High-specific-energy and high-safety negative pole piece structure and battery

By designing the structure of graphite layer, silicon-based active layer, foam nickel layer, solid electrolyte layer and metal lithium foil layer in the battery negative electrode sheet, the problems of volume change of silicon-based negative electrode and instability of SEI film are solved, and the performance of the battery is improved. Cycle stability and charge and discharge performance extend battery life.

CN221885141UActive Publication Date: 2024-10-22TIANMU LAKE INST OF ADVANCED ENERGY STORAGE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323417299.4
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-10-22
Estimated Expiration
2033-12-15

AI Technical Summary

Technical Problem

The volume change of the silicon-based negative electrode during the high-level lithium deintercalation process leads to poor battery cycle performance, unstable SEI film, low first efficiency, and poor conductivity, resulting in short battery life and capacity fading.

Method used

Design a high specific energy and high safety negative electrode sheet structure, including a graphite layer, a silicon-based active layer, a nickel foam layer, a solid electrolyte layer and a metal lithium foil layer. The graphite layer and the silicon-based active layer are coated separately, and the nickel foam layer promotes Lithium intercalation deposition, the solid electrolyte layer isolates the silicon anode from contact with metallic lithium, and the metallic lithium foil layer supplements lithium to improve energy density and cycle performance.

Benefits of technology

It effectively avoids material shedding and SEI film rupture caused by the expansion of the silicon anode, improves lithium ion transmission and electronic conductivity, enhances the cycle stability and charge and discharge performance of the battery, and extends the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221885141U_ABST
    Figure CN221885141U_ABST
Patent Text Reader

Abstract

The utility model provides a high-specific-energy and high-safety negative pole piece structure and a battery, and the high-specific-energy and high-safety negative pole piece structure sequentially comprises a graphite layer, a silicon-based active layer, a foamed nickel layer, a solid electrolyte layer and a metal lithium foil layer from at least one side of a current collector to the outside. According to the utility model, the problem that the silicon negative electrode falls off can be solved through the structural sequence design of the pole pieces, meanwhile, lithium separation can be avoided, the safety performance of the battery is improved, and the charge-discharge performance and the cycle stability performance of the battery are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of battery structure design, in particular to a high-energy-density and high-safety negative electrode plate structure and a battery. Background Art

[0002] As the potential of the specific capacity of traditional graphite anodes has been fully tapped, using silicon-based anode materials to increase battery capacity has become one of the important measures to solve the energy density problem. Compared with graphite anodes, silicon-based anodes have many advantages: higher theoretical specific capacity; better safety; abundant resources and environmental friendliness.

[0003] At the same time, there are some limitations in the commercial application of silicon-based negative electrodes. First, the volume changes significantly and the cycle performance is poor. Compared with graphite, silicon is accompanied by obvious volume changes during the process of high-degree lithium extraction and insertion, resulting in poor battery cycle performance and short life. Different from the intercalation mechanism of graphite, silicon crystals present a three-dimensional phase structure of covalent tetrahedrons. They are charged and discharged by forming Li-Si alloys with lithium. The volume expansion rate of Li-Si alloys can reach 300%. Strong stress will cause the silicon particles to break and fall off the electrode sheet. Second, the SEI film is unstable and has a short service life. The SEI film can effectively prevent the occurrence of battery side reactions, while the SEI film on the surface of the silicon negative electrode will break as the volume of silicon changes. The newly exposed silicon on the surface will continue to generate a new SEI film during the charge and discharge process. The continuously growing SEI film will continuously consume lithium and electrolyte from the positive electrode, ultimately leading to an increase in the internal resistance of the battery and a rapid decay of capacity. Third, the initial efficiency is low. This is because the huge volume expansion of the silicon base itself causes the electrode material to pulverize during the alloying process, making a large amount of Li + Along with the loss of electrode materials, serious irreversible Li + Fourth, the electrical conductivity is poor. The electrical conductivity of silicon at room temperature is low, which hinders the transmission of electrons in the silicon bulk phase and the diffusion of lithium ions, affecting the power performance of the silicon negative electrode.

[0004] At present, the mainstream solution to the above problems is to compound silicon oxygen or silicon carbon with carbon materials such as graphite to form a coating structure to reduce the volume expansion effect of silicon and improve the initial efficiency. These solutions are only optimized from the material perspective, and rarely consider the impact and optimization of the structural structure of the negative electrode plate on the volume effect. Summary of the invention

[0005] The utility model provides a high-specific-energy and high-safety negative electrode plate structure, which comprises a graphite layer, a silicon-based active layer, a foamed nickel layer, a solid electrolyte layer and a metal lithium foil layer in sequence from at least one side of a current collector outward.

[0006] In some embodiments, the current collector is selected from a single metal current collector or a composite current collector. The single metal current collector is selected from one of a copper foil current collector, a titanium foil current collector, and a silver foil current collector. The composite current collector is selected from one of a carbon-coated copper foil, a PI composite copper foil, a PP composite copper foil, or a PET composite copper foil.

[0007] In some embodiments, the graphite layer material is selected from artificial graphite or natural graphite.

[0008] In some embodiments, the graphite layer has a thickness of 10-150 μm. Preferably, the graphite layer has a thickness of 10-50 μm.

[0009] In some embodiments, the silicon-based active layer material is selected from silicon oxide, silicon carbon, nano-silicon, and silicon alloy.

[0010] In some embodiments, the silicon-based active layer has a thickness of 5-150 μm. Preferably, the silicon-based active layer has a thickness of 5-50 μm.

[0011] In some embodiments, the nickel foam layer material has the characteristics of high specific surface area, low density, and high porosity, and the porosity is as high as 60% to 98%.

[0012] In some embodiments, the nickel foam layer has a thickness of 0.05-15 mm.

[0013] In some embodiments, the solid electrolyte is selected from a polymer electrolyte or an oxide electrolyte. The polymer electrolyte is selected from one of polyethylene oxide (PEO), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), and polyvinylidene fluoride (PVDF). The oxide electrolyte is selected from one of lithium phosphorus oxynitride (LiPON), lithium aluminum titanium phosphate (LATP), lithium lanthanum titanium oxide (LLTO), and lithium lanthanum zirconium oxide (LLZO).

[0014] In some embodiments, the solid electrolyte layer has a thickness of 1-20 μm.

[0015] In some embodiments, the metal lithium foil layer can be used as a lithium source for pre-lithiation of the negative electrode and has a thickness of 1-10 μm.

[0016] The utility model also provides a battery, comprising the above-mentioned negative electrode plate structure, and also comprising a counter electrode lithium plate, a positive electrode shell and a negative electrode shell.

[0017] The utility model has the following beneficial effects:

[0018] First, the graphite layer and the silicon-based active layer are coated separately to avoid the active material from falling off and powdering with the current collector when the silicon negative electrode expands, which leads to the inactivation of the active material. At the same time, the graphite layer is placed at the bottom layer to increase the connection stability with the current collector. As a lithium-conducting channel, nickel foam can promote the uniform embedding and deposition of lithium into the silicon-based active layer and the graphite layer, inhibit the formation of lithium dendrites, and because of the high hardness and large porosity of nickel foam, it can not only inhibit the expansion of the silicon negative electrode, but also increase the adsorption of battery electrolytes. At the same time, the conductive properties of nickel foam can improve the electronic conductivity of the battery. The solid electrolyte layer can not only increase the transmission of lithium ions, but also isolate the direct contact between the silicon negative electrode and the metal lithium, avoid the heat generation during the pre-lithiation process and the formation of the inorganic SEI film; at the same time, it can form an electronic insulation layer on the surface of the negative electrode, which can play a sufficient protective role when the thermal runaway diaphragm fails. After injection, the metal lithium foil layer can replenish lithium to the high-silicon negative electrode system, make up for the first-effect loss of the silicon negative electrode, and improve the energy density and cycle performance of the system.

[0019] During the preparation process, at least a portion of the solid electrolyte layer will enter the nickel foam to form a solid electrolyte-nickel foam overlapping penetration layer, which will enhance the interlayer bonding force and make the layer structure more stable. At the same time, the electron and ion transmission channels constructed by the solid electrolyte-nickel foam can regulate the uniformity of the embedding of metallic lithium into the negative electrode active material. During the charge and discharge process, the porous structure of the nickel foam can absorb a large amount of electrolyte, and the active substances such as carbonates in the electrolyte are easily adsorbed on the surface of the nickel foam to form a lithium ion transmission channel, thereby improving the lithium ion conductivity. The optimized and limited design of the thickness of each layer is conducive to maintaining the stability of the interlayer isolation and the stability of the support, while ensuring the matching of the lithium ion transmission and accommodation capacity of each layer, and preventing the problems of capacity reduction and lithium ion accumulation and precipitation caused by the imbalance of lithium ion accommodation capacity between layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 This is an exemplary structure of the high specific energy and high safety negative electrode plate structure of the utility model.

[0022] Figure 2 This is the first lithium insertion and extraction curve of the lithium battery prepared in Example 1. DETAILED DESCRIPTION

[0023] The utility model provides a high-specific-energy and high-safety negative electrode plate structure, which comprises a graphite layer, a silicon-based active layer, a foamed nickel layer, a solid electrolyte layer and a metal lithium foil layer in sequence from at least one side of a current collector outward.

[0024] In some embodiments, the current collector is selected from a single metal current collector or a composite current collector. The single metal current collector is selected from one of a copper foil current collector, a titanium foil current collector, and a silver foil current collector. The composite current collector is selected from one of a carbon-coated copper foil, a PI composite copper foil, a PP composite copper foil, or a PET composite copper foil. The above composite copper foils can all be purchased, for example, the carbon-coated copper foil can be purchased from fxd006A of Shenzhen Feixingda Electronic Materials Co., Ltd., the PI composite copper foil can be purchased from XJY-015 of Advanced Institute (Shenzhen) Technology Co., Ltd., the PP composite copper foil can be purchased from FH-300 of Suzhou Qiandingli Electronic Technology Co., Ltd., and the PET composite copper foil can be purchased from YB-1003 of Advanced Institute (Shenzhen) Technology Co., Ltd.

[0025] In some embodiments, the graphite layer material is selected from artificial graphite or natural graphite.

[0026] In some embodiments, the graphite layer has a thickness of 10-150 μm. Preferably, the graphite layer has a thickness of 10-50 μm.

[0027] In some embodiments, the silicon-based active layer material is selected from silicon oxide, silicon carbon, nano-silicon, and silicon alloy.

[0028] In some embodiments, the silicon-based active layer has a thickness of 5-150 μm. Preferably, the silicon-based active layer has a thickness of 5-50 μm.

[0029] The graphite layer and the silicon-based active layer are coated separately. The graphite layer is close to the current collector, which can prevent the active material from falling off and losing powder when the silicon negative electrode expands, thereby preventing the active material from being inactivated. At the same time, the graphite layer is placed at the bottom layer, which increases the connection stability with the current collector. The silicon-based active layer is on the surface of the graphite layer. During the lithium insertion and pre-lithiation process, due to the high platform voltage of the silicon negative electrode, the risk of lithium precipitation is not likely to occur, and the pre-lithiation is more uniform.

[0030] In some embodiments, the nickel foam layer material has the characteristics of high specific surface area, low density, and high porosity, and the porosity is as high as 60% to 98%.

[0031] In some embodiments, the nickel foam layer has a thickness of 0.05-15 mm. The nickel foam layer should not be too thick. On the one hand, the nickel foam material has a high hardness and is difficult to process if it is too thick. On the other hand, it is difficult to establish a good lithium ion transmission channel if the nickel foam is too thick.

[0032] As a lithium-conducting channel, nickel foam can promote the uniform embedding and deposition of lithium into the silicon-based active layer and graphite layer, and inhibit the formation of lithium dendrites. Nickel foam itself has a high hardness and can play an inhibitory role in the expansion process of the silicon negative electrode. At the same time, the conductive properties of nickel foam can improve the electronic conductivity of the battery, thereby improving the charge and discharge performance of the battery. In addition, the pore structure of nickel foam can increase the adsorption of battery electrolytes, improve the electrolyte diffusion performance and cycle life of the battery.

[0033] In some embodiments, the solid electrolyte is selected from a polymer electrolyte or an oxide electrolyte. The polymer electrolyte is selected from one of polyethylene oxide (PEO), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), and polyvinylidene fluoride (PVDF). The oxide electrolyte is selected from one of lithium phosphorus oxynitride (LiPON), lithium aluminum titanium phosphate (LATP), lithium lanthanum titanium oxide (LLTO), and lithium lanthanum zirconium oxide (LLZO). Preferably, the solid electrolyte is selected from a polymer electrolyte. More preferably, the solid electrolyte is selected from a polyacrylonitrile solid electrolyte. Since nickel foam has a high hardness, it is beneficial to improve the toughness of the electrode and make it easier to process when paired with a polymer electrolyte with good flexibility, and it is also beneficial to establish a good ion transmission channel.

[0034] In some embodiments, the solid electrolyte layer has a thickness of 1-20 μm.

[0035] The solid electrolyte layer can not only increase the transmission of lithium ions, but also isolate the direct contact between the silicon negative electrode and metallic lithium, avoiding heat generation during the pre-lithiation process and the formation of an inorganic SEI film; at the same time, it can form an electronic insulation layer on the surface of the negative electrode, which can provide sufficient protection when the thermal runaway diaphragm fails; and the preferred polyacrylonitrile solid electrolyte in this application has an affinity with lithium, can store excess metallic lithium, and improve the cycle performance.

[0036] During the preparation process, at least a portion of the solid electrolyte layer will enter the nickel foam to form a solid electrolyte-nickel foam overlapping permeation layer, which will enhance the interlayer bonding force and make the layer structure more stable. At the same time, the electron and ion transmission channels constructed by the solid electrolyte-nickel foam can regulate the uniformity of the embedding of metallic lithium into the negative electrode active material. During the charge and discharge process, the porous structure of the nickel foam can absorb a large amount of electrolyte, and the active substances such as carbonates in the electrolyte are easily adsorbed on the surface of the nickel foam, forming a lithium ion transmission channel and improving the lithium ion conductivity.

[0037] In some embodiments, the metal lithium foil layer can be used as a lithium source for pre-lithiation of the negative electrode and has a thickness of 1-10 μm.

[0038] After liquid injection, the metal lithium foil layer can replenish lithium to the high-silicon negative electrode system, make up for the initial loss of the silicon negative electrode, and improve the energy density and cycle performance of the system.

[0039] Each layer of the utility model is prepared with a main material that plays a main functional role of each layer. For example, the graphite layer, silicon-based active layer and solid electrolyte layer are respectively made of graphite, silicon-based active material and solid electrolyte as main materials. In the actual preparation process, it is often necessary to add some other necessary components for the purpose of layer preparation, such as adhesives, etc., and some other additives, such as conductive agents, etc., can also be added as needed. In order to better play the functional role of each layer, the mass of the main material in the solid phase is preferably not less than 80%.

[0040] The utility model also provides a battery, comprising the above-mentioned negative electrode plate structure, and also comprising a counter electrode lithium plate, a positive electrode shell and a negative electrode shell. The lithium plate is connected to the positive electrode shell, and the negative electrode plate structure is connected to the negative electrode shell.

[0041] In order to facilitate the understanding of the present invention, the present invention will be described in more detail below, but the scope of the present invention is not limited thereby.

[0042] An exemplary structure of the high specific energy and high safety negative electrode plate structure provided by the utility model can be as follows Figure 1 As shown, from both sides of the current collector 1 outward, the layers include a graphite layer 2, a silicon-based active layer 3, a nickel foam layer 4, a solid electrolyte layer 5 and a metal lithium foil layer 6 in sequence.

[0043] Example 1

[0044] The negative electrode sheet of this embodiment includes a graphite layer, a silicon-based active layer, a nickel foam layer, a solid electrolyte layer and a metal lithium foil layer on both sides of the current collector. The specific preparation steps are as follows:

[0045] (1) A copper foil current collector with a thickness of 6 μm was selected.

[0046] (2) Graphite, conductive agent and binder are mixed in a mass ratio of 90:5:5 and then subjected to a wet slurrying process to prepare a graphite layer slurry with a solid content of 35-48% and a viscosity of 3000-5000 mpas, wherein the conductive agent is SP, CNTs and graphene compounded in a weight ratio of 1:1:1, and the binder is CMC and SBR compounded in a weight ratio of 1:2. The graphite layer slurry is coated on both sides of the current collector, with a single-side graphite layer thickness of 20 μm, and placed in an oven for low temperature and vacuum treatment before use.

[0047] (3) Silicon-carbon, conductive agent, and binder are mixed in a mass ratio of 94:1:5 and then subjected to a wet slurrying process to prepare a silicon-based active layer slurry with a solid content of 35-48% and a viscosity of 3000-5000 mpas, wherein the conductive agent is a compound of SP, CNTs, and graphene in a weight ratio of 1:1:1, and the binder is a compound of PAA, CMC, and SBR in a weight ratio of 3:1:1. The silicon-based active layer slurry is applied to the outside of the two graphite layers, and the thickness of the silicon-based active layer on one side is 10 μm. The slurry is then moved to an oven for vacuum drying and set aside.

[0048] (4) The nickel foam layer is 1 mm thick and has a porosity of 95%. After ultrasonic cleaning and drying, it is covered on the outside of the two silicon-based active layers and then rolled on a roller press at 100 kg / cm 2 The product is rolled under a pressure of 100° and then set aside for use.

[0049] (5) The solid electrolyte layer material is made of polyacrylonitrile (PAN) with a thickness of 15 μm, which is coated on the outside of the two nickel foam layers. The thickness of the solid electrolyte layer on one side is 10 μm, and it is dried and set aside for use.

[0050] (6) Lithium foil with a thickness of 3 μm was covered on the outside of the two solid electrolyte layers and rolled at 100 kg / cm 2 The final negative electrode sheet is obtained after rolling under pressure.

[0051] In the above steps, the vacuum drying temperature is 100°C, the vacuum pressure is -90Kpa, and the time is 24h; the compaction density of the roller is 1.4-1.7g / m 3 .

[0052] Example 2

[0053] The silicon carbon in the silicon-based active layer described in Example 1 is replaced by silicon monoxide, and the rest are the same.

[0054] Example 3

[0055] The 6 μm copper foil current collector described in Example 1 was replaced with the 4.5 μm carbon-coated copper foil current collector, and the rest were the same.

[0056] Comparative Example 1

[0057] The thickness of the nickel foam layer described in Example 1 was changed to 30 mm, and the rest were the same.

[0058] Comparative Example 2

[0059] The nickel foam layer described in Example 1 was removed, and the rest were the same.

[0060] Comparative Example 3

[0061] The solid electrolyte layer described in Example 1 was removed, and the rest were the same.

[0062] The prepared electrode sheets were roll-pressed and assembled into a button cell with the lithium sheet as the counter electrode for testing.

[0063] Test method:

[0064] (1) According to the process steps: first discharge at 0.1C to 0.005V; then charge at 0.1C to 2V, and test the first effective coulomb efficiency (%) and discharge specific capacity (mAh / g);

[0065] (2) Cycle the above steps 100 times and test the capacity retention rate (%), lithium plating level, and negative electrode expansion rate (%); where negative electrode expansion rate = (negative electrode sheet thickness after cycle - negative electrode sheet thickness before cycle) / negative electrode sheet thickness before cycle * 100%.

[0066] Figure 2 The first lithium deintercalation curve of the lithium battery prepared in Example 1 of the present application is shown, and its first effective coulomb efficiency is as high as 93.01%. The first effective coulomb efficiency of other comparative examples of the present application is shown in Table 1.

[0067] The test results are shown in Table 1.

[0068] Table 1

[0069]

[0070] We divide lithium deposition into 10 levels according to the severity of lithium deposition. The higher the value, the more serious the lithium deposition. The overall distinction of the 10 levels of lithium deposition is shown in Table 2:

[0071] Table 2

[0072] grade Lithium precipitation 0 No lithium precipitation; 1 Point-like lithium deposition, the lithium coverage rate on the negative electrode surface is between 0% and 3%; 2 Very slight lithium deposition, the lithium coverage rate on the negative electrode surface is between 3% and 5%; 3 Slight lithium deposition, the lithium coverage rate on the negative electrode surface is between 5% and 15%; 4 Lithium deposition occurs in a very small part, and the lithium coverage rate on the negative electrode surface is between 15% and 30%; 5 Lithium deposition occurs in a small part, and the lithium coverage rate on the negative electrode surface is between 30% and 45%; 6 Lithium deposition occurs partially, and the lithium coverage rate on the negative electrode surface is between 45% and 60%; 7 Most of them have lithium deposition, and the lithium coverage rate on the negative electrode surface is between 60% and 75%; 8 Lithium is deposited on almost the entire surface, and the lithium coverage rate on the negative electrode surface is between 75% and 90%; 9 The entire surface is lithium deposited, and the lithium coverage rate of the negative electrode surface is ≥90%;

[0073] The negative electrode sheets of Examples 1 to 3 respectively include a graphite layer 2, a silicon-based active layer 3, a nickel foam layer 4, a solid electrolyte layer 5 and a metal lithium foil layer 6 from both sides of the current collector 1 to the outside; while Comparative Examples 1 to 3 are respectively the case where the nickel foam layer is too thick, no nickel foam layer is added, and no solid electrolyte layer is added. The result data in Table 1 show that the negative electrode expansion rate of the negative electrode sheet structure of the embodiment of the present application is significantly lower, and the lithium battery prepared using the negative electrode sheet structure of the embodiment of the present application has a higher first-effect coulomb efficiency, 0.1C discharge specific capacity and cycle stability, and no lithium precipitation occurs. This is because the utility model coats the graphite layer and the silicon-based active layer separately, which increases the connection stability with the current collector, reduces the risk of lithium precipitation, and makes pre-lithiation more uniform; the nickel foam layer has high hardness and large porosity, which can not only inhibit the expansion of the silicon negative electrode, but also improve the lithium ion transmission rate and electronic conductivity of the battery; the solid electrolyte layer avoids heat generation and inorganic SEI film formation during the pre-lithiation process; the metal lithium foil layer can replenish lithium for the high-silicon negative electrode system after liquid injection, make up for the first-effect loss of the silicon negative electrode, and improve the energy density and cycle performance of the system. This shows that the utility model can solve the problem of silicon negative electrode shedding through the sequential design of the pole piece structure, while avoiding lithium precipitation, improving the safety performance of the battery, and effectively improving the battery's charge and discharge performance and cycle stability.

[0074] The above embodiments are only used to illustrate the technical solutions of the present application and are not used to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high specific energy and high safety negative electrode plate structure, It is characterized in that The high specific energy and high safety negative electrode plate structure includes, from at least one side of the current collector outward, a graphite layer, a silicon-based active layer, a nickel foam layer, a solid electrolyte layer and a metal lithium foil layer in sequence.

2. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The graphite layer, silicon-based active layer, nickel foam layer, solid electrolyte layer and metal lithium foil layer are arranged in sequence on both sides of the current collector respectively.

3. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The current collector is selected from a single metal current collector or a composite current collector; the single metal current collector is selected from one of a copper foil current collector, a titanium foil current collector, and a silver foil current collector; the composite current collector is selected from one of a carbon-coated copper foil, a PI composite copper foil, a PP composite copper foil, or a PET composite copper foil.

4. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The graphite layer material is selected from artificial graphite or natural graphite; the thickness is 10-150 μm.

5. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The graphite layer has a thickness of 10-50 μm.

6. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The silicon-based active layer material is selected from one of silicon oxide, silicon carbon, nano silicon and silicon alloy; and the thickness is 5-150 μm.

7. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The thickness of the silicon-based active layer is 5-50 μm.

8. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The foam nickel layer material has a porosity of 60% to 98% and a thickness of 0.05 to 15 mm.

9. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The solid electrolyte is selected from a polymer electrolyte or an oxide electrolyte; and has a thickness of 1-20 μm.

10. The high specific energy and high safety negative electrode plate structure according to claim 9, It is characterized in that The polymer electrolyte is selected from one of polyethylene oxide (PEO), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), and polyvinylidene fluoride (PVDF); the oxide electrolyte is selected from one of lithium phosphorus oxynitride (LiPON), lithium aluminum titanium phosphate (LATP), lithium lanthanum titanium oxide (LLTO), and lithium lanthanum zirconium oxide (LLZO).

11. The high specific energy and high safety negative electrode plate structure according to claim 1, It is characterized in that The thickness of the metal lithium foil layer is 1-10 μm.

12. A battery, It is characterized in that Comprising the negative electrode plate structure according to any one of claims 1 to 11.