Federstahldraht

DE112020006562B4Active Publication Date: 2024-10-10SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
DE112020006562
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-15
Publication Date
2024-10-10
Estimated Expiration
2040-06-15

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Spring steel wire (1) comprising: a main body (10) made of steel and having a linear shape; and an oxidized layer (20) covering an outer circumferential surface (10A) of the main body (10);wherein the steel forming the main body (10) contains not less than 0.5 wt% and not more than 0.7 wt% C, not less than 1 wt% and not more than 2.5 wt% Si, not less than 0.2 wt% and not more than 1 wt% Mn, and not less than 0.5 wt% and not more than 2 wt% Cr, the remainder being Fe and unavoidable impurities, wherein the steel forming the main body (10) has a pearlite structure, and the oxidized layer (20) has a thickness (t) of not less than 2 µm and not more than 5 µm, and wherein the oxidized layer (20) contains not less than 60 wt% Fe3O4 and comprises a first Fe3O4 layer (22) and a second Fe3O4 layer (23) which forms an outer circumferential surface (22A) of the first Fe3O4 layer (22) covers, encloses, wherein the first Fe3O4 layer (22) has a higher Si concentration than a Si concentration of the second Fe3O4 layer (23) and a Si concentration of the main body (10).;
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present disclosure relates to a steel wire for mechanical springs. State of the art

[0002] Oil-quenched and tempered wires (spring steel wires) with an oxidized layer on the outer Circumferential surface, for the purpose of ensuring lubrication during the winding process, are known (see For example, Japanese Patent Application Laid-Open No. JP 2004-52048 A (Patent Literature 1), the Laid-Open Japanese patent application JP 2017- 115 859 A (Patent Literature 2), Japanese patent application laid open JP 2017- 115 228 A (Patent Literature 3) and Japanese Patent Application Laid-Open No. JP 2018-12 868 A (Patent Literature 4)). JP 2014-169470 A (Patent Literature 5) relates to a spring steel wire with an oxidized layer of magnetite and hematite. Wire material for an inclined spiral spring with a core wire made of steel with a pearlite structure and a Plating layer of copper or a copper alloy, which covers the surface of the core wire, is known from DE 11 2017 002 913 T5 (Patent Literature 6). DE 694 31 200 T2 (Patent Literature 7) describes an oil-hardened wire which a steel wire with an oxide layer on it and a lubricating coating of lubricating oil and / or organic The thickness of the oxide layer is between 0.5 and 1.0 µm.

[0003] Steel wire rods with an FeO layer as scale inner layer on the surface of a steel and a Fe SiO - 2 4 Layer formed in an interface between FeO layer and the steel are known from EP 2 113 580 B1 (Patent Literature 8). EP 2 166 114 B1 (Patent Literature 9) relates to a method for producing a steel wire with excellent mechanical descaling properties. The steel wire has an FeSiO layer. 2 4 Quotation list Patent literature Patent literature 1: JP 2004- 52 048 A Patent literature 2: JP 2004- 115 859 A Patent literature 3: JP 2017- 115 228 A Patent literature 4: JP 2018- 12 868 A Patent literature 5: JP 2014- 169 470 A Patent literature 6: DE 11 2017 002 913 T5 Patent literature 7: DE 694 31 200 T2 Patent literature 8: EP 2 113 580 B1 Patent literature 9: EP 2 166 114 B1 Summary of the invention

[0004] A spring steel wire according to the present disclosure is defined in claim 1. Short description of the drawings Fig. 1 is a diagram showing the structure of a spring steel wire; Fig. 2 is a schematic cross-sectional view showing the structure of the spring steel wire; Fig. 3 is a schematic cross-sectional view showing the structure of an oxidized layer of the spring steel wire shows; Fig. 4 is a flow chart schematically illustrating a process for manufacturing a spring steel wire; Fig. 5 is a schematic cross-sectional view showing the structure of an oxidized layer of a spring steel wire according to embodiment 2; and Fig. 6 is an SEM image of the oxidized layer. Description of embodiments [Problem to be solved by the present disclosure]

[0005] As explained above, one technique to improve lubricity when winding an oil-quenched and tempered wire as a spring steel wire into a spring by coating the outer peripheral surface of the wire with covered with an oxidized layer. The steel that forms the oil-quenched and tempered wire has a tempered martensite structure. The tempered martensite structure includes a matrix of martensitic phase and fine carbides dispersed in the matrix. Covering the surface of the steel wire, which has such tempered martensite structure, with an oxidized layer, can improve the lubricity during the winding process ensure.

[0006] On the other hand, a hard-drawn wire can be used as a spring steel wire. The steel that forms the hard-drawn wire has a pearlite structure. The pearlite structure with alternating laminated ferrite and cementite (Fe C) layers differs considerably from the tempered martensite structure described above. Consequently, it is 3 For the hard-drawn wire, it is necessary to consider a way to achieve a lubricity suitable for the pearlite structure Against this background, it is an object of the present disclosure to provide a spring steel wire made of hard-drawn wire that shows excellent lubricity when subjected to the winding process is subjected to. [Advantageous Effects of the Present Disclosure]

[0007] The spring steel wire according to the present disclosure may comprise a spring steel wire made of hard drawn wire which ensures excellent lubricity during the winding process. [Description of Embodiments of the Present Disclosure]

[0008] First, embodiments of the present disclosure will be listed and described. A spring steel wire according to the present disclosure includes a main body made of a steel and having a line shape and an oxidized layer covering an outer peripheral surface of the main body. The steel that forms the main body, contains not less than 0.5 mass% and not more than 0.7 mass% C (carbon), not less than 1.0 mass% and not more than 2.5 mass% Si (silicon), not less than 0.2 mass% and not more than 1.0 mass% Mn (manganese) and not less than 0.5 mass% and not more than 2.0 mass% Cr (chromium), the remainder being Fe (iron) and are unavoidable impurities. The steel that forms the main body has a pearlite structure. The oxidized Layer has a thickness of not less than 2 µm and not more than 5 µm. The oxidized layer contains not less than 60 mass% Fe O and includes a first and a second Fe O layer as specified in claim 1. 3 4 3 4

[0009] The structure of the steel constituting the main body of the spring steel wire of the present disclosure is the Pearlite structure. That is, the spring steel wire of the present disclosure is a hard-drawn wire. In the spring steel wire of the present disclosure, the outer peripheral surface of the main body having the pearlite structure is provided with the oxidized Layer with a thickness of not less than 2 µm and not more than 5 µm. The oxidized layer contains at least 60 mass% Fe O . According to the studies conducted by the inventors, when the oxidized 3 4 Layer contains at least 60 mass% Fe O, the flaking of the oxidized layer from the main body with the 3 4 Pearlite structure is suppressed and high lubricity during the winding process is ensured.

[0010] As described above, the spring steel wire according to the present disclosure is a spring steel wire made of hard-drawn wire which shows excellent lubricity when subjected to the winding process The oxidized layer preferably contains 70 mass% or more of Fe O and more preferably 80 mass% 3 4 or more Fe O . 3 4

[0011] The reasons for limiting the component composition of the steel forming the main body to The areas described above will now be described.

[0012] Carbon (C): not less than 0.5 mass% and not more than 0.7 mass%

[0013] Carbon is an element that greatly influences the strength of steel. To ensure sufficient To achieve greater strength than a spring steel wire, it is necessary that the carbon content is not less than 0.5 mass% On the other hand, an increased carbon content can reduce toughness, making machining difficult. To ensure sufficient toughness, it is necessary that the carbon content does not exceed 0.7 mass% To improve toughness and facilitate machining, the carbon content cannot exceed 0.6 mass%.

[0014] Silicon (Si): not less than 1 mass% and not more than 2.5 mass% Silicon has the property of suppressing softening as a result of heating (resistance to softening) To prevent softening as a result of heating when winding the spring steel wire into a spring as well as during To suppress the use of the spring, it is necessary that the silicon content is not less than 1 mass%, and it cannot be less than 1.2 mass%. On the other hand, silicon, if used in an excessive amount, reduces To ensure sufficient toughness, it is necessary that the silicon content not more than 2.5 mass%. From the point of view of focusing on toughness, the silicon content cannot more than 2% by mass or not more than 1.6% by mass.

[0015] Manganese (Mn): not less than 0.2 mass% and not more than 1 mass% Manganese is an element that is added as a deoxidizer during steel production. To function as the deoxidizer, it is necessary that the manganese content is not less than 0.2 mass%, and it can not less than 0.5 mass%. On the other hand, if manganese is added in an excessive amount, the toughness and reduces the machinability during hot forming. Therefore, it is necessary that the manganese content is not more than 1% by mass, and it cannot be more than 0.9% by mass.

[0016] Chromium (Cr): not less than 0.5 mass% and not more than 2 mass% Chromium acts as a carbide-forming element in the steel and contributes to the refinement of the metal structure as a result of The formation of fine carbides and also contributes to the suppression of softening during heating. To ensure that these effects are achieved, it is necessary that chromium is present in an amount of not less than 0.5 % by mass. On the other hand, chromium, when added in an excessive amount, causes deterioration of toughness. Therefore, the added amount of chromium must not exceed 2 mass%. From the point of view of focusing on toughness, the amount of chromium added can not exceed 1.5 mass % or not more than 1% by mass. Unavoidable contamination

[0017] During the process of producing the steel that forms a spring steel wire, phosphorus (P), sulfur (S) etc. inevitably mixed into the steel. Phosphorus and sulfur call when they are contained in excessive amounts cause grain boundary segregation and create inclusions, thereby deteriorating the properties of the steel. Therefore, the phosphorus content and the sulfur content are each preferably not more than 0.025 mass%. Furthermore, the Total content of unavoidable impurities preferably not more than 0.3 mass%.

[0018] In the spring steel wire described above, the oxidized layer includes a first Fe O layer and a second 3 4 Fe O layer covering an outer peripheral surface of the first Fe O layer. The first Fe O layer has a 3 4 3 4 3 4 higher Si concentration than a Si concentration of the second Fe O layer and a Si concentration of the 3 4 main body. The presence of the first Fe O layer with a high Si concentration between the second Fe O - 3 4 3 4 layer and the main body further suppresses the peeling of the oxidized layer from the main body.

[0019] In the spring steel wire described above, the oxidized layer may further comprise a FeO layer between the first FeO layer and the main body. The state of oxidation to the extent that the FeO layer 3 4 formed between the first Fe O layer and the main body can suppress the formation of a Fe O layer, 3 4 2 3 which peels off easily.

[0020] Although the FeO layer may cover the entire outer peripheral surface of the main body, in the above described spring steel wire the FeO layer the outer peripheral surface of the main body preferably partially. In a part of the main body where its outer peripheral surface is not in contact with the FeO layer, the main body and the first Fe O layer are preferably in contact with each other. Such a 3 4 Design further suppresses the peeling of the oxidized layer from the main body.

[0021] In the spring steel wire described above, the first Fe O layer may have a Si concentration of not less 3 4 than 2.5 mass% and not more than 6 mass% and a Cr concentration of not less than 1.5 mass% and not more than 3 mass%. Such a design can prevent the oxidized layer from peeling off from the main body additionally suppress.

[0022] In the spring steel wire described above, the first Fe O layer may have a thickness of not less than 0.3 µm 3 4 and not more than 1.5 µm. Such a design suppresses the flaking of the oxidized layer from the Main body additionally. [Details of Embodiments of the Present Invention]

[0023] Embodiments of the spring steel wire according to the present disclosure are described below with reference to the drawings. In the following drawings, the same or corresponding parts are identified by the same reference numbers and their description is not repeated. (Embodiment 1)

[0024] Fig. 1 is a schematic diagram showing the structure of a spring steel wire. Fig. 2 is a schematic Cross-sectional view showing the structure of the spring steel wire. Fig. 2 shows a cross-section perpendicular to the Longitudinal direction of the spring steel wire.

[0025] Referring to Fig. 1 and Fig. 2, a spring steel wire 1 according to the present embodiment includes a main body 10 made of steel and having a line shape, and an oxidized layer 20, which an outer peripheral surface 10A of the main body 10. The oxidized layer 20 has an outer Circumferential surface 20A, which forms an outer circumferential surface of the spring steel wire 1. Referring to Fig. 2, the Spring steel wire 1 has a diameter ϕ of, for example, not less than 2.0 mm and not more than 8.0 mm. oxidized layer 20 has a thickness t of not less than 2 µm and not more than 5 µm.

[0026] The steel forming the main body 10 contains not less than 0.5 mass% and not more than 0.7 mass% C, not less than 1 mass% and not more than 2.5 mass% Si, not less than 0.2 mass% and not more than 1 mass- % Mn and not less than 0.5 mass% and not more than 2 mass% Cr, the remainder being Fe (iron) and unavoidable impurities. The steel forming the main body 10 may have a component composition that meets JIS SWOSC-V. The steel forming the main body 10 can be, for example, SAE 9254V. The steel forming the Main body 10 may be one based on such a steel grade, wherein the amount of C is within the above described component composition range may be increased. The steel forming the main body 10, has a pearlite structure. Spring steel wire 1 is a hard-drawn wire.

[0027] The structure of the oxidized layer 20 will be described in detail below. Fig. 3 is a schematic Cross-sectional view showing the structure of the oxidized layer 20 of the spring steel wire 1. Referring to Fig. 3 the oxidized layer 20 covers the entire outer peripheral surface 10A of the main body 10. The oxidized layer 20 is in contact with the outer peripheral surface 10A of the main body 10. The oxidized layer 20 contains 60 mass% or more Fe O . 3 4

[0028] The oxidized layer 20 includes a FeO layer 21, a first FeO layer 22, a second FeO layer 23 and 3 4 3 4 a Fe O layer 24. The FeO layer 21 is arranged on the outer peripheral surface 10A of the main body 10. The 2 3 FeO layer 21 is in contact with the outer peripheral surface 10A of the main body 10. The first FeO layer 22 is 3 4 arranged on an outer peripheral surface 21A of the FeO layer 21. The first FeO layer 22 is in contact with the 3 4 outer peripheral surface 21A of the FeO layer 21. The first FeO layer 22 surrounds the entire circumference of the outer 3 4 Circumferential surface 10A of the main body 10. The FeO layer 21 is located between the first Fe O layer 22 and the 3 4 Main body 10.

[0029] The second Fe O layer 23 is arranged on an outer peripheral surface 22A of the first Fe O layer 22. The second Fe 3 4 3 4 O layer 23 is in contact with the outer peripheral surface 22A of the first Fe O layer 22. The second Fe O layer 3 4 3 4 3 4 23 is in contact with the entire outer peripheral surface 22A of the first Fe O layer 22. The second Fe O layer 23 3 4 3 4 surrounds the entire circumference of the outer peripheral surface 10A of the main body 10 and the outer peripheral surface 22A the first Fe O layer 22. 3 4

[0030] The Fe O layer 24 is arranged on an outer peripheral surface 23A of the second Fe O layer 23. The Fe O - 2 3 3 4 2 3 Layer 24 is in contact with the outer peripheral surface 23A of the second Fe O layer 23. The Fe O layer 24 can 3 4 2 3 cover all or part of the outer peripheral surface 23A of the second Fe O layer 23. The Fe O layer 24 3 4 2 3 is not an indispensable element of the spring steel wire of the present disclosure and is not required. The Fe O - 2 3 Layer 24 has its outer peripheral surface 24A, which is the outer peripheral surface 20A of the oxidized layer 20 or the outer peripheral surface of the spring steel wire 1. If the Fe O layer 24 is on a part of the outer peripheral surface 2 3 23A of the second Fe O layer 23, forms in a part of the outer peripheral surface 23A of the second Fe O layer 3 4 3 4 23, on which there is no Fe O layer 24, the outer peripheral surface 23A of the second Fe O layer 23, the outer 2 3 3 4 Circumferential surface 20A of the oxidized layer 20 or the outer circumferential surface of the spring steel wire 1. If no Fe O - 2 3 Layer 24 is present, the outer peripheral surface 23A of the second Fe O layer 23 is the outer peripheral surface 20A of the 3 4 oxidized layer 20 or the outer peripheral surface of the spring steel wire 1.

[0031] The first Fe O layer 22 has a Si concentration that is higher than the Si concentration of the second Fe O 3 4 3 4 Layer 23 and the Si concentration of the main body 10. The Si concentration of the first Fe O layer 22 is 3 4 for example, not less than 2.5 mass% and not more than 6 mass%. The first Fe O layer 22 has, for example, 3 4 a Cr concentration of not less than 1.5 mass% and not more than 3 mass%.

[0032] In the spring steel wire 1 of the present embodiment, the outer peripheral surface 10A of the main body 10, which has the pearlite structure, with the oxidized layer 20 having a thickness of not less than 2 µm and not more than 5 µm. The oxidized layer 20 contains 60 mass% or more Fe O . This suppresses the flaking of the 3 4 oxidized layer 20 from the main body 10, which has the pearlite structure, and provides high lubricity during Winding the spring steel wire 1 into a spring. As a result, the spring steel wire 1 is a spring steel wire made of hard-drawn wire, which ensures excellent lubricity during the winding process.

[0033] The oxidized layer 20 of the present embodiment includes the first Fe O layer 22 and the second Fe O 3 4 3 4 Layer 23 covering the outer peripheral surface 22A of the first Fe O layer 22. The Si concentration of the first Fe 3 4 3 O layer 22 is higher than the Si concentration of the second Fe O layer 23 and the Si concentration of the main body 4 3 4 10. Providing such a first Fe O layer 22 is not necessary for the spring steel wire of the present disclosure 3 4 indispensable. However, the presence of such a first Fe O layer 22 suppresses the flaking of the oxidized 3 4 Layer 20 of the main body 10 additionally.

[0034] The oxidized layer 20 of the present embodiment includes the FeO layer 21 between the first FeO - 3 4 Layer 22 and the main body 10. Although the presence of the FeO layer 21 is important for the spring steel wire of the present disclosure is not indispensable, the state of oxidation suppresses to the extent that the FeO Layer 21 is formed between the first Fe O layer 22 and the main body 10, the formation of the Fe O layer 3 4 2 3 24, which easily flakes off. The percentage of the FeO layer 21 in the oxidized layer 20, for example, is no more than 5 mass%. The percentage of the FeO layer 21 in the oxidized layer 20 is preferably not more than 1 mass% and more preferably not more than 0.1 mass%.

[0035] In the spring steel wire 1 of the present embodiment, the first Fe O layer may have a thickness of not 3 4 less than 0.3 µm and not more than 1.5 µm. This can prevent the oxidized layer 20 from flaking off the Main body additionally suppressed.

[0036] An exemplary method for producing the spring steel wire 1 will now be described with reference to Fig. 4. Fig. 4 is a flowchart showing the method for manufacturing the spring steel wire 1 of the present embodiment schematically illustrated. Referring to Fig. 4, in the process for producing the spring steel wire 1 in the In the present embodiment, a step for producing the wire material is first carried out as step S10. In step S10 is a wire material made of steel the steel contains not less than 0.5 mass% and not more than 0.7 mass% C, not less than 1.0 mass% and not more than 2.5 mass% Si, not less than 0.2 mass% and not more than 1.0 mass% Mn and not less than 0.5 mass% and not more than 2.0 mass% Cr, the remainder being Fe and unavoidable impurities.

[0037] Next, a patenting step is performed as step S20 with reference to Fig. 4. In step S20, Referring to Fig. 4, the wire material produced in step S10 is subjected to patenting. In detail, the Wire material is subjected to a heat treatment in which the wire material is heated to a temperature range not lower than the austenitizing temperature (A point) and then quickly to a temperature range higher than the 1 Starting temperature of the martensitic transformation (M point) is cooled and kept in the temperature range. S This gives the wire material a fine pearlite structure with a small lamella spacing. In the patenting process, the process of heating the wire material to the temperature range not lower than the A point under the 1 point of view that the occurrence of decarburization is suppressed, preferably in an inert gas atmosphere carried out.

[0038] Next, referring to Fig. 4, a step of removing the surface layer is designated as a step S30 In step S30, a surface layer of the wire material which was patented in step S20 In detail, the wire material is passed through a scraping nozzle, whereby a decarburized layer or the like on the surface formed by the patenting is removed Although this step is not an indispensable step, even if a decarburized layer or the like is present in As a result of patenting on the surface, such a layer can be removed by this step is carried out.

[0039] Next, an annealing step is carried out as a step S40. In the step S40, the wire material whose Surface layer was removed in step S30, is subjected to annealing. In detail, the Wire material is subjected to a heat treatment in which the wire material is heated to a temperature range not lower than 600°C and not higher than 700°C in an inert gas (for example nitrogen or argon gas) atmosphere and for a period of not less than one hour and not longer than ten hours While annealing is a heat treatment that is carried out to soften a wire material In the present embodiment, an oxidized layer 20 is formed in this step S40 and the structure in the oxidized layer 20.

[0040] In the present embodiment, the above-described heat treatment carried out in step S40 carried out, the surface part of the wire material and thereby forms an oxidized layer 20. The area that not become the oxidized layer 20, forms the main body 10 (see Fig. 2 and others). From the point of view, To easily form an oxidized layer 20 with a high percentage of Fe O, the heat treatment 3 4 For example, heating the wire material to about 600°C in a nitrogen atmosphere. This forms the oxidized layer 20 with a high percentage of Fe O , because the surface part is filled by the oxygen, the 3 4 as an impurity in the nitrogen, argon or other inert gas, as well as by the oxygen that inevitably enters the heat treatment furnace, is oxidized. The oxidized layer 20 of the present However, the embodiment should be thick with a thickness of not less than 2 µm and not more than 5 µm. Furthermore, the oxidized layer 20 of the present embodiment, the first Fe O layer with a high Si concentration 3 4 From the point of view of forming such an oxidized layer 20, the heating temperature and the Atmosphere in the furnace can be controlled. Although the atmosphere in the furnace has a strong influence and may cause the conditions to vary depending on the system, the heating temperature will be higher than usual and is not lower than 650°C and preferably not lower than 680°C. Also regarding the atmosphere, Instead of the usual inert gas atmosphere, an atmosphere in which the inert gas is deliberately mixed with air can be used. or an atmosphere in which the inert gas is mixed with water vapor. The procedure as above makes it possible to form an oxidized layer 20 with the desired composition and structure.

[0041] Next, a shot peening step is performed as step S50. In step S50, the wire material that forms the Annealing in step S40, with the oxidized layer 20 formed thereon, subjected to shot peening Although this step is not essential, performing this step can make the brittle Fe O layer 2 3 24 formed on the surface of the oxidized layer 20 and also the percentages of FeO, Fe O and Fe 3 4 O in the oxidized layer 20. In detail, the intensity and time of the shot peening are adjusted so that 2 3 that the Fe O layer 24 from the 2 3 oxidized layer 20 is removed and the first Fe O layer 22 and the second Fe O layer 23 remain. 3 4 3 4

[0042] Next, a wire drawing step is performed as step S60. In step S50, the wire material, the which has undergone shot peening in step S50, is subjected to the wire drawing process (drawing process). Processing (reduction of area) in the wire drawing process in step S60 can be set as applicable for example, the reduction in area may be set at not less than 60% and not more than 80% Here, the ´´reduction in area´´ refers to a cross section perpendicular to the longitudinal direction of the wire material and refers to a value, expressed in percent, obtained by dividing a Difference between the cross-sectional areas before and after the wire drawing process by the average area before Wire drawing process.

[0043] Next, a step of forming the oxidized layer is performed as step S70. In step S70, the Wire material (steel wire), after it has undergone the wire drawing process in step S60, the heat treatment to further form the oxidized layer 20. In the case that the oxidized layer 20 has been formed as in Step S40 is desired, this step S70 can be omitted. Step S70 is carried out if the oxidized layer 20 formed in step S40 has an insufficient thickness or if the composition and / or Structure of the oxidized layer 20 must be adjusted. The heat treatment conditions in step S70 are the same as those in step S40.

[0044] The spring steel wire 1 according to the present embodiment is produced by the method described above In particular, performing steps S40 and S70, as applicable, can produce the spring steel wire 1 with the oxidized layer 20 with the desired thickness, composition and structure. (Embodiment 2)

[0045] Now, a further embodiment, Embodiment 2, will be described. The spring steel wire of the Embodiment 2 has basically a similar structure and similar effects to those of Embodiment 1. The Spring steel wire of embodiment 2 differs from that of embodiment 1 in the structure of the oxidized layer. Fig. 5 is a schematic cross-sectional view showing the structure of the oxidized layer of the spring steel wire in Embodiment 2 shows.

[0046] Referring to Fig. 5, in the spring steel wire 1 of Embodiment 2, the FeO layer 21 covers the outer Circumferential surface 10A of the main body 10 partially. In the part of the main body 10 where its outer circumferential surface 10A is not covered with the FeO layer 21, the main body 10 and the first FeO layer 22 are in contact 3 4 The area where the main body 10 and the first Fe O layer 22 are in contact with each other, which is 3 4 formed in this way further suppresses the peeling of the oxidized layer 20 from the main body 10.

[0047] It should be noted that the oxidized layer 20 in Embodiment 2 can be formed by the Heat treatment conditions in steps S40 and S70 in the manufacturing method in Embodiment 1 above be adjusted. Examples (Experiment 1)

[0048] An experiment was conducted to determine the relationship between the thickness of the oxidized layer and the yield when the wire is wound into a spring. The spring steel wire was used in a similar Process as in Embodiment 1 above. Here, the heating temperature in step S40 was set to 700°C and the heating time was adjusted to keep the thickness of the oxidized layer within the range of 0.3 µm to 6.5 µm to produce samples A to E. To obtain the thickness of the oxidized layer, the cross section perpendicular to the longitudinal direction using a scanning electron microscope (SEM) and an average of the thicknesses at four points at diameters orthogonal to each other. The spring steel wire had a Diameter of 1.2 mm. Samples A to E were wound into a spring using a winding machine. Spring had an outer winding diameter of 7 mm, an effective number of turns of 12 and a free length of 32 mm. 100 springs were produced for each sample. The winding machine used was a VF-720ST, manufactured by Shinko Machinery Co., Ltd.

[0049] For the feathers obtained, the yield was calculated by removing those with a difference of more than 0.5 mm from the target free length (32 mm) and those where seizing was observed on the surface Here, the ´´free length´´ means the total length of the spring in the state where no load is applied to the spring is applied. The experimental results are shown in Table 1. [Table 1] Thickness of the oxidized layer (µm) Surface condition Yield (%) A 0.3 Eating observed 73 B 1,2 Eating observed 81 C 2.2 Good 96 D 4.5 Good 95 E 6.5 Eating observed 83

[0050] Referring to Table 1, for samples C and D, in which the oxidized layer had a thickness of not less than 2 µm and not more than 5 µm, the surface condition was good and a high yield was ensured. On the other hand, for samples A, B and E with the oxidized layer having a thickness outside the range of not less than 2 µm and not more than 5 µm, scuffing occurred on the surface, resulting in a low yield. In samples A and B with a thin oxidized layer, seizure may have occurred as a result of the insufficient lubricity. On the other hand, in sample E with a thick oxidized layer, the appearance of Local flaking of the oxidized layer may cause seizure.

[0051] The above experimental results show that the oxidized layer has a thickness of not less than 2 µm and should be more than 5 µm. (Experiment 2)

[0052] An experiment was conducted to investigate the effects of the formation of the first Fe O layer with a high Si- 3 4 concentration. The spring steel wire was prepared in a similar manner as in Experiment 1 above, and the The yield and the condition of the surface during the formation of the feathers were investigated. In Experiment 2, the Heating temperature in the heat treatment in step S40 is set to 750°C or 800°C, and in the state of increased Diffusion rate of Si and other elements in the steel, the heating time was adjusted and thereby the thickness of the first Fe O layer. The thickness of the first Fe O layer was measured using a SEM. Fig. 6 shows a 3 4 3 4 Example of SEM observation. Measurement using an energy dispersive spectrometer (EDS) confirmed that the oxidized layer 20 in Fig. 6 comprises the FeO layer 21, the first Fe O layer 22, the second Fe O layer 23 and the 3 4 3 4 Fe O layer 24 and that the first Fe O layer 22 had a higher Si concentration than that in the 2 3 3 4 Main body 10 and the second Fe O layer 23. The experimental results are shown in Table 2. [Table 2] 3 4 Thickness of the first Fe O layer (µm) Thickness of the oxidized layer (µm) Surface condition Yield (%) 3 4 F 2.2 0.2 Good 96 G 2.1 1.1 Good 98 H 2.2 2.2 Good 98 I 6.5 0.3 Eating observed 83 J 6.3 1.2 Good 85 K 6.4 2.4 Good 85

[0053] Referring to Table 2, in the samples F to H with the oxidized layer having a thickness of not less than 2 µm and not more than 5 µm, a further improvement in yield than in Experiment 1 was confirmed. Also in samples I to K with the oxidized layer with a thickness of over 5 µm, the occurrence of scuffing would probably be suppressed, which leads to an improved yield. This may presumably be the case because the formation of the first Fe O layer 22 3 4 Peeling of the oxidized layer 20 from the main body 10 has been suppressed. (Experiment 3)

[0054] An experiment was conducted to determine the relationship between the composition between the oxidized layer and the yield. The spring steel wire was prepared in a similar manner as in Experiment 1 above, and the yield and condition of the surfaces when the springs are formed was In Experiment 3, the atmosphere in the heat treatment was changed in step S40 to composition of the oxidized layer. In particular, in sample L, air was deliberately exposed to the atmosphere to increase the oxygen partial pressure and thereby accelerate the oxidation. On the other hand, In sample N, an inert gas is introduced into the furnace to reduce the oxygen partial pressure and thereby inhibit oxidation. The composition of the oxidized layer was determined using a reference intensity ratio (reference intensity ratio, RIR) method, which uses X-ray diffraction. In detail, a sample made by cutting the spring steel wire to a length of about 2 cm and two or three of the cut wires were arranged next to each other. A copper tube was used as an X-ray source, taking into account the depth of penetration of the X-rays into the sample. A wide-angle measurement was using a parallel beam method (where the X-ray irradiation area is a square with sides of about 15 mm) and thus the mass ratio (FeO:Fe O :Fe O in mass%) of the oxides from the 3 4 2 3 Intensity ratios of the diffraction peaks were obtained. The experimental results are shown in Table 3. [Table 3] Composition of the oxidized layer FeO:FeO:FeO Thickness of the oxidized yield 3 4 2 Surface condition Layer (µm) (Mass ratio) (%) 3 L 2.2 3:72:25 Good 88 M 2.2 6:88:6 Good 96 N 2.1 35:60:5 Good 93

[0055] Referring to Table 3, in the sample L obtained by accelerating the oxidation, the Oxidation of Fe O increased more than the percentage of Fe O. On the other hand, in the sample N, which was 2 3 3 4 Suppressing the oxidation, the oxidation of FeO increased less than the percentage of FeO increased. 3 4 Although the surface condition was good in all samples, compared to sample M, the yield in both samples L and N. This can be interpreted as an indication that, although no feeding has yet occurred, a slight adhesion between the spring steel wire and the working tool during the winding process.

[0056] In detail, in sample L with a high percentage of Fe O, the brittle Fe O layer 24 forms on the 2 3 2 3 surface of the oxidized layer 20, which leads to the lowest yield. On the other hand, in sample N with a high Percentage of FeO reduces the yield compared to sample M, although it is better than the yield of sample L with the brittle Fe O layer 24 on the surface of the oxidized layer 20. From the above, 2 3 It can be said that the percentage of Fe O in the oxidized layer is preferably high, and it is, for example, 3 4 preferably not less than 80 mass%. It can also be said that the percentage of Fe O in the oxidized 2 3 layer is preferably low, and for example it is preferably not more than 10 mass%.

[0057] It should be understood that the embodiments and examples disclosed herein are in all respects are illustrative and not restrictive. The scope of the present invention is rather defined by the terms of Claims are defined as the above description and are intended to cover any modifications within the scope and a Meaning equivalent to the terms of the patent claims. List of reference symbols

[0058] 1: spring steel wire; 10: main body; 10A: outer peripheral surface; 20: oxidized layer; 20A: outer peripheral surface; 21: FeO layer; 21A: outer peripheral surface; 22: first FeO layer; 22A: outer peripheral surface; 23: second FeO layer 3 4 3 4 layer; 23A: outer peripheral surface; 24: Fe O layer; 24A: outer peripheral surface; ϕ: diameter of the 2 3 spring steel wire; and t: thickness of the oxidized layer.

Claims

1. Spring steel wire (1), comprising: a main body (10) made of steel and having a linear shape; and an oxidized layer (20) covering an outer peripheral surface (10A) of the main body (10); wherein the steel forming the main body (10) contains not less than 0.5 mass% and not more than 0.7 mass% C, not less than 1 mass% and not more than 2.5 mass% Si, not less than 0.2 mass% and not more than 1 mass% Mn and contains not less than 0.5 mass% and not more than 2 mass% Cr, the remainder being Fe and unavoidable Contaminants are wherein the steel forming the main body (10) has a pearlite structure and the oxidized layer (20) has a thickness (t) of not less than 2 µm and not more than 5 µm and wherein the oxidized layer (20) contains not less than 60 mass% Fe O and a first Fe O layer (22) and a 3 4 3 4 second Fe O layer (23) covering an outer peripheral surface (22A) of the first Fe O layer (22), 3 4 3 4 wherein the first Fe O layer (22) has a higher Si concentration than a Si concentration of the second Fe O layer (23) 3 4 3 4 and a Si concentration of the main body (10).

2. Spring steel wire (1) according to claim 1, in which the oxidized layer (20) further comprises a FeO layer (21) between the first Fe O layer (22) and the main body (10). 3 4 3. Spring steel wire (1) according to claim 2, in which the FeO layer (21) partially covers the outer peripheral surface (10A) of the main body (10) and in a piece of the main body (10) in which its outer peripheral surface (10A) is not covered with the FeO layer (21) the main body (10) and the first Fe O layer (22) are in contact with each other. 3 4 4. Spring steel wire (1) according to at least one of claims 1 to 3, in which the first Fe O layer (22) is a Si- 3 4 Concentration of not less than 2.5 mass% and not more than 6 mass% and a Cr concentration of not less than 1.5 mass% and not more than 3 mass%.

5. Spring steel wire (1) according to at least one of claims 1 to 4, wherein the first Fe O layer (22) has a thickness of 3 4 not less than 0.3 µm and not more than 1.5 µm.

Citation Information

Patent Citations

  • Wire material for an inclined coil spring, inclined coil spring and manufacturing process for it

    DE112017002913T5

  • Oil hardened wires and method of making them

    DE69431200T2

  • Steel wire rod excellent in mechanical descaling

    EP2113580B1

  • Method for production of steel material having excellent scale detachment

    EP2166114B1

  • Air supply unit for pneumatic heat pump

    JP1977000048A