Method for recovering ammonia from vanadium processing for ammonium processing and wastewater reuse

The method recovers ammonia and treats wastewater in vanadium processing by forming ammonium metavanadate and polyvanadate, using a polyacid ester to precipitate impurities and recover ammonia, addressing emissions and pollution in conventional processes, achieving high-purity vanadium products and wastewater reuse.

DE102019124431B4Active Publication Date: 2024-11-14ZHONGFANLIAN TECH DEV CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE102019124431
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-13
Filing Date
2019-09-11
Publication Date
2024-11-14
Estimated Expiration
2039-09-11

AI Technical Summary

Technical Problem

Conventional vanadium extraction processes generate ammonia emissions and wastewater containing harmful substances, leading to resource waste and environmental pollution, with existing treatments being complex and ineffective.

Method used

A method for recovering ammonia and treating wastewater by using ammonium metavanadate and ammonium polyvanadate to form ammonium metavanadate and ammonium polyvanadate, employing a polyacid ester (flocculant) to precipitate impurities, and a thermal separation technique to recover ammonia, ensuring zero emissions and wastewater reuse.

Benefits of technology

Achieves zero ammonia emissions and high-purity vanadium products with 99.5 to 99.99% purity, effectively treating wastewater for reuse, reducing environmental impact and resource waste.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Method for recovering ammonia from vanadium processing for ammonium processing and wastewater reuse, comprising a vanadium processing process: 1) Processing of ammonium metavanadate and ammonium polyvanadate; 2) Using ammonium metavanadate and ammonium polyvanadate to produce high-purity vanadium pentoxide, the process comprising the following steps: a) Alkali dissolution: Dissolving ammonium metavanadate (NH4VO3) or ammonium polyvanadate ((NH4)2V6O 16 ) in an alkaline solution, heating of the ammonium metavanadate (NH4VO3) or the ammonium polyvanadate ((NH4)2V6O 16 ) to dissolve, producing a large amount of ammonia (NH3), subjecting the ammonia (NH3) and the water to a thermal separation technique so that the ammonia (NH3) enters a recovery tower, while steam falls into a reactor; b) Adjusting the pH: Adjusting the pH of the mixture of the alkali and the ammonium metavanadate (NH4VO3) or the ammonium polyvanadate ((NH4)2V6O 16 ) with an acid during dissolution, during which ammonia (NH3) enters the recovery tower and some of the ammonia (NH3) is converted to metallic ammonium (NH4) due to the action of the acid + ) forms; c, Synthesis: where ammonium (NH4) + ) within a sodium vanadate concentrate (Na3VO4 concentrate) and ammonia (NH3) cannot be volatilized; d, Washing: wherein a large amount of sodium salts is present in the ammonium metavanadate (NH4VO3) and the ammonium metavanadate (NH4VO3) is mixed with a certain amount of ammonium protective water (NH4 + protective water (R)) must be washed and finally sprayed with a suitable amount of pure water, resulting in highly pure ammonium metavanadate (NH4VO3); e. Drying: Baking the ammonium metavanadate (NH4VO3) in an environment of 40 to 60 °C to remove water (H2O) from the ammonium metavanadate (NH4VO3) at this temperature; and f, Firing: Conversion of ammonium metavanadate (NH4VO3) to vanadium pentoxide (V2O5) in a furnace at 450 to 550 °C, whereby the ammonium (NH4 + ) in which ammonium metavanadate (NH4VO3) is converted to ammonia (NH3) at high temperature, and all of the ammonia (NH3) is fed into an ammonia (NH3) recovery tower or ammonia (NH3) recovery device for enrichment; introducing a strong acid into the ammonia (NH3) recovery tower or the ammonia (NH3) recovery device to convert ammonium (NH4) +) to process; wherein the step of processing the ammonium metavanadate or the ammonium polyvanadate includes: processing an ore, pulverizing by a ball mill, adding a conversion agent, pelletizing into a sphere shape of Ø 8-12 mm, roasting the pelletized vanadium material at 800-850 °C, leaching, adjusting the pH, enriching to obtain a sodium vanadate concentrate or a vanadyl sulfate concentrate, conversion, removing an impurity and synthesizing to the ammonium metavanadate or the ammonium polyvanadate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention belongs to the technical field of vanadium processing and, in particular, relates to a process for recovering ammonia from vanadium processing for ammonium processing and wastewater reuse. background

[0002] The element vanadium is widely used in the steel, non-ferrous metal, chemical, alloy, superconducting materials and automotive industries and is an important strategic material.

[0003] In nature, the element vanadium is extremely finely dispersed, usually in the form of V(III) and V(IV). V(III) is in the majority, and trivalent vanadium can be intercalated into a silicate mineral crystal lattice in an isomorphic form, while tetravalent vanadium can be found in an isomorphic form in a silicon-oxygen tetrahedral structure. Such ores are difficult to leach. To leach trivalent or tetravalent vanadium, the crystal structures must be disrupted to release the vanadium from the crystal structures.

[0004] Conventional vanadium extraction processes can be summarized into two representative types: a roasted vanadium extraction process (a fire vanadium extraction process) and a wet vanadium extraction process.

[0005] The wet vanadium extraction process consists in directly acid leaching a vanadium-bearing ore to obtain a vanadium-bearing liquid from a vanadium mineral under highly concentrated acid conditions, even in an environment in the presence of heat and pressure and an oxidizing agent. The fire vanadium extraction process consists in subjecting an ore to high-temperature oxidation roasting to oxidize the low-valent vanadium and convert it into pentavalent vanadium, followed by wet leaching to obtain a vanadium-bearing liquid to extract vanadium from the ore. In the roasted vanadium extraction process, bituminous coal is subjected to oxidation / sodium roasting with the addition of salt to form a vanadium-bearing clinker; the vanadium-bearing clinker is directly leached with process water (i.e.,Immersion in water) to obtain an eluate with a lower vanadium concentration; ammonium chloride is added to precipitate vanadium to obtain an ammonium metavanadate precipitate, and then crude vanadium pentoxide (crude vanadium) is obtained by roasting; the crude vanadium is subjected to caustic solubilization, impurity removal, and secondary vanadium precipitation by ammonium chloride to obtain ammonium metavanadate; the ammonium metavanadate is thermally decomposed to obtain a vanadium pentoxide product with a purity of more than 98%; this constitutes a "two-stage sodium roasting vanadium precipitation process" or a "salt-roasting vanadium extraction process".Alternatively, lime, limestone, or any other calcium-containing compound is used as an additive for pelleting with the coal for roasting, so that vanadium is oxidized to a water-insoluble calcium salt of vanadium; then the calcium salt is carbonized and leached to form a vanadium-containing solution, which is then leached with an acid or a dilute alkali solution; subsequently, hydrolysis of the vanadium precipitate, extraction from solution, or ion exchange is carried out, and pyrolysis is used to refine the vanadium.

[0006] Shortly after the vanadium ore is roasted with the salt to form the vanadium-bearing clinker, water, an acid, or an alkali must be used to leach the trivalent vanadium, tetravalent vanadium, or pentavalent vanadium from the vanadium-bearing clinker; then, the vanadium salt is separated from the other components in the eluate by extraction and back-extraction or ion exchange; finally, the vanadium salt reacts with ammonia water or any other ammonium salt to form an ammonium metavanadate precipitate, and the ammonium metavanadate precipitate is thermally decomposed to obtain a high-purity vanadium pentoxide product.

[0007] However, in the roasted vanadium extraction process, ammonia gas or the like is released from a roaster, and when acid (sulfuric acid) is used for leaching, a large amount of wastewater is generated. This wastewater contains sulfuric acid and sulfur dioxide, and even if neutralization treatment is performed, the wastewater still contains sulfate and other harmful substances (such as ammonia nitrogen and residual sulfate radicals). The conventional vanadium extraction process is complex, and the most difficult to control and manage are ammonia emissions and wastewater treatment. If the ammonia and wastewater generated in the above process are not treated technically, it not only wastes resources but also causes environmental pollution of rivers and lakes, and even damages human drinking water sources.

[0008] CN 1 06 430 307 A discloses a process for producing high-purity zirconium dioxide. Acid precipitates are combined with sulfur-containing precipitates and dissolved in water. The resulting product is then purified to remove impurities. This process reduces the loss of wash solution and extends the service life of the exchange resins, thus lowering production costs.

[0009] US Pat. No. 4,061,711 A discloses a process for recovering vanadium by leaching a vanadium-containing material in an ammoniacal medium at high temperatures and pressures. Subsequently, the soluble ammonium metavanadate is separated, precipitated, and further separated to obtain the desired vanadium. Summary

[0010] In view of the problems of the prior art process, it is an object of the present invention to prepare ammonium metavanadate (NH4VO3) and ammonium polyvanadate (NH4)2V6O 16 from the beginning of mining and smelting and capture all the emitted ammonia (NH3) to produce ammonium (NH4 + ) in the process for the preparation of high-purity vanadium pentoxide (V2O5) using ammonium metavanadate (NH4VO3) or ammonium polyvanadate (NH4)2V6O 16 to form a wastewater treatment plant, thereby ensuring zero emission of the exhaust gas, and to effectively treat all the wastewater generated in the above process using a technique with a polyacid ester (a patented product, also known as a flocculant), thereby ensuring that all the wastewater is not discharged but reused, and causing the purity of all products to reach 99.5 to 99.99%.

[0011] The present invention is implemented by the following technical solutions.

[0012] A process for recovering ammonia from vanadium processing for ammonium processing and wastewater reuse, wherein a vanadium processing process includes: 1) processing ammonium metavanadate and ammonium polyvanadate; 2) using the ammonium metavanadate and ammonium polyvanadate to process high-purity vanadium pentoxide, the process including the following steps: a, Alkali dissolution: Dissolving ammonium metavanadate (NH4VO3) or ammonium polyvanadate (NH4)2V6O 16 in a lye (NaOH), heating the ammonium metavanadate (NH4VO3) or the ammonium polyvanadate (NH4)2V6O 16for dissolving, producing a large amount of ammonia (NH3), subjecting the ammonia (NH3) and water to a thermal separation technique, so that the ammonia (NH3) enters a recovery tower while water vapor falls into a reactor; b, pH adjustment: adjusting the pH with an acid during dissolving, during which ammonia (NH3) enters the recovery tower and a part of the ammonia (NH3) forms metallic ammonium (NH4) due to the action of the acid + ) is formed; c, synthesis: where ammonium (NH4 + ) is located within a sodium vanadate concentrate (Na3VO4 concentrate) and ammonia (NH3) cannot be volatilized; d, washing: where a large amount of sodium salts is present in the ammonium metavanadate (NH4VO3) and the ammonium metavanadate (NH4VO3) is washed with a certain amount of ammonium protective water (NH4 +-protective water) and finally sprayed with an appropriate amount of pure water, thereby obtaining high-purity ammonium metavanadate (NH4VO3); e, drying: baking the ammonium metavanadate (NH4VO3) in an environment of 40 to 60 °C to remove water (H2O) from the ammonium metavanadate (NH4VO3) at this temperature; and f, firing: converting the ammonium metavanadate (NH4VO3) into vanadium pentoxide (V2O5) in a kiln at 450 to 550 °C, whereby the ammonium (NH4 + ) in which ammonium metavanadate (NH4VO3) is converted into ammonia (NH3) at high temperature, and introducing all of the ammonia (NH3) into an ammonia (NH3) recovery tower or an ammonia (NH3) recovery device for enrichment; introducing a strong acid into the ammonia (NH3) recovery tower or the ammonia (NH3) recovery device to convert the ammonia (NH3) to various ammonium (NH4 + ) to catch.

[0013] According to the invention, the step of processing the ammonium metavanadate or the ammonium polyvanadate includes: processing an ore, pulverizing with a ball mill, adding a converting agent, pelletizing into a spherical shape of Ø 8 to 12 mm, roasting the pelletized vanadium material in an environment of 800 to 850 °C, leaching, adjusting the pH, concentrating to obtain a sodium vanadate concentrate or a vanadyl sulfate concentrate, converting, removing an impurity, and synthesizing into the ammonium metavanadate or the ammonium polyvanadate.

[0014] Preferably, the leaching step is: leaching a roasted vanadium pellet (V pellet) and water or acid leaching the converted or oxidized vanadium (V) using one of the methods of cold leaching, warm leaching and spray leaching to form a sodium vanadate solution (Na3VO4 solution) or a vanadyl sulfate concentrate (VOSO4 concentrate).

[0015] Preferably, the enrichment step is: water leaching a low-grade vanadium ore (V ore) with a concentration of 2 to 10 g / L, adjusting the pH to 6 to 5 with an acid to convert the contained vanadium (V) into a cation, enriching using a cationic resin such as 731 or 717, and back-extracting with sodium hydroxide (NaOH) when the resin is saturated, whereby the enriched vanadium content can reach 120 to 150 g / L.

[0016] Preferably, the acid-leached vanadium concentrate is enriched using any of triphenyl phosphate TPP, (C e H5O)3PO, di(2-ethylhexyl)-phosphate (C 16 H 35 O4P), an extractant P-204 and a component of the organic phase of sulfonated kerosene and back-extracted with a strong acid (sulfuric acid) to enrich the vanadium concentrate to 120 to 150 g / L.

[0017] Preferably, the step of converting consists in that: based on the water leaching, the caustic back-extraction and the cold pH adjustment, the sodium vanadate concentrate (Na3VO4 concentrate) forms a red color when it encounters an acid, and thus the sodium vanadate concentrate (Na3VO4 concentrate) is heated to decouple an acid phase thereof from a vanadium ion, thereby converting the concentrate into a watery or oily state.

[0018] Preferably, the step of removing an impurity is: to ensure the quality of the ammonium metavanadate (NH4VO3), subjecting the converted sodium vanadate concentrate (Na3VO4 concentrate) to removal of the impurity with 2% polyacid ester (a patented product, also known as a flocculant) so that a non-metallic impurity is dissolved, precipitated and pressure filtered or filtered, and then storing the concentrate for further use.

[0019] Preferably, the synthesizing step is: adding 1.1 times ammonium chloride (NH4Cl), 1.5 times ammonium sulfate (NH4)2SO4 or 1.8 times ammonium nitrate (NH4NO3) to the processed concentrate according to different vanadium contents and stirring and synthesizing to obtain the ammonium metavanadate (NH4VO3).

[0020] Preferably, the method of synthesizing the ammonium metavanadate (NH4VO3) is as follows: (1) using an ammonium mother solution (NH4 + solution) containing synthesized ammonium metavanadate (NH4VO3), determining a specific gravity of 24 to 25 using a Baume pycnometer (°Bé), heating or condensing the ammonium mother solution (NH4 + solution) to a specific gravity of 28 to 29, adding 10% ammonium chloride (NH4Cl), ammonium sulfate (NH4)2SO4 or ammonium nitrate (NH4NO3) to the ammonium mother solution (NH4 + solution), stirring to dissolve, activating the ammonium mother solution (NH4 + solution), then determining the specific gravity to 32 to 34 using the Baume pycnometer (°Bé), adding 2% of the polyacid ester (a patented product, also known as a flocculant) to the ammonium mother solution (NH4 +-solution), stirring to dissolve impurities, thereby removing insoluble ammonium salt, sodium and sodium salt and feeding it into a re-synthesis stage for further use; and (2) when the ammonium vanadate (NH4VO3) is synthesized, preparing the vanadium content of the sodium vanadate concentrate (Na3VO4 concentrate) to 100 to 120 g / L, feeding the ammonium mother solution (NH4 + solution) in a volume ratio of 45 to 55%, stirring for 1 to 2 hours, thereby forming solid ammonium metavanadate (NH4VO3) therein, the vanadium content being 0.2 to 0.5 g / L at an upper layer of the concentrate, dewatering or drying to obtain the ammonium metavanadate (NH4VO3), and reusing the used ammonium mother liquor for synthesis according to the operation method of (1).

[0021] The vanadyl sulfate concentrate obtained by acid leaching and back extraction with a strong acid in the leaching step is heated to 60 to 90 °C and neutralized to a pH of 4 to 5 using liquid ammonium, whereby the ammonium polyvanadate (NH4)2V6O 16 is received.

[0022] The present invention has the following advantages: 1. During the smelting of a vanadium ore resource (V resource), a roasted powder or pellet is leached with acid or water, and the leached vanadium (V) concentration is generally 4 to 10 g / L, so enrichment treatment using an organic phase or resin is required; however, enrichment requires a large amount of water and generally generates 150 to 300 tons of acidic wastewater per ton of product. 2. The present process uses lime (CaO) or sodium hydroxide (NaOH) to neutralize to a pH of 7.6 to 7.8, but the wastewater cannot be discharged because the wastewater contains a large amount of heavy metals such as chromium (Cr) and titanium (Ti), and impurities and toxic components such as silicon (Si), calcium (Ca), magnesium (Mg) and soil, and different mineral springs produce various impurities.Currently, the widely used evaporation process may not achieve the control effect, and it is unrealistic to evaporate 150 to 300 tons of wastewater per ton of vanadium pentoxide (V2O5). Even advanced isolation membrane technology cannot achieve the desired effect, because the isolation membrane can only handle a conductivity of 300 to 500 S / m, and the conductivity of the wastewater at this point has reached 5,000 to 10,000 S / m, making it impossible for the wastewater to pass through the isolation membrane. Therefore, the present process adds a polyacid ester (a patented product, also known as a flocculant) to the neutralized wastewater. All impurities, heavy metals, and toxic components can be dissolved and precipitated after 20 to 30 minutes of stirring. The precipitated particles are fine, suspended, and not prone to precipitation. 3. In the present process, a certain amount of amorphous precipitated silica (SiO2) is added, which mainly has the following functions in wastewater treatment: (1) adsorption; (2) color removal; (3) precipitation of suspended impurities; and (4) refining, etc. Therefore, the present process can accelerate the precipitation of the above suspended substances and facilitate clarification filtration. 4. The present process can produce ammonium metavanadate (NH4VO3) and ammonium polyvanadate (NH4)2V6O 16 directly extract from the beginning of mining and melting and capture all emitted ammonia (NH3) to produce ammonium (NH4 + ) in the process of processing high-purity vanadium pentoxide (V2O5) using ammonium metavanadate (NH4VO3) or ammonium polyvanadate (NH4)2V e O 16thereby ensuring zero emission of the exhaust gas, and effectively treat all the wastewater generated in the above process using a technique with a polyacid ester (a patented product, also known as a flocculant), thereby ensuring that all the wastewater is not discharged but reused, and causing the purity of all products to reach 99.5 to 99.99%. 5. A "conversion inducer for vanadium-containing filtered solid during vanadium ore smelting and roasting" derived from the present process has been filed as a national patent (Patent No.: CN 108 034 807 A) and can be used as a separate product for the conversion of a vanadium ore product. 6. The polyacid ester used in the present invention is concentrated phosphodiester, which is a patented product of invention, also known as flocculant, available from Taicang Changfeng Chemical Plant in Jiangsu Province. Detailed description

[0023] The following further describes the present invention with reference to illustrative embodiments, which are not intended to limit the scope of the present invention, and all materials implemented based on the techniques of the present invention described above are intended to fall within the scope of the present invention. I. Ammonium metavanadate (NH4VO3) and ammonium polyvanadate (NH4)2V6O 16 can be processed from the beginning of mining and smelting using a “one-step process”.

[0024] A vanadium crude ore is leached to obtain a sodium vanadate concentrate (with different grades processed by different processes according to different crude vanadium grades) to obtain the ammonium metavanadate (NH4VO3) and the ammonium polyvanadate (NH4)2V6O 16 The procedure is generally as follows: Vanadium ore → ore processing → pulverization → addition of the conversion agent ↓ Pelleting → Roasting → Leaching → Adjusting the pH value → Enrichment ↓ Obtaining the sodium vanadate concentrate → Adjusting the pH → Conversion ↓ Synthesis → Obtaining ammonium metavanadate or ammonium polyvanadate 1. Vanadium ore: vanadium slag, vanadium sludge or coal gangue containing vanadium (V). 2. Ore processing: Impurities other than vanadium (V) are removed. 3. Pulverization: The vanadium slag, vanadium sludge or coal gangue containing vanadium (V) is pulverized using a ball mill. 4. Addition of the conversion agent: Various conversion agents or oxidizing agents, such as soda (Na2CO3), barite (BaSO4) or other cerium salts, are added to various vanadium ore resources (V resources), and a salt (NaCl) may also be added. 5. Pelletizing: Low-grade vanadium ore resources (V ore resources), such as vanadium oxide mud and coal gangue, are formed into a spherical shape of Ø 8 to 12 mm, and high-grade vanadium ore resources (V ore resources) can be made into a powder. 6. Roasting: The ground powder and pelletized vanadium material are roasted (or fired) at 800 to 850 °C in different roasters or different facilities to achieve the purposes of converting and oxidizing vanadium (V). 7. Leaching: The roasted vanadium powder (V-powder) or vanadium pellets (V-pellets) are water-leached or acid-leached using cold leaching, warm leaching or spray leaching for the purpose of leaching the converted or oxidized vanadium (V) to form a sodium vanadate concentrate (Na3VO4 concentrate) or vanadyl sulfate concentrate (VOSO4 concentrate). 8. Adjusting pH: The pH is adjusted using various extraction methods, but does not need to be adjusted in the case of acid leaching. 9. Enrichment: A low-grade vanadium ore (V ore) is water-leached and generally has a concentration of 2 to 10 g / L; therefore, the pH must be adjusted to 6 to 5 with an acid to convert the contained vanadium (V) into a cation. A cationic resin, such as 731 or 717, is used for enrichment, and sodium hydroxide (NaOH) is used for back-extraction when the resin is saturated. The enriched vanadium content can generally reach 120 to 150 g / L. In the case of acid leaching, the concentrate can be leached with triphenyl phosphate (TPP) or (C6H5O)3PO, or by di(2-ethylhexyl) phosphate (C 16 H 35 O4P), an extractant P-204 and a component of the organic phase of sulfonated kerosene and back-extracted with a strong acid (sulfuric acid), which can also enrich the vanadium concentrate to 120 to 150 g / L. 10. Obtaining: Sodium vanadate concentrate (Na3VO4 concentrate) or vanadyl sulfate concentrate (VOSO4 concentrate) is obtained accordingly. Sodium vanadate concentrate (Na3VO4 concentrate) is processed by water leaching, acid extraction, and alkali back-extraction, while vanadyl sulfate concentrate (VOSO4 concentrate) is processed by acid leaching and strong acid back-extraction. 11. Adjusting the pH: The resulting vanadium concentrate varies with different enrichment and back-extraction processes. A water-leached concentrate is back-extracted with sodium hydroxide (NaOH) to produce an alkaline concentrate called sodium vanadate concentrate (Na3VO4 concentrate), in which case the pH must be adjusted to 7.8 to 8.5 for further use. A concentrate that has been acid-leached and back-extracted with a strong acid does not require pH adjustment for further use. 12. Conversion: Based on water leaching, caustic back extraction, and cold pH adjustment, the sodium vanadate concentrate (Na3VO4 concentrate) forms a red color when it encounters an acid, and thus the sodium vanadate concentrate (Na3VO4 concentrate) must be suitably heated to decouple an acid phase thereof from a vanadium ion, thereby converting the concentrate into a watery or oily state (see 4 for acid leaching and strong acid back extraction). 13. Removal of impurities: To ensure the quality of ammonium metavanadate (NH4VO3), the reformed sodium vanadate concentrate (Na3VO4 concentrate) must be subjected to impurity removal with 2% polyacid ester (a patented product, also known as flocculant) so that non-metallic impurities are dissolved, precipitated, and pressure filtered or filtered, and then the concentrate is stored for further use (see 4 for acid leaching and strong acid back extraction). 14. Synthesis: Ammonium chloride (NH4Cl), ammonium sulfate (NH4)2SO4 or ammonium nitrate (NH4NO3) is added to the above-prepared concentrate according to different vanadium contents (1+1.2 to 1.6 or so), and the concentrate is stirred and synthesized to obtain ammonium metavanadate (NH4VO3).

[0025] The procedure for synthesizing ammonium metavanadate (NH4VO3) is as follows: (1) Using an ammonium mother solution (NH4 + solution) containing synthesized ammonium metavanadate (NH4VO3), determining a specific gravity of 24 to 25 using a Baume pycnometer (°Be), heating or condensing the ammonium mother solution (NH4 + solution) to a specific gravity of 28 to 29, adding 10% ammonium chloride (NH4Cl), ammonium sulfate (NH4)2SO4 or ammonium nitrate (NH4NO3) to the ammonium mother solution (NH4 + -solution), stirring to dissolve, activating the ammonium mother solution (NH4 solution), then determining the specific gravity to 32 to 34 using the Baume pycnometer (°Bé), adding 2% of the polyacid ester (a patented product, also known as a flocculant) to the ammonium mother solution (NH4 + -solution), stirring to dissolve an impurity, thereby removing insoluble ammonium salt, sodium and sodium salt and introducing into a resynthesis stage for further use; and (2) when the ammonium vanadate (NH4VO3) is synthesized, preparing the vanadium content of the sodium vanadate concentrate (Na3VO4 concentrate) to 100 to 120 g / L, feeding the ammonium mother solution (NH4) prepared in (1) + solution) in a volume ratio of 45 to 55%, stirring for 1 to 2 hours, thereby forming solid ammonium metavanadate (NH4VO3) therein, the vanadium content being 0.2 to 0.5 g / L at an upper layer of the concentrate, dewatering or drying to obtain the ammonium metavanadate (NH4VO3), and reusing the used ammonium mother liquor for synthesis according to the operation method of (1).

[0026] A concentrate obtained by acid leaching and back extraction with a strong acid should be heated to 60 to 90 °C and neutralized to a pH of 4 to 5 using liquid ammonium, which yields the ammonium polyvanadate (NH4)2V e O 16 is received. II. In the process of processing high-purity vanadium pentoxide (V2O5) using ammonium metavanadate (NH4VO3) or ammonium polyvanadate (NH4)2V e O 16 all the ammonia is recovered to process ammonium.

[0027] The procedure and processing method are as follows: Alkali dissolution → pH adjustment → Synthesis → Washing → Drying ↓ Burning → Ammonium 1. Caustic soda dissolution: A caustic soda dissolution process (NaOH dissolution) is necessary for the preparation of high-purity vanadium pentoxide (V2O5) using ammonium metavanadate (NH4VO3) or ammonium polyvanadate (NH4)2V e O 16 ; the process of lye dissolution is heating the ammonium metavanadate (NH4VO3) or the ammonium polyvanadate (NH4)2V e O 16to dissolve, which inevitably produces a large amount of ammonia (NH3); the ammonia (NH3) and water must undergo a thermal separation technique, so that the ammonia (NH3) enters a recovery tower, while water vapor falls into a reactor. 2. Adjusting the pH: During the process of adjusting the pH with an acid during dissolution, ammonia (NH3) enters the recovery tower, and a part forms metallic ammonium (NH4) due to the action of the acid. + ), which leads to the regeneration and purification of ammonia (NH3). 3. Synthesis: Since ammonium (NH4 + ) in the sodium vanadate concentrate (Na3VO4 concentrate), the ammonia (NH3) should not evaporate. 4. Washing: Since high-purity ammonium metavanadate (NH4VO3) is obtained from a concentrate of ammonium vanadate (NH4VO3) and alkali (NaOH), a large amount of sodium salts is present in the ammonium metavanadate (NH4VO3), and the ammonium metavanadate (NH4VO3) must be washed with a certain amount of ammonium (NH4 + -)protective water (otherwise sodium vanadate dissolves in the water) and finally sprayed with an appropriate amount of pure water to obtain the high-purity ammonium metavanadate (NH4VO3). 5. Drying: The ammonium metavanadate (NH4VO3) is baked in an environment of 40 to 60 °C; due to an internal factor, at such a temperature only water (H2O) can be removed from the ammonium metavanadate (NH4VO3), but the ammonium (NH3) is unlikely to volatilize. 6. Firing: The ammonium metavanadate (NH4VO3) is converted into vanadium pentoxide (V2O5) in a kiln at 450 to 550 °C, and the ammonium (NH4 +) in the ammonium metavanadate (NH4VO3) is converted to ammonia (NH3) at high temperature; then, all of the ammonia (NH3) must be added to an ammonia (NH3) recovery tower or ammonia (NH3) recovery device for enrichment. Hydrochloric acid (HCl) is added to the ammonia (NH3) recovery tower or ammonia (NH3) recovery device to form ammonium chloride (NH4Cl), sulfuric acid (H2SO4) is added to form ammonium sulfate (NH4)2SO4, and nitric acid (HNO3) is added to form ammonium nitrate (NH4NO3). This process has served many purposes, not only that the high purity vanadium pentoxide (V2O5) is obtained, but also that all the ammonia (NH3) is captured to produce ammonium (NH4 + ), not only prevents the evaporation of ammonia (NH3) and purifies the air, but also reduces costs and increases economic benefits.

[0028] The above is only a detailed description of one possible embodiment of the present invention, and the embodiment is not intended to limit the patentable scope of the present invention, and any equivalent implementation or modification made without departing from the concept of the present invention is intended to fall within the patentable scope of the present invention.

Claims

[1] A process for recovering ammonia from vanadium processing for ammonium treatment and wastewater reuse, wherein a vanadium treatment process comprises: 1) Processing of ammonium metavanadate and ammonium polyvanadate; 2) Using the ammonium metavanadate and the ammonium polyvanadate to prepare high-purity vanadium pentoxide, the process comprising the following steps: a, Alkali dissolution: Dissolving the ammonium metavanadate (NH4VO3) or the ammonium polyvanadate ((NH4)2V6O 16 ) in a lye, heating the ammonium metavanadate (NH4VO3) or the ammonium polyvanadate ((NH4)2V6O 16 ) to dissolve, producing a large amount of ammonia (NH3), subjecting the ammonia (NH3) and water to a thermal separation technique so that the ammonia (NH3) enters a recovery tower while water vapor falls into a reactor; b, Adjusting the pH: Adjusting the pH of the mixture of the alkali and the ammonium metavanadate (NH4VO3) or the ammonium polyvanadate ((NH4)2V6O 16 ) with an acid during dissolution, during which ammonia (NH3) enters the recovery tower and part of the ammonia (NH3) due to the action of the acid forms metallic ammonium (NH4 + ) forms; c, Synthesis: where ammonium (NH4 + ) is located within a sodium vanadate concentrate (Na3VO4 concentrate) and ammonia (NH3) cannot be volatilized; d, Washing: where a large amount of sodium salts is present in the ammonium metavanadate (NH4VO3) and the ammonium metavanadate (NH4VO3) is washed with a certain amount of ammonium protective water (NH4 + protective water (R)) and finally sprayed with an appropriate amount of pure water, thereby obtaining high-purity ammonium metavanadate (NH4VO3); e, drying: baking the ammonium metavanadate (NH4VO3) in an environment of 40 to 60 °C to remove water (H2O) from the ammonium metavanadate (NH4VO3) at this temperature; and f, Firing: Converting the ammonium metavanadate (NH4VO3) into vanadium pentoxide (V2O5) in a kiln at 450 to 550 °C, whereby the ammonium (NH4 + ) in which ammonium metavanadate (NH4VO3) is converted into ammonia (NH3) at the high temperature, and introducing all of the ammonia (NH3) into an ammonia (NH3) recovery tower or an ammonia (NH3) recovery device for enrichment; introducing a strong acid into the ammonia (NH3) recovery tower or the ammonia (NH3) recovery device to convert ammonium (NH4 +); wherein the step of processing the ammonium metavanadate or the ammonium polyvanadate includes: processing an ore, pulverizing by a ball mill, adding a converting agent, pelletizing into a spherical shape of Ø 8-12 mm, roasting the pelletized vanadium material at 800-850 °C, leaching, adjusting the pH, concentrating to obtain a sodium vanadate concentrate or a vanadyl sulfate concentrate, converting, removing an impurity, and synthesizing into the ammonium metavanadate or the ammonium polyvanadate. [2] A process for recovering ammonia from vanadium processing for ammonium upgrading and wastewater reuse according to claim 1, wherein the leaching step is: water or acid leaching of a roasted vanadium pellet (V pellet) by one of cold leaching, warm leaching or spray leaching, thereby leaching the converted or oxidized vanadium (V) to form a sodium vanadate concentrate (Na3VO4 concentrate) or vanadyl sulfate concentrate (VOSO4 concentrate). [3] A method for recovering ammonia from vanadium processing for ammonium upgrading and wastewater reuse according to claim 1, wherein the enriching step is: water-leaching a low-grade vanadium ore (V ore) having a concentration of 2 to 10 g / L, adjusting the pH to 6 to 5 with an acid to convert the contained vanadium (V) into a cation, enriching using a cationic resin such as 731 or 717, and back-extracting with sodium hydroxide (NaOH) when the resin is saturated, whereby the enriched vanadium content can reach 120 to 150 g / L. [4] A process for recovering ammonia from vanadium processing for ammonium treatment and wastewater reuse according to claim 2, wherein the acid-leached vanadium concentrate is leached with triphenyl phosphate (TPP or (C6H5O)3PO) using any of di(2-ethylhexyl) phosphate (C 16 H 35O4P), an extractant P-204 and a component of the organic phase of sulfonated kerosene and back-extracted with a strong acid to enrich the vanadium concentrate to 120 to 150 g / L. [5] A method for recovering ammonia from vanadium processing for ammonium processing and wastewater reuse according to claim 1, wherein the step of removing an impurity is: To ensure the quality of ammonium metavanadate (NH4VO3), subjecting the converted sodium vanadate concentrate (Na3VO4 concentrate) to impurity removal with 2% polyacid ester so that a non-metallic impurity is dissolved, precipitated and pressure filtered or filtered, and then storing the concentrate for further use. [6] A method for recovering ammonia from vanadium processing for ammonium treatment and wastewater reuse according to claim 1, wherein the synthesizing step is: adding ammonium chloride (NH4Cl), ammonium sulfate ((NH4)2SO4) or ammonium nitrate (NH4NO3) to the processed concentrate according to different vanadium contents and stirring and synthesizing to obtain the ammonium metavanadate (NH4VO3). [7] A method for recovering ammonia from vanadium processing for ammonium treatment and wastewater reuse according to claim 4, wherein the vanadyl sulfate concentrate obtained by acid leaching and back extraction with a strong acid in the leaching step is heated to 60 to 90 °C and neutralized to a pH of 4 to 5 using liquid ammonium, thereby obtaining the ammonium polyvanadate ((NH4)2V6O 16 ) is obtained.

Citation Information

Patent Citations

  • Preparation method of high-purity vanadium pentoxide

    CN106430307A

  • Converting agent for extracting vanadium from raw vanadium ores and using method of converting agent

    CN108034807A

  • Recovery of vanadium values

    US4061711A

  • CN000106430307A