Positive electrode active material for a lithium secondary battery, electrode and battery containing it

Optimized nickel-based lithium composite metal oxide particles with controlled doping and calcination address the durability issues of NCM, enhancing high-voltage stability and reducing side reactions for improved battery performance.

DE202018006941U1Active Publication Date: 2024-11-07LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE202018006941
Authority / Receiving Office
DE · DE
Patent Type
Utility models
Current Assignee / Owner
Priority Date
2018-11-20
Filing Date
2018-11-21
Publication Date
2024-11-07
Estimated Expiration
2028-11-30

AI Technical Summary

Technical Problem

Lithium nickel cobalt manganese oxide (NCM) positive electrode active materials exhibit inferior performance and durability issues when operated at high voltages due to higher Li deintercalation rates and instability at high states of charge, necessitating improved durability characteristics for use in lithium secondary batteries.

Method used

Development of nickel-based lithium composite metal oxide particles with specific crystal grain sizes and controlled doping or coating of metals within the crystal lattice or on the surface, optimized through precise calcination temperatures and metal content, ranging from 2500 to 6000 ppm, to stabilize the structure and reduce reactivity with electrolytes.

Benefits of technology

The optimized nickel-based lithium composite metal oxide particles enhance durability and stability at high voltages, reducing side reactions and gas formation, thereby improving battery performance and lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Positive electrode active material for a lithium secondary battery, wherein the positive electrode active material comprises: a single particle of a nickel-based lithium composite metal oxide, wherein the single particle contains several crystal grains, each crystal grain having a size of 180 nm to 300 nm, as measured by X-ray diffraction analysis with a Cu Kα X-ray beam (X-rα), and a metal doped into a crystal lattice of the single particle, wherein a total weight of the doped metal is 2500 to 6000 ppm, wherein the metal is one or more metals selected from the group consisting of Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery having improved cycle life characteristics at a high voltage, and to an electrode and a battery containing the same. STATE OF THE ART

[0002] With increasing technological development and the demand for mobile devices, the demand for secondary batteries as a power source has increased rapidly. Among these secondary batteries, lithium secondary batteries with high energy density and voltage, long cycle life, and low self-discharge have been commercially marketed and widely used.

[0003] Due to the recent price increase of cobalt (Co), many attempts have been made to increase price competitiveness by replacing lithium cobalt oxide (LCO), currently used as positive electrode active material for small batteries, with inexpensive lithium nickel cobalt manganese oxide (NCM).

[0004] In the case of NCM, the upper voltage limit in commercial cells is 4.2 V. When NCM with an upper voltage limit of 4.35 V is used in a small device, it has the problem of inferior performance compared to LCO. This is because the Li deintercalation of NCM is higher than that of LCO at the same upper voltage limit, and NCM becomes more unstable at high states of charge (SOC). As a result, a rapid deterioration of cycle characteristics occurs when NCM is used at a high voltage of 4.35 V or higher.

[0005] Accordingly, it is necessary to develop NCM positive electrode active materials with improved lifetime characteristics as a cost-effective positive electrode active material that can be operated at a high voltage. DISCLOSURE TECHNICAL PROBLEM

[0006] In order to solve the above problem, it is an object of the present invention to provide a positive electrode active material for a lithium secondary battery having improved cycle life characteristics at a high voltage. TECHNICAL SOLUTION

[0007] An embodiment of the present invention provides a single particle of a nickel-based lithium composite metal oxide containing a plurality of crystal grains.

[0008] In particular, the single particle may comprise a metal doped into a crystal lattice of the single particle, wherein the metal is one or more metals selected from the group consisting of Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B;or a metal compound coated on the surface of the single particle, wherein the metal of the metal compound is one or more metals selected from the group consisting of Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B, together with the metal doped into the crystal lattice of the single particle, wherein the metal is one or more metals selected from the group consisting of Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Mg, Na, Cu, Fe, Ca, S and B, wherein a total weight of the doped metal or the metal in the surface-coated metal compound is 2500 to 6000 ppm and each of the crystal grains contained in the single particle has a size of 180 nm to 300 nm as measured by Cu Kα X-ray (X-rα).;

[0009] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery, the positive electrode containing the above-described positive electrode active material, and a lithium secondary battery containing the positive electrode. EFFECT OF THE INVENTION

[0010] A positive electrode active material for a lithium secondary battery according to the present invention can improve cycle life characteristics at a high voltage. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1A to 1F show scanning electron microscopy (SEM) images of positive electrode active materials prepared in Examples 2, 4, 6, 8, 10, and 12, respectively; Fig. Figures 2A to 2G show TEM-ASTAR and HR-TEM images of Example 2 and Comparative Example 1; Fig. 3A and Fig.3B show the gas generation of positive electrode active materials according to Examples and Comparative Examples; and Fig. 4A and Fig. 4B shows graphs comparing the lifetime characteristics according to Experimental Example 3. BEST MODE FOR CARRYING OUT THE INVENTION

[0011] Hereinafter, a method for producing a positive electrode active material for a lithium secondary battery, a positive electrode active material produced by the method, a positive electrode containing the positive electrode active material, and a lithium secondary battery according to specific embodiments of the present invention will be described.

[0012] In this specification and claims, "multiple crystal grains" means a crystal formed from two or more crystal particles with an average crystallite size within a certain range. Here, the crystallite size of the crystal grain can be quantitatively analyzed by X-ray diffraction (XRD) analysis using Cu Kα X-rays (X-rα). Specifically, the prepared particles are placed in a holder, and the diffraction pattern obtained by irradiating the particles with X-rays is analyzed, thereby quantitatively analyzing the average crystallite size of the crystal grain.

[0013] In the present description and claims, D50 can be defined as a particle size at 50% of a particle size distribution and can be measured by a laser diffraction method.

[0014] Furthermore, it should be understood that the terms or words used in the specification and claims are not to be interpreted with the meaning defined in commonly used dictionaries, but the words or terms are to be interpreted to have a meaning consistent with their meaning in the context of the relevant prior art and the technical idea of ​​the invention, based on the principle that an inventor can reasonably define the meaning of the words or terms to best explain the invention. Positive electrode active material

[0015] The present invention provides two exemplary embodiments of a positive electrode active material in the form of a single particle.

[0016] In particular, individual particles of the two exemplary embodiments can usually contain: 1) a single particle of a nickel-based lithium composite metal oxide; 2) several crystal grains, each with a size of 180 nm to 300 nm, analyzed by X-ray diffraction (XRD) using a Cu-Kα X-ray beam (X-rα); and 3) a metal doped into the crystal lattice, wherein the metal is one or more metals selected from the group consisting of M = Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B. 4) However, the individual particles of the two exemplary embodiments can be distinguished from each other by a surface coating. 4-1) Specifically, the single particle of an exemplary embodiment (hereinafter referred to as “first single particle”) contains the metal doped into its crystal lattice (one or more metals selected from the group consisting of M = Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B), but its surface is not coated. 4-2) The single particle of another exemplary embodiment (hereinafter referred to as “second single particle”) contains the metal (one or more metals selected from the group consisting of M = Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B) doped into its crystal lattice, and a metal oxide (one or more metals selected from the group consisting of M' = Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B) coated on its surface. 4-3) However, in the first and second single particles, the total content of the metal doped into its crystal lattice and the metal of the metal oxide coated on its surface is controlled within a range of 2500 ppm to 6000 ppm. That is, since the first single particle does not contain any metal oxide coated on its surface, the content of the metal doped into its crystal lattice is 2500 ppm to 6000 ppm. Furthermore, in the second single particle, the total content of the metal doped into its crystal lattice and the metal of the metal oxide coated on its surface is 2500 ppm to 6000 ppm.

[0017] The first and second individual particles may have the properties of 1) to 4) and thereby contribute to improving the lifetime characteristics of a battery at a high voltage.

[0018] The properties of 1) to 4) of the first and second individual particles are described in detail below. Shape of the particles and size of the crystal grains

[0019] 1) Generally, a nickel-based lithium composite metal oxide is a secondary particle, but the first and second single particles are a nickel-based lithium composite metal oxide in the form of a single particle.

[0020] Specifically, a secondary particle of a nickel-based lithium composite metal hydroxide prepared by co-precipitation is used as a precursor, this precursor is mixed with a lithium raw material, and this mixture is calcined at a temperature lower than 960°C to obtain a secondary particle of a nickel-based lithium composite metal oxide.

[0021] However, if the calcination temperature is increased to 960°C or higher, the particle no longer exhibits a secondary particle shape, and single particles of the nickel-based lithium composite metal oxide can be obtained. This resulting product can be used as single particles of the first and second embodiments.

[0022] 2) Meanwhile, the secondary particle of a nickel-based lithium composite metal oxide and the single particles of the two embodiments contain multiple crystal grains regardless of the calcination temperature. "Containing multiple crystal grains" here means a crystal composed of two or more crystal particles having an average crystallite size within a certain range.

[0023] The crystallite size of the crystal grain can be quantitatively analyzed by X-ray diffraction (XRD) analysis using a copper Kα X-ray (X-rα). Specifically, the prepared particles are placed in a holder, and the diffraction pattern obtained by irradiating the particles with X-rays is analyzed, thereby quantitatively analyzing the average crystallite size of the crystal grain.

[0024] However, depending on the calcination temperature, a difference in crystal grain size may occur. In particular, when calcination is carried out at a low temperature below 960°C, crystal grains with a size of less than 180 nm may be obtained. That is, when the crystal grain size is less than 180 nm, it is difficult to obtain a single particle with a perfect shape. As a result, there is a risk that the interface between a positive electrode active material and an electrolyte becomes large, and the contact between the particles and the electrolyte increases due to a volume change during charge / discharge. Furthermore, when the average crystallite size of the particles exceeds 300 nm, there is a risk that the capacity will be reduced due to the enlargement of the crystal grains.

[0025] On the other hand, when the single particles of the first and second embodiments are excessively calcined at a temperature of 960°C or higher, particularly at 960°C to 1100°C, for example, at 990°C to 1100°C, coarsening of the crystal grains may occur, and therefore crystal grains having a size of up to 180 nm to 300 nm may be contained.

[0026] As such, the first and second single particles containing the coarsened crystal grains (180 nm to 300 nm) have a lower specific surface area (BET) than the secondary particle of a nickel-based lithium composite metal oxide containing smaller crystal grains, and therefore its reactivity with an electrolyte is low, and gas formation and release of internal metals can be reduced.

[0027] In general, the size of the single particle and the size of the crystal grain in the single particle increase with increasing calcination temperature at the same composition, regardless of the particle shape. However, the results of X-ray diffraction analysis using a Cu Kα X-ray (X-rα) show that the crystal grains in the single particles of the two embodiments have a larger size when overcalcined at a temperature of 990°C (Examples 1 to 6) than those with the same composition overcalcined at a temperature of 1010°C (Examples 7 to 12). This is because the patterns resulting from overcalcination at 1010°C (Examples 7 to 12) are related to the degree of aggregation of the single particles according to the calcination temperature and a measuring device and do not deviate from the general trend.

[0028] When individual particles are overcalcined at 990°C (Examples 1 to 6), relatively small individual particles can aggregate and take on the appearance of secondary particles. Therefore, XRD is assumed to detect the secondary particle-like appearance and interpret the boundaries between the individual particles as grain boundaries, thus capturing the individual particle size as the crystal grain size.

[0029] However, when the individual particles are overcalcined at 1010°C (Examples 7 to 12), relatively large individual particles can be observed separately while maintaining a certain distance from each other. Therefore, XRD is expected to detect individual particles and accurately identify the crystal grain size within the individual particles. Average particle size (D50) and crystal structure

[0030] There are differences in the average particle size (D50) and crystal structure between the secondary particles of the nickel-based lithium composite metal oxide and the individual particles of the two embodiments.

[0031] The average particle size (D50) of the secondary particles of the nickel-based lithium composite metal oxide may be 10 µm to 18 µm, and the average particle size (D50) of the individual particles of the two embodiments may be 3.5 µm or more to 8 µm or less.

[0032] As the particle D50 decreases, the BET specific surface area of ​​an active material increases. However, the BET reduction due to the increase in crystal grain size caused by overcalcination is more pronounced than the BET increase due to a reduction in particle size. As a result, the interface between an electrolyte and a positive electrode active material can be minimized to reduce side reactions and improve battery performance. Furthermore, by producing the active material in the form of small particles, capacity and efficiency can be increased, and the individual particles are easier to manufacture.

[0033] If the average particle size (D50) of the individual particles of the two embodiments is less than 3.5 μm, there is a risk of reducing the durability of the electrolyte and the positive electrode active material. If the average particle size (D50) of the individual particles of the two embodiments is more than 8 μm, there is a risk of capacity reduction due to overcalcination and a reduction in lifetime characteristics. Therefore, the average particle size (D50) of the individual particles of the two embodiments can be controlled in the range of 3.5 μm or more to 8 μm or less.

[0034] The crystal lattice structure of the secondary particles of the nickel-based lithium composite metal oxide, however, can exhibit a layered structure throughout the particle interior. This is due to the uniform formation of a layered structure consisting of lithium (Li) layer - cation mixed layer - lithium (Li) layer - cation mixed layer from the surface of the particle to the center of the particle at a temperature below 960°C.

[0035] In contrast, the individual particles of the two embodiments may have different crystal structures in their central region and in their surface region. This is due to the structural change of the particle surface from the layered structure to a rock salt structure, a spinel structure, or a mixed structure thereof at a temperature of 960°C or higher. In particular, at a temperature of 960°C or higher, 960°C to 1100°C, or, for example, 990°C to 1100°C, a part of the lithium on the surface of the individual particles of the nickel-based lithium composite metal oxide is lost, and the Ni 2+ Ions from the lower region migrate into the underlying lithium (Li) layer, resulting in a gradual degradation of the mixed cation layer. These successive reactions can occur from the surface of the individual particles of the nickel-based lithium composite metal oxide down to a certain depth.

[0036] In particular, the individual particles of the two embodiments can have a surface region and a central region which differ from each other with regard to the crystal lattice structure.

[0037] More specifically, the surface region of the individual particles of the two embodiments may contain a rock salt structure, a spinel structure, or a mixed structure thereof from the surface of an individual particle to a depth of 0.13% to 5.26%, for example, a depth of 0.13% to 2.63% of the radius of the individual particle. Meanwhile, the central region of the individual particles of the two embodiments may have a layered structure from the interface with the surface region to the center of the individual particle.

[0038] The surface area of ​​the rock salt structure, the spinel structure, or the mixed structure thereof of the single particles of the two embodiments can have low reactivity with an electrolyte, can be structurally stable, and can maintain the structural stability even when a charging voltage of more than 4.2 V, 4.4 V or more, or 4.45 V or more is applied, compared with the surface area of ​​the layered structure of the secondary particles of the nickel-based lithium composite metal oxide. composition

[0039] 3) The first single particle may contain a metal (M) doped into the crystal structure of a lithium composite metal oxide represented by the following chemical formula 1; and the second single particle may contain, in addition to the metal (M) doped into the crystal structure of the lithium composite metal oxide represented by the following chemical formula 1, a metal compound coated on the surface of the single particle: Li a (No x Mn y Co2)O 2+b (1) wherein in the chemical formula 1, a, x, y and z represent a molar ratio of each element in the lithium composite metal oxide.

[0040] The metal (M) doped into the crystal lattice of the first and second single particles and the metal (M') of the metal compound coated on the surface of the second single particle may be the same or different from each other, and may each be one or more metals selected from the group consisting of Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Mg, Na, Cu, Fe, Ca, S and B.

[0041] In the first and second individual particles, the element (M) may be located only on a part of the surface of the particle, depending on the position preferred by the element M, and it may be arranged with a concentration gradient from the surface of the particle to the center of the particle, or it may be present uniformly throughout the particle.

[0042] When the first and second single particles are doped or coated and doped with the same element (M), the high-voltage properties of the active material can be further improved due to the stabilization of the surface structure. Among the elements, in particular, the three elements Ti, Mg, and Zr can be doped or coated and doped as element (M), in view of excellent surface structure stabilization effects, or only Zr can be doped or coated and doped.

[0043] The element (M) can be doped or coated and doped in an amount of 2500 ppm to 6000 ppm. If the amount of the element (M) is less than 2500 ppm, the structure-stabilizing effect due to the doping or coating of the element (M) may be poor. If the amount of the element (M) is more than 6000 ppm, there is a risk of capacity reduction and deterioration of the lifetime characteristics and transmission rate characteristics due to increased resistance. The element (M) can be coated or doped in a specific amount of 2500 to 5500 ppm, and more specifically 3500 ppm to 5000 ppm, to achieve an excellent improvement effect by controlling the element (M) content.

[0044] Meanwhile, the chemical formula 1 may correspond to a composition of a well-known secondary particle of a nickel-based lithium composite metal oxide.

[0045] For example, in Chemical Formula 1, lithium (Li) may be contained in an amount equal to a, specifically 0.95≤a≤1.2. If a is less than 0.95, there is a risk of deterioration in the performance characteristics of a battery due to an increase in the interfacial resistance generated at the contact surface between the positive electrode active material and the electrolyte. Conversely, if a is more than 1.2, there is a risk of reduction in the initial discharge capacity of the battery. In view of the effects of combining with the characteristic structure of the active material according to an embodiment of the present invention, a may more specifically satisfy 0.98≤a<1.07, and even more specifically a=1.

[0046] In chemical formula 1, nickel (Ni) is an element that contributes to high voltage and high capacity of a secondary battery. Nickel (Ni) can be used in an amount equal to x, especially 0 <x<0,6, enthalten sein, sofern die Bedingung x+y+z=1 erfüllt ist. Wenn x 0 ist, besteht die Gefahr einer Verschlechterung der Lade- / Entladekapazitätseigenschaften. Wenn x 0,6 oder mehr beträgt, besteht die Gefahr einer Verschlechterung der strukturellen und thermischen Stabilität des Aktivmaterials und, im Ergebnis, einer Verschlechterung der Lebensdauereigenschaften. Im Hinblick auf Hochspannungs- und Hochkapazitätseffekte durch Kontrolle des Nickelgehalts kann das Nickel insbesondere in einer Menge von 0,4≤x<0,6 und noch spezifischer in einer Menge von 0,5≤x<0,6 enthalten sein, sofern die Bedingung x+y+z=1 erfüllt ist.

[0047] Furthermore, in Chemical Formula 1, manganese (Mn) is an element that contributes to improving the thermal stability of the active material, and it can be contained in an amount corresponding to y, specifically 0≤y≤0.4, provided that the condition x+y+z=1 is satisfied. When y is more than 0.4, there is a risk of deterioration of the durability characteristics due to increased release of manganese. With a view to improving the thermal stability of the active material and improving the durability characteristics by controlling the manganese content, the manganese can be contained more specifically in an amount of 0.1≤y<0.4, and even more specifically 0.1≤y≤0.3, provided that the condition x+y+z=1 is satisfied.

[0048] Furthermore, in Chemical Formula 1, cobalt (Co) is an element that contributes to improving the charge / discharge cycle characteristics of the active material, and it can be contained in an amount corresponding to z, specifically 0≤z<1, provided the condition x+y+z=1 is satisfied. When z is 1, there is a risk of deterioration of the charge / discharge capacity due to deterioration of structural stability. Regarding the improvement of the cycle characteristics of the active material by controlling the cobalt content, the cobalt can be contained more specifically in an amount of 0.1≤z<0.4, and even more specifically 0.1≤z≤0.3.

[0049] That is, the chemical formula 1 can satisfy the following conditions: a=1, 0≤b≤0.02, 0.4≤x<0.6, 0.1≤y<0.4, 0.1≤z<0.4, and x+y+z=1, and in particular LiNi 0,5 Co 0,2 Mn 0,3 O2, LiNi 0,5 Co 0,3 Mn 0,2O2 or the like. Any of these or a mixture of two or more of them may be included in the positive electrode active material. Method for producing a positive electrode active material

[0050] The present invention provides a process for producing the individual particles of the two embodiments.

[0051] In particular, the first single particle can be produced by a series of processes including the following steps: Preparing a first mixture containing a lithium composite metal hydroxide particle having a D50 of 8 µm or less, a lithium raw material, and a metal compound (one or more selected from the group consisting of M = Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Mg, Na, Cu, Fe, Ca, S, and B); and

[0052] Calcining the first mixture at a temperature of 960°C or higher.

[0053] In the step of calcining the first mixture at a temperature of 960°C or higher, the single particle of a nickel-based lithium composite metal oxide containing a plurality of crystal grains can be synthesized, and at the same time, the metal (M) of the metal (M) compound can be doped into the crystal lattice of the single particle of the lithium composite metal oxide, thereby obtaining the first single particle.

[0054] Regarding the content of the metal doped in the finally obtained first single particles, the content of the metal (M) compound can be controlled in a range of 2500 ppm to 6000 ppm relative to the total weight of the first mixture.

[0055] Meanwhile, the second single particle can be produced through a series of processes that include the following steps: Preparing a first mixture containing a nickel-based lithium composite metal hydroxide particle having a D50 of 8 µm or less, a lithium raw material, and a metal compound (one or more selected from the group consisting of M = Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Mg, Na, Cu, Fe, Ca, S, and B); Calcining the first mixture at a temperature of 960°C or higher; Producing a second mixture containing the calcined product of the first mixture and a metal compound (one or more selected from the group consisting of M' = Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Mg, Na, Cu, Fe, Ca, S and B); and Calcining the second mixture at a temperature of 350°C to 800°C.

[0056] As in the preparation of the first single particle, in the step of calcining the first mixture at a temperature of 960°C or higher during the preparation of the second single particle, the single particle of a nickel-based lithium composite metal oxide containing a plurality of crystal grains may be synthesized, and at the same time, the metal (M) of the metal (M) compound may be doped into the crystal lattice of the single particle of the lithium composite metal oxide.

[0057] However, in contrast to the preparation of the first single particle, the step of calcining the second mixture at a temperature of 350°C to 800°C may additionally be carried out after the preparation of the second mixture containing the calcined product of the first mixture and the metal (M') compound, thereby obtaining the second single particle.

[0058] Furthermore, the total content of the metal (M) compound and the metal (M') compound may be 2500 ppm to 6000 ppm based on the total weight of the first mixture and the second mixture.

[0059] With regard to the process for producing the first or second single particle, overlaps with the above explanations are omitted and process features are described in detail. Calcination process

[0060] During the preparation of the first and second single particles, when the first mixture, that is, the mixture of the lithium composite metal hydroxide particle having a D50 of 8 μm or less, the lithium raw material, and the metal (M) compound is calcined at a temperature of 960°C or higher, the single particle of the lithium composite metal oxide containing a plurality of crystal grains can be synthesized, and at the same time, the metal (M) of the metal (M) compound can be doped into the crystal lattice of the single particle of the lithium composite metal oxide.

[0061] The calcination temperature can be set at 960°C or higher, taking into account the above-described factors such as the production of single particles, the size control of crystal grains, etc. More specifically, the calcination temperature can be set at a temperature of 960°C to 1100°C, for example, 990°C to 1100°C. Especially when the Ni content is less than 0.6, overcalcination cannot occur at a temperature below 960°C. Therefore, when the calcination temperature is below 960°C, the D50 value of the active material to be produced is not as large as the range of the invention, so there is a risk of deterioration of battery performance due to side reactions between the electrolyte and the positive electrode active material at a high SOC.In contrast, a calcination temperature of more than 1100°C is not preferred because the capacity may decrease due to the enlargement of the crystal grains.

[0062] The overcalcination process can be carried out in an oxidizing atmosphere containing oxygen, more specifically in an atmosphere with an oxygen content of 20 vol% or more.

[0063] The lithium composite metal hydroxide particle having a D50 of 8 µm or less can be a precursor for producing the above-described single particle of one embodiment, which is represented by the following chemical formula 2: (No x Mn y Co2)OH 2+b (2) where in the chemical formula 2 0.95≤a≤1.2, 0≤b≤0.02, 0 <x<0,6, 0≤y≤0,4, 0≤z<1, und x+y+z=1.

[0064] In particular, the average particle size (D50) of the lithium composite metal hydroxide particle can be from 4 μm or more to 8 μm or less. When the positive electrode active material is prepared using the precursor having a size within the above range, it is possible to produce a positive electrode active material with a D50 of 4 μm or more to 8 μm or less in the form of a single particle.

[0065] In particular, the lithium composite metal hydroxide particle having a D50 of 8 µm or less may be an oxide, hydroxide or oxyhydroxide containing nickel, cobalt and manganese as a precursor.

[0066] The precursor can be produced by a conventional method, except that the raw materials of nickel, cobalt, and manganese are used in the amounts defined in Chemical Formula 1, and the average particle size (D50) of the finally produced precursor is 7 μm or less. For example, the precursor can be produced by a solid-phase method in which nickel oxide, cobalt oxide, and manganese oxide are mixed and then subjected to heat treatment, or it can be produced by a coprecipitation method in which the corresponding metal salts containing nickel, cobalt, and manganese are added to a solvent, particularly water or a mixture of water and an organic solvent miscible with water (particularly an alcohol, etc.).

[0067] Furthermore, the lithium raw material may be a lithium-containing oxide, sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, oxyhydroxide, etc., and in particular, Li2CO3, LiNO3, LiNO2, LiOH, LiOH.H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, etc. Any of these or a mixture of two or more thereof may be used. In view of the reaction efficiency and reducing the formation of byproducts during the reaction with the precursor to form the lithium composite metal oxide, the lithium raw material may be Li2O or Li2CO3.

[0068] Furthermore, the raw material of the doping element M may be an element M-containing oxide, sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, oxyhydroxide, etc. Here, M is the same as described above.

[0069] The precursor for forming the lithium composite metal oxide, the lithium raw material, and the raw material of the element M or M' can be used after being mixed in amounts corresponding to the content range of lithium in the finally produced lithium composite metal oxide of the chemical formula 1 and the content range of the element M contained in the positive electrode active material (corresponding to a sum of M and M' in the production process). Coating process

[0070] The method for producing the second single particle may further include the steps of preparing a second mixture containing the calcined product of the first mixture and a metal compound (one or more metals selected from the group consisting of M' = Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Mg, Na, Cu, Fe, Ca, S and B), and calcining the second mixture at a temperature of 350°C to 800°C after the step of calcining the first mixture at a temperature of 960°C or higher.

[0071] When this step is additionally included, a coating layer containing the metal compound (M') may be formed on all or part of the surface of the single particle, and the metal compound may be in the form of, for example, a metal oxide.

[0072] Here, the coating element M' may be an element the same as or different from the doping element M. Furthermore, the raw material of the coating element M' may be an oxide, sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, oxyhydroxide, etc. containing an element M'. Here, M is the same as described above. An additional heat treatment process for forming the coating layer may be carried out, as in the doping process, at a temperature of 350°C to 800°C, more specifically at a temperature of 350°C to 650°C, in an oxidizing atmosphere containing oxygen.

[0073] If the temperature of the secondary heat treatment for the additional coating is lower than 350°C, the coating layer cannot be sufficiently formed, and if the temperature is higher than 800°C, there are problems with cation mixing and deterioration of the capacity and transfer rate characteristics. Post-treatment process

[0074] Meanwhile, a cooling process may optionally be performed after the overcalcination during the production of the first single particle and after the secondary heat treatment during the production of the second single particle.

[0075] The cooling process can be carried out by a common method, especially a method such as natural cooling in an air atmosphere or hot air cooling.

[0076] Since the positive electrode active material for a lithium secondary battery produced by the above-described manufacturing method can exhibit a reduced specific surface area (BET), an interface with an electrolyte can be reduced. Furthermore, the amount of remaining lithium in the active material is reduced by overcalcination, thereby reducing side reactions with an electrolyte. Accordingly, the positive electrode active material can exhibit excellent battery performance and cycle life characteristics when the battery is operated at a high voltage of 4.35 V or more, and in particular, it can exhibit excellent high-temperature cycle life characteristics due to its structural stability. Lithium secondary battery

[0077] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery, wherein the positive electrode contains the positive electrode active material containing one of the single particles of the two embodiments, and a lithium secondary battery containing the positive electrode.

[0078] The positive electrode and the lithium secondary battery, each manufactured using the positive electrode active material described above, can exhibit excellent cycle life characteristics even at a high SOC.

[0079] Specifically, the positive electrode may include a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector and containing the positive electrode active material described above.

[0080] The positive electrode collector is not particularly limited as long as it exhibits conductivity without causing chemical changes in a battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, and aluminum, or stainless steel surface-treated with carbon, nickel, titanium, or silver, can be used. The positive electrode collector can have a thickness of 3 μm to 500 μm, and the adhesion of the positive electrode active material can be improved by forming fine roughness on the surface of the collector. For example, the collector can be in a variety of forms, such as a film, sheet, foil, mesh, porous material, foamed material, nonwoven material, etc.

[0081] Further, the positive electrode active material layer may contain a conductive material and a binder together with the above-described positive electrode active material.

[0082] Here, the conductive material is used to provide an electrode with conductivity and is not particularly limited as long as it has electrical conductivity without causing chemical changes in the battery. Specific examples may include: carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, etc.; graphite such as natural or artificial graphite; metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive whiskers such as zinc oxide, potassium titanate, etc.; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, etc. These can be used alone or as a mixture of two or more thereof. The conductive material may be contained in an amount of 1% to 30% by weight based on the total weight of the positive electrode active material layer.

[0083] The binder also improves the adhesion between the positive electrode active materials and the adhesive force between the positive electrode active material and the collector. Specific examples may include: polyvinylidene fluoride (PVDF), a vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, an ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or combinations thereof. These can be used alone or as a mixture of two or more thereof. The binder may be contained in an amount of 1% to 30% by weight based on the total weight of the positive electrode active material layer.

[0084] The positive electrode can be manufactured by a conventional positive electrode manufacturing method, except for using the above-described positive electrode active material. Specifically, the positive electrode can be manufactured by applying a slurry to form a positive electrode active material layer onto a positive electrode collector, followed by drying and rolling. The slurry is prepared by mixing the above-described positive electrode active material and optionally the binder and conductive material in a solvent. Here, the type and content of the positive electrode active material, the binder, and the conductive material are the same as described above.

[0085] The solvent can be any solvent commonly used in the field and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc. These can be used alone or as a mixture of two or more. Taking into account the coating thickness of the slurry and the production yield, the solvent can be used in an amount sufficient to dissolve or disperse the positive electrode active material, the conductive material, and the binder, and to impart a viscosity to the slurry that allows for excellent thickness uniformity when applied to prepare the positive electrode.

[0086] As an alternative method, the positive electrode can be prepared by casting the slurry for forming the positive electrode active material layer onto a separate support and then laminating a film peeled from the support onto the positive electrode collector.

[0087] Another embodiment of the present invention provides an electrochemical device containing the positive electrode. The electrochemical device may be, in particular, a battery, a capacitor, etc., and more specifically, a lithium secondary battery.

[0088] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode opposite the positive electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte. The positive electrode is the same as described above. In addition, the lithium secondary battery may optionally further include a battery container housing an electrode assembly consisting of the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.

[0089] In the lithium secondary battery, the negative electrode includes a negative electrode collector and a negative electrode active material layer disposed on the negative electrode collector.

[0090] The negative electrode collector is not particularly limited as long as it has high conductivity without causing chemical changes in a battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, or silver, or an aluminum-cadmium alloy can be used. The negative electrode collector can also typically have a thickness of 3 μm to 500 μm, and like the positive electrode collector, the adhesion of the negative electrode active material can be improved by forming fine roughness on the surface of the collector. For example, the collector can be in a variety of forms, such as a film, sheet, foil, mesh, porous material, foamed material, nonwoven material, etc.

[0091] Furthermore, the negative electrode active material layer may optionally contain a binder and a conductive material together with the negative electrode active material. The negative electrode active material layer can be prepared, for example, by applying and drying a slurry for forming the negative electrode on the negative electrode collector, the slurry being prepared by mixing the negative electrode active material and optionally the binder and the conductive material in a solvent, or by casting a composition for forming the negative electrode onto a separate support and then laminating a film peeled from the support onto the negative electrode collector.

[0092] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples may include one or a mixture of two or more of the following: a carbon material such as artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, etc.; a metal compound capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, a Si alloy, a Sn alloy, an Al alloy, etc.; a metal oxide capable of doping and dedoping lithium ions, such as SiO x(0<x<2), SnO2, Vanadiumoxid oder Lithium-Vanadiumoxid, und ein Verbundmaterial, das die Metallverbindung und das Kohlenstoffmaterial enthält, wie ein Si-C-Verbundmaterial oder ein Sn-C-Verbundmaterial. Das Negativelektrodenaktivmaterial kann auch ein Lithiummetalldünnfilm sein. Darüber hinaus können sowohl niederkristalliner als auch hochkristalliner Kohlenstoff usw. als Kohlenstoffmaterial verwendet werden. Der niederkristalline Kohlenstoff ist ein weicher oder harter Kohlenstoff, und der hochkristalline Kohlenstoff ist ein hochtemperaturkalzinierter Kohlenstoff, wie amorpher, plättchenförmiger, flockiger, sphärischer oder faseriger natürlicher Graphit oder künstlicher Graphit, Kish-Graphit, pyrolytischer Kohlenstoff, Kohlenstofffasern auf Mesophasenpechbasis, Mesokohlenstoff-Mikroperlen, Mesophasenpechen, aus Erdöl oder Kohlenteer gewonnene Kokse oder dergleichen.

[0093] In addition, the binder and the conductive material can be the same as described for the positive electrode.

[0094] Meanwhile, the separator in the lithium secondary battery serves to separate the negative electrode and the positive electrode and provide a passage for lithium ions. The separator is not particularly limited as long as it is used as a separator in a conventional lithium secondary battery, and particularly, a separator that has low resistance to electrolyte ion migration and excellent electrolyte solution absorption capability is preferred. Specifically, the separator may be a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, or the like, or a layered structure comprising two or more layers thereof.Alternatively, the separator can be a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fibers, polyethylene terephthalate fibers, or the like. To ensure heat resistance or mechanical strength, the separator can also be a coated separator containing ceramic components or polymeric materials, optionally used in a single- or multi-layer structure.

[0095] Furthermore, the electrolyte used in the present invention may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel polymer electrolyte, an inorganic solid electrolyte, an inorganic molten electrolyte, etc., which can be used in the manufacture of a lithium secondary battery, but the present invention is not limited thereto.

[0096] In particular, the electrolyte may contain an organic solvent and a lithium salt.

[0097] The organic solvent is not particularly limited as long as it can act as a medium that can migrate the ions involved in an electrochemical reaction of a battery. Specifically, the organic solvent can be: an ester-based solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; an ether-based solvent such as dibutyl ether, tetrahydrofuran, etc.; a ketone-based solvent such as cyclohexanone, etc.; an aromatic hydrocarbon-based solvent such as benzene, fluorobenzene, etc.; a carbonate-based solvent such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), etc.; an alcohol-based solvent such as ethyl alcohol, isopropyl alcohol, etc.; Nitriles such as R-CN (where R is a C2 to C20 hydrocarbon group having a linear, branched, or cyclic structure and may contain a doubly bonded aromatic ring or an ether bond), etc.; amides such as dimethylformamide, etc.; dioxolanes such as 1,3-dioxolane, etc.; or sulfolane. Among these compounds, the carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate, propylene carbonate, etc.) with high ionic conductivity and a high dielectric constant, which can increase the charge and discharge performance of a battery, and a linear carbonate-based compound with low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is even more preferable. In this case, if the cyclic carbonate and the chain carbonate are used after mixing in a volume ratio of about 1:1 to about 1:9, excellent performance of the electrolyte can be achieved.

[0098] The lithium salt is not particularly limited as long as it can provide lithium ions used in a lithium secondary battery. Specifically, the lithium salt can be: LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. The concentration of the lithium salt is preferably in a range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, an electrolyte has suitable conductivity and viscosity, so that excellent electrolyte performance can be achieved and lithium ions can migrate effectively.

[0099] In addition to the electrolyte components, in order to improve the life characteristics of the battery, suppress a decrease in battery capacity, improve the discharge capacity of the battery, etc., the electrolyte may further contain one or more additives such as a haloalkylene carbonate-based compound such as difluoroethylene carbonate, etc., pyridine, triethyl phosphite, triethanolamine, a cyclic ether, ethylenediamine, n-glyme, hexaphosphoric triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. Here, the additives may be contained in an amount of 0.1% to 5% by weight based on the total weight of the electrolyte.

[0100] The lithium secondary battery containing the positive electrode active material according to the present invention can stably exhibit excellent discharge capacity, output characteristics, and capacity retention rate, thereby being advantageously used in portable devices such as mobile phones, notebooks, digital cameras, etc., and electric vehicles such as hybrid electric vehicles (HEVs), etc.

[0101] Accordingly, another embodiment of the present invention provides a battery module including the lithium secondary battery as a cell unit, and a battery pack including the same.

[0102] The battery module or battery pack can be used as a power source for one or more medium and large devices, such as a power tool, an electric car, including an electric vehicle (EV), a hybrid electric vehicle and a plug-in hybrid electric vehicle (PHEV), or as an electricity storage system. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0103] The embodiments of the present invention will be described in detail below so that a person skilled in the art having ordinary knowledge in the field of the present invention can easily carry out the present invention. However, the present invention can be implemented in various other embodiments and is not limited to the embodiments described herein. Furthermore, the methods used in the experimental examples for measuring the physical properties of the active materials or precursors are the same as those described below. 1) Mean particle size D50 (µm): The particle sizes at 50% and 10% of the particle size distribution were measured for active materials and precursors, respectively, using a laser diffraction method (Microtrac MT 3000). 2) Crystallite size (nm): The crystal grain sizes (crystallite sizes, X-sizes) of the individual particles were measured using an X-ray diffraction analyzer (Bruker AXS D4-Endeavor XRD) to measure XRD (“X-ray diffraction”) with a Cu Kα X-ray beam (X-rα). 3) Doping amount and metal amount in the surface-coated metal compound: The amount of doped metal and / or the amount of metal in the surface-coated metal compound was measured using an inductively coupled plasma (ICP) spectrometer. Evaluation of the high-temperature properties of a 4.35 V full cell.

[0104] Each of the positive electrode active materials prepared in the following Examples and Comparative Examples, a conductive carbon black material, and a PVdF binder were mixed in a weight ratio of 96:2:2 in an N-methylpyrrolidone solvent to prepare a slurry for forming a positive electrode (viscosity: 5000 mPa s), and the slurry was coated on an aluminum collector with a thickness of 20 μm, dried, and rolled to prepare a positive electrode.

[0105] Further, artificial graphite MCMB (mesocarbon microbeads) as a negative electrode active material, a conductive carbon black material, a PVDF binder, and a BM-L301 dispersant were mixed in a weight ratio of 96.5:0.75:1.25:1.5 in an N-methylpyrrolidone solvent to prepare a slurry for forming a negative electrode, and the slurry was coated on a copper collector to prepare a negative electrode.

[0106] A porous polyethylene separator was placed between the positive and negative electrodes prepared as above to form an electrode assembly. The electrode assembly was housed in a case, and then an electrolyte was injected into the case to fabricate a lithium secondary battery. The electrolyte was prepared by dissolving 1.15 M lithium hexafluorophosphate (LiPF6) in an organic solvent consisting of ethylene carbonate / dimethyl carbonate / ethyl methyl carbonate (volume ratio of the mixture EC / DMC / EMC = 3 / 4 / 3).

[0107] High-temperature cycle life retention rate (%): The thus-prepared lithium secondary batteries were charged at 45°C with constant current / constant voltage (CC / CV) from 0.7 C to 4.35 V / 38 mA and then discharged with constant current (CC) from 0.5 C to 2.5 V, and a discharge capacity was measured. This process was repeated for 1 to 100 cycles, and the results are shown in the Fig. 4A and Fig. 4B shown. Examples 1 to 6 (overcalcination temperature: 990°C)Example 1

[0108] 94.91702 g of Ni 0,5 Co 0,3 Mn 0,2 (OH)2 precursor with a particle size D50 of 4.2 µm, 38.86741 g LiOH as lithium raw material and 0.444807 g ZrO2, 0.010392 g MgO and 0.02594 g TiO2 as raw materials of element M were dry mixed and then overcalcined at 990°C to obtain a LiNi 0,5 Co 0,3 Mn 0,2To prepare O2 positive electrode active material doped with 4000 ppm Zr / Mg / Ti (3500 ppm Zr, 250 ppm Mg and 250 ppm Ti) based on the total weight of the positive electrode active material. Example 2

[0109] A positive electrode active material doped with Zr / Mg / Ti was prepared in the same manner as in Example 1, except that a 5.2 µm precursor was overcalcined at 990°C and 4250 ppm Zr / Mg / Ti (3500 ppm Zr, 250 ppm Mg, and 500 ppm Ti) was doped. Example 3

[0110] LiNi 0,5 Co 0,3 Mn 0,2 O2 doped with 4250 ppm Zr / Mg / Ti from Example 2, 0.026291 g Al2O3 and 0.028722 g B2O3 as raw material of element M' were mixed and calcined at 990°C to prepare a doped positive electrode active material further coated with 900 ppm Al / B (500 ppm Al and 400 ppm B). Example 4

[0111] A positive electrode active material doped with Zr was prepared in the same manner as in Example 1, except that a 5.2 µm precursor was overcalcined at 990°C and 3500 ppm Zr was doped by using 0.444807 g of ZrO2 as the raw material of element M. Example 5

[0112] A positive electrode active material doped with Zr was prepared in the same manner as in Example 1, except that a 5.2 µm precursor was overcalcined at 990°C and 5500 ppm Zr was doped by using 0.698983 g of ZrO2 as the raw material of element M. Example 6

[0113] LiNi 0,5 Co 0,3 Mn 0,2 O2 doped with 4250 ppm Zr / Mg / Ti from Example 2 and 0.078872 g Al2O3 as raw material of element M' were mixed and calcined at 990°C to prepare a doped positive electrode active material further coated with 1500 ppm Al. Examples 7 to 12 (overcalcination temperature: 1010°C)Example 7

[0114] A LiNi 0,5 Co 0,3 Mn 0,2 O2 positive electrode active material doped with 4000 ppm Zr / Mg / Ti (3500 ppm Zr, 250 ppm Mg and 250 ppm Ti) based on the total weight of the positive electrode active material was prepared in the same manner as in Example 1, except that the overcalcination was carried out at a temperature of 1010°C instead of 990°C as in Example 1. Example 8

[0115] A positive electrode active material doped with Zr / Mg / Ti was prepared in the same manner as in Example 1, except that overcalcination was carried out at a temperature of 1010°C instead of 990°C as in Example 2, and 4250 ppm Zr / Mg / Ti (3500 ppm Zr, 250 ppm Mg and 500 ppm Ti) was doped in the same manner as in Example 2. Example 9

[0116] LiNi 0,5 Co 0,3 Mn 0,2 O2 doped with 4250 ppm Zr / Mg / Ti was prepared in the same manner as in Example 3, except that the overcalcination was performed at a temperature of 1010°C instead of 990°C as in Example 3. Subsequently, the doped positive electrode active material was further coated with 900 ppm Al / B (500 ppm Al and 400 ppm B) in the same manner as in Example 3. Example 10

[0117] A positive electrode active material doped with 3500 ppm Zr was prepared in the same manner as in Example 4, except that the overcalcination was carried out at a temperature of 1010°C instead of 990°C as in Example 4. Example 11

[0118] A positive electrode active material doped with 5500 ppm Zr was prepared in the same manner as in Example 5, except that the overcalcination was carried out at a temperature of 1010°C instead of 990°C as in Example 5. Example 12

[0119] LiNi 0,5 Co 0,3 Mn 0,2 O2 doped with 4250 ppm Zr / Mg / Ti was prepared in the same manner as in Example 6, except that the overcalcination was performed at a temperature of 1010°C instead of 990°C as in Example 6. Subsequently, the doped positive electrode active material was further coated with 1500 ppm Al in the same manner as in Example 6. Comparison example 1

[0120] A positive electrode active material doped with 4250 ppm Zr / Mg / Ti was prepared in the same manner as in Example 2, except that the calcination was carried out at a temperature of 920°C. Comparison example 2

[0121] A positive electrode active material doped with 4250 ppm Zr / Mg / Ti was prepared in the same manner as in Example 2, except that the calcination was carried out at a temperature of 950°C. Comparison example 3

[0122] A positive electrode active material doped with 1500 ppm Zr was prepared in the same manner as in Example 4 except that 1500 ppm Zr was doped. Comparison example 4

[0123] A positive electrode active material doped with 7500 ppm Zr was prepared in the same manner as in Example 4 except that 7500 ppm Zr was doped. Comparison example 5

[0124] EinLiNi 0,5 Co 0,3 Mn 0,2 O 2- Positive electrode active material was prepared in the same manner as in Example 4 except that no Zr doping treatment was performed. Comparison example 6

[0125] A positive electrode active material doped with 4250 ppm Zr / Mg / Ti was prepared in the same manner as in Example 2, except that an 11 µm precursor was calcined at a temperature of 920°C. Comparison example 7

[0126] A positive electrode active material doped with 1500 ppm Zr was prepared in the same manner as in Example 4, except that a 12 µm precursor was overcalcined at a temperature of 960°C and doped with 1500 ppm Zr. Experimental Example 1 (Confirmation of crystal grain size by Cu Kα XRD analysis)

[0127] Each of the active materials prepared in Examples 2, 4, 6, 8, 10 and 12 was observed and analyzed using a scanning electron microscope (SEM), etc., and the results are shown in the Fig. 1A (Example 2), 1B (Example 4), 1C (Example 6), 1D (Example 8), 1E (Example 10), and 1F (Example 12). Furthermore, the crystal grain sizes of the positive electrode active materials of Examples 1 to 8 and 10 to 12, as well as Comparative Examples 1 to 7, were confirmed using an X-ray diffraction analyzer (Bruker AXS D4-Endeavor XRD), and the results are shown in Table 1 below.

[0128] In detail, the crystal grain sizes of the positive electrode active materials were calculated by performing X-ray diffraction analysis using a Cu source (Cu Kα), obtaining a full width at half maximum (FWHM) from the analysis results, and then substituting the full width at half maximum into the following equation. τ=(K⋅λ) / (β⋅cosθ)

[0129] The above equation is commonly known as the Scherrer equation, where K is a form factor, usually 0.9, without a unit, λ is the X-ray wavelength, β is the full width at half maximum of a peak with maximum intensity, and θ is an angle of the peak maximum. Substituting the corresponding values ​​into the equation, the crystal grain size τ is calculated. Table 1 Total amount of coating and doping (ppm) Crystal grain size (nm) Example 1 4000 264 Example 2 4250 233 Example 3 5150 207 Example 4 3500 225 Example 5 5500 233 Example 6 5750 229 Example 7 4000 181 Example 8 4250 194 Example 10 3500 194 Example 11 5500 195 Example 12 5750 206 Comparison example 1 4250 151 Comparison example 2 4250 178 Comparison example 3 1500 215 Comparison example 4 7500 239 Comparison example 5 0 232 Comparison example 6 4250 154 Comparison example 7 1500 199

[0130] With reference to the Fig. 1A to 1F, it was confirmed that the active materials prepared according to the present invention were prepared in the form of single particles having a particle size of 3.5 µm to 10 µm.

[0131] Further, referring to Table 1, it was confirmed that when a precursor with an average particle size of 7 μm or less was used and overcalcination was performed at 960°C or higher (Examples 1 to 12), the crystal grain size measured by Cu K-α X-ray (X-rα) was relatively large, ranging from 180 nm to 300 nm. In contrast, when the calcination temperature was lower than 960°C (Comparative Examples 1, 2, and 6), the crystal grain size was less than 180 nm regardless of the precursor size, indicating that overcalcination was not occurring.

[0132] However, for the same compositions, it is common for the size of the individual particle and the size of the crystal grain within the individual particle to increase with increasing calcination temperature. However, according to the results measured with Cu-Kα X-ray (X-rα), the sizes of the crystal grains overcalcined at 960°C (Examples 1 to 6) were larger than those of the crystal grains overcalcined at 1010°C (Examples 7 to 12) when their compositions were the same. This is because the patterns resulting from overcalcination at 1010°C (Examples 7 to 12) relate to the degree of aggregation of the individual particles depending on the calcination temperature and a measuring instrument and do not deviate from the general trend.

[0133] When individual particles are overcalcined at 990°C (Examples 1 to 6), relatively small individual particles can aggregate together and resemble secondary particles. This means that XRD detects the secondary particle-like appearance and recognizes the boundaries between the individual particles as grain boundaries, thus recognizing the individual particle size as the crystal grain size.

[0134] In contrast, when single particles are overcalcined at 1010°C (Examples 7 to 12), relatively large single particles can be observed separately while maintaining a distance from each other. This means that XRD detects the individual single particles and correctly determines the crystal grain size within the single particles.

[0135] In other words, those overcalcined at 1010°C (Examples 7 to 12) had smaller crystal grains than those overcalcined at 960°C (Examples 1 to 6) as measured by a Cu-Kα X-ray (X-rα), which is due to limitations of the measuring instrument.

[0136] However, all those overcalcined at 960 °C (Examples 1 to 6) and those overcalcined at 1010 °C (Examples 7 to 12) had practical crystal grain sizes within the error range (± 1%) of the value measured with a Cu-Kα X-ray (X-rα), ie, within the range of 180 nm to 300 nm. Experimental Example 2 (Evaluation of the Crystal Structure)

[0137] Example 2 and Comparative Example 1 were observed using TEM-ASTAR and HR-TEM instruments. In particular, an HR-TEM image of Example 2 is shown in Fig. 2A, a TEM-ASTAR image of the surface of it in the Fig. 2B and Fig.2C and a TEM-ASTAR image of the central region of it in Fig. 2D. Furthermore, Fig. 2E an HR-TEM image of Comparative Example 1, in Fig. 2F a TEM-ASTAR image of the surface of it and in Fig. 2G shows a TEM-ASTAR image of the central region.

[0138] With reference to the Fig. 2A to 2G, the crystal structure of the surface region can vary depending on the calcination temperature of the precursor, even if the compositions are the same. In particular, Comparative Example 1, which was not overcalcined, showed uniform formation of a layered crystal lattice structure from the surface to the center.

[0139] In contrast, overcalcined Example 2 exhibited different crystal structures at the surface and in the center. Specifically, overcalcined Example 2 had a single particle D50 of 6.8 µm and had a rock salt structure, a spinel structure, or a mixed structure from the surface region to a depth of 25 nm, and the central region of the layered structure. Experimental Example 2 (Evaluation of Gas Generation)

[0140] The positive electrode active materials according to the examples and comparative examples were measured for gas generation, and the results are shown in the following Tables 2 and 3 and in the Fig. 2A and Fig. 2B shown.

[0141] In particular, a method for measuring gas formation is as follows. Two NCM electrodes (loading amount per electrode area: 1000 mg / cm 2) charged at a voltage of 4.35 V (based on a full cell), and two separators were placed on the bottom plate of a button cell and secured with a gasket, and 80 μl of an electrolyte (DEC REF. (EC / PC / DEC=3 / 1 / 6, VC / PS=0.5 / 1 wt%)) was injected twice under vacuum. Each surface was vacuum sealed to a thickness of 0.5 cm using an aluminum bag (Al bag) measuring 6.5*10 cm. Vacuum sealing here refers to sealing under monocellular vacuum sealing conditions of 95 kPa / 93 kPa. Then, each battery was stored in a forced-air oven at 60°C for 2 weeks, and the gas evolution in the battery was measured. Table 2 Type of gas Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Gas formation (µL) H2 0 0 0 0 0 0 CO 586,4 524,8 535,6 597,2222222 402,7 262,2504537 CO2 899,7 891,3 871,1 805,5555556 639,2 412,8856624 CH4 0 0 0 0 0 0 C2H2 0 0 0 0 0 0 C2H4 101,2 118,3 100,8 81,1965812 117,8 0 C2H6 0,0 0,0 0,0 0 0,0 0 C3H6 49,8 50,8 46,8 25,64102564 40,7 26,31578947 C3H8 0,0 0,0 0,0 0 0,0 0 Σ (9 gas types) 1638,6 1582,7 1556,8 1509,6 1203,7 701,4519056 Table 3 Type of gas Example 7 Example 8 Example 9 Example 10 Example 11 Example 12 Gas formation (µL) H2 0 0 0 0 0 0 CO 597,2222222 295,4545455 504,8638132 283,7620579 486,0486049 95,54140127 CO2 805,5555556 795,4545455 885,2140078 1020,900322 612,9612961 286,6242038 CH4 0 0 0 0 0 0 C2H2 0 0 0 0 0 0 C2H4 81,1965812 215,9090909 97,27626459 138,2636656 0 222,9299363 C2H6 0 0 0 0 0 0 C3H6 25,64102564 147,7272727 35,9922179 52,25080386 19,8019802 53,07855626 C3H8 0 0 0 0 0 0 Σ (9 gas types) 1506,410256 1454,545455 1527,237354 1495,2 1116,111611 658,1740977

[0142] With reference to Tables 2 and 3 and the Fig. 3A and Fig.3B, gas formation was significantly reduced when overcalcination was carried out at 990°C or higher (Examples 1 to 12).

[0143] Those overcalcined at 1010°C (Examples 7 to 12) exhibited lower gas evolution than those overcalcined at 960°C (Examples 1 to 6), due to the lower amount of residual lithium and the reduction of cracks within the overcalcined particles and at the particle surface interface. The cracks within the particles and at the particle surface interface are areas where side reactions with the electrolyte can occur. Due to the reduction in the areas where side reactions can occur, gas evolution was significantly reduced. Experimental Example 3 (Evaluation of the high-temperature operating characteristics of the battery)

[0144] Each of the positive electrode active materials according to Examples and Comparative Examples was used to prepare a slurry for forming a positive electrode and a lithium secondary battery, and then their high-temperature life characteristics were evaluated, and the results are shown in the following. Fig. 4A and Fig. 4B shown.

[0145] With reference to the Fig. 4A and Fig.4B, the active materials of Examples 1 to 12, which all had technical combinations of overcalcination of precursor particles and limited dopant (and coating) contents, demonstrated excellent high-voltage and high-temperature lifetime properties. In contrast, Comparative Examples 1 and 2, which did not meet the overcalcination conditions, showed capacity retention of 85% or less at 100 cycles, and the slope gradually increased. Therefore, it is expected that capacity retention would decrease more rapidly after 100 cycles. Comparative Examples 3 and 4, in which the coating and dopant contents did not meet the conditions, showed that capacity retention decreased, and the slope gradually decreased with the cycles. Therefore, it is expected that capacity retention would continue to decrease after 100 cycles.Comparative Example 5, in which no coating and doping were performed, showed excellent initial capacity retention, but a rapid decline after 70 cycles. Comparative Example 6, in which no overcalcination occurred and the precursor size was large, showed a rapid decline in initial capacity retention. Comparative Example 7, in which overcalcination occurred but the precursor size and coating / dopant content did not meet the conditions of the present invention, showed a rapid decline in initial capacity retention and a deterioration in lifetime characteristics with cycles.

[0146] In particular, those overcalcined at 1010°C (Examples 7 to 12) showed excellent battery capacity retention compared to those overcalcined at 990°C (Examples 1 to 6), which may be related to gas generation, as confirmed in Experimental Example 2. In particular, those overcalcined at 1010°C (Examples 7 to 12) and exhibiting low Co release can improve the battery electrochemical properties compared to those overcalcined at 960°C (Examples 1 to 6).

[0147] However, all those overcalcined at 960°C (Examples 1 to 6) and those overcalcined at 1010°C (Examples 7 to 12) showed a remarkable improvement in capacity retention compared to those of the comparative examples.

[0148] While preferred exemplary embodiments of the present invention have been described in detail, the scope of the present invention is not limited to the above embodiments, and it will be apparent to those skilled in the art that various modifications and improvements using the basic concept of the present invention defined in the appended claims are also included within the scope of the present invention.

Claims

[1] A positive electrode active material for a lithium secondary battery, the positive electrode active material comprising: a single particle of a nickel-based lithium composite metal oxide, wherein the single particle contains a plurality of crystal grains, each crystal grain having a size of 180 nm to 300 nm as measured by X-ray diffraction analysis with a Cu Kα X-ray (X-rα), and a metal doped into a crystal lattice of the single particle, wherein a total weight of the doped metal is 2500 to 6000 ppm, wherein the metal is one or more metals selected from the group consisting of Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B. [2] A positive electrode active material for a lithium secondary battery, the positive electrode active material comprising: a single particle of a nickel-based lithium composite metal oxide, wherein the single particle contains a plurality of crystal grains, each crystal grain having a size of 180 nm to 300 nm as measured by Cu-Kα X-ray (X-rα), and a metal doped into a crystal lattice of the single particle, wherein the doped metal is one or more metals selected from the group consisting of Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S, and B;and a metal compound coated on the surface of the single particle, wherein the metal of the metal compound is one or more metals selected from the group consisting of Al, Ti, Mg, Zr, W, Y, Sr, Co, F, Si, Na, Cu, Fe, Ca, S and B, wherein a total content of the metal doped into the crystal lattice of the single particle and the metal in the metal compound coated on its surface is 2500 ppm to 6000 ppm.; [3] The positive electrode active material for a lithium secondary battery according to claim 1 or 2, wherein the single particle includes, in its crystal lattice structure, a surface region having a rock salt structure, a spinel structure, or a mixed structure thereof from the surface of the single particle to a depth of 0.13% to 5.26% of the radius of the single particle of the lithium composite metal oxide, and a central region having a layered structure from the interface with the surface region to the center of the single particle. [4] The positive electrode active material for a lithium secondary battery according to any one of claims 1 to 3, wherein the single particle has an average particle size (D50) of 3.5 µm or more to 8 µm or less. [5] A positive electrode active material for a lithium secondary battery according to any one of claims 1 to 4, wherein the nickel-based lithium composite metal oxide is represented by the following chemical formula 1 Li a (No x Mn y Co2)O 2+b (1) where in the chemical formula 1 0.95≤a≤1.2, 0≤b≤0.02, 0 <x<0,6, 0≤y≤0,4, 0≤z<0 und x+y+z=1. [6] The positive electrode active material for a lithium secondary battery according to claim 5, wherein in the chemical formula 1, a=1, 0≤b≤0.02, 0.4≤x<0.6, 0.1≤y<0.4, 0.1≤z<0.4 and x+y+z=1. [7] A positive electrode active material for a lithium secondary battery according to claim 5, wherein the chemical formula 1 LiNi 0,5 Co 0,2 Mn 0,3 O2 or LiNi 0,5 Co 0,3 Mn 0,2 O2 is. [8] The positive electrode active material for a lithium secondary battery according to any one of claims 1 to 7, wherein the metal doped into a crystal lattice of the single particle is Ti, Mg or Zr. [9] The positive electrode active material for a lithium secondary battery according to any one of claims 1 to 7, wherein the metal doped into a crystal lattice of the single particle is Zr. [10] A positive electrode for a lithium secondary battery, wherein the positive electrode comprises the positive electrode active material according to any one of claims 1 to 9. [11] A lithium secondary battery comprising the positive electrode according to claim 10.