Process and press for manufacturing a molded wood-based part
The controlled pressure relief during steam burst in a continuous press process addresses the issue of long pressing times and internal steam pressure in wood-based molded parts, achieving faster curing and improved part strength through targeted steam burst timing and heating.
Patent Information
- Application Number
- DE102012001293
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2012-01-25
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2032-01-25
AI Technical Summary
Existing methods for producing wood-based molded parts using steam injection technology require long pressing times due to the risk of internal steam pressure causing damage, such as delamination, despite attempts to cool the parts post-pressing, which negates the time advantage of rapid binder curing.
A method and press design that uses a continuous process with controlled pressure relief during steam burst, maintaining excess pressure until the optimal time for steam burst, allowing for targeted temperature increase without additional moisture, thereby influencing the timing and intensity of the steam burst for faster curing.
This approach significantly reduces pressing time by ensuring rapid and controlled steam burst heating, preventing internal steam pressure damage and enhancing the strength of the molded parts, while maintaining high energy input for efficient binder hardening.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to a method for producing a wood-based molded part using a Wood-based material and a thermosetting binder are formed by pressing, whereby the binder hardens. Heat transfer into the wood-based molded part occurs in the form of a steam burst. The invention also relates to a continuous press for the production of such a wood-based molded part.
[0002] Such methods are known from the prior art. The duration of the pressing time is primarily determined by This is influenced by how quickly the binder hardens. For example, a three-layer structure Wood-based panels, consisting of a middle layer, a top layer and a bottom layer, are described below. The solutions known from the state of the art are described.
[0003] To manufacture the board, a three-layer wood-based material mat (fleece) consisting of the The wood-based material and a thermosetting binder are fed into a press. Then a A hot pressing process takes place. The hardening of the binder (glue) in the outer layers occurs through direct contact. Heat is supplied via heated press plates or belts.
[0004] Due to the heat energy introduced into the plate on the one hand and the [unclear] located in the plate on the other hand On the other hand, moisture creates a water vapor pressure gradient in the plate.
[0005] The heat energy required to cure the middle layer is supplied to the plate via the so-called steam burst. The material is introduced. For this purpose, the outer press plates are heated to, for example, 200° Celsius. During pressing, the material is then... Water (glue water) in the surface layers is heated and, upon reaching the boiling point (100°C), is suddenly transferred into the The vapor phase is transferred. Due to the water vapor pressure gradient, this vapor shoots vertically from both sides of the plate into Towards the center of the plate. This process is called a steam burst.
[0006] Due to the temperature gradient between the outer surfaces of the cover layers and the center of the middle layer (the If the temperature difference is, for example, 75°C, the vapor condenses in the still-cool middle layer. In this process, Condensation heat is released, which increases the temperature in the middle layer. The chemical Curing reactions in the middle layer occur faster, and less time passes before the binder hardens. This results in a shorter pressing time. This steam burst principle is used in the production of used in numerous wood-based panel molded parts, for example in the production of chipboard, MDF, OSB, etc.
[0007] It is known from the prior art to optimize the steam burst principle by optimizing the water vapor It is heated beforehand and then injected as hot steam under pressure into the wood-based molded part. This is also referred to as the Steam injection technology. This also allows for a reduction in pressing time to a limited extent.
[0008] However, a disadvantage is that with steam injection technology more water enters the interior of the wood-based material- molded part. Due to the basic principle of pressure and counter-pressure, steam injection technology... Internal pressure in the wood-based molded part is greatly increased. When the press opens, the binder inside the The molded part must already be sufficiently hardened so that the internal vapor pressure does not cause damage (chipping of parts). or leads to destruction of the molded part (delamination). Attempts are being made to mitigate this disadvantage with elaborate cooling systems. to address the need to cool the molded parts after hot pressing. However, the press must still be used in steam injection technology. They remain closed for a comparatively long time, so that the time advantage of the rapid curing of the binder is partially lost. will be lifted again.
[0009] In DE 10 2008 026 258 A1, it was proposed to allow the steam burst to take place under increased pressure. The process described there is characterized by the fact that, prior to heat transfer in the form of a steam burst, the The process air pressure prevailing in the press room compared to the atmospheric pressure prevailing outside the press room. Air pressure is increased, but without adding moisture, especially in the form of, to the wood-based molded part. To supply steam. A press designed for the production of such a wood-based molded part is characterized by a pressure chamber and a device for generating overpressure such that before the Heat transfer in the form of a steam burst occurs when the process air pressure prevails in the press chamber compared to the outside air pressure. The atmospheric pressure prevailing in the press chamber can be increased, but without further increasing the pressure. To supply moisture, especially in the form of water vapor, to the wood-based molded part.
[0010] By applying and maintaining an external overpressure during the pressing process, DE 10 2008 026 258 A1 achieves a rise in the boiling point of water above 100°C. This results in the following: A steam burst at, for example, 120°C transfers significantly more heat energy into the middle layer of the wood-based molded part. can be used. This increased amount of heat, which occurs during the condensation of water vapor in the still cold The release of the middle layer leads to a significantly higher temperature compared to conventional steam burst technology. Middle layer, resulting in significantly faster curing reactions of the adhesive. In summary Using the technique described in DE 10 2008 026 258 A1, the steam burst occurs at a higher temperature, which leads to leading to a reduction in pressing time.
[0011] DE 32 33 241 A1 discloses a discontinuous press in which a pre-formed A lignocellulose mat is inserted. The press has an upper heated tool half and a lower tool half. which are connected to a press table. A pressing chamber is located between the tool halves, essentially forming a press chamber. A closed pressure chamber is formed, whereby a valve allows for a targeted lowering of the process pressure during pressing. This can be done using air pressure.
[0012] One object of the present invention is to provide a technique for manufacturing a wood-based molded part. to provide tools that can further reduce pressing time.
[0013] This problem is solved by a method according to claim 1 or by a press according to claim 5. Advantageous embodiments of the invention are specified in the dependent claims.
[0014] The advantages and features explained below in connection with the method apply The same applies analogously to the devices according to the invention and vice versa.
[0015] Specifically, the present invention relates to the aforementioned method for producing a wood-based material- Molded part in a continuously operating press as well as on a corresponding continuous press for the production directed towards a wood-based molded part.
[0016] The press according to the invention has a pressing chamber which is in the form of a pressing gap as a substantially It is designed as a closed pressure chamber. Before heat transfer in the form of a steam burst, the pressure in the press gap is increased. prevailing process air pressure compared to the atmospheric air pressure prevailing outside the press gap increased by means of a device for generating overpressure.
[0017] The core of the present invention is that during continuous pressing a targeted lowering of the Process air pressure is used to initiate the steam pulse. For this purpose, the continuous system according to the invention is used. The press is equipped with a sealing device that allows the process air pressure to be controlled during pressing. It can be lowered. The sealing device seals the press gap of the continuous press on both sides over a partial length of the Press off, wherein a sealing device connected to the sealing device and influencing the function of the sealing device Pressure control is provided. A targeted pressure release during the pressing process results in a sudden, rapid change. Heating of the material, whereby the timing and process of the heating can be influenced.
[0018] In the method according to the invention, the reduction of the process air pressure is thus achieved by means of the Sealing device which seals the press gap on both sides over a partial length of the press, wherein a control of the Process air pressure via the sealing device connected to and influencing the function of the sealing device Pressure control is performed.
[0019] The present invention is based on the fundamental insights described in DE 10 2008 026 258, as described in DE 10 2008 026 258. They are described below: After that, the steam injection technique, which leads to a technological dead end, in which hot steam is injected, will be discussed. The process of pressing the material into the molded part under pressure is no longer pursued. Instead, a return is made to the... original steam burst technology, in which the steam burst occurs automatically upon reaching the boiling temperature This steam burst technique is improved in DE 10 2008 026 258 by the fact that during the During the pressing process, at least in the press chamber of the press, the air pressure is greater than the atmospheric pressure. Environment. In other words, the pressing process takes place under overpressure, e.g., at 1.5 bar. In such a case Overpressure causes the water to evaporate at higher temperatures, for example at 110°C. The steam burst occurs. still automatic, but this time at a higher temperature. Compared to one below In atmospheric pressure processes, the steam burst may occur somewhat later. time, but with a significantly higher energy content corresponding to the higher boiling point.
[0020] The invention described in DE 10 2008 026 258 A1 takes advantage of the dependence of boiling point and They utilize each other's boiling pressure. An increase in pressure of, for example, 0.5 bar = 500 hPa results in an increase in the The boiling point of the water rises from 100°C to approximately 110°C. This increases the energy content of the water vapor compared to a process taking place at atmospheric pressure. When using the same amount of water can be done with the help of steam This allows more heat to be transferred into the interior of the wood-based molded part. As a result, the achievable [value / temperatur ... Temperature in the middle layer. According to van't Hoff's rule (RGT rule), the reaction rate The temperature roughly doubles when increased by 10°C, resulting in a significantly increased Reaction rate for the chemical curing reactions of the binder. As a result, the pressing time can be determined. significantly shortening the production time, while eliminating the risk of delamination since no additional water vapor is introduced. the molded part is inserted.
[0021] In contrast to the original steam injection technique, in which the steam injection is introduced into the wood-based molded part Thermal energy is essentially increased by increasing the amount of water vapor used. The invention described in DE 10 2008 026 258 A1 is based on the consideration of increasing the reaction rate of to increase the curing reactions of the binder by using more water vapor with the same amount Heat energy is transferred. This allows for a high process temperature without the disadvantages of increased internal pressure. can be achieved.
[0022] The resulting water vapor consists of those moisture components of the air which - Provided that no dry air is used as the process atmosphere – which is already contained in the air anyway, as well as the water vapor, which originates from the glue water of the top layers.
[0023] The following illustration is intended to further clarify the difference between the known steam injection technology and the one described in The invention described in DE 10 2008 026 258 is illustrated as follows: In conventional steam injection technology, the partial pressure ratios result from a combination of (moist) air on the one hand and additionally superheated water vapor introduced into the system on the other hand: ptotal=p( air) + p(H2O)
[0024] Upon reaching the boiling point of 100°C, the steam burst results from the vapor contained in the moist air. Water vapor, as well as water vapor originating from the glue water of the surface layers, and from the additionally introduced superheated steam.
[0025] In the invention described in DE 10 2008 026 258, the introduction of superheated steam is not necessary. No additional equipment is used. The pressure chamber contains only the usual process atmosphere, generally air at normal humidity. Composition (78% nitrogen, 21% oxygen, ...). It follows that: ptotal = p(air)
[0026] The steam burst that occurs when the (increased) boiling temperature of, for example, 110°C is reached contains significantly less moisture and at the same time higher heat energy, which leads to the advantages described above.
[0027] Since the pressing process takes place under overpressure, a pressure chamber is provided in which the desired There is positive pressure. The pressure outside the pressure chamber is then below atmospheric pressure. The prevailing air pressure caused by the weight of the air is to be understood as the ambient air pressure. Process air pressure, on the other hand, refers to the... To understand the air pressure of the environment in which the pressing process takes place. Since the pressing process always occurs in a The pressing process takes place in the pressing chamber, for example in the pressing gap arranged between press plates or belts. Air pressure, in other words, the air pressure prevailing (at least) in the press chamber, to which the wood-based material to be produced- The molded part is exposed. In one embodiment of the invention described in DE 10 2008 026 258, the pressing chamber, especially in the form of the press gap, to achieve the desired overpressure as an essentially A closed pressure chamber is used. In another embodiment of the one described in DE 10 2008 026 258 The invention provides a pressure chamber that, in addition to the actual pressing chamber, encloses further parts of the press. In another embodiment of the invention described in DE 10 2008 026 258, the press has a completely surrounding pressure chamber; the entire press is then located inside the pressure chamber.
[0028] The press described in DE 10 2008 026 258 A1 has suitable technical equipment for this purpose, which These terms are familiar to experts and therefore do not need to be listed individually here. For example, is the If the press gap is designed as a pressure chamber, devices for sealing the press gap are provided, e.g. laterally. attached sealing rings, pressure devices, etc. In discontinuous presses, for example With discontinuously operating single- or multi-stage presses, it is possible to provide lateral sealing surfaces that Seal all four sides when closing the press. In addition to the structural elements and seals for separating the A pressure chamber is a device for generating overpressure. This can be a These are pressure vessels that provide an overpressure of, for example, 0.5 to 10 bar. From this, pressure can be applied. Overpressure is introduced into the pressure chamber via pipes. This can raise the boiling point of the water to, for example, 110°C to 150°C. C will be set.
[0029] In addition to the above findings as described in DE 10 2008 026 258 A1, the present The invention is based on the following considerations: While in the original steam burst method the steam burst always occurred spontaneously, and also in the The technique described in DE 10 2008 026 258 A1, which causes a spontaneous burst of steam, suggests the The present invention presents the principle of retaining the steam burst under increased pressure, but with the The timing of the steam burst can no longer be influenced. In other words, spontaneous steam bursts no longer occur. Instead, the timing of the steam burst is precisely controlled. In other words, the steam burst is... initiated. Therefore, the following will also refer to a "forced steam burst". In other words, A steam movement (steam burst) is achieved by skillfully controlling the pressure profiles during the pressing process. forced within the mat.
[0030] A basic idea of the present invention therefore lies in an additional relief step, namely a A targeted reduction of the previously built-up process air pressure occurs during pressing. In other words, a Pressure relief before the end of the pressing time. Depending on the application, this pressure relief is either partial or completely. In other words, even after pressure relief, an increased process air pressure may still be present, or However, the process air pressure corresponds to the atmospheric air pressure prevailing outside the press chamber.
[0031] This targeted pressure reduction results in extremely rapid temperature increases in the nonwoven fabric. In this process, the temperature rises The indoor temperature not only rises particularly quickly, but also to levels that are not normally reached. This allows it to... This results in a significantly increased energy content. In other words, more energy can be absorbed into the middle layer of the mat. are introduced. This results in a sudden heating of the material, combined with a high energy input. which results in a significant reduction in pressing times.
[0032] This principle will be explained in more detail below. In the method according to the invention, the The increased pressure prevents water on the surface of the mat from boiling. This allows water to boil away at this point. Temperatures well over 100°C can be reached. By deliberately lowering the process air pressure, a An abrupt increase in the mat's internal temperature was observed, caused by the sudden pressure relief. is caused by the resulting water vapor. As is known from the steam burst principle, the Water vapor spreads exclusively towards the center of the mat, which leads to very strong temperature increases. This allows for much larger outputs compared to all other steam burst techniques known from the state of the art. Temperature increases can be measured in an extremely short time. For example, in a fleece where a Pressure relief occurred after approximately 330 minutes of pressing time, with an increase in internal temperature from 70°C by 47K to 117°C. Measured within 10 seconds after pressure release.
[0033] A significant advantage of the present invention is that by selectively forcing the steam burst of the The timing of the steam burst, i.e., the point in time at which the energy is sent to the middle layer of the mat, is optimal. This can be selected. As a result, this leads to a further reduction in pressing time.
[0034] An optimal choice of the timing of the steam burst means that the timing of the pressure relief is chosen in such a way that The remaining time the fleece stays in the press is just sufficient to process the wood-based material. to harden the molded part, i.e., to stabilize the chemical bonds at least to the extent that the wood-based molded part does not burst (delaminate) when the press is opened.
[0035] At the same time, forcing the steam burst by means of a controllable pressure relief means that the strength of the The steam burst can be specifically influenced. In other words, the way in which the pressure is released can be controlled. The process carried out can influence the speed at which the steam burst flows towards the middle layer. This can be regulated by a defined reduction in process pressure. For example, if the process air pressure is allowed to decrease... If the pressure suddenly drops to 1 bar, the steam burst will be violent. If the pressure drops within a certain period of time, the pressure will be significantly reduced. If the degradation time is reduced, for example, by a few seconds, this is gentler on the structure of the molded part. Too rapid a degradation time is not recommended. Pressure relief, which could potentially lead to damage to the structure of the wood matrix, is thus avoided. In other words, a delayed reduction of the process air pressure can affect the structure of the wood-based material being produced. to protect the molded part. Therefore, it is advantageous to have a pressure control system in place, which helps to... The sealing device can be influenced in such a way that the pressure in the press chamber can be specifically changed.
[0036] But also an accelerated reduction of the process air pressure by additionally applying a vacuum and thus a Increasing the pressure differential is possible and can be useful in certain applications. For example, To increase the pressure difference, it is conceivable to create overpressure at the press mouth and a vacuum at the press outlet. to create a vacuum. By applying a vacuum, the water vapor is then literally forced out of the wood-based molded part. sucked out.
[0037] With the methods known so far, more or less long processing times had to be expected, which They were hardly controllable. Controlling or regulating the process was either impossible or only partially possible. The present invention enables enhanced process control and management. While in the systems derived from the In the state of the art, where the process air pressure was the only variable parameter, the method was different. In the present invention, in addition to this process air pressure, the time of pressure reduction is also specified. (“pressure relief”) and the rate of pressure reduction can be influenced. This allows for advantageous and The material structure of the manufactured wood-based molded parts and thus especially their Strength properties are influenced.
[0038] Just as in the method described in DE 10 2008 026 258, the present invention does not intended to introduce moisture, particularly in the form of water vapor, into the wood-based molded part during pressing, to supply. The moisture required for the steam burst is already contained in the wood-based mat. Nevertheless A quantity of moisture can be added to the molded part before the pressing process to aid the process, preferably by spraying or otherwise distributing it onto the fiber fleece. The amount of water sprayed can vary depending on the type of fiber used. Depending on the material, for example, 1 to 2 g per side and millimeter of plate thickness. By introducing these The additional moisture will further intensify the subsequent steam burst.
[0039] Like the method described in DE 10 2008 026 258, the present method is also used in the production of It can be used in numerous wood-based molded parts, for example in the production of chipboard, MDF, HDF, OSB, etc. The wood-based molded parts can be individual pieces or a continuous process running through the press. The process involves an endless part. The inventive method is used on continuously operating presses, for example. on single- or multi-level presses, double belt presses, etc.
[0040] Depending on the type of wood-based molded parts to be produced, the Wood-based material consists of chips, fibers, stalks, etc. For example, urea-based thermosetting binders can be used. , melamine or phenolic resins or mixtures thereof or mixtures of these resins with polymeric diisocyanates (PMDI) or are used with natural binders such as tannin and / or lignin resins.
[0041] An embodiment of the invention is shown below in the single figure with reference to a continuous The working multi-level press is explained in more detail.
[0042] All figures show the invention only schematically and with its essential components. Reference symbols correspond to elements of the same or comparable function.
[0043] In the production of a particleboard 3, in a first process step, wood, wood scraps, and wood molded parts are first used. etc. is machined, i.e., it is processed by suitable comminution methods using knife ring cutters, Longwood chippers, etc., produce the desired optimal chip shape. In a second process step, the chips are thus The produced chips are dried until a final moisture content of 0.5-2% is reached. The chips are then... fractionated, i.e., divided into sieve fractions. Then the separate gluing of the so-called "covering and" takes place. Middle layer chips with thermosetting resins, primarily urea, melamine or phenolic resins or mixtures thereof. from these or with polymeric diisocyanates (PMDI) or also with natural binders such as tannins and / or Lignin resins. After machining, drying, and gluing, the fourth process step involves spreading the glued material. Chips are produced by means of wind or throwing, creating a so-called "chip mat" or "chip fleece". This will be the case. Looking at the fleece's height, the smaller and finer top layer chips are predominantly found at the top and bottom. arranged, while the coarser middle-layer chips are primarily found in the center of chip mat 4. In this In this arrangement, the glued chipboard mat 4 is now fed into a press 10, in which, through the simultaneous action of Heat and pressure compress the chipboard mat 4 to the final desired chipboard thickness. simultaneous hardening of the thermosetting binder.
[0044] The chemical reactivities of the binders used in the top and middle layers (UF, MF, PF, MUF, PMDI etc.) They must be adapted to the requirements of the compaction reactions. Conversely, the The moisture content of the chipboard being produced must be precisely measured to ensure optimal curing. reaction can occur in the top and middle layers and the chipboard 3 not at the moment it passes through the press 10 When the material leaves the structure and the external pressure is thus removed, it delaminates due to excessively high internal vapor pressure, i.e., bursts. The duration of the pressing time is primarily influenced by how quickly the binder hardens.
[0045] The press is a continuous multi-level press 10 with a circulating press belt 12, comprising an upper and a lower belt. The pressing width is, for example, 2.20 m.
[0046] If the large-volume nonwoven fabric is in the form of a chip mat 4 that is initially, for example, 100 to 120 mm thick, When the material is fed into press 10, compression first occurs during the so-called "pre-pressing". Mat 4 is then The material is compressed to its final thickness of, for example, 22 mm through the press jaws. The press jaw temperature during this process... The temperature of the "pre-pressing" process is, for example, 250°C. After a preheating phase of, for example, 80 seconds, the Temperature of the water in the top layers of mat 4 following the "pre-pressing", e.g. 70 to 80°C. The press 10 is then sealed. The press gap 5 again serves as a pressure chamber.
[0047] To seal the press 10, only the press mouth and the press gap 5 need to be sealed. Sealing the entire press 10 is not required. The press gap 5 can be sealed with a simple pressure seal. or sealed by a pressure seal. This is achieved by a lateral sealing of the press gap 5 by means of both The press has 10 laterally mounted sealing devices on each side. This reduces the design effort. Each side of the press 10 has a separate sealing device assigned to it.
[0048] Such a sealing device is, for example, a circumferential, segmented pressure chain 19 or a circumferential pressure belt which seals one side of the press 10. Such a pressure chain 19 consists of links arranged in a row. The printing chain 19 or the printing band engages both at the upper band and at the The lower band attaches and presses between the bands against the lateral narrow surfaces of the mat 4. The pressure chain 19 or The pressure band consists, for example, of a temperature-stable hard rubber material.
[0049] In a particular embodiment of the invention, the pre-pressing already carried out Compression of mat 4 is used. It may even be necessary during or after the "pre-pressing" process. Before applying a sealing device, release air from the press chamber to prevent excessive pressure. To prevent pressure increases.
[0050] However, the sealing of the press gap 5 usually only takes place after the “pre-pressing”, i.e. after the Mat 4 has reached its final thickness, or immediately thereafter. Only at this corresponding position of the When press 10 activates the sealing device, for example, the pressure chains 19 are attached to the sides of press 10. This position is usually located relatively far forward, i.e., the pressure chain 19 starts as early as possible with at the press mouth. The seal towards the press mouth is preferably achieved without any further structural modifications. Effort, solely due to the existence of the mat 4 located there, which is already pressed or has just been supplied.
[0051] The sealing devices 19 extend to both sides of the press 10 in the direction of the press outlet. They However, they do not extend to the end of press cycle 10, but end before. This affects the time of pressure release. determined.
[0052] During the pressing time in which the pressure chain 19 seals the press gap 5, a further controlled process takes place. The temperature and pressure increase until the desired target values are reached, or these values have already been reached and will be increased. The pressure is only held constant. Before the pressing time expires, the built-up pressure is released. For this purpose, the pressure is opened. The side surfaces of mat 4 can be removed by removing the pressure chain 19. This is advantageously done in a targeted, step-by-step manner. and accomplished with the aid of appropriate pressure control. Then, more or less abruptly, it happens. The desired steam burst occurs. More precisely, at a process air pressure of, for example, 3 bar, a A temperature of, for example, 115°C to 123°C in the top layer of the mat 4. If, according to the invention, a Relief (relaxation) occurs because the pressure chain 19 is no longer in contact with the sides of the press 10, then air can escape. The water escapes outwards from the porous middle layer. With the release of pressure, the water evaporates from the outer layers. of the mat 4. A large amount of hydrogen is suddenly produced, which moves into the middle layer (“forced”). (Steam burst). Once it reaches the middle layer, the water vapor condenses again. This transfers a lot of heat into the The middle layer is introduced, causing the temperature (internal plate temperature) to rise very rapidly. This leads to... a sudden warming of the mat 4. This leads to a much greater improvement compared to the previous technique. Faster curing. Chemical reactions proceed more quickly. This shortens the pressing times. speed of Depending on the design, the press can be increased by 15% or more.
[0053] It may be possible to operate the press 10 normally until the desired The feed rate is reached, e.g., 4 seconds per millimeter of plate thickness. If this is the case, the following is done using the corresponding pressure control the sealing according to the invention, for example in the form of the pressure chains 19, "activated". The exact positions at which the print chains 19 are applied or removed can vary. The press system and operating conditions vary. Preferably, the press 10 is designed such that a Variable positioning of the sealing device is possible. When the sealing device is in place, the Feed rate can be increased, for example to 3 seconds per millimeter of plate thickness.
[0054] To achieve the described functionality, it is preferably provided that the printing chain 19 is segmented. to form. This segmentation of the printing chain 19 is therefore advantageously designed not only to form a Redirecting the pressure chain allows for comparatively simple handling. Rather, a Depending on the design of the pressure chain 19, the chain can also be applied and removed in a locally variable manner. With other In other words, the sealing device is preferably designed such that both the point on the side of the press 10, The point at which the sealing device is applied, where sealing therefore begins, as well as the point at which the The sealing device is removed again, i.e., the sealing is cancelled, and is variable, in particular freely selectable.
[0055] All features shown in the description, the figure and the following claims can be both individually as well as in any combination with each other, they may be essential to the invention. Reference symbol list 3 Chipboard 4 chipboard mat 5 Press gap 10 Press 12 Press band 19 Print chain
Claims
1. A method for producing a wood-based molded part (3) using a wood-based base material and a thermosetting binder by pressing in a continuously operating press (10) with a pressing chamber (5), wherein the pressing chamber (5) is designed in the form of a press gap (5) as a substantially closed pressure chamber is, where, to cure the binder, heat is transferred into the wood-based material moulding in the form of a steam jet occurs, Wherein, before the heat transfer in the form of a steam pulse, the process air pressure prevailing in the press gap (5) against the atmospheric air pressure prevailing outside the press nip (5) by means of a device (6, 7) to generate excess pressure, During pressing, a targeted reduction of the process air pressure takes place, wherein the reduction of the process air pressure is carried out by means of a sealing device (19) which seals the press gap (5) seals on both sides over a partial length of the press (10) and wherein a control of the process air pressure is carried out via a device connected to the sealing device (19) and the function of the Pressure control can be influenced by the sealing device (19).
2. Method according to claim 1, characterized in that partial pressure relief takes place before the end of the pressing time.
3. Method according to claim 1, characterized in that before the end of the pressing time a complete pressure relief occurs.
4. Method according to one of claims 1 to 3, characterized in that the process air pressure is at least 0.5 bar above atmospheric pressure.
5. Continuous press (10) for the production of a wood-based material molded part (3) using a Wood-based material and a thermosetting binder, wherein for curing the binder a Heat transfer into the wood-based molded part takes place in the form of a steam jet, wherein the press (10) comprises a circulating processing belt (12) with an upper and lower belt and a pressing chamber (5) and a Device (6, 7) for generating an overpressure such that before the heat transfer in the form of a steam pulse, the process air pressure prevailing in the press chamber (5) compared to that outside the press chamber (5) prevailing atmospheric pressure can be increased, wherein the pressing chamber (5) is designed in the form of a press gap (5) as a substantially closed pressure chamber is, wherein the process air pressure can be specifically reduced during pressing by means of a sealing device (19), wherein the sealing device (19) seals the press gap (5) seals on both sides over a partial length of the press (10) and wherein a sealing device (19) connected to the sealing device (19) and the function of the sealing device (19) can be influenced Pressure control is provided.
6. Press according to claim 5, characterized in that the lateral sealing of the press gap (5) is provided by Sides of the press (10) laterally mounted sealing devices (19), preferably with each side of the press (10) is assigned a separate sealing device (19).
7. Press according to claim 5 or 6, characterized in that the sealing device (19) is designed as a circumferential, segmented pressure chain or as a circulating pressure belt, wherein the pressure chain consists of links arranged in a row where the pressure chain or pressure belt is attached to both the upper belt and the lower belt and is positioned between the Bands press against the narrow lateral surfaces of the wood-based material molded part (3).
Citation Information
Patent Citations
Process for the production of a wood-based molded part
DE102008026258A1
process for pressing molded parts from organic fiber mats
DE3233241A1