Composite ceramic electrolyte particles with hydrophobic protective layer for battery electrodes
The composite ceramic electrolyte particle with a hydrophobic protective layer addresses moisture issues in LLZO particles by using dopamine and composite coatings, enhancing conductivity and preventing deterioration, thus improving battery performance and reducing costs.
Patent Information
- Application Number
- DE202024105963
- Authority / Receiving Office
- DE · DE
- Patent Type
- Utility models
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2034-10-31
AI Technical Summary
LLZO particles in battery electrodes are hydrophilic and prone to moisture, leading to deterioration and undesirable side reactions during production, affecting ionic conductivity.
A composite ceramic electrolyte particle with a hydrophobic protective layer is formed by coating LLZO particles with dopamine layers and hydrophobic barium titanate and zinc oxide composite particles, along with carbon nanotubes and nanoscale amorphous carbons to enhance ionic and electrical conductivity while preventing moisture ingress.
The composite structure improves lithium ion distribution, prevents moisture-induced deterioration, and enhances conductivity, resulting in better battery performance and reduced production costs.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
FIELD OF THE INVENTION
[0001] The invention relates to a battery electrode material and in particular to a composite ceramic electrolyte particle with a hydrophobic protective layer for a battery electrode. BACKGROUND OF THE INVENTION
[0002] A typical battery consists of electrodes (positive and negative) suspended in an electrolyte. In the current state of the art, LLZO (lithium lanthanum zirconium oxide) material is added to the electrodes to increase their ionic conductivity. Because LLZO particles exhibit high ionic conductivity for lithium ions, the lithium ions flowing through the electrode—especially a negative electrode—can be dispersed by the guidance of the dispersed LLZO particles themselves. Thus, the lithium ions can be evenly distributed throughout the negative electrode, preventing abnormal accumulation of lithium ions in the negative electrode slurry and thus undesirable side reactions.
[0003] However, moisture is generated during electrode production. Furthermore, the LLZO particles are hydrophilic and become slightly moist upon reaction with water, forming a lye solution, which leads to deterioration of the material in the negative electrode slurry. SUMMARY OF THE INVENTION
[0004] To overcome the above-mentioned deficiencies in the prior art, the object of the invention is to provide a composite ceramic electrolyte particle with a hydrophobic protective layer for a battery electrode, wherein a first LLZO particle is coated with a first dopamine layer to form a hydrophobic LLZO particle. The hydrophobic LLZO particle, together with the barium titanate composite particles or zinc oxide composite particles, is further coated with a second dopamine layer to form a LLZO composite particle with improved ionic conductivity. The dopamine layer is hydrophobic and serves to prevent water from penetrating the first LLZO particle. The barium titanate composite particles and zinc oxide composite particles are also hydrophobic and can provide further protection for the first LLZO particle.The LLZO composite particle is further coated with an aid containing nanoscale carbon nanotubes and amorphous carbons to increase lithium ion conductivity. The nanoscale amorphous carbons are filled into the gaps between the carbon nanotubes to improve electrical conductivity. The barium titanate composite particles, zinc oxide composite particles, the dopamine layer, the carbon nanotubes, and the nanoscale amorphous carbon form multiple protective structures for the first LLZO particle, which increases the lithium conductivity of the first LLZO particle, prevents reactions of the first LLZO particle and water contact during electrode fabrication, and enables better quality in the production of the battery electrode material. BRIEF DESCRIPTION OF THE ILLUSTRATIONS Fig. shows a schematic view depicting the structure of the LLZO composite particle of the invention. Fig. shows an application of the structure of the invention. Fig. shows a schematic view depicting the complete structure and a partial structure of the second-order LLZO composite particle in the invention. Fig. shows a schematic view depicting the full structure and partial structure of the hydrophobic LLZO particle, where the dehydration-induced polymerization is formed between the OH ion of the dopamine of the first dopamine layer and the third OH ion of the first hydroxide ion layer. Fig. shows a schematic view depicting the complete structure and partial structure of the barium titanate composite particle of the invention. Fig. shows a schematic view depicting the complete structure and partial structure of the zinc oxide composite particle of the invention. Fig. shows a schematic view depicting the structure of the third-order LLZO composite particle of the invention. Fig. shows a cross-sectional view depicting the structure of the LLZO composite particle of the invention. Fig. shows a cross-sectional view depicting the partial structure of the LLZO composite particle of the invention. DETAILED DESCRIPTION OF THE INVENTION
[0005] With reference to the Fig. The invention provides a composite ceramic electrolyte particle with a hydrophobic protective layer for a battery electrode. The composite ceramic electrolyte particle consists of an LLZO composite particle 100. The LLZO composite particle 100 is used in the battery electrode, wherein the battery electrode is intended to be an electrode 10 of a solid-state or semi-solid-state battery. In the application, several LLZO composite particles 100 can be incorporated into the electrode 10, wherein the electrode 10 represents, in particular, a negative electrode of the solid-state or semi-solid-state battery. The size of the LLZO composite particle 100 is 50 nm to 200 nm. The electrode 10 comprises a substrate 11 as a carrier of the material of the electrode 10 and an electrode slurry layer 13 applied to the substrate 11. The electrode slurry layer 13 comprises the LLZO composite particles 100 and an electrode slurry 12 used as a binder.The electrode slurry 12 consists of at least one of the following materials: styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), and an auxiliary material (carbon nanotube or Super-P (conductive carbon black)). A weight fraction of the LLZO composite particles 100 in an electrode slurry layer 13 (particularly a negative electrode slurry layer) is 0.5 wt% to 5 wt%.
[0006] The LLZO composite particle 100 comprises the following elements: A first LLZO particle 15. Since LLZO material exhibits high ionic conductivity, the first LLZO particle 15 serves to guide and distribute the lithium ion pathways as lithium ions flow through the electrode. This causes evenly distributed lithium ion channels to be formed within the electrode, preventing abnormal accumulation of lithium ions in the electrode slurry and undesirable side reactions.
[0007] The first LLZO particle 15 consists of LLZO (lithium lanthanum zirconium oxide, Li7La3Zr2O 12 ) or LLZO doped with at least one metal (such as gallium (Ga) doped LLZO (Li 6.2 Ga 0.8 La3Zr2O 12 ), from aluminum (Al) doped LLZO or from barium (Ba) doped LLZO.
[0008] Since moisture is present during the electrode manufacturing process, the LLZO particles are hydrophilic and can easily become wet, forming alkali. Therefore, in the invention, an outer surface of the first LLZO particle 15 is coated with a protective layer (the following first dopamine layer 35) to prevent the first LLZO particle 15 from becoming wet during the electrode manufacturing process.
[0009] A first hydroxide ion layer (OH-) 24 is deposited on an outer surface of the first LLZO particle 15. The first hydroxide ion layer 24 and the first LLZO particle 15 form a second-order LLZO composite particle 30 (as shown in Fig. shown). The thickness of the first hydroxide ion layer 24 is 0.5 nm to 2 nm. The first hydroxide ion layer 24 is formed by a reaction of Tris molecules (tris(hydroxymethyl)aminomethane, (HOCH2)3CNH2) and includes a plurality of third OH ions. The Tris molecules are added during the manufacturing process of the LLZO composite particle 100. Each of the Tris molecules includes three OH ions, namely a first, a second, and a third OH ion. The first and second OH ions are bonded to oxidizing functional groups on the first LLZO particle 15 through hydrogen bonds. The third OH ion extends outward to an outer side of the first LLZO particle 15 to form the first hydroxide ion layer 24. Fig. shows an example of only two Tris molecules and is not intended to limit the scope of the invention.
[0010] A first dopamine layer 35 is coated on an outer surface of the second-order LLZO composite particle 30. The first dopamine layer 35 and the second-order LLZO composite particle 30 form a hydrophobic LLZO particle 40 (as shown in Fig. shown). The first dopamine layer 35 is formed by a plurality of copolymerized dopamine molecules. A dehydration-induced polymerization is carried out between an OH ion of each of the dopamine molecules of the first dopamine layer 35 and a respective third OH ion of the first hydroxide ion layer 24 to cause the first dopamine layer 35 to be separated by the first hydroxide ion layer 24 (as shown in Fig. shown) is bonded to the second-order LLZO composite particle 30. The thickness of the first dopamine layer 35 is 1 nm to 10 nm.
[0011] Since moisture is present during the electrode slurry manufacturing process and the LLZO particles are hydrophilic, they can easily become moist, forming alkali that destroys the lithium conductivity of the LLZO particles. Therefore, dopamine is used in the invention. The dopamine molecules of the dopamine layer 35 are hydrophobic to protect the first LLZO particle 15 and thus prevent the first LLZO particle 15 from becoming moist.
[0012] An outer hydrophobic layer 41 is coated on an outer surface of the hydrophobic LLZO particle 40. The outer hydrophobic layer 41 and the hydrophobic LLZO particle 40 form the LLZO composite particle 100 (as shown in Fig. shown). The outer hydrophobic layer 41 comprises a plurality of peripheral composite particles 200. Each of the peripheral composite particles 200 is selected from a barium titanate (BaTiO3) composite particle 20 and a zinc oxide (ZnO) composite particle 22. The peripheral composite particles 200, which are distributed on the outer surface of the hydrophobic LLZO particle 40, form a naturally shaped structure, which is formed during stirring in the manufacturing process.
[0013] Regarding the Fig. Each of the peripheral composite particles 200 includes a peripheral particle 210. When the peripheral composite particle 200 is the barium titanate composite particle 20, the peripheral particle 210 is referred to as the barium titanate particle 201. When the peripheral composite particle 200 is the zinc oxide composite particle 22, the peripheral particle 210 is referred to as the zinc oxide particle 221. A second hydroxide ion layer (OH-) 21 is coated on an outer side of the peripheral particle 210. A second dopamine layer 36 is coated on an outer side of the second hydroxide ion layer 21. The size of each of the barium titanate composite particle 20 and the zinc oxide composite particle 22 is 10 nm to 20 nm.
[0014] The second hydroxide ion layer 21 is formed by a reaction of the Tris molecules (tris(hydroxymethyl)aminomethane, (HOCH2)3CNH2) and has a plurality of third OH ions. The Tris molecules are added during the manufacturing process of the LLZO composite particle 100. Each of the Tris molecules has three OH ions, namely the first, second, and third OH ions. The first ions and the second OH ions of the Tris molecules are bonded by hydrogen bonds to oxidizing functional groups on a corresponding barium titanate particle 201 or zinc oxide particle 221. The third OH ions of the Tris molecules extend outward to an outer side of the corresponding barium titanate particle 201 or zinc oxide particle 221 to form the second hydroxide ion layer 21. The Fig. show examples of only two Tris molecules and are not used to limit the scope of the invention.
[0015] The second dopamine layer 36 is formed by a plurality of copolymerized dopamine molecules. A dehydration-induced polymerization is carried out between OH ions of the dopamine molecules of the second dopamine layer 36 and the third OH ions of a corresponding second hydroxide ion layer 21 to cause the second dopamine layer 36 to be bonded through the corresponding second hydroxide ion layer 21 to a corresponding barium titanate particle 201 or zinc oxide particle 221 (as shown in the Fig. shown).
[0016] The ratio of the weight of the outer hydrophobic layer 41 to the weight of the hydrophobic LLZO particle 40 is 1 / 25 to 1 / 10 (4 to 10%). The thickness of the second hydroxide ion layer 21 is 0.5 to 2 nm. The thickness of the second dopamine layer 36 is 1 to 10 nm.
[0017] The outer hydrophobic layer 41 is applied to the outer surface of the hydrophobic LLZO particle 40 by chain-polymerizing the dopamine molecules of the first dopamine layer 35 and the dopamine molecules of the second dopamine layer 36 on the outer hydrophobic layer 41. This is a naturally occurring structure that is formed during stirring during the manufacturing process.
[0018] The purpose of coating the outer hydrophobic layer 41 is that—because the barium titanate particle 201 and the zinc oxide particle 221 are hydrophobic—the barium titanate particle 201 and the zinc oxide particle 221 serve to isolate external water and the first LLZO particle 15 when coated on the outer surface of the hydrophobic LLZO particle 40, preventing the first LLZO particle 15 from becoming wet. Furthermore, the ionic conductivity of the barium titanate particle 201 is higher than that of the first LLZO particle 15, so the barium titanate particle 201 can also provide better ionic conductivity. The zinc oxide particle 221 serves to improve electrode compatibility and can be used as an ionic interface layer. It also serves as the electrode material, reducing capacity loss due to the coating.
[0019] The purpose of applying the second hydroxide ion layer 21 to the outer surface of the peripheral particle 210 is that, because the barium titanate particle 201 and the zinc oxide particle 221 are insoluble in water and the hydroxide ions (OH ions) on the second hydroxide ion layer 21 have polarity, by applying the second hydroxide ion layer 21 to the outer surface of the barium titanate particle 201 and the zinc oxide particle 221, the second dopamine layer 36 can react with the second hydroxide ion layer 21 and adhere more stably to the barium titanate particle 201 and the zinc oxide particle 221.
[0020] A plurality of carbon nanotubes 42 and a plurality of nanoscale amorphous carbons 45 are coated on an outer surface of the LLZO composite particle 100. The carbon nanotubes 42, the nanoscale amorphous carbons 45, and the LLZO composite particle 100 form a third-order LLZO composite particle 50 (as shown in Fig. shown). The size of each of the carbon nanotubes 42 is 200 nm to 500 nm. The size of each of the nanoscale amorphous carbons 45 is 10 nm to 40 nm. Preferably, the nanoscale amorphous carbons 45 are amorphous carbons of a Super P aid.
[0021] The ratio of the total weight of the carbon nanotubes 42 and the amorphous nanoscale carbons 45 to the weight of the first LLZO particle 15 is 0.2 to 2:99.8 to 98.
[0022] The carbon nanotubes 42 and the nanoscale amorphous carbons 45 are further used as auxiliary materials. Since the nanoscale amorphous carbons 45 are in the form of particles and the carbon nanotubes 42 are in the form of long strips, several gaps are formed in the intermediate structure formed by the carbon nanotubes 42, which cannot conduct electric current. Therefore, the nanoscale amorphous carbons 45 are filled into the gaps to transfer the electric charge between the carbon nanotubes 42 by bridging the nanoscale amorphous carbons 35, which further increases the electric current transfer efficiency. The LLZO composite particle 100 coated with the carbon nanotubes 42 has a hairball-like structure (as shown in Fig. shown).
[0023] The advantages of carbon nanotubes (42) are that lithium ions can be easily stabilized between the carbon nanotubes (42), thereby improving lithium-ion conductivity. The very high lithium-ion conductivity helps the entire battery charge and discharge quickly. Furthermore, the use of cobalt can be reduced, thus lowering overall production costs.
[0024] The invention thus relates to a composite ceramic electrolyte particle with a hydrophobic protective layer for a battery electrode, wherein the composite ceramic electrolyte particle represents an LLZO composite particle. The LLZO composite particle comprises a first LLZO particle. A first hydroxide ion layer is coated on the first LLZO particle to form a second-order LLZO composite particle. A first dopamine layer is coated on the second-order LLZO composite particle to form a hydrophobic LLZO particle. An outer hydrophobic layer is coated on the hydrophobic LLZO particle to form the LLZO composite particle. The outer hydrophobic layer comprises a plurality of peripheral composite particles. Each of the peripheral composite particles comprises a peripheral particle. A second hydroxide ion layer is coated on the peripheral particle. A second dopamine layer is coated on the second hydroxide ion layer.
[0025] Having described the invention, it will be obvious that it may be varied in many ways. Such variations are not to be regarded as a departure from the spirit and scope of the invention, and all modifications obvious to one skilled in the art are intended to be included within the scope of the following claims.
Claims
[1] Composite ceramic electrolyte particles with a hydrophobic protective layer for a battery electrode; the composite ceramic electrolyte particle is an LLZO composite particle; the battery electrode is an electrode of a solid-state or semi-solid-state battery; the electrode comprises a substrate as a carrier of the electrode material and an electrode slurry layer coated on the substrate; the LLZO composite particle comprises the following: a first LLZO particle, which serves to guide and distribute the paths of the lithium ions and to ensure that evenly distributed lithium ion channels are formed within the electrode; a first hydroxide ion layer coated on an outer surface of the first LLZO particle; the first hydroxide ion layer and the first LLZO particle form a second-order LLZO composite particle; the first hydroxide ion layer is formed by a reaction of Tris molecules (tris(hydroxymethyl)aminomethane-(HOCH2)3CNH2) and has a plurality of third OH ions; the Tris molecules are added during the manufacturing process of the LLZO composite particle; each of the Tris molecules has three OH ions, namely a first, a second, and a third OH ion; the first ions and the second OH ions of the Tris molecules are bonded to oxidizing functional groups on the first LLZO particle by hydrogen bonds; the third OH ions of the Tris molecules extend outward to an outer side of the first LLZO particle to form the first hydroxide ion layer; a first dopamine layer coated on an outer surface of the second-order LLZO composite particle; the first dopamine layer and the second-order LLZO composite particle form a hydrophobic LLZO particle; the first dopamine layer is formed by a plurality of copolymerized dopamine molecules; dehydration-induced polymerization between OH ions of the dopamine molecules of the first dopamine layer and the third OH ions of the first hydroxide ion layer is intended to cause the first dopamine layer to be bonded to the second-order LLZO composite particle through the first hydroxide ion layer; the dopamine molecules of the dopamine layer are hydrophobic to protect the first LLZO particle and prevent the first LLZO particle from becoming wet; an outer hydrophobic layer coated on an outer surface of the hydrophobic LLZO particle; the outer hydrophobic layer and the hydrophobic LLZO particle form the LLZO composite particle; the outer hydrophobic layer comprises a plurality of peripheral composite particles; each of the peripheral composite particles is selected from a barium titanate (BaTiO3) composite particle and a zinc oxide (ZnO) composite particle; wherein each of the peripheral composite particles comprises a peripheral particle; when the peripheral composite particle is the barium titanate composite particle, the peripheral particle is referred to as a barium titanate particle; when the peripheral composite particle is the zinc oxide composite particle, the peripheral particle is referred to as a zinc oxide particle; a second hydroxide ion layer is coated on an outer side of the peripheral particle; and a second dopamine layer is coated on an outer side of the second hydroxide ion layer; wherein the second hydroxide ion layer is formed by a reaction of the Tris molecules (tris(hydroxymethyl)aminomethane-(HOCH2)3CNH2) and has a plurality of third OH ions; the Tris molecules are added during the manufacturing process of the LLZO composite particle; each of the Tris molecules has three OH ions, namely a first, a second, and a third OH ion; the first ions and second OH ions of the Tris molecules are bonded by hydrogen bonds to oxidizing functional groups on a corresponding barium titanate particle or zinc oxide particle; the third OH ions of the Tris molecules extend outward to an outer side of the corresponding barium titanate particle or zinc oxide particle to form the second hydroxide ion layer; wherein the second dopamine layer is formed by a plurality of copolymerized dopamine molecules; a dehydration-induced polymerization is carried out between OH ions of the dopamine molecules of the second dopamine layer and the third OH ions of a corresponding second hydroxide ion layer to cause the second dopamine layer to be bonded to a corresponding barium titanate particle or zinc oxide particle through the corresponding second hydroxide ion layer; and wherein the outer hydrophobic layer is applied by chain copolymerization of the dopamine molecules of the first dopamine layer and the dopamine molecules of the second dopamine layer on the outer hydrophobic layer of the outer surface of the hydrophobic LLZO particle. [2] Composite ceramic electrolyte particles according to claim 1, wherein the first LLZO particle is LLZO (lithium lanthanum zirconium oxide, Li7La3Zr2O 12) or LLZO doped with at least one metal. [3] The composite ceramic electrolyte particles according to claim 1, wherein the ratio of the weight of the outer hydrophobic layer to the weight of the hydrophobic LLZO particle is 1 / 25 to 1 / 10. [4] The composite ceramic electrolyte particle according to claim 1, wherein the LLZO composite particle is used in a negative electrode. [5] The composite ceramic electrolyte particle according to claim 1, wherein the size of the LLZO composite particle is 50 to 200 nm. [6] The composite ceramic electrolyte particle according to claim 1, wherein the size of the barium titanate composite particle and the zinc oxide composite particle is each 10 to 20 nm. [7] Composite ceramic electrolyte particles according to claim 1, wherein the thickness of the first hydroxide ion layer is 0.5 to 2 nm and the thickness of the second hydroxide ion layer is 0.5 to 2 nm. [8] The composite ceramic electrolyte particles according to claim 1, wherein the thickness of the first dopamine layer is 1 nm to 10 nm; and the thickness of the second dopamine layer is 1 nm to 10 nm. [9] The composite ceramic electrolyte particle according to claim 1, wherein a plurality of carbon nanotubes and a plurality of nano-sized amorphous carbons are coated on an outer surface of the LLZO composite particle; and the carbon nanotubes, the nano-sized amorphous carbons, and the LLZO composite particle form a third-order LLZO composite particle. [10] The composite ceramic electrolyte particles according to claim 9, wherein the size of each of the carbon nanotubes is 200 nm to 500 nm; and the size of each of the amorphous carbons in the nanoscale is 10 nm to 40 nm. [11] The composite ceramic electrolyte particles according to claim 9, wherein a ratio of a total weight of the carbon nanotubes and the nano-sized amorphous carbons and the weight of the first LLZO particle is 0.2-2:99.8-98.