds, epoxy compounds, phenolic compounds, oxetane resins, benzoxazine compounds, arylcyclobutene compounds, perfluorovinyl ether resins, polyimide compounds, and compounds having vinylidene groups; more preferably, it includes at least one of the following groups: other maleimide compounds, aromatic resins having a carbon-carbon double bond at the end, and aromatic resins having a carbon-carbon double bond at the end. The compound comprises at least one of the following groups: aromatic resins, cyanate compounds, (meth)acrylate compounds, epoxy compounds, phenolic compounds, oxetane resins, benzoxazine compounds, arylcyclobutene compounds, perfluorovinyl ether resins, polyimide compounds, and compounds having vinylidene groups. More preferably, it comprises at least one of the following groups: aromatic resins having carbon-carbon double bonds at the ends, and cyanate compounds. More preferably, it comprises at least one of the following groups: aromatic resins having carbon-carbon double bonds at the ends. Even more preferably, it comprises aromatic resins having carbon-carbon double bonds at the ends.
[0162] The content of other thermosetting compounds in the resin composition of this embodiment is preferably 1 part by mass or more, more preferably 10 parts by mass or more, further preferably 30 parts by mass or more, even more preferably 50 parts by mass or more, even more preferably 55 parts by mass or more, and may also be 60 parts by mass or more, 65 parts by mass or more, and preferably 99 parts by mass or less, more preferably 95 parts by mass or less, even more preferably 90 parts by mass or less, and even more preferably 85 parts by mass or less, and may also be less than 80 parts by mass. By setting the content of other thermosetting compounds to the aforementioned lower limit or above, there is a tendency to further improve heat resistance. In addition, by setting the content of other thermosetting compounds to the aforementioned upper limit or below, there is a tendency to further improve low thermal expansion.
[0163] The resin composition in this embodiment may contain only one other thermosetting compound, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0164] <<Other Maleimide Compounds>>
[0165] The resin composition of this embodiment preferably contains other maleimide compounds.
[0166] In this embodiment, other maleimide compounds are preferably compounds having one or more maleimide groups in one molecule (preferably two or more, more preferably two to twelve, further preferably two to six, even more preferably two to four, even more preferably two or three, and even more preferably two maleimide groups).
[0167] In this embodiment, the other maleimide compounds preferably include one or more selected from the group consisting of the compound shown in formula (M0), the compound shown in formula (M1), the compound shown in formula (M2), the compound shown in formula (M3), the compound shown in formula (M5), other maleimide compounds (M6), other maleimide compounds (M7), and other maleimide compounds (M8). More preferably, they include one or more selected from the group consisting of the compound shown in formula (M0), the compound shown in formula (M1), the compound shown in formula (M2), the compound shown in formula (M3), and the compound shown in formula (M5). Even more preferably, they include one or more selected from the group consisting of the compound shown in formula (M1), the compound shown in formula (M2), and the compound shown in formula (M5). Even more preferably, they include the compound shown in formula (M1) and / or the compound shown in formula (M2). When these other maleimide compounds are used in materials for printed circuit boards (e.g., metal foil laminates), excellent heat resistance can be imparted.
[0168]
[0169] (In formula (M0), R) 51 Each independently represents a hydrogen atom, an alkyl group or a phenyl group having 1 to 8 carbon atoms, R 52 Each can be used independently to represent a hydrogen atom or a methyl group, where n1 represents an integer greater than or equal to 1.
[0170] R 51 Each of the following is preferably selected independently from the group consisting of hydrogen atom, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl and phenyl, more preferably hydrogen atom and / or methyl, and even more preferably hydrogen atom.
[0171] R 52 Methyl is preferred.
[0172] n1 is preferably an integer from 1 to 10, more preferably an integer from 1 to 5, even more preferably an integer from 1 to 3, even more preferably 1 or 2, and even more preferably 1.
[0173] Specifically, the following compounds can be cited as preferred examples of formula (M0).
[0174]
[0175] In the above formula, R 8 Each of the hydrogen atom, methyl group, or ethyl group can be represented independently, with methyl group being preferred.
[0176] The compound represented by formula (M0) can be a single compound or a mixture of two or more compounds. Examples of mixtures include mixtures of compounds with different n1 values, and R... 51 and / or R 52 This includes mixtures of compounds with different types of substituents, mixtures of compounds with different bonding positions (meta, para, or ortho) of the maleimide group and oxygen atom relative to the benzene ring, and mixtures of compounds combining two or more of the above-mentioned different positions. The same applies to the compounds shown in formulas (M1) to (M8) below.
[0177]
[0178] (In formula (M1), R) M1 R M2 R M3 and R M4 Each can be used independently to represent a hydrogen atom or an organic group. R M5 and R M6 Each can be used independently to represent a hydrogen atom or an alkyl group. Ar M This indicates a divalent aromatic group. A is an alicyclic group with a 4- to 6-membered ring. R M7 and R M8 Each is an alkyl group, independently. mx is 1 or 2, lx is 0 or 1. R M9 and R M10 Each can be used independently to represent a hydrogen atom or an alkyl group. R M11 R M12 R M13 and R M14 Each can be used independently to represent a hydrogen atom or an organic group. R M15 Each of these groups independently represents an alkyl group (1-10 carbon atoms), an alkoxy group (1-10 carbon atoms), an alkylthio group (1-10 carbon atoms), a cycloalkyl group (3-10 carbon atoms), an aryl group (6-10 carbon atoms), an aryloxy group (6-10 carbon atoms), an arylthio group (6-10 carbon atoms), a halogen atom, a hydroxyl group, or a mercapto group. px represents an integer from 0 to 3. nx represents an integer from 1 to 20.
[0179] R in the formula M1 R M2 R M3 and R M4 Each can be represented independently as a hydrogen atom or an organic group. The organic group here is preferably an alkyl group, more preferably an alkyl group with 1 to 12 carbon atoms, even more preferably an alkyl group with 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred. RM1 and R M3 Each is preferably an alkyl group, R. M2 and R M4 Hydrogen atoms are preferred.
[0180] R M5 and R M6 Each of the hydrogen atoms or alkyl groups is represented independently, preferably an alkyl group. The alkyl group here is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred.
[0181] Ar M The aromatic group representing the divalent group is preferably phenylene, naphthyl, phenanthrene, or anthracene, more preferably phenylene, and even more preferably m-phenylene. Ar M It may have substituents, with alkyl groups being preferred, more preferably alkyl groups having 1 to 12 carbon atoms, further preferably alkyl groups having 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred. However, Ar M Preferably unsubstituted.
[0182] A is a 4- to 6-membered alicyclic group, more preferably a 5-membered alicyclic group (preferably a group that forms an inden ring together with the benzene ring). R M7 and R M8 Each of the components is an alkyl group, preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and particularly preferably a methyl group.
[0183] mx is 1 or 2, preferably 2.
[0184] lx is 0 or 1, preferably 1.
[0185] R M9 and R M10 Each of the above can be used to represent a hydrogen atom or an alkyl group, more preferably an alkyl group. The alkyl group here is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred.
[0186] R M11 R M12 R M13 and R M14 Each can be represented independently as a hydrogen atom or an organic group. The organic group here is preferably an alkyl group, more preferably an alkyl group with 1 to 12 carbon atoms, even more preferably an alkyl group with 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred. R M12 and R M13 Each is preferably an alkyl group, R. M11 and RM14 Hydrogen atoms are preferred.
[0187] R M15 Each of the following can be independently represented: alkyl group with 1 to 10 carbon atoms, alkoxy group with 1 to 10 carbon atoms, alkylthio group with 1 to 10 carbon atoms, cycloalkyl group with 3 to 10 carbon atoms, aryl group with 6 to 10 carbon atoms, aryloxy group with 6 to 10 carbon atoms, arylthio group with 6 to 10 carbon atoms, halogen atom, hydroxyl group or mercapto group, preferably alkyl group with 1 to 4 carbon atoms, cycloalkyl group with 3 to 6 carbon atoms or aryl group with 6 to 10 carbon atoms.
[0188] px represents an integer from 0 to 3, preferably an integer from 0 to 2, more preferably 0 or 1, and even more preferably 0.
[0189] nx represents an integer from 1 to 20. nx can also be an integer less than 10.
[0190] It should be noted that the resin composition of this embodiment may contain only one compound represented by formula (M1) and at least two compounds with different nx values, or it may contain two or more compounds. When two or more compounds are contained, in order to produce a low melting point (low softening point), low melt viscosity, and excellent workability, the average value (average number of repeating units) n of nx in the compound represented by formula (M1) in the resin composition is preferably 0.92 or more, more preferably 0.95 or more, further preferably 1.0 or more, and even more preferably 1.1 or more. In addition, n is preferably 10.0 or less, more preferably 8.0 or less, further preferably 7.0 or less, even more preferably 6.0 or less, and may also be 5.0 or less. The same applies to formulas (M1-1) and the like described later.
[0191] The compound represented by formula (M1) is preferably the compound represented by the following formula (M1-1).
[0192]
[0193] (In formula (M1-1), R) M21 R M22 R M23 and R M24 Each can be used independently to represent a hydrogen atom or an organic group. R M25 and R M26 Each can be used independently to represent a hydrogen atom or an alkyl group. R M27 R M28 R M29 and R M30 Each can be used independently to represent a hydrogen atom or an organic group. R M31 and R M32 Each can be used independently to represent a hydrogen atom or an alkyl group. R M33 R M34 RM35 and R M36 Each can be used independently to represent a hydrogen atom or an organic group. R M37 R M38 and R M39 Each can be used independently to represent a hydrogen atom or an alkyl group. nx represents an integer greater than 1 and less than 20.
[0194] R in the formula M21 R M22 R M23 and R M24 Each can be represented independently as a hydrogen atom or an organic group. The organic group here is preferably an alkyl group, more preferably an alkyl group with 1 to 12 carbon atoms, even more preferably an alkyl group with 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred. R M21 and R M23 Preferably alkyl, R M22 and R M24 Hydrogen atoms are preferred.
[0195] R M25 and R M26 Each of the hydrogen atoms or alkyl groups is represented independently, preferably an alkyl group. The alkyl group here is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred.
[0196] R M27 R M28 R M29 and R M30 Each can be represented independently as a hydrogen atom or an organic group, preferably a hydrogen atom. The organic group here is preferably an alkyl group, more preferably an alkyl group with 1 to 12 carbon atoms, even more preferably an alkyl group with 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred.
[0197] R M31 and R M32 Each of the hydrogen atoms or alkyl groups is represented independently, preferably an alkyl group. The alkyl group here is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred.
[0198] R M33 R M34 R M35 and R M36 Each of these can be used to independently represent a hydrogen atom or an organic group. The organic group here is preferably an alkyl group, more preferably an alkyl group with 1 to 12 carbon atoms, even more preferably an alkyl group with 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred.
[0199] R M33 and R M36 Preferably, hydrogen atoms, R M34 and R M35 Alkyl groups are preferred.
[0200] R M37 R M38 R M39 Each of the hydrogen atoms or alkyl groups is represented independently, preferably an alkyl group. The alkyl group here is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably methyl, ethyl, propyl, or butyl, with methyl being particularly preferred.
[0201] nx represents an integer greater than 1 and less than 20. nx can also be an integer less than 10.
[0202] The compound represented by formula (M1-1) is preferably the compound represented by formula (M1-2) below.
[0203]
[0204] (In formula (M1-2), R) M21 R M22 R M23 and R M24 Each can be used independently to represent a hydrogen atom or an organic group. R M25 and R M26 Each can be used independently to represent a hydrogen atom or an alkyl group. R M27 R M28 R M29 and R M30 Each can be used independently to represent a hydrogen atom or an organic group. R M31 and R M32 Each can be used independently to represent a hydrogen atom or an alkyl group. R M33 R M34 R M35 and R M36 Each can be used independently to represent a hydrogen atom or an organic group. R M37 R M38 and R M39 Each can be used independently to represent a hydrogen atom or an alkyl group. nx represents an integer greater than 1 and less than 20.
[0205] In formula (M1-2), R M21 R M22 R M23 R M24 R M25 R M26 R M27 R M28 R M29 RM30 R M31 R M32 R M33 R M34 R M35 R M36 R M37 R M38 R M39 and nx are respectively related to R in equation (M1-1) M21 R M22 R M23 R M24 R M25 R M26 R M27 R M28 R M29 R M30 R M31 R M32 R M33 R M34 R M35 R M36 R M37 R M38 R M39 It has the same meaning as nx, and the preferred range is also the same.
[0206] The compound represented by formula (M1-1) is preferably the compound represented by formula (M1-3) below, and more preferably the compound represented by formula (M1-4) below.
[0207]
[0208] (In formula (M1-3), nx represents an integer greater than 1 and less than 20.)
[0209] nx can be an integer less than 10.
[0210]
[0211] (In formula (M1-4), nx represents an integer greater than 1 and less than 20.)
[0212] nx can be an integer less than 10.
[0213] The molecular weight of the compound represented by formula (M1) is preferably 500 or more, more preferably 600 or more, and even more preferably 700 or more. By setting it to the aforementioned lower limit or above, the resulting cured product tends to have improved low dielectric properties (Dk and / or Df) and low water absorption. Furthermore, the molecular weight of the compound represented by formula (M1) is preferably 10,000 or less, more preferably 9,000 or less, even more preferably 7,000 or less, even more preferably 5,000 or less, and even more preferably 4,000 or less. By setting it to the aforementioned upper limit or below, the resulting cured product tends to have improved heat resistance and workability.
[0214] Furthermore, details of the compound represented by formula (M1) can be found in International Publication No. 2020-217679, which is incorporated herein by reference.
[0215]
[0216] (In formula (M2), R) 54 Each can be used independently to represent a hydrogen atom or a methyl group, and n4 represents an integer greater than or equal to 1.
[0217] n4 is preferably an integer from 1 to 10, more preferably an integer from 1 to 5, even more preferably an integer from 1 to 3, and even more preferably 1 or 2, or it can be 1.
[0218] The compound represented by formula (M2) can be a mixture of n4 different compounds, preferably a mixture. Additionally, as described in part of the compound represented by formula (M0), it can also be a mixture of other compounds with different components.
[0219]
[0220] (In formula (M3), R) 55 Each of the following can be independently represented: an alkyl group with 1 to 8 carbon atoms, or a phenyl group; n5 represents an integer greater than 1 and less than 10.
[0221] R 55 Each of the following is preferably selected independently from the group consisting of hydrogen atom, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl and phenyl, more preferably hydrogen atom and / or methyl, and even more preferably hydrogen atom.
[0222] n5 is preferably an integer greater than or equal to 1 and less than or equal to 5, more preferably an integer from 1 to 3, and even more preferably 1 or 2.
[0223] The compound represented by formula (M3) can be a mixture of n5 different compounds, preferably a mixture. Additionally, as described in part of the compound represented by formula (M0), it can also be a mixture of other compounds with different components.
[0224]
[0225] (In formula (M5), R) 58 Each independently represents a hydrogen atom, an alkyl group or a phenyl group having 1 to 8 carbon atoms, R 59 Each can be used independently to represent a hydrogen atom or a methyl group, and n6 represents an integer greater than or equal to 1.
[0226] R 58 Each of the following is preferably selected independently from the group consisting of hydrogen atom, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl and phenyl, more preferably hydrogen atom and / or methyl, and even more preferably hydrogen atom.
[0227] R 59 Methyl is preferred.
[0228] n6 is preferably an integer from 1 to 10, more preferably an integer from 1 to 5, even more preferably an integer from 1 to 3, and even more preferably 1 or 2, or it can be 1.
[0229] The compound represented by formula (M5) can be a mixture of n6 different compounds, preferably a mixture. Additionally, as described in part of the compound represented by formula (M0), it can also be a mixture of other compounds with different components.
[0230] Other maleimide compounds (M6) are compounds having the structure shown in formula (M6) and maleimide groups at both ends of the molecular chain.
[0231]
[0232] (In formula (M6), R) 61 R represents a straight-chain or branched alkylene group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. 62 R represents a straight-chain or branched alkylene group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. 63 Each of the following groups independently represents a straight-chain or branched alkyl group with 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group with 2 to 16 carbon atoms. n independently represents an integer from 0 to 10.
[0233] For details of other maleimide compounds (M6) and their manufacturing methods, please refer to paragraphs 0061 to 0066 of International Publication No. 2020 / 262577, the contents of which are incorporated herein by reference.
[0234] Other maleimide compounds (M7) are other maleimide compounds that use an aromatic amine compound (a1) having one or more but less than three alkyl groups on an aromatic ring, an aromatic divinyl compound (a2) having two vinyl groups, and maleic anhydride as reactants (1).
[0235] Other maleimide compounds (M7) are preferably compounds having the structure shown in formula (M7).
[0236]
[0237] (In the above formula (M7), R) 1 R represents alkyl groups with 1 to 10 carbon atoms, each independently. 2 Each of these groups independently represents an alkyl group with 1 to 10 carbon atoms, an alkoxy group with 1 to 10 carbon atoms, an alkylthio group with 1 to 10 carbon atoms; an aryl group with 6 to 10 carbon atoms, an aryloxy group with 6 to 10 carbon atoms, an arylthio group with 6 to 10 carbon atoms; a cycloalkyl group with 3 to 10 carbon atoms; a halogen atom; a hydroxyl group; or a mercapto group.
[0238] R 3 R 4 R 5 and R 6 Each can independently represent a hydrogen atom or a methyl group, and R 3 and R 4 One of them is a hydrogen atom, and the other is a methyl group, R 5 and R 6 One of them is a hydrogen atom, and the other is a methyl group.
[0239] X 1 The substituents are independently represented by the following formula (x), where r is the number of substituents bonded to X. 1 X of the benzene ring 1 The average of the substitution numbers, where p represents an integer from 1 to 3, q represents an integer from 0 to 4, and k represents an integer from 1 to 100.
[0240]
[0241] (In equation (x), R) 7 and R 8 Each can independently represent a hydrogen atom or a methyl group, and R 7 and R 8 One of them is a hydrogen atom, and the other is a methyl group, R 9Each of these groups independently represents an alkyl group with 1 to 10 carbon atoms, an alkoxy group with 1 to 10 carbon atoms, an alkylthio group with 1 to 10 carbon atoms; an aryl group with 6 to 10 carbon atoms, an aryloxy group with 6 to 10 carbon atoms, an arylthio group with 6 to 10 carbon atoms; a cycloalkyl group with 3 to 10 carbon atoms; a halogen atom; a hydroxyl group; or a mercapto group, where t represents an integer from 0 to 4.
[0242] For details of other maleimide compounds (M7) used in this embodiment, please refer to the description in Japanese Patent No. 7160151, the contents of which are incorporated herein by reference.
[0243] Other maleimide compounds (M8) are bis-other maleimide compounds having 8 or more hydrocarbon groups linked in a straight chain, preferably compounds represented by formula (M8). Such other maleimide compounds (M8) tend to have higher stress relaxation ability, resulting in a tendency for a further reduction in the thermal expansion coefficient of the obtained cured product, and tend to have better dielectric constant and dielectric loss tangent isoelectric properties.
[0244]
[0245] (In formula (M8), R) 1 and R 3 Each of the following groups independently represents a hydrocarbon group consisting of eight or more atoms linked in a straight chain: R 2 Each group independently represents a cyclic hydrocarbon group, either substituted or unsubstituted, comprising 4 or more but less than 10 atoms forming the ring, optionally containing heteroatoms, where n represents a number from 1 to 10.
[0246] In formula (M8), R is preferred. 1 and R 3 For Yasinki, R 2 Cycloalkylene groups with alkyl groups having 6 to 8 carbon atoms as substituents.
[0247] For other maleimide compounds (M8), reference can be made to paragraphs 0014 to 0022 of Japanese Patent Application Publication No. 2018-083893 and paragraphs 0012 to 0022 of Japanese Patent Application Publication No. 2018-090728, and these contents are incorporated into this specification.
[0248] Other maleimide compounds can be manufactured by known methods or commercially available products can be used. Examples of commercially available products include, for instance, K·I Chemical Industry, which produces compounds with formula (M0). Co., Ltd. manufactures "BMI-80"; DIC Co., Ltd. manufactures "NE-X-9470S" and "NE-X-9480S" as compounds represented by formula (M1); Yamato Chemical Industry Co., Ltd. manufactures "BMI-2300" as compounds represented by formula (M2); Nippon Kayaku Co., Ltd. manufactures "MIR-3000-70MT" as compounds represented by formula (M3); Nippon Kayaku Co., Ltd. manufactures "MIR-5000" as compounds represented by formula (M5); Nippon Kayaku Co., Ltd. manufactures "MIZ-001" as a maleimide compound (M6); DIC Co., Ltd. manufactures "NE-X-9500" as a maleimide compound (M7); Resonac manufactures "SFR" as another maleimide compound (M8); DESIGNER MOLECULES INC makes "BMI-689", "BMI-1500", "BMI-2500", "BMI-3000", "BMI-5000".
[0249] Other maleimide compounds besides those mentioned above include, for example, N-phenylmaleimide, N-cyclohexylmaleimide, oligomers of phenylmethane maleimide, m-phenylene bismaleimide, 2,2-bis(4-(4-maleimidephenoxy)-phenyl)propane, 4-methyl-1,3-phenylene bismaleimide, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimidephenoxy)benzene, 1,3-bis(4-maleimidephenoxy)benzene, and their prepolymers, as well as prepolymers of these maleimides and amines.
[0250] In addition to the above, reference may be made to the compounds described in paragraphs 0051 to 0068 of International Publication No. 2020 / 262577 and the maleimide compounds described in paragraphs 0009 to 0096 of Japanese Patent Application Publication No. 2025-9839, the contents of which are incorporated herein by reference.
[0251] The maleimide equivalent of other maleimide compounds is preferably 130 g / eq. or more, more preferably 150 g / eq. or more, further preferably 170 g / eq. or more, even more preferably 180 g / eq. or more, even more preferably 200 g / eq. or more, even more preferably 290 g / eq. or more, and preferably 1000 g / eq. or less, more preferably 800 g / eq. or less, even more preferably 700 g / eq. or less, even more preferably 600 g / eq. or less, and even more preferably 500 g / eq. or less. By setting the value to the aforementioned lower limit or above, the resulting cured product tends to have superior low dielectric properties (Dk and / or Df, especially Df). Furthermore, by setting the value to the aforementioned upper limit or below, the resulting cured product tends to have superior peel strength and a further lower coefficient of thermal expansion.
[0252] When the resin composition of this embodiment contains other maleimide compounds, the lower limit of their content relative to 100 parts by weight of the resin solids in the resin composition is preferably 1 part by weight or more, more preferably 5 parts by weight or more, further preferably 10 parts by weight or more, and even more preferably 20 parts by weight or more. Depending on the application, it can be 25 parts by weight or more, 30 parts by weight or more, or 35 parts by weight or more. By making the content of other maleimide compounds 1 part by weight or more, there is a tendency to improve the flame retardancy of the obtained cured product. In addition, the upper limit of the content of other maleimide compounds relative to 100 parts by weight of the resin solids in the resin composition is preferably 90 parts by weight or less, more preferably 80 parts by weight or less, further preferably 70 parts by weight or less, even more preferably 60 parts by weight or less, and even more preferably 55 parts by weight or less. Depending on the application, it can be 50 parts by weight or less or 45 parts by weight or less. By making the content of other maleimide compounds 90 parts by weight or less, there is a tendency to improve peel strength and low water absorption.
[0253] The resin composition in this embodiment may contain only one other maleimide compound, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0254] Furthermore, the resin composition of this embodiment may also be configured to substantially not contain any maleimide compounds other than the maleimide compound (B) shown in formula (M4). "Substantially not" means that the content of maleimide compounds other than the maleimide compound (B) shown in formula (M4) is less than 10% by mass, preferably less than 5% by mass, more preferably less than 3% by mass, and even more preferably less than 1% by mass. By configuring it in this way, the coefficient of thermal expansion of the obtained cured product can be further reduced.
[0255] <<Aromatic resins with carbon-carbon double bonds at the ends>>
[0256] Aromatic resins with carbon-carbon double bonds at the ends refer to compounds, for example, those with carbon-carbon double bonds at the ends and containing aromatic rings, which are compounds that are cured by heat. By combining aromatic resins with carbon-carbon double bonds at the ends and elastomers (A), the compatibility between the two is improved, and the coefficient of thermal expansion of the resulting cured product can be further reduced.
[0257] Specifically, as an aromatic resin having carbon-carbon double bonds at the ends, it preferably includes one or more of the group consisting of polyphenylene ether compounds having carbon-carbon unsaturated double bonds at the ends and polymers having structural units shown in formula (V), and more preferably includes polyphenylene ether compounds having carbon-carbon unsaturated double bonds at the ends.
[0258] When the resin composition of this embodiment includes an aromatic resin having carbon-carbon double bonds at the ends, its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, further preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more. Depending on the application, it is even more preferably 25 parts by mass or more. It is also preferably 95 parts by mass or less, more preferably 80 parts by mass or less, further preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less. Depending on the application, it is even more preferably 55 parts by mass or less, and even more preferably 50 parts by mass or less. It can also be 45 parts by mass or less, 40 parts by mass or less, or 35 parts by mass or less. By setting the content of the aromatic resin having carbon-carbon double bonds at the ends to the lower limit value or above, there is a tendency to further improve compatibility and heat resistance. Furthermore, by setting the content of the aromatic resin having carbon-carbon double bonds at the ends to the upper limit value or below, there is a tendency to further improve low thermal expansion.
[0259] The resin composition of this embodiment may contain only one aromatic resin having a carbon-carbon double bond at the end, or it may contain two or more. When two or more are contained, the total amount is preferably within the range described above.
[0260] <<<Polyphenylene ether compounds with carbon-carbon unsaturated double bonds at the ends>>>
[0261] The resin composition of this embodiment preferably contains a polyphenylene ether compound having carbon-carbon unsaturated double bonds at the ends, and more preferably contains a polyphenylene ether compound having two or more carbon-carbon unsaturated double bonds at the ends.
[0262] Polyphenylene ether compounds containing two or more carbon-carbon unsaturated double bonds at the ends are preferably polyphenylene ether compounds having two or more groups (preferably vinyl benzyl) at the ends as shown in the following formula (Rx-1). By using these polyphenylene ether compounds, there is a tendency to more effectively improve the low dielectric properties (Dk and / or Df) and low water absorption of printed circuit boards, etc.
[0263] The following is a detailed explanation of their features.
[0264] Examples of polyphenylene ether compounds having carbon-carbon unsaturated double bonds at the ends include compounds having a phenylene ether skeleton as shown in the following formula (X1).
[0265]
[0266] (In formula (X1), R) 24 R 25 R 26 and R 27 (The same or different can be selected to represent alkyl, aryl, halogen, or hydrogen atoms with 6 or fewer carbon atoms.)
[0267] Polyphenylene ether compounds having carbon-carbon unsaturated double bonds at the ends may further include repeating units shown in formula (X2) and / or repeating units shown in formula (X3).
[0268] (In formula (X2), R) 28 R 29 R 30 R 34 and R 35 The same or different can be used to indicate alkyl or phenyl groups with 6 or fewer carbon atoms. R 31 R 32 and R 33 (Optional, either the same or different, consisting of alkyl or phenyl groups with 6 or fewer hydrogen atoms.)
[0269]
[0270] (In formula (X3), R) 36 R 37 R 38 R 39 R 40 R 41 R 42 and R 43 (The following can be selected, either the same or different, and can be an alkyl or phenyl group with 6 or fewer carbon atoms, containing hydrogen atoms. -A- can be a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms.)
[0271] Polyphenylene ether compounds having carbon-carbon unsaturated double bonds at the ends are preferably modified polyphenylene ether compounds whose ends are partially or completely functionalized with olefinic unsaturated groups (hereinafter, sometimes referred to as "modified polyphenylene ether compounds (g)"). More preferably, they are modified polyphenylene ether compounds having two or more groups selected from the group consisting of (meth)acryloyl and vinylbenzyl at the ends. By using such modified polyphenylene ether compounds (g), the dielectric loss tangent (Df) of the cured resin composition can be further reduced, and the low water absorption and peel strength can be improved. These modified polyphenylene ether compounds (g) can be used alone or in combination of two or more.
[0272] Examples of modified polyphenylene ether compounds (g) include polyphenylene ether compounds represented by formula (OP).
[0273]
[0274] (In formula (OP), X represents an aromatic group, -(YO)) n1 - indicates a polyphenylene ether structure, n1 represents an integer from 1 to 100, and n2 represents an integer from 1 to 4. Rx is the group shown in formula (Rx-1) or formula (Rx-2).
[0275]
[0276] (In equations (Rx-1) and (Rx-2), R) 1 R 2 and R 3 Each group independently represents a hydrogen atom, alkyl, alkenyl, or alkynyl group. * indicates the bonding site with an oxygen atom. Mc independently represents hydrocarbon groups with 1 to 12 carbon atoms. z represents an integer from 0 to 4. r represents an integer from 0 to 6.
[0277] The aromatic group X shown above may or may not have substituents on the benzene ring, but it is preferred to have substituents. When substituents are present, the substituent Z shown above can be exemplified. It is preferably at least one selected from the group consisting of alkyl, aryl, and halogen atoms having 6 or fewer carbon atoms, more preferably an alkyl group having 3 or fewer carbon atoms, and even more preferably a methyl group.
[0278] Furthermore, the polyphenylene ether structure shown above (YO)n1- may or may not have substituents on the benzene ring, but it is preferable to have substituents. When substituents are present, the substituent Z described above can be cited as an example, preferably an alkyl or phenyl group with 6 or fewer carbon atoms, more preferably an alkyl group with 3 or fewer carbon atoms, and even more preferably a methyl group.
[0279] When n1 and / or n2 are integers of 2 or more, the n1 structural units (YO) and / or n2 structural units can be the same or different. n2 is preferably 2 or more, and more preferably 2.
[0280] In equations (Rx-1) and (Rx-2), R 1 R 2 and R 3 Each can be independently represented by a hydrogen atom, alkyl group, alkenyl group, or alkynyl group.
[0281] R 1 Preferably, it is a hydrogen atom or an alkyl group, more preferably a hydrogen atom or a methyl group, and even more preferably a hydrogen atom.
[0282] R 2 and R 3 Hydrogen atoms or alkyl groups are preferred individually, hydrogen atoms or methyl groups are more preferred, and hydrogen atoms are even more preferred.
[0283] As R 1 R 2 and R 3 The alkyl, alkenyl, or alkynyl groups preferably have 5 or fewer carbon atoms, more preferably 3 or fewer.
[0284] In formula (Rx-1), r represents an integer from 0 to 6, which can be an integer greater than or equal to 1. In addition, it is preferably an integer less than or equal to 5, more preferably an integer less than or equal to 4, further preferably an integer less than or equal to 3, even more preferably 1 or 2, and even more preferably 1.
[0285] In formula (Rx-1), Mc independently represents a hydrocarbon group with 1 to 12 carbon atoms, preferably a hydrocarbon group with 1 to 10 carbon atoms, more preferably a straight-chain or branched alkyl group with 1 to 10 carbon atoms, further preferably methyl, ethyl, isopropyl, isobutyl, tert-butyl, pentyl, octyl or nonyl, and even more preferably methyl, ethyl, isopropyl, isobutyl or tert-butyl.
[0286] In formula (Rx-1), z represents an integer from 0 to 4, preferably an integer from 0 to 3, more preferably an integer from 0 to 2, even more preferably 0 or 1, and even more preferably 0.
[0287] Specific examples of the group represented by formula (Rx-1) are vinylbenzyl and specific examples of the group represented by formula (Rx-2) are (meth)acryloyl.
[0288] In the resin composition of this embodiment, as a polyphenylene ether compound having a carbon-carbon unsaturated double bond at the end, it is also preferable to include both a polyphenylene ether compound belonging to the compound shown in formula (OP) and having a group shown in formula (Rx-1) and a polyphenylene ether compound having a group shown in formula (Rx-2).
[0289] Examples of modified polyphenylene ether compounds (g) include compounds represented by formula (OP-1).
[0290]
[0291] (In formula (OP-1), X represents an aromatic group, -(YO)n2- represents a polyphenylene ether structure, R 1 R 2 and R 3 Each group independently represents a hydrogen atom, alkyl group, alkenyl group, or alkynyl group; n1 represents an integer from 0 to 6; n2 represents an integer from 1 to 100; and n3 represents an integer from 1 to 4.
[0292] The aromatic group X shown above may or may not have substituents on the benzene ring, but it is preferred to have substituents. When substituents are present, the substituent Z shown above can be exemplified. It is preferably at least one selected from the group consisting of alkyl, aryl, and halogen atoms having 6 or fewer carbon atoms, more preferably an alkyl group having 3 or fewer carbon atoms, and even more preferably a methyl group.
[0293] Furthermore, the polyphenylene ether structure shown above (YO)n2- may or may not have substituents on the benzene ring, but it is preferable to have substituents. When substituents are present, the substituent Z described above can be exemplified, preferably an alkyl or phenyl group with 6 or fewer carbon atoms, more preferably an alkyl group with 3 or fewer carbon atoms, and even more preferably a methyl group.
[0294] When n2 and / or n3 are integers of 2 or more, the n2 structural units (YO) and / or n3 structural units can be the same or different. n3 is preferably 2 or more, and more preferably 2.
[0295] The modified polyphenylene ether compound (g) in this embodiment is preferably the compound shown in formula (OP-2).
[0296]
[0297] Here, -(OXO)- is preferably represented by (OP-3) and / or formula (OP-4).
[0298]
[0299] (In formula (OP-3), R) 4 R 5 R 6 R 10 and R 11 Choose either the same or different, which are alkyl or phenyl groups having 6 or fewer carbon atoms. R 7 R 8 and R9 (Optional, either the same or different, consisting of alkyl or phenyl groups with 6 or fewer hydrogen atoms.)
[0300]
[0301] (In formula (OP-4), R) 12 R 13 R 14 R 15 R 16 R 17 R 18 and R 19 (The following can be selected, either the same or different, and can be an alkyl or phenyl group with 6 or fewer carbon atoms, containing hydrogen atoms. -A- can be a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms.)
[0302] In addition, -(YO)- is preferably represented by formula (OP-5).
[0303]
[0304] (In formula (OP-5), R) 20 R 21 Choose either the same or different, which are alkyl or phenyl groups having 6 or fewer carbon atoms. R 22 R 23 (Optional, either the same or different, consisting of alkyl or phenyl groups with 6 or fewer hydrogen atoms.)
[0305] Especially through R 20 and R 21 Each of the resin molecules has one or more methyl and / or cyclohexyl groups, which increases the rigidity of the resin molecules. Molecules with high rigidity have lower mobility compared to molecules with low rigidity, resulting in a longer relaxation time during dielectric relaxation and excellent low dielectric properties (Dk and / or Df, especially Dk), making them preferred.
[0306] An example of formula (OP-5) is the following structure.
[0307]
[0308] For information on polyphenylene ether compounds having the above-described structure, please refer to the description in Japanese Patent Application Publication No. 2019-194312, the contents of which are incorporated herein by reference.
[0309] In formula (OP-2), a and b each independently represent an integer of 0 to 100, and at least one of a and b is an integer of 1 to 100. Each of a and b is independently preferably an integer of 0 to 50, more preferably an integer of 1 to 30, and still more preferably an integer of 1 to 10. When a and / or b is an integer of 2 or more, two or more of -(Y-O)- may each independently be formed by arranging one type of structure, or may be formed by arranging two or more types of structures in a block or random manner.
[0310] In addition, in the case where a plurality of compounds represented by formula (OP-2) are contained, the average value of a is preferably 1<a<10, and the average value of b is preferably 1<b<10.
[0311] Examples of -A- in formula (OP-4) include divalent organic groups such as methylene, ethylidene, 1-methylethylidene, 1,1-propylidene, 1,4-phenylenebis(1-methylethylidene) group, 1,3-phenylenebis(1-methylethylidene) group, cyclohexylidene, phenylmethylene, naphthylmethylene, 1-phenylethylidene, but are not limited thereto.
[0312] Among the compounds represented by the above formula (OP-2), R is preferred 4 , R 5 , R 6 , R 10 , R 11 , R 20 and R 21 are alkyl groups having 3 or less carbon atoms, and R 7 , R 8 , R 9 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , R 18 , R 19 , R 22 and R 23 are hydrogen atoms or alkyl groups having 3 or less carbon atoms. For the polyphenylene ether compound, it is particularly preferred that -(O-X-O)- represented by formula (OP-3) or formula (OP-4) is formula (OP-9), formula (OP-10) and / or formula (OP-11), and -(Y-O)- represented by formula (OP-5) is formula (OP-12) or formula (OP-13). When a and / or b is an integer of 2 or more, two or more of -(Y-O)- each independently have a structure formed by arranging two or more of formula (OP-12) and / or formula (OP-13), or may have a structure formed by arranging formula (OP-12) and formula (OP-13) in a block or random manner.
[0313]
[0314]
[0315] (In formula (OP-10), R) 44 R 45 R 46 and R 47 The atom can be either the same or different, and can be either hydrogen or methyl. -B- is a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms.
[0316] -B- can be given as a specific example that is the same as the specific example of -A- in equation (OP-4).
[0317]
[0318] In formula (OP-11), -B- is a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms.
[0319] -B- can be given as a specific example that is the same as the specific example of -A- in equation (OP-4).
[0320]
[0321]
[0322] The modified polyphenylene ether compound (g) is further preferably the compound shown in formula (OP-14) and / or the compound shown in formula (OP-15), and is further preferably the compound shown in formula (OP-15).
[0323]
[0324] (In equation (OP-14), a and b independently represent integers from 0 to 100, and at least one of a and b is an integer from 1 to 100.)
[0325] In equation (OP-14), a and b have the same meaning as a and b in equation (OP-2), and the preferred range is also the same.
[0326]
[0327] (In equation (OP-15), a and b independently represent integers from 0 to 100, and at least one of a and b is an integer from 1 to 100.)
[0328] In equation (OP-15), a and b have the same meaning as a and b in equation (OP-2), and the preferred range is also the same.
[0329] Alternatively, the polyphenylene ether compound used in this embodiment may also be a compound represented by formula (OP-16).
[0330]
[0331] (In equation (OP-16), x independently represents an integer from 0 to 100, and at least one of the two x's is an integer from 1 to 100.)
[0332] Polyphenylene ether compounds with carbon-carbon unsaturated double bonds at the ends can be manufactured by known methods or commercially available products can be used. Examples of commercially available products include "SA9000" manufactured by SABIC Innovative Plastics, a modified polyphenylene ether compound with a methacryloyl group at the end. Examples of modified polyphenylene ether compounds with a vinyl benzyl group at the end include "OPE-2St1200" and "OPE-2St2200" manufactured by Mitsubishi Gas Chemical Co., Ltd. Alternatively, a modified polyphenylene ether compound with a vinyl benzyl group at the end can be obtained by modifying a hydroxyl-terminated polyphenylene ether compound such as "SA90" manufactured by SABIC Innovative Plastics to a vinyl benzyl group using a vinyl benzyl chloride or similar substance.
[0333] Furthermore, detailed information on polyphenylene ether compounds having carbon-carbon unsaturated double bonds at the ends can be found in paragraphs 0015 to 0048 of Japanese Patent Application Publication No. 2006-028111, Japanese Patent Application Publication No. 2018-131519, International Patent Application Publication No. 2019-138992, International Patent Application Publication No. 2022-054303, Japanese Patent Application Publication No. 2024-544483, and Japanese Patent Application No. 7530718, which are incorporated herein by reference.
[0334] The number-average molecular weight (details as described in the examples below) of polyphenylene ether compounds (preferably modified polyphenylene ether compounds (g)) with terminal carbon-carbon unsaturated double bonds, converted to polystyrene by GPC (gel permeation chromatography), is preferably 500 or more and 3,000 or less. By setting the number-average molecular weight to 500 or more, there is a tendency to further suppress stickiness when the resin composition of this embodiment is formed into a coating film. Furthermore, by setting the number-average molecular weight to 3,000 or less, there is a tendency to further improve solubility in solvents.
[0335] Furthermore, the weight-average molecular weight (according to the method described in the examples below) of the GPC-based polystyrene compound having carbon-carbon unsaturated double bonds at the ends (preferably a modified polyphenylene ether compound (g)) is preferably 800 or more and 10,000 or less, more preferably 800 or more and 5,000 or less. By setting the weight-average molecular weight to the aforementioned lower limit or above, there is a tendency for the relative permittivity (Dk) and dielectric loss tangent (Df) of the cured resin composition to become lower, and by setting it to the aforementioned upper limit or below, there is a tendency for the solubility, low viscosity, and formability of the resin composition in solvents when producing varnishes, etc., as described below below.
[0336] Furthermore, in polyphenylene ether compounds (preferably modified polyphenylene ether compounds (g)) having carbon-carbon unsaturated double bonds at their ends, the equivalent amount of carbon-carbon unsaturated double bonds at the ends is preferably 400 to 5000 g relative to each carbon-carbon unsaturated double bond, more preferably 400 to 2500 g. By making the equivalent amount of carbon-carbon unsaturated double bonds at the ends above the aforementioned lower limit, there is a tendency for the relative dielectric constant (Dk) and dielectric loss tangent (Df) of the cured resin composition to become lower, and by making it below the aforementioned upper limit, there is a tendency for the solubility, low viscosity, and formability of the resin composition in solvents to be further improved.
[0337] The functional group equivalent (equivalent of carbon-carbon unsaturated double bond) in polyphenylene ether compounds with carbon-carbon unsaturated double bonds at the ends is determined by the measurement results of an infrared spectrophotometer, and the double bond amount is calculated from its reciprocal.
[0338] The double bond equivalent [g / eq.] is calculated as follows.
[0339] Weigh and record the weight of the polyphenylene ether compound powder. Place the powder in a volumetric flask and dilute to the specified volume with carbon disulfide to prepare the test sample. Place the sample solution in the measurement cell and set it in an infrared spectrophotometer (FT / IR-4600, manufactured by Nippon Spectrophotometer Co., Ltd.). Then, perform infrared spectrophotometric determination of the sample solution. In the case of vinyl groups in the polyphenylene ether compound, record 905 cm⁻¹. -1 The peak area of the nearby spectrum. In the case where the carbon-carbon unsaturated double bond is methacrylyl, the peak area is recorded at 1640 cm⁻¹. -1 The peak area of the nearby spectrum. The double bond concentration [mol / L] is calculated from this area value and the standard curve as the measured value.
[0340] Next, the double bond equivalent is calculated using the following formula.
[0341] Double bond equivalent [g / eq.] = Weight of powder in the sample [g] / Double bond concentration [mol / L] × Volume of sample solution [L]
[0342] The functional group equivalent of thermosetting compounds other than polyphenylene ether compounds with carbon-carbon unsaturated double bonds at the ends can also be determined using the method described above. However, for compounds (monomers) that can be expressed as a single molecular weight, it is preferred to calculate the functional group equivalent by (theoretical molecular weight ÷ number of functional groups). In cases where two or more other thermosetting compounds are included, the functional group equivalent of the other thermosetting compounds is set as the sum (weighted average) of the values obtained by multiplying the functional group equivalent of each other thermosetting compound by its mass fraction.
[0343] When the resin composition of this embodiment contains a polyphenylene ether compound having carbon-carbon unsaturated double bonds at the ends, the lower limit of its content relative to 100 parts by mass of resin solids in the resin composition is preferably 1 part by mass or more, more preferably 5 parts by mass or more, further preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, and depending on the application, it can be 25 parts by mass or more. By making the content of the polyphenylene ether compound having carbon-carbon unsaturated double bonds at the ends at the aforementioned lower limit, there is a tendency to further improve the formability of the resin composition, the heat resistance of the obtained cured product, the low water absorption, and the low dielectric properties (Dk and / or Df). Furthermore, relative to 100 parts by weight of the resin solids in the resin composition, the upper limit of the content of the polyphenylene ether compound having carbon-carbon unsaturated double bonds at the ends is preferably 90 parts by weight or less, more preferably 80 parts by weight or less, further preferably 70 parts by weight or less, and even more preferably 60 parts by weight or less. Depending on the application, it can be 50 parts by weight or less, 45 parts by weight or less, 40 parts by weight or less, or 35 parts by weight or less. By keeping the content of the polyphenylene ether compound having carbon-carbon unsaturated double bonds at the ends below the above-mentioned upper limit, there is a tendency to obtain cured products with lower dielectric properties (especially lower dielectric loss tangent) and improved chemical resistance.
[0344] The resin composition in this embodiment may contain only one polyphenylene ether compound having a carbon-carbon unsaturated double bond at the end, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0345] <<<Polymers with the structural units shown in formula (V)>>>
[0346] The resin composition of this embodiment may contain a polymer having structural units as shown in Formula (V). By containing a polymer having structural units as shown in Formula (V), a resin composition with excellent low dielectric properties (low relative permittivity, low dielectric loss tangent) can be obtained.
[0347]
[0348] (In formula (V), Ar represents an aromatic hydrocarbon linking group. * indicates a bonding position.)
[0349] The aromatic hydrocarbon linking group can be a group formed solely of an aromatic hydrocarbon optionally having substituents, or a group formed by a combination of an aromatic hydrocarbon optionally having substituents and other linking groups, preferably a group formed solely of an aromatic hydrocarbon optionally having substituents. It should be noted that the substituents optionally present in the aromatic hydrocarbon can include substituent Z (e.g., alkyl groups with 1 to 6 carbon atoms, alkenyl groups with 2 to 6 carbon atoms, alkoxy groups with 2 to 6 carbon atoms, hydroxyl groups, amino groups, carboxyl groups, halogen atoms, etc.). Furthermore, the aforementioned aromatic hydrocarbon preferably does not have substituents.
[0350] Aromatic hydrocarbons typically have divalent linking groups.
[0351] Specifically, the aromatic hydrocarbon linking group may include, optionally, phenylene, naphthyl, anthracenediyl, phenanthrenediyl, biphenyldiyl, and fluorenediyl, with substituted groups being preferred. Substituents may include the aforementioned substituent Z, and the aforementioned phenylene and other groups are preferably unsubstituented.
[0352] Polymers having the structural units shown in formula (V) more preferably include at least one of the structural units shown in formula (V1), formula (V2), and formula (V3). It should be noted that * in the following formulas indicates a bonding position. Furthermore, hereinafter, the structural units shown in formulas (V1) to (V3) are sometimes collectively referred to as "structural unit (a)".
[0353]
[0354] In equations (V1) to (V3), L 1 The linking group is an aromatic hydrocarbon (preferably with 6 to 22 carbon atoms, more preferably 6 to 18, and even more preferably 6 to 10). Specifically, examples include phenylene, naphthyl, anthracenediyl, phenanthrenediyl, biphenyldiyl, and fluorenediyl, which are optionally substituents, with phenylene being the preferred option. Substituents can be exemplified by substituent Z described above, and the aforementioned phenylene and other groups are preferably unsubstituents.
[0355] The compound forming structural unit (a) is preferably a divinyl aromatic compound, such as divinylbenzene, bis(1-methylvinyl)benzene, divinylnaphthalene, divinylanthracene, divinylbiphenyl, divinylphenanthrene, etc. Divinylbenzene is particularly preferred. One of these divinyl aromatic compounds may be used, or two or more may be used as needed.
[0356] That is, the structural unit (a) is preferably a structural unit derived from a divinyl aromatic compound.
[0357] As described above, a polymer having the structural unit shown in formula (V) can be a homopolymer of the compound forming structural unit (a) or a copolymer of structural units derived from other monomers.
[0358] When the polymer having the structural unit shown in formula (V) is a copolymer, the copolymerization ratio of structural unit (a) is preferably 3 mol% or more, more preferably 5 mol% or more, even more preferably 10 mol% or more, and may also be 15 mol% or more. As an upper limit, it is preferably 90 mol% or less, more preferably 85 mol% or less, even more preferably 80 mol% or less, even more preferably 70 mol% or less, more preferably 60 mol% or less, even more preferably 50 mol% or less, even more preferably 40 mol% or less, particularly more preferably 30 mol% or less, and may further be 25 mol% or less, or 20 mol% or less.
[0359] As a structural unit derived from other monomers, an example can be given of a structural unit (b) derived from an aromatic compound having one vinyl group (monovinyl aromatic compound).
[0360] The structural unit (b) derived from a monovinyl aromatic compound is preferably the structural unit shown in the following formula (V4).
[0361]
[0362] In equation (V4), L 2 As a preferred example of an aromatic hydrocarbon linking group, the L group mentioned above can be cited. 1 Examples. * indicates the bonding location.
[0363] R V1 It is a hydrocarbon group (preferably alkyl) with 1 to 12 carbon atoms, consisting of hydrogen atoms. V1 When it is a hydrocarbon group, the number of carbon atoms is preferably 1 to 6, more preferably 1 to 3. V1 and L 2 It can have the above-mentioned substituent Z.
[0364] When the polymer having the structural unit shown in formula (V) is a copolymer containing structural unit (b) derived from a monovinyl aromatic compound, examples of monovinyl aromatic compounds include vinyl aromatic compounds such as styrene, vinylnaphthalene, and vinyl biphenyl; and nucleoalkyl-substituted vinyl aromatic compounds such as o-methylstyrene, m-methylstyrene, p-methylstyrene, o- and p-dimethylstyrene, o-ethylvinylbenzene, m-ethylvinylbenzene, p-ethylvinylbenzene, methylvinylbiphenyl, and ethylvinylbiphenyl. The monovinyl aromatic compounds illustrated herein may suitably have the aforementioned substituent Z. Furthermore, one or more of these monovinyl aromatic compounds may be used. Preferably, structural unit (b) contains a structural unit derived from at least one of the group consisting of o-ethylvinylbenzene, m-ethylvinylbenzene, and p-ethylvinylbenzene, and more preferably, in addition to containing a structural unit derived from at least one of the group consisting of o-ethylvinylbenzene, m-ethylvinylbenzene, and p-ethylvinylbenzene, it also contains a structural unit derived from styrene.
[0365] When the polymer having the structural unit shown in formula (V) is a copolymer containing structural unit (b), the copolymerization ratio of structural unit (b) is preferably 10 mol% or more, more preferably 15 mol% or more, and further preferably 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, or 75 mol% or more. As an upper limit, it is preferably 98 mol% or less, more preferably 90 mol% or less, and even more preferably 85 mol% or less.
[0366] Polymers having the structural units shown in formula (V) may also have other structural units besides structural units (a) and (b). Examples of other structural units include structural units (c) derived from cyclic olefin compounds. Examples of cyclic olefin compounds include hydrocarbons having double bonds within the ring structure. Specifically, in addition to monocyclic cyclic olefins such as cyclobutene, cyclopentene, cyclohexene, and cyclooctene, examples include compounds with a norbornene ring structure such as norbornene and dicyclopentadiene, and cyclic olefin compounds with fused aromatic rings such as indene and acenaphthene. Examples of norbornene compounds include those described in paragraphs 0037 to 0043 of Japanese Patent Application Publication No. 2018-039995, the contents of which are incorporated herein by reference. It should be noted that the cyclic olefin compounds illustrated herein may further have the aforementioned substituent Z.
[0367] When the polymer having the structural unit shown in formula (V) is a copolymer containing structural unit (c), the copolymerization ratio of structural unit (c) is preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more. As an upper limit, it is preferably 90 mol% or less, more preferably 80 mol% or less, even more preferably 70 mol% or less, and can be 50 mol% or less, or 30 mol% or less.
[0368] In polymers having the structural units shown in formula (V), structural units (d) derived from different polymeric compounds (hereinafter also referred to as other polymeric compounds) may be further introduced. Examples of other polymeric compounds (monomers) include compounds containing three vinyl groups. Specifically, examples include 1,3,5-trivinylbenzene, 1,3,5-trivinylnaphthalene, and 1,2,4-trivinylcyclohexane. Alternatively, examples include ethylene glycol diacrylate, butadiene (e.g., 1,3-butadiene), and isoprene. The copolymerization ratio of structural units (d) derived from other polymeric compounds is preferably 30 mol% or less, more preferably 20 mol% or less, and even more preferably 10 mol% or less.
[0369] As one embodiment of a polymer having the structural unit shown in formula (V), a polymer that must have structural unit (a) and includes at least one of structural units (b) and (c) can be exemplified. Furthermore, an embodiment can be exemplified in which the total of structural units (a) to (c) accounts for more than 90 mol%, more than 95 mol%, and particularly more than 98 mol% of all structural units.
[0370] As another embodiment of a polymer having the structural unit shown in formula (V), a polymer that must have structural unit (a) and includes at least one of structural units (b) to (d) can be exemplified. Furthermore, an example can be illustrated in which the total of structural units (a) to (d) accounts for more than 95 mol% and more than 98 mol% of all structural units.
[0371] As another embodiment of a polymer having the structural unit shown in formula (V), a polymer in which structural unit (a) is required, except for the end, preferably contains 90 mol% or more of the structural unit containing an aromatic ring, more preferably 95 mol% or more, and may also contain 100 mol% of the polymer.
[0372] It should be noted that when calculating the mole % relative to all structural units, one structural unit refers to a structural unit derived from one molecule of a monomer (e.g., divinyl aromatic compound, monovinyl aromatic compound, etc.) used in the manufacture of a polymer having the structural unit shown in formula (V).
[0373] The method for manufacturing polymers having the structural units shown in formula (V) is not particularly limited and can be carried out according to conventional methods. For example, polymerizing a raw material containing a divinyl aromatic compound (with monovinyl aromatic compounds, cycloolefin compounds, etc., coexisting as needed) in the presence of a Lewis acid catalyst can be carried out. As a Lewis acid catalyst, metal fluorides such as boron trifluoride or their complexes can be used.
[0374] The structure of the chain ends of polymers having the structural units shown in formula (V) is not particularly limited. However, for groups derived from the aforementioned divinyl aromatic compounds, structures of formula (E1) can be cited. Furthermore, L in formula (E1)... 1 Same as specified in equation (V1) above. * indicates the bonding position.
[0375] *-CH=CH-L 1 -CH=CH2 (E1)
[0376] When the group derived from a monovinyl aromatic compound becomes the chain terminator, structures taking the form of the following formula (E2) can be listed. In the formula, L... 2 and R V1 These have the same meanings as defined in equation (V4) above. * indicates the bonding position.
[0377] *-CH=CH-L 2 -R V1 (E2)
[0378] The polymer having the structural unit shown in formula (V) preferably has a molecular weight of 300 or more, more preferably 500 or more, further preferably 1,000 or more, and even more preferably 1,500 or more, in terms of number average molecular weight (Mn). As an upper limit for the number average molecular weight, it is preferably 130,000 or less, more preferably 120,000 or less, further preferably 110,000 or less, and even more preferably 100,000 or less, but can be 30,000 or less, 10,000 or less, or 5,000 or less.
[0379] The molecular weight of the polymer having the structural unit shown in Formula (V), expressed as a weight-average molecular weight Mw, is preferably 3,000 or more, more preferably 5,000 or more, and even more preferably 10,000 or more. By setting the weight-average molecular weight to the aforementioned lower limit or above, the cured resin composition can effectively exhibit the excellent low dielectric properties (Dk and / or Df), particularly Df, and the dielectric properties after moisture absorption, inherent in the polymer having the structural unit shown in Formula (V). As the upper limit of the weight-average molecular weight Mw, it is preferably 130,000 or less, more preferably 100,000 or less, even more preferably 80,000 or less, and even more preferably 50,000 or less. By setting the weight-average molecular weight to the aforementioned upper limit or below, there is a tendency to avoid embedding defects when the prepreg or resin sheet is laminated onto the circuit forming substrate.
[0380] The monodispersity (Mw / Mn), expressed as the ratio of weight-average molecular weight (Mw) to number-average molecular weight (Mn), is preferably 100 or less, more preferably 50 or less, even more preferably 20 or less, and can be 15 or less, or 12 or less. As a lower limit, it is practically 1.1 or more, preferably 2.0 or more, more preferably 4 or more, even more preferably 5 or more, even more preferably 7 or more, and even more preferably 8 or more.
[0381] The above-mentioned Mw and Mn were measured according to the description of the embodiments described later.
[0382] When the resin composition of this embodiment contains two or more polymers having structural units shown in formula (V), it is preferable that the Mw, Mn, and Mw / Mn of the mixture satisfy the above-mentioned ranges.
[0383] The vinyl equivalent of the polymer having the structural unit shown in formula (V) is preferably 200 g / eq. or more, more preferably 230 g / eq. or more, and even more preferably 250 g / eq. or more, and can be 300 g / eq. or more or 350 g / eq. or more. Furthermore, the vinyl equivalent is preferably 1200 g / eq. or less, more preferably 1000 g / eq. or less, and can be 800 g / eq. or less, 600 g / eq. or less, 500 g / eq. or less, 400 g / eq. or less, or 350 g / eq. or less. By setting the vinyl equivalent to the aforementioned lower limit or above, there is a tendency to improve the storage stability of the resin composition and the flowability of the resin composition. Therefore, the formability is improved, and voids are less likely to occur during the formation of prepregs, etc., leading to a tendency to obtain printed circuit boards with higher reliability. On the other hand, by setting the vinyl equivalent to the aforementioned upper limit or below, there is a tendency to improve the heat resistance of the obtained cured product.
[0384] Polymers having the structural unit shown in Formula (V) preferably exhibit excellent low dielectric properties (Dk and / or Df) in their cured products. For example, in this embodiment, the relative permittivity (Dk) of the cured product of the polymer having the structural unit shown in Formula (V) at 10 GHz, measured by the cavity resonator perturbation method, is preferably 2.80 or less, more preferably 2.60 or less, further preferably 2.50 or less, and even more preferably 2.40 or less. Furthermore, the lower limit of the aforementioned relative permittivity is, for example, actually 1.80 or more. Additionally, the dielectric loss tangent (Df) of the cured product of the polymer having the structural unit shown in Formula (V) at 10 GHz, measured by the cavity resonator perturbation method, is preferably 0.0030 or less, more preferably 0.0020 or less, and even more preferably 0.0010 or less. Furthermore, the lower limit of the aforementioned dielectric loss tangent is, for example, actually 0.0001 or more.
[0385] The relative permittivity (Dk) and dielectric loss tangent (Df) were determined by the following method.
[0386] 4.5g of resin powder was spread into a stainless steel mold with a height of 100mm×30mm×1.0mm, placed in a vacuum press (made by Kitagawa Seiki Co., Ltd.), kept at 200°C for 2 hours, and pressed under a surface pressure of 3.0MPa to produce a cured board.
[0387] After reducing the width of the cured plate to 1.0 mm, it was dried at 120°C for 60 minutes. Then, the relative permittivity (Dk) and dielectric loss tangent (Df) of the dried plate were measured at 10 GHz using a perturbation method cavity resonator. The measurement temperature was set to 23°C.
[0388] In this specification, for polymers having the structural units shown in formula (V), refer to the compounds and their synthesis reaction conditions described in paragraphs 0029 to 0058 of International Publication No. 2017 / 115813, the compounds and their synthesis reaction conditions described in paragraphs 0013 to 0058 of Japanese Patent Application Publication No. 2018-039995, and the compounds described in paragraphs 0008 to 0043 of Japanese Patent Application Publication No. 2018-168347. The following compounds and their synthesis reaction conditions, as well as those described in paragraphs 0014 to 0042 of Japanese Patent Application Publication No. 2006-070136, paragraphs 0014 to 0061 of Japanese Patent Application Publication No. 2006-089683, and paragraphs 0008 to 0036 of Japanese Patent Application Publication No. 2008-248001, are incorporated herein by reference.
[0389] Polymers having the structural units shown in formula (V) can also be commercially available, such as LF-310T50 manufactured by NIPPON STEELC Chemical & Material Co., Ltd.
[0390] When the resin composition of this embodiment contains a polymer having the structural unit shown in formula (V), the lower limit of its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more. Depending on the application, it can be 15 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more. By making the content of the polymer having the structural unit shown in formula (V) the above-mentioned lower limit or more, there is a tendency to effectively achieve low dielectric properties, especially low relative permittivity. In addition, the upper limit of the content of the polymer having the structural unit shown in formula (V) relative to 100 parts by mass of the resin solids in the resin composition is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less. It can also be 50 parts by mass or less, 45 parts by mass or less, 40 parts by mass or less, 35 parts by mass or less, or 30 parts by mass or less. By setting the content of the polymer having the structural unit shown in formula (V) below the above-mentioned upper limit, there is a tendency to improve the peel strength and low water absorption of the metal foil.
[0391] The resin composition of this embodiment may contain only one polymer having the structural unit shown in formula (V), or it may contain two or more. When it contains two or more, the total amount is preferably within the range described above.
[0392] Furthermore, the resin composition in this embodiment can also be formulated to substantially not contain polymers having the structural units shown in formula (V). "Substantially not" means that the content of polymers having the structural units shown in formula (V) is less than 1 part by mass relative to 100 parts by mass of the resin solids in the resin composition, preferably less than 0.1 parts by mass, and more preferably less than 0.01 parts by mass.
[0393] <<Other compounds with carbon-carbon unsaturated double bonds at the ends (compound (XC))>>
[0394] The resin composition of this embodiment may contain other compounds (compounds (XC)) that have carbon-carbon unsaturated double bonds at the ends, in addition to those described above.
[0395] An example of compound (XC) is a low-molecular-weight aromatic vinyl compound.
[0396] Examples of aromatic vinyl compounds include methylstyrene (e.g., 4-methylstyrene), ethyl vinylbenzene, diethyl 4-vinylbenzylphosphonate, 4-vinylbenzyl glycidyl ether, α-methylstyrene, 4-tert-butylstyrene, divinylbenzene, vinyl benzyl ether, 1,3-diisopropenylbenzene, and 1,4-diisopropenylbenzene, with 4-methylstyrene, 4-tert-butylstyrene, and divinylbenzene being preferred.
[0397] Additionally, examples of resins having an isopropylene group as described in International Publication No. 2022 / 210095 (e.g., the compounds described in Synthesis Examples 1, 2, 7, and 8 of that publication) may be incorporated into this specification.
[0398] Another example of other compounds with carbon-carbon unsaturated double bonds at the end (compound (XC)) is vinyl benzyl ether.
[0399] Examples of vinyl benzyl ethers include reaction products generated from the reaction of 4,4'-isopropylidene bis(2,6-dimethylphenol) (tetramethylbisphenol A), hexamethylbiphenol (2,2',3,3',5,5'-hexamethyl-(1,1'-biphenyl)-4,4'-diol), 2,6-dihydroxynaphthalene, etc., with vinyl benzyl chloride and / or vinyl benzyl bromide.
[0400] Furthermore, examples that can be listed include resorcinol, catechol, hydroquinone, 2,7-dihydroxynaphthalene, 2-(diphenylphospho)hydroquinone, bis(2,6-dimethylphenol), 2,2'-biphenol, 4,4-biphenol, 2,2',6,6'-tetramethylbiphenol, 3,3',5,5'-tetrabromo-2,2',6,6'-tetramethylbiphenol, 3,3'-dibromo-2,2',6,6'-tetramethylbiphenol, 4,4'-isopropylidenebis(2,6-dibromophenol) (tetrabromobisphenol A), 4,4'-isopropylidenebis(2,6-dimethylphenol) (tetramethylbisphenol A), 4,4'-isopropylidenebis(2-methylphenol), 4,4'-isopropylidenebis(2-allylphenol), 4,4 '(1,3-Phenylidene diisopropylidene)bisphenol (Bisphenol M), 4,4'-isopropylidene bis(3-phenylphenol), 4,4'-(1,4-Phenylidene diisopropylidene)bisphenol (Bisphenol P), 4,4'-ethoxydiphenol (Bisphenol E), 4,4'-oxodiphenol, 4,4'-thiodiphenol, 4,4'-thiobis(2,6-dimethylphenol), 4,4'-sulfonyldiphenol, 4,4'-sulfonylbis(2,6-dimethylphenol), 4,4'-sulfonylurea diphenol, 4,4'-hexafluoroisopropylidene)bisphenol (Bisphenol AF), 4,4'-(1-phenylethoxy)bisphenol (Bisphenol AP), bis(4-hydroxyphenyl)-2,2-dichloroethylene (Bisphenol C), bis(4-hydroxyphenyl)methane (Bisphenol A) Phenol F), bis(2,6-dimethyl-4-hydroxyphenyl)methane, 4,4'-(cyclopentylene)diphenol, 4,4'-(cyclohexylene)diphenol (bisphenol Z), 4,4'-(cyclododecylene)diphenol, 4,4'-(bicyclo[2.2.1]heptylene)diphenol, 4,4'-(9H-fluorene-9,9-diyl)diphenol, 3,3-bis(4-hydroxyphenyl)isobenzofuran-1(3H)-one, 1-(4-hydroxyphenyl)-3,3-dimethyl-2,3-dihydro-1H-indene-5-ol, 1-(4-hydroxy-3,5-dimethylphenyl)-1,3,3,4,6-pentamethyl-2,3-dihydro-1H-indene-5-ol, 3,3,3',3'-tetramethyl-2,2 Vinyl benzyl ethers are formed by reacting ',3,3'-tetrahydro-1,1'-spirodi[indene]-5,6'-diol (spirodiindene), dihydroxybenzophenone (bisphenol K), tris(4-hydroxyphenyl)methane, tris(4-hydroxyphenyl)ethane, tris(4-hydroxyphenyl)propane, tris(4-hydroxyphenyl)butane, tris(3-methyl-4-hydroxyphenyl)methane, tris(3,5-dimethyl-4-hydroxyphenyl)methane, tetra(4-hydroxyphenyl)ethane, tetra(3,5-dimethyl-4-hydroxyphenyl)ethane, bis(4-hydroxyphenyl)phenylphosphine oxide, dicyclopentadienylbis(2,6-dimethylphenol), dicyclopentadienylbis(o-cresol), dicyclopentadienylbisphenol, etc. with vinyl benzyl chloride or vinyl benzyl bromide.
[0401] In addition to the above, the vinyl benzyl compounds also include the vinyl benzyl ether compounds described in paragraph 0041 of Japanese Patent Application Publication No. 2019-194312, and the compounds described in paragraphs 0008-0032 of Japanese Patent No. 7551036 and paragraphs 0007-0057 of Japanese Patent No. 7530537, the contents of which are incorporated herein by reference.
[0402] In this embodiment, compounds of the inclusion formula (BV) are particularly exemplified as vinyl benzyl compounds. The inclusion formula (BV) compounds effectively suppress thermal expansion during the curing process.
[0403]
[0404] (In formula (BV), Md independently represents hydrocarbon groups with 1 to 12 carbon atoms. w represents an integer from 0 to 4. r represents an integer from 0 to 6.)
[0405] In formula (BV), Md independently represents a hydrocarbon group having 1 to 12 carbon atoms, preferably an alkyl group, more preferably a straight-chain alkyl group, and even more preferably methyl or ethyl.
[0406] In formula (BV), w is an integer from 0 to 4, preferably an integer from 0 to 3, more preferably an integer from 0 to 2, further preferably 0 or 1, and even more preferably 0.
[0407] In formula (BV), r is an integer from 0 to 6, preferably 1 or more, more preferably 2 or more, and preferably 5 or less, more preferably 4 or less, even more preferably 3 or less, and even more preferably 2 or less.
[0408] In this embodiment, the compound represented by formula (BV) is particularly preferred to be the following compound.
[0409]
[0410] In addition to the above, compounds with a vinyl phenyl group at the end as described in International Publication No. 2022 / 210095 (e.g., the compounds described in Synthesis Examples 12-16 of that publication), paragraphs 0029-0039 of Japanese Patent Application Publication No. 2022-85610, paragraphs 0023-0043 of Japanese Patent Application Publication No. 2024-107328, paragraphs 0022-0039 of Japanese Patent Application Publication No. 2024-7493, paragraphs 0010-0053 of Japanese Patent Application Publication No. 2024-139678, vinyl benzyl ether resins as described in paragraph 0041 of Japanese Patent Application Publication No. 2019-194312, and co-oligomers as described in paragraphs 0013-0027 of International Publication No. 2022 / 014599 may also be incorporated into this specification.
[0411] Relative to 100 parts by mass of the resin solids in the resin composition, the content of other compounds (compound (XC)) having terminal carbon-carbon unsaturated double bonds in the resin composition of this embodiment is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and may also be 15 parts by mass or more. Depending on the application, it may be 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more. By setting the content of other compounds (compound (XC)) having terminal carbon-carbon unsaturated double bonds at the above-mentioned lower limit value, there is a tendency to reduce the Df of the obtained cured product. In addition, the upper limit value of the content of other compounds (compound (XC)) having terminal carbon-carbon unsaturated double bonds at the resin composition is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 75 parts by mass or less, depending on the application, it may be 70 parts by mass or less, 65 parts by mass or less, or 55 parts by mass or less. By setting the content of other compounds (compound (XC)) with carbon-carbon unsaturated double bonds at the ends below the above-mentioned upper limit, there is a tendency to improve the formability of the resin composition and the heat resistance of the obtained cured product.
[0412] The resin composition of this embodiment may contain only one other compound (compound (XC)) having a carbon-carbon unsaturated double bond at the end, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0413] <<<Other aromatic resins with carbon-carbon double bonds at the ends>>>
[0414] In addition to the above, for aromatic resins having carbon-carbon double bonds at the ends, reference can be made to paragraphs 0011 to 0025 of International Publication No. 2023 / 176766, paragraphs 0012 to 0033 of International Publication No. 2023 / 176764, paragraphs 0012 to 0033 of International Publication No. 2023 / 176763, and paragraphs 0026 to 0043 of International Publication No. 2023 / 176765, the contents of which are incorporated herein by reference.
[0415] <<Cyanate Compounds>>
[0416] The resin composition of this embodiment may contain a cyanate ester compound. The cyanate ester compound in this embodiment is not particularly limited as long as it contains one or more (preferably two or more, more preferably two to twelve, further preferably two to six, even more preferably two to four, even more preferably two or three, even more preferably two) cyanate ester groups (cyanoxy groups) within one molecule; compounds commonly used in the field of printed circuit boards can be widely used. Furthermore, the cyanate ester compound is preferably a compound in which the cyanate ester group is directly bonded to an aromatic backbone (aromatic ring).
[0417] Preferred cyanate compounds in this embodiment include, for example, at least one selected from the group consisting of phenolic varnish-type cyanate compounds, naphthol aralkyl-type cyanate compounds (naphthol aralkyl-type cyanate), naphthyl ether-type cyanate compounds, biphenyl aralkyl-type cyanate compounds, xylene resin-type cyanate compounds, triphenol methane-type cyanate compounds, adamantane skeleton-type cyanate compounds, bisphenol M-type cyanate compounds, bisphenol A-type cyanate compounds, and diallyl bisphenol A-type cyanate compounds. From the viewpoint of further improving the low water absorption of the obtained cured product, at least one selected from the group consisting of phenolic varnish-type cyanate compounds, naphthol aralkyl-type cyanate compounds, naphthyl ether-type cyanate compounds, xylene resin-type cyanate compounds, bisphenol M-type cyanate compounds, bisphenol A-type cyanate compounds, and diallyl bisphenol A-type cyanate compounds is more preferred; at least one selected from the group consisting of phenolic varnish-type cyanate compounds and naphthol aralkyl-type cyanate compounds is even more preferred; and naphthol aralkyl-type cyanate compounds are even more preferred.
[0418] These cyanate compounds can be prepared using known methods or commercially available products. It should be noted that cyanate compounds with naphthol aralkyl, naphthyl ether, xylene, triphenol methane, or adamantane skeletons have a higher functional group equivalent number and fewer unreacted cyanate groups; therefore, cured resin compositions using these compounds tend to have superior low water absorption. Furthermore, primarily due to the presence of aromatic or adamantane skeletons, there is a tendency for further improved plating adhesion.
[0419] As a naphthol aralkyl cyanate compound, the compound shown in the following formula (1) is more preferred.
[0420]
[0421] (In equation (1), R) 3 Each can be used independently to represent a hydrogen atom or a methyl group, and n3 represents an integer greater than or equal to 1.
[0422] In equation (1), R 3 Each can be represented independently as a hydrogen atom or a methyl group, with hydrogen atom being preferred.
[0423] In formula (1), n3 is an integer of 1 or more, preferably an integer of 1 to 20, more preferably an integer of 1 to 10, and even more preferably an integer of 1 to 6.
[0424] Furthermore, there are no particular limitations on the phenolic varnish-type cyanate compound, but the compound shown in formula (VII) below is preferred.
[0425]
[0426] (In equation (VII), R) 6 Each can be used independently to represent a hydrogen atom or a methyl group, and n7 represents an integer greater than or equal to 1.
[0427] In equation (VII), R 6 Each can be represented independently as a hydrogen atom or a methyl group, with hydrogen atom being preferred.
[0428] In formula (VII), n7 is an integer of 1 or more, preferably an integer of 1 to 20, more preferably an integer of 1 to 10, and even more preferably an integer of 1 to 6.
[0429] As a bisphenol A type cyanate compound, one or more of the group consisting of prepolymers of 2,2-bis(4-cyanoxyphenyl)propane and 2,2-bis(4-cyanoxyphenyl)propane can be used.
[0430] The resin composition of this embodiment preferably contains a cyanate ester compound within a range that does not impair the effects of the present invention. When the resin composition of this embodiment contains a cyanate ester compound, the lower limit of its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 0.1 parts by mass or more, more preferably 2 parts by mass or more, further preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more. By making the content of the cyanate ester compound 0.1 parts by mass or more, there is a tendency for the resulting cured product to have improved heat resistance, flame resistance, chemical resistance, low dielectric properties (low relative permittivity, low dielectric loss tangent), and insulation. When the resin composition of this embodiment contains a cyanate ester compound, the upper limit of the content of the cyanate ester compound relative to 100 parts by mass of the resin solids in the resin composition is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, further preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less.
[0431] The resin composition in this embodiment may contain only one cyanate ester compound, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0432] <<(Methyl)allyl compounds>>
[0433] The resin composition of this embodiment may contain a (methyl)allyl compound. Preferably, the (methyl)allyl compound contains an allyl compound.
[0434] Furthermore, the (methyl)allyl compound is preferably a compound containing two or more (methyl)allyl groups, and more preferably a compound containing two or more allyl groups.
[0435] As a (methyl)allyl compound, it preferably comprises at least one selected from the group consisting of (methyl)allyl isocyanurate compounds, tri(methyl)allyl cyanurate compounds, (methyl)allyl-substituted nadicimide compounds, (methyl)allyl compounds having a glycourea structure, and diallyl phthalate; more preferably, it comprises at least one selected from the group consisting of (methyl)allyl isocyanurate compounds, (methyl)allyl-substituted nadicimide compounds, and (methyl)allyl compounds having a glycourea structure; even more preferably, it comprises (methyl)allyl isocyanurate compounds and / or (methyl)allyl-substituted nadicimide compounds; and even more preferably, it comprises (methyl)allyl-substituted nadicimide compounds.
[0436] Examples of cyanurate tri(methyl)allyl compounds include cyanurate tri(methyl)allyl compounds (e.g., cyanurate triallyl ester with the structure shown below).
[0437]
[0438] In addition, as (methyl)allyl compounds, examples of resins containing allyl groups described in International Publication No. 2022 / 210095 (such as the compounds described in Synthesis Examples 3, 4, 6, 20, and 22 of that publication) are incorporated herein by reference.
[0439] When the resin composition of this embodiment contains a (methyl)allyl compound, its molecular weight is preferably 195 or more, more preferably 300 or more, and can be 400 or more, 500 or more. By setting it to the aforementioned lower limit or above, there is a tendency to further improve low dielectric properties and heat resistance. The molecular weight of the (methyl)allyl compound is also preferably 3000 or less, more preferably 2000 or less, further preferably 1000 or less, and even more preferably 800 or less. By setting it to the aforementioned upper limit or below, there is a tendency to further improve low thermal expansion.
[0440] When the resin composition of this embodiment contains a (methyl)allyl compound, its content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and can be 10 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By setting the content of the (methyl)allyl compound to the above-mentioned lower limit value or above, there is a tendency for excellent formability and further improved heat resistance. In addition, the upper limit value of the content of the (methyl)allyl compound relative to 100 parts by mass of the resin solids in the resin composition is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less. By setting the content of the (methyl)allyl compound to the above-mentioned upper limit value or less, there is a tendency for further improved low thermal expansion.
[0441] The resin composition of this embodiment may contain only one (methyl)allyl compound, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0442] <<<(Methyl)allyl isocyanurate compounds>>>
[0443] There are no particular limitations on (methyl)allyl isocyanurate compounds, as long as they have two or more (methyl)allyl groups and an isocyanurate ring (triazacyclohexanetrione (Nurlat) skeleton). Because (methyl)allyl isocyanurate compounds have a large number of (methyl)allyl groups that serve as crosslinking points, they tend to cure firmly with aromatic resins, maleimide compounds, and other thermosetting compounds that have carbon-carbon double bonds at the ends, resulting in cured products with low dielectric properties (Dk and / or Df) and excellent heat resistance. Compounds with the formula (TA) are preferred as (methyl)allyl isocyanurate compounds.
[0444] Formula (TA)
[0445]
[0446] (In formula (TA), R A (Indicates substituent).
[0447] In formula (TA), R A The term indicates a substituent, more preferably a substituent with a formula weight of 15 to 500.
[0448] R A The first example is an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms. By using allyl compounds having 1 to 22 alkyl groups or 2 to 22 alkenyl groups, it is possible to provide resin compositions with excellent crosslinking properties and yield cured products with high toughness. Thus, even when the resin composition does not contain a substrate such as glass cloth, cracking during etching processes can be suppressed.
[0449] From the viewpoint of improving operability, the aforementioned alkyl and / or alkenyl groups preferably have 3 or more carbon atoms, more preferably 8 or more, further preferably 12 or more, and preferably 18 or less. Therefore, the resin composition exhibits better resin flowability, and the circuit filling properties, etc., are improved when using the resin composition of this embodiment to fabricate multilayer circuit boards, etc.
[0450] R A The second example is a group containing an allyl isocyanurate group. R A When containing an allyl isocyanurate group, the compound represented by formula (TA) is preferably the compound represented by formula (TA-1).
[0451] Formula (TA-1)
[0452]
[0453] (In formula (TA-1), R A2 (It is a divalent linker.)
[0454] In formula (TA-1), R A2 Preferably, it is a divalent linker with a formula weight of 54 to 250, more preferably a divalent linker with a formula weight of 54 to 250 and carbon atoms at both ends, and even more preferably an aliphatic hydrocarbon group with 2 to 20 carbon atoms (wherein, the aliphatic hydrocarbon group may include an ether group, and may also have a hydroxyl group). More specifically, R A2 Preferably, it is a group represented by any of the following formulas (i) to (iii).
[0455]
[0456] (In equations (i) to (iii), p) c1 The number of repeating units of the methylene group is an integer from 2 to 18. c2 Indicates the number of repeating units of the oxyethylidene group, which is 0 or 1. * indicates the bonding site.
[0457] The above p c1 Preferably, it is an integer from 2 to 10, more preferably an integer from 3 to 8, and even more preferably an integer from 3 to 5.
[0458] The above p c2 It can be 0 or 1, but 1 is preferred.
[0459] R A The third example is a phosphorus-based substituent.
[0460] R A2 The first example is preferred.
[0461] In this embodiment, the equivalent of the reactive group (allyl) in the compound represented by formula (TA) is preferably 1000 g / eq. or less. It is believed that if the aforementioned equivalent is 1000 g / eq. or less, a high Tg can be obtained more reliably.
[0462] Examples of alkyl groups having 1 to 22 carbon atoms include straight-chain or branched alkyl groups, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, and docosyl. Examples of alkenyl groups having 2 to 22 carbon atoms include allyl and decenyl.
[0463] Specific examples of compounds represented by formula (TA) include, for example, triallyl isocyanurate, 5-octyl-1,3-diallyl isocyanurate, 5-dodecyl-1,3-diallyl isocyanurate, 5-tetradecyl-1,3-diallyl isocyanurate, 5-hexadecyl-1,3-diallyl isocyanurate, 5-octadecyl-1,3-diallyl isocyanurate, 5-eicosyl-1,3-diallyl isocyanurate, 5-docodecyl-1,3-diallyl isocyanurate, and 5-decenyl-1,3-diallyl isocyanurate. They can be used alone or in combination of two or more, and can also be used in the form of prepolymers.
[0464] The method of manufacturing the compound shown in formula (TA) is not particularly limited. For example, it can be obtained by reacting diallyl isocyanurate with an alkyl halide in an aprotic polar solvent such as N,N'-dimethylformamide in the presence of alkaline substances such as sodium hydroxide, potassium carbonate, and triethylamine at a temperature of about 60°C to 150°C.
[0465] Alternatively, commercially available products can be used as the compounds represented by formula (TA). There are no particular limitations on commercially available products; examples include L-DAIC manufactured by Shikoku Chemical Industry Co., Ltd., and P-DAIC manufactured by Shikoku Chemical Industry Co., Ltd., which has phosphorus-based substituents. As a triallyl isocyanurate, TAIC manufactured by Shin-Mitsubishi Corporation can be cited as an example. As a compound represented by formula (TA-1), DD-1 manufactured by Shikoku Chemical Industry Co., Ltd. can be cited as an example.
[0466] The molecular weight of the (methyl)allyl isocyanurate compound (preferably the compound shown in formula (TA)) is preferably 200 or more, more preferably 300 or more, and can be 400 or more, or 500 or more. By setting the aforementioned molecular weight to the aforementioned lower limit or above, there is a tendency to further improve the low dielectric properties (Dk and / or Df) and heat resistance of the obtained cured product. Furthermore, the molecular weight of the (methyl)allyl isocyanurate compound (preferably the compound shown in formula (TA)) is preferably 3000 or less, more preferably 2000 or less, further preferably 1000 or less, and even more preferably 800 or less. By setting the aforementioned molecular weight to the aforementioned upper limit or below, there is a tendency to further improve the low thermal expansion properties of the obtained cured product.
[0467] When the resin composition of this embodiment contains a (methyl)allyl isocyanurate compound, its content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and can be 10 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By setting the content of the (methyl)allyl isocyanurate compound to the aforementioned lower limit or above, there is a tendency to further improve the formability of the resin composition, the heat resistance of the obtained cured product, and the low thermal expansion. In addition, the upper limit of the content of the (methyl)allyl isocyanurate compound relative to 100 parts by mass of the resin solids in the resin composition is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and can also be 20 parts by mass or less. By setting the content of the (methyl)allyl isocyanurate compound to the aforementioned upper limit or below, there is a tendency to further improve the heat resistance and low dielectric properties (Dk and / or Df) of the obtained cured product.
[0468] The resin composition of this embodiment may contain only one (methyl)allyl isocyanurate compound, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0469] <<<(Methyl)allyl-substituted nadicimide compounds>>>
[0470] As a (methyl)allyl-substituted nadicimide compound, there is no particular limitation as long as the molecule has two or more (methyl)allyl-substituted nadicimide groups. Specific examples include compounds represented by the following formula (AN-1).
[0471]
[0472] In formula (AN-1), R1 independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and R2 represents an alkylene group, phenylene group, biphenylene group, naphthylene group, or a group represented by formula (AN-2) or formula (AN-3) having 1 to 6 carbon atoms.
[0473]
[0474] (In formula (AN-2), R3 represents a group represented by methylene, isopropylidene, -C(=O)-, -O-, -S-, or -S(=O)2-.)
[0475]
[0476] (In formula (AN-3), R4 independently represents an alkylene group having 1 to 4 carbon atoms or a cycloalkylene group having 5 to 8 carbon atoms.)
[0477] In addition, the compound shown in formula (AN-1) may also be a commercially available product. There are no particular limitations on what constitutes a commercially available product; examples include the compound shown in formula (AN-4) (BANI-M (manufactured by Maruzen Petrochemical Co., Ltd.)) and the compound shown in formula (AN-5) (BANI-X (manufactured by Maruzen Petrochemical Co., Ltd.)). One or more of these compounds may be used.
[0478] Formula (AN-4)
[0479]
[0480]
[0481] The molecular weight of the (methyl)allyl-substituted nadicimide compound (preferably the compound shown in formula (AN)) is preferably 400 or more, more preferably 500 or more, and may also be 550 or more. Setting the molecular weight of the (methyl)allyl-substituted nadicimide compound to the aforementioned lower limit or above tends to further improve low dielectric properties, low thermal expansion, and heat resistance. The molecular weight of the (methyl)allyl-substituted nadicimide compound (preferably the compound shown in formula (AN)) is also preferably 1500 or less, more preferably 1000 or less, and even more preferably 800 or less, and may be 700 or less, or 600 or less. Setting the molecular weight of the (methyl)allyl-substituted nadicimide compound to the aforementioned upper limit or below tends to further improve formability and peel strength.
[0482] When the resin composition of this embodiment contains a (methyl)allyl-substituted nadicimide compound (preferably a compound represented by formula (AN)), its content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, further preferably 5 parts by mass or more, and can be 10 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By setting the content of the (methyl)allyl-substituted nadicimide compound to the aforementioned lower limit or above, there is a tendency to improve formability, low dielectric properties, low thermal expansion, and further improve heat resistance. In addition, the upper limit of the content of the (methyl)allyl-substituted nadicimide compound (preferably a compound represented by formula (AN)) relative to 100 parts by mass of the resin solids in the resin composition is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less, and can also be 20 parts by mass or less. By setting the content of the (methyl)allyl-substituted nadicimide compound to the aforementioned upper limit or less, there is a tendency to further improve formability and peel strength.
[0483] The resin composition of this embodiment may contain only one (methyl)allyl-substituted nadicimide compound, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0484] <<<Methyl)allylic compounds with a glycourea structure>>>
[0485] As for (methyl)allyl compounds with a glycourea structure, there are no particular limitations as long as the compound contains a glycourea structure and two or more (methyl)allyl groups. When a (methyl)allyl compound with a glycourea structure is compounded into a resin composition, the number of (methyl)allyl groups can be increased, i.e., the number of crosslinking points can be increased. Therefore, similar to (methyl)allyl isocyanurate compounds, when firmly cured with aromatic resins containing carbon-carbon double bonds at the ends, maleimide compounds, and other thermosetting compounds, there is a tendency to obtain cured products with low dielectric properties (Dk and / or Df) and excellent heat resistance.
[0486] In this embodiment, the (methyl)allyl compound having a glycourea structure is preferably a compound represented by formula (GU).
[0487] Formula (GU)
[0488]
[0489] (In formula (GU), R) 1 Each can be a hydrogen atom or a substituent, R. 1 At least two of them are groups containing (methyl)allyl groups. R 2 Each can be represented independently by a hydrogen atom, alkyl group, or aryl group.
[0490] In formula (GU), R 1 The preferred components are hydrogen atoms, alkyl groups having 1 to 5 carbon atoms, or alkenyl groups having 2 to 5 carbon atoms, preferably alkenyl groups having 2 to 5 carbon atoms, more preferably (methyl)allyl, and even more preferably allyl.
[0491] In formula (GU), R 1 Preferably, 3 or 4 of the groups are (methyl)allyl groups, more preferably 4 of the groups are (methyl)allyl groups.
[0492] In formula (GU), R 2 Each of the following is preferably a hydrogen atom, an alkyl group or a phenyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or a methyl group, and even more preferably two R groups. 2 It consists entirely of hydrogen atoms.
[0493] As a specific example of a compound represented by formula (GU), 1,3,4,6-tetraallylglycourea (in formula (GU), R...) can be cited.1 All are allyl, R 2 (A compound consisting entirely of hydrogen atoms).
[0494] (Methyl)allyl compounds having a glycourea structure can also be used commercially available products. As commercially available products, there are no particular limitations; for example, TA-G manufactured by Shikoku Chemical Industry Co., Ltd. can be cited.
[0495] The molecular weight of the (methyl)allyl compound having a glycourea structure (preferred to be the compound shown in formula (GU)) is preferably 195 or more, more preferably 220 or more, and even more preferably 250 or more, and can be 300 or more, or 400 or more. By setting the molecular weight of the (methyl)allyl compound having a glycourea structure to the aforementioned lower limit or above, there is a tendency to further improve the heat resistance and low thermal expansion of the obtained cured product. The molecular weight of the (methyl)allyl compound having a glycourea structure (preferred to be the compound shown in formula (GU)) is also preferably 1500 or less, more preferably 1000 or less, and even more preferably 800 or less, and can be 700 or less, or 600 or less. By setting the molecular weight of the (methyl)allyl compound having a glycourea structure to the aforementioned upper limit or below, there is a tendency to further improve the low dielectric properties (Dk and / or Df) and heat resistance of the obtained cured product.
[0496] When the resin composition of this embodiment contains a (methyl)allyl compound having a glycourea structure (preferred to be a compound represented by formula (GU)), its content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, further preferably 5 parts by mass or more, and can be 10 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By setting the content of the (methyl)allyl compound having a glycourea structure to the above-mentioned lower limit value or above, there is a tendency to further improve the formability of the resin composition and the heat resistance and low thermal expansion of the obtained cured product. In addition, the upper limit value of the content of the (methyl)allyl compound having a glycourea structure (preferred to be a compound represented by formula (GU)) relative to 100 parts by mass of the resin solids in the resin composition is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, further preferably 25 parts by mass or less, and can also be 20 parts by mass or less. By setting the content of the (methyl)allyl compound having a glycourea structure to the aforementioned upper limit value or below, there is a tendency to further improve the low dielectric properties (Dk and / or Df) of the obtained cured product.
[0497] The resin composition of this embodiment may contain only one (methyl)allyl compound having a glycourea structure, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0498] <<<(Meth)acrylate compounds>>>
[0499] The resin composition of this embodiment may contain a (meth)acrylate compound. It should be noted that, in this specification, the (meth)acrylate compound that also belongs to the category of polyphenylene ether compounds having carbon-carbon unsaturated double bonds at the ends is defined as a polyphenylene ether compound having carbon-carbon unsaturated double bonds at the ends.
[0500] The (meth)acrylate compound used in this embodiment can be a monofunctional (meth)acrylate compound containing one (meth)acryloyloxy group per molecule, or a polyfunctional (meth)acrylate compound containing two or more (meth)acryloyloxy groups per molecule. In this embodiment, a polyfunctional (meth)acrylate compound is preferred.
[0501] The polyfunctional (meth)acrylate compound used in this embodiment is preferably a compound having 3 to 5 (meth)acryloyloxy groups, more preferably a compound having 3 or 4 (meth)acryloyloxy groups, and even more preferably a compound having 3 (meth)acryloyloxy groups. The (meth)acrylate compound is preferably a compound having methacryloyloxy groups.
[0502] Polyfunctional (meth)acrylate compounds, due to the large number of (meth)acrylate groups that serve as crosslinking points, can be firmly cured with aromatic resins, maleimide compounds, and other thermosetting compounds that have carbon-carbon double bonds at the ends, resulting in cured products with low dielectric properties (Dk and / or Df) and excellent heat resistance. The compound shown in formula (MA) is preferred as a polyfunctional (meth)acrylate compound.
[0503] Formula (MA)
[0504]
[0505] (In formula (MA), R) 1 R represents a hydrogen atom or substituent. 2 Each can be used independently to represent a hydrogen atom or a methyl group.
[0506] In formula (MA), R 1 The substituent represents a hydrogen atom or a substituent, more preferably a substituent with a formula weight of 15 to 500, even more preferably a substituent with a formula weight of 15 to 300, even more preferably a substituent with a formula weight of 15 to 100, and even more preferably a substituent with a formula weight of 15 to 50.
[0507] R 1Preferably, the compound is a hydrocarbon group or (meth)acryloyloxy group, more preferably a hydrocarbon group having 22 or fewer carbon atoms, and even more preferably an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms. By using a compound having an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms, a resin composition with excellent crosslinking properties and high toughness can be provided. Therefore, even when the resin composition does not contain a substrate such as glass cloth, cracking during etching processes can be suppressed.
[0508] From the viewpoint of improving operability, the number of carbon atoms in the aforementioned alkyl and / or alkenyl groups is preferably 2 or more, but can be 8 or more, further can be 12 or more, or can be 18 or less. Therefore, the resin composition exhibits better resin flowability, and the circuit filling properties, etc., are improved when using the resin composition of this embodiment to fabricate multilayer circuit boards, etc.
[0509] In this embodiment, the (meth)acryloyl equivalent of the compound represented by formula (MA) is preferably 1000 g / eq. or less. If the aforementioned equivalent is 1000 g / eq. or less, there is a tendency to obtain a higher Tg more reliably. The lower limit of the (meth)acryloyl equivalent is, for example, 99 g / eq. or more.
[0510] As for the alkyl group having 1 to 22 carbon atoms, straight-chain alkyl groups having 1 to 22 carbon atoms or branched alkyl groups having 3 to 22 carbon atoms are preferred, and examples include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, docosyl, etc. Furthermore, as for the alkenyl group having 2 to 22 carbon atoms, alkenyl groups having 2 to 15 carbon atoms are preferred, and examples include allyl, decenyl, etc.
[0511] Specific examples of compounds represented by formula (MA) include trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol tetra(meth)acrylate, etc. They can be used alone or in combination of two or more, and can also be used in the form of prepolymers.
[0512] Alternatively, commercially available products can be used as the compound represented by formula (MA). There are no particular limitations on what constitutes a commercially available product; for example, "NK Ester TMPT" manufactured by Shin-Nakamura Chemical Industry Co., Ltd. can be cited as an example of a trimethylolpropane trimethacrylate.
[0513] The molecular weight of the polyfunctional (meth)acrylate compound is preferably 200 or more, more preferably 300 or more, and can be 330 or more, 400 or more, or 500 or more. By setting the aforementioned molecular weight to the aforementioned lower limit or above, there is a tendency to further improve the low dielectric properties (Dk and / or Df) and heat resistance of the obtained cured product. In addition, the molecular weight of the (meth)acrylate compound (preferably the compound shown in formula (MA)) is preferably 3000 or less, more preferably 2000 or less, more preferably 1000 or less, and even more preferably 800 or less. By setting the aforementioned molecular weight to the aforementioned upper limit or below, there is a tendency to further improve the low thermal expansion properties of the obtained cured product.
[0514] Regarding (meth)acrylate compounds, in addition to the above, reference may be made to resins having (meth)acryloyl groups as described in International Publication No. 2022 / 210095 (e.g., the compounds described in Synthesis Examples 5 and 21 of that publication), resins having (meth)acryloyl groups as described in Japanese Patent No. 6962507 (e.g., the compounds described in Examples 1 to 9), compounds described in paragraph 0049 of Japanese Patent Application Publication No. 2019-194312, and resins having (meth)acryloyl groups as described in paragraphs 0010 to 0096 of Japanese Patent Application Publication No. 2024-159338, the contents of which are incorporated herein by reference.
[0515] When the resin composition of this embodiment contains a (meth)acrylate compound, its content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and can be 10 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By setting the content of the (meth)acrylate compound to the above-mentioned lower limit or above, there is a tendency to further improve the formability of the resin composition, the heat resistance of the obtained cured product, and the low thermal expansion. In addition, the upper limit of the content of the (meth)acrylate compound relative to 100 parts by mass of the resin solids in the resin composition is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and can also be 20 parts by mass or less. By setting the content of the (meth)acrylate compound to the aforementioned upper limit or less, there is a tendency to further improve the heat resistance and low dielectric properties (Dk and / or Df) of the obtained cured product.
[0516] The resin composition of this embodiment may contain only one (meth)acrylate compound, or it may contain two or more. When two or more compounds are contained, the total amount is preferably within the range described above.
[0517] <<Epoxy Compounds>>
[0518] The resin composition of this embodiment may contain an epoxy compound.
[0519] There are no particular limitations on the type of epoxy compound, as long as it is a compound or resin having one or more epoxy groups in one molecule (preferably 2 to 12, more preferably 2 to 6, further preferably 2 to 4, even more preferably 2 or 3, and even more preferably 2). It can be widely used in the field of printed circuit boards.
[0520] Examples of the aforementioned epoxy compounds include: phenolic varnish-type epoxy resins, bisphenol A phenolic varnish-type epoxy resins, glycidyl ester-type epoxy resins, aralkylphenolic varnish-type epoxy resins, biphenyl aralkyl-type epoxy resins, naphthyl ether-type epoxy resins, cresol phenolic varnish-type epoxy resins, polyfunctional phenolic epoxy resins, naphthyl-type epoxy resins, anthracene-type epoxy resins, naphthalene skeleton-modified phenolic varnish-type epoxy resins, phenolic aralkyl-type epoxy resins, naphtholic aralkyl-type epoxy resins, dicyclopentadiene-type epoxy resins, biphenyl-type epoxy resins, alicyclic epoxy resins, polyol-type epoxy resins, phosphorus-containing epoxy resins, glycidylamines, glycidyl esters, compounds obtained by epoxidizing double bonds of butadiene, etc., and compounds obtained by reacting hydroxyl-containing organosilicon resins with epichlorohydrin, etc. Using these compounds improves the formability and adhesion of the resin composition. From the viewpoint of further improving flame retardancy and heat resistance, the epoxy compound is preferably selected from one or more of the group consisting of biphenyl aryl epoxy resin, naphthalene ether epoxy resin, polyfunctional phenolic epoxy resin and naphthalene epoxy resin, and more preferably biphenyl aryl epoxy resin.
[0521] When the resin composition of this embodiment contains an epoxy compound, its content is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By making the epoxy compound content 0.1 parts by mass or more, there is a tendency to improve the peel strength and toughness of the metal foil. The upper limit of the epoxy compound content relative to 100 parts by mass of the resin solids in the resin composition is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, and may also be 8 parts by mass or less, or 5 parts by mass or less. By making the epoxy compound content 50 parts by mass or less, there is a tendency to improve the electrical properties of the resulting cured product.
[0522] The resin composition in this embodiment may contain only one epoxy compound, or it may contain two or more. When it contains two or more epoxy compounds, the total amount is preferably within the range described above.
[0523] Furthermore, the resin composition in this embodiment can also be formulated to be substantially free of epoxy compounds. "Substantially free" means that, relative to 100 parts by weight of the resin solids in the resin composition, the content of epoxy compounds is less than 0.1 parts by weight, preferably less than 0.01 parts by weight, and further less than 0.001 parts by weight.
[0524] <<Phenolic Compounds>>
[0525] The resin composition of this embodiment may contain phenolic compounds.
[0526] Phenolic compounds are not particularly limited as long as they are compounds that have one or more phenolic hydroxyl groups in one molecule (preferably 2 to 12, more preferably 2 to 6, even more preferably 2 to 4, even more preferably 2 or 3, even more preferably 2), and can be widely used in the field of printed circuit boards.
[0527] Examples of the aforementioned phenolic compounds include phenolic varnish resins, bisphenol A type phenolic varnish resins, glycidyl ester type phenolic resins, aralkyl phenolic varnish resins, biphenyl aralkyl type phenolic resins, cresol phenolic varnish resins, polyfunctional phenolic resins, naphthol resins, naphthol phenolic varnish resins, polyfunctional naphthol resins, anthracene type phenolic resins, naphthalene skeleton modified phenolic varnish resins, phenolic aralkyl type phenolic resins, naphthol aralkyl type phenolic resins, dicyclopentadiene type phenolic resins, biphenyl type phenolic resins, alicyclic phenolic resins, polyol type phenolic resins, phosphorus-containing phenolic resins, and hydroxyl-containing organosilicon resins. From the viewpoint of further improving the flame retardancy of the obtained cured product, it is preferable to select at least one from the group consisting of biphenyl aralkyl type phenolic resins, naphthol aralkyl type phenolic resins, phosphorus-containing phenolic resins, and hydroxyl-containing organosilicon resins.
[0528] In addition, as for phenolic compounds, reference can be made to paragraphs 0012 to 0025 of International Publication No. 2023 / 176765, the contents of which are incorporated herein by reference.
[0529] When the resin composition of this embodiment contains a phenolic compound, its content relative to 100 parts by weight of the resin solids in the resin composition is preferably 0.1 parts by weight or more, more preferably 1 part by weight or more, and even more preferably 2 parts by weight or more. Furthermore, it is preferably 50 parts by weight or less, more preferably 30 parts by weight or less, even more preferably 20 parts by weight or less, and even more preferably 10 parts by weight or less, and may also be 5 parts by weight or less.
[0530] The resin composition in this embodiment may contain only one phenolic compound, or it may contain two or more. When it contains two or more, the total amount is preferably within the range described above.
[0531] Furthermore, the resin composition in this embodiment can also be formulated to be substantially free of phenolic compounds. "Substantially free" means that the content of phenolic compounds is less than 0.1 parts by mass relative to 100 parts by mass of the resin solids in the resin composition.
[0532] <<Oxycyclic Butane Compounds>>
[0533] The resin composition of this embodiment may contain an oxetane compound.
[0534] Oxycyclic butane compounds are not particularly limited as long as they have one or more (preferably 2 to 12, more preferably 2 to 6, further preferably 2 to 4, even more preferably 2 or 3, and even more preferably 2) oxycyclic butyl groups, and can be widely used in the field of printed circuit boards.
[0535] Examples of oxetane compounds include oxetane, alkyloxetanes (e.g., 2-methyloxetane, 2,2-dimethyloxetane, 3-methyloxetane, 3,3-dimethyloxetane, etc.), 3-methyl-3-methoxymethyloxetane, 3,3-bis(trifluoromethyl)oxetane, 2-chloromethyloxetane, 3,3-bis(chloromethyl)oxetane, biphenyl-type oxetane, OXT-101 (manufactured by TOAGOSEI CO.,LTD.), OXT-121 (manufactured by TOAGOSEI CO.,LTD.), etc.
[0536] The resin composition of this embodiment preferably contains an oxetane compound within a range that does not impair the effects of the present invention. When the resin composition of this embodiment contains an oxetane compound, its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more. By making the content of the oxetane compound 0.1 parts by mass or more, there is a tendency to improve the peel strength and toughness of the metal foil of the obtained cured product. When the resin composition of this embodiment contains an oxetane compound, the upper limit of the content of the oxetane compound relative to 100 parts by mass of the resin solids in the resin composition is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, and even more preferably 8 parts by mass or less. By making the content of the oxetane compound 50 parts by mass or less, there is a tendency to improve the electrical properties of the obtained cured product.
[0537] The resin composition in this embodiment may contain only one oxetane compound, or it may contain two or more. When it contains two or more compounds, the total amount is preferably within the range described above.
[0538] Furthermore, the resin composition in this embodiment can also be formulated to be substantially free of oxetane compounds. "Substantially free" means that the content of oxetane compounds is less than 0.1 parts by weight relative to 100 parts by weight of the resin solids in the resin composition.
[0539] <<Benzoxazine Compounds>>
[0540] The resin composition of this embodiment may contain benzoxazine compounds.
[0541] As a benzoxazine compound, there is no particular limitation as long as it is a compound having two or more (preferably 2 to 12, more preferably 2 to 6, further preferably 2 to 4, even more preferably 2 or 3, and even more preferably 2) dihydrobenzoxazine rings in one molecule, and it can be widely used in the field of printed circuit boards.
[0542] Examples of benzoxazine compounds include bisphenol A type benzoxazine BA-BXZ (manufactured by Konishi Chemical Co., Ltd.), bisphenol F type benzoxazine BF-BXZ (manufactured by Konishi Chemical Co., Ltd.), and bisphenol S type benzoxazine BS-BXZ (manufactured by Konishi Chemical Co., Ltd.).
[0543] The resin composition of this embodiment preferably contains a benzoxazine compound within a range that does not impair the effects of the present invention. When the resin composition of this embodiment contains a benzoxazine compound, its content is preferably 0.1 parts by weight or more, and preferably 50 parts by weight or less, relative to 100 parts by weight of the resin solids in the resin composition.
[0544] The resin composition in this embodiment may contain only one benzoxazine compound, or it may contain two or more. When it contains two or more compounds, the total amount is preferably within the range described above.
[0545] Alternatively, the resin composition in this embodiment can also be formulated to be substantially free of benzoxazine compounds. "Substantially free" means that the content of benzoxazine compounds is less than 0.1 parts by weight per 100 parts by weight of the resin solids in the resin composition.
[0546] <<Compounds containing vinylidene>>
[0547] The resin composition of this embodiment may contain compounds having vinylidene content.
[0548] Examples of compounds having vinylidene properties include compounds containing one or more -CH=CH- groups in their molecules, with compounds containing one -CH=CH- group being preferred. Furthermore, compounds that are both vinylidene compounds and maleimide compounds are designated as maleimide compounds.
[0549] Specific examples of compounds having vinylidene content include acenaphthene and pyracylene, with acenaphthene being more preferred.
[0550] In this specification, as with the imidazole compounds described above, compounds that are also compounds having vinylidene properties, but are explicitly stated as components other than compounds having vinylidene properties (e.g., free radical polymerization initiators), are defined as compounds that do not have vinylidene properties.
[0551] Flame retardants
[0552] The resin composition of this embodiment may contain a flame retardant. Examples of flame retardants include phosphorus-based flame retardants, halogen-based flame retardants, inorganic flame retardants, and organosilicon-based flame retardants, with phosphorus-based flame retardants being preferred.
[0553] As flame retardants, known flame retardants can be used, such as: brominated epoxy resins, brominated polycarbonates, brominated polystyrene, brominated styrene, brominated phthalimide, tetrabromobisphenol A, pentabromobenzyl (meth)acrylate, pentabromotoluene, tribromophenol, hexabromobenzene, decabromodiphenyl ether, bis-1,2-pentabromophenyl ethane, chlorinated polystyrene, chlorinated paraffin and other halogenated flame retardants; phosphorus-containing flame retardants such as red phosphorus; tricresyl phosphate, triphenyl phosphate, 2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, toluene diphenyl phosphate, tri(xyl) phosphate, trialkyl phosphate, dialkyl phosphate, tri(chloroethyl) phosphate. Monomer-type phosphate esters; phosphorus-based flame retardants such as phosphazenes, phenoxyphosphazenes, 1,3-phenylenebis[2,6-di(dimethyl)phosphate], bis(diphenyl)phosphine oxide-based dimethylbis(diphenyl)phosphine oxide, phosphate ester-based condensed phosphate esters of di(dimethyl)phosphine, 6H-dibenzo[c,e][1,2]oxaphosphazene-6,6'-[1,4-phenylenebis(methylene)]bis-6,6'-dioxide, and phosphine-based dialkylphosphine aluminum salts of phosphine metal salts; inorganic flame retardants such as aluminum hydroxide, magnesium hydroxide, some boehmite, zinc borate, and antimony trioxide; and organosilicon-based flame retardants such as organosilicon rubber and organosilicon resin.
[0554] In this embodiment, 1,3-phenylenebis(2,6-bis(di(xylyl)phosphate) does not impair the low dielectric properties (Dk and / or Df), and is therefore preferred.
[0555] When the resin composition of this embodiment contains a flame retardant, the content of the flame retardant is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and preferably 30 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less.
[0556] Flame retardants can be used alone or in combination of two or more. When using two or more, the total amount shall be within the range mentioned above.
[0557] <Active Ester Compounds>
[0558] The resin composition of this embodiment may contain an active ester compound without impairing the effects of the present invention. There are no particular limitations on the active ester compound; for example, reference can be made to paragraphs 0064-0066 of International Publication No. 2021 / 172317, the contents of which are incorporated herein by reference.
[0559] When the resin composition of this embodiment contains an active ester compound, it is preferably 1 part by mass or more, and more preferably 50 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition.
[0560] The resin composition in this embodiment may contain only one active ester compound, or it may contain two or more. When it contains two or more, the total amount is preferably within the range described above.
[0561] Furthermore, the resin composition in this embodiment can also be formulated to be substantially free of active ester compounds. "Substantially free" means that the content of active ester compounds is less than 1 part by weight relative to 100 parts by weight of the resin solids in the resin composition, preferably less than 0.1 parts by weight, and more preferably less than 0.01 parts by weight.
[0562] <Dispersant>
[0563] The resin composition of this embodiment may contain a dispersant. As a dispersant, it is preferable to use a dispersant commonly used in coatings, and there is no particular limitation on its type. The dispersant is preferably a wetting dispersant of the copolymer matrix; specific examples include BYK Japan KK's DISPERBYK (registered trademark) - 110, 111, 161, 180, 2009, 2152, 2155, BYK (registered trademark) - W996, W9010, W903, W940, etc.
[0564] When the resin composition of this embodiment contains a dispersant, the lower limit of its content is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and may also be 0.3 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. Furthermore, the upper limit of the dispersant content is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and may also be 3 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition.
[0565] Dispersants can be used alone or in combination of two or more. When using two or more, the total amount shall be within the range mentioned above.
[0566] Solvent
[0567] The resin composition of this embodiment may contain a solvent, preferably an organic solvent. When containing a solvent, the resin composition of this embodiment is in a form (solution or varnish) in which at least a portion, preferably all, of the above-mentioned solid resin components are dissolved or compatible with the solvent. As a solvent, there are no particular limitations as long as it is a polar or non-polar organic solvent capable of dissolving or compatibility with at least a portion, preferably all, of the above-mentioned solid resin components. Examples of polar organic solvents include ketones (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), cellosols (e.g., propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, etc.), esters (e.g., ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, isoamyl acetate, ethyl lactate, methyl methoxypropionate, methyl hydroxyisobutyrate, etc.), and amides (e.g., dimethoxyacetamide, dimethylformamide, etc.). Examples of non-polar organic solvents include aromatic hydrocarbons (e.g., toluene, xylene, etc.).
[0568] Solvents may be used alone or in combination of two or more. When using two or more solvents, the total amount shall be within the range described above.
[0569] <Curing Accelerator>
[0570] The resin composition of this embodiment may further include a curing accelerator.
[0571] As a curing accelerator, there are no particular limitations. Examples include imidazoles such as 2-ethyl-4-methylimidazolium, 2-phenyl-4-methylimidazolium, and triphenylimidazolium; organic peroxides such as benzoyl peroxide, lauroyl peroxide, acetyl peroxide, p-chlorobenzoyl peroxide, di-tert-butyldisperoxyphthalate, α,α'-di(tert-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3; azobisonitriles (e.g., azobisisobutyronitrile), 2,2-azobis(2,4,4-trimethylpentane), and N,N-dimethylbenzylamine, N,N-dimethylaniline, and N,N-dimethyltoluidine. Tertiary amines such as 2-N-ethylaniline ethanol, tri-n-butylamine, pyridine, quinoline, N-methylmorpholine, triethanolamine, triethylenediamine, tetramethylbutyldiamine, and N-methylpiperidine; phenols such as phenol, xylenol, cresol, resorcinol, and catechol; high-temperature decomposition free radical generators such as 2,3-dimethyl-2,3-diphenylbutane; organometallic salts such as lead naphthenate, lead stearate, zinc naphthenate, zinc octanoate, manganese octanoate, tin oleate, dibutyltin maleate, manganese naphthenate, cobalt naphthenate, and iron acetylacetone; substances formed by dissolving these organometallic salts in phenol, bisphenol, and other hydroxyl-containing compounds; inorganic metal salts such as tin chloride, zinc chloride, and aluminum chloride; organotin compounds such as dioctyltin oxide, other alkyltin, and alkyltin oxide. The preferred curing accelerator is at least one selected from the group consisting of imidazoles, organometallic salts and organic peroxides, more preferably at least one selected from the group consisting of imidazoles and organic peroxides, and even more preferably an organic peroxide.
[0572] When the resin composition of this embodiment includes a curing accelerator, the lower limit of its content relative to 100 parts by weight of the resin solids in the resin composition is preferably 0.005 parts by weight or more, more preferably 0.01 parts by weight or more, further preferably 0.05 parts by weight or more, and even more preferably 0.08 parts by weight or more. Furthermore, the upper limit of the content of the curing accelerator relative to 100 parts by weight of the resin solids in the resin composition is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, further preferably 3 parts by weight or less, even more preferably 2 parts by weight or less, even more preferably 1.0 parts by weight or less, even more preferably 0.8 parts by weight or less, even more preferably 0.5 parts by weight or less, particularly preferably 0.3 parts by weight or less, and depending on the application, it can be 0.2 parts by weight or less, or 0.15 parts by weight or less. The resin composition of this embodiment is preferred in that it can fully cure the resin composition even when the content of the curing accelerator is set to the above-mentioned upper limit value.
[0573] Curing accelerators can be used alone or in combination of two or more. When using two or more, the total amount shall be within the range mentioned above.
[0574] <Filling Material>
[0575] The resin composition of this embodiment may include filler materials. By including filler materials, the dielectric properties (relative permittivity and / or dielectric loss tangent), flame retardancy, low thermal expansion, and other physical properties of the resin composition and its cured product can be further improved.
[0576] Furthermore, the filling material used in this embodiment preferably exhibits excellent low dielectric properties (Dk and / or Df). For example, the relative permittivity (Dk) of the filling material used in this embodiment at a frequency of 10 GHz, measured according to the cavity resonator perturbation method, is preferably 8.0 or less, more preferably 6.0 or less, and even more preferably 4.0 or less. Additionally, the lower limit of the relative permittivity is, for example, actually 2.0 or more. Furthermore, the dielectric loss tangent (Df) of the filling material used in this embodiment at a frequency of 10 GHz, measured according to the cavity resonator perturbation method, is preferably 0.05 or less, more preferably 0.01 or less. Additionally, the lower limit of the dielectric loss tangent is, for example, actually 0.0001 or more.
[0577] The type of filler material used in this embodiment is not particularly limited, and filler materials commonly used in the art can be used appropriately. Specifically, examples include: natural silica, fused silica, synthetic silica, amorphous silica, fumed silica (AEROSIL), hollow silica, and other silica; metal oxides such as alumina, white carbon, titanium dioxide, titanium oxide, zinc oxide, magnesium oxide, and zirconium oxide; composite oxides such as zinc borate, zinc stannate, forsterite, barium titanate, strontium titanate, and calcium titanate; nitrides such as boron nitride, condensed boron nitride, silicon nitride, and aluminum nitride; and metal hydroxides such as aluminum hydroxide, heat-treated aluminum hydroxide (aluminum hydroxide that has had a portion of its water of crystallization removed by heat treatment), boehmite, and magnesium hydroxide (including hydrated aluminum hydroxide). Inorganic filler materials include: molybdenum oxide, zinc molybdate, and other molybdenum compounds; barium sulfate, clay, kaolin, talc, calcined clay, calcined kaolin, calcined talc, mica, E-glass, A-glass, NE-glass, NER-glass, C-glass, L-glass, D-glass, S-glass, M-glass G20, glass short fibers (including E-glass, T-glass, D-glass, S-glass, Q-glass, and other glass micropowders), insulated glass, spherical glass, etc. Organic filler materials also include styrene-type, butadiene-type, acrylic-type rubber powders, core-shell rubber powders, silicone resin powders, silicone rubber powders, silicone composite powders, etc.
[0578] In this embodiment, inorganic filler materials are preferred, and more preferably, they include one or more selected from the group consisting of silica, aluminum hydroxide, talc, aluminum nitride, boron nitride, magnesium olivine, titanium oxide, barium titanate, strontium titanate, and calcium titanate. From the viewpoint of low dielectric properties (Dk and / or Df), it is more preferable that they include one or more selected from the group consisting of silica and aluminum hydroxide, and even more preferably, they include silica. By using these inorganic filler materials, the heat resistance, dielectric properties, thermal expansion properties, dimensional stability, flame retardancy, and other properties of the cured resin composition are further improved.
[0579] The content of filler material in the resin composition of this embodiment can be appropriately set according to the desired characteristics and is not particularly limited. It is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. Depending on the application, it can be 30 parts by mass or more, 50 parts by mass or more, 100 parts by mass or more, or 120 parts by mass or more. By setting it to the aforementioned lower limit or above, there is a tendency for the obtained cured product to have better low thermal expansion and low dielectric loss tangent. Furthermore, the upper limit of the filler material content relative to 100 parts by mass of the resin solids in the resin composition is preferably 300 parts by mass or less, more preferably 250 parts by mass or less, even more preferably 200 parts by mass or less, and even more preferably 180 parts by mass or less. Depending on the application, it can be 150 parts by mass or less, or 100 parts by mass or less. By setting it to the aforementioned upper limit or below, there is a tendency for the formability of the resin composition to be further improved.
[0580] In the resin composition of this embodiment, as an example of a preferred embodiment, the content of the filler material can be 1 to 95% by mass of the components other than the solvent, preferably 10% to 50% by mass, and more preferably 10% to 30% by mass.
[0581] The resin composition of this embodiment may contain only one filler material, or it may contain two or more fillers. When two or more fillers are contained, the total amount is preferably within the range described above.
[0582] In the resin composition of this embodiment, when a filler material, particularly an inorganic filler material, is used, a silane coupling agent may be further included. By including a silane coupling agent, there is a tendency to further improve the dispersibility of the filler material and the adhesion strength between the resin component and the filler material and the substrate described later.
[0583] As a silane coupling agent, there is no particular limitation, and examples of silane coupling agents commonly used in the surface treatment of inorganic materials include aminosilane compounds (e.g., γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, etc.), epoxysilane compounds (e.g., γ-epoxypropoxypropyltrimethoxysilane, etc.), vinylsilane compounds (e.g., vinyltrimethoxysilane, vinyltriethoxysilane, tetravinylsilane, triethylvinylsilane, 1,3-vinyltetramethylsiloxane, etc.), styrylsilane compounds (e.g., 4-vinylphenyltrimethoxysilane, etc.), acrylic silane compounds (e.g., γ-acryloyloxypropyltrimethoxysilane, etc.), cationic silane compounds (e.g., N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride, etc.), phenylsilane compounds, etc. Preferably, it comprises at least one selected from the group consisting of vinyl silane compounds, styrene silane compounds, and acrylic silane compounds, more preferably vinyl silane compounds. The silane coupling agent can be used alone or in combination of two or more.
[0584] The content of the silane coupling agent is not particularly limited, but can be 0.1 to 5.0 parts by weight relative to 100 parts by weight of the solid resin component in the resin composition.
[0585] <Elastomers>
[0586] The resin composition of this embodiment may contain an elastomer. The elastomer may be thermoplastic, thermosetting, or neither thermoplastic nor thermosetting, but is preferably thermoplastic.
[0587] The elastomer used in this embodiment is not particularly limited, and examples include at least one selected from the group consisting of polyisoprene, polybutadiene, styrene-butadiene, butyl rubber, ethylene-propylene rubber, styrene-butadiene-ethylene, styrene-butadiene-styrene, styrene-isoprene-styrene, styrene-ethylene-butene-styrene, styrene-propylene-styrene, styrene-ethylene-propylene-styrene, fluororubber, silicone rubber, their hydrides, their alkyl compounds, and their copolymers.
[0588] In addition, examples of elastomers include oligomers or polymers with curable vinyl functional groups described in paragraphs 0044 and 0045 of Japanese Patent Application Publication No. 2019-194312, and polybutadiene resins are also included in this specification.
[0589] The number-average molecular weight of the elastomer (preferably a thermoplastic elastomer) used in this embodiment is preferably 1000 or more. By having a number-average molecular weight of 1000 or more, the resulting cured product tends to have superior low dielectric properties (Dk and / or Df, especially low dielectric loss tangent). The number-average molecular weight is preferably 1500 or more, more preferably 2000 or more, and depending on the application, it can be 600,000 or more, 700,000 or more, or 800,000 or more. The upper limit of the number-average molecular weight of the elastomer is preferably 400,000 or less, more preferably 350,000 or less, and even more preferably 300,000 or less. By setting it below the aforementioned upper limit, there is a tendency for the solubility of the elastomer component in the resin composition to increase.
[0590] When the resin composition of this embodiment contains two or more elastomers, it is preferable that the number average molecular weight of their mixture satisfies the above-mentioned range.
[0591] The elastomer used in this embodiment can be a resin comprising a polybutadiene structure. Optionally, some or all of the polybutadiene structure is hydrogenated. Specific examples include Nippon Soda Corporation's B-1000, B-2000, B-3000, BI-2000, BI-3000, CRAY VALLEY Corporation's Ricon100, Ricon130, Ricon131, Ricon142, Ricon150, Ricon181, Ricon184, etc.
[0592] The elastomer used in this embodiment can be a resin having a poly(meth)acrylate structure. Specific examples include Teisan Resin manufactured by Nagase ChemteX, and ME-2000, W-197C, KG-15, and KG-3000 manufactured by Negami Kogyo Co., Ltd.
[0593] The elastomer used in this embodiment can be a resin having a polycarbonate structure. Sometimes, a resin having a polycarbonate structure is referred to as a "polycarbonate resin." Examples of such resins include carbonate resins without reactive groups, hydroxyl-containing carbonate resins, phenolic hydroxyl-containing carbonate resins, carboxyl-containing carbonate resins, acid anhydride-containing carbonate resins, isocyanate-containing carbonate resins, urethane-containing carbonate resins, and epoxy-containing carbonate resins. Here, "reactive group" refers to functional groups such as hydroxyl, phenolic hydroxyl, carboxyl, acid anhydride, isocyanate, urethane, and epoxy groups that can react with other components.
[0594] Specific examples of polycarbonate resins include FPC0220 and FPC2136 manufactured by Mitsubishi Gas Chemical Co., Ltd., and T6002 and T6001 (polycarbonate diol) manufactured by Asahi Kasei Corporation.
[0595] The elastomers used in this embodiment can be resins having a polysiloxane structure. Specific examples include SMP-2006, SMP-2003PGMEA, SMP-5005PGMEA, KR-510, and SMP-7014-3S manufactured by Shin-Etsu Chemical Industry Co., Ltd.
[0596] Examples of elastomers used in this embodiment include resins having a polyalkylene structure and / or a polyalkylene oxide structure. The polyalkylene oxide structure is preferably a polyalkylene oxide structure with 2 to 15 carbon atoms, more preferably a polyalkylene oxide structure with 3 to 10 carbon atoms, and particularly preferably a polyalkylene oxide structure with 5 to 6 carbon atoms. Specific examples of resins having a polyalkylene structure and / or a polyalkylene oxide structure include PTXG-1000 and PTXG-1800 manufactured by Asahi Kasei Corporation.
[0597] The elastomer used in this embodiment can be a resin having a polyisoprene structure. Specific examples include KL-610 and KL613 manufactured by Kuraray.
[0598] The elastomer used in this embodiment can be a resin having a polyisobutylene structure. Specific examples include SIBSTAR-073T (styrene-isobutylene-styrene triblock copolymer) and SIBSTAR-042D (styrene-isobutylene diblock copolymer) manufactured by Kaneka Corporation.
[0599] In this embodiment, the elastomer is preferably an elastomer comprising styrene monomer units and conjugated diene monomer units (hereinafter referred to as "elastomer (e)"). By using such an elastomer (e), the low dielectric properties (Dk and / or Df, especially low dielectric loss tangent) of the cured product are superior.
[0600] The elastomer (e) described above comprises styrene monomer units. By comprising styrene monomer units, the solubility of elastomer (e) in resin compositions is improved. Examples of styrene monomers include styrene, α-methylstyrene, p-methylstyrene, divinylbenzene (vinylstyrene), N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene, among which styrene, α-methylstyrene, and p-methylstyrene are preferred from the viewpoint of availability and productivity. Styrene is particularly preferred.
[0601] The content of styrene monomer units in the elastomer (e) described above is preferably 10% by mass or more of all monomer units, more preferably 13% by mass or more, even more preferably 15% by mass or more, and preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less. By keeping the content of styrene monomer units below the aforementioned upper limit, the adhesion and bonding properties with the substrate, etc., become better. In addition, if the content of styrene monomer units is above the aforementioned lower limit, adhesion enhancement can be suppressed, residue and stop marks are less likely to occur, and there is a tendency for the adhesive surfaces to peel off easily, which is therefore preferred.
[0602] The elastomer (e) may contain only one type of styrene monomer unit, or it may contain two or more types. When it contains two or more types, the total amount is preferably within the range described above.
[0603] The method for determining the content of styrene monomer units in the elastomer (e) of this embodiment can be found in International Publication No. 2017 / 126469, the contents of which are incorporated herein by reference. The same applies to conjugated diene monomer units, etc., which will be described later.
[0604] The elastomer (e) described above comprises a conjugated diene monomer unit. By comprising a conjugated diene monomer unit, the solubility of the elastomer (e) in the resin composition is improved. As a conjugated diene monomer, there is no particular limitation as long as it is a diene having a pair of conjugated double bonds. Examples of conjugated diene monomers include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, and farnesene, with 1,3-butadiene and isoprene being preferred, and 1,3-butadiene being more preferred.
[0605] The elastomer (e) may contain only one conjugated diene monomer unit or more than two.
[0606] In the elastomer (e) described above, the mass ratio of styrene monomer units to conjugated diene monomer units is preferably in the range of 5 / 95 to 80 / 20, more preferably in the range of 7 / 93 to 77 / 23, and even more preferably in the range of 10 / 90 to 70 / 30. When the mass ratio of styrene polymer units to conjugated diene monomer units is in the range of 5 / 95 to 80 / 20, adhesion enhancement can be suppressed and high adhesive strength can be maintained, resulting in good peelability between the bonded surfaces.
[0607] The elastomer (e) mentioned above can be one in which all the conjugated diene bonds of the elastomer are hydrogenated, or only some of them are hydrogenated, or they can be unhydrogenated.
[0608] The elastomer (e) described above may or may not contain other monomer units besides styrene monomer units and conjugated diene monomer units. Examples of other monomer units include aromatic vinyl compound units other than styrene monomer units.
[0609] The elastomer (e) preferably has a total of styrene monomer units and conjugated diene monomer units of 90% or more by mass of all monomer units, more preferably 95% or more by mass, even more preferably 97% or more by mass, and even more preferably 99% or more by mass.
[0610] As described above, the elastomer (e) may contain only one styrene monomer unit and one conjugated diene monomer unit, or it may contain two or more. When it contains two or more, the total amount is preferably within the range described above.
[0611] The elastomer (e) used in this embodiment can be a block polymer or a random polymer. Alternatively, it can be a hydrogenated elastomer in which the conjugated diene monomer unit is hydrogenated, an unhydrogenated elastomer, or a partially hydrogenated elastomer, preferably an unhydrogenated or partially hydrogenated elastomer.
[0612] In one embodiment of this invention, the elastomer (e) is a hydrogenated elastomer. Here, a hydrogenated elastomer refers to, for example, a material in an elastomer whose double bonds based on conjugated diene monomer units are hydrogenated, including materials with a hydrogenation rate of 80% or more, in addition to materials with a hydrogenation rate of 100%. The hydrogenation rate of the hydrogenated elastomer is preferably 85% or more, more preferably 90% or more, and even more preferably 95% or more. In this embodiment, the hydrogenation rate is determined by… 1 The results of H-NMR spectroscopy were calculated.
[0613] In one embodiment of this invention, the elastomer (e) is an unhydrogenated elastomer. Here, an unhydrogenated elastomer refers to one in which the proportion of hydrogenated double bonds in the double bonds based on conjugated diene monomer units, i.e., the hydrogenation rate, is 20% or less. The hydrogenation rate is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less.
[0614] On the other hand, partially hydrogenated elastomers refer to elastomers in which a portion of the double bond based on the conjugated diene monomer unit is hydrogenated, typically referring to elastomers with a hydrogenation rate of less than 80% and greater than 20%.
[0615] Commercially available products that can be used as elastomers (e) in this embodiment include SEPTON (registered trademark) 2104, V9461, S8104 manufactured by Kuraray Co., Ltd.; SOE (registered trademark) S1606, S1613, S1609, S1605 manufactured by Asahi Kasei Corporation; H1041, H1043, P2000, MP10 manufactured by Tuftec (registered trademark) manufactured by Asahi Kasei Corporation; and DYNARON (registered trademark) 9901P, TR2250 manufactured by JSR Co., Ltd.
[0616] The elastomer used in this embodiment can also be a liquid diene. A liquid diene refers to a liquid elastomer containing conjugated diene monomer units. Examples of conjugated diene monomers include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, and farnesene, with 1,3-butadiene and isoprene being preferred, and 1,3-butadiene being more preferred.
[0617] Examples of liquid dienes used in this embodiment include liquid polybutadiene, liquid polyisoprene, modified liquid polybutadiene, modified liquid polyisoprene, a copolymer of liquid acrylonitrile-butadiene, and a copolymer of liquid styrene-butadiene.
[0618] Furthermore, there are no particular limitations on the number-average molecular weight of the liquid diene, as long as it is liquid at 20°C, but it is preferably 500 or more and 10,000 or less.
[0619] The elastomer used in this embodiment can also be the elastomer described in Japanese Patent Application Publication No. 2022-33057. For example, Kraton Corporation's MD3501 can be used as such a commercially available product.
[0620] When the resin composition of this embodiment includes an elastomer (preferably including elastomer (e)), its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 8 parts by mass or more. Depending on the application, it can be 10 parts by mass or more, or 12 parts by mass or more. By setting it to the aforementioned lower limit or above, there is a tendency to further improve the dielectric properties (low dielectric loss tangent). In addition, the upper limit of the elastomer content relative to 100 parts by mass of the resin solids in the resin composition is preferably 45 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 35 parts by mass or less, even more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less. Depending on the application, it can be 20 parts by mass or less, or 15 parts by mass or less. By setting it to the aforementioned upper limit or below, there is a tendency to further improve the heat resistance.
[0621] The resin composition of this embodiment may contain only one type of elastomer, or it may contain two or more types. When it contains two or more types, the total amount is preferably within the range described above.
[0622] Furthermore, the resin composition in this embodiment can also be formulated to be substantially free of elastomers. "Substantially free" means that the content of elastomers is less than 1 part by weight relative to 100 parts by weight of the resin solids in the resin composition, preferably less than 0.1 parts by weight, and more preferably less than 0.01 parts by weight.
[0623] <Other Ingredients>
[0624] In addition to the components described above, the resin composition of this embodiment may also contain various polymeric compounds such as thermoplastic resins and their oligomers, petroleum resins, and various additives. Examples of additives include at least one selected from the group consisting of ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, flow modifiers, lubricants, defoamers, leveling agents, gloss agents, and polymerization inhibitors.
[0625] Examples of polymerization inhibitors include quinones, phenols, nitroso compounds, hydroxylamines, organoboronic acid compounds, and compounds with phenolic hydroxyl groups. Specifically, examples include 2-nitrophenol, 4-methoxyphenol, 4-tert-butylcatechol, pyrogallol, tert-butylhydroquinone, 1,4-benzoquinone, 2-hydroxybenzophenone, cuprous chloride, phenothiazine, tetrachlorobenzoquinone, naphthylamine, β-naphthol, 2,6-di-tert-butyl-4-cresol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), pyridine, nitrobenzene, dinitrobenzene, picric acid, 4-toluidine, methylene blue, reaction products of copper with organic chelating agents, methyl salicylate, dibutylhydroxytoluene, 1,1-diphenyl-2-picrylhydrazyl free radical, hydroquinone, hydroquinone monomethyl ether, methanol, N-nitroso-N-phenylhydroxylamine aluminum, triethyl borate, tributyl borate, triisopropyl borate, 2,3-dihydroxynaphthalene, 4-methoxy-1-naphthol, methylhydroquinone, etc. Furthermore, the polymerization inhibitors used are not limited to those mentioned above.
[0626] Furthermore, the resin composition of this embodiment can also be formulated to be substantially free of free radical polymerization initiators (including initiators that are photopolymerization initiators and initiators that are curing accelerators). "Substantially free" means that the content of free radical polymerization initiators contained in the resin composition is less than 0.005 parts by weight relative to 100 parts by weight of the resin solids, preferably less than 0.003 parts by weight, more preferably less than 0.001 parts by weight, and even more preferably less than 0.0001 parts by weight.
[0627] In the resin composition of this embodiment, the total content of the polyphenylene ether compound other than that described in the above-mentioned <<<polyphenylene ether compound having carbon-carbon unsaturated double bonds at the ends>>> and the thermoplastic elastomer other than that described in the above-mentioned <elastomer> section is preferably 3% by mass or less of the resin solids content, more preferably 1% by mass or less. By setting it in this way, the effects of the present invention can be exerted more effectively.
[0628] Furthermore, the total content of polyphenylene ether compounds other than those described in the above-mentioned <<<polyphenylene ether compounds having carbon-carbon unsaturated double bonds at the ends>>> and butadiene-based elastomers without a styrene backbone is preferably 3% by mass or less, more preferably 1% by mass or less, of the resin solids content. With this configuration, the effects of the present invention can be more effectively achieved.
[0629] Furthermore, the total content of the polyphenylene ether compound other than the polyphenylene ether compound shown in formula (OP) and the butadiene-based elastomer without a styrene backbone is preferably 3% by mass or less of the resin solids content, more preferably 1% by mass or less. By setting it in this way, the effects of the present invention can be more effectively exerted.
[0630] <Application>
[0631] The resin composition of this embodiment is used in the form of a cured product. Specifically, the resin composition of this embodiment is suitable for use as a resin composition for electronic materials such as materials with low relative permittivity and / or low dielectric loss tangent, insulating layers for printed circuit boards, and materials for semiconductor packaging. The resin composition of this embodiment is suitable for use as a prepreg, a metal-clad laminate using prepreg, a resin composite sheet, and a material for printed circuit boards.
[0632] The resin composition of this embodiment preferably has a low relative permittivity (Dk) and dielectric loss tangent (Df) of its cured product.
[0633] When the resin composition of this embodiment is formed into a cured plate (without metal foil) with a thickness of 1.0 mm, the relative permittivity (Dk) at a frequency of 10 GHz, measured by the cavity resonator perturbation method, is preferably 2.50 or less. There is no particular requirement for the lower limit of the relative permittivity (Dk), but it is typically 0.01 or more. Furthermore, the dielectric loss tangent (Df) at a frequency of 10 GHz, measured by the cavity resonator perturbation method when the cured plate (without metal foil) is formed into a cured plate with a thickness of 1.0 mm, is preferably 0.0020 or less, more preferably 0.0015 or less. There is no particular limitation on the lower limit of the dielectric loss tangent (Df), but it is typically 0.0001 or more. Alternatively, the resin composition can be cured using free radical curing. Free radical curing tends to cure rapidly within a specific temperature range, thus allowing for a more dense curing of the resin composition and further improving the low dielectric properties (Dk and / or Df) of the resulting cured product. That is, one example of the resin composition in this embodiment is a free radical curable resin composition.
[0634] The dielectric loss tangent (Df) and relative permittivity (Dk) of the above-mentioned cured material were determined more specifically by the methods described in the embodiments described later.
[0635] In addition, the resin composition of this embodiment preferably has a low coefficient of thermal expansion when it is cured.
[0636] When the resin composition of this embodiment is formed into a cured plate (without metal foil) with a thickness of 1.0 mm, the thermal expansion rate measured at 260°C to 280°C is preferably 200 ppm / °C or less, more preferably 160 ppm / °C or less, and even more preferably 100 ppm / °C or less. In fact, it is 0 ppm / °C or more.
[0637] In addition, when measuring the same sample at 50°C to 280°C as described above, the coefficient of thermal expansion is preferably 100 ppm / °C or less, more preferably 70 ppm / °C or less, and in practice, it is 0 ppm / °C or more.
[0638] In addition, the resin composition of this embodiment preferably has a high glass transition temperature (Tanσ) when it is cured.
[0639] When the resin composition of this embodiment is molded into a cured plate (without metal foil) with a thickness of 1.0 mm, the glass transition temperature (Tanδ) measured according to JIS C6481 5.17.2 using a dynamic viscoelasticity measuring device (DMA) is preferably 250°C or higher. The upper limit of the above-mentioned glass transition temperature (Tanδ) is not particularly limited, for example, it is 400°C or lower.
[0640] The resin composition of this embodiment is used as a prepreg, resin composite sheet, or other layered material (including film, sheet, etc.) that serves as an insulating layer for a printed circuit board. When producing this layered material, its thickness is preferably 5 μm or more, more preferably 10 μm or more. As an upper limit for thickness, it is preferably 200 μm or less, more preferably 180 μm or less. It should be noted that the thickness of the layered material mentioned above, for example, when the resin composition of this embodiment is impregnated with glass cloth, refers to the thickness including the glass cloth.
[0641] The material formed from the resin composition of this embodiment can be used for pattern formation by exposure and development, or for applications without exposure and development. It is particularly suitable for applications without exposure and development.
[0642] <<Prepreg>>
[0643] The prepreg of this embodiment is formed from a substrate (prepreg substrate) and the resin composition of this embodiment. The prepreg of this embodiment is obtained, for example, by applying the resin composition of this embodiment to the substrate (e.g., impregnation and / or coating), and then semi-curing it by heating (e.g., drying at 120-220°C for 2-15 minutes). At this time, the amount of resin composition adhering to the substrate, i.e., the amount of resin composition (including filler material) relative to the total amount of the semi-cured prepreg, is preferably in the range of 20-99% by mass, more preferably in the range of 20-80% by mass.
[0644] There are no particular limitations on the substrate material, as long as it is used in various printed circuit board materials. Examples of substrate materials include glass fibers (such as E-glass, D-glass, L-glass, S-glass, T-glass, Q-glass, UN-glass, NE-glass, NER-glass, spherical glass, etc.), inorganic fibers other than glass (such as quartz), and organic fibers (such as polyimide, polyamide, polyester, liquid crystal polyester, polytetrafluoroethylene, etc.). There are no particular limitations on the form of the substrate, and examples include woven fabrics, non-woven fabrics, rovings, chopped strand mats, and surface-treated mats. These substrates can be used alone or in combination of two or more. Among these substrates, from the viewpoint of dimensional stability, woven fabrics with super-opening fiber treatment and mesh blocking treatment are preferred; from the viewpoint of strength and low water absorption, substrates with a thickness of 200 μm or less and a weight of 250 g / m³ are preferred. 2 From the viewpoint of moisture absorption and heat resistance, the following glass fabrics are preferably surface-treated with epoxy silane, amino silane, etc. From the viewpoint of electrical properties, low-dielectric glass cloths formed of glass fibers exhibiting low relative permittivity and low dielectric loss tangent, such as L-glass, NE-glass, NER-glass, and Q-glass, are more preferred.
[0645] Examples of substrates with low relative permittivity include those with a relative permittivity of 5.0 or less (preferably 3.0 to 4.9). Examples of substrates with low dielectric loss tangent include those with a dielectric loss tangent of 0.006 or less (preferably 0.001 to 0.005). The relative permittivity and dielectric loss tangent are set as values measured using a perturbation method cavity resonator at a frequency of 10 GHz.
[0646] <<Metal Foil-Coated Laminates>>
[0647] The metal-clad laminate of this embodiment comprises at least one layer formed from the prepreg of this embodiment and metal foil disposed on one or both sides of the layer formed from the prepreg. As a method for manufacturing the metal-clad laminate of this embodiment, for example, a method can be described by disposing of at least one sheet of the prepreg of this embodiment (preferably overlapping two or more sheets) and depositing metal foil on one or both sides thereon to form a laminate. More specifically, it can be manufactured by depositing metal foil such as copper or aluminum on one or both sides of the prepreg and then laminating them. The number of prepreg sheets is preferably 1 to 10 sheets, more preferably 2 to 10 sheets, and even more preferably 2 to 9 sheets.
[0648] As for the metal foil, there is no particular limitation as long as it is used as a material for printed circuit boards; examples include rolled copper foil, electrolytic copper foil, and other copper foils. The thickness of the metal foil (preferably copper foil) is not particularly limited and can be approximately 1.5 to 70 μm. Furthermore, when using copper foil as the metal foil, it is preferable to adjust the surface roughness Rz of the copper foil, as measured according to JIS B0601:2013, to be 0.2 to 4.0 μm. By setting the surface roughness Rz of the copper foil to 0.2 μm or more, the surface roughness of the copper foil becomes an appropriate value, and there is a tendency to further improve the peel strength of the copper foil. On the other hand, by setting the surface roughness Rz of the copper foil to 4.0 μm or less, the surface roughness of the copper foil becomes an appropriate value, and there is a tendency to further improve the dielectric loss tangent characteristics of the obtained cured product. From the viewpoint of the dielectric loss tangent characteristics of the obtained cured product and the peel strength of the copper foil, the surface roughness Rz of the copper foil is more preferably 0.5 μm or more, further preferably 0.6 μm or more, particularly preferably 0.7 μm or more, and even more preferably 3.5 μm or less, further preferably 3.0 μm or less, and particularly preferably 2.0 μm or less.
[0649] As a method for lamination forming, methods commonly used in forming laminates and multilayer boards for printed circuit boards can be cited. More specifically, methods using multi-stage presses, multi-stage vacuum presses, continuous forming machines, autoclave forming machines, etc., to perform lamination forming under conditions of approximately 180-350°C, heating time of approximately 100-300 minutes, and surface pressure of approximately 1-10 MPa can be cited. Alternatively, multilayer boards can also be manufactured by combining the prepreg of this embodiment with separately manufactured wiring boards for inner layers and laminating them. As a method for manufacturing multilayer boards, for example, copper foil of approximately 35 μm is disposed on both sides of a sheet of prepreg of this embodiment, and after lamination forming using the above forming method, an inner layer circuit is formed. This circuit is then blackened to form an inner layer circuit board. Then, this inner layer circuit board and the prepreg of this embodiment are alternately disposed one sheet at a time, and copper foil is disposed on the outermost layer. Lamination forming is performed under the above conditions, preferably under vacuum, thereby producing a multilayer board. The metal-clad laminate of this embodiment is suitable for use as a printed circuit board.
[0650] The peel strength of the metal-clad foil laminate of this embodiment, measured according to section 5.7 "Peel Strength" of JIS C6481, is preferably 0.30 kN / m or more, more preferably 0.35 kN / m or more, and even more preferably 0.50 kN / m or more. There is no particular limitation on the upper limit of the peel strength; for example, even 2.00 kN / m or less is sufficient to meet the required performance.
[0651] As described above, the electronic material resin composition obtained by using the resin composition of this embodiment (a resin composition containing a combination of specific components) can have the following properties after curing: low dielectric properties (low dielectric constant, low dielectric loss tangent), low thermal expansion, heat resistance, excellent appearance of the cured product, moisture absorption and heat resistance, peel strength to metal foil, resistance to adhesive residue removal, crack resistance, and excellent high-density processability.
[0652] Printed Circuit Boards
[0653] The printed circuit board of this embodiment is a printed circuit board comprising an insulating layer and a conductor layer disposed on the surface of the aforementioned insulating layer. The aforementioned insulating layer comprises at least one of a layer formed from the resin composition of this embodiment and a layer formed from the prepreg of this embodiment. Such a printed circuit board can be manufactured according to conventional methods, and the manufacturing method is not particularly limited. Hereinafter, an example of a method for manufacturing a printed circuit board is shown. First, a copper-clad laminate or a metal-clad laminate as described above is prepared. Next, the surface of the metal-clad laminate is etched to form inner layer circuits, thus creating an inner layer substrate. On the surface of the inner layer circuits of the inner layer substrate, a surface treatment is performed as needed to improve the adhesion strength. Then, the required number of the aforementioned prepregs are stacked on the surface of the inner layer circuits, and then metal foils for outer layer circuits are stacked on the outside of them. The substrate is then heated and pressed to integrally form the circuit. In this way, a multilayer laminate in which a substrate and an insulating layer formed from a cured resin composition are formed between the metal foils for inner and outer layer circuits is manufactured. Next, after drilling holes for through holes and vias on the multi-layered laminate, a plated metal film is formed on the wall of the hole to conduct the metal foil used for inner layer circuits and outer layer circuits. Then, the metal foil used for outer layer circuits is etched to form the outer layer circuits, thereby manufacturing a printed circuit board.
[0654] The printed circuit board obtained in the above manufacturing example has an insulating layer and a conductor layer formed on the surface of the insulating layer. The insulating layer is composed of the resin composition of this embodiment and / or its cured form. That is, the layer formed by the prepreg of this embodiment (for example, a prepreg formed from a substrate and the resin composition of this embodiment impregnated or coated thereon) and the resin composition of the metal foil laminate of this embodiment becomes the insulating layer of this embodiment.
[0655] Furthermore, this embodiment also relates to a semiconductor device including the aforementioned printed circuit board. Detailed information about the semiconductor device can be found in paragraphs 0200-0202 of Japanese Patent Application Publication No. 2021-021027, and this information is incorporated herein by reference.
[0656] Furthermore, the insulating layer formed from the cured resin composition of this embodiment preferably has a reduced surface roughness after the roughening treatment. Specifically, the arithmetic mean roughness Ra of the surface of the roughened insulating layer is preferably 200 nm or less, more preferably 150 nm or less, and particularly preferably 100 nm or less. The lower limit of the arithmetic mean roughness Ra is not particularly limited, and for example, it can be 10 nm or more. The arithmetic mean roughness Ra of the surface of the insulating layer is measured using a non-contact surface roughness meter, in VSI mode, with a 50x lens.
[0657] The non-contact surface roughness meter used is the Veeco Instruments WYKONT3300.
[0658] <<Resin Composite Sheet>>
[0659] The resin composite sheet of this embodiment includes a support and a layer formed of the resin composition of this embodiment disposed on the surface of the support. The resin composite sheet can be used as an additive film or a dry film solder resist. There are no particular limitations on the manufacturing method of the resin composite sheet; for example, a method can be described by coating a solution obtained by dissolving the resin composition of this embodiment in a solvent onto a support and then drying it to obtain the resin composite sheet.
[0660] Examples of supports used here include polyethylene film, polypropylene film, polycarbonate film, polyethylene terephthalate film, ethylene tetrafluoroethylene copolymer film, and release films with release agents coated on the surface of these films, organic film substrates such as polyimide film, conductor foils such as copper foil and aluminum foil, glass plates, SUS (Steel Use Stainless) plates, FRP (Fiber-Reinforced Plastics) and other plate-shaped supports, without particular limitation.
[0661] As a coating method, examples include applying a solution obtained by dissolving the resin composition of this embodiment in a solvent onto a support using a bar coater, die coater, doctor blade, Baker applicator, etc. Alternatively, after drying, the support can be peeled off or etched from the resin composite sheet on which the support and resin composition are stacked, thereby producing a single-layer sheet. It should be noted that by supplying the solution obtained by dissolving the resin composition of this embodiment in a solvent to a mold having a sheet-like cavity and drying it, a single-layer sheet can also be obtained without using a support.
[0662] It should be noted that in the fabrication of the single-layer sheet or resin composite sheet in this embodiment, the drying conditions for solvent removal are not particularly limited. If the temperature is low, the solvent is likely to remain in the resin composition; if the temperature is high, the resin composition will cure. Therefore, it is preferable to perform the drying process at a temperature of 20°C to 200°C for 1 to 90 minutes. Furthermore, the single-layer sheet or resin composite sheet can be used in an uncured state where only the solvent has been dried, or it can be used in a semi-cured (B-stage) state as needed. Moreover, the thickness of the resin layer in the single-layer sheet or resin composite sheet of this embodiment can be adjusted by the concentration of the solution of the resin composition of this embodiment used in the coating process and the coating thickness, and is not particularly limited. Generally, when the coating thickness is too thick, solvent is likely to remain during drying; therefore, a thickness of 0.1 to 500 μm is preferred.
[0663] Example
[0664] The following examples illustrate the present invention in more detail. The materials, amounts, proportions, processing contents, and processing steps shown in the following examples can be appropriately modified without departing from the spirit of the invention. Therefore, the scope of protection of the present invention is not limited to the specific examples shown below.
[0665] If the measuring instruments used in the embodiments are difficult to obtain due to production stoppages or other reasons, other instruments with equivalent performance can be used for measurement.
[0666] <Determination of weight-average molecular weight and number-average molecular weight>
[0667] The weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the compounds (including resins) were determined by gel permeation chromatography (GPC). A standard curve based on monodisperse polystyrene was prepared using a pump (Shimadzu Corporation LC-20AD), a differential refractive index detector (Shimadzu Corporation RID-20A), a GPC column (Showa Denko Corporation GPC KF-801, 802, 803, 804), tetrahydrofuran as solvent, at a flow rate of 1.0 mL / min and a column temperature of 40 °C.
[0668] <Determination of parameters α and β>
[0669] The parameters α and β in resin (A) are obtained through 1 The H-NMR determination yielded the results. The synthesized resin was dissolved in a mixed solvent of heptane and methanol, and the process of drying was repeated to remove residual solvent from the recovered solid. Then, the recovered solid was dissolved in CDCl3 (containing 0.03 vol% TMS (tetramethylsilane)) for further processing. 1 H-NMR determination. During the determination... 1The parameters α and β of each resin were calculated using the formulas shown below in ¹H-NMR. The peak position of TMS (tetramethylsilane) was set to 0 ppm.
[0670] [Mathematical Expression 4]
[0671]
[0672] (The parentheses in equations (α) and (β) indicate) 1 (The integral value between the corresponding chemical shift values in H-NMR.)
[0673] <Synthesis Example 1: Synthesis of Resin (A1)>
[0674] In a flask equipped with a thermometer and a cooling tube, 520 g of toluene, 0.75 g of activated clay, 150 g of 1,3-diisopropenylbenzene (manufactured by Tokyo Chemical Co., Ltd.), and a stir bar were added. The mixture was heated to an internal temperature of 50°C while stirring. Then, it was slowly heated to an internal temperature of 70°C over 5 hours, and the reaction was carried out at 70°C for another hour. After natural cooling, the activated clay was removed by filtration, and the solvent was removed by distillation under heating and reduced pressure, thereby obtaining 129 g of solid resin.
[0675] The obtained resin (A) has a Mw of 1193, a Mn of 693, and a Mw / Mn ratio of 1.7. In formula (Tx), the parameters α and β are 0.63, β, and n+o+p, respectively, and 3.4. All structures within parentheses in formulas (a), (b), and (c) of (Tx) have the same molecular weight. The Mn of the synthesized resin is assumed to be the average molecular weight, and n+o+p is calculated. Furthermore, GPC analysis confirmed that the residual monomer content is less than 1% by mass.
[0676] For the obtained resin (A1), Figure 1 The middle shows 1 H-NMR spectrum.
[0677] <Synthesis Example 2: Synthesis of Resin (A2)>
[0678] In a flask equipped with a thermometer, a Dean-Stark apparatus, and a stirrer, 184.5 g of m-bis(α-hydroxyisopropyl)benzene (product name Meta-diol, manufactured by Sumitomo Chemical Co., Ltd.), 125 g of toluene, 0.12 g of p-toluenesulfonic acid monohydrate, and 0.4 g of pure water were added. The mixture was heated to an internal temperature of 120°C while nitrogen was introduced, and the reaction was carried out for 4 hours. A dehydration reaction produced 1,3-diisopropenylbenzene (34.1 g of water was removed, approximately the same as the theoretical amount). After natural cooling, 300 g of toluene and 200 g of pure water were added. The mixture was repeatedly washed with 200 g of pure water until the waste liquid became neutral, thus obtaining the product in solution form. The system was concentrated under reduced pressure to obtain 300 g of a toluene solution containing 1,3-diisopropenylbenzene.
[0679] Add 260g of toluene and 1.5g of activated clay to a flask equipped with a thermometer, cooling pipe, and stirrer. Heat the flask to an internal temperature of 70°C while stirring. Then, control the dropping rate by adding 150g of the toluene solution containing 1,3-diisopropenylbenzene, as described above, while keeping the internal temperature below 80°C. After the addition, stir until the internal temperature drops to 70°C. Then, similarly, add 150g of the toluene solution containing 1,3-diisopropenylbenzene, and allow the reaction to continue for 1.5 hours after the addition is complete. At the end of the reaction, add 400g of toluene and remove the solids by filtration.
[0680] The filtrate was distilled under reduced pressure to remove the solvent, yielding 123 g of solid resin. The obtained resin (A2) had a Mw of 1980, a Mn of 890, and a Mw / Mn ratio of 2.2. In formula (Tx), parameter α was 0.66, parameter β was 0.78, and n+o+p was 4.6. All structures within parentheses in formulas (a), (b), and (c) of (Tx) had the same molecular weight. The Mn of the synthesized resin was assumed to be the average molecular weight, and n+o+p was calculated. Furthermore, GPC analysis confirmed that the residual monomer content was less than 1% by mass. The functional group equivalent (isopropenyl equivalent) of the obtained resin (A2) was 571 g / eq. The functional group equivalent (g / eq.) of resin (A2) was calculated by (number-average molecular weight (Mn) ÷ 2) ÷ β.
[0681] <Synthesis Example 3: Synthesis of Resin (A3)>
[0682] In a flask equipped with a thermometer, a Dean-Stark apparatus, and a stirrer, 184.5 g of m-bis(α-hydroxyisopropyl)benzene (product name Meta-diol, manufactured by Sumitomo Chemical Co., Ltd.), 125 g of toluene, 0.12 g of p-toluenesulfonic acid monohydrate, and 0.4 g of pure water were added. The mixture was heated to an internal temperature of 120°C while nitrogen was introduced, and the reaction was carried out for 4 hours. A dehydration reaction produced 1,3-diisopropenylbenzene (34.1 g of water was removed, approximately the same as the theoretical amount). After natural cooling, 300 g of toluene and 200 g of pure water were added. The mixture was repeatedly washed with 200 g of pure water until the waste liquid became neutral, thus obtaining the product in solution form. The system was concentrated under reduced pressure to obtain 300 g of a toluene solution containing 1,3-diisopropenylbenzene.
[0683] In a flask equipped with a thermometer, cooling tube, and stirrer, 130 g of toluene, 0.3 g of activated clay, and 300 g of the aforementioned toluene solution containing 1,3-diisopropenylbenzene were added. The mixture was heated to an internal temperature of 50°C while stirring. Then, it was slowly heated to an internal temperature of 80°C over 5 hours, and the reaction was carried out at 80°C for another hour. After natural cooling, the catalyst was removed by filtration, and the solvent was removed by distillation under heating and reduced pressure, thereby obtaining 129 g of solid resin.
[0684] The obtained resin (A3) has a molecular weight (Mw) of 1380, a molecular weight (Mn) of 710, and a Mw / Mn ratio of 1.9. In formula (Tx), the parameters α and β are 0.81, β is 0.88, and n+o+p is 3.5. All structures within parentheses in formulas (a), (b), and (c) of Tx have the same molecular weight. The Mn of the synthesized resin is assumed to be the average molecular weight, and n+o+p is calculated. Furthermore, GPC analysis confirmed that the residual monomer content is less than 1% by mass. The functional group equivalent (isopropenyl equivalent) of the obtained resin (A3) is 403 g / eq. The functional group equivalent (g / eq.) of resin (A3) is calculated by (number-average molecular weight (Mn) ÷ 2) ÷ β.
[0685] Example 1
[0686] The resin (A1) and resin (B1) (manufactured by K. Chemical Industry Co., LTD., BMI-70) obtained in Synthesis Example 1 above were dissolved and mixed using methyl ethyl ketone and toluene to obtain a varnish. The mixing amounts of the above components are expressed as values based on the amount of solids.
[0687] <Preparation of test pieces for 1.0mm thick cured boards>
[0688] The solvent was evaporated from the obtained varnish to obtain a resin composition powder. Using the obtained resin composition powder, a cured board was made as follows: 4.5g of the resin composition powder was spread in a stainless steel mold with a height of 100mm × 30mm × 1.0mm, placed in a vacuum press (manufactured by Kitagawa Seiki Co., Ltd.), and pressed at 200°C for 2 hours with a surface pressure of 3.0MPa.
[0689] The obtained cured plates were used to evaluate the relative permittivity (Dk), dielectric loss tangent (Df), coefficient of thermal expansion (CTE), and glass transition temperature (Tg). The evaluation results are shown in the table below.
[0690] <Determination Methods and Evaluation Methods>
[0691] <Dielectric Properties>
[0692] The resulting cured plate was reduced to a width of 1.0 mm and then dried at 120°C for 60 minutes. For the dried sample, the relative permittivity (Dk) and dielectric loss tangent (Df) were measured at a frequency of 10 GHz using a perturbation method cavity resonator. The measurement temperature was set to 23°C.
[0693] The measurement results will be evaluated as follows.
[0694] The perturbation method cavity resonator used is the P5005A manufactured by Keysight Technology.
[0695] <<Relative Permittivity (Dk)>>
[0696] A: Below 2.50
[0697] B: Greater than 2.50
[0698] <<Dielectric Loss Tangent (Df)>>
[0699] A: Below 0.0015
[0700] B: Greater than 0.0015 and less than 0.0020
[0701] C: Greater than 0.0020
[0702] Coefficient of linear thermal expansion (CTE)
[0703] For the sample obtained by reducing the above-mentioned cured plate (cured at 200°C) to 3.0 mm square, the coefficient of thermal expansion was determined by TMA (Thermo-Mechanical Analysis) according to JIS C 6481 5.19, and its value was calculated. The unit is expressed in ppm / °C.
[0704] The thermomechanical analysis apparatus used was a TMAQ400 manufactured by TA Instruments Japan Inc. The temperature was increased from 25°C to 303°C at a rate of 10°C per minute, then cooled, and then increased again from 25°C to 303°C for measurement. The measurement results are evaluated as follows. α² represents the coefficient of thermal expansion between 260 and 280°C. 总 It represents the coefficient of thermal expansion from 50 to 280℃.
[0705] The measurement results will be evaluated as follows.
[0706] (α2)
[0707] A: Below 100ppm / ℃
[0708] B: Greater than 100 ppm / ℃ and less than 160 ppm / ℃
[0709] C: Greater than 160 ppm / ℃ and less than 200 ppm / ℃
[0710] D: Greater than 200ppm / ℃
[0711] (α) 总 )
[0712] A: Below 70ppm / ℃
[0713] B: Greater than 70 ppm / ℃ and less than 100 ppm / ℃
[0714] C: Greater than 100ppm / ℃
[0715] Glass transition temperature (Tg)
[0716] For the sample obtained by reducing the above-mentioned cured plate to 12.7mm × 30mm, the glass transition temperature was measured using a dynamic viscoelasticity measuring device according to JIS C6481 5.17.2 via the DMA (Dynamic Mechanical Analysis) bending method. The peak temperature of the loss tangent (Tanδ) was taken as the glass transition temperature. The unit is expressed in °C.
[0717] The dynamic viscoelasticity analysis apparatus used was the DMA 850, manufactured by TA Instruments Japan Inc.
[0718] The measurement results will be evaluated as follows.
[0719] A: Above 250℃
[0720] B: Less than 250℃
[0721] C: The device broke during testing, making measurement impossible.
[0722] Example 2
[0723] In Example 1, the content of resin (A1) was changed to 50 parts by mass, and the content of resin (B1) was changed to 50 parts by mass, and the same procedure was followed otherwise.
[0724] Example 3
[0725] In Example 1, the content of resin (A1) was changed to 60 parts by mass and the content of resin (B1) was changed to 40 parts by mass, and the same procedure was followed otherwise.
[0726] Example 4
[0727] In Example 1, 1 part by weight of 2-nitrophenol (polymerization inhibitor, manufactured by Tokyo Chemical Industry Co., Ltd.) was added, and the same procedure was followed otherwise.
[0728] Example 5
[0729] In Example 1, the content of resin (A1) was changed to 29 parts by mass, the content of resin (B1) was changed to 57 parts by mass, and 13 parts by mass of 1,2-bis(4-vinylphenyl)ethane (manufactured by Angene International) was added, and the same procedure was performed otherwise.
[0730] Example 6
[0731] In Example 1, unmixed resin (A1) was mixed with 50 parts by weight of resin (A2) obtained in Example 2, and the content of resin (B1) was set to 50 parts by weight. Otherwise, the process was the same as in Example 1.
[0732] Example 7
[0733] In Example 1, unmixed resin (A1) was mixed with 50 parts by weight of resin (A2) obtained in Mixed Example 2, the content of resin (B1) was set to 50 parts by weight, and the content of manganese octoate (manufactured by Nippon Kagaku Sangyo Co., Ltd.) was set to 0.1 parts by weight. Otherwise, the same procedure as in Example 1 was followed.
[0734] Example 8
[0735] In Example 1, 50 parts by weight of resin (A3) obtained in Example 3 were mixed with unmixed resin (A1), and the content of resin (B1) was set to 50 parts by weight. Otherwise, the same procedure as in Example 1 was followed.
[0736] Comparative Example 1
[0737] In Example 1, the content of resin (A1) was changed to 45 parts by mass, resin (B1) was not mixed, and resin (B2) (manufactured by DIC Corporation, NE-X-9470S, maleimide compound equivalent to formula (M1)) was mixed in 55 parts by mass, and the same procedure was performed otherwise.
[0738] Comparative Example 2
[0739] In Example 1, the content of resin (A1) was changed to 50 parts by weight, and 50 parts by weight of unmixed resin (B1) and mixed resin (B3) (manufactured by DIC Corporation, NE-X-9500, equivalent to maleimide compound (M7)) were prepared, and the same procedure was followed.
[0740] Comparative Example 3
[0741] In Example 1, the content of resin (A1) was changed to 60 parts by mass, unmixed resin (B1) and mixed resin (B4) (manufactured by Nippon Kayaku Co., Ltd., MIR-3000-70MT, equivalent to maleimide compound (M3)) 40 parts by mass, and the same procedure was performed otherwise.
[0742] Comparative Example 4
[0743] In Example 1, 63 parts by weight of unmixed resin (B1) and mixed resin (B2) were used, and the same procedure was followed otherwise.
[0744] Comparative Example 5
[0745] In Example 1, the content of resin (A1) was changed to 45 parts by weight, unmixed resin (B1) was used, and mixed resin (B4) was used to make 55 parts by weight. Otherwise, the same procedure was followed.
[0746] [Table 1]
[0747]
[0748] [Table 2]
[0749]
[0750] [Table 3]
[0751]
[0752] The invention has been described in detail using specific methods, but those skilled in the art will understand that various modifications can be made without departing from the intent and scope of the invention.
Claims
1. A resin composition, wherein, Relative to 10 to 90 parts by mass of resin A, the resin contains 90 to 10 parts by mass of maleimide compound B represented by formula (M4). The resin A is the resin shown in formula (T). In formula (T), Ma independently represents hydrocarbon groups with 1 to 12 carbon atoms arbitrarily substituted by halogen atoms, x represents an integer from 0 to 4, and R is a divalent group. In formula (M4), R 56 respectively and independently represent a hydrogen atom, a methyl group or an ethyl group, R 57 respectively and independently represent a hydrogen atom or a methyl group.
2. The resin composition according to claim 1, wherein, R is a group containing an indane structure.
3. The resin composition according to claim 1, wherein, R is a group containing the following structure. In formula (Tx), n, o, and p are the average number of repeating units. n represents a number greater than 0 and less than 20. o and p represent numbers from 0 to 20, respectively, satisfying 1.0 ≤ n + o + p ≤ 20.
0. Ma represents hydrocarbon groups with 1 to 12 carbon atoms arbitrarily replaced by halogen atoms. x represents an integer from 0 to 4. Structural units (a), (b), and (c) are bonded to structural units (a), (b), and (c) or other groups at *, respectively. Each structural unit is randomly bonded.
4. The resin composition according to claim 3, wherein, The parameter α in resin A, calculated by formula (α), is 0.20 or higher and 1.00 or lower, and the parameter β, calculated by formula (β), is 0.20 or higher and 3.00 or lower. The number-average molecular weight of resin A is 400 to 3000. The parentheses in equation (α) indicate 1 The integral value between the corresponding chemical shift values in H-NMR, the part in parentheses in equation (β) represents 1 The integral value between the corresponding chemical shift values in H-NMR.
5. The resin composition according to claim 1, wherein, The compound represented by formula (M4) includes the following compounds. In the formula, Me is methyl and Et is ethyl.
6. The resin composition according to claim 1, wherein, R is a group containing the following structure. The parameter α in resin A, calculated by formula (α), is 0.20 or higher and 1.00 or lower, and the parameter β, calculated by formula (β), is 0.20 or higher and 3.00 or lower. The number-average molecular weight of resin A is 400 to 3000. The compound represented by formula (M4) includes the following compounds. In equation (Tx), n, o, and p are the average number of repeating units, where n represents a number greater than 0 and less than 20, o and p represent numbers from 0 to 20 respectively, satisfying 1.0 ≤ n + o + p ≤ 20.0, Ma represents hydrocarbon groups with 1 to 12 carbon atoms arbitrarily substituted by halogen atoms, and x represents an integer from 0 to 4. Structural units (a), (b), and (c) are bonded to structural units (a), (b), and (c) or other groups at the * position, respectively. Each structural unit is randomly bonded. The parentheses in equation (α) indicate 1 The integral value between the corresponding chemical shift values in H-NMR, the part in parentheses in equation (β) represents 1 The integral value between the corresponding chemical shift values in H-NMR. In the formula, Me is methyl and Et is ethyl.
7. The resin composition according to any one of claims 1 to 6, further comprising a compound represented by formula (BV), In formula (BV), Md independently represents hydrocarbon groups with 1 to 12 carbon atoms, w represents an integer from 0 to 4, and r represents an integer from 0 to 6.
8. The resin composition according to any one of claims 1 to 6, further comprising a filler material.
9. The resin composition according to any one of claims 1 to 6, further comprising at least one selected from the group consisting of ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, flow modifiers, lubricants, defoamers, leveling agents, gloss agents, and polymerization inhibitors.
10. The resin composition according to any one of claims 1 to 6, for use in printed circuit boards.
11. A cured product, which is a cured product of the resin composition according to any one of claims 1 to 6.
12. A prepreg formed from a substrate and a resin composition according to any one of claims 1 to 6.
13. A metal foil laminate comprising at least one prepreg as described in claim 12 and a metal foil disposed on one or both sides of the prepreg.
14. A resin composite sheet comprising a support and a layer formed of the resin composition according to any one of claims 1 to 6 disposed on the surface of said support.
15. A printed circuit board comprising an insulating layer and a conductor layer disposed on a surface of the insulating layer. The insulating layer comprises a layer formed from the resin composition of any one of claims 1 to 6.
16. A semiconductor device comprising the printed circuit board of claim 15.
Citation Information
Patent Citations
Air conditioner
JP1988070057A
Fuel controller for engine
JP1988080032A
Throttle valve controller for car-mounted internal combustion engine
JP1988080036A
Semiconductor memory device
JP1988090096A
Manufacture of basic refractories
JP1988100053A