INSULATED WIRE WITH ADHESIVE COATING

The insulated wire with an adhesive layer of modified polyolefin and polyester resin/elastomer addresses adhesion issues by ensuring strong bonding between the insulating jacket and adhesive layers, enhancing stability and adhesion to backing parts.

DE112019006404B4Active Publication Date: 2024-10-02AUTONETWORKS TECH LTD +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE112019006404
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-25
Filing Date
2019-12-05
Publication Date
2024-10-02
Estimated Expiration
2039-12-05

AI Technical Summary

Technical Problem

Insulated wires with adhesive layers face adhesion issues between the insulating jacket layer and the adhesive layer, particularly when polyvinyl chloride is used, leading to detachment and reduced adhesion when loads are applied.

Method used

The insulated wire features an adhesive layer composed of modified polyolefin and one or more materials selected from a polyester resin and a polyester elastomer, ensuring excellent adhesion to both the insulating jacket layer and the adhesive backing part, even if the jacket layer contains polyvinyl chloride.

Benefits of technology

The solution provides enhanced adhesion between the insulating jacket layer and the adhesive layer, distributing loads evenly and preventing detachment, thereby maintaining the wire's stability and adhesion to the adhesive backing part.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Insulated wire (1, 11) with an adhesive layer, comprising: a conductor (2); an insulating sheath (3) covering an outer circumference of the conductor (2); and an adhesive layer (4) provided on an outer surface of the insulating sheath (3) for hot-melt bonding, wherein the adhesive layer (4) comprises: component A: a modified polyolefin; and component B: one or more materials selected from a polyester resin and a polyester elastomer, the adhesive layer (4) comprising 10 to 70 parts of component B per 100 parts of the total of components A and B, component A having a melting point between 80°C and 185°C, component B having a melting point between 80°C and 185°C and a tensile strength between 19 MPa and 50 MPa, measured according to JIS K7161, and the adhesive layer (4) having a softening point between 80°C and 170°C.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to an insulated wire having an adhesive layer, and more particularly to an insulated wire with adhesive layer, which has on the outside of an insulating coating covering a conductor an adhesive layer with thermal adhesive properties. TECHNICAL BACKGROUND

[0002] Vehicles, such as automobiles, and electrical and electronic devices use a large number insulated wires with a conductor and an insulating sheath covering the outer circumference of the conductor. In recent years, the number of insulated wires used has increased as automobiles and electrical and electronic devices are becoming increasingly powerful. Traditionally, such insulated wires used by attaching them to the body of a vehicle using small fastening parts such as clamps or clips. automobile, to the housing of a device or the like. Due to the increasing number of insulated Wires that are used, however, the space occupied by small fastening parts and the like increases, and the aim is to save space.

[0003] To address the above problem, the use of an insulated wire with a Adhesive layer on the outer circumference consisting of a modified polyolefin, as in JP 2002 - 237 219 A discloses that the insulated wire is directly attached to the body, housing or the like by means of the adhesive layer is attached without using any small fixing parts or the like, which is effective for saving space.

[0004] JP H10 - 149 725 A discloses a flame-retardant multilayer film and a flat cable comprising This one has excellent durability and electrical insulation. A flame-retardant, pressure-sensitive adhesive layer is formed on a film substrate made of a thermoplastic polyester resin (a), consisting of a thermoplastic polyolefin resin (b) with pressure-sensitive adhesive properties and a thermoplastic polyester resin (c) with pressure-sensitive adhesive properties. The above-mentioned substrate and / or the adhesive layer are protected by a Flame retardants have been used to make it flame-retardant. OVERVIEW OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0005] Conventionally, the material used for the insulating sheath covering the outer circumference of the conductor is A polyvinyl chloride composition is often used. The adhesive layer is thus applied to the outside of the insulating sheath layer of the insulated wire that it is in contact with the insulating sheath layer, there is However, there is a problem that polyvinyl chloride, which is often used for the insulating sheath, has a weak adhesiveness to the modified polyolefin forming the adhesive layer of JP 2002 - 237 219 A, so that it can detachment at the interface between the insulating sheath layer and the adhesive layer may occur. If the When the interface between the insulating coating layer and the adhesive layer peels off, a load is concentrated on the wire, on the adhesive layer on the outside, and the adhesive strength of the entire wire decreases.

[0006] Although it is less likely that detachment will occur at the interface between the insulating Sheath layer and the adhesive layer as described above, if the insulating sheath is not polyvinyl chloride The aim is to improve the adhesion between the adhesive layer and an adhesive carrier part in order to insulated wire with adhesive layer firmly attached to the adhesive carrier part, such as the body of an automobile, the housing a device or the like.

[0007] In view of the above-mentioned problem, the present disclosure has as its object to provide an isolated To provide a wire with an adhesive layer having as outer layer an adhesive layer which is applied to both an insulating It has excellent adhesion properties both on the sheath layer and on an adhesive carrier part. MEANS FOR SOLVING THE TASK

[0008] An insulated wire with adhesive layer of the present disclosure has the features of claim 1. EFFECT OF THE INVENTION

[0009] According to the insulated wire with adhesive layer of the present disclosure, the adhesive layer has both on the It has excellent adhesion properties both on the insulating sheath layer and on the adhesive carrier part. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a perspective view showing an external appearance of an insulated wire with adhesive layer according to the present disclosure. Fig. 2 is a sectional view along AA in Fig. 1. Fig. 3 is a sectional view showing the insulated wire with adhesive layer according to the present disclosure is glued to an adhesive carrier part. Fig. 4 is a sectional view showing two insulated wires with adhesive layer according to the present Revelation are bundled and glued. Fig. 5 is an illustration of a method for evaluating the adhesive strength of the insulated wire with Adhesive layer, where Fig. 5A shows a method for bonding an insulated wire with adhesive layer to a adhesive backing part and Fig. 5B shows a procedure of peeling test of the insulated wire with adhesive layer. ASPECTS OF THE INVENTION

[0010] First, aspects of the present disclosure are enumerated and described.

[0011] (1) An insulated wire with adhesive layer of the present disclosure comprises a conductor, an insulating Sheath layer covering an outer periphery of the conductor and an adhesive layer on an outer side of the insulating sheath layer and is used for hot-gluing, wherein the adhesive layer (A) is a modified Polyolefin and (B) one or more materials selected from a polyester resin and a Polyester elastomer, and the adhesive layer 10 to 70 parts of component (B) per 100 parts of the total of the Contains components (A) and (B).

[0012] According to the insulated wire with adhesive layer of the present disclosure, an adhesive layer with thermal adhesive properties comprising (A) a modified polyolefin and (B) one or more materials that selected from a polyester resin and a polyester elastomer, thereby enabling the insulated wire with adhesive layer is held firmly to an adhesive carrier part, even if the insulating sheath layer is polyvinyl chloride contains, since the adhesive strength between the insulating sheath layer and the adhesive layer is excellent, and also the adhesive strength between the adhesive carrier part and the adhesive layer is excellent.

[0013] If the adhesion between the insulating sheath layer and the adhesive layer is insufficient, detachment at the interface between the insulating sheath layer and the adhesive layer when a load is applied to the wire, and the load is concentrated on the adhesive layer, which is bonded directly to the adhesive carrier part. the adhesive layer is stretched and tears where the layer becomes thin, and the wire detaches from the adhesive carrier part. Wire with adhesive layer of the present disclosure has excellent adhesion between the insulating Sheath layer and the adhesive layer, the load is distributed over the entire wire without the adhesive layer stretched in certain places, making it less likely that the wire will come loose.

[0014] The insulating sheath layer may contain a polyvinyl chloride. Although previously commonly used Adhesive layers had poor adhesion to an insulating sheath layer containing polyvinyl chloride, The adhesive layer according to the present disclosure has excellent adhesion to an insulating Coating layer containing polyvinyl chloride, and the effect achieved by the present disclosure becomes apparent.

[0015] (3) The adhesive layer preferably contains (A) the modified polyolefin and (B) the polyester resin. If the component (B) Contains polyester resin, the adhesion to the insulating sheath layer is excellent.

[0016] (4) The adhesive layer preferably contains (A) the modified polyolefin and (B) the polyester elastomer. If the Component (B) contains polyester elastomer, the flexibility is excellent.

[0017] (5) The adhesive layer is preferably formed around an entire circumference in a circumferential direction on the outside of the insulating sheath layer. This is advantageous because the adhesive surface between the adhesive layer and of the insulating sheath layer. This is also advantageous because the adhesive layer is thus is circular, and thus even assuming that the adhesive layer and the insulating sheath detach from each other, the wire is held without immediately coming loose. DETAILED DESIGNS

[0018] Specific examples of an insulated wire with adhesive layer of the present disclosure are given below with reference to the drawings. It should be noted that the disclosure is not limited to these illustrative examples.

[0019] An insulated wire 1 with an adhesive layer comprises an insulated wire having a conductor 2 and an insulating Sheath layer 3 covering the outer circumference of the conductor 2, and further comprises on the outside thereof a Adhesive layer 4 containing (A) a modified polyolefin and (B) one or more materials selected from a polyester resin and a polyester elastomer. The adhesive layer 4 softens and bonds at a temperature that is lower than the heat-resistant temperature of the insulating sheath layer 3.

[0020] The adhesive layer 4 contains (A) a modified polyolefin. The component (A) forming the adhesive layer 4 is a Polyolefin into which functional groups have been introduced by using a base polyolefin derived from α-olefin as a monomer with a polymerizable monomer containing functional groups such as the carboxyl group, ester group and acid anhydride group, has been copolymerized or graft polymerized. Due to the insertion of these functional materials, the adhesion to the adhesive carrier part 5 at the time of bonding is excellent. If The modified polyolefin has the acid anhydride group, the adhesive properties are particularly excellent. modified polyolefin can be used alone, or two or more types can be used in combination become.

[0021] The melting point of component (A) is preferably not more than 185 °C and particularly preferably not more than 160 °C. If the melting point is 185 °C or less, an increase in the softening point of the adhesive layer 4 are suppressed, and deterioration of the conductor 2 or the insulating sheath layer 3 due to The heat generated when bonding is carried out is less likely. On the other hand, the Lower limit of the melting point, although not particularly limited, preferably not less than 80 °C. If the melting point is 80 °C or more, the adhesive layer 4 stabilizes at the operating temperature of the insulated Wire 1 with the adhesive layer slightly. The melting point of component (A) is determined at a dynamic Differential Scanning Calorimetry (DSC) by the peak temperature of the endothermic Peaks shown.

[0022] In the present disclosure, the polyester resin and the polyester elastomer used as the component (B) consisting of a dibasic acid and a polyol, whereby a block copolymer consisting of a hard segment with high crystallinity and a soft segment with low crystallinity is called a polyester elastomer, and a Polymer having a substantially uniform crystallinity as a whole, without distinction between hard and soft segments, called polyester resin.

[0023] The adhesive layer 4 contains (B) one or more materials selected from a polyester resin and a Polyester elastomer. As the component (B) forming the adhesive layer 4, either a polyester resin or a Polyester elastomer may be used, or both may be used in combination. If component (B) is a Polyester resin, the adhesion to the insulating coating layer 3 is excellent, and when component (B) a polyester elastomer, the flexibility is excellent. Component (B) preferably has a low melting point and excellent tensile strength.

[0024] The melting point of component (B) is preferably not more than 185 °C and particularly preferably not more than 160 °C. If the melting point is 185 °C or less, an increase in the softening point of the adhesive layer 4 are suppressed, and deterioration of the conductor 2 or the insulating sheath layer 3 due to the heat, generated when bonding is performed is less likely. On the other hand, the lower limit of the melting point, although it is not particularly limited, preferably not less than 80 °C. If the melting point 80 °C or more, the adhesive layer 4 stabilizes at the operating temperature of the insulated wire 1 with the Adhesive layer slightly. The melting point of component (B) is determined by differential scanning calorimetry (DSC). Differential Scanning Calorimetry (DSC) is represented by the peak temperature of the endothermic peak.

[0025] The polyester resin is not particularly limited, and examples thereof include polymers containing an aromatic dibasic acid and a short-chain aliphatic glycol as main materials, such as polyethylene terephthalate (PET), polytrimethylene terephthalate, polybutylene terephthalate (PBT), polyethylene naphthalate (PEN) and polybutylene naphthalate (PBN). From the point of view of lowering the melting point, the polyester resin forming the adhesive layer 4 is particularly preferably a polymer with a low degree of polymerization or a polymer obtained by copolymerizing an aliphatic dibasic acid, an isophthalic acid, a long-chain or alicyclic glycol, a Polyether polyol and the like as a third component in polymerizing the above-mentioned resin and reducing the symmetry of the molecules.

[0026] The polyester elastomer consists of a block copolymer of hard and soft segments. Examples of the hard segment include a crystalline polyester, such as the aforementioned PET or PBN. Examples of the soft Segment include an aliphatic polyether or an aliphatic polyester.

[0027] The breaking strength of component (B), measured according to JIS K7161, is preferably not less than 19 MPa and particularly preferably not less than 20 MPa. The breaking strength of component (B) is not particularly but may also be measured according to JIS K7161, not more than 50 MPa and preferably not more than 40 MPa. For example, the breaking strength of the polyester resin can be adjusted by the degree of polymerization and the components that are copolymerized are suitably adjusted, and the breaking strength of the polyester elastomer can be adjusted accordingly by the type and proportion of hard and soft segments.

[0028] The content of component (B) is preferably not less than 10 parts per 100 parts of the total of components (A) and (B), and particularly preferably not less than 20 parts. If the content of component (B) is 10 parts or more, the adhesion to the insulating coating layer 3 is excellent. On the other hand, if the adhesive carrier part 5 contains, for example, polyolefin, the adhesive strength on the adhesive carrier part 5 may decrease if the content of component (B) in the adhesive layer 4 is too high. From this point of view, the Content of component (B) preferably not more than 70 parts per 100 parts of the total of components (A) and (B). If the adhesive carrier part 5 is made of a polyester resin or a metal and does not contain polyolefin, the Adhesive layer 4 contains more than 70 parts of component (B).

[0029] The adhesive layer 4 may consist of a single layer or may be formed by laminating several layers If the adhesive layer 4 is formed from several layers, the adhesive strength between the insulating sheath layer 3 and the adhesive layer 4, for example, by using a layer containing a large amount of component (B) is arranged as an inner layer on the side of the insulating sheath layer 3. At the same time it is only necessary that the sum of the adhesive layers as a whole contains components (A) and (B) and 10 to Contains 70 parts of component (B).

[0030] The adhesive layer 4 may contain components other than (A) a modified polyolefin, (B) a polyester resin and a Polyester elastomer, as long as the purpose of the present disclosure is not impaired. Examples of Other components include additives such as an inorganic filler, a plasticizer, a stabilizer, a Pigment, an antioxidant and a tackifier. The adhesive layer 4 may also contain other polymer components such as which contain components (A) and (B). If other polymer components are included, it is ensuring the adhesion of the adhesive layer 4 to the insulating sheath layer 3 and the adhesive carrier part 5 It is preferred that the content of the other polymer components is not more than 30 parts per 100 parts of the total polymer components that form the adhesive layer 4.

[0031] Examples of the inorganic filler used as an additive include silica, diatomaceous earth, glass beads, talc, clay, Aluminium oxide, a metal oxide such as magnesium oxide, zinc oxide, antimony trioxide or molybdenum oxide, a metal hydroxide such as Magnesium hydroxide, a metal carbonate such as calcium carbonate or magnesium carbonate, a metal boric acid such as zinc borate or barium metaborate, and hydrotalcite. These can be used alone, or two or more of them can be used in combination can be used.

[0032] The softening point of the adhesive layer 4 is preferably at least lower than the softening point of the insulating sheath layer 3. In particular, the softening point thereof is preferably 80 to 170 °C. If the softening point is 170 °C or less, deterioration of the conductor 2 or the insulating Sheath layer 3 and deformation of the insulating sheath layer 3 due to the heat when bonding the adhesive layer 4 less likely. On the other hand, the adhesive layer 4 stabilizes at the operating temperature of the insulated wire 1 with the adhesive layer easily if the softening point is 80 °C or more. The softening point of the adhesive layer 4 and the softening point of the insulating coating layer 3 are determined by differential scanning calorimetry (DSC). Differential Scanning Calorimetry (DSC) is represented by the peak temperature of the endothermic peak.

[0033] As the insulated wire arranged on the inside of the adhesive layer 4, a conventional insulated wire as it is widely used. In particular, it is sufficient if an insulated wire with a conductor 2 and an insulating sheath layer 3 covering the outer circumference of the conductor 2.

[0034] For the conductor 2, copper is usually used, but instead of copper, another metal material, such as Aluminum or magnesium. These metal materials can be alloys. Examples of other Metal materials for forming an alloy include iron, nickel, magnesium, silicon, and a combination thereof. The conductor 2 may be formed from a single wire or may be formed from a twisted wire formed by Twisting several strands of wire together.

[0035] Illustrative examples of the material constituting the insulating sheath layer 3 include polyvinyl chloride (PVC), rubber and polyolefin. These can be used alone, or two or more of them can be used In addition, various additives can be added to these materials if necessary.

[0036] In general, the insulating sheath is often formed to comprise polyvinyl chloride. However, the Adhesive strength between polyvinyl chloride and the modified polyolefin contained in the adhesive layer 4 is weak, and with a conventional adhesive layer, detachment occurs at the interface between the adhesive layer and the insulating sheath layer. In the present disclosure, however, the adhesive layer 4 (A) contains a modified polyolefin and (B) one or more materials selected from polyester resin and a Polyester elastomer, and therefore the adhesive layer 4 and the insulating sheath layer 3 have an excellent adhesion, even if the insulating sheath layer 3 contains polyvinyl chloride.

[0037] For example, the respective materials forming the insulating sheath layer 3 and the adhesive layer 4 may be heated and kneaded, and the layers can be formed using an extrusion machine That is, the insulated wire is made by combining the polymer that forms the insulating sheath layer 3 and various additive components added as required, and extruding the heated and kneaded composition around the conductor 2 with an extrusion machine to form the insulating sheath layer 3 Then, the insulated wire 1 with the adhesive layer can be produced by mixing the components (A) and (B) and various additive components added as required, and the heated and kneaded composition is extruded on the outside of the insulated wire with an extrusion machine to to form the adhesive layer 4. If the insulating sheath layer 3 and the adhesive layer 4 are simultaneously Using a two-layer extrusion machine, each layer is extruded in a molten State laminated, and thus the adhesion between the insulating sheath layer 3 and the adhesive layer 4 excellent.

[0038] The adhesive layer 4 can be applied around the entire circumference in the circumferential direction on the outside of the insulating Sheath layer 3 may be formed so that it is circular in cross-section, as shown in Fig. 1 and Fig. 2, or it may be formed only on a portion in the circumferential direction on the outside of the insulating sheath layer 3. If the adhesive layer 4 is applied around the entire circumference of the outside of the insulating sheath layer 3, the adhesive surface between the adhesive layer 4 and the insulating sheath layer 3 is larger, and the adhesive strength is excellent. Also, if the adhesive layer 4 is circular, even assuming that the adhesive layer 4 and the insulating sheath layer 3 detach from each other, the wire can be held if it is within the range of the tensile strength of the adhesive layer 4 without the wire coming loose immediately. The adhesive layer 4 does not need to be applied over the entire surface in the longitudinal direction of the insulated wire.

[0039] The thickness of the conductor 2 and the thickness of the insulating sheath layer 3 can be in the area of ​​the insulated wires that are normally used. On the other hand, the thickness of the adhesive layer 4 is preferably 0.03 to 0.3 mm. If it is 0.03 mm or more, a sufficient bonding surface is easily secured, and if it is 0.3 mm or less, it can prevent the thickness of the insulated wire 1 with the adhesive layer as a whole from being excessively increases.

[0040] In the insulated wire 1 with the adhesive layer, the adhesive layer 4 can be softened and bonded by heating. Method of heating is not particularly limited, and examples thereof include, besides directly heating the insulated wire 1 with the adhesive layer or the adhesive carrier part 5 also the generation of frictional heat between the adhesive layer 4 and the adhesive carrier part 5 using an ultrasonic generator, such as a horn H, as shown in Fig. 3 When heated with an ultrasonic generator, the adhesive point can be heated locally without affecting the temperature of the entire insulated wire 1 with the adhesive layer excessively, causing deterioration of the conductor 2 or the insulating sheath layer 3 due to heat.

[0041] Here, the insulating coating layer 3 and the adhesive layer 4 are provided separately, and by heating at a temperature not higher than the softening point of the adhesive layer 4 and not higher than the Softening point of the insulating sheath layer 3, a deformation of the insulating sheath layer 3 at the time of the bonding can be suppressed, and the insulated wire 1 with the adhesive layer can be used without affecting its Properties as insulated wire can be glued.

[0042] The adhesive support member 5 to which the insulated wire 1 is bonded with the adhesive layer is not particularly limited, and examples thereof include a member made of a resin such as polyolefin or polyester, and a member made of a metal, such as iron, aluminum or stainless steel. Polyolefin elements are often used in vehicles, such as automobiles, used, and since the insulated wire 1 with the adhesive layer according to the present disclosure is a modified Contains polyolefin in the adhesive layer 4, the adhesion to polyolefin elements is particularly excellent.

[0043] The insulated wire 1 with the adhesive layer according to the present disclosure not only shows in fixing Wires on automobile bodies, on device housings or the like have a beneficial effect, but even if several insulated wires with adhesive layer are bundled by gluing and used in bundled condition as shown in Fig. 4.

[0044] Although an embodiment of the present disclosure has been described in detail above, the The present invention is in no way limited to the above embodiment, and various Modifications may be made without departing from the essence of the invention. EXAMPLES OF IMPLEMENTATION

[0045] Hereinafter, the present disclosure will be detailed using illustrative examples described, but the present invention is not limited to the embodiments. Preparation of an insulating polyvinyl chloride sheath composition

[0046] 100 parts polyvinyl chloride (“TK-1300”, manufactured by Shin-Etsu Chemical), 30 parts plasticizer (n-MOTM ´´Monocizer W-750´´, manufactured by DIC Corporation), 5 parts Ca / Zn heat stabilizer (´´ADK STAB RUP-100´´, manufactured by Adeka) and 5 parts calcium carbonate (´´Super 1700´´, manufactured by Maruo Calcium) were Kneaded using a twin-screw extruder to form an insulating polyvinyl chloride sheath layer. composition. Preparation of an insulating polypropylene sheath layer composition

[0047] 92 parts polypropylene (´´Novatec EC9´´, manufactured by Japan Polypropylene Corporation), 8 parts thermoplastic Elastomer (´´Tuftec M1913´´, manufactured by Asahi Kasei)), 70 parts magnesium hydroxide (´´Kisma 5´´, manufactured by Kyowa Chemical) and 0.5 parts hindered phenolic antioxidants ('Irganox 1010', manufactured by BASF) were kneaded using a twin-screw extruder to produce an insulating polypropylene sheath layer. composition. Manufacturing an insulated wire

[0048] An insulated wire was prepared by extruding the prepared insulating sheath material composition by 2 a twisted conductor with a conductor cross-sectional area of ​​0.13 mm and a sheath thickness of 0.2 mm manufactured. Preparation of an adhesive layer composition

[0049] An adhesive layer composition was prepared by combining components (A) and (B) in the amounts shown in Tables 1 to 3 using the materials listed below and kneading the combined Components were manufactured using a twin-screw extruder. Note that samples 21, 22 and 23 and samples 31 and 32 each consist of only one of the components (A) or (B).

[0050] Component (A) - Modified PP1 Manufactured by Toyobo: Toyotac M-312 (tensile strength 25.8 MPa) - Modified PP2 Manufactured by Mitsui Chemicals: Admer QE060 (tensile strength 35.0 MPa) Component (B) - Polyester resin 1 Manufactured by Toyobo: Vyloshot GM-955-RK20 (tensile strength 4.0 MPa, melting point 160 °C) - Polyester resin 2 Manufactured by Toagosei: Aron Melt PES-120L (tensile strength 36.5 MPa, melting point 120 °C) - Polyester elastomer 1 Manufactured by Toray Dupont: Hytrel 3046 (tensile strength 23.4 MPa, melting point 160 °C) - Polyester elastomer 2 Manufactured by Toray Dupont: Hytrel 4047N (tensile strength 19.1 MPa, melting point 182 °C) Formation of the adhesive layer

[0051] By extruding each of the adhesive layer compositions at 200 °C around the entire circumference on the The outside of the insulated wire with an insulating sheath layer of polyvinyl chloride or polypropylene was an adhesive layer with a thickness of 0.1 mm is formed. Evaluation

[0052] As shown in Fig. 5A, an insulated wire 11 with adhesive layer was placed on an adhesive carrier part 16 so that he came into contact with it 1 cm from its edge, and the remaining section of the insulated wire 11 with The adhesive layer was protected with a release film 17, after which irradiation with 20 kHz ultrasound from above through the Horn H for 10 seconds, and the insulated wire 11 with the adhesive layer and the adhesive carrier part 16 were bonded together. The bonded section was cooled to room temperature and, as shown in Fig. 5B of Fig. 5 As shown, the section protected with the release film was folded back 180 degrees towards the glued edge and pulled at a speed of 50 mm / s in the axial direction to the insulated wire 11 with adhesive layer Tables 1 to 3 show the maximum test force exerted when peeling the insulated wire 11 It should be noted that a plate-like material made of one of the Materials polypropylene (PP), polyethylene terephthalate (PET) or aluminum (AL), as shown in Tables 1 to 3 is shown. Table 1 sample 1 2 3 4 5 6 Adhesive layer (A) Modified PP1 80 80 80 80 80 80 Modified PP2 - - - - - - (B) Polyester resin 1 20 20 20 20 20 20 Polyester resin 2 - - - - - - Polyester elastomer 1 - - - - - - Polyester elastomer 2 - - - - - - Insulating sheath layer PVC PVC PVC PP PP PP Adhesive carrier part PP PET AL PP PET AL Max. test force (N) 8.2 9.1 7.6 12.2 13.2 11.6 Table 2 sample 7 8 9 10 11 12 Adhesive layer (A) Modified PP1 - 80 80 80 90 70 Modified PP2 80 - - - - - (B) Polyester resin 1 20 - - - 10 30 Polyester resin 2 - 20 - - - - Polyester elastomer 1 - - 20 - - - Polyester elastomer 2 - - - 20 - - Insulating sheath layer PVC PVC PVC PVC PVC PVC Adhesive carrier part PP PP PP PP PP PP Max. test force (N) 10.2 10.6 7.2 8.1 7.4 4.1 Table 3 Sample Sample 21 22 23 24 25 31 32 Adhesive layer (A) Modified PP1 100 - - 95 20 100 100 Modified PP2 - - - - - - - (B) Polyester resin 1 - 100 - 5 80 - - Polyester resin 2 - - - - - - - Polyester elastomer 1 - - 100 - - - - Polyester elastomer 2 - - - - - - - Insulating sheath layer PVC PVC PVC PVC PVC PP PP Adhesive carrier part PP PP PP PP PP PET AL Max. test force (N) 0.2 0.4 0.1 1.2 1.6 8.4 6.9

[0053] Samples 1 to 12, in which the adhesive layer contains components (A) and (B) and the content of Component (B) is within the scope of the above disclosure, show on both the insulating sheath layer and also on the adhesive carrier part an excellent adhesion, and the holding power of the Wire on the adhesive carrier part is large. In particular, samples 1 to 8, which contain polyester resin as component (B), show use, a particularly excellent adhesion to the insulating sheath layer and the adhesive carrier part, and It occurred because of the detachment at the interface between the insulating sheath layer and the adhesive layer and between the adhesive carrier part and the adhesive layer is less likely to occur, to a cohesive Failure or breakage within the adhesive layer. In such cases, it is less likely that the Adhesive layer fails and the holding force of the wire increases when a material with a high tensile strength is used for the Component (A) or (B) is used, such as in samples 7 and 8. In addition, samples 9 and 10, which use polyester elastomer as component (B), have excellent flexibility, although the holding force of the wire is slightly lower than that of samples 1 and 8, which use polyester resin as component (B).

[0054] On the other hand, Sample 21 in which the adhesive layer does not contain the component (B) and Sample 24 in which contains only a small amount of component (B), has poor adhesion to the adhesive carrier part, which Polyvinyl chloride. Samples 22 and 23, in which the adhesive layer does not contain component (A), and the Sample 25, which contains a large amount of component (B), is in terms of adhesion to the adhesive carrier part, which is made of polypropylene. It should be noted that even if the adhesive layer does not contain component (B) contains, the adhesion between the insulating sheath layer and the adhesive layer is sufficient and the wire is the adhesive carrier part when the insulating sheath layer is made of polypropylene (samples 31 and 32). However, when comparing samples 31 and 32 with samples 5 and 6, it is obvious that the adhesion between the adhesive layer and the adhesive carrier part is improved and the adhesion of the wire is improved, since the adhesive layer contains component (B) in addition to component (A). LIST OF REFERENCE SYMBOLS 1 Insulated wire with adhesive layer 2 conductors 3 Insulating sheath layer 4 adhesive layer 5 Adhesive carrier part 11 Insulated wire with adhesive layer 16 Adhesive carrier part 17 Separating film H Horn (ultrasonic generator)

Claims

1. Insulated wire (1, 11) with an adhesive layer, comprising: a conductor (2); an insulating sheath layer (3) covering an outer periphery of the conductor (2); and an adhesive layer (4) provided on an outer side of the insulating sheath layer (3) and for hot-bonding serves, wherein the adhesive layer (4) contains: Component A: a modified polyolefin; and Component B: one or more materials selected from a polyester resin and a polyester elastomer, the adhesive layer (4) contains 10 to 70 parts of component B per 100 parts of the total of components A and B, component A has a melting point between 80°C and 185°C, Component B has a melting point between 80°C and 185°C and a breaking strength between 19 MPa and 50 MPa, measured according to JIS K7161, and the adhesive layer (4) has a softening point between 80°C and 170°C.

2. Insulated wire (1, 11) with adhesive layer (4) according to claim 1, wherein the insulating sheath layer (3) is a polyvinyl chloride contains.

3. Insulated wire (1, 11) with adhesive layer (4) according to claim 1 or 2, wherein the adhesive layer (A) comprises the modified polyolefin and (B) the polyester resin.

4. Insulated wire (1, 11) with adhesive layer according to claim 1 or 2, wherein the adhesive layer (A) comprises the modified polyolefin and (B) the polyester elastomer.

5. Insulated wire (1, 11) with adhesive layer according to one of claims 1 to 4, wherein the adhesive layer (4) is entire circumference in a circumferential direction on the outside of the insulating jacket layer (3).

Citation Information

Patent Citations

  • Fire-resistant adhesive film and flat cable using this film

    JP1998149725A

  • Electric wire with welded layer and method of manufacturing electric wire with welded layer

    JP2002237219A

  • JP000H10149725A

  • JP002002237219A