Front laminated film for TOPCon battery and TOPCon battery

By adopting a multi-layer anti-reflection passivation layer structure in N-TOPCon batteries, including silicon oxide, alumina and silicon nitride, the power loss problem under the PID-p type is solved, and the battery's anti-PID performance and efficiency are significantly improved. .

CN221977945UActive Publication Date: 2024-11-08HANWHA SOLARONE QIDONG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323498006.X
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-21
Publication Date
2024-11-08
Estimated Expiration
2033-12-21

AI Technical Summary

Technical Problem

The frontal PID phenomenon of N-TOPCon batteries under the PID-p type results in a power loss of up to 25%, and the prior art cannot mitigate this problem by increasing the refractive index of the anti-reflective passivation laminate film.

Method used

Using five layers of anti-reflection passivation layer structures deposited from the inside to the outside, including silicon oxide, alumina, silicon nitride and other materials, the AlOx+SiOx+SiN stacked film is formed by adjusting the resistivity and thickness to improve the stacking. The breakdown voltage of the membrane and suppresses the PID-p phenomenon.

Benefits of technology

It effectively improves the anti-PID performance of solar cells, further improves the battery efficiency, and significantly reduces the power loss caused by PID-p.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221977945U_ABST
    Figure CN221977945U_ABST
Patent Text Reader

Abstract

The utility model relates to a front laminated film for a TOPCon battery and the TOPCon battery. The front laminated film comprises a boron emitter, a first antireflection passivation layer, a second antireflection passivation layer, a third antireflection passivation layer, a fourth antireflection passivation layer and a fifth antireflection passivation layer which are sequentially deposited on the front surface of an N-type silicon substrate from inside to outside, the first anti-reflection passivation layer is made of silicon oxide, the second anti-reflection passivation layer is made of aluminum oxide, the third anti-reflection passivation layer is made of silicon oxide, the fourth anti-reflection passivation layer is made of silicon nitride, and the fifth anti-reflection passivation layer is made of silicon oxide. According to the front laminated film for the TOPCon battery, the PID resistance of a solar battery piece can be improved, and the efficiency of the solar battery piece can be further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a front laminated film for a TOPCon battery and a TOPCon battery. Background Art

[0002] PID (Potential Induced Degradation) is one of the main types of degradation common in crystalline silicon solar cells. The PID phenomenon can seriously reduce the performance of photovoltaic modules. In severe cases, the power loss can even be as high as 30% or more.

[0003] There are three known PID modes: PID-s (shunt type), PID-p (depolarization type) and PID-c (corrosion type). PID-s mainly occurs when the solar cell is at a negative potential relative to the glass plate of the module, and Na+ migrates from the glass through the anti-reflection passivation stack film to the Si substrate, accumulates at the stacking fault inside the Si, penetrates the pn junction, and causes the shunt phenomenon of the battery. At the solar cell level, the front anti-reflection passivation stack film plays an important role in suppressing the PID effect. By increasing the refractive index of the anti-reflection passivation stack film, the battery will be less susceptible to the PID-s effect. In the PID-p process, when the solar cell is at a negative potential relative to the glass plate of the module, the positive charge is driven into the anti-reflection passivation stack film, resulting in a decrease in the negative charge in the stack film, reducing the field passivation effect of the stack film, thereby reducing the opening voltage and short-circuit current of the battery. This type of PID can no longer be mitigated by increasing the refractive index of the anti-reflection passivation stack film. Currently, the front PID of the N-TOPCon battery belongs to the PID-p type. Different front anti-reflection passivation stacked film structures will cause different power losses.

[0004] Currently, the laminated film structure on the front of the N-TOPCon battery is a stacked structure of AlOx layer and SiNx layer. For N-TOPCon batteries with this structure, the power loss caused by PID-p is as high as 25%. Utility Model Content

[0005] The utility model aims to provide a front laminated film for a TOPCon battery and a TOPCon battery.

[0006] In order to achieve the above object, a technical solution adopted by the utility model is:

[0007] A front laminated film for a TOPCon cell comprises a boron emitter, a first anti-reflection passivation layer, a second anti-reflection passivation layer, a third anti-reflection passivation layer, a fourth anti-reflection passivation layer and a fifth anti-reflection passivation layer which are sequentially deposited on the front of an N-type silicon substrate from the inside to the outside, wherein the first anti-reflection passivation layer is made of silicon oxide, the second anti-reflection passivation layer is made of aluminum oxide, the third anti-reflection passivation layer is made of silicon oxide, the fourth anti-reflection passivation layer is made of silicon nitride and the fifth anti-reflection passivation layer is made of silicon oxide.

[0008] In some embodiments, the resistivity of the first anti-reflection passivation layer is 10 15 -10 16 Ω.cm.

[0009] In some embodiments, the resistivity of the third anti-reflection passivation layer is 10 9 -10 14 Ω.cm.

[0010] In some embodiments, the resistivity of the fifth anti-reflection passivation layer is 10 9 -10 14 Ω.cm.

[0011] In some embodiments, the thickness of the first anti-reflection passivation layer is 4 nm-6 nm.

[0012] In some embodiments, the thickness of the second anti-reflection passivation layer is 8 nm-15 nm.

[0013] In some embodiments, the thickness of the third anti-reflection passivation layer is 8 nm-12 nm.

[0014] In some embodiments, the fourth anti-reflection passivation layer has a thickness of 70 nm-85 nm.

[0015] In some embodiments, the fifth anti-reflection passivation layer has a thickness of 8 nm-12 nm.

[0016] In some embodiments, the fourth anti-reflection passivation layer is provided with multiple layers.

[0017] In some embodiments, the fourth anti-reflection passivation layer is provided with three layers, which are a first SiNx layer, a second SiNx layer, and a third SiNx layer, respectively, from close to the silicon substrate to away from the silicon substrate. The refractive index range of the first SiNx layer is 2.1-2.2, and the thickness of the layer is 15-25nm; the refractive index of the second SiNx layer is 2.0-2.1, and the thickness of the layer is 20-30nm; the refractive index of the third SiNx layer is 1.9-2.0, and the thickness of the layer is 30-40nm.

[0018] Another technical solution adopted by the utility model is:

[0019] A solar cell comprises a solar silicon wafer and the front-side laminated film for a TOPCon cell.

[0020] Due to the application of the above technical solution, the utility model has the following advantages compared with the prior art:

[0021] The front laminated film for the TOPCon cell provided by the utility model can improve the anti-PID performance of the solar cell and further improve the efficiency of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Attached Figure 1 This is a schematic diagram of the structure of the front laminated film for the TOPCon battery provided by the utility model;

[0023] Attached Figure 2 This is a schematic diagram of the structure of the TOPCon battery provided by the utility model.

[0024] In the above attached figure:

[0025] 1-N-type silicon substrate; 2-boron emitter; 3-first anti-reflection passivation layer; 4-second anti-reflection passivation layer; 5-third anti-reflection passivation layer; 6-fourth anti-reflection passivation layer; 7-fifth anti-reflection passivation layer; 8-tunneling oxide layer; 9-N-type doped polysilicon layer; 10-back passivation layer. DETAILED DESCRIPTION

[0026] The technical solution of the utility model will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments of the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.

[0027] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0028] Example 1

[0029] See also Figure 1-Figure 2 The front laminated film for the TOPCon cell shown includes a boron emitter 2, a first anti-reflection passivation layer 3, a second anti-reflection passivation layer 4, a third anti-reflection passivation layer 5, a fourth anti-reflection passivation layer 6, and a fifth anti-reflection passivation layer 7, which are sequentially deposited on the front of an N-type silicon substrate 1 from the inside to the outside. The first anti-reflection passivation layer 3 is made of silicon oxide (SiOx), the second anti-reflection passivation layer 4 is made of aluminum oxide (AlOx), the third anti-reflection passivation layer 5 is made of silicon oxide (SiOx), the fourth anti-reflection passivation layer 6 is made of silicon nitride (SiNx), and the fifth anti-reflection passivation layer 7 is made of silicon oxide (SiOx).

[0030] The resistivity of the first anti-reflection passivation layer 3 in this example is 10 15 -10 16 Ω.cm; the resistivity of the third anti-reflection passivation layer 5 is 10 9 -10 14 Ω.cm; the resistivity of the fifth anti-reflection passivation layer 7 is 10 9 -10 14 Ω.cm.

[0031] In this example, the thickness of the first anti-reflection passivation layer 3 is 4nm-6nm; the thickness of the second anti-reflection passivation layer 4 is 8nm-15nm; it is characterized in that the thickness of the third anti-reflection passivation layer 5 is 8nm-12nm; the thickness of the fourth anti-reflection passivation layer 6 is 70nm-85nm; the thickness of the fifth anti-reflection passivation layer 7 is 8nm-12nm.

[0032] In some embodiments, the material of the first anti-reflection passivation layer 3 is silicon oxide (SiOx) and the preparation method is thermal oxidation. The equipment can be a tubular quartz tube, the oxidation temperature is 600°C-800°C, and the time is 30 minutes-1 hour. The SiOx film prepared by thermal oxidation has a resistivity of up to 10 15 -10 16 Ω.cm is a very good insulator that can block various ions or impurities from entering the silicon matrix and can form a non-polar siloxane structure with the silicon surface. This structure can not only combine with the dangling bonds on the silicon surface to form a good chemical passivation, but also, because it is non-polar, it does not affect the field passivation effect of the second anti-reflection passivation layer 4 (AlOx film).

[0033] The second anti-reflection passivation layer 4 has a thickness of 8 nm to 15 nm, and can be prepared by a PECVD method or an ALD method.

[0034] The thickness of the third anti-reflection passivation layer 5 is 8nm-12nm, and it can be prepared by PECVD or ALD method, and the resistivity can reach 10 9 -1014 Ω.cm. The breakdown voltage of the conventional AlOx+SiNx stacked film is about 7.0 eV. Since the band gap of the third anti-reflection passivation layer 5SiOx thin film is large, about 9.0 eV, adding SiOx to the back passivation stack, i.e. AlOx+SiOx+SiN stacked film, can significantly increase the breakdown voltage of the stacked film. When the solar cell is in a bias state, Na + Or other positive charges drift into the stacked film. If it is an AlOx+SiNx stacked film, Na + Or other positive charges will reduce the fixed negative charge of AlOx, thereby reducing the field passivation effect of AlOx. However, if it is AlOx+SiOx+SiN stacked film, the positive charge passing through the AlOx+SiOx+SiNx stacked film will encounter the greatest resistance when passing through the SiOx+SiN stacked film. Therefore, Na+ or other positive charges will not affect the field passivation effect of AlOx, thereby suppressing the PID-p phenomenon.

[0035] The fourth anti-reflection passivation layer 6 can be provided with one or more layers, and the multi-layer fourth anti-reflection passivation layer 6 is located between the third anti-reflection passivation layer 5 and the fifth anti-reflection passivation layer 7. The refractive index and film thickness of each layer of SiNx are different. Generally, the refractive index increases from close to the silicon substrate to away from the silicon substrate, and the total film thickness is controlled at 70nm-85nm.

[0036] In one embodiment, the fourth anti-reflection passivation layer 6 is provided with three layers, and the three layers of the fourth anti-reflection passivation layer 6 are arranged from close to the silicon substrate to away from the silicon substrate: the refractive index of the first SiNx layer is in the range of 2.1-2.2, and the thickness of the layer is 15-25nm; the refractive index of the second SiNx layer is 2.0-2.1, and the thickness of the layer is 20-30nm; the refractive index of the third SiNx layer is 1.9-2.0, and the thickness of the layer is 30-40nm. This structure is to reduce the absorption of light by the SiNx film layer and increase the amount of light passing through the film layer into the silicon substrate.

[0037] The thickness of the fifth anti-reflection passivation layer 7 is 8nm-12nm, and the preparation method can be prepared by PECVD or ALD. Compared with SiNx film, silicon oxide (SiOx) film has a low refractive index and a low extinction coefficient. SiOx film can be used as an anti-reflection structure of SiNx / SiOx stacking, reducing the reflectivity of light and increasing the amount of light entering the silicon substrate, thereby improving the short-circuit current of the solar cell.

[0038] In this example, for N-type batteries, the front side must be diffused with boron, that is, the silicon wafer after texturing is placed in a diffusion furnace, and BCl3 is introduced to form a B-doped layer of about 2 to 1 um on the front side of the silicon wafer. This boron-doped layer is the PN junction of the N-type battery, that is, the boron emitter.

[0039] Example 2

[0040] The present example provides a solar cell, including a solar silicon wafer and a front laminated film for a TOPCon cell, the front laminated film including a boron emitter 2, a first anti-reflection passivation layer 3, a second anti-reflection passivation layer 4, a third anti-reflection passivation layer 5, a fourth anti-reflection passivation layer 6, and a fifth anti-reflection passivation layer 7, which are sequentially deposited on the front of an N-type silicon substrate 1 from the inside to the outside, the first anti-reflection passivation layer 3 is made of silicon oxide (SiOx), the second anti-reflection passivation layer 4 is made of aluminum oxide (AlOx), the third anti-reflection passivation layer 5 is made of silicon oxide (SiOx), the fourth anti-reflection passivation layer 6 is made of silicon nitride (SiNx), and the fifth anti-reflection passivation layer 7 is made of silicon oxide (SiOx); a tunneling oxide layer 8, an N-type doped polysilicon layer 9, and a back passivation layer 10 are sequentially deposited on the back of the solar silicon wafer, the tunneling oxide layer 8 is a SiOx layer, and the back passivation layer 10 is a SiNx layer.

[0041] Comparative Example

[0042] The front stacked film includes a boron emitter, an AlOx layer, and a SiNx layer deposited on the front of the solar silicon wafer from the inside to the outside.

[0043] The solar cells of Example 2 and the comparative example were tested under PID conditions, where the PID conditions were -13 kV, 34° C. (±1° C.), and operated for 23 hours.

[0044] The electrical performance data of the solar cells of Example 2 and the comparative example are shown in Table 1 below:

[0045] Table 1 Electrical performance data of solar cells of Example 2 and Comparative Example

[0046]

[0047] It can be seen from the above table that the Uoc, Isc, FF, and Eta of the solar cell of Example 2 are respectively greater than the Uoc, Isc, FF, and Eta of the comparative example.

[0048] The solar cell provided by the utility model can improve the anti-PID performance of the solar cell and further improve the efficiency of the solar cell by arranging a front laminated film for the TOPCon cell.

[0049] The above embodiments are only for illustrating the technical concept and features of the utility model, and their purpose is to enable people familiar with the technology to understand the content of the utility model and implement it accordingly, and they cannot be used to limit the protection scope of the utility model. Any equivalent changes or modifications made according to the spirit of the utility model should be included in the protection scope of the utility model.

Claims

1. A front laminated film for a TOPCon battery, characterized in that: The invention comprises a boron emitter, a first anti-reflection passivation layer, a second anti-reflection passivation layer, a third anti-reflection passivation layer, a fourth anti-reflection passivation layer and a fifth anti-reflection passivation layer which are sequentially deposited on the front surface of an N-type silicon substrate from the inside to the outside. The material of the first anti-reflection passivation layer is silicon oxide, the material of the second anti-reflection passivation layer is aluminum oxide, the material of the third anti-reflection passivation layer is silicon oxide, the material of the fourth anti-reflection passivation layer is silicon nitride, and the material of the fifth anti-reflection passivation layer is silicon oxide.

2. The front laminated film for TOPCon battery according to claim 1, characterized in that: The resistivity of the first anti-reflection passivation layer is 10 15 -10 16 Ω.cm.

3. The front laminated film for TOPCon battery according to claim 1, characterized in that: The resistivity of the third anti-reflection passivation layer is 10 9 -10 14 Ω.cm.

4. The front laminated film for TOPCon battery according to claim 1, characterized in that: The resistivity of the fifth anti-reflection passivation layer is 10 9 -10 14 Ω.cm.

5. The front laminated film for TOPCon battery according to claim 2, characterized in that: The thickness of the first anti-reflection passivation layer is 4nm-6nm; the thickness of the third anti-reflection passivation layer is 8nm-12nm.

6. The front laminated film for TOPCon battery according to claim 1, characterized in that: The thickness of the fifth anti-reflection passivation layer is 8nm-12nm.

7. The front laminated film for TOPCon battery according to claim 1, characterized in that: The thickness of the second anti-reflection passivation layer is 8nm-15nm; the thickness of the fourth anti-reflection passivation layer is 70nm-85nm.

8. The front laminated film for TOPCon battery according to claim 1, characterized in that: The fourth anti-reflection passivation layer is provided with multiple layers.

9. The front laminated film for TOPCon battery according to claim 8, characterized in that: The fourth anti-reflection passivation layer is provided with three layers, which are the first SiNx layer, the second SiNx layer, and the third SiNx layer in the direction from close to the silicon substrate to away from the silicon substrate. The refractive index range of the first SiNx layer is 2.1-2.2, and the thickness of the layer is 15-25nm; the refractive index of the second SiNx layer is 2.0-2.1, and the thickness of the layer is 20-30nm; the refractive index of the third SiNx layer is 1.9-2.0, and the thickness of the layer is 30-40nm.

10. A TOPCon battery, characterized in that: The invention comprises a solar silicon wafer and a front-side laminated film for a TOPCon cell as claimed in any one of claims 1 to 9.