P-type back contact passivation contact crystalline silicon solar cell
By using alternating local passivation contact areas and an aluminum oxide surface passivation layer in crystalline silicon solar cells on a p-type silicon substrate, combined with a silicon oxynitride auxiliary passivation layer, the photoelectric conversion efficiency improvement and manufacturing of p-type silicon cells are solved. The problem of high cost is achieved by efficient photoelectric conversion and improved stability.
Patent Information
- Application Number
- CN202420439274.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2034-03-07
AI Technical Summary
Existing crystalline silicon solar cells based on p-type silicon have bottlenecks in improving photoelectric conversion efficiency and have high manufacturing costs, making it difficult to compete with TOPCon cells based on n-type silicon.
Local electron passivation contact areas and local hole passivation contact areas are alternately distributed on the back of the battery, combined with aluminum oxide as a surface passivation layer, and an auxiliary passivation layer of silicon oxynitride or silicon nitride is added on the back to form an interdigitated shape. structure to improve photoelectric conversion efficiency and stability.
It achieves excellent surface passivation and selective passage of photogenerated carriers on the back of the battery, avoids shading loss of the front metal electrode, improves photoelectric conversion efficiency, reduces manufacturing costs, and improves the working stability of the battery in extreme environments.
Smart Images

Figure CN221885123U_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solar cells and mainly provides a p-type back-contact passivated contact crystalline silicon solar cell. Background Art
[0002] Photovoltaic power generation uses the photoelectric effect of semiconductor materials to directly convert solar radiation into electrical energy. Photovoltaic power generation is green and environmentally friendly, can be sustainable, can solve the energy and environmental crisis of mankind, and has an important strategic position in future energy development. The development of high-efficiency, low-cost solar cells is the key to promoting the stable and rapid development of the photovoltaic power generation industry.
[0003] Among all kinds of solar cells, crystalline silicon solar cells (crystalline silicon cells for short) have developed the fastest in battery research and application due to their high photoelectric conversion efficiency, stable performance and low manufacturing cost, and their industrialization technology is the most mature and their market share is the highest. Among the various crystalline silicon cells currently popularized in industrialization, the most mainstream are PERC (passivated emitter and rear cell) cells and TOPCon (Tunnel oxide and passivated contact) cells. Among them, the production capacity of PERC cells using p-type silicon as substrate occupies about 60% of the market, and its industrial photoelectric conversion efficiency is 24%-24.5%; the production capacity of TOPCon cells using n-type silicon as substrate occupies about 30% of the market, and its industrial photoelectric conversion efficiency is 25.5%-26%. TOPCon cells use passivation contact technology, that is, tunneling silicon oxide and doped polysilicon to achieve extremely excellent surface passivation, selective passage of photogenerated carriers and one-dimensional efficient collection. Relatively speaking, PERC cells still use traditional pn junctions or high-low junctions as field passivation, and do not use more advanced passivation contact technology, which makes the improvement of PERC cell conversion efficiency encounter bottlenecks. Since the cost of pulling single crystals of p-type silicon is lower than that of n-type silicon, crystalline silicon cells with p-type silicon as substrate are more cost-effective when the photovoltaic conversion efficiency of the cells is the same. Moreover, the current production capacity of industrial PERC cells still dominates. Therefore, it is of great significance to further develop efficient and low-cost crystalline silicon cells with p-type silicon as substrate. If the passivation contact technology can be applied to p-type PERC cells, this can solve the bottleneck encountered in improving its photovoltaic conversion efficiency, and the manufacturing cost can be further reduced, thereby effectively enhancing the market competitiveness of PERC cells. Utility Model Content
[0004] In order to solve the above problems, the utility model provides a p-type back-contact passivated contact crystalline silicon solar cell (referred to as p-IBC cell). The p-IBC cell adopts a local electron passivation contact area as the n-region and a local hole passivation contact area as the p-region, and all the n-region and the p-region are designed to form a forked finger-like alternating distribution on the back of the cell, thereby achieving extremely excellent surface passivation, selective passage and efficient collection of photogenerated carriers on the back of the cell, and completely avoiding the shading loss of the metal electrode on the front of the cell. Furthermore, the front of the cell adopts aluminum oxide with a strong negative charge content as a surface passivation layer, which can achieve excellent field passivation and interface passivation. Through the scheme described in the utility model, the photoelectric conversion efficiency of industrial crystalline silicon cells with p-type silicon as a substrate can be greatly improved, and the manufacturing cost of the cell can be greatly reduced. The p-IBC cell has a simple structure and can be realized by using the existing cell preparation method, which is suitable for industrialization.
[0005] The utility model discloses a p-type back-contact passivated contact crystalline silicon solar cell, comprising: a p-type single crystal silicon substrate; aluminum oxide formed on the first surface of the substrate as a passivation layer; silicon nitride formed on the aluminum oxide passivation layer; local electron passivation contact areas and local hole passivation contact areas formed on the second surface of the substrate opposite to the first surface and alternately distributed, and an electrical insulation isolation area between adjacent local electron passivation contact areas and local hole passivation contact areas; a first metal electrode and a second metal electrode formed on the second surface of the substrate, the first metal electrode forming contact with the local electron passivation contact area, and the second metal electrode forming contact with the local hole passivation contact area.
[0006] As an optional solution, the electrically insulating isolation region is the single crystal silicon substrate itself between adjacent local electron passivation contact regions and local hole passivation contact regions.
[0007] As an optional scheme, the p-type back-contact passivated contact crystalline silicon solar cell also includes: an auxiliary passivation layer formed on the second surface of the substrate; the auxiliary passivation layer is located on the surface of the local electron passivation contact area, the surface of the local hole passivation contact area, and the surface of the electrical insulation isolation area, and serves as the electrical insulation isolation area.
[0008] As an optional solution, the auxiliary passivation layer is silicon oxynitride or silicon nitride.
[0009] As an optional solution, when the auxiliary passivation layer is silicon oxynitride, the thickness is 10-200 nm and the refractive index is 1.6-1.8.
[0010] As an optional solution, when the auxiliary passivation layer is silicon nitride, the thickness is 10-200 nm and the refractive index is 1.9-2.2.
[0011] As an alternative, the aluminum oxide layer has a 12 cm -2 Negative charge, thickness range is 3-20nm, and refractive index is 1.6-1.7.
[0012] As an optional solution, the local electron passivation contact region is composed of tunneling silicon oxide and phosphorus-doped polysilicon; the local hole passivation contact region is composed of tunneling silicon oxide and boron-doped polysilicon.
[0013] As an optional scheme, in the local electron passivation contact area, the thickness of the tunneling silicon oxide is 1.2-1.6nm, and the refractive index is 1.45-1.5; the thickness of the phosphorus-doped polysilicon is 5-500nm; in the local hole passivation contact area, the thickness of the tunneling silicon oxide is 1.2-1.6nm, and the refractive index is 1.45-1.5; the thickness of the boron-doped polysilicon is 5-500nm.
[0014] As an optional solution, the thickness of the silicon nitride on the front side of the battery is 50-70 nm, and the refractive index is 1.9-2.1.
[0015] The utility model has the following beneficial effects:
[0016] (1) The p-type back-contact passivated contact crystalline silicon cell provided by the utility model adopts a local electron passivation contact area as an n-region and a local hole passivation contact area as a p-region, and the n-region and the p-region are all designed to be alternately distributed on the back of the cell, thereby achieving extremely excellent surface passivation, selective passage and efficient collection of photogenerated carriers on the back of the cell, and completely avoiding the shading loss of the metal electrode on the front of the cell. Therefore, the p-IBC cell can achieve excellent photoelectric conversion efficiency.
[0017] (2) The p-IBC battery provided by the utility model uses aluminum oxide with a strong negative charge content as a surface passivation layer on the front side, which is also an important basis for obtaining a high photoelectric conversion efficiency. First, the sufficiently high content of negative charge in aluminum oxide can form an accumulation layer of majority carriers (holes) on the front surface of the battery, which can achieve excellent field passivation and interface passivation. Secondly, the use of aluminum oxide as the front surface passivation layer can avoid the use of a high-low junction field on the front surface using boron doping. Therefore, on the one hand, the manufacturing cost of the battery can be reduced; on the other hand, the Auger recombination caused by the boron doping process to the p-type silicon substrate can be avoided. In addition, the large number of dislocation defects caused by boron atoms in the high-temperature heat treatment of the high-temperature process of boron doping and the corresponding lattice distortion caused to the silicon substrate can be avoided.
[0018] (3) The p-IBC battery provided by the utility model has an auxiliary passivation layer of silicon oxynitride (or silicon nitride) on the back side, which can enhance the working stability of the battery in various extreme application environments (especially high humidity and high temperature environments). Furthermore, the silicon oxynitride (or silicon nitride) can also be used as an electrical insulating isolation material between the p-region and the n-region on the back side of the battery, and has excellent electrical insulation performance, which can effectively reduce the reverse saturation current density of the battery. In addition, this layer of silicon oxynitride (or silicon nitride) can also play an excellent passivation role on the silicon substrate of this electrically insulating isolation area, and can reflect sunlight back to the battery body and the front side through optical reflection, so as to further enhance the utilization rate of solar photons.
[0019] (4) The p-IBC battery described in the present invention has a simple structure and can be realized by using the existing battery preparation method. It can effectively improve the photoelectric conversion efficiency of industrial crystalline silicon batteries using p-type silicon as a substrate, and can also effectively reduce the production cost of the battery, and is suitable for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 .Schematic diagram of the structure of a p-type back-contact passivated contact crystalline silicon solar cell (with a back-side auxiliary passivation layer) given in Example 1.
[0021] Among them, 1 is a p-type single crystal silicon substrate, 2 is aluminum oxide, 3 is silicon nitride, 4 is tunneling silicon oxide, 5 is phosphorus-doped polysilicon, 6 is boron-doped polysilicon, 7.1 represents the electrical insulation isolation area between the local electron passivation contact area and the local hole passivation contact area on the back of the battery, 7.2 is the auxiliary passivation layer silicon oxynitride on the back of the battery, 8 is the metallized electrode of the local electron passivation contact area, and 9 is the metallized electrode of the local hole passivation contact area. Among them, 4 and 5 constitute the local electron passivation contact area, and 4 and 6 constitute the local hole passivation contact area.
[0022] Figure 2 .Schematic diagram of the structure of a p-type back-contact passivated contact crystalline silicon solar cell given in Example 2 (without a back-side auxiliary passivation layer).
[0023] Among them, 1 is a p-type single crystal silicon substrate, 2 is aluminum oxide, 3 is silicon nitride, 4 is tunneling silicon oxide, 5 is phosphorus-doped polysilicon, 6 is boron-doped polysilicon, 7 is a metallized electrode of a local electron passivation contact area, and 8 is a metallized electrode of a local hole passivation contact area. Among them, 4 and 5 constitute a local electron passivation contact area, 4 and 6 constitute a local hole passivation contact area, and the electrical insulation isolation area between adjacent n-regions and p-regions on the back of the battery is the p-type single crystal silicon substrate itself. DETAILED DESCRIPTION
[0024] In order to better understand the present invention, the present invention will be further described below in conjunction with specific embodiments and drawings. Obviously, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.
[0025] The utility model provides a p-type back-contact passivated contact crystalline silicon solar cell (referred to as p-IBC cell), and the p-IBC cell has the following characteristics:
[0026] A p-type (boron or gallium doped) single crystal silicon wafer is used as the substrate material.
[0027] The front side of the battery uses negatively charged aluminum oxide as a passivation layer to achieve excellent field passivation and interface passivation. The aluminum oxide layer has a charge of more than 10 12 cm -2 The negative charge of the battery is 3-20nm thick and has a refractive index of 1.6-1.7. On top of the aluminum oxide layer on the front of the battery is a layer of silicon nitride as an anti-reflection film, which is 50-70nm thick and has a refractive index of 1.9-2.1.
[0028] The back of the battery uses a local electron passivation contact area as the n-region, and a local hole passivation contact area as the p-region; specifically, the local electron passivation contact area and the local hole passivation contact area can be designed with a grid line pattern and nested with each other, thereby forming a typical interdigitated alternating distribution, that is, an interdigitated electrode.
[0029] The local electron passivation contact region is composed of tunneling silicon oxide and phosphorus-doped polysilicon. The thickness of the tunneling silicon oxide is 1.2-1.6nm, and the refractive index is 1.45-1.5. The thickness of the phosphorus-doped polysilicon is 5-500nm. The local hole passivation contact region is composed of tunneling silicon oxide and boron-doped polysilicon. The thickness of the tunneling silicon oxide is 1.2-1.6nm, and the refractive index is 1.45-1.5. The thickness of the boron-doped polysilicon is 5-500nm.
[0030] Between the n-regions and p-regions alternately distributed on the back side of the battery is an electrically insulating isolation region, whose electrical insulating isolation function can be achieved by depositing a material with electrical insulating properties in the region, or by the silicon substrate material itself.
[0031] Optionally, outside the local electron passivation contact area and the local hole passivation contact area alternately distributed on the back of the battery, there is a layer of silicon oxynitride or silicon nitride as an auxiliary passivation layer. The thickness of silicon oxynitride is 10-200nm, and the refractive index is 1.6-1.8. The thickness of silicon nitride is 10-200nm, and the refractive index is 1.9-2.2. It is not limited to this.
[0032] The main function of this auxiliary passivation layer is to enhance the working stability of the battery in various extreme environments (especially high humidity and high temperature environments). Furthermore, this auxiliary passivation layer can also be used as a buffer barrier layer for screen-printed metallization in the back end of battery preparation to ensure that the metal paste can be confined within the doped (phosphorus or boron) polysilicon layer after rapid thermal treatment and sintering, and diffuse through the polysilicon and tunnel silicon oxide to enter the silicon substrate as little as possible, thereby reducing Auger recombination.
[0033] In addition, when silicon oxynitride or silicon nitride is used as the auxiliary passivation layer on the back side, this layer of silicon oxynitride or silicon nitride will also be deposited between the local electron passivation contact area and the local hole passivation contact area alternately distributed on the back side during preparation (for example, by vapor deposition), and thus can also serve as an electrically insulating isolation area between the adjacent n-region and p-region on the back side. In the absence of an auxiliary passivation layer on the back side, the electrically insulating isolation area between the adjacent n-region and p-region on the back side of the battery is the p-type single crystal silicon substrate itself.
[0034] The back of the cell also has a metallized electrode with a local electron passivation contact area and a local hole passivation contact area.
[0035] In the case of having a back-side auxiliary passivation layer, the metallized electrode needs to be able to just pass through this auxiliary passivation layer and form contact with the local electron passivation contact area or the local hole passivation contact area. This can be achieved through the screen printing metal paste combined with rapid thermal processing and sintering technology in battery preparation.
[0036] In the case of no back auxiliary passivation layer, the metallized electrode directly contacts the local electron passivation contact area or the local hole passivation contact area.
[0037] Specifically, Example 1 provides a p-type back-contact passivated contact crystalline silicon solar cell (with a back-side auxiliary passivation layer). Figure 1 As shown, the p-IBC cell mainly includes a p-type monocrystalline silicon substrate 1; aluminum oxide 2 formed on the front of the p-type monocrystalline silicon substrate 1, silicon nitride formed on the surface of the aluminum oxide 2; local electron passivation contact areas and local hole passivation contact areas formed on the back of the p-type monocrystalline silicon substrate 1 and distributed alternately; an auxiliary passivation layer of silicon oxynitride 7.2 formed on the back of the p-type monocrystalline silicon substrate 1; and a metallized electrode 8 of the local electron passivation contact area and a metallized electrode 9 of the local hole passivation contact area. Among them, the area between adjacent local electron passivation contact areas and local hole passivation contact areas is an electrically insulating isolation area, and the material of the electrically insulating isolation area is also silicon oxynitride 7.1.
[0038] The pattern design of the local electron passivation contact area (n-region for short), the local hole passivation contact area (p-region for short), and the back electrical insulation isolation area between the n-region and the p-region on the back of the p-IBC battery is as follows: The n-region and the p-region adopt a gate line pattern design, and are nested with each other to form a typical interdigitated alternating distribution. Among them, the gate line width of the n-region is 600μm, and the spacing between two adjacent n-region gate lines (i.e., the distance between the axis lines) is 1000μm. The gate line width of the p-region is 200μm, and the spacing between two adjacent p-region gate lines (i.e., the distance between the axis lines) is 1000μm. The pattern of the electrical insulation isolation area between the adjacent n-region and p-region on the back is also a gate line pattern, and its line width is 100μm.
[0039] Furthermore, Example 1 also provides a method for preparing the p-IBC battery, which mainly includes the following steps:
[0040] Step 1. Select a 182mm*182mm p-type monocrystalline silicon wafer with a bulk resistivity of 1Ω·cm.
[0041] Step 2: polishing and etching the p-type silicon wafer using a sodium hydroxide solution to remove the damaged layer on the surface of the silicon wafer.
[0042] Step 3. Use thermal oxidation technology to prepare tunneling silicon oxide on the surface of the silicon wafer. The thickness is 1.3nm and the refractive index is 1.46.
[0043] Step 4. Use LPCVD to prepare intrinsic amorphous silicon on the back of the battery (any side of the silicon wafer can be selected as the back of the battery, and the other side is the front of the battery) with a thickness of 150nm. The LPCVD intrinsic amorphous silicon plated on the front of the battery is very small, mainly produced in a very narrow range at the edge of the front of the battery, and this effect can be eliminated by wet chemical etching later.
[0044] Step 5: Use masked ion implantation to implant boron ions locally on the back of the battery. The implantation energy is 5 keV and the dose is 6·10 15 cm -2 The localized boron implantation area (i.e., p-region) adopts a gate line pattern design with a line width of 200μm and a spacing of 1000μm between two adjacent p-region gate lines. The pattern of the process mask in ion implantation is consistent with the pattern design of the local hole passivation contact area on the back of the battery.
[0045] Step 6. Anneal the boron implanted in step 5 by furnace thermal annealing. During the annealing, the amorphous silicon on the back of the battery is fully crystallized into polysilicon, and the ion-implanted boron also completes the impurity activation and redistribution in the polysilicon layer. The annealing temperature is 975°C, the time is 30-40 minutes, and the nitrogen atmosphere is used. After annealing, the square resistance of the local boron-doped polysilicon layer on the back of the battery is 90-100Ω / □.
[0046] Step 7: Use masked ion implantation to locally implant phosphorus ions on the back of the battery. The implantation energy is 15 keV and the dose is 5.10 15 cm -2 The localized phosphorus implantation area (i.e., n-region) adopts a gate line pattern design with a line width of 600μm and a spacing of 1000μm between two adjacent n-region gate lines. The pattern of the process mask in ion implantation is consistent with the pattern design of the local electronic passivation contact area on the back of the battery.
[0047] Step 8. Use furnace tube thermal annealing to activate the phosphorus ion implanted in step 7 and redistribute it in the polysilicon layer. The annealing temperature is 850°C, the time is 30-40 minutes, and the nitrogen atmosphere is used. After annealing, the square resistance of the local phosphorus-doped polysilicon layer on the back of the battery is 80-90Ω / □.
[0048] Step 9. Use low-damage laser etching technology to etch the area between the adjacent n-region and p-region on the back of the battery, so that this area has electrical insulation properties. The laser etching process needs to be able to achieve precise alignment.
[0049] Step 10. Use PECVD to deposit silicon oxynitride as an auxiliary passivation layer on the back of the battery, with a thickness of 100nm and a refractive index of 1.75. In addition, this layer of silicon oxynitride has two functions: one is to serve as a protective layer on the back of the battery to effectively block the wet chemical etching in the subsequent step 11. The second is to serve as a buffer barrier layer for screen-printed metallization in the subsequent step 14 to ensure that the silver paste can be confined within the doped (boron or phosphorus) polysilicon layer after rapid thermal treatment and sintering, and to minimize overdiffusion through the doped polysilicon and tunneling silicon oxide into the silicon substrate.
[0050] Understandably, Figure 1 The electrically insulating isolation region 7.1 and the auxiliary passivation layer silicon oxynitride 7.2 on the back side of the cell shown in the figure are both formed by depositing silicon oxynitride on the back side of the cell by the PECVD method in this step.
[0051] In this step, silicon oxynitride is also deposited on the area between the adjacent n-region and p-region on the back of the battery. This layer of silicon oxynitride can achieve better electrical insulation isolation between the n-region and the p-region, and also has a good surface passivation effect on the p-type silicon substrate.
[0052] Step 11. Use the "single-sided water floating" wet etching method to chemically etch a small amount of doped (boron or phosphorus) polysilicon, silicon oxynitride and silicon oxide on the front side of the battery (mainly concentrated at the edge) and completely etch them away; and use this step to texturize the front side of the battery. The details are as follows:
[0053] First, a mixed solution of nitric acid and hydrofluoric acid is used in combination with a single-sided water-floating wet etching method to etch away the doped (boron or phosphorus) polysilicon that is plated and doped to the front edge of the battery. In the mixed solution of nitric acid and hydrofluoric acid, the mass concentration of nitric acid is 40%, the mass concentration of hydrofluoric acid is 4%, the solution temperature is 7°C, and the etching time is 1-2 minutes.
[0054] Then, a hydrofluoric acid solution is used in combination with a single-sided water-floating wet etching method to etch away the silicon oxynitride and thin silicon oxide that are plated around the front edge of the battery. The hydrofluoric acid concentration is 3% and the etching time is 2-3 minutes.
[0055] Finally, the front of the battery is textured by wet etching with a KOH solution with a single-sided water float. The mass concentration of the KOH solution is 2%, the temperature is 70°C, and the etching time is 5-6 minutes. Thus, a random pyramid-shaped texture is formed on the front of the battery.
[0056] It should be emphasized that in all wet chemical etchings in this step, the silicon oxynitride deposited on the back of the battery in step 10 plays a good protective role on the back of the battery. Through this step of chemical etching, electrical insulation isolation is also achieved between the front and back of the battery.
[0057] Step 12. Aluminum oxide is prepared on the front of the battery by atomic layer deposition. The thickness is 7nm and the refractive index is 1.65. The aluminum oxide deposited by atomic layer deposition has a refractive index higher than 10 12 cm -2 of negative charge.
[0058] Step 13. Use the PECVD method to deposit silicon nitride as an anti-reflection film on the front of the battery. The thickness is 60-65nm and the refractive index is 2.0.
[0059] Step 14. Metallization of the n-region and p-region on the back of the cell
[0060] The back of the battery is metallized by screen printing metal paste combined with rapid heat treatment sintering. Silver paste is used for metallization of both the n-zone and the p-zone. Alignment technology is required here, that is, it must be able to achieve: alignment between the n-zone and the corresponding metallized area, and alignment between the p-zone and the corresponding metallized area. The metallized areas of the n-zone and p-zone also use a grid line pattern design, with a line width of 35μm, and their respective axis lines coincide with the axis lines of the corresponding n-zone or p-zone. The actual peak temperature of rapid heat treatment sintering is 720-750℃, the time at the peak temperature is 2-4 seconds, and the atmosphere is compressed air.
[0061] The preparation of the p-type back contact passivated contact crystalline silicon solar cell described in Example 1 is now completed.
[0062] Specifically, Example 2 provides a p-type back contact passivated contact crystalline silicon solar cell (without a back auxiliary passivation layer). Figure 2 As shown, the p-IBC cell mainly includes a p-type monocrystalline silicon substrate 1; aluminum oxide 2 formed on the front of the p-type monocrystalline silicon substrate 1, silicon nitride formed on the surface of the aluminum oxide 2; local electron passivation contact areas and local hole passivation contact areas formed on the back of the p-type monocrystalline silicon substrate 1 and alternately distributed; and metallized electrodes 7 of the local electron passivation contact areas and metallized electrodes 8 of the local hole passivation contact areas. Among them, the area between adjacent local electron passivation contact areas and local hole passivation contact areas is an electrically insulating isolation area 7, which is the p-type monocrystalline silicon substrate itself.
[0063] The pattern design of the n-region, the p-region, and the electrically insulating isolation region therebetween on the back side of the p-IBC battery of Example 2 is the same as that of Example 1.
[0064] Example 2 also provides a method for preparing the p-IBC battery, which mainly includes the following steps:
[0065] Among them, step 1 to step 9 are the same as in Example 1 and will not be repeated here.
[0066] Step 10. Use atmospheric pressure chemical vapor deposition (APCVD) to prepare a layer of silicon oxide on the back of the battery, with a thickness of 30-40nm and a refractive index of 1.46. Use chain inline APCVD equipment, so this layer of silicon oxide is only prepared on the back of the battery. The role of this layer of silicon oxide is to serve as a protective layer on the back of the battery to effectively block the wet chemical etching in the subsequent step 11.
[0067] Step 11. First, use the "single-sided water floating" wet etching method to chemically etch a small amount of doped (boron or phosphorus) polysilicon and silicon oxide on the front side of the battery (mainly concentrated at the edge) and etch them all away. Then, use the "single-sided water floating" alkaline solution etching method to texturize the front side of the battery. Finally, use hydrofluoric acid solution to etch away the silicon oxide deposited by APCVD on the back side of the battery in step 10. The details are as follows:
[0068] (1) A mixed solution of nitric acid and hydrofluoric acid is used in combination with a single-sided water-floating wet etching method to etch away the doped (boron or phosphorus) polysilicon that is plated and doped around the front edge of the battery. In the mixed solution of nitric acid and hydrofluoric acid, the mass concentration of nitric acid is 40%, the mass concentration of hydrofluoric acid is 4%, the solution temperature is 7° C., and the etching time is 1-2 minutes.
[0069] (2) A hydrofluoric acid solution is used in combination with a single-sided water-floating wet etching method to etch away the thin layer of silicon oxide on the front side of the battery. The hydrofluoric acid concentration is 1% and the cleaning time is 15-30 seconds.
[0070] (3) The front side of the battery is textured by a wet etching method using a KOH solution with a single-sided water float. The mass concentration of the KOH solution is 2%, the temperature is 70° C., and the etching time is 5-6 minutes, thereby forming a random pyramid-shaped textured surface on the front side of the silicon wafer.
[0071] (4) The APCVD silicon oxide deposited on the back of the battery is etched away by wet etching with hydrofluoric acid solution. The hydrofluoric acid concentration is 3% and the cleaning time is 3 minutes.
[0072] It should be emphasized that in all wet chemical etchings in this step, the silicon oxide deposited on the back of the battery by APCVD in step 10 plays a good protective role on the back of the battery. Through this step of chemical etching, electrical insulation isolation is also achieved between the front and back of the battery.
[0073] Step 12. Aluminum oxide is prepared on the front of the battery by atomic layer deposition. The thickness is 7nm and the refractive index is 1.65. The aluminum oxide deposited by atomic layer deposition has a refractive index higher than 10 12 cm -2 of negative charge.
[0074] Step 13. Use the PECVD method to deposit silicon nitride as an anti-reflection film on the front of the battery. The thickness is 60-65nm and the refractive index is 2.0.
[0075] Step 14. Metallize the n-region and p-region on the back of the battery. Both the n-region and the p-region are metallized with metallic silver (Ag). The masked magnetron sputtering method is adopted. The solid part of the mask blocks the sputtered Ag atoms from flying to the substrate, and the hollow part of the mask allows the sputtered Ag atoms to fly to the substrate. The mask pattern is consistent with the metallization pattern on the back of the battery. Alignment technology is required here, that is, it is necessary to achieve: alignment between the n-region and the corresponding metallization area, and alignment between the p-region and the corresponding metallization area. The metallization areas of the n-region and the p-region are also designed with a gate line pattern. The metal line width of the n-region is 200μm, and the metal line width of the p-region is 100μm. The respective axis lines coincide with the axis lines of the corresponding n-region or p-region. Then, the sputtered Ag is thermally annealed at an annealing temperature of 400-425°C, an annealing time of 10 minutes, and a nitrogen atmosphere.
[0076] The preparation of the p-type back contact passivated contact crystalline silicon solar cell described in Example 2 is now completed.
[0077] Finally, it should be noted that although the embodiments of the present invention are described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments and application fields. The above-mentioned specific embodiments are merely illustrative and instructive, and are used to help understand the method of the present invention and its core idea, but are not restrictive. Under the guidance of this specification, ordinary technicians in this field can also make many forms of changes, improvements and equivalent implementations in the specific implementation methods and application scopes without departing from the scope of protection of the principles of the present invention and the claims, which should also be regarded as the protection scope of the present invention.
Claims
1. A p-type back contact passivated contact crystalline silicon solar cell, characterized in that: include: p-type single crystal silicon substrate; Aluminum oxide formed on the first surface of the substrate as a passivation layer; Silicon nitride formed on the aluminum oxide passivation layer; Local electron passivation contact regions and local hole passivation contact regions are formed on a second surface of the substrate opposite to the first surface and are alternately distributed, and an electrical insulation isolation region is formed between adjacent local electron passivation contact regions and local hole passivation contact regions; A first metal electrode and a second metal electrode are formed on the second surface of the substrate, wherein the first metal electrode is in contact with the local electron passivation contact region, and the second metal electrode is in contact with the local hole passivation contact region.
2. The p-type back contact passivated contact crystalline silicon solar cell according to claim 1, characterized in that: The electrically insulating isolation region is the single crystal silicon substrate itself between the adjacent local electron passivation contact region and the local hole passivation contact region.
3. The p-type back contact passivated contact crystalline silicon solar cell according to claim 1, characterized in that: Also includes: An auxiliary passivation layer is formed on the second surface of the substrate; the auxiliary passivation layer is located on the surface of the local electron passivation contact area, the surface of the local hole passivation contact area, and the surface of the electrical insulation isolation area, and serves as the electrical insulation isolation area.
4. The p-type back contact passivated contact crystalline silicon solar cell according to claim 3, characterized in that: The auxiliary passivation layer is silicon oxynitride or silicon nitride.
5. The p-type back contact passivated contact crystalline silicon solar cell according to claim 4, characterized in that: When the auxiliary passivation layer is silicon oxynitride, the thickness is 10-200 nm and the refractive index is 1.6-1.
8.
6. The p-type back contact passivated contact crystalline silicon solar cell according to claim 4, characterized in that: When the auxiliary passivation layer is silicon nitride, the thickness is 10-200 nm and the refractive index is 1.9-2.
2.
7. The p-type back-contact passivated crystalline silicon solar cell according to any one of claims 1 to 6, characterized in that: The aluminum oxide layer has a thickness greater than 10 12 cm -2 Negative charge, thickness range is 3-20nm, and refractive index is 1.6-1.
7.
8. The p-type back-contact passivated crystalline silicon solar cell according to any one of claims 1 to 6, characterized in that: The local electron passivation contact region is composed of tunneling silicon oxide and phosphorus-doped polysilicon; the local hole passivation contact region is composed of tunneling silicon oxide and boron-doped polysilicon.
9. The p-type back contact passivated contact crystalline silicon solar cell according to claim 8, characterized in that: In the local electronic passivation contact region, the thickness of the tunneling silicon oxide is 1.2-1.6 nm, and the refractive index is 1.45-1.5; the thickness of the phosphorus-doped polysilicon is 5-500 nm; In the local hole passivation contact area, the thickness of the tunneling silicon oxide is 1.2-1.6 nm, and the refractive index is 1.45-1.5; the thickness of the boron-doped polysilicon is 5-500 nm.
10. The p-type back-contact passivated crystalline silicon solar cell according to any one of claims 1 to 6, characterized in that: The thickness of silicon nitride on the aluminum oxide passivation layer on the first surface of the substrate is 50-70 nm, and the refractive index is 1.9-2.1.
Citation Information
Cited By
Back-contact photovoltaic cell piece, back-contact photovoltaic cell assembly and preparation methods of back-contact photovoltaic cell piece and back-contact photovoltaic cell assembly
CN120035266A