Battery monomer, battery and electric device

By setting the insulating coating and inorganic insulating filler with thickness on the negative electrode sheet without the negative electrode battery, the short circuit and capacity loss in the battery caused by dendrites at the end of the negative electrode are solved, and the reliability and cycling performance of the battery are improved.

CN222015467UActive Publication Date: 2024-11-15CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323160727.X
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-11-22
Publication Date
2024-11-15
Estimated Expiration
2033-11-22

AI Technical Summary

Technical Problem

The growth of dendrites at the negative end of the negative electrode without the negative electrode leads to short circuits and irreversible loss of capacity in the battery, affecting the reliability and cycling performance of the battery.

Method used

By providing an insulating coating on the negative electrode sheet, its thickness is configured to be greater than 1.1 times the theoretical thickness of the metal deposition layer during charging and the thickness of the interface modification layer, and smaller than the metal deposition layer, the positive electrode active material layer and the interface modification during charging. The sum of the thicknesses of the layers is used to improve the density and uniformity of the insulating coating by using inorganic insulating fillers, and reduce the growth of dendrites bypassing the insulating coating.

Benefits of technology

It effectively avoids metal deposition on the insulating coating, reduces the short circuit problem in the battery caused by dendrites bypassing the insulating coating, improves the reliability and cycling performance of the battery, and avoids irreversible capacity loss due to dendrites breakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222015467U_ABST
    Figure CN222015467U_ABST
Patent Text Reader

Abstract

The utility model discloses a battery monomer, a battery and a power utilization device, the battery monomer comprises a positive pole piece and a negative pole piece, the positive pole piece comprises a positive current collector and a positive active material layer located on at least one side of the positive current collector; the negative pole piece comprises a negative current collector and two insulating coatings arranged on the surface, close to the positive pole piece, of the negative current collector, the distance between the two insulating coatings is larger than the width of the positive active material layer, and the two insulating coatings do not directly face the positive active material layer; the negative pole piece also optionally comprises an interface modification layer which is arranged on the negative current collector and is positioned between the two insulating coatings; the thickness of the insulating coating is configured to be larger than the sum of 1.1 times of the theoretical thickness of the metal deposition layer deposited when the battery cell is charged and the thickness of the optional interface modification layer, and is smaller than the sum of the theoretical thickness of the metal deposition layer deposited when the battery cell is charged, the thickness of the positive electrode active material layer and the thickness of the optional interface modification layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a battery cell, a battery and an electrical device. Background Art

[0002] As energy and environmental issues become increasingly prominent, the new energy industry has received more and more attention. In order to further improve the energy density of batteries, negative electrode-free batteries have been developed. However, the problem of dendrite growth at the negative end of negative electrode-free batteries has become one of the key issues restricting their commercialization. Utility Model Content

[0003] The present application provides a battery cell, a battery and an electrical device, which can make the battery have high reliability, good cycle performance and good processing performance.

[0004] In a first aspect, the present application provides a battery cell, comprising a positive electrode plate and a negative electrode plate, wherein the positive electrode plate comprises a positive electrode collector and a positive electrode active material layer located on at least one side of the positive electrode collector; the negative electrode plate comprises a negative electrode collector and two insulating coatings arranged on the surface of the negative electrode collector close to the positive electrode plate, the distance between the two insulating coatings is greater than the width of the positive electrode active material layer, and the two insulating coatings are not directly opposite to the positive electrode active material layer; the negative electrode plate may also optionally comprise an interface modification layer arranged on the negative electrode collector and located between the two insulating coatings; the thickness of the insulating coating is configured to be greater than 1.1 times the theoretical thickness of the metal deposition layer deposited when the battery cell is charged and the sum of the thickness of the optional interface modification layer, and less than the sum of the theoretical thickness of the metal deposition layer deposited when the battery cell is charged, the thickness of the positive electrode active material layer and the thickness of the optional interface modification layer.

[0005] In the embodiment of the present application, the thickness of the insulating coating is configured to be greater than 1.1 times the theoretical thickness of the metal deposition layer deposited when the battery cell is charged and the thickness of the optional interface modification layer. Due to the poor electronic conductivity of the insulating coating, metal deposition on the insulating coating can be avoided as much as possible. The problem of internal short circuit in the battery caused by the growth of dendrites at the negative terminal bypassing the insulating coating can also be effectively reduced, thereby improving the reliability of the battery, reducing the irreversible capacity loss caused by dendrite breakage, and improving the cycle performance of the battery.

[0006] At the same time, the thickness of the insulating coating is also configured to be less than the sum of the theoretical thickness of the metal deposition layer deposited when the battery cell is charged, the thickness of the positive electrode active material layer, and the thickness of the optional interface modification layer. Because, when the thickness of the insulating coating is too large, it will not only increase the weight of the battery cell and reduce the energy density of the battery cell, but also cause the bulging problem of the battery cell after assembly, affecting the processing performance of the battery cell; in addition, when the thickness of the insulating coating is too large, it will also cause misalignment when the pole pieces are stacked, increase the ion transmission path between the positive and negative electrodes, and further affect the cycle performance of the battery cell.

[0007] Therefore, the battery cell provided by the embodiment of the present application can have high reliability, good cycle performance and good processing performance.

[0008] In some embodiments, the thickness of the insulating coating is configured to be greater than 1.25 times the theoretical thickness of the metal deposition layer deposited when the battery cell is charged and the thickness of an optional interface modification layer, and less than the sum of the theoretical thickness of the metal deposition layer deposited when the battery cell is charged, the thickness of the positive electrode active material layer and the thickness of an optional interface modification layer.

[0009] This can further reduce the problem of short circuit in the battery caused by the growth of dendrites at the negative terminal bypassing the insulating coating, improve the reliability of the battery, and further reduce the irreversible loss of capacity caused by dendrite breakage, thereby improving the cycle performance of the battery.

[0010] In some embodiments, the capacity per unit area of ​​the positive electrode active material layer is recorded as M mAh / cm 2 The theoretical gram capacity of the metal deposited when the battery cell is charged is recorded as C a mAh / g, the theoretical density of the metal deposited when the battery cell is charged is recorded as ρ a g / cm 3 , then the theoretical thickness of the metal deposition layer deposited when the battery cell is charged is (10000×M) / (C a ×ρ a ), unit is μm.

[0011] In some embodiments, the density of the insulating coating is greater than or equal to 20%, and can be 50%-80%. This can reduce the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0012] In some embodiments, an inorganic insulating filler is dispersed in the insulating coating.

[0013] In some embodiments, the volume distribution particle size Dv50 of the inorganic insulating filler is less than or equal to 2 μm, and can be selected as 0.001 μm-0.5 μm. When the volume distribution particle size Dv50 of the inorganic insulating filler is within the above range, it is conducive to the close stacking of the inorganic insulating filler, and can also improve the density of the insulating coating, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0014] In some embodiments, the thickness of the insulating coating is recorded as H0 μm, the volume distribution particle size Dv50 of the inorganic insulating filler is recorded as D0 μm, and H0 / D0 ≥ 5. This can improve the density and uniformity of the insulating coating, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and also making the battery have high reliability and good cycle performance.

[0015] In some embodiments, the tap density of the inorganic insulating filler is 0.8 g / cm 3 -2.0g / cm 3 , optional 0.95g / cm 3 -1.40g / cm 3 When the tap density of the inorganic insulating filler is within the above range, the density of the insulating coating can be improved, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery and making the battery have high reliability and good cycle performance.

[0016] In some embodiments, the specific surface area of ​​the inorganic insulating filler is 3m 2 / g-25m 2 / g, optional 7m 2 / g-20m 2 When the specific surface area of ​​the inorganic insulating filler is within the above range, the density of the insulating coating can be improved, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and also making the battery have high reliability and good cycle performance.

[0017] In some embodiments, the surface density of the insulating coating is 0.06 mg / cm 2 -13.0mg / cm 2 , optional 0.10mg / cm 2 -3.50mg / cm 2When the surface density of the insulating coating is within the above range, the density and uniformity of the insulating coating can be improved, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery and making the battery have high reliability and good cycle performance.

[0018] In some embodiments, the two insulating coatings are respectively a first insulating coating and a second insulating coating, the first insulating coating is located on the negative electrode tab side of the negative electrode plate, the width of the first insulating coating is recorded as W1, the width of the second insulating coating is recorded as W2, W1 is greater than or equal to 0.5 mm, W2 is greater than or equal to 0.5 mm, and W1 / W2 is greater than or equal to 0.5, which can be selected as 1-3. The current density distribution in the negative electrode tab area is usually large and the temperature in the negative electrode tab area is higher, so that the metal deposition growth is looser and it is easier to form dendrites in the negative electrode tab area. By adjusting W1 / W2 within the above range, the performance of the battery can be further improved and the internal short circuit problem of the battery can be further reduced.

[0019] In some embodiments, W1 is 0.5 mm-20 mm, optionally 1 mm-15 mm.

[0020] In some embodiments, W2 is 0.5 mm-10 mm, optionally 1 mm-5 mm.

[0021] In some embodiments, the insulating coating includes a first sublayer and a second sublayer located between the first sublayer and the negative electrode current collector, the first sublayer is not dispersed with inorganic insulating fillers, and the second sublayer is dispersed with inorganic insulating fillers. This can make the insulating coating better bonded to the separator, and can further reduce the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0022] In some embodiments, the insulating coating includes a first sublayer and a second sublayer located between the first sublayer and the negative electrode current collector, the first sublayer is dispersed with an inorganic insulating filler, the second sublayer is dispersed with an inorganic insulating filler, and the weight content of the inorganic insulating filler in the first sublayer is less than the weight content of the inorganic insulating filler in the second sublayer. This can make the insulating coating better bonded to the separator, and can further reduce the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0023] In some embodiments, the ratio of the thickness of the first sublayer to the second sublayer is (0.1-0.9): 1, and can be optionally (0.2-0.5): 1. When the ratio of the thickness of the first sublayer to the second sublayer is within the above range, the insulating coating can be better bonded to the isolation film, and the insulating coating can have high density, high uniformity and good resistance to dendrite puncture, thereby further reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and also making the battery have high reliability and good cycle performance.

[0024] In some embodiments, the width of the interface modification layer is greater than the width of the positive electrode active material layer, which is beneficial for the metal to be preferentially deposited on the interface modification layer when the battery is charged, and to avoid metal deposition on the insulating coating as much as possible, thereby reducing the capacity loss of the battery.

[0025] In some embodiments, the battery cell further includes a separator, the separator is located between the positive electrode sheet and the negative electrode sheet, and the bonding force between the insulating coating and the separator is greater than the bonding force between the interface modification layer and the separator. This can make the insulating coating and the separator bond better, and can further reduce the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0026] In some embodiments, the bonding force between the insulating coating and the isolation film is 3N / m-50N / m, and can be 4N / m-25N / m. This can make the insulating coating and the isolation film bond better, and can further reduce the negative end dendrites growing along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0027] In some embodiments, the two insulating coatings are respectively a first insulating coating and a second insulating coating, the first insulating coating is located on the negative electrode ear side of the negative electrode plate, the width of the first insulating coating is recorded as W1, the width of the second insulating coating is recorded as W2, and the width of the interface modification layer is recorded as W a , W1 / W a 0.01-0.1, optionally 0.01-0.05; and / or, W2 / W a The ratio of the negative electrode to the negative electrode is 0.01-0.1, and can be 0.01-0.05. This is beneficial to improving the processability of the negative electrode sheet and can also make the battery have a high energy density.

[0028] In some embodiments, the width of the interface modification layer is 50 mm-200 mm, and can be optionally 70 mm-150 mm.

[0029] In some embodiments, the thickness of the interface modification layer is 1 μm-50 μm, and can be 1 μm-20 μm.

[0030] In some embodiments, the interface modification layer is dispersed with an alkali metal affinity material, and the alkali metal affinity material is a sodium affinity material or a lithium affinity material. Thus, the interface modification layer can provide some active points to induce uniform metal deposition, thereby improving the cycle performance of the battery, and further reducing the problem of internal short circuit of the battery caused by dendrite growth at the negative terminal during the battery charging and discharging process, so that the battery has high reliability.

[0031] In some embodiments, the battery cell is a negative electrode-free sodium battery cell or a negative electrode-free lithium battery cell.

[0032] In a second aspect, the present application provides a battery, comprising the battery cell of the first aspect of the present application.

[0033] In a third aspect, the present application provides an electrical device, comprising the battery of the second aspect of the present application, wherein the battery is used to provide electrical energy.

[0034] The electric device of the present application includes the battery provided by the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some implementation methods of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0036] Figure 1 A schematic diagram of the structure of an electrode assembly provided in some embodiments of the present application is shown.

[0037] Figure 2 Show Figure 1 Schematic diagram of the structure of the electrode assembly after charging.

[0038] Figure 3 Schematic diagrams of the structures of electrode assemblies provided in other embodiments of the present application are shown.

[0039] Figure 4 Show Figure 3 Schematic diagram of the structure of the electrode assembly after charging.

[0040] Figure 5Schematic diagrams of the structures of electrode assemblies provided in some other embodiments of the present application are shown.

[0041] Figure 6 A schematic diagram of an electrical device including a battery provided in an embodiment of the present application as a power source is shown.

[0042] In the drawings, the drawings are not necessarily drawn to scale.

[0043] The reference numerals are explained as follows: 101, negative electrode current collector; 102, insulating coating; 1021, first sublayer; 1022, second sublayer; 103, interface modification layer; 104, metal deposition layer; 201, positive electrode current collector; 202, positive electrode active material layer; 300, isolation film; T, thickness direction; W, width direction. DETAILED DESCRIPTION

[0044] Hereinafter, the battery cells, batteries and electrical devices of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0045] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0046] If there is no special explanation, all embodiments and optional embodiments of the present application may be combined with each other to form a new technical solution without conflict, and such a technical solution shall be deemed to be included in the disclosure of the present application.

[0047] If there is no special explanation, all the technical features and optional technical features of the present application may be combined with each other to form a new technical solution without conflict, and such a technical solution shall be deemed to be included in the disclosure of the present application.

[0048] Reference to "embodiment" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments.

[0049] Unless otherwise specified, all technical and scientific terms used in this application have the same meaning as those commonly understood by technicians in the technical field to which this application belongs; the terms used in this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0050] Unless otherwise specified, the values ​​of the parameters mentioned in this application can be measured by various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise specified, the test temperature of each parameter is 25°C.

[0051] The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship.

[0052] In the description of the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0053] In the embodiments of the present application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments. It should be understood that the thickness, length, width and other dimensions of the various components in the embodiments of the present application shown in the drawings are only exemplary and should not constitute any limitation to the present application.

[0054] In the present application, the terms "plurality" and "multiple" refer to two or more.

[0055] The battery mentioned in the embodiments of the present application may be a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the present application may include a battery cell, a battery module or a battery pack.

[0056] A battery cell is the smallest unit of a battery, which can independently realize the functions of charging and discharging. The battery cell can be cylindrical, rectangular or in other shapes, etc., which is not limited in the embodiments of the present application.

[0057] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed connection through a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a case and battery cells, and the battery cells or battery modules are accommodated in the case. In some embodiments, the case may serve as part of the chassis structure of the vehicle. For example, part of the case may become at least a part of the floor of the vehicle, or part of the case may become at least a part of the crossbeam and longitudinal beam of the vehicle.

[0058] In some embodiments, the battery may be an energy storage device, which includes an energy storage container, an energy storage cabinet, and the like.

[0059] In some embodiments, battery cells may be assembled into a battery module. The battery module may contain multiple battery cells, and the specific number may be adjusted according to the application and capacity of the battery module.

[0060] In some embodiments, the battery modules may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0061] In some embodiments, the battery cells can also be directly assembled into a battery pack. The battery pack can contain multiple battery cells, and the specific number can be adjusted according to the application and capacity of the battery pack.

[0062] The embodiment of the present application provides a battery cell. The battery cell is a battery cell without a negative electrode, for example, a sodium battery cell without a negative electrode or a lithium battery cell without a negative electrode.

[0063] A battery without a negative electrode generally refers to a battery that does not actively set a negative electrode active material layer on the negative electrode side during the manufacturing process of the battery. For example, during the manufacturing process of the battery, a negative electrode active material layer is not formed by coating or deposition of carbonaceous active materials (such as graphite, hard carbon, etc.) at the negative electrode. When the battery is charged for the first time, ions gain electrons on the negative electrode side and are deposited at the negative electrode to form metals. When discharged, the metals can be converted into ions and return to the positive electrode, realizing cyclic charge and discharge. Compared with other batteries, batteries without negative electrodes can achieve higher energy density because they do not have a conventional negative electrode active material layer.

[0064] The battery cell includes an electrode assembly and an outer package. The electrode assembly can be a wound structure or a laminated structure, which is not limited in the embodiments of the present application. The outer package can be used to encapsulate the electrode assembly. The outer package can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT) and polybutylene succinate (PBS). The number of electrode assemblies contained in the battery cell can be one or more, which can be adjusted according to demand.

[0065] Figure 1 A schematic diagram of the structure of an electrode assembly provided in some embodiments of the present application is shown. Figure 2 Show Figure 1 Schematic diagram of the structure of the electrode assembly after charging.

[0066] like Figure 1 and Figure 2 As shown, the electrode assembly of the battery cell includes a separator 300, a positive electrode sheet and a negative electrode sheet, and the separator 300 is located between the positive electrode sheet and the negative electrode sheet.

[0067] The positive electrode plate includes a positive electrode current collector 201 and a positive electrode active material layer 202 located on at least one side of the positive electrode current collector 201. The negative electrode plate includes a negative electrode current collector 101 and two insulating coatings 102 arranged on the surface of the negative electrode current collector 101 close to the positive electrode plate, the distance between the two insulating coatings 102 is greater than the width of the positive electrode active material layer 202, and the two insulating coatings 102 are not directly opposite to the positive electrode active material layer 202.

[0068] The negative electrode sheet further optionally includes an interface modification layer 103 disposed on the negative electrode current collector 101 and between the two insulating coatings 102. "Optionally" means that the interface modification layer 103 may or may not be disposed on the negative electrode current collector 101 of the negative electrode sheet.

[0069] The thickness of the insulating coating 102 is configured to be greater than 1.1 times the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged and the thickness of the optional interface modification layer 103, and less than the sum of the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged, the thickness of the positive electrode active material layer 202 and the thickness of the optional interface modification layer 103.

[0070] For example, when the interface modification layer 103 is not provided on the negative electrode current collector 101 of the negative electrode sheet (i.e., the thickness of the interface modification layer 103 is 0), the thickness of the insulating coating 102 is configured to be greater than 1.1 times the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged, and less than the sum of the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged and the thickness of the positive electrode active material layer 202; when the interface modification layer 103 is provided on the negative electrode current collector 101 of the negative electrode sheet, the thickness of the insulating coating 102 is configured to be greater than 1.1 times the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged and the sum of the thickness of the interface modification layer 103, and less than the sum of the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged, the thickness of the positive electrode active material layer 202, and the thickness of the interface modification layer 103.

[0071] For safety reasons, the negative electrode plate usually includes an overhang area (i.e., the area where the negative electrode and the positive electrode do not overlap) and a non-overhang area (i.e., the area where the negative electrode and the positive electrode overlap). During the battery charging and discharging process, the overhang area will have serious dendrite problems. The continuous growth of dendrites will pierce the isolation membrane, causing an internal short circuit and posing a safety hazard to the battery.

[0072] Currently, when an insulating coating is provided on the negative electrode current collector, the thickness rebound problem during the metal deposition process and the local unevenness of the metal deposition are not considered, which results in the problem of internal short circuit in the battery caused by dendrite growth at the negative terminal.

[0073] In the embodiment of the present application, the thickness of the insulating coating is configured to be greater than 1.1 times the theoretical thickness of the metal deposition layer deposited when the battery cell is charged and the thickness of the optional interface modification layer. Due to the poor electronic conductivity of the insulating coating, metal deposition on the insulating coating can be avoided as much as possible. The problem of internal short circuit in the battery caused by the growth of dendrites at the negative terminal bypassing the insulating coating can also be effectively reduced, thereby improving the reliability of the battery, reducing the irreversible capacity loss caused by dendrite breakage, and improving the cycle performance of the battery.

[0074] At the same time, the thickness of the insulating coating is also configured to be less than the sum of the theoretical thickness of the metal deposition layer deposited when the battery cell is charged, the thickness of the positive electrode active material layer, and the thickness of the optional interface modification layer. Because, when the thickness of the insulating coating is too large, it will not only increase the weight of the battery cell and reduce the energy density of the battery cell, but also cause the bulging problem of the battery cell after assembly, affecting the processing performance of the battery cell; in addition, when the thickness of the insulating coating is too large, it will also cause misalignment when the pole pieces are stacked, increase the ion transmission path between the positive and negative electrodes, and further affect the cycle performance of the battery cell.

[0075] Therefore, the battery cell provided by the embodiment of the present application can have high reliability, good cycle performance and good processing performance.

[0076] Optionally, the thickness of the insulating coating 102 is configured to be greater than 1.25 times the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged and the thickness of the optional interface modification layer 103, and less than the sum of the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged, the thickness of the positive electrode active material layer 202 and the thickness of the optional interface modification layer 103.

[0077] Optionally, the thickness of the insulating coating 102 is configured to be greater than 1.3 times the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged and the thickness of the optional interface modification layer 103, and less than the sum of the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged, the thickness of the positive electrode active material layer 202 and the thickness of the optional interface modification layer 103.

[0078] This can further reduce the problem of short circuit in the battery caused by the growth of dendrites at the negative terminal bypassing the insulating coating, improve the reliability of the battery, and further reduce the irreversible loss of capacity caused by dendrite breakage, thereby improving the cycle performance of the battery.

[0079] The capacity per unit area of ​​the positive electrode active material layer 202 is denoted as M mAh / cm 2 The theoretical gram capacity of the metal deposited when the battery cell is charged is recorded as C a mAh / g, the theoretical density of the metal deposited when the battery cell is charged is recorded as ρ a g / cm 3 , then the theoretical thickness of the metal deposition layer 104 deposited when the battery cell is charged is (10000×M) / (C a ×ρ a ), the unit is μm. 10000 is the coefficient for conversion between units (i.e. micrometers and centimeters).

[0080] The mass of the positive electrode active material per unit area of ​​the positive electrode active material layer is recorded as m1 g / cm 2, the mass gram capacity of the positive electrode active material is recorded as C1 mAh / g, then M=m1×C1.

[0081] The capacity per unit area of ​​the positive electrode active material layer and the mass gram capacity of the positive electrode active material can be obtained by testing a button cell. During the test, a button cell can be assembled in an argon atmosphere glove box with a metal sheet (such as a lithium sheet or a sodium sheet) that is the same as the metal deposited when the battery cell is charged as a counter electrode and a positive electrode sheet.

[0082] At 25°C, the prepared button battery was left to stand for 6 hours, fully charged at 0.1C and fully discharged at 0.1C to obtain the discharge capacity. Then, the capacity per unit area of ​​the positive electrode active material layer and the mass gram capacity of the positive electrode active material can be calculated based on the discharge capacity.

[0083] The isolation film of the button cell may be a polyethylene film with a thickness of 12 μm.

[0084] The solvent of the electrolyte of the button cell may be diethylene glycol dimethyl ether (DEGDME), the solute may be LiPF6 or NaPF6 (the type of metal ions is consistent with the type of metal deposited when the battery cell is charged), and the concentration is 1 mol / L.

[0085] The assembly process of the button cell can adopt the technology known in the art, for example, it can be assembled from the positive electrode shell from bottom to top, or it can be assembled from the negative electrode shell from bottom to top, and the entire assembly process is carried out in an argon atmosphere glove box with a water content of less than 10ppm.

[0086] The thickness of the insulating coating, the thickness of the positive electrode active material layer, and the thickness of the interface modification layer can be measured using a micrometer. For accuracy, multiple positions (e.g., 5-10) can be taken for measurement and then the average value is taken.

[0087] In some embodiments, the metal deposition layer 104 deposited when the battery cell is charged may be a sodium metal layer or a lithium metal layer.

[0088] When the metal deposition layer 104 deposited during battery cell charging is a sodium metal layer, the theoretical gram capacity C of the metal (i.e., sodium) deposited during battery cell charging is a mAh / g is 1166mAh / g, and the theoretical density of the metal (i.e. sodium) deposited when the battery cell is charged is ρ a g / cm 3 0.968g / cm 3 (i.e. density at 25°C).

[0089] When the metal deposition layer 104 deposited during battery cell charging is a lithium metal layer, the theoretical gram capacity C of the metal (i.e., lithium) deposited during battery cell charging is amAh / g is 3860mAh / g, and the theoretical density of the metal (i.e. lithium) deposited when the battery cell is charged is ρ a g / cm 3 0.534 g / cm 3 (i.e. density at 25°C).

[0090] In some embodiments, the density of the insulating coating 102 may be greater than or equal to 20%, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and also making the battery have high reliability and good cycle performance.

[0091] Optionally, the density of the insulating coating 102 may be 30%-85%, 50%-80%, thereby further reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby further reducing the internal short circuit problem of the battery.

[0092] The density of the insulating coating is well known in the art and can be measured using instruments and methods known in the art. The density of the insulating coating = (P1 / P2) × 100%. P1 represents the apparent density of the sample, which can be calculated based on the weight and volume of the sample; P2 represents the true density of the sample, which can be measured using a true density tester using an inert gas (such as nitrogen) as a medium and a gas displacement method in accordance with GB / T 24586-2009. During the test, a sample of a suitable size can be cut out from the area of ​​the negative electrode sheet that contains the insulating coating but does not contain the interface modification layer for testing. When the insulating coating is located on both surfaces of the negative electrode current collector, the insulating coating on one side can be scraped off for testing.

[0093] In some embodiments, inorganic insulating fillers are dispersed in the insulating coating 102. The inorganic insulating fillers are electronic insulating materials, which are conducive to the metal being preferentially deposited on the interface modification layer or the negative electrode current collector, and avoiding the metal being deposited on the insulating coating as much as possible, thereby reducing the capacity loss of the battery.

[0094] The density of the insulating coating is related to the parameters of the insulating coating (such as thickness, surface density, etc.), the parameters of the inorganic insulating filler in the insulating coating (such as particle size, particle morphology, particle stacking morphology), and the content of the inorganic insulating filler and the binder. The density of the insulating coating can be adjusted by adjusting one or more of the above parameters.

[0095] In some embodiments, the volume distribution particle size Dv50 of the inorganic insulating filler may be less than or equal to 2 μm, and may be optionally 0.001 μm-0.5 μm. When the volume distribution particle size Dv50 of the inorganic insulating filler is within the above range, it is conducive to the close stacking of the inorganic insulating filler, and can also improve the density of the insulating coating, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0096] The volume distribution particle size Dv50 of the material is well known in the art, which indicates the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 50%, and can be measured using instruments and methods well known in the art. For example, it can be conveniently measured using a laser particle size analyzer with reference to GB / T19077-2016. The test instrument can be the Mastersizer 2000E laser particle size analyzer of Malvern Instruments Ltd., UK.

[0097] In some embodiments, the thickness of the insulating coating 102 is recorded as H0 μm, the volume distribution particle size Dv50 of the inorganic insulating filler is recorded as D0 μm, and H0 / D0 ≥ 5. H0 / D0 can reflect the number of stacked layers of the inorganic insulating filler. When the number of stacked layers of the inorganic insulating filler is large, the density and uniformity of the insulating coating can be improved, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0098] In some embodiments, the tap density of the inorganic insulating filler may be 0.8 g / cm 3 -2.0g / cm 3 , optional 0.95g / cm 3 -1.40g / cm 3 When the tap density of the inorganic insulating filler is within the above range, the density of the insulating coating can be improved, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery and making the battery have high reliability and good cycle performance.

[0099] The tap density of a material is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured using a powder tap density tester in accordance with GB / T 5162-2006. The test instrument can be Dandong Better BT-301, and the test parameters are as follows: vibration frequency 250±15 times / min, amplitude 3±0.2mm, vibration number 5000 times, and measuring cylinder 25mL.

[0100] In some embodiments, the specific surface area of ​​the inorganic insulating filler may be 3 m 2 / g-25m 2 / g, optional 7m 2 / g-20m 2 When the specific surface area of ​​the inorganic insulating filler is within the above range, the density of the insulating coating can be improved, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and also making the battery have high reliability and good cycle performance.

[0101] The specific surface area of ​​a material is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured by using the nitrogen adsorption specific surface area analysis test method according to GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method, wherein the nitrogen adsorption specific surface area analysis test can be measured using the ASAP 3020 surface area and pore size analyzer from Micromeritics, USA.

[0102] The inorganic insulating filler in the insulating coating is a known material and can also be directly commercially available. In some embodiments, the inorganic insulating filler in the insulating coating includes one or more of ceramics, silicates, minerals, and glasses. Optionally, the inorganic insulating filler includes one or more of aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, aluminum magnesium silicate, lithium magnesium silicate, sodium magnesium silicate, boehmite, mica, bentonite, hectorite, kaolin, and talc.

[0103] The insulating coating layer also contains a binder, which is used to bind the inorganic insulating filler to the negative electrode current collector. The binder in the insulating coating layer is a known material and can also be directly commercially available. In some embodiments, the binder in the insulating coating includes styrene-butadiene copolymer, acrylate-styrene-butadiene copolymer, acrylonitrile-butadiene copolymer, acrylonitrile-butadiene-styrene copolymer, acrylic rubber, butyl rubber, styrene-butadiene rubber, fluororubber, polyethylene, polypropylene, ethylene propylene diene rubber (EPM), ethylene propylene diene rubber (EPDM), polyethylene oxide, polyepichlorohydrin, polyvinyl pyrrolidone, polyphosphazene, polyacrylonitrile, polystyrene, polyvinyl pyridine, chlorosulfonated polyethylene, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, hydroxypropyl methylcellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene, polyacrylic acid (PAA), polyimide, polyamideimide, polyimide-polyamideimide copolymer, and one or more of the polymers in which the foregoing polymers are partially or fully substituted with alkali metals.

[0104] In some embodiments, the weight content of the inorganic insulating filler in the insulating coating may be 10%-90%, optionally 10%-80%, and more optionally 20%-70%, based on the total weight of the insulating coating.

[0105] In some embodiments, the weight content of the binder in the insulating coating may be greater than or equal to 10%, optionally 20%-90%, and more optionally 30%-80%, based on the total weight of the insulating coating.

[0106] By adjusting the weight content of the inorganic insulating filler and / or binder in the insulating coating within the above range, the density and uniformity of the insulating coating can be improved, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery and making the battery have high reliability and good cycle performance.

[0107] In some embodiments, the surface density of the insulating coating can be 0.06 mg / cm 2 -13.0mg / cm 2 , optional 0.10mg / cm 2 -3.50mg / cm 2 When the surface density of the insulating coating is within the above range, the density and uniformity of the insulating coating can be improved, thereby reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery and making the battery have high reliability and good cycle performance.

[0108] In some embodiments, the two insulating coatings 102 are respectively a first insulating coating and a second insulating coating. The first insulating coating is located on the negative electrode ear side of the negative electrode plate. The width of the first insulating coating is recorded as W1, and the width of the second insulating coating is recorded as W2. W1 is greater than or equal to 0.5 mm, W2 is greater than or equal to 0.5 mm, and W1 / W2 is greater than or equal to 0.5, which can be selected as 1-3.

[0109] The current density in the negative electrode tab area is usually widely distributed and the temperature in the negative electrode tab area is higher, so the metal deposition growth is looser and it is easier to form dendrites in the negative electrode tab area. By adjusting W1 / W2 within the above range, the performance of the battery can be further improved and the internal short circuit problem of the battery can be further reduced.

[0110] In some embodiments, the width W1 of the first insulating coating layer may be 0.5 mm-20 mm, and may be 1 mm-15 mm.

[0111] In some embodiments, the width W2 of the second insulating coating layer may be 0.5 mm-10 mm, and may be 1 mm-5 mm.

[0112] The width of the first insulating coating, the width of the second insulating coating, and the width of the interface modification layer can be measured using a soft ruler with a minimum quantile of 0.5 mm. For accuracy, multiple positions (e.g., 5-10) can be taken for measurement and then the average value is taken.

[0113] Figure 3 Schematic diagrams of the structures of electrode assemblies provided in other embodiments of the present application are shown. Figure 4 Show Figure 3 Schematic diagram of the structure of the electrode assembly after charging.

[0114] like Figure 3 and Figure 4 As shown, the negative electrode plate includes an interface modification layer 103, and the interface modification layer 103 is located between two insulating coatings 102. The interface modification layer 103 is an alkali metal affinity material layer, such as a sodium affinity layer or a lithium affinity layer.

[0115] Setting an interface modification layer on the negative electrode surface of the negative electrode-free battery can induce uniform metal deposition and alleviate the volume expansion of the negative electrode plate during the charging and discharging process, thereby further reducing the internal short circuit problem of the battery caused by dendrite growth at the negative end during the charging and discharging process of the battery, making the battery have high reliability and good cycle performance.

[0116] In some embodiments, the width of the interface modification layer 103 is greater than the width of the positive electrode active material layer 202. This is beneficial for the metal to be preferentially deposited on the interface modification layer when the battery is charged, and to avoid metal deposition on the insulating coating as much as possible, thereby reducing the capacity loss of the battery.

[0117] In some embodiments, the bonding force between the insulating coating 102 and the isolation film 300 may be greater than the bonding force between the interface modification layer 103 and the isolation film 300. This can make the insulating coating and the isolation film bonded better, and can further reduce the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0118] In some embodiments, the bonding force between the insulating coating 102 and the isolation film 300 may be 3N / m-50N / m, and may be 4N / m-25N / m. This may allow the insulating coating to bond better to the isolation film, and may further reduce the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and may also allow the battery to have high reliability and good cycle performance.

[0119] In some embodiments, the two insulating coatings 102 are respectively a first insulating coating and a second insulating coating. The first insulating coating is located on the negative electrode ear side of the negative electrode sheet. The width of the first insulating coating is recorded as W1, the width of the second insulating coating is recorded as W2, and the width of the interface modification layer 103 is recorded as W a , W1 / W a It can be 0.01-0.1, and can be 0.01-0.05; and / or, W2 / W a It can be 0.01-0.1, and can be optionally 0.01-0.05. This is beneficial to improving the processability of the negative electrode sheet and can also make the battery have a high energy density.

[0120] In some embodiments, the width of the interface modification layer 103 may be 50 mm-200 mm, and may be 70 mm-150 mm.

[0121] In some embodiments, the thickness of the interface modification layer 103 may be 1 μm-50 μm, and may be 1 μm-20 μm.

[0122] In some embodiments, alkali metal affinity materials are dispersed in the interface modification layer 103, and the alkali metal affinity materials are sodium affinity materials or lithium affinity materials. Thus, the interface modification layer can provide some active points to induce uniform metal deposition, thereby improving the cycle performance of the battery, and further reducing the problem of internal short circuit of the battery caused by dendrite growth at the negative terminal during the battery charging and discharging process, so that the battery has high reliability.

[0123] In some embodiments, the alkali metal affinity material in the interface modification layer 103 is a known material and can also be directly commercially available, for example, it can include one or more of carbon materials, metals, metal alloys, and metal oxides. The metal elements in the metals, metal alloys, and metal oxides are all known elements, for example, they can include one or more of Zn, Ag, Al, Mg, Sn, and Au.

[0124] In some embodiments, the carbon material may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, carbon nanofibers, soft carbon, and hard carbon.

[0125] In order to improve the battery performance, the negative electrode of the negative electrode-free battery can also be provided with some conventional substances that can be used as negative electrode active materials, such as carbon materials. Although these substances have a certain capacity, due to their low content and the fact that they are not used as the main negative electrode active materials in the battery, the battery thus constructed can still be regarded as a negative electrode-free battery. The CB (Cell Balance) value of a negative electrode-free battery is usually very small. For example, in some embodiments, the CB value of a negative electrode-free battery can be less than or equal to 0.1. The CB value is the unit area capacity of the negative electrode in the battery divided by the unit area capacity of the positive electrode. Since the negative electrode-free battery does not contain or only contains a small amount of negative electrode active materials, the unit area capacity of the negative electrode is small, and thus the CB value is very small, for example, usually less than or equal to 0.1.

[0126] The interface modification layer may also include a binder. The binder is a known material and may also be directly commercially available. In some embodiments, the binder in the interface modification layer 103 may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), sodium carboxymethyl cellulose (CMC), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0127] In some embodiments, the weight content of the alkali metal affinity material in the interface modification layer 103 may be 2%-98%, optionally 5%-80%, based on the total weight of the interface modification layer 103 .

[0128] In some embodiments, the weight content of the binder in the interface modification layer 103 may be 2%-98%, optionally 20%-95%, based on the total weight of the interface modification layer 103 .

[0129] Figure 5 Schematic diagrams of the structures of electrode assemblies provided in some other embodiments of the present application are shown.

[0130] like Figure 5As shown, in some embodiments, the insulating coating 102 may include a first sublayer 1021 and a second sublayer 1022 located between the first sublayer 1021 and the negative electrode current collector 101 .

[0131] In some embodiments, the first sublayer 1021 is not dispersed with inorganic insulating fillers, and the second sublayer 1022 is dispersed with inorganic insulating fillers. This can make the insulating coating and the isolation film bonded better, and can further reduce the negative terminal dendrites growing along the pores of the insulating coating during the battery charging and discharging process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance. At this time, the weight content of the binder in the first sublayer 1021 is 100%.

[0132] In some embodiments, inorganic insulating fillers are dispersed in the first sublayer 1021, and inorganic insulating fillers are dispersed in the second sublayer 1022, and the weight content of the inorganic insulating fillers in the first sublayer 1021 is less than the weight content of the inorganic insulating fillers in the second sublayer 1022. This can make the insulating coating and the isolation film bond better, and can further reduce the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and can also make the battery have high reliability and good cycle performance.

[0133] In some embodiments, the weight content of the binder in the first sub-layer 1021 is greater than or equal to 15%, and the weight content of the inorganic insulating filler is less than or equal to 85%, based on the total weight of the first sub-layer.

[0134] This can make the insulating coating and the isolation membrane bond better, and can further reduce the continuous growth of dendrites at the negative end along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery and making the battery have high reliability and good cycle performance.

[0135] In some embodiments, the weight content of the binder in the second sub-layer 1022 may be 1%-30%, and the weight content of the inorganic insulating filler may be 70%-99%, based on the total weight of the second sub-layer.

[0136] Optionally, the weight content of the binder in the second sub-layer 1022 may be 5%-30%, and the weight content of the inorganic insulating filler may be 70%-95%, based on the total weight of the second sub-layer.

[0137] As a result, the insulating coating has high density, high uniformity and good resistance to dendrite penetration, which can reduce the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during battery charging and discharging, thereby reducing the internal short circuit problem of the battery and making the battery have high reliability and good cycle performance.

[0138] The types of inorganic insulating fillers in the first sublayer and the second sublayer can be the same or different, and the types of binders in the first sublayer and the second sublayer can be the same or different. The types of inorganic insulating fillers and binders can be as described above and will not be repeated here.

[0139] In some embodiments, the thickness ratio of the first sublayer 1021 to the second sublayer 1022 may be (0.1-0.9): 1, and may be (0.2-0.5): 1. When the thickness ratio of the first sublayer to the second sublayer is within the above range, the insulating coating and the isolation film can be better bonded, and the insulating coating can have high density, high uniformity, and good resistance to dendrite puncture, thereby further reducing the continuous growth of dendrites at the negative terminal along the pores of the insulating coating during the battery charge and discharge process, thereby reducing the internal short circuit problem of the battery, and also making the battery have high reliability and good cycle performance.

[0140] In some embodiments, the negative electrode current collector 101 may include one or more of a metal foil, a metal foam current collector, a metal mesh current collector, a carbon felt current collector, a carbon cloth current collector, a carbon paper current collector, and a composite current collector.

[0141] In some embodiments, the negative electrode current collector 101 may have a porous structure. For example, the negative electrode current collector 101 may include one or more of a porous aluminum foil, a porous copper foil, and a porous stainless steel foil.

[0142] In some embodiments, the negative electrode current collector 101 may include a polymer material base layer and a conductive metal layer formed on at least one side of the polymer material base layer.

[0143] Optionally, the metal material in the conductive metal layer may include one or more of copper, copper alloy, aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy.

[0144] Optionally, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0145] The preparation method of the negative electrode sheet is well known. In some embodiments, the interface modification layer slurry and the insulating coating slurry can be coated on the negative electrode current collector and dried. The coating method can include gravure coating, micro gravure coating, extrusion coating, transfer coating or spraying.

[0146] The positive electrode sheet includes a positive current collector 201 and a positive active material layer 202 located on at least one side of the positive current collector 201. The positive current collector 201 has two surfaces opposite to each other in its thickness direction, and the positive active material layer 202 is located on either or both of the two opposite surfaces of the positive current collector 201. Figures 1 to 5 As shown, the positive electrode active material layer 202 is located on one side of the positive electrode current collector 201 , but the present application is not limited thereto.

[0147] The positive electrode active material layer 202 includes a positive electrode active material.

[0148] When the battery cell is a negative electrode-free lithium battery cell, the positive electrode active material includes a material capable of extracting and inserting lithium. As an example, the positive electrode active material may include one or more of a lithium transition metal oxide, a lithium-containing phosphate, and their respective modified compounds. Examples of lithium transition metal oxides may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of lithium-containing phosphates may include one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.

[0149] When the battery cell is a sodium battery cell without a negative electrode, the positive electrode active material includes a material capable of extracting and embedding sodium. As an example, the positive electrode active material may include one or more of a layered transition metal oxide (including P2 type, O3 type, etc.), a polyanion material (such as phosphate, fluorophosphate, pyrophosphate, sulfate, etc.), and a Prussian material.

[0150] In some embodiments, the positive electrode active material may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, Na 0.67 MO2 (M may include at least two of Fe, Co, Cr, Mn, Ni, V, Ti, and Mo), NaMO2 (M may include at least two of Fe, Co, Ni, V, Ti, and Mo), NaFePO4, NaMnPO4, NaCoPO4, Na4Fe3(PO4)2O7, Na3V2(PO4)2F3, Na3V2(PO4)3, sodium iron pyrophosphate, Prussian blue, Prussian white, and one or more of their respective modified compounds.

[0151] The modified compounds of the above-mentioned positive electrode active materials may be the ones that undergo doping modification and / or surface coating modification on the positive electrode active materials.

[0152] In some embodiments, the positive active material layer 202 may further include a positive conductive agent, which may include, for example, one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0153] In some embodiments, the positive electrode active material layer 202 may further include a positive electrode binder. As an example, the positive electrode binder may include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorine-containing acrylic resin, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), carboxymethyl chitosan (CMCS) One or more.

[0154] In some embodiments, the thickness of the positive electrode active material layer 202 may be 60 μm-150 μm, and may be 68 μm-135 μm.

[0155] In some embodiments, the positive electrode current collector 201 may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one side of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0156] The positive electrode active material layer 202 is usually formed by coating the positive electrode slurry on the positive electrode current collector 201, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, optional positive electrode conductive agent, optional positive electrode binder and any other components in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP).

[0157] The separator 300 is disposed between the positive electrode sheet and the negative electrode sheet, and mainly plays the role of preventing internal short circuit. The present application has no particular limitation on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0158] In some embodiments, the material of the isolation film 300 may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation film 300 may be a single-layer film or a multi-layer composite film. When the isolation film is a multi-layer composite film, the materials of each layer are the same or different.

[0159] The battery cell also includes an electrolyte. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can include one or more selected from solid electrolytes and liquid electrolytes (ie, electrolytes).

[0160] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0161] When the battery cell is a negative electrode-free lithium battery cell, as an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0162] When the battery cell is a negative electrode-free sodium battery cell, as an example, the electrolyte salt may include one or more of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobis(oxalatophosphate) (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP).

[0163] In some embodiments, the solvent may include one or more of an ester solvent, a sulfone solvent, and an ether solvent. As an example, the solvent may include but is not limited to one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), diethyl sulfone (ESE), dimethoxymethane (DMM), diethylene glycol dimethyl ether (DG), ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (DEGDME), and tetraethylene glycol dimethyl ether.

[0164] In some embodiments, the electrolyte may also optionally include additives, for example, additives that can improve certain properties of the battery, such as additives that improve the overcharge performance of the battery, additives that improve the high temperature performance of the battery, additives that improve the low temperature power performance of the battery, etc.

[0165] The preparation method of battery cells is well known. In some embodiments, the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, and the above-mentioned electrolyte is injected after drying. After packaging, standing, formation and other processes, a battery cell is obtained. Multiple battery cells can also be further connected in series, in parallel or in mixed connection to form a battery module. Multiple battery modules can also be connected in series, in parallel or in mixed connection to form a battery pack. In some embodiments, multiple battery cells can also directly form a battery pack.

[0166] The embodiment of the present application also provides an electrical device, which includes a battery provided in the embodiment of the present application, and the battery is used to provide electrical energy. The battery can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0167] The electrical device can select a specific type of battery, such as a battery cell, a battery module or a battery pack, according to its usage requirements.

[0168] Figure 6 Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used.

[0169] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a battery cell may be used as a power source.

[0170] Example

[0171] The following examples describe the disclosure of the present application in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present application are apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0172] Example 1

[0173] (1) Preparation of negative electrode sheet

[0174] Carbon nanotubes (CNT) and sodium carboxymethyl cellulose (CMC) were fully stirred and mixed in a proper amount of solvent deionized water at a weight ratio of 80:20 to form an interface modification layer slurry.

[0175] The inorganic insulating filler alumina and the binder polyacrylic acid (PAA) were fully stirred and mixed in an appropriate amount of solvent deionized water at a weight ratio of 70:30 to form an insulating coating slurry. The volume distribution particle size Dv50 of the alumina was 0.25 μm and the tap density was 1.38 g / cm 3 , specific surface area is 13.4m 2 / g.

[0176] The interface modification layer slurry is coated on the surface of the negative electrode current collector copper foil, and the insulating coating slurry is coated on both sides of the interface modification layer slurry in the width direction. After drying and welding the negative electrode tab, the negative electrode sheet is obtained.

[0177] The thickness of the interface modification layer is 5 μm, and the thickness of the two insulating coatings is 20.4 μm.

[0178] (2) Preparation of positive electrode sheet

[0179] The positive electrode active material sodium iron pyrophosphate, the conductive agent carbon black (Super P), and the binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an appropriate amount of solvent NMP at a weight ratio of 90:5:5 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained. The mass of the positive electrode active material per unit area in the positive electrode active material layer is 0.01568g / cm 2 The mass capacity of the positive electrode active material is 100 mAh / g, and the capacity per unit area of ​​the positive electrode active material layer is 1.568 mAh / cm 2 , the thickness of the positive electrode active material layer is 101 μm.

[0180] (3) Preparation of electrolyte

[0181] The fully dried NaPF6 was dissolved in diethylene glycol dimethyl ether (DEGDME) to prepare an electrolyte with a concentration of 1 mol / L.

[0182] (4) Preparation of isolation membrane

[0183] A porous polyethylene membrane was used as the separator.

[0184] (5) Preparation of batteries

[0185] The positive electrode sheet, the separator, and the negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, a negative electrode-free sodium battery is obtained.

[0186] Example 2

[0187] The preparation method of the battery is similar to that of Example 1, except that in the preparation of the negative electrode plate, the thickness of the insulating coating is 22.5 μm.

[0188] Example 3

[0189] The preparation method of the battery is similar to that of Example 1, except that in the preparation of the negative electrode plate, the thickness of the insulating coating is 30.0 μm.

[0190] Example 4

[0191] The preparation method of the battery is similar to that of Example 1, except that in the preparation of the negative electrode sheet, the thickness of the insulating coating is 20.0 μm, and the mass of the positive electrode active material per unit area in the positive electrode active material layer is 0.00941 g / cm 2 The mass capacity of the positive electrode active material is 100 mAh / g, and the capacity per unit area of ​​the positive electrode active material layer is 0.941 mAh / cm 2 , the thickness of the positive electrode active material layer is 68 μm.

[0192] Example 5

[0193] The preparation method of the battery is similar to that of Example 1, except that in the preparation of the negative electrode sheet, the thickness of the insulating coating is 33.5 μm, and the mass of the positive electrode active material per unit area in the positive electrode active material layer is 0.02509 g / cm 2 The mass capacity of the positive electrode active material is 100 mAh / g, and the capacity per unit area of ​​the positive electrode active material layer is 2.509 mAh / cm 2 , the thickness of the positive electrode active material layer is 135 μm.

[0194] Comparative Example 1

[0195] The preparation method of the battery is similar to that of Example 1, except that the preparation process of the negative electrode plate is different.

[0196] Carbon nanotubes (CNT) and sodium carboxymethyl cellulose (CMC) were fully stirred and mixed in a proper amount of solvent deionized water at a weight ratio of 80:20 to form an interface modification layer slurry.

[0197] The interface modification layer slurry is coated on the surface of the negative electrode current collector copper foil, and after drying and welding the negative electrode tab, a negative electrode sheet is obtained.

[0198] Comparative Example 2

[0199] The preparation method of the battery is similar to that of Example 5, except that in the preparation of the negative electrode plate, the thickness of the insulating coating is 5.0 μm.

[0200] Comparative Example 3

[0201] The preparation method of the battery is similar to that of Example 5, except that in the preparation of the negative electrode plate, the thickness of the insulating coating is 27.2 μm.

[0202] Comparative Example 4

[0203] The preparation method of the battery is similar to that of Example 1, except that in the preparation of the negative electrode plate, the thickness of the insulating coating is 130.0 μm.

[0204] Performance Testing

[0205] (1) Cyclic performance test

[0206] At 25°C, the prepared battery was charged at 1C constant current to a voltage of 3.65V, then charged at 3.65V constant voltage to a current of 0.05C, and after standing for 5 minutes, the battery was discharged at 1C constant current to a voltage of 2.0V. This is a charge and discharge cycle process, and the discharge capacity this time is the discharge capacity of the battery after the first cycle. The battery was cycled 500 times in the above manner.

[0207] The capacity retention rate of the battery after 500 cycles = the discharge capacity after 500 cycles / the discharge capacity after the first cycle.

[0208] (2) Sodium analysis test

[0209] At 25°C, the prepared battery was charged at a constant current of 5C to a voltage of 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C. After standing for 5 minutes, the battery was discharged at a constant current of 1C to a voltage of 2.0V. This was a charge and discharge cycle. The battery was cycled 10 times in the above manner, then charged at a constant current of 5C to a voltage of 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C, and the battery was disassembled to observe the sodium precipitation at the junction of the interface modification layer at the negative terminal and the insulating coating.

[0210] The degree of sodium precipitation can be determined as follows.

[0211] Failure: The width of the area where sodium dendrites are precipitated is greater than or equal to 80% of the width of the insulating coating.

[0212] Severe precipitation: The width of the area where sodium dendrites are precipitated is greater than or equal to 50% but less than 80% of the width of the insulating coating.

[0213] Moderate precipitation: The width of the area where sodium dendrites are precipitated is greater than or equal to 20% but less than 50% of the width of the insulating coating.

[0214] Slight precipitation: The width of the area where sodium dendrites are precipitated is greater than or equal to 5% but less than 20% of the width of the insulating coating.

[0215] No precipitation: The width of the area where sodium dendrites are precipitated is less than 5% of the width of the insulating coating.

[0216] The test results are shown in Table 1 and Table 2. In Table 2, since no insulating coating is provided on the negative electrode current collector of Comparative Example 1, "failure" means that the width of the region where sodium dendrites are precipitated is greater than 5 mm.

[0217] Table 1

[0218]

[0219] Table 2

[0220]

[0221] It can be seen from the test results of Examples 1 to 5 and Comparative Examples 2 to 3 that configuring the thickness of the insulating coating to be greater than 1.1 times the theoretical thickness of the metal deposition layer deposited when the battery is charged and the sum of the thickness of the interface modification layer can reduce the degree of sodium precipitation on the surface of the negative electrode plate, thereby effectively reducing the problem of internal short circuit in the battery caused by dendrite growth at the negative terminal position, and can also improve the cycle performance of the battery.

[0222] From the test results of Examples 1 to 5 and Comparative Example 4, it can be seen that the thickness of the insulating coating is configured to be less than the theoretical thickness of the metal deposition layer deposited when the battery is charged, the thickness of the positive electrode active material layer and the thickness of the interface modification layer, which can improve the cycle performance of the battery. This is because when the thickness of the insulating coating is configured to be greater than the theoretical thickness of the metal deposition layer deposited when the battery is charged, the thickness of the positive electrode active material layer and the thickness of the interface modification layer, misalignment occurs when the pole pieces are stacked, thereby causing the ion transmission path between the positive electrode and the negative electrode to become longer, thereby affecting the performance of the battery.

[0223] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A battery cell, comprising a positive electrode sheet and a negative electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector; The negative electrode plate comprises a negative electrode current collector and two insulating coatings arranged on the surface of the negative electrode current collector close to the positive electrode plate, the distance between the two insulating coatings is greater than the width of the positive electrode active material layer, and the two insulating coatings are not directly opposite to the positive electrode active material layer; The negative electrode plate may further include an interface modification layer disposed on the negative electrode current collector and between the two insulating coatings; The thickness of the insulating coating is configured to be greater than 1.1 times the theoretical thickness of the metal deposition layer deposited when the battery cell is charged and the thickness of an optional interface modification layer, and less than the sum of the theoretical thickness of the metal deposition layer deposited when the battery cell is charged, the thickness of the positive electrode active material layer and the thickness of an optional interface modification layer.

2. The battery cell according to claim 1, characterized in that: The thickness of the insulating coating is configured to be greater than 1.25 times the theoretical thickness of the metal deposition layer deposited when the battery cell is charged and the thickness of an optional interface modification layer, and less than the sum of the theoretical thickness of the metal deposition layer deposited when the battery cell is charged, the thickness of the positive electrode active material layer and the thickness of an optional interface modification layer.

3. The battery cell according to claim 1, characterized in that: The capacity per unit area of ​​the positive electrode active material layer is recorded as M mAh / cm 2 The theoretical gram capacity of the metal deposited when the battery cell is charged is recorded as C a mAh / g, the theoretical density of the metal deposited when the battery cell is charged is recorded as ρ a g / cm 3 , then the theoretical thickness of the metal deposition layer deposited when the battery cell is charged is (10000×M) / (C a ×ρ a ), unit is μm.

4. The battery cell according to claim 1, characterized in that: The density of the insulating coating is greater than or equal to 20%.

5. The battery cell according to claim 4, characterized in that: The density of the insulating coating is 50%-80%.

6. The battery cell according to claim 1, characterized in that: The two insulating coatings are respectively a first insulating coating and a second insulating coating, the first insulating coating is located on the negative electrode ear side of the negative electrode plate, the width of the first insulating coating is recorded as W1, the width of the second insulating coating is recorded as W2, W1 is greater than or equal to 0.5 mm, W2 is greater than or equal to 0.5 mm, and W1 / W2 is greater than or equal to 0.

5.

7. The battery cell according to claim 6, characterized in that: W1 / W2 is 1-3.

8. The battery cell according to claim 6, characterized in that: W1 is 0.5 mm to 20 mm; and / or, W2 is 0.5mm-10mm.

9. The battery cell according to claim 8, characterized in that: W1 is 1 mm to 15 mm; and / or W2 is 1mm-5mm.

10. The battery cell according to claim 1, characterized in that: The width of the interface modification layer is greater than the width of the positive electrode active material layer.

11. The battery cell according to any one of claims 1 to 10, characterized in that: The battery cell further includes a separator, which is located between the positive electrode sheet and the negative electrode sheet. The bonding force between the insulating coating and the isolation film is greater than the bonding force between the interface modification layer and the isolation film; and / or, The bonding force between the insulating coating and the isolation film is 3N / m-50N / m.

12. The battery cell according to claim 11, characterized in that: The bonding force between the insulating coating and the isolation film is 4N / m-25N / m.

13. The battery cell according to claim 1, characterized in that: The two insulating coatings are respectively a first insulating coating and a second insulating coating. The first insulating coating is located on the negative electrode ear side of the negative electrode plate. The width of the first insulating coating is recorded as W1, the width of the second insulating coating is recorded as W2, and the width of the interface modification layer is recorded as W a , W1 / W a is 0.01-0.1; and / or, W2 / W a It is 0.01-0.

1.

14. The battery cell according to claim 13, characterized in that: W1 / W a is 0.01-0.05; and / or, W2 / W a It is 0.01-0.

05.

15. The battery cell according to claim 1, characterized in that: The width of the interface modification layer is 50 mm to 200 mm; and / or, The thickness of the interface modification layer is 1 μm-50 μm.

16. The battery cell according to claim 15, characterized in that: The width of the interface modification layer is 70 mm to 150 mm; and / or, The thickness of the interface modification layer is 1 μm-20 μm.

17. The battery cell according to claim 1, characterized in that: The battery cell is a negative electrode-free sodium battery cell or a negative electrode-free lithium battery cell.

18. A battery, characterized in that: A battery cell comprising the battery cell according to any one of claims 1 to 17.

19. An electrical device, characterized in that: The battery according to claim 18 is used to provide electrical energy.