Current collector, electrode plates and battery

By setting recesses on the surface of the metal wires of the current collector and controlling the ratio of their diameter to roughness, and combining them with a conductive layer, the problem of low bonding strength between the active material layer and the current collector is solved, thereby reducing the battery's internal resistance and improving its electrochemical performance.

CN224986291UActive Publication Date: 2026-11-17EVE ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522417937.5
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2025-11-13
Publication Date
2026-11-17
Estimated Expiration
2035-11-13

AI Technical Summary

Technical Problem

In existing lithium batteries, the bonding strength between the active material layer and the current collector surface is low, resulting in poor electrode structure stability and high interface impedance, which increases the battery's internal resistance.

Method used

By creating recesses on the surface of the metal wires in the current collection mesh and controlling the ratio of the wire diameter to the surface roughness, an interlocking structure is formed, which enhances the bonding force between the active material and the mesh body. The conductive layer reduces the interfacial contact resistance and optimizes the current collection effect.

Benefits of technology

This improved the bonding strength between the active material and the current collector, reduced the battery's internal resistance, and enhanced electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN224986291U_ABST
    Figure CN224986291U_ABST
Patent Text Reader

Abstract

This application discloses a current collector, an electrode, and a battery, belonging to the field of battery technology. The current collector includes a mesh body, which comprises multiple cross-connected metal wires. The surfaces of the metal wires are partially concave to form recesses, and the ratio of the wire diameter to its surface roughness Ra is 125-357. This application uses recesses on the surface of the metal wires to embed the active material within these recesses, forming an interlocking structure and improving the bonding force between the active material and the mesh body. By controlling the ratio of the wire diameter to its surface roughness Ra, the surface of the metal wires has appropriately sized and numerous recesses, allowing the active material to fully, tightly, and firmly contact the mesh body, reducing the internal resistance of the battery cell. Simultaneously, it ensures that the active material fully fills the recesses, reducing the interfacial impedance between the mesh body and the active material, further reducing the internal resistance of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and in particular to a current collector, electrode, and battery. Background Technology

[0002] Lithium-ion batteries possess advantages such as high operating voltage, high energy density, low self-discharge, long cycle life, wide operating temperature range, no memory effect, and safety, making them widely used in electronic devices. Electrode sheets are a crucial component of lithium-ion batteries, comprising a current collector and an active material layer adhered to one side of the current collector. Electrode sheet preparation typically involves uniformly mixing active materials, conductive agents, binders, and solvents in a specific ratio, coating this mixture onto the current collector, drying it, and then performing rolling and slitting steps to obtain the electrode sheet. However, due to the relatively smooth surface of the current collector, the bonding strength between the active material layer and the current collector surface is relatively low, reducing the structural stability of the electrode and also leading to higher interfacial impedance, increasing the battery's internal resistance. Utility Model Content

[0003] This application provides a current collector, an electrode, and a battery, which can improve the technical problems of relatively low bonding strength between the active material layer and the current collector surface, and high internal resistance of the battery cell.

[0004] In a first aspect, embodiments of this application provide a current collection mesh, including a mesh body, the mesh body including a plurality of cross-connected metal wires, the surface of the metal wires being partially concave to form a recess, and the ratio of the diameter of the metal wire to the surface roughness Ra of the metal wire is 125~357.

[0005] This application creates recesses on the surface of a metal wire, allowing the active material to embed within these recesses and form an interlocking structure. This enhances the bonding force between the active material and the mesh body. By controlling the ratio of the wire diameter to its surface roughness Ra, the surface of the wire is designed with appropriately sized recesses. This ensures that the active material (including active substances, conductive agents, and binders) can fully, tightly, and firmly contact the mesh body, reducing the internal resistance of the battery cell. Simultaneously, it ensures that the active material fully fills the recesses, reducing the interfacial impedance between the mesh body and the active material, further lowering the internal resistance of the battery cell.

[0006] Optionally, the diameter of the metal wire is 0.15mm to 0.30mm.

[0007] This application achieves a sufficient current conduction path in the mesh body 10 by reasonably setting the diameter of the metal wire, thereby improving the current collection effect of the mesh body and reducing the internal resistance of the battery cell. At the same time, the appropriate diameter of the metal wire ensures that the area ratio of the mesh body is relatively high, which not only results in a larger filling amount of active material, but also a larger contact area between the active material through the mesh body and the active material on the other side, further reducing the internal resistance of the battery cell. Moreover, the active materials on both sides of the mesh body form an effective bond, thereby improving the bonding strength between the active material and the mesh body.

[0008] Optionally, the surface roughness Ra of the metal wire 11 is 0.7 μm to 1.5 μm.

[0009] This application achieves this by rationally setting the surface roughness Ra of the metal wire, resulting in the formation of physical anchoring points with excellent structure and an appropriate number on the surface of the metal wire. This allows the active material to be in close contact with the mesh body, which not only reduces the internal resistance of the battery cell but also improves the bonding force between the active material and the mesh body. At the same time, it ensures that the active material is fully and completely filled in the recesses on the surface of the metal wire, reducing the interfacial impedance and further reducing the internal resistance of the battery cell.

[0010] Optionally, the cross-section of the wire is polygonal.

[0011] This application sets the cross-section of the metal wire to be polygonal. On the one hand, the polygonal structure facilitates the full etching of the metal wire by physical etching methods such as laser, thereby resulting in a higher bonding force between the active material and the mesh body. On the other hand, the polygonal structure allows the active material to slide better into the mesh of the current collector during the dry preparation of the electrode, achieving full filling of the mesh and reducing the internal resistance of the cell.

[0012] Optionally, the cross-section of the wire is quadrilateral, the wire has four surfaces, and all four surfaces extend at an angle relative to the thickness direction of the mesh body.

[0013] This application sets the cross-section of the metal wire to a quadrilateral shape, with all four surfaces of the metal wire extending at an angle relative to the thickness direction of the mesh body. This not only makes physical etching such as laser etching easier, but also allows the angled surfaces to act as guides, guiding the active material into the mesh openings of the current collector during dry electrode preparation.

[0014] Optionally, the current collector also includes a conductive layer that covers the surface of the metal wires.

[0015] This application provides a conductive layer on the surface of a metal wire. The conductive layer covers the surface of the metal wire, and on the one hand, the conductive layer and the metal wire work together to form a dual conductive path. When the metal wire experiences a conduction interruption due to local microcracks, the conductive layer covering its surface can continue to conduct current, improving the current collection effect of the current collector 100. On the other hand, the conductive layer itself has a low resistivity and can act as a conductive bridge between the metal wire and the active material, reducing the interfacial contact resistance when the metal wire and the active material are in direct contact, and reducing the internal resistance of the battery cell.

[0016] Optionally, the conductive layer includes a carbon layer.

[0017] This application sets the conductive layer to include a carbon layer with extremely low resistivity. The carbon layer can form a continuous conductive network with the conductive agent in the active material, reducing the interfacial contact resistance between the metal wire and the active material, and reducing the internal resistance of the battery cell. Furthermore, the nano-sized carbon layer can fully fill the depressions on the surface of the metal wire, further reducing the internal resistance of the battery cell.

[0018] Optionally, the recessed portion includes one of acid-etched recessed portion, laser-etched recessed portion, and physical extrusion recessed portion; and / or, the mesh body includes one of aluminum mesh, nickel mesh, and stainless steel mesh.

[0019] This application can form uniform depressions on the metal wire through acid etching, laser etching or physical extrusion, thereby increasing the surface roughness Ra of the metal wire and enhancing the bonding force between the mesh body and the active material; by setting different types of mesh bodies, it can be applied to different application scenarios.

[0020] Secondly, this application provides an electrode sheet, including the current collection network provided in the first aspect of this application; and an active material layer disposed on the current collection network.

[0021] The electrode of this application includes the current collector provided in the first aspect of this application, which enables the active material layer to adhere tightly, fully and firmly to the current collector, thereby reducing the internal resistance of the cell.

[0022] Thirdly, this application provides a battery including the electrode provided in the second aspect of this application.

[0023] The battery of this application includes the electrode provided in the second aspect, thus the battery has low internal resistance and excellent electrochemical performance. Attached Figure Description To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0024] To gain a more complete understanding of this application and its beneficial effects, the following description will be provided in conjunction with the accompanying drawings, wherein the same reference numerals in the following description denote the same parts.

[0025] Figure 1 This is a schematic diagram of the structure of the current collection network provided in an embodiment of this application; Figure 2 yes Figure 1 An enlarged schematic diagram of part A in the middle; Figure 3 This is a schematic diagram of the cross-sectional structure of a metal wire; Figure 4 This is a schematic diagram of the cross-sectional structure of the mesh formed by adjacent metal wires; Figure 5 This is a schematic diagram of the electrode structure provided in an embodiment of this application.

[0026] Explanation of reference numerals in the attached figures: 100. Current collector; 10. Mesh body; 11. Metal wire; 111. Recess; 112. Surface; 101. Mesh opening; 110. Active material layer; 200, Electrode. Detailed Implementation

[0027] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. Furthermore, it should be understood that the specific embodiments described herein are only for illustration and explanation of this application and are not intended to limit this application. In this application, unless otherwise stated, directional terms such as "inner" and "outer" refer to the outline of the device.

[0028] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more features. In the description of this application, "multiple" means two or more, "at least one" means one or more, and "multiple" means two or more, unless otherwise explicitly specified. In this application, unless otherwise stated, directional terms such as "inner" and "outer" refer to the outline of the device.

[0029] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used in this application's specification is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items. Additionally, in the description of this application, the term "comprising" means "including but not limited to".

[0030] The technical solution of this application is as follows: Firstly, this application provides a data collection network 100, please refer to [link to relevant documentation]. Figures 1 to 4 , Figures 1 to 4 This is a schematic diagram of the structure of the current collection mesh 100 provided in the embodiments of this application. The current collection mesh 100 includes a mesh body 10, and the mesh body 10 includes multiple metal wires 11 that are cross-connected. The surface 112 of the metal wires 11 is partially concave to form a recess 111 (e.g., Figure 2 As shown), the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 125~357, for example, it can be 125, 150, 167, 208, 250, 300, 350, 357, etc.

[0031] This application sets the mesh body 10 to include multiple cross-connected metal wires 11 to form a mesh structure. The current collector 100 of the mesh structure can not only form multiple conductive paths, but also the three-dimensional mesh structure can increase the contact area between the mesh body 10 and the active materials (including active substances, conductive agents and binders), thereby reducing the internal resistance of the battery cell and improving the specific capacity, energy density and other electrochemical performance of the battery cell.

[0032] It is understandable that a recessed portion 111 is formed by locally recessing the surface 112 of the metal wire 11. The recessed portion 111 can form a physical anchoring point, allowing the active material to be embedded inside the recessed portion 111, thereby forming an interlocking structure and improving the bonding force between the active material and the mesh body 10. The recessed portion 111 can also increase the surface roughness of the metal wire 11, allowing more active material to adhere to the mesh body 10, further improving the electrochemical performance of the battery.

[0033] Understandably, by controlling the ratio of the diameter of the metal wire 11 to its surface roughness Ra to be between 125 and 357, the surface roughness Ra of metal wires 11 with different diameters is ensured to be within an optimal range. This results in the surface 112 of the metal wire 11 having recesses 111 of appropriate degree and quantity, allowing the active material to fully, tightly (meaning the active material is fully filled in the recesses 111, and the active material is in close contact with the surface 112 of the recesses 111), and firmly in contact with the mesh body 10, reducing the internal resistance of the battery cell. Simultaneously, ensuring the active material fully fills the recesses 111 reduces the interfacial impedance between the mesh body 10 and the active material, further reducing the internal resistance of the battery cell. Furthermore, by controlling the ratio of the diameter of the metal wire 11 to its surface roughness Ra, excessive damage to the structure of the metal wire 11 is avoided, ensuring excellent current collection performance of the mesh body 10 and maintaining the mechanical strength of the metal wire 11, thus ensuring the mechanical strength of the mesh body 10.

[0034] In some embodiments, the diameter of the metal wire 11 is 0.15mm to 0.30mm, for example, it can be 0.15mm, 0.20mm, 0.25mm, 0.30mm, etc.

[0035] This application controls the diameter of the metal wire 11 to be 0.15mm~0.30mm, resulting in a better cross-sectional area of ​​the current collection path of the metal wire 11. This allows the mesh body 10 to form a sufficient current conduction path and ensures uniform current distribution, thereby improving the current collection effect of the mesh body 10 and reducing the internal resistance of the battery cell. At the same time, the suitable diameter of the metal wire 11 ensures that the area ratio of the mesh 101 of the mesh body 10 is relatively high. This not only results in a larger filling amount of active material, but also a larger contact area between the active material through the mesh 101 of the mesh body 10 and the active material on the other side, further reducing the internal resistance of the battery cell. Furthermore, the active materials on both sides of the mesh body 10 form an effective bond, thereby improving the bonding strength between the active material and the mesh body 10.

[0036] It is understandable that by controlling the diameter of the metal wire 11, the recess 111 formed on the surface 112 of the metal wire 11 within a suitable diameter range can be well matched with the particle size of the active material, so that the active material can fully fill the recess 111 and improve the energy density of the battery.

[0037] In some embodiments, the surface roughness Ra of the metal wire 11 is 0.7μm to 1.5μm, for example, it can be 0.7μm, 0.8μm, 0.9μm, 1.0μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, etc.

[0038] This application controls the surface roughness Ra of the metal wire 11 to 0.7μm~1.5μm. The suitable roughness allows the surface 112 of the metal wire 11 to form physical anchoring points with excellent structure and appropriate number, thereby enabling the active material to be in close contact with the mesh body 10. This not only reduces the internal resistance of the battery cell, but also improves the bonding force between the active material and the mesh body 10. At the same time, it ensures that the active material is fully and completely filled in the recesses 111 of the surface 112 of the metal wire 11, reducing the interface impedance and further reducing the internal resistance of the battery cell.

[0039] In some embodiments, please refer to Figure 3 and Figure 4 The cross-section of the metal wire 11 is polygonal.

[0040] This application sets the cross-section of the metal wire 11 to be polygonal. On the one hand, the polygonal structure facilitates the thorough etching of the metal wire 11 by physical etching methods such as laser etching, forming recesses 111 and ensuring that the surface roughness Ra of the metal wire 11 is within the required range, thereby resulting in a higher bonding force between the active material and the mesh body 10. On the other hand, the polygonal structure allows the active material to better slide into the mesh openings 101 of the current collector 100 during the dry fabrication of the electrode 200, achieving full filling of the mesh openings 101 and reducing the internal resistance of the cell. At the same time, the multiple edges of the polygonal structure can form an interlocking structure, allowing the active material to be locked in the mesh openings 101. In other words, this application improves the bonding force between the active material and the mesh body 10 through the synergy of macroscopic edges and microscopic recesses 111.

[0041] It is understandable that the planar and edge structure of the polygonal structure can guide the current to be conducted evenly along multiple planes, reduce the current accumulation in a single area, and enable the mesh body 10 to achieve a better current collection effect and reduce the internal resistance of the cell.

[0042] For example, when the cross-section of the wire 11 is polygonal, the diameter of the wire 11 refers to the length of the longest diagonal among the multiple diagonals.

[0043] In some embodiments, please refer to Figure 3 and Figure 4 The metal wire 11 has a quadrilateral cross-section and four surfaces 112, all of which extend obliquely relative to the thickness direction of the mesh body 10. The thickness direction of the mesh openings 101 is... Figure 4 The direction in which the X-axis lies.

[0044] This application, by setting the cross-section of the metal wire 11 to a quadrilateral shape, with all four surfaces 112 of the metal wire 11 extending obliquely relative to the thickness direction of the mesh body 10, not only makes physical etching such as laser etching easier but also improves the etching effect. Simultaneously, the obliquely set surfaces 112 can act as guides, guiding the active material into the mesh openings 101 of the current collector 100 during the dry fabrication of the electrode 200. Additionally, please refer to... Figure 4 Macroscopic mesh 101 is formed between adjacent metal wires 11, which allows the active material to be embedded in a gradient, increasing the compaction density of the active material and thus increasing the energy density of the battery cell.

[0045] In some embodiments, the current collector 100 further includes a conductive layer that covers the surface 112 of the metal wire 11.

[0046] This application provides a conductive layer on the surface 112 of the metal wire 11. The recessed portion 111 ensures that the conductive layer is in close and firm contact with the surface 112 of the metal wire 11. The conductive layer covers the surface 112 of the metal wire 11 (the mesh 101 is not covered by the conductive layer). The conductive layer and the metal wire 11 work together to form a dual conductive path. When the metal wire 11 experiences a conduction interruption due to local microcracks, the conductive layer covering its surface 112 can continue to conduct current, thereby improving the current collection effect of the current collector 100.

[0047] It is understandable that the surface 112 of the metal wire 11 may have an oxide film with extremely high resistivity, while the conductive layer itself has low resistivity. The conductive layer can serve as a conductive bridge between the metal wire 11 and the active material, reducing the interfacial contact resistance when the metal wire 11 is in direct contact with the active material, and reducing the internal resistance of the battery cell.

[0048] In some embodiments, the conductive layer includes a carbon layer.

[0049] This application sets the conductive layer to include a carbon layer. On the one hand, the carbon layer has extremely low resistivity and can form a continuous conductive network with the conductive agent in the active material, reducing the interfacial contact resistance between the metal wire 11 and the active material, and reducing the internal resistance of the battery cell. On the other hand, the nano-sized carbon layer can fully fill the recesses 111 on the surface 112 of the metal wire 11. Compared with the contact gap between the active material and the metal wire 11, the contact gap between the carbon layer and the metal wire 11 is smaller, further reducing the internal resistance of the battery cell.

[0050] Understandably, the carbon layer has a high roughness, resulting in a strong bond between it and the active material.

[0051] For example, the carbon layer includes one of a conductive graphite layer, a graphene layer, an acetylene black layer, and carbon black.

[0052] For example, the carbon layer is formed by deposition methods such as chemical plating and physical plating.

[0053] In some embodiments, the recess 111 includes one of acid-etched recess, laser-etched recess, and physical extrusion recess.

[0054] This application sets the recess 111 to include one of acid-etched recess, laser-etched recess, and physical extrusion recess. By means of acid etching, laser etching, or physical extrusion, a uniform recess 111 can be formed on the metal wire 11, thereby increasing the surface roughness Ra of the metal wire 11 and thus improving the bonding force between the mesh body 10 and the active material.

[0055] In some embodiments, the mesh body 10 includes one of aluminum mesh, nickel mesh, and stainless steel mesh.

[0056] This application sets the mesh body 10 to include one of aluminum mesh, nickel mesh, and stainless steel mesh. Aluminum mesh has good conductivity, which can improve the current collection effect of mesh body 10, and aluminum has low density, which can reduce the mass (weight) of the battery cell. Nickel mesh has good conductivity and corrosion resistance, which can significantly improve the current collection effect of mesh body 10. Stainless steel mesh has good corrosion resistance and long service life. By setting different types of mesh body 10, it can be suitable for different application scenarios.

[0057] For example, the recess 111 is an acid-etched recess. The acid used in the acid etching will not cause a corrosion layer to form on the surface 112 of the metal wire 11, thereby not affecting the conductivity of the mesh body 10.

[0058] For example, in addition to the current collector 100, circular holes can be punched in the foil, and the foil surface can be acid-treated to increase the adhesion between the surface and the film.

[0059] Secondly, this application provides an electrode 200, please refer to... Figure 5 , Figure 5 This is a schematic diagram of the structure of the electrode 200 provided in the embodiment of this application. The electrode 200 includes a current collector 100 and an active material layer 110 provided in the first aspect of this application. The active material layer 110 is disposed on the current collector 100.

[0060] The electrode 200 of this application includes the current collector 100 provided in the first aspect of this application, which enables the active material layer 110 to adhere tightly, fully and firmly to the current collector 100, thereby reducing the internal resistance of the battery cell. At the same time, the presence of the active material layer 110 provides conditions for the electrochemical reaction to proceed.

[0061] For example, the preparation method of electrode 200 is as follows: First, acid etching is performed on the surface of the mesh body 10 to form surface defects, that is, a recess 111 is formed on the surface 112 of the metal wire 11; then, active material is filled into the mesh 101 and wrapped around the mesh body 10; the active material is composited on both sides of the current collector 100 by hot pressing, and an active material layer 110 is formed on both sides of the current collector 100. Electrode 200 is obtained by dry preparation. The bonding strength between the active material layer 110 and the current collector 100 can be improved by hot pressing.

[0062] For example, the preparation method of electrode 200 is as follows: first, acid etching is performed on the surface of mesh body 10 to form surface defects, that is, a recess 111 is formed on the surface 112 of metal wire 11; then, conductive adhesive is brushed on both sides of mesh body 10; then, a pre-prepared active material layer 110 is attached to both sides of mesh body 10 or an active slurry is coated, and after drying, electrode 200 is obtained.

[0063] Thirdly, this application provides a battery including the electrode 200 provided in the second aspect of this application.

[0064] The battery of this application includes the electrode 200 provided in the second aspect, thus the battery has low internal resistance and excellent electrochemical performance.

[0065] The present application will be specifically described below through specific embodiments. These embodiments are only some embodiments of the present application and are not intended to limit the present application. Unless otherwise specified, the raw materials used in the following embodiments are all commercially available products.

[0066] Example 1 This embodiment provides a method for preparing electrode 200, including the following steps: (1) Laser etching is performed on the surface of the mesh body 10 to form surface defects, that is, a recess 111 is formed on the surface 112 of the metal wire 11. The mesh body 10 is an aluminum mesh, the diameter of the metal wire 11 is 0.25 mm, the surface roughness Ra of the metal wire 11 after laser etching is 1.2 mm, the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 208, and the surface roughness Ra of the metal wire 11 is tested using a shape measurement laser microscopy system.

[0067] (2) The active material is filled into the mesh 101 and wrapped around the mesh body 10. The active material is then composited on both sides of the current collector 100 by hot pressing, forming an active material layer 110 on both sides of the current collector 100. The mass percentage of electrolytic manganese dioxide, expanded graphite and polytetrafluoroethylene in the active material layer 110 is 94%:4%:2%.

[0068] Example 2 This embodiment provides a method for preparing an electrode 200. Compared with Embodiment 1, the only difference is that the diameter of the metal wire 11 in step (1) is 0.15 mm, and the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 125. The other aspects are consistent with Embodiment 1 and will not be repeated here.

[0069] Example 3 This embodiment provides a method for preparing an electrode 200. Compared with Embodiment 1, the only difference is that the diameter of the metal wire 11 in step (1) is 0.30 mm, and the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 250. The other aspects are consistent with Embodiment 1 and will not be repeated here.

[0070] Example 4 This embodiment provides a method for preparing an electrode 200. Compared with Embodiment 1, the only difference is that the surface roughness Ra of the metal wire 11 after laser etching in step (1) is 1.5 mm, and the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 167. The other aspects are consistent with Embodiment 1 and will not be repeated here.

[0071] Example 5 This embodiment provides a method for preparing an electrode 200. Compared with Embodiment 1, the only difference is that the surface roughness Ra of the metal wire 11 after laser etching in step (1) is 0.7 mm, and the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 357. The other aspects are consistent with Embodiment 1 and will not be repeated here.

[0072] Comparative Example 1 This comparative example provides a method for preparing an electrode 200. Compared with Example 1, the only difference is that the surface roughness Ra of the metal wire 11 after laser etching in step (1) is 0.5 mm, and the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 500. The other aspects are consistent with Example 1 and will not be repeated here.

[0073] Comparative Example 2 This comparative example provides a method for preparing an electrode 200. Compared with Example 1, the only difference is that in step (1), the diameter of the metal wire 11 is 0.10 mm, the surface roughness Ra of the metal wire 11 after laser etching is 1.2 mm, and the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 83. The other aspects are consistent with Example 1 and will not be repeated here.

[0074] The performance of the electrode sheets 200 prepared in Examples 1-5 and Comparative Examples 1-2 was tested, and the results are shown in Table 1.

[0075] (1) The peel force was tested using a universal tensile testing machine. The specific method was as follows: a) Cutting the electrode 200: Cut the electrode 200 prepared in Examples 1-5 and Comparative Examples 1-2 into test samples with a length x width of 150mm x 30mm; b) Attaching and fixing the electrode 200: Take a flat thin steel plate with a length of 250mm and a width of 30mm. First, attach a strip of double-sided tape (the length should be greater than the length of the test sample and the same width as the test sample) to the center of the thin steel plate. Smooth it with force to ensure that the double-sided tape is tightly attached to the center of the thin steel plate. Peel off the double-sided tape and attach the test sample to the tape strip so that the test sample and the tape are completely matched and attached. Attach another layer of double-sided tape to the side of the test sample away from the thin steel plate and smooth it with force; c) Installation test: The universal tensile testing machine has two clamps, one above and one below. Insert the thin steel plate with the test sample attached and fixed into the lower clamp and fix it vertically; peel off 2cm of the bottom of the double-sided tape on the side of the test sample away from the thin steel plate. After the test sample is inserted into the upper clamp without the double-sided tape, it is fixed vertically so that the test sample fixed by the lower clamp is at 180° with the test sample fixed by the upper clamp. After the test sample is fixed, the calibration is zeroed first. The test width is set to 30mm, the peel length of electrode 200 is 100mm, and the peel speed is 80mm / min. The peel force of electrode 200 can be obtained by starting the test.

[0076] (2) The electrode sheets 200 prepared in Examples 1-5 and Comparative Examples 1-2 were assembled into lithium manganese cylindrical batteries CR17335, and the internal resistance of the batteries was tested. The assembly method of the lithium manganese cylindrical battery CR17335 is as follows: the positive electrode sheet 200 is cleaned with ultrasonic powder to remove the tab position, the tab is welded, and tab adhesive is applied. The positive electrode sheet 200, the separator, and the lithium metal sheet are stacked and wound into a core and put into a steel shell. After welding the cap, electrolyte is injected and sealed.

[0077] The battery internal resistance is measured using an internal resistance meter that can automatically or manually measure and record the internal resistance range of 0Ω to 20Ω with an accuracy of 0.01Ω.

[0078] Table 1

[0079] As shown in Table 1, the data from Examples 1-5 and Comparative Examples 1-2 indicate that when the ratio of the diameter of the metal wire 11 to its surface roughness Ra is within the range of 125-357, the peel force of the electrode 200 is greater than 0.1 N / mm, the internal resistance of the battery is less than 225Ω, and the battery performance is superior. This is mainly because when the ratio of the diameter of the metal wire 11 to its surface roughness Ra is within this range, the degree and number of depressions 111 on the surface 112 of the metal wire 11 are appropriate, ensuring sufficient, tight, and firm contact between the active material layer 110 and the current collector 100, thereby improving the peel force of the electrode 200 and reducing the internal resistance of the battery.

[0080] As can be seen from the data of Example 1 and Comparative Example 1, when the diameter of the metal wire 11 is the same, when the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 500, the peeling force of the electrode 200 is only 0.07 N / mm, and the internal resistance of the battery is as high as 287.46Ω. This is mainly because the surface roughness Ra of the metal wire 11 in Comparative Example 1 is too small, which makes the recess 111 of the surface 112 of the metal wire 11 limited, thereby significantly reducing the bonding strength between the active material layer 110 and the current collector 100, and making the bonding between the active material layer 110 and the current collector 100 loose, resulting in a large internal resistance of the cell.

[0081] As can be seen from the data of Comparative Example 2, when the ratio of the diameter of the metal wire 11 to the surface roughness Ra of the metal wire 11 is 83, the internal resistance of the battery is as high as 249.8Ω. This is mainly because the diameter of the metal wire 11 in Comparative Example 2 is too small, which makes the cross-sectional area of ​​the current collection path of the metal wire 11 small, the current collection effect of the current collection network 100 poor, and the internal resistance of the cell increases.

[0082] The embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the embodiments above are only for the purpose of helping to understand the methods and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A current collection network (100), characterized in that, The mesh body (10) includes a plurality of cross-connected metal wires (11), the surface (112) of the metal wires (11) is partially concave to form a recess (111), and the ratio of the diameter of the metal wires (11) to the surface roughness Ra of the metal wires (11) is 125~357.

2. The current collector web (100) according to claim 1, characterized in that The diameter of the metal wire (11) is 0.15mm to 0.30mm.

3. The current collector web (100) according to claim 1 or 2, characterized in that The surface roughness Ra of the metal wire (11) is 0.7μm~1.5μm.

4. The current collector web (100) according to any one of claims 1 to 3, characterized in that The cross-section of the metal wire (11) is polygonal.

5. The current collector web (100) according to claim 4, characterized in that The cross-section of the metal wire (11) is quadrilateral, and the metal wire (11) has four surfaces (112), and the four surfaces (112) extend obliquely relative to the thickness direction of the mesh body (10).

6. The current collector web (100) according to any one of claims 1 to 5, characterized in that The current collector (100) also includes a conductive layer that covers the surface (112) of the metal wire (11).

7. The current collector web (100) according to claim 6, characterized in that The conductive layer includes a carbon layer.

8. The current collector web (100) of claim 1, wherein, The recessed portion (111) includes one of acid-etched recessed portions, laser-etched recessed portions, and physical extrusion recessed portions; and / or, The mesh body (10) includes one of aluminum mesh, nickel mesh and stainless steel mesh.

9. A pole piece (200), characterized by, include: The collection network (100) according to any one of claims 1 to 8; and An active material layer (110) is disposed on the current collection network (100).

10. A battery, characterized by Includes the electrode (200) as described in claim 9.