SIC epitaxy wafer and method for its production

By controlling the thickness and surface roughness of SiC epitaxial wafers through optimized CVD conditions, the formation of triangular defects is minimized, enhancing device yield and reliability in high breakdown voltage devices.

DE112018002540B4Active Publication Date: 2024-12-05MITSUBISHI ELECTRIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE112018002540
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-05-17
Filing Date
2018-01-18
Publication Date
2024-12-05
Estimated Expiration
2038-01-18

AI Technical Summary

Technical Problem

The formation of triangular defects in SiC epitaxial wafers, particularly in high breakdown voltage devices, significantly reduces device yield due to non-uniformity in the epitaxial layer thickness and surface roughness, which affects electrical properties and reliability.

Method used

The SiC epitaxial wafer is produced with a controlled layer thickness of 18 μm to 350 μm and an arithmetic mean roughness value of 0.60 to 3.00 nm, using specific CVD conditions of 3 kPa to 12 kPa pressure, 1.0 to 1.5 C/Si ratio, and 1500 °C to 1750 °C growth temperature, reducing triangular defects and improving surface uniformity.

Benefits of technology

This approach enhances device yield by minimizing triangular defects and ensuring uniform surface roughness, thereby improving the reliability and performance of SiC epitaxial wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

SiC epitaxy wafers (11, 12, 13, 14) with a SiC epitaxy layer (2), wherein the SiC epitaxic layer (2) has a layer thickness of 18 µm to 350 µm and an arithmetic mean roughness of 0.80 nm to 3.00 nm, and where the dopant concentration is 1×10 14 / cm 3 up to 5×10 15 / cm 3 amounts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to a technology for increasing the device yield of SiC epitaxial wafers. Relevant state of the art

[0002] Silicon carbide (SiC) has a wider band gap than silicon (Si) and possesses excellent physical properties, such as electric field strength versus dielectric breakdown, saturated electron velocity, and thermal conductivity, as well as excellent properties as a material for semiconductor power devices. In particular, a power device using SiC can achieve a size reduction and a significant reduction in power loss, and energy savings can be realized at the time of energy conversion of the power source.

[0003] A power device using SiC (hereinafter referred to as a "SiC power device") thus contributes to improvements in electric vehicles and enhancements in solar cell systems, so that such a SiC power device has potential as a first-class device for realizing a low-carbon or low-carbon society.

[0004] To manufacture a SiC power device, a drift layer of a semiconductor device must be formed in advance on a SiC substrate. The drift layer is laboriously formed by precisely controlling the layer thickness and carrier concentration using a chemical vapor deposition (CVD) method or the like. Furthermore, the drift layer is formed by epitaxial growth on the substrate because the layer thickness and carrier concentration of the drift layer are essentially defined by the device design specifications, and furthermore, the carrier concentration of the drift layer must be controlled even more precisely than on the substrate.

[0005] Hereinafter, a wafer in which an epitaxial growth layer is formed on a SiC substrate is referred to as an epitaxial wafer. A SiC power device is fabricated by subjecting an epitaxial wafer to various processes. The proportion of devices with the desired properties among the devices fabricated from a wafer, i.e., the device yield, is highly dependent on the uniformity of the electrical properties of the epitaxial growth layer.

[0006] Thus, if there is a local region in the plane of the epitaxial wafer where the electric field against dielectric breakdown is weaker than in other regions, or where a relatively high current flows when a constant voltage is applied, the electrical properties of a device with such a region are considered to be inferior. For example, a low breakdown voltage characteristic will result in leakage current even when the applied voltage is relatively low.

[0007] In other words, the primary factor determining device yield is the crystal uniformity of the epitaxial wafer. One factor that hinders the crystal uniformity of the epitaxial wafer is the presence of device-killer defects, such as triangular defects observed on the surface of the epitaxial wafer or debris due to a defect at the time of epitaxial growth.

[0008] To improve device yield, some methods for obtaining high-quality epitaxial SiC layers have been proposed.

[0009] For example, JP 5 353 800 B2 describes a technique for forming a high-quality SiC epitaxial layer in which, by specifying one condition of pressure and substrate temperature, the other condition is alternated between a high-specified condition and a lower-specified condition during layer formation.

[0010] Furthermore, JP 2005-109408 A describes a technique in which a vertical hot-wall CVD epitaxial growth apparatus uses a susceptor that prevents peeling or cracking of a coating material on the surface of the susceptor. Such a vertical hot-wall CVD epitaxial growth apparatus can form a flat, high-purity SiC epitaxial growth layer at high speed.

[0011] Furthermore, the publication SAMESHIMA, J. [et al.]: Relation between defects on 4H-SiC epitaxial surface and gate oxide reliability. In: Materials Science Forum, Vol. 740-742, 2013, pp. 745-748 describes that fabricating a device using an epitaxial growth layer with step bundling results in non-uniformity of the gate oxide layer, which adversely affects its reliability.

[0012] From document DE 11 2014 004 068 T5, a silicon carbide epitaxial substrate with a main surface is known, which comprises a carrier substrate and a silicon carbide epitaxial layer formed on the carrier substrate and having the main surface. The main surface has a surface roughness of 0.6 nm or less. Furthermore, a ratio of the standard deviation of a nitrogen concentration in the silicon carbide epitaxial layer on a surface layer having the main surface within a plane of the silicon carbide epitaxial substrate to a mean value of the nitrogen concentration in the silicon carbide epitaxial layer on the surface layer within the plane of the silicon carbide epitaxial substrate is 15% or less.

[0013] From document US 2016 / 0 181 375 A1, a silicon carbide semiconductor substrate is known, comprising: a base substrate having a main surface with an outer diameter of not less than 100 mm and made of single-crystal silicon carbide; and an epitaxial layer formed on the main surface. The silicon carbide semiconductor substrate has a deformation amount of not less than -100 µm and not more than 100 µm when the substrate temperature is room temperature, and has a deformation amount of not less than -1.5 mm and not more than 1.5 mm when the substrate temperature is 400°C. Short descriptionProblem to be solved with the invention

[0014] One of the device-killer defects that reduces device yield is a triangular defect. It is generally known that the primary cause of triangular defects is tiny SiC grains adhering to a front surface of the substrate before and during the formation of the epitaxial growth layer. However, there are also unique triangular defects that have causes other than these. These unique triangular defects manifest themselves as a thicker epitaxial layer when the epitaxial layer is grown under general growth conditions.

[0015] In a device using an epitaxial layer with a layer thickness of several tens of µm or more, such as a high breakdown voltage device, particularly one having a breakdown voltage of 3.3 kV or more, the unique triangle defect may be a definite cause of the reduction in device yield.

[0016] The present invention has been made to solve the above-described problems, and the object of the present invention is to increase the device yield in a SiC epitaxial wafer. Means to solve the problems

[0017] The object is achieved by a SiC epitaxial wafer having the features of claim 1. Advantageous further developments arise from subclaims 2 to 4. Furthermore, the object is achieved by a method for producing a SiC epitaxial wafer having the features of claim 5. An advantageous further development of the method arises from subclaim 6. Effects of the invention

[0018] A SiC epitaxial wafer according to the present invention comprises a SiC epitaxial layer. The SiC epitaxial layer has a layer thickness of 18 µm to 350 µm and an arithmetic mean roughness of 0.60 to 3.00 nm. This improves device yield.

[0019] A method for manufacturing a SiC epitaxial wafer according to the present invention comprises placing a SiC substrate in a reaction furnace of a CVD apparatus and forming a SiC epitaxial layer having a layer thickness of 18 µm to 350 µm on the SiC substrate.

[0020] The conditions for forming the SiC epitaxial layer are as follows: the pressure in the reaction furnace is 3 kPa to 12 kPa, the C / Si ratio of the material gas supplied to a reaction furnace is 1.0 to 1.5, and the growth temperature is 1500 °C to 1750 °C. In this way, a SiC epitaxial wafer with high device yield can be produced.

[0021] These and other objects, features, aspects and advantages of the present invention will become more apparent from the following detailed description of the present invention when taken in conjunction with the accompanying drawings. Brief description of the drawings

[0022] The drawings show: Fig. 1 is a graphical representation illustrating a relationship between a layer thickness of a SiC epitaxial layer and a generation frequency of triangular defects; Fig. 2 is a graph illustrating a correlation between the surface roughness of the SiC epitaxial layer and the number of triangular defects; Fig. 3 is a sectional view showing a configuration of a SiC epitaxial wafer according to Embodiment 1; Fig. 4 is a graphical representation for explaining the evaluation area dependence of a surface roughness value for the same wafer; Fig. 5 is a sectional view showing a configuration of a SiC epitaxial wafer according to Embodiment 2; Fig. 6 is a sectional view showing a configuration of a SiC epitaxial wafer according to Embodiment 3; Fig. 7 is a sectional view showing a configuration of a SiC epitaxial wafer according to Embodiment 4. Description of the embodiments

[0023] Embodiments of the present invention will now be described with reference to the accompanying drawings. In the following description, similar components are denoted by the same reference numerals, and their names and functions are the same. A detailed description thereof is therefore omitted. A. Embodiment 1A-1. Configuration

[0024] As described above, there are device-killer defects in a SiC epitaxial layer, which are referred to as triangular defects. It is known that the main cause of triangular defects is tiny SiC grains adhering to a front surface of the substrate before and during the formation of the SiC epitaxial growth layer. However, there are also distinct triangular defects that occur due to causes other than these. Such a distinct triangular defect manifests itself as a thicker formation of the SiC epitaxial layer when the growth of the SiC epitaxial layer takes place under general growth conditions, as shown in Fig. 1 is illustrated.

[0025] Fig. Figure 1 shows a graph illustrating the relationship between the thickness of the SiC epitaxial layer and the frequency of triangular defects. The SiC epitaxial layer is coated with a nitrogen dopant at a concentration of approximately 1×10 15 / cm 3 According to Fig. 1 shows that when the SiC epitaxial layer reaches a thickness of 18 µm or more, the frequency of triangular defects increases significantly.

[0026] Thus, in a case where the SiC epitaxial layer has a layer thickness of several tens of µm or more, such as in particular a high breakdown voltage device having a breakdown voltage of 3.3 kV or more, the frequent generation of the triangular defects is the definite cause for the reduction of the device yield.

[0027] The inventors conducted extensive studies on triangular defects that cause yield reduction in high breakdown voltage devices with SiC epitaxial layers with a thickness of 18 µm or more. As a result, the inventors found a clear correlation between the surface roughness of the SiC epitaxial layer and the number of triangular defects.

[0028] Fig. Figure 2 shows a graph illustrating the correlation between the surface roughness of the SiC epitaxial layer and the occurrence frequency of triangular defects. The vertical axis of the graph represents the number of triangular defects per wafer [pieces / Wf] observed on the front surface of the SiC epitaxial layer when the SiC epitaxial layer is formed with a layer thickness of 18 μm or more on a 4-inch SiC substrate. The horizontal axis of the graph represents the entire surface average of the arithmetic mean roughness (Ra) (hereinafter referred to simply as the "entire front surface of the SiC epitaxial layer") of the SiC epitaxial layer in the wafer.

[0029] As per Fig. As can be seen from Figure 2, with the increase in the average arithmetic mean roughness (Ra) of the SiC epitaxial layer over the entire surface, the number of triangular defects decreases significantly. In particular, when the arithmetic mean roughness (Ra) is 1.0 nm or more, the number of defects is approximately 0 pcs / Wf. It is considered that the reason for this is that with the increase in the surface roughness of the epitaxial layer, a surface warp increases in size, the microscopic dislocation angle changes at the front surface, and the terrace width decreases, so that two-dimensional nucleus growth at the front surface is suppressed. The terrace is an atomically smooth surface between adjacent steps on the front surface of the SiC epitaxial layer.

[0030] As further provided for in Fig. As can be seen from Figure 2, as the average arithmetic mean roughness (Ra) of the SiC epitaxial layer over the entire surface further increases, the number of triangular defects increases significantly. This is because the atomic arrangement in the SiC epitaxial layer is disturbed. To increase the device yield of a 4-inch SiC epitaxial wafer, the number of triangular defects must be 10 pcs / Wf or less. Therefore, it is desirable that the average arithmetic mean roughness (Ra) of the SiC epitaxial layer over the entire surface be 0.60 nm to 3.00 nm.

[0031] In this specification, the term "the entire surface of the SiC epitaxial layer in the wafer" does not refer to the entire surface of the SiC epitaxial layer in the small piece obtained by dicing the wafer. This term refers to an area excluding 5 mm from the wafer edge in the entire growth surface of the SiC epitaxial layer in the SiC epitaxial wafer with a diameter of 100 mm or more. The area of ​​the entire surface of the SiC epitaxial layer in a wafer with a diameter of 100 mm or more is 63.5 cm. 2 or more.

[0032] The diameter of the SiC epitaxial wafer may be 150 mm or 200 mm, in each case, “the entire surface of the SiC epitaxial layer in the wafer” means the area excluding 5 mm from the wafer edge in the entire growth surface of the epitaxial layer in the SiC epitaxial wafer.

[0033] Fig. 3 is a cross-sectional view illustrating a configuration of a SiC epitaxial wafer 11 according to Embodiment 1. The SiC epitaxial wafer 11 includes a SiC substrate 1 and a drift layer 2. The drift layer 2 is formed on the upper surface of the SiC substrate 1; in other words, the SiC substrate 1 is formed on the lower surface of the drift layer 2. The SiC substrate 1 is obtained, for example, by dividing an ingot grown by a sublimation method and subjecting it to a mirror-polishing process. The drift layer 2 is formed by epitaxial growth on the SiC substrate 1. That is, the drift layer 2 constitutes the SiC epitaxial layer.

[0034] When the SiC epitaxial layer thickness is set to 18 µm or more, triangular defects are generally generated on the surface at a frequency of 20 [pieces / Wf] or more due to the two-dimensional nucleus growth described above, which has an adverse impact on the device. Therefore, reducing these defects is essential. According to Fig. 2, by specifying the arithmetic mean roughness (Ra) of the SiC epitaxial layer over the entire surface to a value of 0.60 nm to 3.00 nm, a reduction in the number of triangular defects to 10 pieces / Wf or less is ensured, thus increasing device yield. Therefore, the average arithmetic mean roughness (Ra) of the drift layer over the entire surface is specified to a value of 0.60 nm to 3.00 nm.

[0035] In Embodiment 1, the surface roughness of the SiC epitaxial layer is evaluated over the entire surface of the SiC epitaxial layer on the wafer. The evaluation aims to reduce triangular defects on the entire surface of the SiC epitaxial layer and improve yield, and for this reason, the surface roughness evaluation range is expanded as much as possible. In contrast, in JP 2005-109408 A, the surface roughness evaluation range is an area of ​​10 µm. 2 .

[0036] Fig. Figure 4 shows a graphical representation explaining the evaluation area dependence of a surface roughness value in the same wafer. For example, if the evaluation area is the entire surface (approx. 63.5 cm 2) for the SiC epitaxial wafer with a diameter of 100 mm, the arithmetic mean roughness Ra = 0.60 nm. However, if the evaluation area is an area of ​​10 µm 2 (0.000001 cm 2 ), the arithmetic mean roughness Ra = 0.19 nm. As can be seen from Fig. As can be seen in Figure 4, the surface roughness evaluation results for the same wafer vary significantly depending on the evaluation area. Therefore, two surface roughness values ​​that refer to different evaluation areas cannot be treated as equal.

[0037] Furthermore, in the epitaxial layer having a square-average surface roughness of 1.60 nm, as disclosed in JP 2005-109408 A, step bundling occurs; therefore, a reduction in device yield is unavoidable. In contrast, in Embodiment 1, the drift layer 2 forming the SiC epitaxial layer is formed such that the total area average of the arithmetic mean roughness (Ra) has a value of 0.60 nm to 3.00 nm. Thus, no significant unevenness such as step bundling is observed in the SiC epitaxial layer, and the entire surface has a uniform surface roughness, which has no adverse effect on the reliability of the oxide layer at the time of device fabrication. Although it has been mentioned above that the SiC epitaxial layer is approximately 1×10 15 / cm 3of a nitrogen dopant, however, the permissible concentration of the nitrogen dopant for the SiC epitaxial layer is in a range of 1×10 14 / cm 3 up to 5×10 ı5 / cm 3 .

[0038] Furthermore, in Embodiment 1, nitrogen (N) has been described as the doping material, but phosphorus (P), arsenic (As), antimony (Sb), aluminum (Al), boron (B), gallium (Ga), indium (In) or the like can also be used as the doping material.

[0039] In Embodiment 1, the evaluation area for the arithmetic mean roughness (Ra) of the SiC epitaxial layer has been described as the entire front surface, but for a larger wafer, the evaluation area of ​​the arithmetic mean roughness (Ra) may not necessarily be the entire surface, and an area of ​​63.5 cm 2 or more may be sufficient as an evaluation area. A-2. Manufacturing process

[0040] The manufacturing process of a SiC epitaxial wafer 11 is described below.

[0041] First, a SiC substrate 1 is provided. The SiC substrate 1 is an n-type 4H-SiC substrate doped with nitrogen as a dopant with an average concentration of 1×10 17 cm -3 up to 1×10 20 cm -3 The SiC substrate 1 has a thickness of 300 µm to 400 µm. The front surface of the SiC substrate 1 has an inclination angle of approximately 4° in the [11-20] direction relative to the (0001) plane.

[0042] Next, the SiC substrate 1 is placed in a reaction furnace of a CVD apparatus and heated to a desired heating temperature. Subsequently, hydrogen as the carrier gas, a cleaning gas for the front surface of the SiC substrate, monosilane and propane as the material gases, and nitrogen as the dopant gas are introduced, respectively. The pressure in the reaction furnace is controlled between 3 kPa and 12 kPa to initiate SiC epitaxial growth. The C / Si ratio of the supplied material gases is set to a value of 1.0 to 1.5, and the growth temperature is set to a value of 1500 °C to 1700 °C. The nitrogen flow rate is controlled such that the dopant concentration of the drift layer 2 has a value of 1×10 14 cm -3 up to 5×10 15 cm -3The layer is formed at a growth rate of 9 µm / h or more, and the drift layer 2 is formed with a thickness of 18 µm to 350 µm. It should be noted that the upper limit of the layer thickness of the drift layer 2 is 350 µm from the perspective of productivity and device specifications.

[0043] As a result of the evaluation of the SiC epitaxial wafer 11 formed under the above conditions by the photoluminescence topography method, the basal plane dislocation density (BPD density) is on average 1 piece / cm 2 or less over the entire surface of the wafer. The steps described above produce a SiC epitaxial wafer with very few triangular defects, which become noticeable when the SiC epitaxial layer is thickened, and with no local irregularities such as step bundling. A-3. Effect

[0044] The SiC epitaxial layer 11 of Embodiment 1 includes the drift layer 2, which is a SiC epitaxial layer. The drift layer 2 has a layer thickness of 18 μm to 350 μm. When the layer thickness of the SiC epitaxial layer is increased to 18 μm or more, the number of triangular defects generally increases. However, by setting the arithmetic mean roughness of the drift layer 2 in the wafer to a value of 0.60 nm to 3.00 nm, the number of triangular defects can be significantly reduced. Thus, the device yield is improved.

[0045] Furthermore, in the SiC epitaxial wafer 11, the dopant concentration of the drift layer 2, which is the SiC epitaxial layer, is 1×10 14 / cm 3 up to 5×10 15 / cm 3. Therefore, the average of the arithmetic mean roughness of the drift layer 2 in the wafer, considered over the entire surface, is specified with a value of 0.60 nm to 3.00 nm.

[0046] In the manufacturing method of a SiC epitaxial wafer 1 according to Embodiment 1, the SiC substrate 1 is placed in a reaction furnace of a CVD apparatus, and the drift layer 2, which is a SiC epitaxial layer with a film thickness of 18 μm to 350 μm, is formed on the SiC substrate 1. The conditions for forming the drift layer 2 are as follows: the pressure in the reaction furnace is 3 kPa to 12 kPa, the C / Si ratio of the material gas supplied to the reaction furnace is 1.0 to 1.5, and the growth temperature is 1500 °C to 1750 °C. In this way, the number of triangular defects in the drift layer 2 can be significantly reduced, and the device yield is improved. B. Embodiment 2

[0047] In the following description, the same components as in Embodiment 1 are denoted by the same reference numerals, and a detailed description thereof will be omitted if necessary. B-1. Configuration

[0048] Fig. 5 is a cross-sectional view illustrating a configuration of a SiC epitaxial wafer 12 according to Embodiment 2. The SiC epitaxial wafer 12 includes a SiC substrate 1, a medium concentration layer 3 formed on the SiC substrate 1, and a drift layer 2 formed on the medium concentration layer 3. While the drift layer 2 is formed directly on the SiC substrate 1 in the SiC epitaxial wafer 11 of Embodiment 1, the medium concentration layer 3 is formed between the SiC substrate 1 and the drift layer 2 in the SiC epitaxial wafer 12 of Embodiment 2.

[0049] Medium concentration layer 3 and drift layer 2 form the SiC epitaxial layers. The dopant concentration of medium concentration layer 3 is equal to or lower than the dopant concentration of SiC substrate 1 and equal to or higher than the dopant concentration of drift layer 2.

[0050] The conditions for forming medium-concentration layer 3 are as follows. For example, the C / Si ratio of the supplied material gases is set to a value of 1.0 to 1.5, and the growth temperature is set to a value of 1500°C to 1700°C. The nitrogen flow rate is controlled such that the dopant concentration reaches a value of 1×10 17 [cm -3 ] to 2×10 19 [cm -3 ] is achieved. The layer thickness of medium concentration layer 3 is 0.3 µm to 20 µm, and the growth rate is 1 µm / h or more. B-2. Effect

[0051] The SiC epitaxial wafer 12 according to Embodiment 2 has a medium-concentration layer 3 disposed between the SiC substrate 1 and the drift layer 2. With this configuration, lattice mismatch caused by the difference in dopant concentration between the SiC substrate 1 and the drift layer 2 can be mitigated, and crystal defects due to stress in the SiC epitaxial layer caused by the lattice mismatch can be reduced. This improves device yield more than the SiC epitaxial wafer 11 of Embodiment 1. C. Embodiment 3

[0052] Hereinafter, the same components as those described in Embodiments 1 and 2 are denoted by the same reference numerals, and a detailed description thereof will be omitted if necessary. C-1. Configuration

[0053] Fig. 6 is a sectional view showing a configuration of a SiC epitaxial wafer 13 according to Embodiment 3. The SiC epitaxial wafer 13 includes a SiC substrate 1, a medium concentration layer 3 formed on the SiC substrate 1, a concentration gradient layer 4 formed on the medium concentration layer 3, and a drift layer 2 formed on the concentration gradient layer 4. The SiC epitaxial wafer 13 has a configuration in which a concentration gradient layer 4 is added between the medium concentration layer 3 and the drift layer 2 in the SiC epitaxial wafer 12 of Embodiment 2.

[0054] The concentration gradient layer 4 is provided such that the dopant concentration is low on the lower side, ie the side adjacent to the intermediate concentration layer 3, and high on the upper side, ie the side adjacent to the drift layer 2, in such a way that the dopant concentration becomes continuously or gradually lower from the intermediate concentration layer 3 to the drift layer 2.

[0055] Concentration gradient layer 4, intermediate concentration layer 3, and drift layer 2 constitute the SiC epitaxial layers. The conditions for forming concentration gradient layer 4 are as follows. For example, the C / Si ratio of the supplied material gases is set to a value of 1.0 to 1.5, and the growth temperature is set to a temperature of 1500°C to 1700°C. The nitrogen flow rate is controlled so that the dopant concentration of concentration gradient layer 4 has the concentration distribution described above. C-2. Effect

[0056] The SiC epitaxial wafer 13 according to Embodiment 3 has the concentration gradient layer 4 disposed between the intermediate concentration layer 3 and the drift layer 2. This can reduce crystal defects due to lattice mismatch caused by the difference in dopant concentration between the intermediate concentration layer 3 and the drift layer 2. This further improves the device yield compared to the SiC epitaxial wafer 12 according to Embodiment 2. D. Embodiment 4

[0057] In the following, the same components as in Embodiments 1 to 3 are denoted by the same reference numerals, and a detailed description thereof will be omitted if necessary. D-1. Configuration

[0058] Fig.7 shows a sectional view illustrating a configuration of a SiC epitaxial wafer 14 according to Embodiment 4. The SiC epitaxial wafer 14 has a SiC epitaxial layer 5. The SiC epitaxial wafer 14 is formed by removing the SiC substrate 1 from the SiC epitaxial wafer 1 according to Embodiment 1. That is, the SiC epitaxial layer 5 corresponds to the drift layer 2 in the SiC epitaxial wafer 11 of Embodiment 1.

[0059] By removing the SiC substrate 1, it is possible to use the SiC epitaxial layer 5 not as a drift layer according to Embodiment 1, but as a SiC substrate. The layer thickness of the SiC epitaxial layer 5 is desirably 100 µm or more. D-2. Effect

[0060] The method for manufacturing the SiC epitaxial wafer 14 according to Embodiment 4 forms the SiC epitaxial layer 5 with a layer thickness of 18 μm to 350 μm and removes the SiC substrate 1 after forming the SiC epitaxial layer 5. Then, by using the SiC epitaxial layer 5 as the SiC substrate, the SiC epitaxial layer with remarkably high quality can be formed on the SiC epitaxial layer 5. Thus, device killer defects can be reduced and device yield can be increased.

[0061] In the embodiments described above, the material qualities, materials, dimensions, shapes, relative arrangement relationships, or execution conditions of the respective components may be described in some cases. However, the above description is for illustrative purposes only and is not intended to limit the description of the present invention. Therefore, it is understood that numerous other modifications and changes (including any changes or omissions of optional components, as well as free combinations between different embodiments) can be made without departing from the scope of the invention. List of reference symbols 1 SiC substrate 2 Drift layer 3 layer with medium concentration 4 layer with concentration gradient 11 SiC epitaxial wafers 12 SiC epitaxial wafers 13 SiC epitaxial wafers 14 SiC-Epitaxiewafer

Claims

[1] SiC epitaxial wafer (11, 12, 13, 14) with a SiC epitaxial layer (2), wherein the SiC epitaxial layer (2) has a layer thickness of 18 µm to 350 µm and an arithmetic mean roughness of 0.80 nm to 3.00 nm, and where the dopant concentration is 1×10 14 / cm 3 up to 5×10 15 / cm 3 amounts. [2] The SiC epitaxial wafer (11, 12, 13, 14) according to claim 1, wherein an evaluation range of the arithmetic mean value of the roughness of the SiC epitaxial layer (2) is the entire surface of the SiC epitaxial layer (2). [3] SiC epitaxial wafer (11, 12, 13, 14) according to claim 1 or 2, wherein the dopant is nitrogen. [4] The SiC epitaxial wafer (11, 12, 13, 14) according to any one of claims 1 to 3, further comprising a SiC substrate (1) formed on a lower surface of the SiC epitaxial layer (2). [5] Method for producing a SiC epitaxial wafer (11, 12, 13, 14) according to one of claims 1 to 4, the method comprising the following steps: - placing a SiC substrate (1) in a reaction furnace of a CVD device; and - forming a SiC epitaxial layer (2) with a layer thickness of 18 µm to 350 µm on the SiC substrate (1), - wherein the conditions for forming the SiC epitaxial layer (2) are as follows: the pressure in the reaction furnace is 3 kPa to 12 kPa, the C / Si ratio of the material gas supplied to a reaction furnace is 1.0 to 1.5, and the growth temperature is 1500 °C to 1750 °C. [6] A method for producing a SiC epitaxial wafer (11, 12, 13, 14) according to claim 5, the method further comprising the step of: Removing the SiC substrate (1) after forming the SiC epitaxial layer (2).

Citation Information

Patent Citations

  • Compound neutral water treating valve

    JP1998009408A

  • Method for manufacturing silicon carbide epitaxial films

    JP5353800B2

  • Silicon carbide epitaxial substrate, method for manufacturing a silicon carbide epitaxial substrate, method for manufacturing a silicon carbide semiconductor device, silicon carbide growth device, and silicon carbide growth device element

    DE112014004068T5

  • Silicon carbide semiconductor substrate, method for manufacturing silicon carbide semiconductor substrate, and method for manufacturing silicon carbide semiconductor device

    US20160181375A1

  • JP200S