Welded structure, individual battery cells and battery pack

By using a laser welding structure and protective layer between the tab assembly and the terminal post, the problems of large space occupation and welding defects in the connection between the terminal post and the tab assembly are solved, thereby improving the energy density and performance of the battery.

CN224986594UActive Publication Date: 2026-11-17HUIZHOU EVE POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522380823.8
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2025-11-07
Publication Date
2026-11-17
Estimated Expiration
2035-11-07

AI Technical Summary

Technical Problem

The connection method of the terminals and tabs in existing batteries takes up a lot of space, and ultrasonic welding is prone to grain coarsening and compositional segregation, which affects corrosion resistance and mechanical properties.

Method used

The electrode assembly and electrode post are laser-welded together, and a protective layer is added to suppress grain coarsening and compositional segregation. The connecting piece is eliminated, increasing space utilization.

Benefits of technology

It improves the battery's energy density, enhances corrosion resistance and mechanical properties, and reduces welding defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN224986594U_ABST
    Figure CN224986594U_ABST
Patent Text Reader

Abstract

This utility model relates to the field of battery technology, providing a welding structure, a single battery cell, and a battery pack. The welding structure includes a terminal post, a tab assembly, and a protective layer. The tab assembly is laser-welded to the terminal post, forming a molten pool within both. Along the direction from the terminal post to the tab assembly, the molten pool exhibits a decreasing cross-sectional width. The tab assembly includes at least two stacked tabs, and at least two tabs are ultrasonically welded. The protective layer is disposed between the terminal post and the tab assembly. This increases the utilization rate of the battery's internal space, improves the battery's energy density, and suppresses grain coarsening and compositional segregation during the ultrasonic welding process of the tab assembly. It also prevents localized compositional inhomogeneity during the ultrasonic welding process, which could affect the corrosion resistance and mechanical properties of the tab assembly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This utility model relates to the field of battery technology, specifically to a welding structure, a single battery cell, and a battery pack. Background Technology

[0002] In related technologies, the market demands supercharging and high energy density for power batteries, requiring batteries to maintain stability under high current and minimize structural space to meet these requirements. For the battery's terminals and tabs, they are typically connected by connecting tabs, usually through welding. However, this method of connecting terminals, connecting tabs, and tabs occupies considerable internal battery space. Eliminating the connecting tabs, after ultrasonic welding of several positive or negative electrode tabs, can easily lead to surface contaminants, causing uneven local composition and affecting corrosion resistance and mechanical properties. Utility Model Content

[0003] The embodiments of this utility model provide a welding structure, a single battery cell, and a battery pack, which can increase the utilization rate of internal space, suppress grain coarsening and compositional segregation during the ultrasonic welding of the electrode assembly, and avoid affecting corrosion resistance and mechanical properties.

[0004] In a first aspect, embodiments of the present invention provide a welding structure, comprising: pole; A tab assembly is laser-welded to the electrode post, and a molten pool is formed inside both. The molten pool has a decreasing cross-sectional width along the direction from the electrode post to the tab assembly. The tab assembly includes at least two stacked tabs, and at least two of the tabs are ultrasonically welded. A protective layer is disposed between the pole post and the tab assembly.

[0005] This can increase the utilization rate of the battery's internal space, improve the battery's energy density, and suppress grain coarsening and compositional segregation during the process of ultrasonic welding of the tabs to form the tab assembly. It can also prevent localized compositional inhomogeneity during the process of ultrasonic welding of the tabs to form the tab assembly, which would affect the corrosion resistance and mechanical properties of the tab assembly.

[0006] In one embodiment, the protective layer is a metal particle layer with a particle size of N, satisfying: 50 nanometers ≤ N ≤ 200 nanometers.

[0007] This prevents the protective layer from affecting the fluidity of the molten pool and prevents the failure of grain refinement from causing welding defects.

[0008] In one embodiment, the thickness of the protective layer is D, which satisfies: 50 nanometers ≤ D ≤ 500 nanometers.

[0009] Thus, the protective layer is prevented from affecting the fluidity of the molten pool, and welding defects caused by the failure of grain refinement are avoided.

[0010] In an embodiment, the surface roughness of the protective layer is Ra, which satisfies: 0<Ra≤0.1 micrometer.

[0011] Thus, insufficient bonding strength of the tab ultrasonic welding caused by excessive surface roughness of the protective layer is avoided.

[0012] In an embodiment, the molten pool penetrates through the protective layer and extends into the tab group.

[0013] Thus, reliable connection among the pole, the protective layer and the tab group is ensured.

[0014] In an embodiment, the pole includes a first metal layer and a second metal layer, the first metal layer, the second metal layer and the tab group are stacked in sequence, wherein the melting points of the first metal layer and the second metal layer are different.

[0015] Thus, a metal compound can be formed after welding, so as to improve the hardness and the apparent tensile strength.

[0016] In an embodiment, the melting point of the first metal layer is lower than the melting point of the second metal layer, and / or the melting point of the second metal layer is the same as the melting point of the tab group.

[0017] Thus, the laser needs to penetrate the metal layers with different melting points at the first metal layer and the second metal layer, and the laser does not need to penetrate the metal layers with different melting points at the second metal layer and the first welding position.

[0018] In an embodiment, a side of the first metal layer away from the second metal layer is configured with a groove, and the groove bottom surface of the groove is the acting surface of welding equipment.

[0019] Thus, the thickness of the laser welding area of the pole can be reduced, the power of the laser is lowered, thereby reducing the welding cost and welding difficulty, and facilitating the positioning of the pole by the welding equipment.

[0020] In a second aspect, an embodiment of the present invention provides a unit cell, including the welding structure as described above.

[0021] Thus, the utilization rate of the internal space of the battery can be increased, the energy density of the battery is improved, and the phenomena of grain coarsening and component segregation occurring in the process of forming the tab group by tab ultrasonic welding can be inhibited, so as to avoid non-uniform local components occurring in the process of forming the tab group by tab ultrasonic welding from affecting the corrosion resistance and mechanical properties of the tab group.

[0022] In a third aspect, an embodiment of the present invention provides a battery pack, including the unit cell as described above.

[0023] This can increase the utilization rate of the battery's internal space, improve the battery's energy density, and suppress grain coarsening and compositional segregation during the process of ultrasonic welding of the tabs to form the tab assembly. It can also prevent localized compositional inhomogeneity during the process of ultrasonic welding of the tabs to form the tab assembly, which would affect the corrosion resistance and mechanical properties of the tab assembly.

[0024] The beneficial effects of the embodiments of this utility model are as follows: In embodiments of this invention, by directly welding the tab assembly to the terminal post, the use of connecting tabs can be eliminated, thereby increasing the utilization rate of internal space and improving the energy density of the battery. The protective layer can suppress grain coarsening and compositional segregation during the ultrasonic welding process of the tab assembly, and avoid localized compositional inhomogeneity during the ultrasonic welding process, which would affect the corrosion resistance and mechanical properties of the tab assembly. Attached Figure Description

[0025] To more clearly illustrate the technical solutions in the embodiments of this utility model, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this utility model. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Figure 1 This is an exploded view of a single battery cell provided in an embodiment of this utility model; Figure 2 This is a cross-sectional view of a single battery cell provided in an embodiment of this utility model; Figure 3 yes Figure 2 A magnified view of part A in the middle.

[0027] Explanation of reference numerals in the attached figures: 1. Pole post; 11. First metal layer; 12. Second metal layer; 13. Groove; 2. Electrode assembly; 3. Protective layer; 4. Molten pool; 5. Individual battery cell. Detailed Implementation

[0028] The technical solutions of the present utility model will be clearly and completely described below with reference to the accompanying drawings of the embodiments. Obviously, the described embodiments are only some embodiments of the present utility model, and not all embodiments. Based on the embodiments of the present utility model, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present utility model. In addition, it should be understood that the specific embodiments described herein are only for illustration and explanation of the present utility model and are not intended to limit the present utility model. In the present utility model, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in actual use or operation, specifically the drawing directions in the accompanying drawings; while "inner" and "outer" refer to the outline of the device.

[0029] This application provides a battery pack. The battery pack includes a battery box and battery modules disposed within the battery box. The battery modules include multiple individual battery cells 5. The battery box provides a space for accommodating the individual battery cells 5, and the battery box can adopt various structures. In some embodiments, the battery box includes a box body and a box cover that overlap each other. The box body and the box cover together define an accommodating space for accommodating the individual battery cells 5. The box body can be a hollow structure, and the box cover can be a plate-like structure, with the box cover closing onto the opening side of the box body so that the box cover and the box body together define the accommodating space. Both the box body and the box cover can be hollow structures with an opening on one side, with the opening of the box cover closing onto the opening side of the box body. Of course, the battery box formed by the box cover and the box body can be of various shapes, such as a cylinder, a cuboid, etc.

[0030] In a battery pack, multiple individual cells 5 can be configured. These individual cells 5 can be connected in series, parallel, or in a hybrid configuration. A hybrid configuration means that multiple individual cells 5 are connected in both series and parallel configurations. Multiple individual cells 5 can be directly connected in series, parallel, or in a hybrid configuration, and then the entire assembly of these individual cells 5 is housed within a battery box. Alternatively, the battery pack can consist of multiple individual cells 5 first connected in series, parallel, or in a hybrid configuration to form battery modules, and then these battery modules are connected in series, parallel, or in a hybrid configuration to form a whole, which is then housed within a battery box. The battery pack may also include other structures; for example, it may include a busbar component for electrical connection between the multiple individual cells 5.

[0031] Each individual cell 5 can be a secondary battery or a primary battery; it can also be a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, but is not limited to these. The individual cell 5 can be cylindrical, flat, cuboid, or other shapes.

[0032] like Figure 1 and Figure 2As shown in the illustration, this application also provides a single-cell battery 5. The single-cell battery 5 includes a housing, a top cover assembly, and electrode assemblies and other functional components located within the housing. The top cover assembly includes a top cover, electrode posts 1, and electrode tabs 2 disposed on the top cover. The electrode posts 1 and electrode tabs 2 are laser-welded together.

[0033] like Figures 1 to 3 As shown in the embodiment of this application, a welding structure is also provided. The welding structure includes an electrode post 1, an electrode lug group 2, and a protective layer 3. The electrode lug group 2 is laser welded to the electrode post 1, and a molten pool 4 is formed inside the two. Along the direction from the electrode post 1 to the electrode lug group 2, the molten pool 4 has a decreasing cross-sectional width. The electrode lug group 2 includes at least two stacked electrodes, and at least two electrodes are ultrasonically welded. The protective layer 3 is disposed between the electrode post 1 and the electrode lug group 2.

[0034] In this embodiment, by directly welding the tab assembly 2 to the electrode post 1, the use of connecting pieces can be eliminated, thereby increasing the utilization rate of internal space and improving the energy density of the battery. The protective layer 3 can suppress grain coarsening and compositional segregation during the ultrasonic welding process of the tab assembly 2, and avoid local compositional inhomogeneity during the ultrasonic welding process of the tab assembly 2, which would affect the corrosion resistance and mechanical properties of the tab assembly 2.

[0035] It is understandable that the electrode post 1 and the tab assembly 2 are directly welded together without the need for a connecting piece between them. Since the connecting piece has a certain thickness, removing the connecting piece can free up that height space, thereby increasing the utilization rate of the internal space and thus improving the energy density of the battery.

[0036] In some embodiments, the terminal post 1 and the tab assembly 2 are laser welded. Since the cross-sectional width of the molten pool 4 tends to decrease along the direction from the terminal post 1 to the tab assembly 2, the side of the terminal post 1 away from the tab assembly 2 is used as the welding surface. This allows the terminal post 1 and the tab assembly 2 to be laser welded on the outside of the battery, which can prevent metal spatter generated during welding from contacting the core pack and potentially causing a short circuit in the battery.

[0037] In some embodiments, the tab assembly 2 is an assembly of several positive electrode tabs ultrasonically welded together, or an assembly of several negative electrode tabs ultrasonically welded together. After the several positive electrode tabs or several negative electrode tabs are ultrasonically welded together to form the tab assembly 2, it can be compacted to its minimum thickness along the height direction inside the battery, and then the tab assembly 2 is laser-welded to the electrode post 1. This maximizes the utilization of the battery's internal space, effectively improving the internal space utilization rate, thereby increasing the battery's energy density.

[0038] After several positive or negative electrode tabs are ultrasonically welded together to form electrode group 2, electrode post 1 is then laser-welded to electrode group 2. The protective layer 3 can be applied to electrode group 2 by coating. Furthermore, the protective layer 3 is applied to the surface of the uppermost positive or negative electrode tab before the ultrasonic welding of the several positive or negative electrode tabs to form electrode group 2. This allows the protective layer 3 to suppress grain coarsening and compositional segregation during the ultrasonic welding process of forming electrode group 2, thereby preventing the formation of pores from gases or residual contaminants adsorbed at the ultrasonic welding interface during melting, and preventing contaminants from the ultrasonic welding interface from causing localized compositional inhomogeneity that affects corrosion resistance and mechanical properties.

[0039] In some embodiments, the protective layer 3 may also be disposed between the pole post 1 and the tab assembly 2 by other means such as bonding. The present application embodiment does not limit the fixing method of the protective layer 3.

[0040] It should be noted that the cross-sectional width of the molten pool 4 can decrease linearly or exponentially along the direction from the pole post 1 to the tab group 2. For example, the molten pool 4 can be set in the shape of a teardrop or an inverted cone. Of course, the cross-sectional width of the molten pool 4 can also remain unchanged at first along the direction from the pole post 1 to the tab group 2, and then decrease linearly.

[0041] In some embodiments, the protective layer 3 is a metal particle layer with a particle size of N, satisfying: 50 nanometers ≤ N ≤ 200 nanometers.

[0042] Understandably, the protective layer 3 is a layer of metal particles to ensure good flowability. The particle size of the metal particles in the protective layer 3 is set in the range of 50 nanometers to 200 nanometers to avoid the protective layer 3 affecting the flowability of the molten pool 4 and to prevent the failure of grain refinement effect, which could lead to welding defects.

[0043] If the particle size of the metal particles in the protective layer 3 is less than 50 nanometers, the grain refinement effect will fail, resulting in welding defects.

[0044] If the particle size of the metal particles in the protective layer 3 is greater than 200 nanometers, it will affect the fluidity of the molten pool 4, causing the laser penetration welding to fail to fuse the pole post 1 and the tab assembly 2.

[0045] In some embodiments, the particle size of the metal particles in the protective layer 3 is set to 50 nanometers, 100 nanometers, 150 nanometers, 200 nanometers, or any value between the two.

[0046] In some embodiments, the protective layer 3 is a nano-metal layer. For example, the protective layer 3 is Ni / Ti alloy particles.

[0047] like Figure 2 and Figure 3As shown, in some embodiments, the thickness D of the protective layer 3 satisfies: 50 nm ≤ D ≤ 500 nm.

[0048] It can be understood that the thickness of the protective layer 3 is set in the range from 50 nm to 500 nm, so as to avoid the protective layer 3 affecting the fluidity of the molten pool 4 and prevent the failure of grain refinement effect from causing welding defects.

[0049] If the thickness of the protective layer 3 is less than 50 nm, the excessively thin protective layer 3 will lead to the failure of the grain refinement effect, resulting in welding defects.

[0050] If the thickness of the protective layer 3 is greater than 500 nm, the excessively thick protective layer 3 will affect the fluidity of the molten pool 4, resulting in the failure of laser penetration welding to fuse the pole post 1 and the tab group 2.

[0051] In some embodiments, the thickness of the protective layer 3 is set to 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or any value between any two of the foregoing values.

[0052] In some embodiments, the surface roughness Ra of the protective layer 3 satisfies: 0 < Ra ≤ 0.1 μm.

[0053] It can be understood that the surface roughness of the protective layer 3 is set below 0.1 μm, so as to avoid insufficient bonding strength of the tab during ultrasonic welding caused by excessively high surface roughness of the protective layer 3.

[0054] In some embodiments, the surface roughness of the protective layer 3 is set to 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, or any value between any two of the foregoing values.

[0055] In some embodiments, the molten pool 4 penetrates through the protective layer 3 and extends into the tab group 2.

[0056] It can be understood that the molten pool 4 penetrates through the pole post 1 and the protective layer 3 and extends into the tab group 2, so as to ensure reliable connection among the pole post 1, the protective layer 3 and the tab group 2. In addition, the protective layer 3 can also improve the current-carrying capacity of the pole post 1 and the tabs.

[0057] In some embodiments, the end of the molten pool 4 away from the pole post 1 includes a plurality of protruding portions, all of which extend into the tab group 2.

[0058] In some embodiments, the end of the molten pool 4 away from the pole post 1 is configured in a wave shape, which has wave crests and wave troughs. The wave crests extend into the tab group 2, and the wave troughs are located in the pole post 1 or in the tab group 2.

[0059] In some embodiments, the electrode post 1 includes a first metal layer 11 and a second metal layer 12, and the first metal layer 11, the second metal layer 12 and the tab group 2 are stacked in sequence, wherein the first metal layer 11 and the second metal layer 12 have different melting points.

[0060] When electrode 1 is the negative electrode, it is made of a composite material of a first metal layer 11 and a second metal layer 12. The first and second metal layers 12 are located between the first metal layer 11 and the tab assembly 2. Generally, when the individual battery cell 5 is placed vertically, the first metal layer 11 is located above the second metal layer 12. The first metal layer 11 and the second metal layer 12 have different melting points. During the laser welding process, it is necessary to penetrate the metal layers with different melting points, which can form a metal compound after welding, thereby increasing the hardness and tensile strength.

[0061] In some embodiments, the first metal layer 11 is an aluminum layer and the second metal layer 12 is a copper layer.

[0062] In some embodiments, the melting point of the first metal layer 11 is lower than that of the second metal layer 12, and / or the melting point of the second metal layer 12 is the same as that of the tab assembly 2.

[0063] Understandably, the melting point of the first metal layer 11 is lower than that of the second metal layer 12. During laser welding, this interface needs to penetrate metal layers with different melting points. The melting point of the second metal layer 12 is the same as that of the electrode 1, so this interface does not need to penetrate metal layers with different melting points during laser welding. Because the melting point of the first metal layer 11 is lower than that of the second metal layer 12, laser welding requires a higher power density to penetrate the second metal layer 12.

[0064] In some embodiments, the first metal layer 11 is made of aluminum, and the second metal layer 12 and the pole post 1 are both made of copper.

[0065] In some embodiments, a groove 13 is formed on the side of the first metal layer 11 away from the second metal layer 12, and the bottom surface of the groove 13 is the working surface of the welding equipment.

[0066] It is understandable that by forming a groove 13 on the side of the first metal layer 11 away from the second metal layer 12, and using the bottom surface of the groove 13 as the welding surface, the thickness of the laser welding area of ​​the electrode 1 can be reduced, the laser power can be lowered, thereby reducing welding costs and welding difficulty. At the same time, the groove 13 can also facilitate the positioning of the electrode 1 by the welding equipment, enabling the welding equipment to quickly and accurately confirm the welding surface, which is beneficial to improving welding efficiency and welding accuracy.

[0067] The embodiments of this utility model have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this utility model. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this utility model. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this utility model. Therefore, the content of this specification should not be construed as a limitation of this utility model.

Claims

1. A welded structure, characterized in that, comprising: a pole (1); a tab group (2), which is laser-welded to the pole (1), and a molten pool (4) is formed inside the two; along the direction from the pole (1) to the tab group (2), the molten pool (4) has a trend of decreasing cross-sectional width, wherein the tab group (2) comprises at least two stacked tabs, and at least two of the tabs are ultrasonically welded; a protective layer (3), arranged between the pole (1) and the tab group (2).

2. The welded structure according to claim 1, characterized in that, The protective layer (3) is a metal particle layer, with a particle size of N, which satisfies: 50 nm ≤ N ≤ 200 nm.

3. The welded structure according to claim 1, characterized in that, The thickness of the protective layer (3) is D, which satisfies: 50 nm ≤ D ≤ 500 nm.

4. The welded structure according to claim 1, characterized in that, The surface roughness of the protective layer (3) is Ra, which satisfies: 0 < Ra ≤ 0.1 μm.

5. The welded structure according to any one of claims 1 to 4, characterized in that, The molten pool (4) penetrates through the protective layer (3) and extends into the tab group (2).

6. The welded structure according to any one of claims 1 to 4, characterized in that, The pole (1) comprises a first metal layer (11) and a second metal layer (12), the first metal layer (11), the second metal layer (12) and the tab group (2) are stacked in sequence, wherein the melting points of the first metal layer (11) and the second metal layer (12) are different.

7. The welded structure according to claim 6, characterized in that, The melting point of the first metal layer (11) is lower than the melting point of the second metal layer (12), and / or, the melting point of the second metal layer (12) is the same as the melting point of the tab group (2).

8. The welded structure according to claim 6, characterized in that, A groove (13) is formed on the side of the first metal layer (11) facing away from the second metal layer (12), and the groove bottom surface of the groove (13) is the acting surface of a welding device.

9. A single-cell battery cell (5), characterized in that, comprising the welding structure as described in any one of claims 1 to 8.

10. A battery pack, characterized in that, comprising the cell (5) as described in claim 9.