Synthesis of abietic acid-based macromer for polyester resin process
A 2-step process synthesizes bio-based polyesters from abietic acid-glycerol macromers, addressing health and environmental concerns of bisphenol A toners by producing toners with controlled properties and improved performance.
Patent Information
- Application Number
- DE102013200469
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2012-01-26
- Filing Date
- 2013-01-15
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2033-01-15
AI Technical Summary
Current polyester-based toners derived from bisphenol A pose health risks and environmental concerns, and there is a need for sustainable, bio-based alternatives that can reduce reliance on fossil resources and minimize waste.
A 2-step process is employed to synthesize bio-based polyesters using abietic acid-glycerol macromers, which are then polycondensed with diacids to produce a binder resin for emulsion aggregation toners, offering greater control over polymerization and higher biomass content.
The process results in bio-based polyesters with controlled properties, reducing environmental impact and health risks, while providing toners with improved molecular weights, softening points, and gloss levels, and enhanced energy efficiency.
Abstract
Description
[0001] This disclosure relates to bio-based polyester resins used for the production of emulsion aggregation toners can be used, on processes for producing the bio-based polyester resins and on Emulsion aggregation toners that include bio-based resins.
[0002] Emulsion aggregation toners (EA toners) are used in the formation of printed and / or xerographic images. used. Emulsion aggregation processes usually involve the formation of an emulsion latex from resin particles. small size, for example with a diameter of approximately 5 nm to approximately 500 nm, by heating the resin, Optionally, if required, with solvent, in water, or by preparing a latex in water using a Emulsion polymerization. An optional colorant dispersion, for example a water-dispersed pigment, is optional. with an additional resin, it is formed separately. The colorant dispersion is added to the emulsion latex mixture. and then an aggregating agent or a complexing agent is added and / or the aggregation is otherwise carried out. A process is initiated to form aggregated toner particles. The aggregated toner particles are heated to coalesce. / to enable melting, resulting in aggregated, molten toner particles.
[0003] Due to energy and environmental directives, rising and highly fluctuating oil prices, and public / political In light of the rapid depletion of fossil resources, sustainable monomers must be created that are derived from are derived from biomaterials. By using biologically renewable raw materials, manufacturers can reduce their to improve the carbon balance and move towards a zero-carbon or even a carbon-neutral balance. Bio-based polymers can also be extremely attractive in terms of specific energy and emission savings. The use of bio-based raw materials can reduce the amount of plastic destined for landfill. lower costs, facilitate the creation of new income sources for domestic agriculture, and improve economic conditions. Reduce risks and the uncertainty associated with dependence on imported oil from unstable regions.
[0004] Furthermore, many current polyester-based toners are derived from bisphenol A monomer. Bisphenol A It has been identified as a carcinogen and endocrine disruptor that negatively impacts health development. Canada, several countries in Europe and the USA want to ban Bisphenol A.
[0005] US 1 998 744 A discloses the esterification of glycerol and abietic acid to form a macromer which is combined with Phthalic anhydride is polycondensed. US 2009 / 0047593A1 discloses an emulsion aggregation toner with a core and a shell, wherein the core is an amorphous polyester, a wax, a crystalline polyester and a contains optional dye and wherein the casing contains an amorphous polyester and a wax and is essentially free of crystalline polyester. US 2009 / 0142689A1 discloses emulsion aggregation toners that are a polyester wax resin. comprising, wherein the polyester wax resin contains a wax that is chemically incorporated into the main chain of the polyester resin US 2006 / 0235121A1 discloses temperature-switchable pressure-sensitive adhesives consisting of an elastomer and a Crystallizable abietic acid derivative as a tackifier. US 2010 / 0205853A1 describes a process for the production of Biodiesel is produced from crude vegetable oils, especially Jatropha (Jatropha curcas) and Karanja (Pongamia pinnata). The bioactive components, fatty acids and polar materials are selectively extracted from the crude oils by liquid-liquid- Extraction with a polar solvent removes the oil into the solvent phase, and the remaining oil as a residue can It is directly transesterified. After transesterification, the glycerol phase is separated and the crude biodiesel is neutralized and through adsorption of unwanted components such as residual glycerin, gum, soap, salts, etc. via a Adsorbent bed such as Celite is used for purification. An improved polycondensation process for bio-based [products / materials] is presented here. (“environmentally friendly”) polyesters synthesized from pre-formed macromers, as well as the corresponding Compositions disclosed that are used in the manufacture of binder polymers for imaging applications such as Emulsion aggregation toners (EA toners) are useful.
[0006] In this description and the claims that follow, singular forms such as ‘a’, ‘an’ and ‘the’´´ The plural forms, unless the context clearly indicates otherwise. All areas revealed here encompass all Endpoints and intermediate values, unless explicitly specified otherwise by the context. Furthermore, reference can be made to... A number of terms are used, which are defined as follows: The term ‘functional group’ refers, for example, to a group of atoms that are arranged in a certain way are arranged according to the chemical properties of the group and the molecule on which it adheres to, determines. Examples of functional groups include halogen atoms, hydroxyl groups, Carboxylic acid groups and the like.
[0007] The expression ‘optional’ [in its gender-specific variations] or ‘optional’ can be for example, referring to cases in which the circumstance described below may or may not occur, and includes cases where the circumstance occurs and cases where the circumstance does not occur.
[0008] The expressions ‘one or more’ and ‘at least one’ [in their gender-specific variations] refer, for example, to cases in which one of the circumstances described below occurs, and to cases in which in which more than one of the circumstances described below occurs.
[0009] The term ‘bio-based’ refers, for example, to products made from biological raw materials. are produced from living organisms such as plants, trees, algae, bacteria, yeasts, fungi, protozoa, Insects and animals were preserved or produced using renewable raw materials. Bio-based products serve often as a replacement for products based on fossil materials, and are usually low in terms of greenhouse gases. neutral and leave a smaller ecological footprint, meaning they produce less waste and require less Less energy and water. Bio-based products typically consume less natural resources during their production. Resources are saved, thereby reducing costs and making them better for the environment.
[0010] The bio-based polyesters can be obtained using a two-step process. In the first step, a 100% Mol.% bio-based abietic acid-glycerol macromer through esterification between bio-based abietic acid, and Bio-based glycerol is formed, with the esterification process involving heating for at least 4 hours. In the second step, the In the first step, the macromer formed is polycondensed with at least two diacids in the presence of a catalyst to form to form the final polyester product that is used as a binder in imaging materials such as EA toners The final polyester product has a softening point temperature of 90 °C to 150 °C and an acidity level of 8. has a KOH content of up to 16 mg / g and is at least 80 mol% bio-based.
[0011] The abietic acid used to form the macromer can be obtained as an impure compound (purity level of approximately 70%) and can be used without further purification. Glycerol or glycerin is a waste product of the Biodiesel production, which is obtained from triglycerides, i.e., the transesterification of crude vegetable oil. The pre-forming of the The abietic acid-glycerol macromer in the first step ensures the complete reaction of the primary bio-based Resin component. Macromer synthesis can be monitored using nuclear magnetic resonance (NMR) to determine the formation. to ensure that at this point the remaining monomers can be added to the final polymer product. On the other hand, more side reactions occur if all the required monomers are added in advance. (Bulk addition), instead of using a macromer formation step, which results in a darker resin color and a Early termination of the polymer chain occurs, resulting in very low molecular weights. When adding the bulk of the With monomers, the reaction time is much longer, and the resulting composition and its properties are not predictable. The reaction time of the 2-step polymerization reaction can be reduced to approximately half the time of Bulk addition methods can be used, and vacuum distillation is not necessary to prepare the bioresin. synthesize.
[0012] Thus, the macromer process offers much greater control over the polymerization process, and through the Bulk synthesis of the macromer can provide the bio-starting monomer for many different formulations. This can be provided by varying the monomers from the second step. Furthermore, the monomers in the 2-step- The processes produced resins with higher C / O ratios than resins produced using bulk addition methods. and there is no acid functionality requirement via citric acid or trimellitin anhydride addition. The aid of the Resins produced using a 2-step process can have a C / O ratio in the range of approximately 5.5 to approximately 10.0. For example, approximately 6.0 to approximately 9.0 or approximately 7.0 to approximately 8.0. The C / O ratio can be higher. be approximately 5.5 or approximately 6.0 or approximately 6.5 or approximately 7.0 or approximately 7.5 or approximately 8.0.
[0013] The reaction scheme (below) highlights the first step of an embodiment of the disclosed 2-step process. which is the formation of the abietic acid-glycerol macromer.
[0014] The formation of the ester bond between the abietic acid and the glycerol can be monitored by means of NMR. Both the proton and carbon NMR spectra show a specific peak shift. For example, In this reaction, when the acid of abietic acid and the hydroxyl of glycerol combine to form an ester bond 13 When reacting, a shift in the C-NMR of the carbonyl group of abietic acid was observed.
[0015] Step 2 is shown below, wherein the macromer synthesized in step 1 is further combined with two diacids, sebacic acid and isophthalic acid reacts to form the polymer of interest (polymer fragment shown): Sebabic acid is also a bio-based monomer derived from castor oil, while isophthalic acid is derived from The oxidation of meta-xylene using oxygen is synthetically produced.
[0016] The resin-based macromer is 100 mol% bio-based and is present in an amount such that for the Polyester formulations provide a biomass content of more than 80 mol%, thereby obtaining a polyester will be at least 80 mol% bio-based, for example at least 85 mol%, 90 mol% or 95 mol%. Of course Polyesters can also be formulated with a biomass content of less than 80 mol%, for example from at least 70 mol%, 60 mol% or 50 mol% or even lower.
[0017] The polyester can be 100 mol% bio-based if the isophthalic acid is replaced by a bio-based aromatic The monomer or a linear bio-based diacid such as succinic acid is replaced. Succinic acid has the following structure: and can be biologically metabolized together with oxalic acid, fumaric acid and malic acid as part of an anaerobic process Submerged culture fermentation is produced using various types of bacteria and molds. The manufacturing process is from Lockwood, LB, "Production of Organic Acids by Fermentation". In Microbial Technology, Peppler, HJ and Perlman, D. Eds., Academic Press: New York, pp. 356 - 387 (1979).
[0018] Other suitable diaacids include adipic acid, azelaic acid, and glutaric acid. Azelaic acid is produced by chemical means. Synthesis produced from oleic acid. Oleic acid is a monosaturated fatty acid with 18 carbon atoms, found in most Azelaic acid is found in animal fats and vegetable oils. It can be produced by the oxidative cleavage of oleic acid with chromic acid. or produced by ozonolysis. Ozonolysis is described in Cyberlipid, 2009, at www.cyberlipid.org / cyberlip / home0001.htm reveals that azelaic acid has the following structure:
[0019] In the step of polycondensing the abietic acid-based macromer with the diacids, the macromer can be in a quantity of, for example, approximately 5 to 95 mol% of the polyester resin, such as approximately 5 to approximately 80 mol%, approximately 10 to approximately 70 mol%, approximately 20 to approximately 60 mol%; or approximately 40 to approximately 60 mol% of the polyester resin. The total amount of diacid can be, for example, approximately 5 to approximately 95 mol%, such as approximately 5 to approximately 80 mol%, approximately 10 to approximately 70 mol%; approximately 20 up to approximately 60 mol%; or approximately 40 to approximately 60 mol% of the polyester resin may be selected.
[0020] Polycondensation catalysts include tetraalkyl titanates such as titanium(iv) butoxide or titanium(iv) isopropoxide; Dialkyltin oxides such as dibutyltin oxide; tetraalkyltins such as dibutyltin dilaurate; dialkyltin oxide hydroxides such as Butyltin oxide hydroxide; aluminum alkoxides; alkylzinc; dialkylzinc; zinc oxide; tin oxide; and combinations thereof. Catalysts can be present in amounts of, for example, approximately 0.001 mol%, approximately 0.55 mol%, or approximately 0.001 mol. % to approximately 0.30 mol% or approximately 0.25 mol% to approximately 0.55 mol% based on the starting dioic acid or the The starting diester, which was used to form the polyester resin, is used.
[0021] The polyester resin can, for example, be in an amount of approximately 5 to approximately 50 wt.% of the Toner components such as approximately 5 to approximately 25 wt.%, approximately 10 to approximately 35 wt.%, approximately 30 to approximately 40% by weight or approximately 25 to approximately 50% by weight of the toner components may be present. Polyester resin can have a number-averaged molecular weight (M ) (measured by gel permeation chromatography, GPC) n from, for example, approximately 1000 to approximately 50,000, or approximately 2000 to approximately 25,000. 10,000 to approximately 20,000 and a weight-averaged molecular weight (M ) of, for example, approximately 2000 to w approximately 100,000, such as approximately 3,000 to approximately 30,000 or approximately 5,000 to approximately 25,000 (certainly) (using GPC with polystyrene standards). The molecular weight distribution (M / M) of the wn Polyester resin can, for example, range from approximately 1 to approximately 15, such as approximately 1.5 to approximately 10 or approximately 3 to approximately 8 or approximately 2 to approximately 3.5.
[0022] The polyester resin can have a glass transition temperature (Tg) of, for example, approximately 30 °C to approximately 120 °C such as approximately 40 °C to approximately 90 °C or approximately 45 °C to approximately 75 °C.
[0023] The polyester resin has a softening point (Ts) of 90 °C to 150 °C, for example approximately 95 °C to approximately 135 °C or approximately 100 °C to approximately 120 °C. Different softening points can affect toners with to produce different gloss levels. For example, resins with a softening point of 101 °C produce up to 103 °C in some embodiments toners with a higher gloss value than toners made using resins with were produced at a softening point of 105 °C or higher.
[0024] The polyester resin has an acid value of 8 to 16 mg KOH / g or preferably approximately 10 to approximately 14 mg KOH / g. The acid value (or the "neutralization number" or "acidity number" or "acidity") can be measured. This is done by dissolving a known amount of a polymer sample in an organic solvent and applying a Potassium hydroxide solution (KOH solution) of known concentration and Phenolphthalein is used as a color indicator for titration. The acid number is the mass of potassium hydroxide in milligrams, which required to neutralize one gram of the chemical substance. With regard to polyester resins, the acid number of Measured value for the amount of carboxylic acid groups in a polyester molecule.
[0025] Dyes, waxes and other additives used to form toner compositions, can be present in surfactant-containing dispersions. Furthermore, toner particles can be caused by Emulsion aggregation processes are formed, whereby the resin and other components of the toner come into contact with one or more surfactants are placed, an emulsion is formed and toner particles aggregate and coalesce, can optionally be washed, dried and harvested.
[0026] One, two or more surfactants can be used. The surfactants can be ionic surfactants and non-ionic surfactants. Ionic surfactants must be selected. Anionic surfactants and cationic surfactants are distinguished from the term "ionic surfactants". The surfactant can be present in an amount of approximately 0.01 to approximately 5% by weight of the toner composition, such as... for example, approximately 0.75 to approximately 4 wt% of the toner composition or approximately 1 to approximately 3 wt% the toner composition.
[0027] Examples of suitable non-ionic surfactants are polyacrylic acid, methalose, methylcellulose, ethylcellulose, Propylcellulose, hydroxyethylcellulose, carboxymethylcellulose, polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, Polyoxyethylene octyl ether, polyoxyethylene octyl phenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, Polyoxyethylene stearyl ether, polyoxyethylene nonyl phenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol, available from Rhone- Poulenac as IGEPAL CA-210™, IGEPAL CA-520™, IGEPAL CA-720™, IGEPAL CO-890™, IGEPAL CO- 720™, IGEPAL CO-290™, IGEPAL CA-210™, ANTAROX 890™ and ANTAROX 897™. Others Examples of suitable non-ionic surfactants include a block copolymer of polyethylene oxide and polypropylene oxide, including those commercially available as SYNPERONIC PE / F, e.g. SYNPERONIC PE / F 108.
[0028] Suitable anionic surfactants include sulfates and sulfonates, sodium dodecyl sulfate (SDS), Sodium dodecylbenzenesulfonate, sodium dodecylnaphthalene sulfate, dialkylbenzene alkyl sulfates and sulfonates, acids such as Abietic acid, available from Aldrich, NEOGEN R™, NEOGEN SC™, available from Daiichi Kogyo Seiyaku, Combinations thereof and the like. Other suitable anionic surfactants include DOWFAX™ 2A1, a Alkyldiphenyl oxide disulfonate from The Dow Chemical Company, and / or TAYCA POWER BN2060 from Tayca Corporation (Japan), which are branched sodium dodecylbenzenesulfonates. Combinations of these surfactants are possible. and any of the above-mentioned anionic surfactants can be used.
[0029] Examples of cationic surfactants that are usually positively charged are Alkylbenzyldimethylammonium chloride, dialkylbenzenealkylammonium chloride, lauryltrimethylammonium chloride, Alkylbenzylmethylammonium chloride, Alkylbenzyldimethylammonium bromide, Cetylpyridinium bromide, Benzalkonium chloride, C -, C -, C -Trimethylammonium bromides, halide salts of quaternized polyoxyethylalkylamines, 12 15 17 Dodecylbenzyltriethylammonium chloride, MIRAPOL™ and ALKAQUAT™, available from Alkaril Chemical Company, SANIZOL™ (Benzalkonium Chloride), available from Kao Chemicals, and the like, as well as mixtures thereof.
[0030] The resin emulsion can be prepared such that it contains a wax. In these embodiments, the Emulsion resin and wax particles at the desired loading levels, thus enabling a single resin- and wax emulsion is produced instead of separate resin and wax emulsions. Furthermore, the combined emulsion the reduction of the amount of surfactant required for the production of separate emulsions Incorporation into toner compositions is required. This is particularly helpful when the incorporation of the otherwise it would be difficult to incorporate the wax into the emulsion. However, the wax can also be emulsified separately, for example with a resin, and are incorporated separately into final products.
[0031] In addition to the polymer binder resin, the toners can also contain a wax, either a single type of wax or a Contains a mixture of two or more, preferably different, waxes. A single wax can be used to... Toner formulations are added to, for example, certain toner properties such as the shape of the toner particles, Presence and quantity of wax on the toner particle surface, charge and / or melting characteristics, gloss, To improve detachment, offset properties, and the like. Alternatively, a combination of waxes can be added. to give the toner composition several properties.
[0032] Examples of suitable waxes include waxes derived from natural plant waxes, natural animal waxes Waxes, mineral waxes, synthetic waxes, and functionalized waxes are selected. Natural Plant-based waxes include, for example, carnauba wax, candelilla wax, rice wax, rhus wax, jojoba oil, and Japan wax. and myrtle wax. Examples of natural animal waxes include beeswax, Punic wax, lanolin, and lacquer wax. Shellac wax and spermaceti wax. Mineral-based waxes include, for example, paraffin wax and microcrystalline wax. Wax, montan wax, mountain wax, ceresin wax, petroleum wax, and petroleum wax. Synthetic waxes include For example, Fischer-Tropsch wax; acrylate wax; fatty acid amide wax; silicone wax; polytetrafluoroethylene wax; Polyethylene wax; ester waxes obtained from higher fatty acids and higher alcohols, such as stearyl stearate and Behenyl behenate; ester waxes obtained from higher fatty acid and monovalent or multivalent lower alcohol are, such as butyl stearate, propyl oleate, glyceride monostearate, glyceride distearate and pentaerythritol tetrabehenate; Ester waxes obtained from higher fatty acids and multivalent alcohol multimers, such as Diethylene glycol monostearate, diglyceryl distearate, dipropylene glycol distearate and triglyceryl tetrastearate; sorbitan ester waxes from higher fatty acids such as sorbitan monostearate and cholesterol fatty acid ester waxes from higher fatty acids such as Cholesteryl stearate; polypropylene wax; and mixtures thereof.
[0033] In some embodiments, the wax can be made from polypropylenes and polyethylenes, which are commercially available from Allied Chemical and Baker Petrolite are available (for example, POLYWAX™ polyethylene waxes from Baker Petrolite), Wax emulsions available from Michelman Inc. and the Daniels Products Company, EPOLENE N-15, commercially available from Eastman Chemical Products, Inc., offers VISCOL 550-P, a low-weight-average polypropylene. Molecular weight available from Sanyo Kasei KK, as well as similar materials. Commercially available Polyethylenes typically have a molecular weight (Mw) of approximately 500 to approximately 2000, such as... approximately 1000 to approximately 1500, while the commercially available polypropylenes used have a molecular weight from approximately 1000 to approximately 10,000. Examples of functionalized waxes are amines, amides, imides, esters, quaternary amines, carboxylic acids or acrylic polymer emulsion, for example JONCRYL 74, 89, 130, 537 and 538, each available from Johnson Diversey, Inc., and chlorinated polyethylenes and polypropylenes, which are commercially available from Allied Chemical, Petrolite Corporation and Johnson Diversey, Inc., are available. The polyethylene and polypropylene compositions may be selected from those shown in British Patent No. 1,442,835.
[0034] The toners can dissolve the wax in an amount of, for example, approximately 1 to approximately 25 wt.% of the toner, such as for example, approximately 3 to approximately 15 wt% of the toner, on a dry basis, or approximately 5 to approximately 20 wt% of the toner or approximately 5 to approximately 11% by weight of the toner.
[0035] The toners can also contain at least one dye. For example, dyes or pigments include, such as They are used here: pigment, dye, mixtures of pigment and dye, pigment mixtures, Dye mixtures and the like. For the sake of simplicity, the term "dye" will be used as it is here. Such dyes, colorants, pigments and mixtures include, unless a specific pigment or a A specific dye component is defined. The dye can be a pigment, a colorant, a mixture thereof, carbon black, Magnetite, black, cyan, magenta, yellow, red, green, blue, brown and mixtures thereof in an amount of approximately 0.1 to comprise approximately 35% by weight based on the total weight of the composition, for example approximately 1 to approximately 25% by weight or approximately 2 to approximately 15% by weight.
[0036] The dye, for example carbon black, cyan, magenta and / or yellow, can be incorporated in an amount which is sufficient to give the toner the desired color. Generally, pigment or colorant is added in a Amount in the range of approximately 1 to approximately 35 wt% of solid-based toner particles is used, for example from approximately 5 to approximately 25 wt.% or approximately 5 to approximately 15 wt.%. However, other quantities are also possible. can be used outside of these areas.
[0037] Coagulants used in the emulsion aggregation processes for the production of toners include Monovalent metallic coagulants, divalent metallic coagulants, polyion coagulants, and the like. As shown here. When used, “polyioncoagulant” refers to a coagulant that is a salt or an oxide, for example a Metal salt or metal oxide consisting of a metal species with a valence of at least 3, at least 4 or at least 5 is formed. Suitable coagulants include, for example, aluminum-based coagulants such as Polyaluminium halides such as polyaluminium fluoride and polyaluminium chloride (PAC), polyaluminium silicates such as Polyaluminium sulfosilicate (PASS), polyaluminium hydroxide, polyaluminium phosphate, aluminum sulfate and the like. Other suitable coagulants include tetraalkyltitinates, dialkyltin oxide, tetraalkyltin oxide hydroxide, dialkyltin oxide hydroxide, aluminum alkoxides, Alkylzinc, dialkylzinc, zinc oxides, tin oxide, dibutyltin oxide, dibutyltin oxide hydroxide, tetraalkyltin, and the like. If Since the coagulant is a polyion coagulant, the coagulants can contain any number of polyion atoms. For example Suitable polyaluminum compounds can range from approximately 2 to approximately 13, such as approximately 3 to approximately 8. or contain approximately 4 to approximately 7 aluminium ions in the compound.
[0038] The coagulants can be incorporated into the toner particles during particle aggregation. In itself, this can Coagulant in the toner particles in an amount of approximately 0 to approximately 5 wt% of the toner particles, such as... approximately more than 0 to approximately 3 wt.% or approximately 0.5 to 2 wt.% of toner particles on a dry weight basis present, excluding external additives.
[0039] In the formation of emulsion aggregation toner particles, which are the amorphous polyester resins disclosed herein Any suitable emulsion aggregation process can be used and modified without restriction. These processes typically include the basic process steps of mixing an emulsion containing a Polymer or resin, optionally one or more waxes, optionally one or more dyes, optionally one or several surfactants, an optional coagulant and one or more optional additives to form a slurry form; of heating the slurry to form aggregated particles in the slurry; of stopping the Aggregation of the particles by adjusting the pH value; and by heating the aggregated particles in the slurry, to coalesce the particles into toner particles; and then to recover them, optionally to wash them, and optionally to... Drying of the obtained emulsion aggregation toner particles.
[0040] The toner particles can have a circularity of approximately 0.920 to approximately 0.999, for example approximately 0.940 up to approximately 0.980 or approximately 0.962 up to approximately 0.980 or approximately more than or equal to 0.965 up to approximately 0.990 exhibit. A circularity of 1.000 indicates a perfectly circular sphere. The circularity can for example, measured with a Sysmex FPIA 2100 analyzer.
[0041] Emulsion aggregation methods offer better control over the distribution of toner particle sizes by They limit the amount of both fine and coarse toner particles in the toner. In some embodiments The toner particles possess a relatively narrow particle size distribution with a lower number-averaged geometric Standard deviation (GSDn) of approximately 1.15 to approximately 1.40, such as approximately 1.15 to approximately 1.25 or approximately 1.20 to approximately 1.35. The toner particles can also exhibit an upper volume-averaged geometric shape. Standard deviation (GSDv) in the range of approximately 1.15 to approximately 1.35, such as approximately 1.15 to approximately 1.21 or approximately 1.18 to approximately 1.30.
[0042] The toner particles can have a volume-averaged diameter (also known as "volume-averaged") particle diameter (or D) from approximately 3 to approximately 25 µm, such as approximately... 50v exhibit thicknesses of 4 to approximately 15 µm or approximately 5 to approximately 12 µm.
[0043] D , GSDv and GSDn can be measured using a measuring instrument, for example the Beckman Coulter 50v Multisizer 3, according to the manufacturer's instructions. Representative sampling can be carried out as follows. The following steps can be performed: a small toner sample (approximately 1 g) can be taken and filtered through a 25 µm sieve and then be added to an isotonic solution to obtain a concentration of approximately 10%, with the sample then run through a Beckman Coulter Multisizer 3.
[0044] The toner particles can have a form factor of approximately 105 to approximately 170, such as approximately 110 to approximately 160 or approximately 115 to approximately 130 SF1*a. Using scanning electron microscopy (SEM) and Image analysis (IA) can be used to analyze or determine the form factor. The average particle shapes are 2 Quantified according to the following form factor (SF1*a) formula: SF1*a = 100μd / (4A), where A is the area of the particle. and whose main axis is. A perfectly circular or spherical particle has a form factor of exactly 100. The form factor SF1*a increases when the shape has a larger surface area and is more irregular or elongated. becomes.
[0045] The characteristics of the toner particles can be determined using a suitable method and a suitable device. are and are not limited to the instruments and procedures listed in the section above.
[0046] The toner particles can have a weight-averaged molecular weight (Mw) in the range of approximately 2500 to approximately 60,000 Da, a number-averaged molecular weight (Mn) in the range of approximately 1,500 to approximately 18,000 Da, and a MWD (ratio of Mw to Mn of the toner particles, a measure of the polydispersity or width of the polymer) of exhibit approximately 1.7 to approximately 10. With regard to cyan and yellow toners, the toner particles can have a Mw of approximately 2500 to approximately 45,000 Da, a Mn of approximately 1500 to approximately 15,000 Da and an MWD of approximately 1.7 up to approximately 10. With regard to black and magenta toners, the toner particles can have a Mw of approximately 2500 to approximately 45,000 Da, a Mn of approximately 1500 to approximately 15,000 Da and an MWD of approximately 1.7 up to approximately 10.
[0047] Furthermore, the toners can, if desired, have a specific ratio between the molecular weight of the latex binder and molecular weight of the toner particles, which are determined according to the emulsion aggregation process. were obtained. As understood in the field, the binding agent undergoes cross-linking during processing, the extent of networking can be controlled during the process. The ratio is best under Reference is made to the molecular peak values (Mp) for the binder, which represent the highest peak of the Mw. According to the present disclosure, the binder can have Mp values in the range of approximately 5000 to approximately 30,000. For example, they exhibit values of approximately 7500 to approximately 29,000 Da. The toner particles produced from the binder Furthermore, they can exhibit a high molecular peak, for example from approximately 5000 to approximately 32,000. for example, approximately 7500 to approximately 31,500 Da, which indicates that the molecular peak depends on the properties of the binder and is not affected by another component such as the dye.
[0048] The toners produced according to the present disclosure can exhibit excellent charge characteristics. exhibit these characteristics when exposed to conditions of extreme relative humidity (RH). The low humidity zone Zone C can have approximately 12 °C / 15% RH, while the high humidity zone (Zone A) can have approximately 28 °C / 85% RH may exhibit rF. Toners of the present disclosure may have an initial toner charge / mass ratio (Q / M) of approximately -2 µC / g to approximately -50 µC / g, such as approximately -4 µC / g to approximately -35 µC / g and one Endoner charge after surface additive mixing from approximately -8 µC / g to approximately -40 µC / g, for example from exhibit temperatures of approximately -10 µC / g to approximately -25 µC / g.
[0049] The toners can exhibit a thermal cohesion at 54 °C of, for example, approximately 0% to approximately 60%, as For example, approximately 5% to approximately 20%, or approximately 0% to approximately 10%, or approximately 5%. Toners can exhibit a thermal cohesion at 55 °C of, for example, approximately 0% to approximately 80%, such as approximately... 5% to approximately 20%, or approximately 0% to approximately 60%, or approximately 8%. The toners can have a Thermal cohesion at 56 °C ranges from approximately 0% to approximately 90%, for example, from approximately 5% to approximately 30% or approximately 0% to approximately 70% or approximately 20%.
[0050] The toners can withstand a cold offset temperature of, for example, approximately 100 °C to approximately 140 °C. for example, approximately 110 °C to approximately 130 °C or approximately 115 °C to approximately 120 °C.
[0051] The toner compositions can produce a gloss (measured at the minimum fixing temperature, MFT) of approximately 10 to approximately 50 gloss units, such as approximately 20 to approximately 40 gloss units or approximately 25 to exhibit approximately 35 gloss units, with measurements obtained on a BYK 75 degree microgloss meter. "Gloss units" refers to the gloss units according to Gardner (GGE), measured on smooth paper (for example) 2 Xerox 90 g / m² COLOR XPRESSIONS+ paper or Xerox 4024 paper). The toners can produce 40 gloss units (TG40) at a Temperature from, for example, approximately 170 °C to approximately 210 °C, or, for example, approximately 180 °C to approximately 200 °C C or approximately 185 °C to approximately 195 °C. The toners can have a peak gloss of, for example, approximately 40 GGE to approximately 75 GGE, such as approximately 50 GGE to approximately 70 GGE or approximately 55 GGE to approximately 65 GGE.
[0052] The fold fixation MFT is measured by folding images that are fixed at various fixing temperatures. were measured, and subsequently a defined mass was rolled over the folded area. The print can also be folded using a commercially available folding device such as the Duplo D-590 paper folder. The paper sheets are then unfolded, and any toner that has broken off from the paper sheet is removed from the surface. wiped. Then the fractionated area is compared with an internal reference table. Smaller fractionated areas indicate better toner adhesion, and the temperature required for acceptable adhesion is considered to be Crease-fixing MFT is defined. The toner compositions can have a crease-fixing MFT of, for example, approximately 115 °C. up to approximately 145 °C, such as approximately 120 °C to approximately 140 °C or approximately 125 °C to approximately 135 °C exhibit.
[0053] In a three-necked round-bottom flask, which is equipped with a blade stirrer, a thermocouple and a with a The Dean-Stark trap, equipped with a water-cooled condenser, contained 83 g of abietic acid (70%). Purity grade; 275 mmol; 1.0 equivalent mass), 25.3 g 99.5% glycerol (275 mmol; 1.0 equivalent mass) and 0.201 g Fascat 4100 catalyst was added. The contents of the flask were heated with stirring and nitrogen. The temperature was The temperature was gradually increased to 225 °C and held at this temperature for 4 to 5 hours. After the esterified product The amount formed was 13.9 g sebacic acid (68.8 mmol; 0.15 equivalent mass) and 19.04 g isophthalic acid (115 mmol; 0.25 (equivalent mass) and 0.191 g of Fascat 4100 catalyst were added to the piston and heating at 220 °C was continued for 14 h. This continued until the softening point (Ts) of the resin reached 115.7 °C. The Ts of the resin was determined using the Mettler test. The FP800 thermal system, consisting of an FP80 central processor and an FP83 dropping cell, was measured. The temperature was programmed to increase by 1 °C / min until the target temperature is reached.
[0054] After the polymer resin had cooled to room temperature, the polymer was cut into small pieces with a chisel. Pieces were broken off and a small portion was ground in an M20 IKA Works mill. The ground polymer was with regard to its molecular weight by gel permeation chromatography (GPC), with regard to its Glass transition temperature (Tg) determined by differential scanning calorimetry (DSC) and viscosity determined by a AR-2000 Rheometric Scientific Rheometer analyzes the acid value (or the "neutralization number" or "acid number"). or ‘acidity’) was measured by dissolving a known amount of a polymer sample in an organic solvent dissolved and titrated with a potassium hydroxide solution of known concentration and phenolphthalein as a color indicator. The acid number is the mass of potassium hydroxide (KOH) in milligrams required to dissolve one gram of the chemical to neutralize the substance. In this case, the acid number served as a measure of the amount of carboxylic acid groups in the substance. Polyester molecule.
[0055] In a three-necked round-bottom flask, which is equipped with a blade stirrer, a thermocouple and a with a The Dean-Stark trap, equipped with a water-cooled condenser, contained 83 g of abietic acid (70%). Purity grade; 275 mmol; 1.0 equivalent mass), 25.3 g 99.5% glycerol (275 mmol; 1.0 equivalent mass) and 0.201 g Fascat 4100 catalyst was added. The contents of the flask were heated with stirring and nitrogen. The temperature was The temperature was gradually increased to 225 °C and held at this temperature for 10 to 13 hours. After the esterified product The amount formed was 13.9 g sebacic acid (68.8 mmol; 0.15 equivalent mass) and 19.04 g isophthalic acid (115 mmol; 0.25 (equivalent mass) and 0.191 g of Fascat 4100 catalyst were added to the piston and heating at 220 °C was continued for 14 h. The process continued until the resin temperature (Ts) reached 121.6 °C. The resin temperature was measured using the Mettler FP800 thermosystem. The temperature was measured using a device consisting of an FP80 central processor and an FP83 dropping cell. It is programmed to increase by 1 °C / min until the target temperature is reached.
[0056] After the polymer resin had cooled to room temperature, the polymer was cut into small pieces with a chisel. Pieces were broken off and a small portion was ground in an M20 IKA Werke mill. The ground polymer sample was Analyzed using GPC, DDK, rheology and acid value.
[0057] 133.87 g of resin-1 emulsion (18.65 wt.- %), 32.65 g crystalline resin emulsion (35.17 wt%), 18.76 g IGI wax dispersion (30.98 wt%) and 21.95 g cyan pigment PB15:3 (17.21 wt%) was added. Separately, 0.54 g of Al(SO₄) (27.85 wt%) was added as a flocculant during the 2 4 3 Homogenizing agents were added. The mixture was heated to 39.3 °C to separate the particles while stirring at 300 rpm. Aggregate. Particle size was monitored with a Coulter counter until the core particles reached a volume-averaged size. Particle size of 4.94 mm with a GSDv of 1.25 had been achieved, and then 94.58 g of resin 1 emulsion were used as Shell material added, resulting in particles with a core-shell structure and an average particle size of 5.60 µm and a GSDv of 1.23 were obtained. The pH of the reaction slurry was then adjusted under The amount of NaOH solution used was increased to 8.45 wt%, and 1.16 g of Versene 100 (ETDA, 39 wt%) were added thereafter. added to stop toner growth. After toner growth was stopped, the reaction mixture was heated to 78 °C and the pH value was adjusted using acetic acid / Sodium acetate (HAc / NaAc) buffer solution, pH 5.7) reduced to 7.65 to achieve coalescence. After the The toner was coalesced and quenched, resulting in a final particle size of 5.96 µm with a GSDv of 1.29 and a GSDn of 1.41 was obtained. The toner slurry was then cooled to room temperature and sieved (25 mm) and filtration separately, followed by washing and freeze-drying.
[0058] In Example 1, the first step of the polymerization leads to the synthesis of (1R,4aR,4bR)-2,3-Dihydroxypropyl7- isopropyl-1,4a-dimethyl-1,2,3,4,4a,4b,5,6,10,10a-decahydrophenanthrene-1-carboxylate or abietin glycerol diol macromer. The results of the analyses of this reaction are shown in Table 1 (below). Table 1. Acidity level Mw Mn PDI Tg (start) Tg (mid) Tg (end) 17, 2 1513 1436 1,05 37, 0 42, 0 47, 1
[0059] The results show that the acidity level (AL) of the macromer is high for a diol, which corresponds to 30% This is due to impurities found in abietic acid, such as diacids or other less reactive substances. Monoacids. Regardless, the purity level of the abietic acid does not impair the quality of the final polymer product. or does not affect them. A study found that the products made from crude tall oil, fatty acids and Rosin resin mixtures from several tips were found when analyzed by gas chromatography. The two The predominant rosin resins were abietic and dehydroabietic acid. Oleic, linoleic, palmitic, and stearic acids were The primary fatty acids, with oleic and linoleic acids being predominant. Using Wiley Mass Spectral In the library of GC-MS (Taylor et al., J. Chromatogr. Sci. 39, 270-272 (2001)), unimportant rosin components were identified. (Isopimaric, pimaric, and neoabietic acid) identified. The presence of bulky groups near the The carboxylic acid group of rosin resins inhibits transesterification because of the molecular activity between the carboxylic acid and hydroxyl follows the sequence of primary -> secondary -> tertiary acids, which then leads to free acid groups leads (analyzed by titration). The second step of polymerization leads to a polymeric material that is very exhibits similar properties to two BPA-containing resins produced using known methods were (BPA resins 1 and 2). The polydispersity of resins 1 and 2 is broader than that of BPA resins 1 and 2, due to the shorter chain population of the polymers (a result of the purity of the abietic acid). However, the broad Polydispersity does not affect the resin characteristics or rheology. Resin 2 was used for a longer period than resin 1. The first step involved a reaction, resulting in minimal networking. Despite this networking, Harz 2 was still too 100% soluble in tetrahydrofuran (TFH), without gel formation. Overall, the rheology of the resins shows 1 and 2 a good viscosity transition from low to high temperatures, which is suitable for amorphous resins for EA toners are characteristic.
[0060] In the following Table 2 are the test formulations and properties of resins 1 and 2 with the BPA resins 1 and 2 compared. Table 2. Tg Monomers (mol Ts (° (Insert) Resin ID Biocontent Acidity Mn Mw / Equ.) C) °C Rosin resin glycerol sebacic acid iPA Macromere (Eq.) (Eq.) Resin 1 0.60 0.15 0.25 86.1% 115.7 55.3 14.5 1755 29888 Harz 2 0.60 0.15 0.25 86.1% 121.6 53.7 8.4 1300 26718 129, BPA resin 1 k. A. 0% 55.2 12.7 5600 53300 0 BPA resin 2 k. A. 0% 118.0 58.8 14.7 5000 19400 *iPA = Isophthalic acid
Claims
1. A process for producing a bio-based polyester resin, the process comprising: Providing a bio-based glycerol which is a transester product of crude vegetable oil; Providing a bio-based abietic acid; Carrying out an esterification reaction between the bio-based glycerol and the bio-based abietic acid to produce a 100 mol% bio-based abietic acid-glycerol macromer; wherein the esterification comprises heating for at least 4 h includes; and Polycondensing the macromer with at least two diacids in the presence of a catalyst to produce the bio-based to obtain resin, wherein the polyester resin has a softening point temperature of 90 °C to 150 °C and an acid value of 8 to 16 mg KOH / g and wherein the polyester resin is at least 80 mol% bio-based.
2. The method according to claim 1, wherein the at least one diacid is a mixture of sebacic acid and either Isophthalic acid or succinic acid.
3. The method according to claim 1, wherein the at least one diacid is selected from the group consisting of sebacic acid, succinic acid, isophthalic acid, adipic acid, azelaic acid and glutaric acid.
4. The process according to claim 1, wherein the ratio of the macromer in the polyester resin is 5 to 95 mol% of the polyester resin amounts.
5. The process according to claim 1, wherein the polyester resin has a glass transition temperature of 30°C to 120°C.
Citation Information
Patent Citations
Baking enamel
US1998744A
Temperature switchable adhesives comprising crystallizable abietic acid derivative-based tackifiers
US20060235121A1
Toner compositions and processes
US20090047593A1
Polyester-wax based emulsion aggregation toner compositions
US20090142689A1
Process for the Preparation of Biodiesel from Vegetable Oils Containing High FFA
US20100205853A1