Anode material for lithium-ion batteries based on carbon aerogel composites

A carbon-airgel composite anode for lithium-ion batteries, using purified recycled activated carbon, addresses the scarcity and environmental issues of traditional materials, achieving enhanced performance and sustainability.

DE102023112318A1Pending Publication Date: 2024-11-14DEUTSCHES ZENTRUM FÜR LUFT UND RAUMFAHRT E V
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
DE102023112318
Authority / Receiving Office
DE · DE
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-14

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The invention relates to an anode material for lithium-ion batteries based on carbon aerogel composites.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to an anode material for lithium-ion batteries based on carbon aerogel composites.

[0002] The production of lithium-ion batteries (LIBs) is an energy-intensive process that requires large quantities of raw materials. Many of the materials, such as graphite, cobalt, and lithium, are unavailable in Germany and Europe. The use of secondary raw materials is therefore a key aspect in the development of battery components. Graphite is often used as an anode material in the current state of the art. Both the production of synthetic graphite and the extraction and purification of natural graphite negatively impact the carbon footprint of batteries. This could be partially reduced by using alternative raw materials.

[0003] Excellent cycling stability has already been achieved in LIBs using anodes made from biomass such as coffee husks, banana fibers, rice straw, or wheat straw. The porous nanostructure plays a crucial role in this process, providing a large electrode-electrolyte interface for the charge-transfer reaction.

[0004] WO 2020 / 020810 A1 describes a filler containing recycled activated carbon (recovered carbon black; rCB) with an iodine value measured according to ASTM D-1510-17 in the range of 9 g / kg to 160 g / kg. A composite of rubber and the aforementioned carbon black is described. The composite is described in particular as a tire, for example, a vehicle tire.

[0005] Sebastiäo MR Costa, David Fowler, Germano A. Carreira, Inês Portugal, and Carlos M. Silva (Production and Upgrading of Recovered Carbon Black from the Pyrolysis of End-of-Life Tires) Materials 2022, 15, 2030. https: / / doi.org / 10.3390 / ma15062030 describe that growing awareness of fossil fuel dependence, waste recycling, and greenhouse gas emissions in recent decades has led to the development of new solutions for numerous markets. The tire industry is no exception. With more than 1.5 billion tires produced worldwide annually, environmental concerns regarding their recycling or disposal at the end of their lifespan are raised.Pyrolysis enables the recovery of both energy and material from waste tires, yielding valuable gaseous, liquid, and solid fractions. The latter, known as recycled carbon black (rCB), has been intensively researched in recent years to ensure its quality for market applications. These studies have shown that the quality of rCB depends on the composition of the feedstock and the pyrolysis conditions, such as reactor type, temperature range, heating rate, and residence time. Recent developments in activation and demineralization techniques aim to produce rCB with specific chemical, physical, and morphological properties for specific applications. The automotive industry, the largest consumer of carbon black, has set specific targets for using recycled materials (such as rCB) according to the principles of sustainability and the circular economy.This review summarizes the pyrolysis of waste tires for the production of syngas, oil, and rCB, focusing on process conditions, product yield, and composition. A further analysis of the solid properties, including their impact on the use of rCB as a replacement for commercial CB in the tire industry, and purification and modification post-treatment processes for rCB upgrading are also investigated.

[0006] Somi Doja, Lava Kumar Pillari and Lukas Bichler, Renewable and Sustainable Energy Reviews 155 (2022) 111860; Processing and activation of tire-derived char: A review; describe, among other things, the demineralization of soot with acid before or after activation.

[0007] Recycled activated carbon (RCB) within the meaning of the present invention is obtainable, for example, by a process described in WO 2013 / 095145A1 and the prior art cited therein. The recycled activated carbon consists of approximately 99.4 wt.% carbon, 0.1 wt.% silicon, and 0.5 wt.% sulfur. The electrical conductivity of the carbon black is Fig. 1. The specific surface area determined by nitrogen physisorption is 67 m 2 / g, the mesopore volume is 0.4 cm 3 / g. The pore size distribution (BJH method) is in the Fig. 2. The average pore size is 50-70 nm.

[0008] Carbon aerogels are excellent candidates for anode materials due to their high surface area, pore volume, and tunable porosity and pore size. They demonstrate superior performance compared to graphite. Carbon aerogels can be produced from various starting materials such as lignin, cellulose, chitin, chitosan, and precursors such as resorcinol-formaldehyde, melamine-formaldehyde, and other organic aerogels.

[0009] DLR Magazine, 2020, 164, pp. 30-31, generally describes the use of tire waste, particularly soot in the form of recycled activated carbon for anode material for LIBs. Used tires are processed through a thermal process (pyrolysis) under the exclusion of oxygen. The organic compounds in the used tires are first broken down. The gases generated during the process are condensed, producing so-called TPO (Tire Pyrolysis Oil). The oil produced is used, for example, to generate energy for industrial processes or further processed in refineries. At the end of the process, a carbon-containing valuable material remains – the so-called crude recovered carbon black (see also WO 2013 / 095145A1).

[0010] In addition to carbon black, this valuable material also contains up to 25% ash, which consists of additives used in tire production. These are primarily silicate compounds and zinc components.

[0011] The object of the present invention is to produce anode material for lithium-ion batteries with increased cycle stability and to optimize the energy density of the lithium-ion batteries, in particular to improve their service life and CO2 footprint.

[0012] This object is achieved in a first embodiment by an anode material for a lithium-ion battery comprising a carbon aerogel composite of aerogel and recycled activated carbon, characterized in that the recycled activated carbon is substantially free of ash, silicate compounds and zinc components.

[0013] The invention thus relates to a conductive composite material which, in addition to a conventional binder, contains a carbon aerogel and recycled activated carbon (rcB) and can be used as anode material in lithium-ion batteries.

[0014] The aforementioned object was achieved in particular by combining a carbon aerogel with processed soot from scrap tires. It is particularly important that the soot contains essentially no ash, silicate compounds, or zinc components. These reduce the conductivity of a corresponding aerogel-soot composite material. The combination according to the invention leads to a significant improvement in the specific capacitance. The removal of ash, silicate compounds, and zinc compounds is achieved by conventional methods, for example, by treating the soot with sulfuric acid.

[0015] Particularly preferred within the meaning of the present invention is an anode material characterized by containing 1 to 50 wt.%, in particular 2 to 6 wt.%, of recycled activated carbon based on the amount of aerogel. If the proportion is too low, the recycled activated carbon is not homogeneously distributed throughout the aerogel, and the advantages of the material are not apparent. Higher proportions (>6 wt.%) were not investigated; presumably, activated carbon with a low specific surface area will reduce the total surface area of ​​the composite and thus potentially negatively impact the capacity.

[0016] A further embodiment of the invention consists in a process for producing the anode material defined above, which is characterized in that (a) adding the recycled activated carbon to the sol-gel solution during the synthesis of an aerogel or (b) the recycled activated carbon is mixed with an aerogel and (c) the carbonization is carried out according to known methods.

[0017] Particularly preferably, within the meaning of the present invention, the process is realized by using an aerogel based on organic or biopolymer-based starting material. Biomass, in particular from coffee hulls, banana fibers, rice or wheat straw, as the starting material for producing the aerogels.

[0018] Table 1 shows the specific discharge capacities of the pure materials based on laboratory cells, as well as the composite materials after 1, 5, and 100 cycles. The cells were discharged at 0.5C. It can be seen that the pure materials (carbon aerogel and recovered carbon black) exhibit very low capacities after 100 cycles. By combining both materials, specific discharge capacities of up to 1560 mAh g can be achieved. -1after 100 cycles. The capacity that can be drawn from a battery depends on the discharge method, i.e., the discharge current, the battery's final discharge voltage (the voltage at which discharge ends), and, of course, the state of charge. Various discharge methods are common, including: constant current discharge, constant resistance discharge, or constant power discharge. Depending on the discharge method, the battery's capacity varies. Therefore, it is useful to specify both the discharge current and the final discharge voltage in a meaningful nominal capacity specification.

[0019] The addition of recycled activated carbon (rCB) to the aerogel leads to an increase in electrical conductivity and a significant increase in capacity.

[0020] An anode material based on organic or biopolymer-based carbon aerogels in combination with purified soot obtained from used tires (recovered carbon black rCB) represents an alternative. This material combination not only leads to high-performance LIBs but also to a significant reduction in raw material dependence and increased sustainability. Table 1: Specific discharge capacities of carbon aerogel, recovered carbon black and carbon aerogel composites: Specific discharge capacity [mAh g -1 ] 1 cycle 5 cycles 100 cycles Carbon aerogel 12 10 79 Recovered carbon black (rCB) 235 157 115 2 wt% rCB (S) 532 130 146 2 wt% rCB (M) 533 205 194 4 wt% rCB (S) 486 176 193 4 wt% rCB (M) 3750 1647 1464 6 wt% rCB (S) 312 163 148 6 wt% rCB (M) 3664 1788 1561

[0021] The discharge capacity is determined by cycling the cell (charge-discharge cycles). Example:

[0022] Production of carbon aerogel composites Production of the composites

[0023] The composites were: 1.) directly during the synthesis of the aerogels (S) and 2.) subsequently produced by grinding (M).

[0024] The aerogels were synthesized according to a known method (Muehlemann SE, Huber L, Zhao S, Matam SK, Koebel MM (2018) Facile synthesis of resorcinolmelamine-formaldehyde based carbon xerogel. Materials Today: Proceedings 5: 13776. DOI: https: / / doi.org / 10.1016 / j.matpr.2018.02.018).

[0025] 1.) 2 wt.%, 4 wt.% and 6 wt.% of the additive recovered carbon black (rCB) were added to the sol solution (Costa SMR, Fowler D, Carreira GA, Portugal I, Silva CM (2022) Production and Upgrading of Recovered Carbon Black from the Pyrolysis of End-of-Life Tires. Materials 15: 2030. This publication shows that the composition of the rCB can vary greatly depending on the pyrolysis temperature and pressure. In general, the carbon content is 76 to 90 wt.%, hydrogen 0.7 to 10 wt.%, nitrogen up to 2 wt.% and sulfur 2 to 4.5 wt.%).

[0026] 2) The organic aerogels were mixed with 2 wt%, 4 wt% and 6 wt% of the additive recovered carbon black (rCB) and milled in a commercially available vibratory mill at 30 Hz for 30 seconds. Carbonization

[0027] The aforementioned aerogel composites were carbonized in a nitrogen atmosphere at 800°C for 1 hour. They can be chemically or physically activated if necessary. Activation could be carried out using a gas (CO2) or steam. Chemical treatments with alkalis (KOH) or acids (HNO3) can also lead to surface activation. Electrode production • Binder solution ◯ The PVDF binder (polyvinylidene fluoride) was dissolved in the solvent NMP (N-methyl-2-pyrrolidone). Sufficient solvent was added until a viscous (η~ 1.7 mPa s) paste was formed. The binder content was typically up to 10 wt.%. • Suspension ◯ The binder solution was added to the carbon aerogel composite in a mass ratio of 1:9 and mixed in a mortar for one hour. • Coating ◯ The suspension was applied to a commercially available copper foil using the doctor blade method and dried for approximately 12 hours at 60°C. The electrodes were then punched out with a diameter of 12 mm. Battery cell construction • Electrodes and electrolyte The button cell assembly in the half-cell configuration was carried out under an argon atmosphere. Pure lithium was used as the cathode, and 80 µL of LiPF6 (lithium hexafluorophosphate) was used as the electrolyte. The button cell was compressed using a hydraulic press at 50 kg / cm³. The aerogel composite electrode was tested against pure lithium in a half-cell configuration. LiPF6 (lithium hexafluorophosphate) was used as the electrolyte. characterization

[0028] In Fig. Figure 3 shows the discharge capacity curve of the carbon aerogel composites. The half-cells exhibit a constant discharge capacity. Furthermore, it can be seen that the use of the composite material increases the discharge capacity to approximately 1500 mAh g. -1 could be increased. Fig. Figure 3 shows the discharge capacity of carbon aerogel composites over 35 cycles. QUOTES CONTAINED IN THE DESCRIPTION

[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature

[0000] WO 2020 / 020810 A1

[0004] WO 2013 / 095145A1 [0007, 0009] Cited non-patent literature

[0000] Sebastiäo M. R. Costa, David Fowler, Germano A. Carreira, Inês Portugal, and Carlos M. Silva (Production and Upgrading of Recovered Carbon Black from the Pyrolysis of End-of-Life Tires) Materials 2022, 15, 2030. https: / / doi.org / 10.3390 / ma15062030

[0005] Somi Doja, Lava Kumar Pillari und Lukas Bichler, Renewable and Sustainable Energy Reviews 155 (2022) 111860

[0006] DLR-Magazin, 2020, 164, S. 30-31

[0009] Muehlemann SE, Huber L, Zhao S, Matam SK, Koebel MM (2018) Facile synthesis of resorcinolmelamine-formaldehyde based carbon xerogel. Materials Today: Proceedings 5: 13776. DOI: https: / / doi.org / 10.1016 / j.matpr.2018.02.018

[0024] Costa SMR, Fowler D, Carreira GA, Portugal I, Silva CM (2022) Production and Upgrading of Recovered Carbon Black from the Pyrolysis of End-of-Life Tires. Materials 15: 2030

[0025]

Claims

[1] Anode material for a lithium-ion battery comprising a carbon aerogel composite of aerogel and recycled activated carbon, characterized by that the activated carbon is free of ash, silicate compounds and zinc components. [2] Anode material according to claim 1, characterized by that it contains 1 to 50 wt.% of activated carbon based on the amount of aerogel. [3] A process for producing anode material according to claim 1, characterized by that one (a) adding the activated carbon to the sol-gel solution during the synthesis of an aerogel or (b) the activated carbon is mixed with an aerogel and (c) carries out the carbonisation by methods known per se. [4] Method according to claim 3, characterized by that an aerogel of organic origin or a biopolymer-based starting material is used. [5] Method according to claim 3 or 4, characterized bythat biomass, in particular coffee husks, banana fibers, rice or wheat straw, is used as starting material for the production of aerogels. [6] Method according to claim 3 or 4, characterized by that lignin, cellulose, chitin and / or chitosan are used as starting materials for the production of the aerogels.

Citation Information

Patent Citations

  • A method for obtaining a carbon black powder by pyrolyzing scrap rubber, the carbon black thus obtained and the use thereof

    WO2013095145A1

  • Recovered carbon black and composite material comprising said recovered carbon black

    WO2020020810A1