Solvent-free process for the production of lithium-ion batteries

Multifunctional carbon blacks address the limitations of AC in lithium-ion battery manufacturing by enhancing conductivity and mechanical stability, leading to higher energy density and longer-lasting batteries with reduced production time and costs.

DE112023001463T5Pending Publication Date: 2025-01-02CABOT CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
DE112023001463
Authority / Receiving Office
DE · DE
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-03-21
Filing Date
2023-03-17
Publication Date
2025-01-02

AI Technical Summary

Technical Problem

Existing dry manufacturing processes for lithium-ion batteries face issues with components like activated carbon (AC) containing high impurities, leading to irreversible capacity loss, water uptake, and reduced conductivity, which negatively affect battery performance and require high loading levels, limiting active material content and increasing costs.

Method used

The use of multifunctional carbon blacks with specific morphology and surface chemistry to act as fibrillating agents, conductive additives, and mechanical reinforcements, replacing AC, thereby improving electrode conductivity and mechanical stability without the need for high loading levels.

Benefits of technology

The multifunctional carbon blacks enhance electrode performance by reducing binder and additive requirements, increasing active material loading, improving fibrillation, and maintaining uniform distribution, resulting in higher energy density and longer lifespan batteries with reduced manufacturing time and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A solvent-free process uses a multifunctional carbon black to fabricate compositions and electrodes for lithium-ion batteries. The multifunctional carbon black offers two or more desirable properties, such as acting as a conductive carbon additive, a fibrillating agent, and / or a mechanical reinforcement. In one example, an electroactive material, such as graphite or a lithium transition metal compound, a binder, and a multifunctional carbon black are combined in one or more steps. The binder is mixed under high shear in the presence of the multifunctional carbon black. The resulting composition can be formed into a film that can be deposited onto a suitable substrate to fabricate an electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Government support

[0001] This invention was made with government support under award number DE-EE0009109.0000, granted by the Office of Energy Efficiency and Renewable Energy (EERE) of the U.S. Department of Energy. The government holds certain rights to the invention. Related registrations

[0002] This application incorporates, pursuant to 35 USC 119(e), the preliminary US application No. 63 / 322,074, which was filed on March 21, 2022, and is incorporated in full by reference. Background of the invention

[0003] Lithium-ion batteries (LIBs) are widely used sources of electrical energy for numerous applications, ranging from electronic devices to electric vehicles. A lithium-ion battery typically includes a negative electrode and a positive electrode in an arrangement that allows lithium ions and electrons to move to and from the electrodes during charging and discharging. An electrolyte solution in contact with the electrodes forms a conductive medium in which the ions can move. To prevent a direct reaction between the electrodes, an ion-permeable separator is used to physically and electrically isolate them. During operation, electrical contact is established with the electrodes, allowing electrons to flow through the device to deliver electric current and lithium ions to migrate through the electrolyte from one electrode to the other.

[0004] Most commercially available lithium-ion batteries have anodes containing graphite, a material that can intercalate lithium. Typically, lithium is added to the graphite anode during the charging cycle and removed when the battery is used. Other anode materials used in addition to or as an alternative to graphite include lithium titanate, tin oxide, silicon (Si), and SiO₂. x (where x is usually 1.04, 1.06, etc.).

[0005] Cathodes typically comprise a conductive substrate supporting a mixture containing at least one electrochemically active material and a binder. The electroactive material, for example, a lithium transition metal oxide, is capable of absorbing and releasing lithium ions. As with the anode, the binder is used to provide the electrode with mechanical integrity and stability.

[0006] Since the electroactive material and the binder often have poor electrical conductivity or even insulating properties, cathodes often contain an additional component that improves the electrode's electrical conductivity. Conductive additives, such as carbon conductive additives, are also found in LIB anode compositions.

[0007] To manufacture the electrode, the active electrode material, e.g., graphite, is mixed with a binder, usually a polymer or resin. Many existing manufacturing processes use casting techniques based on wet slurries that contain not only the binder but also solvents, plasticizers, and other additives. During manufacturing, the slurry is applied to a conductive substrate or extruded. Since the solvent is detrimental to the final product, it is removed by drying.

[0008] Drying processes, especially those for solvent removal, are time-consuming and slow down the overall production process. They can also increase costs and raise environmental concerns, usually due to the toxicity of the solvent, such as NMP. Regarding the final product, solvent removal during the drying process often leads to binder migration to the electrode surface. While minimal migration may be acceptable in some cases, it is problematic in others. This is particularly true for highly charged electrodes (thick, > 4.5 mAh / cm²). 2 For example, in electrodes, migration is further intensified, leading to delamination and poor electrode performance.

[0009] As a result, "dry" alternatives are being developed that aim to reduce or eliminate the drying step associated with slurry techniques. While dry processes also produce electrodes, which typically contain an electroactive material, a binder, and a conductive additive, they do not require the use of a solvent.

[0010] Dry approaches that have been proposed include high-shear mixing with a fibrillable binder, the use of sacrificial binders that are removed during electrode processing, dry powder spraying, electrostatic spray deposition, cold plasma deposition, sputtering, and powder printing, to name a few. In some cases, a fibrillation promoter is incorporated into the binder, and the resulting formulation is mixed under high shear to fibrillate the binder, creating a tissue-like structure that can better hold the materials together and support the active material.

[0011] The most commonly used additive to promote the fibrillation of binders is activated carbon (AC). AC is generally derived from carbon-containing raw materials such as bamboo, coconut shells, willow peat, wood, coconut fibers, lignite, coal, and petroleum pitch. Activation is achieved through physical or chemical processes known in engineering. For many applications, AC powders are milled to a particle size of a few tens of micrometers (µm) prior to activation. Summary of the invention

[0012] While dry manufacturing processes have the potential to eliminate many of the problems caused by the addition and / or removal of (often harmful) solvents, problems remain.

[0013] For example, current "dry" manufacturing processes use not only the active electrode material but also many other components such as fibrillation promoters, conductive additives, and binders. Since many of these components are not involved in the electrochemical reactions that generate electrical energy, they can negatively affect certain performance characteristics (e.g., capacity and energy density) of the battery because they effectively reduce the amount of active material that can be contained in a given volume.

[0014] Modern fibrillating agents like ACs often contain a high proportion of impurities. The large surface area and oxygen-containing groups typical of ACs also tend to promote significant water absorption. These properties can contribute to irreversible capacity loss and impair battery performance. Furthermore, ACs do not contribute sufficient conductivity, necessitating the addition of more conductive additives to the overall formulation. Even as a simple fibrillation promoter, AC often requires relatively high concentrations (in many cases 5 to 10 wt%), which in itself limits the amount of active material that can be absorbed.

[0015] There is therefore a need for compositions and procedures that solve at least some of the problems associated with existing approaches.

[0016] In general, the invention relates to the use of certain carbon blacks to achieve the necessary improvements in the manufacturing method, the product electrode, and / or the assembled battery. In particular, the invention relates to the use of these materials in connection with dry or solvent-free electrode manufacturing processes.

[0017] The carbon blacks have a selected morphology and / or surface chemistry and can fulfill two or more functions in connection with dry (solvent-free) electrode manufacturing processes. For example, the multifunctional carbon blacks described here can act as fibrillating agents, serve as AC replacements, as conductive carbon additives, and / or as mechanical reinforcement (or, in other words, as bonding agents that impart mechanical strength and flexibility to a product electrode).

[0018] In general, a "multifunctional" carbon black (CB) can be defined as one that effectively deforms or fibrillates a binder used in a solvent-free process, contributes to the electronic / ionic conductivity of the electrode, and / or provides mechanical advantages. In certain cases, a multifunctional CB may be considered capable of fibrillating a fibrillable binder at a loading of no more than 5 wt%. At this loading, the multifunctional CB also acts as a conductive carbon additive, reducing the in-plane resistance of the electrode. In many cases, mechanical advantages are also achieved.

[0019] For many drying processes, the multifunctional CB has a BET value that is no greater than approximately 1600 m. 2 / g, e.g. from about 35 to about 1600 m 2 / g, and an OAN value that is not greater than approximately 650 ml / 100 g, e.g. within a range of 120 to approximately 650 ml / 100 g.

[0020] Other desirable CB properties include high surface roughness (with macroporosity near the particle surface), good electronic conductivity (with a powder resistance of about 1.0 Ohm·cm or less, measured at a compressed density of 0.5 g / cm³). 3 ).

[0021] In addition to the BET and OAN properties mentioned above, many multifunctional CBs that can be used are characterized by one or more of the following features: a surface energy of approximately 15 mJ / m² 2 or less, a microcrystalline planar size according to Raman (La) of at least about 17 Å, a mesopore volume of at least about 0.1 cm³ 3 / g and a macropore volume of at least approximately 0.2 cm³ 3 / g. The total mesopore and macropore volume can be at least approximately 1 cm³ 3 / g.

[0022] For some anode applications, the solvent-free process yields a CB with a BET value of approximately 35 to approximately 1600 m. 2 / g, for example in a range of about 55 to about 200 m 2 / g, and an OAN value of approximately 120 to approximately 650 ml / 100 g, for example in a range of approximately 130 to approximately 240 ml / 100 g, is used. In other examples, the CB has one or more of the following properties: a surface energy of approximately 15 mJ / m². 2 or less, a microcrystalline planar size according to Raman (L a ) of at least approximately 17 Å, a mesopore volume of at least approximately 0.1 cm³ 3 / g (e.g., from about 0.1 to about 0.25 cm 3 / g) and a macropore volume of at least approximately 0.1 cm³ 3 / g (e.g. from about 0.1 to about 0.4 cm 3 / g). The total mesopore and macropore volume can be at least approximately 0.2 cm³ 3 g (e.g. from about 0.2 to about 0.8 cm 3 / g).

[0023] For some cathode applications, a carbon black with a BET value of approximately 35 to approximately 1600 m is used in the solvent-free process. 2 / g, for example, in a range of approximately 500 to approximately 1600, and an OAN value of approximately 120 to approximately 650 ml / 100 g, for example, in a range of approximately 250 to approximately 650 ml / 100 g. In other examples, the CB has one or more of the following properties: a surface energy of approximately 15 mJ / m². 2 or less, a microcrystalline planar size according to Raman (L a ) of at least approximately 17 Å, a mesopore volume of at least approximately 0.1 cm³ 3 / g (e.g. at least about 0.35 cm 3 / g) and a macropore volume of at least approximately 0.2 cm³ 3 / g (e.g. at least about 0.4 cm 3 / g). The total volume of mesopores and macropores can be at least approximately 1 cm³ 3 / g.

[0024] In many embodiments, the process described here is carried out without the addition of liquid (usually a solvent). The ingredients are provided in the form of loose, particulate materials such as free-flowing or pourable powders, flakes, globules, granules, pellets, and so on.

[0025] In some cases, however, it is possible to use small amounts of liquid (e.g., solvent) to perform the procedure described here, usually in a step other than the fibrillation step. When liquid is added, the amount is generally no more than about 10% by weight of the total amount of components used. In many cases, liquid, e.g., solvent, is added in an amount of no more than 1% by weight.

[0026] One aspect of the invention relates to a method for producing an electrode composition. The method comprises combining an active electrode material, a binder, and a multifunctional carbon black, e.g., the multifunctional carbon black described herein, and processing the binder in the presence of the multifunctional carbon black. Many implementations of this method are carried out without the addition of a liquid (usually a solvent).

[0027] In general, the binder can be any semi-crystalline polymer. Accordingly, the process can be carried out with binders that are conventionally considered "fibrillable," as well as with those that are conventionally considered "non-fibrillable"; combinations thereof can also be used.

[0028] In one description, a method for producing an electrode composition comprises: combining an active electrode material, a fibrillable binder, and a multifunctional carbon black, e.g., one with a BET value of no more than about 1600 m. 2 / g and an OAN value of no more than approximately 650 ml / 100 g, and subjecting the binder to a fibrillation process in the presence of the multifunctional carbon black.

[0029] Another aspect of the invention is a method for producing an electrode composition. The method comprises processing a binder (e.g., subjecting the binder to high shear) in the presence of a multifunctional carbon black with properties as described above, and adding an electrodeactive material before, during, or after processing the binder. The binder can be a fibrillable binder, a non-fibrillable binder, or a combination thereof.

[0030] In certain embodiments, the process described here is carried out without the addition of any fibrillating agent other than the multifunctional carbon. In this case, the carbon black used performs all the functionality of the binder processing (e.g., fibrillation) and completely replaces conventional fibrillating agents such as activated carbon. Besides using a binder processing component (e.g., fibrillation component) consisting of multifunctional carbon black as described here, it is also possible to use a binder processing component that consists essentially of or contains the multifunctional carbon black. For example, in some instances, the multifunctional carbon black is used in combination with varying amounts of a conventional fibrillating agent, such as activated carbon.It is also possible to combine a multifunctional CB with another multifunctional CB and / or with a conventional conductive carbon additive (CCA).

[0031] The electroactive material, the binder (e.g., a fibrillable binder), and the multifunctional CB can be combined in a single step, with subsequent processing of the binder (e.g., fibrillation). In other embodiments, the components are combined sequentially. For example, the binder is first processed (e.g., fibrillated) in the presence of the multifunctional additive, followed by a mixing step with the electroactive material. Other sequences are possible. Uniform distribution of the components can be achieved under different (often milder) conditions than those used for processing the binder (e.g., fibrillation). Low-shear mixing techniques can also prevent particle fragmentation and preserve particle size.

[0032] The resulting electrode composition, typically a loose, particulate material such as a free-flowing powder, containing the electroactive material, processed (e.g., fibrillated) binder, multifunctional CB, and optionally other components, can be further processed. For example, the composition can be formed into a free-standing film that can be deposited onto an electrically conductive substrate or support to form an electrode. In one approach, the composition is calendered and laminated onto a conductive film substrate. The calendering process can be performed at or above room temperature, e.g., at a temperature similar to or near the glass transition temperature of the polymer. The lamination step can be performed during or after the composition has been calendered.The resulting product electrode can be assembled into a LIB battery, where one or both electrodes are manufactured using a solvent-free process. In one example, both electrodes are manufactured according to the methods described here.

[0033] Another aspect of the invention is a dry-processed film containing an active electrode material, a commonly processed binder (e.g., fibrillated), and a multifunctional carbon black. Before drying, the dry-processed film has a weight equal to or within 1% by weight of its theoretical weight. The multifunctional carbon black has a BET value of no more than approximately 1600 m. 2 / g and an OAN value of no more than approximately 650 ml / 100 g. In some examples, the multifunctional carbon black also exhibits at least one of the following properties: a surface energy of 15 mJ / m² 2or less, a microcrystalline planar size according to Raman (La) of at least 17 Å, a mesopore volume of at least 0.35 cm³ 3 / g and a macropore volume of at least 0.2 cm³ 3 / g. The total mesopore and macropore volume can be at least approximately 1 cm³ 3 / g.

[0034] In one embodiment, the electrode produced using the techniques described here has an in-plane resistance that is no greater than that of a reference electrode produced using AC.

[0035] The application of embodiments of the invention offers many advantages. For example, the use of a multifunctional CB can reduce the amount of binders and / or conventional processing additives required in the manufacturing process, thereby increasing the potential loading with active materials and leading to electrodes with higher energy density and thus to batteries. The approaches described here can reduce or eliminate the need for ACs. In many cases, smaller amounts of additives are required, increasing the available content of active electrode materials, resulting in batteries with higher energy density and longer lifespan. The multifunctional CB additive can improve binder fibrillation and material distribution across the electrode. Improved adhesion and mechanical stability are further potential advantages.Dry-processed electrodes manufactured with the carbon blacks described here exhibit good charge transfer. The reduction in electrode impedance expected with a multifunctional CB additive can improve cell capacity and charging performance, opening up possibilities for thicker electrodes and batteries with higher energy density and faster charging capability.

[0036] While migration of the binder is often observed in electrodes produced by slurry, the method and composition described here appear to result in a uniform distribution across the electrode. The fibrillated binder holds the electroactive particles (together with the conductive additives) together (cohesion) and simultaneously holds the electrode film layer firmly to the metal substrate (adhesion).

[0037] The solvent-free techniques described here reduce or eliminate the use of harmful solvents such as N-methyl-2-pyrrolidone (NMP) and similar substances. Bypassing the drying step associated with slurry (or other "wet" processes) can simplify and accelerate manufacturing and reduce the footprint of the electrode production line. These advantages, along with the reduction or elimination of the need for solvent recycling or emission control measures, can contribute to overall cost reductions.

[0038] In some embodiments, the dry process can be carried out with a binder that is not normally intended as a fibrillable binder, thereby expanding the production possibilities.

[0039] The above and other features of the invention, including various design details and combinations of parts, as well as other advantages, are now described in more detail with reference to the accompanying drawings and specified in the claims. It is understood that the particular method and apparatus embodying the invention are shown only for illustration and not as a limitation of the invention. The principles and features of this invention can be used in various and numerous embodiments without departing from the scope of the invention. Brief description of the drawings

[0040] In the accompanying drawings, the reference numerals refer to the same parts in the different views. The drawings are not necessarily to scale; instead, the emphasis has been placed on illustrating the principles of the invention. From the drawings: Fig. 1A and Fig. 1B are SEM images (low and high magnification) of the cross-section of a reference electrode (comparison electrode) produced in a dry process using activated carbon (AC); Fig. 1C is a mapping of elemental fluorine via the electrode of Fig. 1A; Fig. 1D and Fig. 1E are SEM images (low and high magnification) of cross-sections of an electrode produced in a dry process using an unmodified CB additive; Fig. 1F is a mapping of elemental fluorine via the electrode of Fig. 1D; Fig. 1G and Fig. 1H are SEM images (low and high magnification) of cross-sections of an electrode produced using a dry process, where the CB used is a heat-treated version of the CB. Fig. 1C and Fig. 1D was; Fig. 1I is a mapping of elemental fluorine via the electrode of Fig. 1G; Fig. Figure 2 shows the in-plane resistance of the electrodes of Fig. 1A and Fig. 1B (Reference); Fig. 1D and Fig. 1E (unmodified CB); and Fig. 1G and Fig. 1H (heat-treated CB); Fig. 3 compares the tensile strength for the freestanding graphite electrode film and the in-plane resistivity for a reference graphite electrode produced by dry process using activated carbon and graphite electrodes produced by dry process using different CB specifications, sorted by BET surface parameter; Fig. 4 compares the tensile strength and modulus of elasticity for a freestanding NCM reference electrode film produced by dry process using activated carbon and NCM electrode films produced by dry process using different CB specifications at a loading of 5 wt.% in the formulation; Fig. 5 compares the tensile strength and modulus of elasticity for freestanding NCM electrode films produced by dry process using various CB specifications at 2 wt% loading in the formulation; Fig. 6 compares the in-plane resistance for an NCM reference electrode produced by a dry process using activated carbon and an NCM electrode produced by a dry process using selected CBs. Fig. 7 compares the tensile strength and modulus of elasticity for freestanding NCM electrode films produced in a dry process using CB specifications with 1 wt% loading in the formulation, where the CB material is in loose and pelletized form. Fig. Figure 8 is a diagram showing the 0.2C, 0.5C, 1C, 2C and 3C discharge capacity of button cells with NCM622 cathodes using the conductive additives disclosed herein. Fig. Figure 9 is a diagram showing the C / 20 discharge capacity of button cells with NCM622 cathodes using the conductive additives disclosed herein. Fig. Figure 10 is a diagram showing the irreversible capacity of the first cycle of button cells with NCM622 cathodes using the conductive additives disclosed herein. Fig. Figure 11 is a diagram showing the cyclic discharge capacity of button half-cells with NCM622 cathode using the conductive additive disclosed herein. Detailed description of preferred embodiments

[0041] The invention is described in more detail below with reference to the accompanying drawings, which illustrate exemplary embodiments of the invention. However, this invention can be embodied in many different forms and should not be interpreted as being limited to the embodiments presented here; rather, these embodiments are provided so that this disclosure is thorough and complete and fully conveys the scope of the invention to the person skilled in the art.

[0042] As used here, the term "and / or" encompasses any and all combinations of one or more of the points listed. Furthermore, all conjunctions used are to be understood in the broadest possible sense. Thus, the word "or" is to be understood as a logical "or" and not as a logical "exclusively or," unless the context clearly requires otherwise. Moreover, the singular forms and the articles "ein," "eine," and "der / die" also include the plural forms, unless explicitly stated otherwise.It is further understood that the terms "contains," "includes," "containing," and / or "comprising," when used in this description, specify the presence of the mentioned features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. Furthermore, it is understood that when an element, including a component or subsystem, is described and / or represented as being connected or coupled to another element, it may be directly connected or coupled to the other element, or there may be intervening elements.

[0043] It is understood that, although terms such as "first" and "second" are used here to describe different elements, these elements should not be restricted by these terms. These terms are used only to distinguish one element from another. Thus, an element discussed below may be referred to as the second element, and similarly, a second element may be referred to as the first element, without this deviating from the teaching of the present invention.

[0044] Unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as they would be commonly understood by a person skilled in the art in the field to which this invention belongs. It is further understood that terms as defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning in the context of the relevant field and that they should not be interpreted in an idealized or overly formal sense unless expressly defined as such herein.

[0045] The invention relates generally to the manufacture of electrodes for electrochemical cells, in many cases for batteries, such as LIBs. In one example, the batteries of interest are rechargeable LIBs.

[0046] Lithium-ion batteries (LIBs) are typically named after the acronyms for the electroactive material used to form the cathode, often an intercalation compound. The embodiments described here can be implemented with or adapted to various types of lithium-ion batteries currently known in the art (such as LCO, LMO, NCM, NCA, LCP, LFP, LFMP, LFSF, or LTS, to name a few), or with LIBs developed in the future.

[0047] Many electrode manufacturing processes for electrochemical cell applications involve the production of an electrode assembly (anode or cathode) that can be applied (coated, extruded, laminated, etc.) to a conductive substrate. In this assembly, the active electrode material is mixed with a binder (e.g., polymers, resins, etc.) that serves to bond and hold the active materials together. Often, liquids for dissolving or carrying the binder, plasticizers, and / or other additives are also included.

[0048] In a conventional solvent-based process, the polymer binder and other components are generally mixed with a suitable liquid to form a slurry, which can then be applied to the substrate. Typically, liquid amounts of at least approximately 40%, based on the total weight of the components used, are employed; many wet processes require even higher amounts of solvent. As the solvent is removed (e.g., during drying), the binder becomes increasingly tacky and adheres to the existing particles and / or the substrate.

[0049] In contrast to slurry-based processes, the embodiments described here employ a "solvent-free" process, also referred to as a "dry" process. In this solvent-free approach, some and usually all of the components (e.g., active material, binder, additives, etc.) required to produce the electrode composition are provided as loose particulate material, such as free-flowing powders, flakes, pellets, globules, etc. The processes described here may include one or more steps for mixing these components (e.g., using a loose particle mixing system) as well as at least one step for processing the binder. For example, if the binder is subjected to certain shear forces, this can lead to deformation of the binder, such as elongation, the formation of binder strands, entanglement, etc.In some types of binders, this is referred to as "fibrillation" of the binder.

[0050] In many aspects of the invention, the components are combined, and the binder is processed, e.g., fibrillated, without the addition of a liquid, e.g., a solvent.

[0051] While most embodiments involve a process carried out without the addition of liquid and entirely solvent-free, in some cases small amounts of liquid, such as solvent, may be used to moisten at least some of the particles to be mixed. This can occur, for example, in the formation of a premix, which is then completely dried before subsequent operations. In one embodiment, any solvent used to form such a premix is ​​removed, for example, by drying, before the binder is deformed. The processing (e.g., fibrillation) of the binder is then carried out with loose, free-flowing, or pourable particles under completely solvent-free conditions.

[0052] Suitable solvents can be selected from those commonly used in LIB production, including but not limited to N-methylpyrrolidone (NMP), acetone, alcohols, and water. The solvent can be removed by standard drying procedures. It is expected that such small amounts of solvent can be completely or almost completely removed.

[0053] In many applications, the amount of solvent used is no more than approximately, and often less than, 1 wt% of the total product electrode composition (a composition containing electroactive material, processed (e.g., fibrillated) binder, and other components, e.g., an additive component). To illustrate, the amount of solvent used ranges from approximately 0 to a maximum of 1 wt%, such as approximately 0 to approximately 0.2, to approximately 0.4, to approximately 0.6, to approximately 0.8 wt%; or from approximately 0.2 to approximately 0.4, to approximately 0.6, to approximately 0.8, to approximately 1 wt%; or from approximately 0.2 to approximately 0.4, to approximately 0.6, to approximately 0.8, to approximately 1 wt%; or from approximately 0.4 to approximately 0.6, to approximately 0.8, to approximately 1 wt%. or from approximately 0.6 to approximately 0.8, to approximately 1.0 wt%; or from approximately 0.8 to approximately 1 wt%, based on the total weight of the ingredients used.

[0054] In other situations, the solvent can be added in amounts within a range of about 0 to about 10 wt%, for example, within a range of about 0 to about 2, to about 4, to about 6 to about 8 wt%; or from about 2 to about 4, to about 6, to about 8, to about 10 wt%; or from about 4 to about 6, to about 8 to about 10 wt%; or from about 6 to about 8, to about 10 wt%; or from about 8 to about 10 wt%.

[0055] While the ingredients can be mixed and the binder processed, e.g., fibrillated, without the use of a solvent, some electrode manufacturing processes use a small amount of solvent in a post-processing step (a process that takes place after the dry electrode composition has been formed) to "moisten" a product film, e.g., during calendering. Such a process is also referred to here as a "dry" process.

[0056] Finished products, e.g., electrodes, freestanding films, or films laminated onto the current collector, produced using the solvent-free or dry process described herein, are identifiable by the fact that they contain no detectable processing solvents or solvent residues. In contrast, a product produced using a wet process (slurry) typically contains detectable solvents and / or solvent residues. Another approach expects electrode products or films produced according to embodiments of the invention to exhibit a uniform or substantially uniform distribution of the binder over the electrode or film thickness; generally, less uniformity is observed with wet processes, often resulting in binder migration towards the film surface.

[0057] The solvent-free process described here uses the following components: an electroactive component (a material or combination of materials that participates in the electrochemical charge / discharge reactions of an electrochemical cell, such as through absorption or desorption of lithium); a binder, which may be a fibrillable or non-fibrillable binder; and a multifunctional carbon black (CB). In some cases, additional components may be included.

[0058] In many LIB anodes, the electroactive material (here also referred to as "active electrode material" or simply "active material" or "AM") is graphite, e.g., natural graphite, synthetic graphite (e.g., massive synthetic graphite (MAG)), or mixtures of both. Mesocarbon microspheres (MCMB), carbon fibers on mesophase pitch (MCF), and gas-phase grown carbon fibers (VGCF) can also be used. In other embodiments, the active anode compound comprises, consists substantially of, or is composed of silicon, such as silicon-graphite composites, graphite with nanosilicon (Si), or SiO₂. x Particles.

[0059] The principles described here can also be used with other active anode materials, such as those already known, currently being researched, or those to be developed in the future. Examples include, but are not limited to: (a) intercalation / deintercalation materials (e.g., carbon-based materials, porous carbon, graphene, TiO2, Li4Ti5O) 12 , etc.); (b) Alloying / dealloying materials (e.g. Si, SiO) x , doped Si, Ge, Sn, Al, Bi, SnO2 , etc.); and (c) conversion materials (e.g., transition metal oxides (Mn x O y , NiO, Fe x O y , CuO, Cu2O, MoO2, etc.), metal sulfides, metal phosphides and metal nitrides, represented by the formula M x X y , with X = S, P, N)).

[0060] The amount of active anode material can vary depending on the type of energy storage device. In illustrative examples, the amount of active anode material (e.g., graphite) is at least 80 wt.%, e.g., at least 85, at least 90, at least 95, or at least 99 wt.%, based on the total weight of the (dry) electrode composition. The active anode material, e.g., graphite, can be provided in an amount of approximately 80 to approximately 85, 90, 93, 96, or 99 wt.%; or from approximately 85 to approximately 90, 93, 96, or 99 wt.%; or from approximately 90 to approximately 93, 96, or 99 wt.%; or from approximately 93 to approximately 96 or 99 wt.%; or from approximately 96 to approximately 99 wt.%.

[0061] In the dry process for the production of LIB cathodes, LCO (lithium cobalt oxide), LMO (lithium manganese oxide), NCM (lithium nickel cobalt manganese oxide), NCA (lithium nickel cobalt aluminum oxide), LCP (lithium cobalt phosphate), LFP (lithium iron phosphate), LMFP (lithium manganese iron phosphate), LFSF (lithium iron fluorosulfate), and LTS (lithium titanium sulfide) can be used. Materials such as these are generally referred to here as "lithium transition metal compounds," e.g., "lithium transition metal oxides." In addition to cathode materials based on intercalation chemistry, e.g.,... B. where chemical reactions usually take place in which a single electron is transferred, other types of cathode materials (e.g. with lithium ions inserted into FeF3) can transfer multiple electrons through more complex reaction mechanisms, the so-called conversion reactions.Other active cathode materials known in the field of technology or developed in the future can also be used.

[0062] In some embodiments, NCM (also referred to as "NMC") or NCA cathode compositions are used for the dry process described here. These materials are generally known to those skilled in the art. Furthermore, many battery-compatible formulations in powder form (such as NCM 622) are commercially available.

[0063] In detail, NCM can be defined by the formula Li 1+x (Ni y Co 1-y-z Mn z ) 1-x O2 can be represented, where x is in the range of 0 to 1, y is in the range of 0 to 1 (e.g., 0.3–0.8), and z is in the range of 0 to 1 (e.g., 0.1–0.3). Examples of NCMs are Li 1+x (Ni 0.33 CO 0.33 Mn 0.33 ) 1-x O2, Li 1+x (Ni 0.4 Co 0.3 Mn 0.3 ) 1-x O2, Li 1+x (Ni 0.4Co 0.2 Mn 0.4 ) 1-x O2, Li 1+x (Ni 0.4 Co 0.1 Mn 0.5 ) 1-x O2, Li 1+x (Ni 0.5 Co 0.1 Mn 0.4 ) 1-x O2, Li 1+x (Ni 0.5 Co 0.3 Mn 0.2 ) 1-x O2, Li 1+x (Ni 0.5 Co 0.2 Mn 0.3 ) 1-x O2, Li 1+x (Ni 0.6 Co 0.2 Mn 0.2 ) 1-x O2, Li 1+x (Ni 0.8 Co 0.1 Mn 0.1 ) 1-x O2 and Li1+x(Ni0.9C0.05Mn0.05)1-xO2.

[0064] NCA can be expressed by the formula Li 1+x (Ni y Co 1-y-z Al z ) 1-x O2 can be represented, where x, y, and z are in the range of 0 to 1. An example of an NCA is Li. 1+x (Ni 0.8 Co 0.15 Al 0.05 ) 1-x O2.

[0065] The amount of electroactive cathode material used can vary depending on the type of energy storage device. In illustrative examples, the amount of NCM or NCA is at least 90 wt%, e.g., at least 93%, at least 96%, at least 98%, or at least 99 wt%, based on the total weight of the (dry) electrode composition. NCM or NCA can be provided in amounts ranging from approximately 90% to approximately 93%, 96%, or 99 wt%; or from approximately 93% to approximately 96% or 99 wt%; or from approximately 96% to approximately 99 wt%.

[0066] In addition to the active material, a binder is used in the dry process described here. Generally, the binder can be any semi-crystalline polymer.

[0067] In some embodiments, the binder is a fibrillable binder. The fibrillable binder may be provided in a binder component that consists of, is substantially composed of, or comprises the fibrillable binder.

[0068] Under certain processing conditions, such as mixing under high shear forces in the presence of a fibrillating agent, a fibrillable binder is capable of generating fibrils that form a network capable of connecting and supporting other particles present in the formulation. Specifically, fibrillation of the binder is thought to create a matrix, lattice, or network of fibrils, imparting mechanical structure to the electrode. In a product electrode, a fibrillated binder can be detected in SEM images, which show the presence of fibrils wrapped around at least some of the particles present, such as the active material particles. Other indirect techniques that can be used to assess the relative degree of fibrillation of the binder include, for example, energy-dispersive X-ray spectroscopy (EDX), powder rheology, and tensile strength.EDX allows for the mapping of the fluorine distribution throughout the dry electrode and the evaluation of the effectiveness of binder fibrillation. Powder rheology measures the cohesive interaction between particles in the free-flowing electrode powder mixture, while tensile strength testing measures the strength of the free-standing electrode film; both are representative of the degree of binder fibrillation. In some cases, poor or nonexistent fibrillation can be inferred from dry product electrode films that crumble or detach from the substrate.

[0069] In some embodiments, the fibrillable binder is a fibrillable fluoropolymer, such as polytetrafluoroethylene or PTFE. Other binders that may be considered fibrillable include, but are not limited to, ultra-high molecular weight polypropylene, polyethylene and copolymers, and any combination thereof.

[0070] The fibrillable binder (alone or as part of a binder component (e.g., in a polymer mixture)) can be provided in an amount of approximately 1 to approximately 10 wt%, e.g., approximately 1-2, 2-3, 3-4, 4-5, 5-6, 6-7, 7-8, 8-9, 9-10 wt%. In one example, the fibrillable binder is provided in an amount of approximately 5 wt%. In other examples, the fibrillable binder is provided in an amount within a range of approximately 1 to: approximately 2, approximately 3, approximately 4, approximately 5, approximately 6, approximately 7, approximately 8, approximately 9 wt%; or from approximately 2 to: approximately 3, approximately 4, approximately 5, approximately 6, approximately 7, approximately 8, approximately 9, approximately 10 wt%. or from about 3 to: about 4, about 5, about 6, about 7, about 8, about 9, about 10 wt.%; or from about 4 to: about 5, about 6, about 7, about 8, about 9, about 10 wt.%; or from about 5 to: about 6, about 7, about 8, about 9, about 10; or from about 6 to: about 7, about 8, about 9, about 10 wt.%; or from about 7 to: about 8, about 9, about 10 wt.%%; or from about 8 to about 9, about 10 wt.%.

[0071] However, a fibrillable binder is not used in all situations. Therefore, in some embodiments of the invention, a binder component is used that consists of, is substantially composed of, or comprises one or more non-fibrillable binders. As used herein, the term "non-fibrillable" binder refers to a binder that is difficult to fibrill under the same conditions sufficient for the fibrillation of a "fibrillable" binder. Nevertheless, a non-fibrillable binder can be deformed, e.g., stretched, elongated, twisted, etc., often to a considerable extent, even without complete fibrillation, by applying aspects of the invention (under the same or substantially the same processing conditions used for a fibrillable counterpart).

[0072] Without being bound to any particular interpretation or mechanism, fibrillation can be considered an extreme phenomenon in which the binder polymer (starting as a colloidal particle) is stretched to a very thin thickness, forming very long (high aspect ratio) strands (ribbons) capable of bridging more than two electroactive particles and thus holding them together. The embodiments described here can also result in a non-fibrillable binder being stretched and / or entangled, creating CB-binder composites and / or being coated with CB. Even if not fully fibrillated, such a "processed" non-fibrillable binder can still act as an adhesive, bonding and binding the electroactive particles together, thus ensuring adhesion to the current collector.Deformations of a non-fibrillable binder can be observed using at least some of the techniques mentioned above.

[0073] In one example, the non-fibrillable binder is a fluoropolymer such as polyvinylidene fluoride (PVDF). Other examples of binders that can be considered non-fibrillable include poly(vinyldifluoroethylene-co-hexafluoropropylene) (PVDF-HFP), polyimides, and water-soluble binders such as poly(ethylene) oxide, polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyvinyl acetate, polyethylene-co-vinyl acetate, some polyolefins, cellulose, and cellulose derivatives, to name just a few. Other possible non-fibrillable binders include polyethylene and polypropylene (except ultra-high molecular weight), ethylene propylene diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber, as well as copolymers and mixtures thereof. In one example, the non-fibrillable binder is a cellulose ester, a cellulose ether, cellulose nitrate, a carboxyalkylcellulose, a cellulose salt, and a cellulose salt derivative.In some embodiments, the microparticle-shaped, non-fibrillable binder is selected from at least one of cellulose, cellulose acetate, methylcellulose, ethylcellulose, hydroxypropylcellulose (HPC), hydroxyethylcellulose (HEC), cellulose nitrate, carboxymethylcellulose (CMC), carboxyethylcellulose, carboxypropylcellulose, carboxyisopropylcellulose, sodium cellulose, sodium cellulose nitrate, and sodium carboxyalkylcellulose. Other examples employ combinations of a non-fibrillable binder, e.g., PVDF, and a non-fibrillable binder, e.g., PTFE.

[0074] The amounts of non-fibrillable binders that can be used are the same or similar to those used for fibrillable binders. Other suitable amounts can be determined, for example, through routine testing.

[0075] Fibrillable binders can also be used in combination with non-fibrillable binders.

[0076] Electrode compositions typically contain components such as conductive additives (e.g., conductive carbon additives or CCA), plasticizers, etc. In the case of solvent-free processes, common techniques require a binder for fibrillation (also called a "fibrillazing agent") or an auxiliary agent, usually AC.

[0077] It has been discovered that conventional fibrillating additives (e.g., AC) can be supplemented and often completely replaced by a CB material, which offers several advantages. Certain carbon blacks, for example, can serve as fibrillating (or in some cases, deforming) binders, as conductive additives (to create conductive networks, e.g., long-range conductivity of the electrode), and as mechanical reinforcing aids (providing mechanical support, stability, and / or flexibility to the electrode product, often the coating, layer, or film commonly applied to the conductive substrate to form a battery electrode).

[0078] In general, CBs are materials that exist as aggregates, which in turn are formed from CB primary particles. In most cases, the primary particles do not exist independently of the CB aggregate. While the primary particles can have a mean diameter ranging from about 10 nanometers (nm) to about 50 nm, e.g., from about 10 nm to about 15 nm; from about 10 nm to about 20 nm; from about 10 nm to about 25 nm; from about 10 nm to about 30 nm; or from about 10 nm to about 40 nm, the aggregates can be considerably larger. CB aggregates have fractal geometries and are often referred to in the scientific community as CB "particles" (not to be confused with the "primary particles" mentioned above).

[0079] Many types of carbon monoxide (CBs) are produced in a furnace reactor by pyrolysis of a hydrocarbon feedstock (FS) with hot combustion gases to generate combustion products containing particulate CBs. The properties of a particular CB often depend on the production conditions and can be altered or modified by changes in temperature, pressure, FS, residence time, quench temperature, throughput, and / or other parameters.

[0080] As is well known in the field, CBs can be described by specific properties that are determined according to established procedures, often standardized protocols. For example, CBs can be characterized by their Brunauer-Emmett-Teller (BET) surface area, measured, for example, according to ASTM D 6556-10; by their oil adsorption capacity (OAN), determined, for example, according to ASTM D 2414-16; and by their statistical thickness surface areas (STSAs), a property that can be determined according to ASTM D 6556-10.

[0081] For a particular CB, it may also be of interest in some cases to specify the ratio of its STSA to its BET surface area (STSA:BET ratio).

[0082] The crystalline regions of CBs can be traversed by an L a Crystallite size is characterized and determined by Raman spectroscopy. L ais defined as 43.5 x (area of ​​the G-band / area of ​​the D-band). The crystallite size can provide an indication of the degree of graphitization, with a higher L a The value correlates with a higher degree of graphitization. The Raman measurements of L a These findings are based on Gruber et al., “Raman studies of heattreated carbon blacks”, Carbon Vol. 32 (7), pp. 1377–1382, 1994, which is referenced here. The Raman spectrum of carbon contains two large “resonance” bands at approximately 1340 cm⁻¹. -1 and 1580 cm -1 , which are referred to as the "D" and "G" bands. It is generally assumed that the D-band corresponds to the unordered sp 2 Carbon and the G-band correspond to the graphitic or “ordered” sp 2 to be assigned to carbon. Using an empirical approach, the ratio of the G / D bands and an L measured by X-ray diffraction (XRD) are ahighly correlated, and a regression analysis reveals the empirical relationship: La=43.5×(area of ​​the G band / area of ​​the D band), where L a is calculated in Angstroms. A higher L a The value therefore corresponds to a more ordered crystalline structure.

[0083] The crystalline domains can be divided by an L c Crystallite size can be characterized. The L cCrystallite size was determined by X-ray diffraction using an X-ray diffractometer (PANalytical X'Pert Pro, PANalytical BV) with a copper tube, a tube voltage of 45 kV, and a tube current of 40 mA. A sample of soot particles was packed into a sample holder (an accessory of the diffractometer), and the measurement was performed over an angular range (2θ) from 10° to 80° at a rate of 0.14° / min. The peak positions and the full width at half maximum (FWHM) were calculated using the diffractometer software. Lanthanum hexaboride (LaB6) was used as an X-ray standard to calibrate the measurement angle. The crystallite size L was determined from the obtained measurements. c Determined using the Scherrer equation: L c (Å) = K*λ / (β*cosθ), where K is the form factor constant (0,9); λ is the wavelength of the characteristic X-ray line of Cu K α1(1.54056 Å); β is the peak width at half the maximum in radians; and θ is determined by taking half the measurement angle peak position (2θ).

[0084] The cleanliness of the surface can be described by the surface energy (SEP) of the CB, a property that can be determined by dynamic vapor (water) sorption (DVS) or water spreading pressure (e.g., described in US Patent No. 10,886,535 B2, issued on January 5, 2021, to Korchev et al. and incorporated herein by reference).

[0085] The mean pore diameter and pore volume can be determined in accordance with the techniques described in EP Barrett, LG Joyner, PP Halenda, J. Am. Chem. Soc. 1951, 73, 373-380 (BJH method).

[0086] Other techniques that can be used to investigate carbon atoms include Fourier-transform infrared spectroscopy (FTIR), thermogravimetric analysis (TGA), X-ray photoelectron spectroscopy (XPS), scanning electron microscopy (SEM), and transmission electron microscopy (TEM). FTIR spectroscopy is particularly useful for determining the nature of the functional surface groups, while SEM / TEM techniques help to illustrate the size and morphology of the particles. XPS is frequently used to determine the elemental composition of a material, and TGA can provide information about the decomposition and oxidation properties of carbon atoms.

[0087] Tables 1A and 1B below show the physical properties of illustrative CBs, namely CB1 to CB17. Table 1A Probe BET SA, m / g 2 STSA, m / g 2 OAN, mL / 100 g SEP mJ / m 2 La Raman, Å (IG / (IG+ID)) Lc XRD, Å % Cr Raman CB1 36 35 125 k.A. k.A. k.A. k.A. CB2 59 59 220 4 26,1 37,5 19,7 CB3 100 100 231 2,6 27,1 39,6 20,1 CB4 131 97 230 28 13 23 k.A. CB5 134 136 311 3,3 43,5 44,2 22,4 CB6 169 144 155 10,2 26,4 37,7 18,8 CB7 541 254 225 25,9 k.A. k.A. k.A. CB8 717 182 249 15 k.A. k.A. k.A. CB9 855 k.A. 280 6,7 25,5 37 k.A. CB10 1055 317 278 11 17,2 28,3 k.A. CB11 1389 423 328 14,7 17 28,1 k.A. CB12 1491 507 k.A. 12,5 k.A. k.A. k.A. CB13 1388 1330 490 6,7 22,8 34,4 k.A. CB14 1420 585 330 13,4 17,7 28,7 13,5 CB15 1430 1415 605 2,5 20,9 32,4 12,8 CB16 1420 389 181 13 k.A. k.A. 12,5 CB17 60 60 230 10 19 k.A. k.A. Table 1B Probe Pore ​​volume (cm 3 / g) according to BJH (pore size < 2 nm) Pore ​​volume (cm 3 / g) according to BJH (Porengröße 2nm-50nm) Pore ​​volume (cm 3 / g) nach BJH (Porengröße >50nm) Total pore volume (cm³) 3 / G) CB1 k.A. k.A. k.A. k.A. CB2 k.A. k.A. k.A. k.A. CB3 0,003 0,15 0,21 0,36 CB4 k.A. 0,1 0,15 0,26 CB5 k.A. k.A. k.A. k.A. CB6 0,004 0,21 0,36 0,57 CB7 0,008 0,32 0,56 0,89 CB8 0,005 0,25 0,35 0,61 CB9 0,015 0,66 1,54 2,21 CB10 0,013 0,43 1,2 1,6 CB11 0,02 1,07 0,93 2,02 CB12 0,028 0,49 0,64 1,15 CB13 0,03 1,48 1,4 2,91 CB14 0,024 0,85 1,61 2,48 CB15 k.A. 1,47 0,4 2,22 CB16 0,01 0,94 0,17 1,12 CB17 k.A. k.A. k.A. k.A.

[0088] Various carbon compounds (CBs) have been and are being developed for applications as conductive carbon additives (CCAs). Attractive electrical conductivity is often combined with a high specific surface area and a pronounced structure (the arrangement of the primary CB particles within an aggregate) and porosity. CBs that can be added to anode and / or cathode compositions for lithium-ion batteries (LIBs) produced by a slurry process are described, for example, in the international publications WO 2020 / 197670 and WO 2020 / 197673, both published to Cabot Corp. on October 1, 2020. Both are incorporated herein in full by reference.

[0089] Examples of commercially available CBs that can be effective as CCAs are the soot particles LITX® 50, LITX® 63, LITX® 66, LITX® 200, LITX® 300, LITX® HP and LITX® MAX 90 available from Cabot Corporation; the products C-NERGY™ C45, C-NERGY™ C65 and SUPER P® from Imerys, the products Li-400, Li-250, Li-100 and Li-435 from Denka, and the products EC300 and EC600 from Ketjen.

[0090] In addition to electrical conductivity, which is desirable for LIB applications, other properties that contribute to the multifunctionality of a CB may include one, several, or all of the following: surface roughness, surface chemistry (surface energy), particle strength, and particle size.

[0091] Typically, CB surface roughness is related to particle porosity, which is described, for example, by pore volume or pore size distribution. RMS surface roughness (calculated as the root mean square of the measured microscopic peaks and valleys of a surface) is known to correlate with surface pore size (e.g., on a similar order of magnitude). For example, 2 nm pores may indicate an approximate RMS surface roughness of 1 nm.

[0092] In general, CB porosity can fall into one or more of the following categories: microporosity, defined by pores with a diameter of less than 2 nm; mesoporosity, defined by pores with a diameter between 2 and 50 nm; and macroporosity, defined by pores with a diameter of more than 50 nm.

[0093] The pore size distribution and pore volume of carbon black can be determined using gas physisorption methods such as nitrogen adsorption porosimetry. This involves measuring nitrogen gas adsorption using BET analysis, followed by fitting the adsorption isotherms with various models, such as DFT (density function theory) and the BJH (Barrett-Joyner-Halenda) model, depending on the pore size range of interest. The BJH adsorption model was used to fit the N₂ adsorption isotherm and to calculate the meso- and macropore volumes presented here.

[0094] Without wishing to be bound to a specific interpretation, it is assumed that the fibrillating properties in multifunctional CBs are at least partially determined by the macroporosity of the particle, with the macropores serving as anchoring points for the interlocking of the binder on the CB surface and stretching the binder into fibrils when high shear forces are applied.

[0095] While some carbon blacks are predominantly microporous materials, there are techniques to increase porosity and / or to produce carbon blacks with tailored porosity types.

[0096] Contact of a carbon black feedstock with an oxidizing agent stream can, for example, increase the porosity, particularly the mesoporous character, of the carbon black product. Increasing the porosity of furnace blacks can be achieved by extending the residence time in the soot reactor, thus allowing the exhaust gas more time to attack and etch the carbon surface. Another method involves adding alkaline earth metal ions to the soot feedstock, as these ions are known to catalyze the etching of the soot by the exhaust gas. Both methods involve in-situ etching of the carbon black, i.e., within the furnace reactor during production, to produce soot with internal porosity. Some approaches that can be used to modify carbon blacks are described, for example, in US Patent Nos. 8,895,142 B2, to Kyrlidis et al., and 10,087,330 B2, to Green et al., both of which are incorporated herein by reference.Commercially available modified carbon blacks that can be used are available from Cabot Corporation. In Tables 1A and 1B above, CB 15 is the steam-etched version of CB4.

[0097] It has been found that fibrillation properties also depend on surface chemistry or activity, a function often related to the manufacturing and / or heating process used in the production of a particular CB. In many cases, surface chemistry or activity is associated with oxygen-containing groups on the CB surface. In some cases, well-fibrillating CB candidates lack oxygen-containing surface groups or are depleted of them, so they tend to be less hydrophilic (more hydrophobic).

[0098] For example, it is assumed that effective fibrillation is driven at least partially by the affinity (adhesion) of the carbon binder (CB) to the binder, e.g., a fibrillable binder. Thus, in one application, the preferred multifunctional CBs for successful fibrillation of a binder such as PTFE are hydrophobic CBs (i.e., CBs lacking oxygen-containing surface groups) and / or CBs with low surface energy. The oxygen content can be measured by inert gas fusion. CBs with low surface chemistry have an oxygen content in the range of approximately 10 ppm to approximately 5000 ppm, e.g., from approximately 100 ppm to approximately 1000 ppm.

[0099] The presence of oxygen-containing surface groups can be reduced or minimized by techniques such as heat treatment or other surface modification processes, as are known in the industry or may be developed in the future. Surface-modified, e.g., heat-treated carbon blacks (CBs) can be compared with and distinguished from ordinary carbon blacks by X-ray scattering, Raman spectroscopy, surface energy measurements by gas adsorption, or other known methods. In some cases, heat-treated and other surface-modified CBs also tend to exhibit lower moisture absorption during processing. In Tables 1A and 1B, CB9 is a heat-treated version of CB11, while CB3 is a heat-treated version of CB4.

[0100] Other CB properties to consider for multifunctional CB candidates relate to their physical shape. For example, CB particle size is a property that can be determined using particle size distribution (PSD) techniques and / or scanning electron microscopy (SEM). The strength of the CB particles (represented as particle hardness and / or particle cohesion) also likely plays a role in the multifunctional nature of the selected CB. Particle strength enables the CB to effectively stretch the polymer binder; together with particle roughness, this can represent very important mechanical properties for achieving the desired fibrillation of the binder. Particle strength can be measured by an individual pellet crash test, oscillatory viscoelastic measurements, or other methods known in the industry.

[0101] Initially (before the CB was mixed, particularly under high shear), the D50 particle size of the multifunctional CB used can range from approximately 0.5 to approximately 20 µm, e.g., from approximately 1 to approximately 10 µm, or from approximately 2 to approximately 5 µm. As a result of binder processing, e.g., fibrillation (usually under high shear conditions), the initial multifunctional CB particles can break down into smaller particles, which may have a particle size in the range of approximately 0.05 to approximately 1 µm, e.g., from approximately 0.1 to approximately 0.3 µm.

[0102] A multifunctional CB can be combined with a second CB (which may or may not be multifunctional), e.g. in a CB mixture.

[0103] The CB particle material can be supplied in any number of forms. Very loose CB-containing powders, for example, have proven particularly effective in some of the dry processes tested. Such powdered materials can be characterized by their particle size, BET, and / or other properties. In many cases, the powders used have a density of no more than approximately 100 g / cm³. 3 .

[0104] Less loose CB particles, e.g., in the form of jet-milled pellets, can also be used. CB powders can be pelletized using established techniques and equipment. In one example, CB is pelletized with an emulsion solution of the binder used to prepare the electrode composition described here. Other approaches use an emulsion solution of a different binder, e.g., a binder belonging to the same chemical family or possessing similar functionally active groups that can combine or otherwise interact with the binder used to carry out the drying process. It is assumed that this increases the energetic interaction of the pelletized CB with the binder used to prepare the electrode composition.

[0105] The pellet size for pure CB can range from approximately 0.1 mm to approximately 5 mm. For example, the pellet size could be from approximately 0.1 mm to approximately: 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 mm; or from approximately 0.5 mm to approximately: 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 mm; or from approximately 1 to approximately: 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 mm; or from approximately 1.5 mm to approximately: 2, 2.5, 3, 3.5, 4, 4.5, 5 mm; or from approximately 2 mm to approximately: 2.5, 3, 3.5, 4, 4.5, 5 mm. or from about 2.5 to about: 3, 3.5, 4, 4.5, 5 mm; or from about 3 to about 3.5, 4, 4.5, 5 mm; or from about 3.5 to about: 4, 4.5, 5 mm; or from about 4 to about: 4.5, 5 mm; or from about 4.5 to about 5 mm.

[0106] Carbon black granules can also be useful in certain situations. In many cases, carbon black granules are a dense form of carbon black, without the polymer content of the final product. Generally, carbon black granules can be produced using a conventional pelletizing process associated with carbon black production. It is also possible to produce carbon black granules by dispersing loose carbon black in water and then spray-drying.

[0107] In some embodiments, the granules used change their shape and / or function during the solvent-free processes described here. For example, an initial CB granule can be used to process a polymeric binder, such as fibrillate. The comminution that occurs during this process can release smaller CB units. In the presence of an electroactive material, the fragmentation of the granule can improve the distribution of the smaller CB units in the electrode composition, resulting in electrode films with improved electrical conductivity and / or mechanical strength.

[0108] The surface roughness and / or surface energy of the granules is often controlled by the selection of the particles that comprise the granules. For example, the surface roughness can be chosen based on the surface texture created by the primary particles and / or aggregates that make up the secondary granules. Such a surface is rough on a dimensional level where the roughness is created by bumps and valleys in the nano / micro range on the surface of the CB granules.

[0109] A multifunctional CB in granular form can have a particle size in the micrometer range, e.g., 1-10 µm, such as: from about 1 to about 2, 3, 4, 5, 6, 7, 8, 9 µm; or from about 2 to about 3, 4, 5, 6, 7, 8, 9, 10 µm; or from about 3 to about 4, 5, 6, 7, 8, 9, 10 µm; or from about 4 to about 5, 6, 7, 8, 9, 10 µm; or from about 5 to about 6, 7, 8, 9, 10 µm; or from about 6 to about 7, 8, 9, 10 µm; or from approximately 7 to approximately 8, 9, 10 µm; or from approximately 8 to approximately 9, 10 µm; or from approximately 9 to approximately 10 µm. For some granules, the original size can be reduced to various grades by milling, e.g., from approximately 10 micrometers to less than 1 micrometer. A combination of sizes is used in some applications.

[0110] The strength of the granules can also be taken into account. It can be minimized by forming the granules without (or with a minimal content of) binder during granule formation; higher granule strength can be achieved by using different concentrations of binders and / or different types of binders. In some embodiments, the binder used to form the CB granules is the same or a similar binder to the binder used in the dry process, e.g., a fibrillable binder.

[0111] Some embodiments use granules that become brittle during processing, e.g., during fibrillation. In such cases, the strength of the granules can be controlled so that it is high enough to fibrillate or deform the polymeric binder, and low enough to cause the granules to break apart and release conductive and reinforcing carbon units, such as aggregates.

[0112] The granulated CB can be used as a multifunctional additive alone or in combination with another form of CB, which in some cases may also be multifunctional.

[0113] The binder (CB) used in the dry processes described here is selected or tailored to fulfill two or more functions. In certain embodiments, various CB attributes are matched to achieve the best possible combination of electrical conductivity, binder fibrillation, and / or mechanical properties. A CB considered an excellent CCA additive may not necessarily prove to be a good or even adequate fibrillation aid. Therefore, a selection process, and sometimes a trade-off, may be necessary to use a CB that exhibits good electrical conductivity along with good fibrillation properties. Achieving or optimizing the multifunctional character of a CB may rely on experimental evaluations testing the performance of films and / or electrodes produced using a solvent-free process.Suitable CBs can also be selected taking into account their properties, e.g. in relation to a specific drying process protocol or specific conditions.

[0114] In one example, the CB is selected to combine a sufficient surface area (e.g., measured by BET N2 adsorption) for optimal binder processing, e.g., fibrillation, while simultaneously ensuring that the specific CB agglomerates used (e.g., CB pellets or CB particles from the jet mill) can break down into particles small enough, e.g., less than 2 micrometers (µm), to maximize surface interactions between CB particles and binder, thus effectively processing the binder, e.g., fibrillating it.

[0115] The CB used in the dry process described here can have a BET value not greater than approximately 1600 m 2 / g is, for example, not larger than approximately: 1500, 1400, 1300, 1200, 1100, 1000, 900, 800, 700, 600, 500, 400, 300, 200, 100 or 35 m 2 / g. The BET value can range from approximately 35 to approximately 1600, such as from approximately 35 to approximately: 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500; or from approximately 100 to approximately: 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 200 to about: 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 300 to about: 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 400 to about: 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 500 to about: 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 600 to about: 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 700 to about 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 800 to about: 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600;or from about 900 to about: 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 1000 to about: 1100, 1200, 1300, 1400, 1500, 1600; or from about 1100 to about: 1200, 1300, 1400, 1500, 1600; or from about 1200 to about: 1300, 1400, 1500, 1600; or from about 1300 to about 1400, 1500, 1600; or from about 1400 to about: 1500 m; 2 / g, 1600; or from about 1500 to about 1600.

[0116] The CB used in the dry process described here can have an OAN value of no more than approximately 650 ml / 100 g, e.g., no more than approximately 600, no more than approximately 500, no more than approximately 400, no more than approximately 300, no more than approximately 250, no more than approximately 200, no more than approximately 150, no more than approximately 120 ml / 100 g. The multifunctional CB can have an OAN value in the range of approximately 120 to approximately 650 ml / 100 g, e.g., from approximately 120 to approximately 200, to approximately 300, to approximately 400, to approximately 500, to approximately 600, to approximately 650 ml / 100 g. or from about 200 to about 300, to about 400, to about 500, to about 600, to about 650 ml / 100 g; or from about 300 to about 400, to about 500, to about 600, to about 650 ml / 100 g; or from about 400 to about 500, or to about 600, to about 650 ml / 100 g; or from about 500 to about 600, to about 650 ml / 100 g; or from about 600 to about 650 ml / 100 g.

[0117] LIB anodes can be manufactured using a dry process with a CB whose BET value is no greater than approximately 1600 m. 2 / g, such as not greater than approximately 1500, not greater than approximately 1200, not greater than approximately 1000, not greater than approximately 700, not greater than approximately 500, not greater than approximately 200, not greater than approximately 100 or not greater than approximately 35 m 2 / g. The BET value can range from approximately 35 to approximately 1600 m. 2 / g. For example, the BET value can range from approximately 35 to approximately 50, to approximately 75, to approximately 100, to approximately 150, to approximately 200; or from approximately 50 to approximately 75, to approximately 100, to approximately 150, to approximately 200; or from approximately 75 to approximately 100, to approximately 150, to approximately 200; or from approximately 100 to approximately 150, to approximately 200; or from approximately 150 to approximately 200 m 2 / g. In one example, the selected CB has a BET value in the range of approximately 55 to approximately 200 m. 2 / G.

[0118] For anode applications, the CB used in the solvent-free process described here can have an OAN value not greater than approximately 650 ml / 100 g, e.g., not greater than approximately 500, not greater than approximately 400, not greater than approximately 300, not greater than approximately 240, not greater than approximately 200, not greater than approximately 150, not greater than approximately 120 ml / 100 g.In one embodiment, the CB selected for the production of a LIB anode by a dry process has an OAN value within a range of approximately 120 to approximately 650 ml / 100 g, such as within a range of approximately 120 to approximately 150, to approximately 200, to approximately 240, to approximately 300 ml / 100 g; or from approximately 120 to approximately 150 to approximately 200 to approximately 240 to approximately 300 ml / 100 g; or from approximately 120 to approximately 150, to approximately 200, to approximately 240, to approximately 300 ml / 100 g; or from approximately 150 to approximately 200, to approximately 240, to approximately 300 ml / 100 g; or from approximately 200 to approximately 240, to approximately 300 ml / 100 g; or from approximately 240 to approximately 300 ml / 100 g; or from approximately 240 to approximately 300 ml / 100 g. In one example, the selected CB has an OAN value in the range of approximately 130 to approximately 240 ml / 100 g.

[0119] LIB cathodes can be manufactured using a dry process that employs a CB with a BET value of at least 90 m. 2 / g, such as at least 90, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500 up to about 1600 m 2 / g. The BET value can range from approximately 500 to approximately 1600 m 2 / g lie, for example, in a range from about 800 to about: 900, 1000, 1100, 1200, 1300, 1400, 1500; or from about 900 to about: 1000, 1100, 1200, 1300, 1400, 1500, 1600; or from about 1000 to about 1100, 1200, 1300, 1400, 1500, 1600; or from about 1100 to about: 1200, 1300, 1400, 1500, 1600; or from about 1200 to about 1300, 1400, 1500, 1600; or from about 1300 to about 1400, 1500, 1600; or from about 1400 to about 1500, 1600 m 2 / g, or from about 1500 to about 1600 m 2 / g. In one example, the selected CB has a BET value within a range of approximately 1350 to approximately 1600 m. 2 / g. In another example, the selected CB has a BET value in a range of approximately 50 to approximately 190, such as in a range of approximately 90 to approximately 100 m. 2 / g. In another example, the CB has a BET value between 500 and 650 m. 2 / G.

[0120] For cathode applications, the CB used in the solvent-free process described here can have an OAN value of no more than approximately 650 ml / 100 g, e.g., less than approximately 600, less than approximately 500, less than approximately 500, less than approximately 400, less than approximately 300, less than approximately 250, less than approximately 200, down to approximately 120 ml / 100 g. The CB can have an OAN value in the range of approximately 120 to approximately 250, to approximately 350, to approximately 450, to approximately 550; or from approximately 250 to approximately 350, to approximately 450, to approximately 550, to approximately 650; or from approximately 350 to approximately 450, to approximately 550, to approximately 650. or from approximately 450 to approximately 550, up to approximately 650 ml / 100 g; or from approximately 550 to approximately 650 ml / 100 g. In one example, the selected CB has an OAN value in the range of approximately 250 to approximately 650 ml / 100 g.

[0121] In many cases, CBs that can be used to produce LIB cathodes using the dry process described here have a BET surface area in the range of approximately 80 to approximately 1600 m². 2 / g and an OAN value in the range of approximately 120 to approximately 650 ml / 100 g. An example of a CB that can be used to manufacture a LIB cathode has a relatively high BET surface area (e.g., in the range of approximately 1350 to approximately 1600 m²). 2 / g), combined with a relatively low OAN value (e.g., in the range of approximately 120 to approximately 220 ml / 100 g). Another example of a CB that can be used to fabricate a LIB cathode has a BET surface area in the range of approximately 80 to approximately 200 m². 2 / g and an OAN value in a range of approximately 140 to approximately 280 m 2 / g, such as 240 or less, for example, in a range of approximately 140 to approximately 180 ml / 100 g. Another example of a CB has a BET value in the range of approximately 500 to approximately 1600 mL. 2 / g and an OAN value in the range of approximately 180 to approximately 650 ml / 100 g. Another example of a CB that can be used to manufacture a LIB cathode has a BET surface area of ​​less than 650 m². 2 / g (e.g. in a range of about 500 to about 650 m) 2 / g) and an OAN value in the range of approximately 180 to approximately 260 ml / 100 g.

[0122] In many cases, CBs that can be used to produce LIB anodes using the dry process described here have a BET surface area in the range of approximately 35 to approximately 1600 m². 2 / g and an OAN value in the range of approximately 120 to approximately 650 ml / 100 g. An exemplary CB that can be used to manufacture a LIB anode has a relatively low BET surface area (e.g., in the range of approximately 50 to approximately 200 m²). 2 / g) in conjunction with an OAN value in the range of approximately 130 to approximately 240 ml / 100 g.

[0123] In many cases, the multifunctional CB has an L a Crystallite size of at least 17 Å, for example from 17 Å to 50 Å. For example, the CB can have an L a Crystallite size from about 17 Å to: about 20, about 30, about 40 Å; or from about 20 Å to about 30, to about 40, to about 50 Å; or from about 30 Å to: about 40, about 50 Å; or from about 40 to about 50 Å.

[0124] The multifunctional CB described here can have a surface energy (SEP) of less than or equal to 15 mJ / m². 2 exhibit, e.g., from about 1 to about 10 mJ / m² 2, such as from about 1 to: about 3, about 5, about 7, about 9 mJ / m 2 ; or from about 3 to: about 5, about 7, about 9, about 10 mJ / m² 2 ; or from about 5 to: about 7, about 9, about 10 mJ / m² 2 ; or from about 7 to about 9, about 10 mJ / m² 2 ; or from about 9 to about 10 mJ / m² 2 .

[0125] Regarding porosity, the multifunctional CB can have a mesopore volume of at least 0.35 cm³. 3 / g, e.g. from about 0.35 to about 2 cm 3 / g, and a total mesopore and macropore volume of at least 1 cm³ 3 / g, e.g. from about 1 to about 3 cm 3 / g. In some embodiments, the mesopore volume in CBs with a large surface area (e.g., BET) is greater than approximately 800 m³. 2 / g) for example from about 0.35 to: about 0.5, about 1, about 1.5; from about 0.5 to: about 1, about 1.5 cm 3 / g, about 2; or from about 1 to: about 1.5, about 2; or from about 1.5 to about 2 cm 3 / G.

[0126] The total volumes of the mesopores and macropores, which are characteristic of multifunctional CBs, can be at least 0.2 cm³ 3 The volume per gram is typically higher. In one example, the multifunctional CB used to manufacture an anode composition has a total volume of mesopores and macropores in a range of approximately 0.2 to approximately 0.8 cm³. 3 / g. Multifunctional CBs suitable for the production of a cathode composition often have a total mesoporosity and macroporosity of at least 1 cm. 3 / G.

[0127] The total mesopore and macropore volume can range from approximately 1 to: approximately 1.5, approximately 2, approximately 2.5 cm³ 3 / g; or from about 1.5 to: about 2.0, about 2.5, about 3 cm 3 / g; or from about 2 to: about 2.5, about 3 cm 3 / g; or from about 2.5 to about 3 cm 3 / g.

[0128] In many embodiments, the multifunctional CB has a percentage crystallinity of at least 22%, e.g., from 23% to 50%, e.g., in a range of about 23% to about 30%, 35%, 40%, 45%; or from about 30% to about 35%, 40%, 45%, 50%; or from about 35% to about 40%, 45%, 50%; or from about 40% to about 45%, 50%; or from about 45% to about 50%.

[0129] Examples of suitable CB materials that can be used include commercially available specifications such as: Vulcan® Series CB such as Vulcan® XCmax 22, Black Pearl® Series CB such as BP 2000 Carbon Black, PBX® Series CB such as PBX 51, LITX® Series CB such as LITX HP from Cabot Corporation.

[0130] Electrode compositions manufactured using a solvent-free process such as the one described here typically contain a multifunctional CB (as described here), an active electrode material, and a "processed" binder. Some product electrode compositions, particularly those manufactured with a fibrillable binder, contain a post-fibrillation binder (also referred to here as a "fibrillated binder") that often exhibits high aspect ratio fibrils. Compositions manufactured with non-fibrillable binders still contain a "processed" binder, namely a binder that is "deformed" (stretched, entangled, etc.), but perhaps to a lesser extent than fibrillable binders under the same or substantially the same fibrillation conditions. A processed, e.g.,Fibrillated binders can be detected using the techniques described above. Successful binder processing, such as fibrillation, is often reflected in the quality of the resulting product, such as an electrode film. In some cases, electrode assemblies manufactured with non-fibrillable binders contain an "undeformed" (globular, rounded, spherical, etc.) binder. Even in such cases, a multifunctional binder can serve as both a binder and mechanical reinforcement for the electrode, while simultaneously imparting the desired electrical properties.

[0131] The electrode compositions can be used to form an anode, a cathode, or both, for example, for incorporation into a device such as a LIB. One, several, or all of the properties that characterize multifunctional CBs can be evaluated in the product electrode composition (in which the binder has been processed, e.g., fibrillated), in product electrodes (e.g., films) commonly obtained by further processing of the product electrode composition, in composite electrodes (in which the product electrode, e.g., the film, has been applied to the appropriate substrate), and / or in the batteries described herein. The electrode can be tested, for example, for adhesion (evaluating the bonding of the electrode film to a substrate), cohesion (evaluating how well the particles are bound to one another), electrode resistance, and / or other properties by methods known in the art.

[0132] With respect to the total weight of the electrode composition, the multifunctional CB can be provided in an amount ranging from approximately 0.1 to approximately 10 wt%, e.g., from approximately 0.3 to approximately 5.0 wt%, or from approximately 0.3 to approximately 3 wt%. Thus, in one embodiment, the multifunctional CB is present in the composition in an amount ranging from approximately 0.3 to approximately 0.5, approximately 1.0, approximately 1.5, approximately 2.0, approximately 2.5; or from approximately 0.5 to approximately 1.0, approximately 1.5, approximately 2.0, approximately 2.5; or from approximately 1.0 to approximately 1.5, approximately 2.0, approximately 2.5, approximately 3.0; or from approximately 1.5 to approximately 2.0, approximately 2.5, approximately 3.0. or from about 2.0 to about 2.5, about 3.0; or from about 2.5 to about 3.0. In some embodiments, CB amounts of more than about 3 wt.% are used, such as between 3 and 5 wt.% of the product electrode composition, e.g., between 3 and 3.5, 4 or 4.5 wt.%; between 3.5 and 4, 4.5 or 5 wt.%; between 4 and 4.5 or 5 wt.%.- %; or between 4.5 and 5 wt.%. Specific amounts can be selected both within and outside these ranges.

[0133] In many cases, this amount is equal to or preferably less than the amount of AC required to achieve the same or substantially the same electrode power. An alternative approach anticipates that smaller amounts of the multifunctional CB will be needed to achieve a power level determined by AC, thereby freeing up additional volume for electroactive material.

[0134] For an exemplary LIB graphite anode composition, the loading of the multifunctional CB is not greater than about 5 wt% and often not greater than about 3 wt%, for example, not greater than 1 wt%. In certain examples, the loading with the multifunctional CB is in the range of about 0.1 wt% to about 1.0 wt%, for example, in the range of about 0.1 to about 0.5 wt% or from about 0.5 to about 1 wt%. In other examples, higher loadings are used, e.g., in the range of about 1 to about 5 wt%, such as a loading of at least about 4.5 wt%, 4.0 wt%, 3.5 wt%, 3.0 wt%, 2.5 wt%, 2.0 wt%, or 1.5 wt%.

[0135] For an exemplary NCM cathode composition, the loading with the multifunctional CB is no more than approximately 5 wt% and often no more than approximately 3 wt%, for example, no more than 1 wt%. In certain examples, the loading with the multifunctional CB is in the range of approximately 0.1 wt% to approximately 1.0 wt%, such as in the range of approximately 0.1 to approximately 0.5 wt% or from approximately 0.5 to approximately 1 wt%. In other examples, higher loadings are used, e.g., in the range of approximately 1 to approximately 5 wt%, such as a loading of at least approximately 4.5 wt%, 4.0 wt%, 3.5 wt%, 3.0 wt%, 2.5 wt%, 2.0 wt%, or 1.5 wt%.

[0136] It has been found that, at least in some cases, a multifunctional CB that has proven effective when added to an anode composition exhibits different properties than a multifunctional CB that has proven effective in cathode compositions.

[0137] In some embodiments, graphite anodes are produced with CBs that have a relatively clean surface (e.g. obtained by heat treatment), a relatively small surface area and structure, and an underdeveloped meso- and macroporosity.

[0138] In other embodiments, NCM cathodes are produced using CBs that have a relatively large surface area and structure as well as pronounced meso- and macroporosity (such as those obtained by steam etching).

[0139] The relative amounts of the multifunctional CB additive to the fibrillable binder can range from a ratio of 5:1 to 0.1:10, e.g., from approximately 1:1 to 0.1:10, from 0.5:1 to 0.1:10; from 5:1 to 0.5:10, from 5:1 to 1:5; from 5:1 to 5:10 by weight. In certain cases, the weight ratio between the multifunctional CB additive and the fibrillable binder is 1:1.

[0140] In one embodiment, the electrode composition contains active material in an amount of about 90 wt.% to about 99 wt.%, e.g. up to 98.0 wt.%, fibrillable binder in an amount of about 1 wt.% to about 5 wt.% and a multifunctional CB additive in an amount of about 0.3 wt.% to about 5 wt.%.

[0141] In many cases, the solvent-free procedure described here is performed without any other fibrillating agents besides a multifunctional CB additive. In other cases, a multifunctional CB can be combined with another, e.g., a conventional fibrillating agent such as AC.

[0142] The term “fibrilliant aid” or “fibrilliant” as used here refers to a material other than the binder or the active electrode material that promotes the fibrilliance of a fibrillable binder. “Additional” or “other” fibrilliant aid or “additional” or “other” fibrilliant refers to a material other than the multifunctional CB described above (i.e., a material that excludes or is not such a material).

[0143] In further embodiments, a multifunctional CB is used in combination with a substantially non-fibrillating conductive additive, e.g., a conventional CCA. The term "additional conductive additive" as used here refers to a different material (i.e., a material that excludes or is not such). Typically, the additional conductive additives lack fibrillating functionality or it is substantially absent.

[0144] Plasticizers and / or other materials commonly used in electrode assemblies may also be present.

[0145] In some examples, a multifunctional carbon carbide (CB) is used together with another (additional) material, such as a conventional fibrillating agent like AC, a hard carbon, graphite, graphene, other non-fibrillating conductive additives, plasticizers, or combinations thereof. In some applications, a multifunctional CB is combined with AC in a ratio of approximately 95:5 to approximately 50:50.

[0146] In other examples, a carbon-based additive is used that contains at least two carbon blacks with one or more different properties, e.g., with respect to their BET. Mixtures of carbon blacks with different structural OANs and / or mixtures with different carbon morphologies are also possible, i.e., activated carbon or graphite with one or more carbon blacks. At least one component in the mixture is a multifunctional carbon black.

[0147] As already mentioned, many aspects of the invention relate to methods for producing electrode compositions, electrode products (e.g. films), electrodes (in which an electrode product such as a film has been applied to a conductive substrate) and / or batteries.

[0148] Turning first to the dry process described above, which is used to prepare the electrode composition, the execution of this process pursues at least two objectives: the mixing of some and usually all of the components, which in most cases are in the form of loose (e.g., flowable or free-flowing) particles; and the processing of the binder in the presence of a multifunctional CB. In some embodiments, each of these two objectives is achieved by one or more mixing operations carried out under specific shear conditions using suitable equipment.

[0149] Low-shear mixing may be chosen, for example, to distribute the ingredients as evenly as possible, e.g., using a roller mill. The term "low-shear mixing" as used here refers to mixing carried out under conditions that are insufficient or substantially insufficient to fibrillate a fibrillable binder. Relying on low-shear mixing can also avoid excessive particle fragmentation, which is often a consideration for some electroactive materials.

[0150] In many cases, the binder is mixed under high shear in the presence of a multifunctional CB. As used here, the term "high-shear mixing" refers to shear conditions strong enough to deform (e.g., stretch, entangle) a binder to a degree sufficient to produce a film electrode using a solvent-free technique. In the case of fibrillable binders, "high-shear mixing" refers to mixing under shear conditions sufficient to fibrillate the binder.

[0151] Without committing to a specific interpretation, it is assumed that a binder polymer, in the presence of a multifunctional CB additive and under high shear conditions, deforms, stretches, elongates, and entangles. The surface energy and / or surface roughness properties that characterize the CB can facilitate the retention of the binder polymer, and the two (CB and polymer) can be squeezed between electroactive particles, resulting in stretching of the binder polymer. When CB particles are dispersed in or on the surface of the binder, they are thought to be able to hold adjacent polymer domains together.Other contributing factors include polymer-polymer interactions (which are likely to increase with increasing polymer strain and / or multidirectional shear forces), interactions between electroactive particles and polymer binders (which may be related to surface energy and / or other factors).

[0152] Under the same or nearly the same high shear conditions, these phenomena tend to be more pronounced when the binder used is a fibrillable binder. The surface and other CB properties favor the entanglement of the polymer here and there. When all particles move under high shear, the polymer is stretched, forming very long, very thin strands (with a high aspect ratio). Typically, these effects are less pronounced with a non-fibrillable binder processed under the same or substantially the same high shear conditions. Or, to put it another way, a non-fibrillable binder may require higher shear conditions to achieve results approaching complete fibrillation.

[0153] In addition to the processing advantages described above, the multifunctional CB can improve electrical conductivity and, in many cases, act as a mechanical reinforcement by holding together both fibrillable and non-fibrillable polymer binders that are wholly or partially “deformed” (stretched, tangled, etc.) or “undeformed” (globular, rounded, spherical, etc.).

[0154] In some situations, high-shear mixing can also be used to break down the particles into smaller fragments. Larger CB particles or granules, such as CB pellets, can be broken down into smaller particles that are evenly distributed throughout the electrode composition, thereby improving electrical conductivity and / or mechanical properties.

[0155] Specific shear values ​​can depend on the size of the operation, the materials involved, the type of mixing equipment, and / or other factors. Low or high mixing settings can be established or optimized based on past experience, routine experiments, etc.

[0156] The components can be combined in any order to obtain a mixture that is preferably well dispersed, e.g., with a uniform distribution of the components; in other words, a homogeneous mixture. In one example, the CB is homogeneously distributed on the surface of the electroactive material and the binder.

[0157] The processing of the binder (e.g. fibrillation) can be carried out on any mixture or pre-blend that combines the multifunctional CB additive and the binder.

[0158] Suitable techniques that can be used or adapted to carry out the steps of mixing and / or processing the binder, e.g., fibrillation, include mechanical stirring, shaking, agitation, etc., and can rely on equipment such as jet mills, tube mills, acoustic mixers, extruders, planetary mixers, other mixing devices, e.g., laboratory-scale mixers, equipment suitable for pilot-scale investigations, for industrial-scale manufacturing, etc.

[0159] In stepwise processes, one type of equipment can be used for the first step (e.g., producing a premix) and a different type of equipment for the subsequent step (e.g., fibrillation). The same applies to shear and / or other mixing parameters.

[0160] In one embodiment, the multifunctional CB additive is first combined with the binder using high-shear equipment to process the binder, e.g., by fibrillation. In some cases, this high-shear process also breaks down the CB particles (pelleted granules or other particles that can be comminuted under high shear conditions) into smaller fragments. The resulting mixture is then blended with the electroactive material (graphite in one example); the use of low shear conditions during this step favors the preservation of particle size (e.g., of the electroactive material).

[0161] In another embodiment, the multifunctional CB is first combined with the electroactive material in a premixing step, which is carried out, for example, under low shear to achieve a uniform distribution of these two components. The binder is then added to this premix and processed under high shear conditions, e.g., fibrillated.

[0162] In another embodiment, the electrochemically active material, the binder and the multifunctional CB are mixed (e.g. under low shear conditions); the mixture is then subjected to high shear conditions to process the binder, e.g. fibrillate it.

[0163] Other processes are possible. For example, the electroactive material can first be mixed with the binder, followed by the addition of the multifunctional CB additive and then processing (e.g., fibrillation) of the binder under high shear conditions.

[0164] Low-shear mixing and / or high-shear processing (e.g., fibrillation) can be performed in one or more (two, three, four, five, six, etc.) stages or pulses, which may last for a suitable period of time, e.g., within a range of approximately 10 seconds to approximately 5 minutes; e.g., within a range of approximately 30 seconds to approximately 1 minute, to approximately 90 seconds, to approximately 2 minutes, to approximately 2.5 minutes, to approximately 3 minutes, to approximately 4 minutes, to approximately 5 minutes; from approximately 1 minute to approximately 90 seconds, to approximately 2 minutes, to approximately 3 minutes, to approximately 4 minutes, to approximately 5 minutes; from approximately 90 seconds to approximately 3 minutes, to approximately 4 minutes, to approximately 5 minutes; from approximately 2 minutes to approximately 3 minutes, to approximately 4 minutes, to approximately 5 minutes; from approximately 3 minutes to approximately 4 minutes, to approximately 5 minutes; From approximately 4 minutes to approximately 5 minutes. Other time intervals can also be used.The duration of two, more, or all impulses can be the same or different.

[0165] A pulse can be followed by a resting or cooling phase. Resting phases can occur at ambient temperature, e.g., room temperature. Cooling can occur to a temperature below ambient temperature, e.g., below room temperature, often at 0 °C or below, e.g., at a temperature in the range of approximately -5 to approximately 5 °C.

[0166] The resting or cooling time can depend on the temperatures reached during mixing, the quantities processed, etc. In many cases, cooling takes a few minutes, e.g., 10 minutes to half an hour or longer. Cooling times can vary in duration and / or temperature conditions.

[0167] To illustrate, a binder-containing composition can be subjected to high-shear mixing at approximately 25,000 to 10,000 revolutions per minute, optionally at approximately 18,000 revolutions per minute, for half a minute and then cooled for 10 minutes to a temperature at or below freezing, e.g., approximately -10 °C. Low-shear mixing can be carried out at approximately 2,000 to 4,000 revolutions per minute for 1 minute, followed by 10 minutes of cooling at approximately 0 °C.

[0168] In one example, a premix of a multifunctional CB additive and an electroactive material is prepared using an acoustic mixer, e.g., for several minutes at a force of 100 G. The resulting mixture is combined with the binder at fibrillation parameters, e.g., using a laboratory jet mill at a pressure rate of 100-90-90-10 psi.

[0169] In another example, all components are mixed in a tube mill (e.g. an IKA Tube Mill 100) at 25,000 rpm in a pulsed process in which mixing and rest phases alternate, followed by a longer mixing process.

[0170] The mixing and / or processing steps, e.g., fibrillation, can be monitored by visual inspection, hand calendering, powder rheology, or other suitable techniques. For example, a small quantity can be handled and sheared by hand or passed through a hand calender. Endpoints can be established based on experience, routine trials, visual inspection, etc. The success of these processes can also be determined by SEM, performance, and / or other techniques commonly performed on the electrode product, e.g., an electrode film.

[0171] The resulting electrode composition (containing at least one active electrode material, a multifunctional CB and a deformed, e.g. fibrillated, binder) may be in the form of pellets, powders (often loose powders) or other forms of free-flowing or loose particulate materials.

[0172] As an optional step, the electrode composition can be sieved to remove unwanted clumps.

[0173] After mixing and processing, e.g., fibrillation, the composition, which may have been sieved, can be formed into a product electrode using any suitable technique known in the art or developed in the future. In one embodiment, the composition is formed into a film by calendering, a process that can be carried out at or above room temperature, e.g., at a temperature similar to or close to the glass transition temperature of the polymer. In a typical calendering process, the electrode composition is subjected to heat and pressure by means of an extruder. The softened material is passed through (e.g., vertical) calender rolls to produce an electrode plate or film. In many embodiments, the film is freestanding, a property that can be described as a 150 µm thick film standing on its own, with no part of the film attached to a support, e.g., a substrate.is in contact with a substrate.

[0174] The desired layer thickness can be achieved by adjusting the gap between the rollers and, in some cases, by adjusting other process parameters.

[0175] The roller temperature can range from room temperature (20 °C) to approximately 200 °C. High roller temperatures can result in a thinner freestanding film on the first pass, while lower temperatures produce a thinner film. The roller speed can also vary. In illustrative examples, the roller speed is set to approximately 0.17 meters per minute (m / min) to approximately 1.3 m / min. A slower roller speed tends to produce a thinner freestanding film on the first pass compared to a faster roller speed. The hydraulic pressure used can range from approximately 1,000 psi to approximately 7,000 psi. Again, a higher pressure can result in a thinner freestanding film on the first pass compared to the thicker films achieved with a lower pressure.

[0176] Further passes through the roller mill can be carried out to reduce the film thickness until the desired thickness and loading are achieved. In certain embodiments, the film thickness is in a range of approximately 40 µm to approximately 300 µm, e.g., from approximately 50 to approximately 200 µm, from approximately 100 µm to approximately 150 µm. Film thicknesses in the range of 50 to 100, 50 to 150, 50 to 200, 50 to 250 µm are also possible; or from 100 to 150, 100 to 200, 100 to 250, 100 to 300 µm; or from 150 to 200, 150 to 250, 150 to 300 µm. or from 200 to 250, from 200 to 300; or from 250 to 300 µm. Desired loadings can be approximately 10 mg / cm². 2 up to about 50 mg / cm² 2 be.

[0177] Freestanding films produced using a multifunctional CB in a solvent-free process are expected to exhibit good mechanical properties. One reliable method for evaluating these mechanical properties is tensile strength testing. For example, a graphite anode is expected to have a tensile strength of at least 100 kPa, while an NCM cathode film is expected to have a tensile strength of at least 500 kPa. In one example, the freestanding film has a tensile strength of at least 0.1 MPa and a thickness ranging from 80 µm to 500 µm. In many cases, the mechanical performance of the film was at least as good as that of a comparable film produced using AC.

[0178] In an optional step, the film is thermally activated, for example, to soften the binder and prepare the electrode product for application to a substrate. In the laboratory, this process can be carried out, for example, on a hot plate at 100° Celsius (C). Larger-scale methods include temperature-controlled roller calenders, convection and / or microwave dryers, and so on.

[0179] The film (which is typically free-standing and contains active electrode material, a multifunctional CB, and a processed, e.g., fibrillated, binder) can be applied to a conductive substrate or support (e.g., an aluminum or copper current collector). In one embodiment, the film is laminated to a carbon-coated copper foil by calendering the two together, e.g., using a horizontal hot roller at a suitable roller temperature, roller speed, and hydraulic pressure.

[0180] The roller temperature can range from approximately 80 to approximately 100 °C. Excessively high temperatures can increase blistering and impair adhesion, while excessively low temperatures can also negatively affect adhesion.

[0181] The roller speed can be set between approximately 0.17 m / min and approximately 1.3 m / min, e.g., approximately 0.5 m / min, while the hydraulic pressure can be set between approximately 500 psi and approximately 2,000 psi. Other settings can also be used. The pressure can be optimized to be high enough to promote adhesion to the substrate without altering the loading, porosity, or other properties. In some embodiments, lamination is performed before setting the final thickness and / or porosity of the film electrode.

[0182] In some cases, film formation and application to the substrate can be achieved in a single step. For example, a powder electrode composition and a substrate film can be passed together through calender rollers under conditions suitable for producing a laminate, where the composition is pressed into a film of the required thickness and bonded to the film. This approach avoids the formation of a self-supporting film.

[0183] The laminated structure can be shaped and / or dimensioned for specific applications such as electrochemical cells, e.g., LIBs, e.g., rechargeable LIBs, etc.

[0184] Electrodes manufactured as described herein can be incorporated into a lithium-ion battery using methods known in the art, such as those described in "Lithium Ion Batteries Fundamentals and Applications" by Yuping Wu, CRC Press, (2015). In certain embodiments, the batteries are button cells, such as 2032 button cells, cylindrical 18650 cells, pouch cells, and others.

[0185] In an illustrative example, a LIB comprises an anode manufactured using a dry process. The anode contains a multifunctional CB, e.g., in an amount of no more than 5 wt%, an active graphite anode material (e.g., natural graphite, synthetic graphite, or mixtures of both; commercially available graphite types such as MCMB, MCF, VGCF, MAG, etc.), and a fibrillated binder. As described above, the active graphite material and the fibrillated binder can be present in the anode in amounts of at least 80 wt% and no more than 5 wt%, respectively.

[0186] The second (opposite) electrode in the battery can also be manufactured using a solvent-free process. In one embodiment, both electrodes in the battery contain a multifunctional CB, as described above.

[0187] It is also possible to produce the second electrode using a conventional dry process (e.g. with AC), by slurry production, or by another non-dry technique.

[0188] In addition to the two electrodes, a typical LIB contains a suitable electrolyte. Examples include ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC), LiPF6; ethylene carbonate-diethyl carbonate (EC-DEC, LiPF6); or (EC-DMC), LiPF6. Furthermore, the electrolyte composition may include special additives known to enhance the performance of SiO₂. xor silicon-containing anodes, e.g., fluorinated carbonates such as fluoroethylene carbonate and others. In the laboratory, a suitable glass fiber microfilter (e.g., Whatman GF / A) can be used as a separator, which absorbs the electrolyte and prevents electrical contact between the electrodes, but allows the diffusion of Li ions. In some cases, polypropylene / polyethylene membrane separators (e.g., Celgard 2300) can also be used.

[0189] The composition or morphology of the electrodes and / or batteries described herein can be characterized by various techniques. Examples include, but are not limited to, electron microscopy, e.g., TEM, SEM, X-ray tomography, Raman spectrometry, and other suitable qualitative or quantitative analytical methods. In one example, SEM data for graphite electrodes fabricated using the dry process with the multifunctional additive described herein showed the presence of ribbon-like binder fibrils, indicating effective fibrillation.

[0190] The quantity or absence of solvents can be determined by weight testing. This involves drying the wet-cast electrode until its weight reaches the theoretically calculated value based on the known solids content of the slurry, or until the electrode weight stabilizes and remains unchanged for at least 3 minutes. For an electrode produced entirely without solvents, the weight will remain constant throughout the evaluation period. In other words, the weight of the newly produced electrode (before drying) will be equal to or within 1% by weight of the theoretical weight (i.e., the weight obtained by adding the weights of the individual components of the process).

[0191] Another approach that can be used to detect a solvent (e.g., NMP) is based on attenuated total reflection Fourier transform infrared spectroscopy (FTIR-ATR) combined with gas chromatography (GC). In many cases, dry-processed electrode films can be distinguished from slurry-based products by very low or undetectable solvent residues. A substantially uniform distribution of the binder without migration towards the film surface is another characteristic frequently associated with an electrode product manufactured using a solvent-free process.

[0192] The flexibility properties that characterize the electrode (its ability to resist cracking) can be measured by visual inspection when bending a film by hand or with a mandrel bending tester. In certain designs, the electrode is evaluated and expected to pass a mandrel bar test with a diameter of 10 mm without any cracks being visible to the naked eye. In one illustration, the electrode was found to pass a bending test using an 8 mm diameter pin as the mandrel.

[0193] The performance of the electrodes can be tested using established techniques or adapted or developed methods. Suitable methods include, for example, in-plane and thru-plane electrode conductivity, electrochemical impedance spectroscopy (EIS), constant current charge-discharge, hybrid pulse power capability (HPPC), and cycling.

[0194] In many cases, electrodes fabricated using a solvent-free process with a multifunctional CB perform at least as well as, and often better than, a comparison electrode (here also referred to as a "reference") containing the same amounts of active electrode material (e.g., graphite), binder, and a conventional fibrillating agent such as AC. Alternatively, the amounts of multifunctional additives required to achieve the performance attainable with AC are typically lower in electrodes fabricated according to the embodiments described herein.

[0195] In one embodiment, a graphite anode produced using a dry process and containing a multifunctional CB in a concentration of no more than about 1 wt% shows at least as good performance (measured by in-plane resistance, rate capability, first cycle efficiency) as a reference electrode containing higher amounts (e.g. 5 wt%) of AC.

[0196] Good mechanical properties are also expected from electrodes fabricated with a multifunctional CB in a solvent-free process. Reliable mechanical evaluation techniques include peel tests (e.g., 90°, 180°, T-peel, various fixings), tensile tests, and flexure tests (mandrel tests), to name a few. In many cases, the electrode fabricated with a multifunctional CB performed at least as well as a reference electrode fabricated with AC.

[0197] Without wishing to be bound to a specific interpretation, it is assumed that by using a multifunctional CB as described here, ribbon-like binder strands or fibrils can be generated that may be long enough to envelop and hold together particles of the electroactive material.

[0198] The multifunctional CB thus appears to be able to process the binder even in relatively small quantities, e.g. fibrillating it, creating effective conductive networks in electrodes and simultaneously contributing to the desired mechanical properties.

[0199] The compositions and processes described here can also be used (e.g., built-in) and / or adapted for the manufacture of other energy storage devices, such as primary alkaline batteries, primary lithium batteries, nickel-metal hydride batteries, sodium batteries, lithium-sulfur batteries, lithium-air batteries, and supercapacitors. Methods for manufacturing such devices are known in the art and are described, for example, in the "Battery Reference Book" by T.R. Crompton, Newness (2000).

[0200] The principles described here can also be used or adapted for semi-dry processes. Such processes often include one step that is a wet step (or slurry step). Other steps are carried out without the addition of liquid (e.g., solvent).

[0201] An example of a semi-dry process involves situations where two or more electrode components, such as the electroactive material and a multifunctional binder, are first mixed together in the presence of a liquid (e.g., solvent), followed by a drying step to remove the solvent. The remaining processing steps can then be carried out without the addition of any liquid (e.g., solvent). For example, the dried premix (containing the electroactive material and binder) can be combined with the binder, and the binder can be processed (e.g., fibrillated) in the absence of any liquid, such as solvent.

[0202] The invention is further illustrated by the following, non-limited examples. Illustrative materials and methods

[0203] The materials used for the solvent-free electrode process and formulation included Targrey graphite BTR 918-2A, Targrey lithium nickel manganese cobalt oxide NCM622 (SNCM03006), and standard activated carbon with a surface area of ​​1500 cm². 2 / g, electrically conductive CB Ketjenblack EC-600J from Lion Co., C-NERGY™ SUPER C65 Carbon Black from Imerys, and Acetylene Black Li-435 from Denka. All other CB specifications were from Cabot Corporation. The fibrillable binder was polytetrafluoroethylene (PTFE). The physical properties of the carbon blacks used in the following examples are given in Tables 1A and 1B above.

[0204] Generally, the graphite electrodes were produced in several steps. In a first step (S1), the electrode components were combined and mixed under conditions suitable for fibrillating the binder (e.g., by mixing under high shear). The second step (S2) involved passing the powder mixture from S1 through a vertical calender set to the gap appropriate for the desired film thickness. The freestanding films obtained from S2 were laminated onto a current collector in a third step (S3).

[0205] A similar sequence of steps was followed in the production of cathode electrodes.

[0206] The thickness of the solvent-free electrodes was measured using a manual drop gauge with a flat measuring contact head of 7.14 mm diameter.

[0207] The strength and Young's (elasticity) modulus of the dry films were measured using the Mecmesin MultiTest-dV motorized force tester with a load of 10N.

[0208] The sheet resistance of the solvent-free electrodes was measured using a commercially available Signatone Pro4-4400 system (SP4 probe head connected to the rear of a Keithley 2410-C source meter). The reported values ​​were normalized to the electrode thickness and are given as electrode resistance in ohms per centimeter. Example 1

[0209] In this example, freestanding graphite anode films were produced in two steps (S1 and S2), using a jet mill as a high shear mixing device in S1, and then laminated onto current collectors to form electrodes (S3).

[0210] In step S1, the electrode components were premixed using a Resodyn acoustic mixer (S1-1) and subsequently blended using a 4-inch jet mill (S1-2). Specifically, premixing step S1-1 was performed to ensure a uniform distribution of the powder components in the mixture. This step involved a 5-minute premix of a carbon additive and the electrodeactive material (graphite) in the acoustic mixer at 100% intensity and automatic frequency, followed by the addition of the polymer and blending at the same settings for another minute. The next mixing step, S1-2, involved fibrillating the binder and included passing the premixed material through the laboratory-scale jet mill at a pressure rate of 100-90-90-10 psi.

[0211] In S2, the powder mixture obtained in S1 was passed through a vertical calender at room temperature to obtain freestanding films with a thickness between 110 and 190 µm.

[0212] In S3, the freestanding electrode films obtained in S2 were thermally activated on a heating plate set to 100 °C and then laminated onto the carbon-coated, 9 µm thick copper foil (MTI Corporation) by calendering them together with a horizontal hot roller calender preheated to 80 °C.

[0213] The composition of the electrode formulations used (A1 and A2 used CB, while A3 used activated carbon and served as a reference) is listed in Table A: Table A Formulierungsnummer Aktives Material Kohlenstoffadditiv Bindemittel A1 90% Graphit 5% CB11 5% PTFE A2 90% Graphit 5% CB9 5% PTFE A3 90% Graphit 5% AC 5% PTFE

[0214] SEM photographs (low and high magnification) and fluorine element mapping of cross-sections of electrode films A1, A2 and A3 as reference (90% graphite, 5% PTFE and 5% additive) are in the Fig. 1A to 1I are shown.

[0215] The fibrils of the binder are easily visible in formulations containing activated carbon (AC) (SEM photos 1A and 1B). Fibrils are also easily recognizable in electrode A2 (see SEM photos 1G and 1H). This suggests that certain carbon binders (CBs) can act as fibrillating additives on their own, similar to traditionally used AC, and thus replace AC in the formulation.

[0216] Some fibrils are also visible in the SEM images 1D and 1E of electrode A1, although to a lesser extent than in A2. This supports the idea that surface chemistry plays a role and that PTFE interacts more readily with the cleaner surface of the heat-treated material.

[0217] Fig. 1C, Fig. 1F and Fig. Figure 1 shows images of elemental fluorine confirming a uniform distribution across the electrode. No migration phenomenon was observed (as is very often the case with electrodes prepared by suspension). Example 2

[0218] The compositions A1 to A3 in Table A were further tested with regard to the electrical properties of the product. The electrode films were produced as in Example 1, with the difference that, in addition to the combination of acoustic mixer and jet mill in (S1), the mixture was further processed using an IKA Tube Mill 100 for 15 seconds at 25,000 rpm.

[0219] While the fibrillation capability of AC and carbon particles CB9 is similar, as shown in Example 1, CB9 offers the additional advantage of lower electrode resistance when tested with the same load. Fig. Figure 2 shows that both CB-containing electrodes, namely A1 and A2, showed an improved in-plane resistance compared to the AC-containing reference electrode, namely A3.

[0220] Since the in-plane resistance of A2 was almost as low as that of A1, the improved fibrillation observed in A2 could lead to CB9 (the heat-treated version of CB11) being preferred overall, at least in some dry-process applications. Example 3

[0221] The graphite electrodes in this example were produced using the same method as in Example 1, except that the jet mill in (S1) was replaced by an IKA Tube Mill 100, in which the electrode components were processed at 25,000 rpm, 6 x 15 second mixing pulses with 45 second pauses in between, followed by 2 minutes of direct mixing at 25,000 rpm.

[0222] In S2, the powder mixture obtained in S1 was passed through a vertical calender at room temperature to obtain freestanding films with a thickness between 120 and 135 µm.

[0223] The electrode formulations used (designated B1 to B7, with B8 serving as a reference) are listed in Table B below. Table B Formulierungsnummer Aktives Material Kohlenstoffadditiv Bindemittel B1 90% Graphit 5% CB1 5% PTFE B2 90% Graphit 5% CB3 5% PTFE B3 90% Graphit 5% CB4 5% PTFE B4 90% Graphit 5% CB9 5% PTFE B5 90% Graphit 5% CB11 5% PTFE B6 90% Graphit 5% CB14 5% PTFE B7 90% Graphit 5% CB15 5% PTFE B8 90% Graphit 5% AC 5% PTFE

[0224] Fig. Figure 3 compares the tensile strength of a graphite film and the in-plane resistance of a graphite electrode containing AC (see reference electrode composition B8 in Table B) with electrodes formulated with various CBs, namely additives CB1, CB3, CB4, CB9, CB11, CB14, and CB15 (from Tables 1A and 1B). All electrodes were prepared using a dry process and contained the CB additive at a loading of 5 wt%, graphite (90 wt%), and PTFE (5 wt%). As in Fig. As shown in Figure 3, the dry-process electrodes using carbon blacks (CBs) believed to have good fibrillating properties (see, for example, carbon blacks CB9, CB11, CB14, and CB15) also exhibited low in-plane resistances, which were very similar to or better than those observed with a good CCA additive such as carbon black CB4 (from Table 1). Furthermore, the use of CBs believed to be potentially good fibrillators (e.g., carbon blacks CB1, CB3, CB4, CB9, CB11, CB14, and CB15 from Table 1) produced electrodes with lower in-plane resistances than those observed with AC.

[0225] In one example, a freestanding graphite film containing CB3 showed a moderate improvement in tensile strength and in-plane resistance compared to the data observed with CB4 (unheat-treated). This supports the idea that chemistry plays a role and that PTFE interacts more readily with the cleaner surface of the heat-treated CB3 material.

[0226] In another example, freestanding graphite films containing CB15 (steam-etched) showed a significant improvement in tensile strength and in-plane resistance compared to those with CB4 (non-steam-etched). This supports the idea that chemistry and morphology play a role and that PTFE containing CB15, which has a cleaner surface, larger surface area, higher structure, and more developed meso- and macroporosity than steam-etched material, is more likely to fibrillate and be more uniformly distributed in the electrode.

[0227] Since CBs with a relatively small surface area (e.g., carbon blacks CB1 and CB3) can cause less formation of solid electrolyte interphases (SEI) (the growth of SEI is considered a major factor in the capacity degradation of LIBs) compared to CBs with a relatively large surface area (e.g., carbon blacks CB9, CB11, CB14, CB15), the improved battery performance expected with the smaller surface area CB particles may lead to this type of performance additive being preferred overall, at least in some dry process applications. Example 4

[0228] In this example, freestanding NCM622 cathode films were produced in two steps (S1 and S2), using the IKA Tube Mill 100 as a high shear mixing device in S1 and subsequently laminating to current collectors to produce electrodes (S3).

[0229] In step S1, the electrode components were premixed using a Resodyn acoustic mixer (S1-1) and subsequently mixed using the IKA Tube Mill 100 (S1-2). Specifically, premixing step S1-1 was performed to ensure a uniform distribution of the powder components in the mixture. This step involved premixing a carbon additive and the electrodeactive material (NCM622) in the acoustic mixer for 5 minutes at 100% intensity and automatic frequency, followed by the addition of the polymer and mixing at the same settings for another minute. The next mixing step, S1-2, involved fibrillating the binder. This step consisted of passing a premixed material through the IKA Tube Mill 100 at 25,000 rpm, with six 15-second mixing pulses separated by 45-second intervals, followed by three minutes of continuous mixing at 5,000 rpm.

[0230] In S2, the powder mixture obtained in S1 was passed through a vertical calender at 100 °C to obtain freestanding films with a thickness between 110 and 170 µm.

[0231] In S3, the freestanding electrode films obtained in S2 were laminated onto the carbon-coated aluminum foil current collector by calendering them together using a vertical hot roller calender preheated to 100 °C.

[0232] The electrode formulations used (designated C1 to C6 and D1 to D6) are listed in Table C and D respectively: Table C Formulierungsnummer Aktives Material Kohlenstoffadditiv Bindemittel Freistehender Elektrodenfilm C1 90% NCM622 5% CB1 5% PTFE Missed C2 90% NCM622 5% CB3 5% PTFE Missed C3 90% NCM622 5% CB5 5% PTFE Missed C4 90% NCM622 5% CB9 5% PTFE Passed C5 90% NCM622 5% CB15 5% PTFE Passed C6 90% NCM622 5% AC 5% PTFE Missed Table D Formulation number Active material Carbon additive binder Freestanding electrode film D1 94% NCM622 2% CB7 4% PTFE Missed D2 94% NCM622 2% CB8 4% PTFE Missed D3 94% NCM622 2% CB10 4% PTFE Passed D4 94% NCM622 2% CB12 4% PTFE Passed D5 94% NCM622 2% CB13 4% PTFE Passed D6 94% NCM622 2% CB15 4% PTFE Passed

[0233] Fig.Figure 4 compares the tensile strength and modulus of elasticity of a freestanding NCM electrode film containing AC (see reference electrode composition C6 in Table C) with electrodes formulated with different CBs, namely additives CB1, CB3, CB5, CB9, and CB15 (from Tables 1A and 1B). All electrodes were manufactured using a dry process and contained the CB additive at a loading of 5 wt%, NCM622 (90 wt%), and PTFE (5 wt%). As in Fig. As shown in Figure 4, the dry-process electrode films with added CB exhibited better strength than the AC-containing reference. In some cases, formulations containing certain CBs, namely CB1, CB3, and CB5, showed a relatively high modulus of elasticity (over 400 N / mm²). 2) and appeared stiff and difficult to process further. In other cases, formulations with CBs of a specific morphology, namely CB9 and CB15, exhibited a good balance between tensile strength (over 1000 kPa) and modulus of elasticity (below 400 N / mm²). 2 ) and formed flexible, freestanding cathode films that passed quality control and were able to be laminated onto current collectors.

[0234] Fig. Figure 5 compares the tensile strength and modulus of elasticity of NCM electrode films (see electrode compositions in Table D) formulated using different CBs, namely CB7, CB8, CB10, CB12, CB13, and CB15 (from Tables 1A and 1B). All electrodes were manufactured using a dry process and contained the CB additive at a loading of 2 wt%, NCM622 (94 wt%), and PTFE (4 wt%). Similar to the data in Fig.4. The results reported for the formulations with 5 wt% CB, 90 wt% NCM622, and 5 wt% PTFE showed that CBs with advanced morphology, namely CB10, CB12, CB13, and CB15, enabled the formation of flexible, freestanding electrode films compared to films obtained with CBs with less advanced morphology, namely CB7 and CB8. The results suggest that the relatively high BET, OAN values, and pore volume types of the carbon additive, namely CB9, CB10, CB12, CB13, and CB15, are generally preferred as processing particles, at least in some dry process applications.

[0235] As in Fig. Figure 6 shows that the electrode formulation with carbon black (formulation C4 in Fig. 6) also a lower electrode resistance compared with the AC-containing reference (namely formulation C6); the lower resistance is known to have a positive effect on battery performance. Example 5

[0236] In this example, the NCM cathode electrodes were produced in three steps: first, by forming a freestanding, dry-processed film (S1 and S2) using a twin-screw extruder as a high-shear mixing device, followed by laminating it onto the current collector (S3).

[0237] In S1, the dry electrode powder mixture was produced in a three-stage process. Specifically, in S1-1, three electrode components (NCM622, PTFE, and carbon) were first premixed in powder form in a rotary drum for 30 minutes to achieve a more uniform distribution. In S1-2, the premixed powders were processed in a twin-screw extruder at a temperature of 100 °C, a throughput of 3 kg / h, and a screw speed of 400 rpm to disperse the carbon and fibrillate the binder. The resulting electrode powder mixture was in flake form. In S1-3, the flake material obtained in S1-2 was post-processed at low shear in an IKA mill at 5000 rpm for 20 seconds to restore its powder form.

[0238] In S2, the powder electrode mixture obtained in S1 was passed through a vertical calender at 100 °C to obtain a freestanding film. The final thickness of the dry electrode film was in the range of 110–120 µm.

[0239] In S3, the freestanding electrode films obtained in S2 were laminated onto the carbon-coated aluminum foil current collector by calendering them together using a vertical hot roller calender preheated to 100 °C.

[0240] The electrode formulations used (designated E1 and E2) are listed in Table F. Table E electrode Active material Carbon additive binder Freestanding electrode film E1 97% NCM622 1% CB2 2% PTFE Missed E2 97% NCM622 1% CB12 (loose form) 2% PTFE Passed E3 97% NCM622 1% CB12 (pelleted form) 2% PTFE Passed

[0241] Formulations E1, E2, and E3 produced flakes of similar appearance in S1-2. Upon calendering (S2), only formulations E2 and E3 formed a freestanding cathode film. The tensile strength and modulus of elasticity for these films are shown in Fig.Figure 7 shows that formulation E1 did not form a freestanding film but crumbled before the target thickness of 110 µm was reached. Consequently, dry process electrodes could not be produced with formulation E1. This could indicate that a carbon additive such as CB 12, either in flake or pellet form, should be used as a processing particle, at least in some dry process applications. Example 6

[0242] The graphite electrodes in this example were prepared using the same method as in Example 3, except that in step (S2) the calendering was carried out in two steps at different temperatures. In one case, the powder mixture obtained in S1 for the production of freestanding films for tensile tests was first passed through a vertical calender at room temperature, followed by a second pass through the calender preheated to 80 °C to obtain freestanding films with a thickness between 250 and 280 µm.In another case, the powder mixture obtained in S1 for the production of dry electrodes for testing peel strength (adhesion) was passed in a first step through a vertical calender preheated to 100 °C and in a second step to 80 °C, followed by the lamination of the dry film onto the current collector by passing them together through a vertical calender preheated to 80 °C.

[0243] The electrode formulations used (F1 to F4) are listed in the following table F. Table F Formulation number Active material Carbon additive binder Tensile strength peel strength F1 90% Graphit 5% carbon 5% PTFE 237 kPa 0.035 N F2 90% Graphit 5% carbon 3.75% PTFE, 1.25% PVDF 187 kPa Not available F3 90% Graphit 5% carbon 2.5% PTFE, 2.5% PVDF 107 kPa 0,089 N F4 90% Graphit 5% carbon 5% PVDF Missed Missed

[0244] All electrodes were produced using a dry process and contained the carbon additive at a loading of 5 wt%, graphite (90 wt%), and binder (5 wt%). As can be seen from Table F, a dry-process freestanding electrode film using a fibrillable binder expected to stretch easily and form fibrils (e.g., PTFE) also exhibited higher tensile strength than those in which a fibrillable PTFE binder was partially replaced by a non-fibrillable binder, namely PVDF (e.g., PTFE / PVDF in ratios of 75:25 and 50:50, respectively, in formulations F2 and F3). A formulation containing only a non-fibrillable binder (e.g., PVDF) did not result in a freestanding film and failed on the first calender pass.On the other hand, the partial replacement of PTFE with PVDF in the formulation improved the adhesion of the free-standing film to the current collector (see formulations F3 and F1 in Table F for comparison). This supports the idea that while the presence of a fibrillable binder enables the formation of dry electrodes, non-fibrillable binders can be used to improve other electrode properties, such as electrode adhesion to the current collector and first-cycle irreversibility, which is determined by the PTFE performance on the anode side of the battery, to name just a few. Example 6

[0245] NCM electrodes with two different formulations were manufactured using dry and wet processes (slurry casting) and tested in 2032 button half-cells.

[0246] Dry processed NCM cathodes, namely G1, were manufactured using the same procedure as in Example 4.

[0247] Wet-processed NCM cathodes, specifically G2, were manufactured using a two-stage mixing process with a Thinky ARE310 planetary centrifugal mixer. The first step involved 20 minutes of mixing (12 minutes of active mixing) of a grinding base consisting of conductive carbon additive (CCA) / PVDF / NMP with two small tungsten carbide (WC) grinding media. After adding NCM622 powder to the grinding base, the second step involved mixing for another 20 minutes (12 minutes of active mixing) without media. Both the NCM and CCA powders were pre-dried for 20 minutes at 130 °C. The electrode slurry was applied to a 15 µm thick aluminum foil using an automatic doctor blade coater (model MSK-AFA-III from MTI Corp.). The NMP was evaporated for 20 minutes in a convection oven set to 80 °C and then dried in a vacuum oven at approximately 100 °C. The dry electrode loading was 24.4 mg / cm². 2on aluminum foils that were calendered to a density of 3.4 g / cc using a manual roller press.

[0248] The electrode formulations used (designated G1 and G2, with the G2 formulation being prepared using the slurry (wet) process) and their properties are listed in Table F below. Electrode G2 used an electrode formulation and exhibited electrode properties that are standard for NCM cathodes in EV applications and therefore served as the baseline. Table G Electrode number Process type formulation Active material loading [mg / cm³] 2 Electrode density [g / cm³] 3 Electrode capacity [mAh / cm] 2 G1 Dry 95% NCM, 2% CB15, 3% PTFE 33,1 3,7 5,6 G2 Wet 97% NCM, 1.5% CB3, 1.5% PVDF 24,4 3,4 3,9

[0249] Cathodes G1 and G2 (from Table G) were tested in 2032 button cell half-cells. To manufacture the button cells, discs with a diameter of fifteen millimeters were stamped and dried under vacuum at 100 °C for at least four hours. The discs were calendered to the desired density (as shown in Table G) using a manual roller press and assembled into 2032 button cells in an argon-filled glovebox (M-Braun) for testing against lithium foil. Glass fiber microfilters (Whatman GF / A) were used as separators. The electrolyte consisted of 100 microliters of ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC) 1%, and LiPF6 1M (BASF).

[0250] The stated capacities are normalized in mAh / g of the active cathode mass. The performance of the button half-cells at room temperature (25 °C) was measured by first shaping them with two C / 5-D / 5 charge-discharge cycles, then charging them at a rate of 1 C and discharging them at C / 5, 1 C, 2 C, and 3 C. The results ( Fig. 8) show that the dry-processed G1 formulation has better or comparable capacity at C rates up to 1 C (0.2 C, 0.5 C and 1.0 C) compared to the slurry-processed baseline formulation G2. Example 7

[0251] Two sets of cathodes were fabricated using the same dry and wet (slurry casting) processes as described in Example 6. The electrode formulations used (designated H1 to H4, with H3 and H4 serving as the baseline for the wet process for the dry-fabricated H1 and H2, respectively) and the properties of the resulting cathodes are listed in Table H below. All cathodes contained the carbon additive at a loading of 1 wt%, NCM622 (96 wt%), and a binder (3 wt%) prepared with two different carbons, namely C12 and CB15, and 3.9 ± 0.2 mg / cm³. 2 or 3.8 ± 0.1 mg / cm³ 2 was calendered. Table H Electrode number Process type formulation Active material loading [mg / cm³] 2 Electrode density [g / cm³] 3 Electrode capacity [mAh / cm] 2 H1 Dry 96% NCM, 1% CB12, 3% PTFE 26,5 3,9 4,5 H2 Dry 96% NCM, 1% CB15, 3% PTFE 26,2 3,8 4,5 H3 Wet 96% NCM, 1% CB12, 3% PVDF 26,5 3,9 4,5 H4 Wet 96% NCM, 1% CB15, 3% PVDF 26,2 3,8 4,5

[0252] The cathodes, namely H1, H2, H3, and H4, were tested in 2032 button cells. For the production of the button cells, discs with a diameter of fifteen millimeters were stamped and dried under vacuum at 100 °C for at least four hours. The discs were calendered to the desired electrode density using a manual roller press and assembled into 2032 button cells in an argon-filled glovebox (M-Braun) for testing against graphite anodes containing 3% CB, 5% PVDF, and 92% natural graphite. Celgard filters were used as separators. The electrolyte consisted of 200 microliters of ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC) 1%, and LiPF6 1M (BASF).

[0253] Cells were produced with each formulation and the initial C / 20 capacity and irreversible loss in the first cycle were measured ( Fig. 9 or Fig.10) The group of cells whose cathode formulation contained CB12 (from Tables 1A and 1B) and was manufactured using the dry process showed comparable discharge capacity and improved (lower) first-cycle irreversibility loss compared to the cells with wet-processed cathodes. The group of cells whose cathode formulation contained CB15 (from Tables 1A and 1B) and which was manufactured using the dry process exhibited discharge capacity and first-cycle irreversibility comparable to those of the wet-processed cathodes in both cases. In both cases, the performance of the dry-processed cathodes was comparable to or better than that of the wet-processed cathodes, suggesting that the dry process can replace the conventional slurry process without affecting the electrochemical performance of the battery. Example 8

[0254] Dry-processed NCM cathodes containing 2 wt% CB, namely CB15 (from Tables 1A and 1B), NCM622 (94 wt%), and PTFE (4 wt%), were prepared using the same procedure as in Example 4 and tested in 2032 button half-cells as described in Example 6. The dry cathodes were treated with an active material loading of 33.5 mg / cm². 2 and a capacity of 5.6 mAh / cm² 2 produced and calendered at 3.6 g / cc.

[0255] The cycle life of the button cell half-cells was measured by charging and discharging them at +25 °C at a rate of 1 C. A discharge rate of C / 20 was used for the first 5 cycles, followed by a discharge rate of C / 10 for the next 2 cycles, and a discharge rate of C / 5 for the long-term cycle. The discharge capacity measured during the cycles was close to the theoretical capacity of the NCM622, as shown in Fig. 11 shown.

[0256] While this invention has been shown and described in particular with reference to preferred embodiments, the person skilled in the art understands that various changes to the form and details can be made without deviating from the scope of the invention as defined by the attached claims. QUOTES INCLUDED IN THE DESCRIPTION

[0000] This list of documents cited by the applicant was automatically generated and is included solely for the reader's convenience. The list is not part of the German patent or utility model application. The DPMA accepts no liability for any errors or omissions. Cited patent literature

[0000] US 63 / 322,074

[0002] US 10,886,535 B2

[0084] WO 2020 / 197670

[0088] WO 2020 / 197673

[0088] US 8,895,142 B2

[0096] US 10,087,330 B2

[0096] Cited non-patent literature

[0000] Raman studies of heat-treated carbon blacks", Carbon Vol. 32 (7), pp. 1377-1382, 1994

[0082] EP Barrett, LG Joyner, PP Halenda, J. Am. Chem. Soc. 1951, 73, 373-380

[0085]

Claims

[1] A process for producing an electrode composition, the process comprising: Combining an active electrode material, a binder and a multifunctional carbon black; and Processing the binder in the presence of carbon black, whereby: the process is carried out without the addition of solvent; and the multifunctional carbon black has a BET value of not more than about 1600 m 2 / g and an OAN value of not more than about 650 ml / 100 g. [2] The method of claim 1, wherein the active electrode material is graphite and the multifunctional carbon black has a BET value in the range of about 35 to about 1600 m 2 / g and an OAN value in the range of about 120 to about 650 ml / 100 g. [3] The method of claim 1, wherein the active electrode material is graphite and the multifunctional carbon black has a BET value in the range of about 50 to about 200 m 2 / g and an OAN value in the range of about 130 to about 240 ml / 100 g. [4] The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 80 to about 1600 m 2 / g and an OAN value in a range of about 120 to about 650 ml / 100 g. [5] The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 500 to about 1600 m 2 / g and an OAN value in a range of about 180 to about 650 ml / 100 g. [6] The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 80 to about 200 m 2 / g and an OAN value in a range of about 140 to about 280 ml / 100 g. [7] The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 1350 to about 1600 m 2 / g and an OAN value in a range of about 120 to about 220 ml / 100 g. [8] The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 500 to about 650 m 2 / g and an OAN value in a range of about 180 to about 260 ml / 100 g. [9] A process according to any one of the preceding claims, wherein the multifunctional carbon black has one or more of the following properties: a surface energy of about 15 mJ / m 2 or less, a microcrystalline planar size according to Raman (La) of at least about 17 Å, a mesopore volume of at least about 0.35 cm 3 / g, a total mesopore and macropore volume of at least 1.0 cm3 / g and a percentage crystallinity of at least 22%. [10] A method according to any one of the preceding claims, wherein the active electrode material, the binder, the multifunctional carbon black and the electrode composition are loose particulate materials. [11] A method according to any one of the preceding claims, wherein the binder is fibrillatable, non-fibrillatable or a combination thereof. [12] The method of claim 11, wherein the binder is PTFE, PVDF or a combination thereof. [13] A process according to any one of the preceding claims, wherein the multifunctional carbon black is provided as a loose powder, pellets or granules. [14] A method according to any one of the preceding claims, wherein processing the binder in the presence of the multifunctional carbon black comprises a high shear process sufficient to fibrillate a fibrillatable binder. [15] The method of claim 15, wherein the high shearing process deforms a non-fibrillatable binder. [16] A process according to any one of the preceding claims, wherein the combination of the active electrode material, the binder and the carbon black additive is carried out at shear conditions which are lower than the shear conditions used in processing the binder in the presence of the carbon black additive. [17] A process according to any one of the preceding claims, wherein the process is carried out in the presence of the multifunctional carbon black as the sole fibrillation aid. [18] The process according to any one of claims 1 to 16, wherein the process is carried out in the presence of the multifunctional carbon black and at least one other material selected from the group consisting of activated carbon, another multifunctional carbon black and a conductive carbon additive. [19] A method further comprising applying the electrode composition prepared according to any one of the preceding claims to a conductive substrate to form a battery electrode. [20] The method of any one of claims 1 to 18, further comprising processing the electrode composition to form a free-standing film. [21] The method of claim 20, wherein the free-standing film is prepared by calendering the electrode composition. [22] The method of claim 20, wherein the free-standing film has a tensile strength of at least 0.1 MPa and a thickness in a range of about 80 to 500 µm. [23] A process for producing an electrode composition, the process comprising: Combining an active electrode material, a fibrillatable binder, and a multifunctional carbon black; and Subjecting the fibrillatable binder to a fibrillation process in the presence of the multifunctional carbon black, wherein: the process is carried out in the absence of solvent and the multifunctional carbon black has a BET value of not more than 1600 m 2 / g and an OAN value of not more than 650 ml / 100 g. [24] The method of claim 23, wherein the active electrode material is graphite and the multifunctional carbon black has a BET value in the range of about 35 to about 1600 m 2 / g and an OAN value in the range of about 120 to about 650 ml / 100 g. [24-1] The method of claim 23, wherein the active electrode material is graphite and the multifunctional carbon black has a BET value in the range of about 50 to about 200 m 2 / g and an OAN value in the range of about 130 to about 240 ml / 100 g. [25] The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in the range of about 80 to about 1600 m 2 / g and an OAN value in the range of about 120 to about 650 ml / 100 g. [26] The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 500 to about 1600 m 2 / g and an OAN value in a range of about 180 to about 650 ml / 100 g. [27] The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 80 to about 200 m 2 / g and an OAN value in a range of about 140 to about 280 ml / 100 g. [28] The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 1350 to about 1600 m 2 / g and an OAN value in a range of about 120 to about 220 ml / 100 g. [29] The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in the range of about 500 to about 650 m 2 / g and an OAN value in the range of about 180 to about 260 ml / 100 g. [30] A process according to any one of claims 23 to 29, wherein the multifunctional carbon black has one or more of the following properties: a surface energy of about 15 mJ / m 2 or less, a microcrystalline planar size according to Raman (La) of at least about 17 Å, a mesopore volume of at least about 0.35 cm 3 / g, a total mesopore and macropore volume of at least 1.0 cm 3 / g and a percentage crystallinity of at least 22%. [31] A process according to any one of claims 23 to 30, wherein the process is carried out in the presence of the multifunctional carbon black as the sole fibrillation aid. [32] The process according to any one of claims 23 to 30, wherein the process is carried out in the presence of the multifunctional carbon black and at least one other material selected from the group consisting of activated carbon, another multifunctional carbon black and a conductive carbon additive. [33] A method according to any one of claims 23 to 32, further comprising a mixing operation carried out at shear conditions lower than the shear conditions used in the fibrillation operation. [34] The method of any one of claims 23 to 33, further comprising premixing the active electrode material and the multifunctional carbon black. [35] A method according to any one of claims 23 to 33, wherein the active electrode material is added before, during or after fibrillation of the binder. [36] A method according to any one of claims 23 to 35, wherein the fibrillatable binder is PTFE. [37] The method of any one of claims 23 to 36, wherein the electrode composition contains active electrode material in an amount of about 90 wt% to about 98 wt%, fibrillatable binder in an amount of about 1 wt% to about 5 wt%, and multifunctional carbon black in an amount of about 0.3 wt% to about 5 wt%. [38] A method according to any one of claims 23 to 37, wherein the multifunctional carbon black is heat treated or vapor etched. [39] A process according to any one of claims 23 to 38, wherein the multifunctional carbon black is provided as a loose powder, in pelletized form or as granules. [40] A method according to any one of claims 23 to 39, wherein the electrode active material, the fibrillatable binder, the multifunctional carbon black and the electrode composition are loose particulate materials. [41] A dry-processed film electrode comprising: an active electrode material, a processed binder, and a multifunctional carbon black, wherein the film electrode contains a solvent residue prior to each drying process in an amount of not more than 1 wt.% based on the theoretical weight of the film electrode, wherein the multifunctional carbon black has a BET value of not more than about 1600 m 2 / g and an OAN value of not more than about 650 ml / 100 g. [42] The dry-processed film of claim 41, wherein the active electrode material is graphite and the multifunctional carbon black has a BET value in a range of about 35 to about 1600 m 2 / g and an OAN value in a range of about 120 to about 650 ml / 100 g. [43] The dry-processed film of claim 41, wherein the active electrode material is graphite and the multifunctional carbon black has a BET value in the range of about 50 to about 200 m 2 / g and an OAN value in the range of about 130 to about 240 ml / 100 g. [44] The dry-processed film of claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 80 to about 1600 m 2 / g and an OAN value in a range of about 120 to about 650 ml / 100 g. [45] The dry-processed film of claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 500 to about 1600 m 2 / g and an OAN value in a range of about 180 to about 650 ml / 100 g. [46] The dry-processed film of claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 80 to about 200 m 2 / g and an OAN value in a range of about 140 to about 280 ml / 100 g. [47] The dry-processed film of claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 1350 to about 1600 m 2 / g and an OAN value in a range of about 120 to about 220 ml / 100 g. [48] ​​The dry-processed film of claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 500 to about 650 m 2 / g and an OAN value in a range of about 180 to about 260 ml / 100 g. [49] The dry-processed film of any one of claims 41 to 48, wherein the multifunctional carbon black has one or more of the following properties: a surface energy of about 15 mJ / m 2 or less, a microcrystalline planar size according to Raman (La) of at least about 17 Å, a mesopore volume of at least about 0.35 cm 3 / g, a total mesopore and macropore volume of at least 1.0 cm 3 / g and a percentage crystallinity of at least 22%. [50] A dry-processed film electrode according to any one of claims 41 to 49, wherein the multifunctional carbon black is the only fibrillation aid in the film electrode. [51] The dry-processed film electrode according to any one of claims 41 to 49, further comprising at least one additional material selected from the group consisting of activated carbon, another multifunctional carbon black, and a conductive carbon additive. [52] A dry-processed film electrode according to any one of claims 41 to 51, wherein the dry-processed film electrode is free-standing or laminated to a substrate. [53] A process for producing an electrode composition, the process comprising: (a) subjecting a binder to high shear conditions in the presence of a multifunctional carbon black to process the binder; and (b) adding an active electrode material before, during or after step (a), wherein: the multifunctional carbon black has a BET value of not more than about 1500 m 2 / g and an OAN value of not more than about 650 ml / 100 g and the process is carried out without the addition of a solvent. [54] The method of claim 53, wherein the active electrode material is graphite and the multifunctional carbon black has a BET value in the range of about 35 to about 1600 m 2 / g and an OAN value in the range of about 120 to about 650 ml / 100 g. [55] The method of claim 53, wherein the active electrode material is graphite and the carbon black has a BET value in the range of about 50 to about 200 m 2 / g and an OAN value in the range of about 130 to about 240 ml / 100 g. [56] The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 80 to about 1600 m 2 / g and an OAN value in a range of about 120 to about 650 ml / 100 g. [57] The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 500 to about 1600 m 2 / g and an OAN value in a range of about 180 to about 650 ml / 100 g. [58] The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 80 to about 200 m 2 / g and an OAN value in a range of about 140 to about 280 ml / 100 g. [59] The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 1350 to about 1600 m 2 / g and an OAN value in a range of about 120 to about 220 ml / 100 g. [60] The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a BET value in a range of about 500 to about 650 m 2 / g and an OAN value in a range of about 180 to about 260 ml / 100 g. [61] A process according to any one of claims 53 to 60, wherein the multifunctional carbon black has one or more of the following properties: a surface energy of about 15 mJ / m 2 or less, a microcrystalline planar size according to Raman (La) of at least about 17 Å, a mesopore volume of at least about 0.35 cm 3 / g, a total mesopore and macropore volume of at least 1.0 cm 3 / g and a percentage crystallinity of at least 22%. [62] A process according to any one of claims 53 to 61, wherein the process is carried out in the presence of the multifunctional carbon black as the sole fibrillation aid.

Citation Information

Patent Citations

  • Mesoporous carbon black and processes for making same

    US10087330B2

  • Electrodes containing carbon black particles and related methods

    US10886535B2

  • Solvent-Free Process for Preparing Lithium-Ion Batteries

    US63322074P0

  • High surface area and low structure carbon blacks for energy storage applications

    US8895142B2

  • Anode electrode compositions for battery applications

    WO2020197670A1