METHOD FOR NICKEL-FREE PHOSPHATION OF METALLIC SURFACES

DE502016016773D1Active Publication Date: 2024-11-14CHEMETALL GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502016016773
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-04-07
Filing Date
2016-04-07
Publication Date
2024-11-14
Estimated Expiration
2036-04-07

AI Technical Summary

Technical Problem

Nickel-containing phosphating solutions are undesirable due to toxicity and environmental concerns, and nickel-free alternatives often result in suboptimal corrosion and paint adhesion on metallic surfaces, especially under electrocoating conditions.

Method used

A nickel-free phosphating method using an acidic aqueous composition with zinc, manganese, and phosphate ions, followed by a rinse composition containing specific metal ions and polymers, to achieve comparable electrochemical properties and improved adhesion and corrosion resistance.

Benefits of technology

The method provides a nickel-free phosphating process that enhances corrosion protection and paint adhesion on metallic surfaces, matching or exceeding the performance of nickel-containing systems, while reducing environmental impact.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a process for the essentially nickel-free phosphating of a metallic surface, a corresponding phosphating composition and a correspondingly phosphate-coated metallic surface.

[0002] Phosphate coatings on metallic surfaces are well known in the art. Such coatings serve to protect metallic surfaces against corrosion and also act as adhesion promoters for subsequent paint coatings.

[0003] Such phosphate coatings are mainly used in the automotive industry and general industry.

[0004] WO 95 / 33083 A1 discloses a process for coating phosphated metal substrates with organic coatings, wherein the substrates are treated with an aqueous solution after phosphating and before application of the first organic coating.

[0005] The subsequent coating layers are primarily cathodically deposited electrocoats (ECDs), in addition to powder coatings and wet coatings. Since a current must flow between the metallic surface and the treatment bath during the deposition of ECDs, it is important to maintain a defined electrical conductivity of the phosphate coating to ensure efficient and homogeneous deposition.

[0006] Therefore, phosphate coatings are typically applied using a nickel-containing phosphating solution. The nickel deposited in this way, either elementally or as an alloy component, e.g., Zn / Ni, ensures the coating's appropriate conductivity during the subsequent electrocoating process.

[0007] However, due to their high toxicity and environmental impact, nickel ions are no longer desirable as components of treatment solutions and should therefore be avoided if possible or at least their content reduced.

[0008] The use of nickel-free or low-nickel phosphating solutions is known in principle, but this is limited to certain substrates such as steel.

[0009] In the case of the nickel-poor or nickel-free systems mentioned, under given KTL deposition conditions, the coating may also be subject to suboptimal

[0010] Substrate surface results in poor corrosion and paint adhesion values.

[0011] The object of the present invention was therefore to provide a process by which metallic surfaces can be phosphated in a substantially nickel-free manner, wherein, with regard to their electrochemical properties, these surfaces are comparable or almost comparable to the metallic surfaces which have been treated with nickel-containing phosphating solutions, and in particular, the aforementioned disadvantages of the prior art are avoided.

[0012] This object is achieved by a method according to claim 1 and a phosphate-coated metallic surface according to claim 13.

[0013] In the method disclosed herein for the substantially nickel-free phosphating of a metallic surface, a metallic surface, optionally after cleaning and / or activation, is first treated with an acidic aqueous phosphating composition comprising zinc ions, manganese ions and phosphate ions, optionally rinsed and / or dried, and then treated with an aqueous rinsing composition comprising at least one type of metal ion selected from the group consisting of the ions of molybdenum, copper, silver, gold, palladium, tin, antimony, titanium, zirconium and hafnium and / or at least one polymer selected from the group consisting of the polymer classes polyamines, polyethyleneamines, polyanilines, polyimines, polyethyleneimines, polythiophenes and polypyrroles and mixtures and copolymers thereof, wherein both the phosphating composition and the rinsing composition are substantially nickel-free. Definitions:

[0014] On the one hand, an uncoated metallic surface, but on the other hand, a metallic surface already coated with a conversion coating can also be treated with the method according to the invention. Therefore, whenever reference is made to a "metallic surface" in the following, this always includes a metallic surface already coated with a conversion coating.

[0015] For the purposes of the present invention, an "aqueous composition" refers to a composition that contains at least partially, preferably predominantly, water as a solvent. In addition to dissolved components, it may also comprise dispersed, i.e., emulsified and / or suspended components.

[0016] For the purposes of the present invention, "phosphate ions" also include hydrogen phosphate, dihydrogen phosphate, and phosphoric acid. Pyrophosphoric acid and polyphosphoric acid, as well as all their partially and fully deprotonated forms, are also included.

[0017] For the purposes of the present invention, "metal ion" means either a metal cation, a complex metal cation or a complex metal anion.

[0018] If a composition contains less than 0.3 g / l of nickel ions, it shall be considered "essentially nickel-free" for the purposes of the present invention.

[0019] The metallic surface is preferably steel, hot-dip galvanizing, electrolytic galvanizing, aluminum, or their alloys, such as Zn / Fe or Zn / Mg. Hot-dip galvanizing and electrolytic galvanizing are each particularly applied to steel. In particular, the metallic surface is at least partially galvanized.

[0020] The process according to the invention is particularly suitable for multi-metal applications.

[0021] If a metallic surface is to be coated that is not freshly hot-dip galvanized, it is advantageous to first clean, especially degrease, the metallic surface in an aqueous cleaning composition before treatment with the phosphating composition. For this purpose, an acidic, neutral, alkaline, or strongly alkaline cleaning composition can be used, but optionally also an acidic or neutral pickling composition.

[0022] An alkaline or strongly alkaline cleaning composition has proven particularly advantageous.

[0023] In addition to at least one surfactant, the aqueous cleaning composition may optionally also contain a cleaning agent and / or other additives such as complexing agents. The use of an activating cleaner is also possible.

[0024] After cleaning / pickling, the metallic surface is then advantageously rinsed at least once with water, whereby an additive dissolved in water, such as a nitrite or surfactant, may also be added to the water if necessary.

[0025] Before treating the metallic surface with the phosphating composition, it is advantageous to treat it with an activating composition. The activating composition serves to deposit a multitude of extremely fine phosphate particles as seed crystals on the metallic surface. These help in the subsequent process step, upon contact with the phosphating composition—preferably without intermediate rinsing—to form a particularly crystalline phosphate layer with the highest possible number of densely arranged fine phosphate crystals or a largely continuous phosphate layer.

[0026] Acidic or alkaline compositions based on titanium phosphate or zinc phosphate are particularly suitable as activation compositions.

[0027] However, it may also be advantageous to add activating agents, in particular titanium phosphate or zinc phosphate, to the cleaning composition, thus carrying out cleaning and activation in one step.

[0028] The acidic aqueous phosphating composition includes zinc ions, manganese ions and phosphate ions.

[0029] The phosphating composition can be obtained from a concentrate by diluting with a suitable solvent, preferably with water, by a factor between 1 and 100, preferably between 5 and 50, and if necessary adding a pH-modifying substance.

[0030] The phosphating composition preferably comprises the following components in the following preferred and particularly preferred concentration ranges: Zn 0.3 to 3.0 g / l 0.5 to 2.0 g / l Mn 0.3 to 2.0 g / l 0.5 to 1.5 g / l Phosphate (calculated as P 2 O 5 ) 8 to 25 g / l 10 to 18 g / l free fluoride 30 to 250 mg / l 50 to 180 mg / l Complex fluoride (calculated e.g. as SiF 6 2-< and / or BF 4 -< ) 0 to 5 g / l 0.5 to 3 g / l

[0031] However, with regard to manganese ions, a concentration in the range of 0.3 to 2.5 g / l has already proven to be advantageous, and with regard to free fluoride, a concentration in the range of 10 to 250 mg / l has already proven to be advantageous.

[0032] The complex fluoride is preferably tetrafluoroborate (BF 4 -< ) and / or hexafluorosilicate (SiF 6 2-< ).

[0033] Especially when treating aluminum and / or galvanized material, a content of complex fluoride as well as simple fluoride, for example sodium fluoride, in the phosphating composition is advantageous.

[0034] Al 3+< is a bath poison in phosphating systems and can be removed from the system by complexing it with fluoride, e.g., as cryolite. Complex fluorides are added to the bath as "fluoride buffers," since otherwise the fluoride content would quickly drop and no coating would form. Fluoride thus supports the formation of the phosphate layer and thus indirectly improves paint adhesion and corrosion protection. Complex fluoride also helps prevent defects such as specks on galvanized material.

[0035] Particularly in the treatment of aluminum, it is further advantageous if the phosphating composition contains Fe(III). An Fe(III) content in the range of 0.001 to 0.2 g / l is preferred, particularly preferably 0.005 to 0.1 g / l, and most particularly preferably 0.01 to 0.05 g / l is preferred.

[0036] In addition, the phosphating composition preferably contains at least one accelerator selected from the group consisting of the following compounds in the following preferred and particularly preferred concentration ranges: Nitroguanidine 0.2 to 3.0 g / l 0.2 to 1.55 g / l H 2 O 2 10 to 100 mg / l 15 to 50 mg / l Nitroguanidine / H 2 O 2 0.2 to 2.0 g / l / 10 to 50 mg / l 0.2 to 1.5 g / l / 15 to 30 mg / l nitrite 30 to 300 mg / l 90 to 150 mg / l Hydroxylamin 0.1 to 5 g / l 0.4 to 3 g / l

[0037] However, with regard to nitroguanidine, a concentration in the range of 0.1 to 3.0 g / l and with regard to H 2 O 2, a concentration in the range of 5 to 200 mg / l has already proven to be advantageous.

[0038] Most preferably, the at least one accelerator is H 2 O 2 .

[0039] However, the phosphating composition contains less than 0.5 g / l, preferably less than 0.1 g / l and more preferably less than 0.01 g / l of nitrate.

[0040] Particularly on a galvanized surface, the nitrate in the phosphating composition further accelerates the coating formation reaction, which leads to lower coating weights but, above all, reduces the incorporation of manganese into the crystal. However, if the manganese content of the phosphate coating is too low, this compromises its alkali resistance.

[0041] Alkali resistance, in turn, plays a crucial role in subsequent cathodic electrocoating. This involves electrolytic decomposition of water at the substrate surface, forming hydroxide ions. This leads to an increase in the pH at the substrate interface. While this is the only way the electrocoat can agglomerate and be deposited, the increased pH can also damage the crystalline phosphate layer.

[0042] The phosphating composition preferably has a temperature in the range of 30 to 55 °C.

[0043] Furthermore, the phosphating composition can be characterized by the following preferred and particularly preferred parameter ranges: FS 0.3 to 2.0 0.7 to 1.6 FS (dim.) 0.5 to 8 1 to 6 GSF 12 to 28 22 to 26 GS 12 to 45 18 to 35 S-value 0.01 to 0.2 0.03 to 0.15 Temperature °C 30 to 50 °C 35 to 45 °C

[0044] However, with regard to the FS parameter, a value in the range of 0.2 to 2.5 has already proven to be advantageous, and with regard to the temperature, a value in the range of 30 to 55 °C has already proven to be advantageous.

[0045] Where "FS" stands for free acid, "FS (dil.)" for free acid (diluted), "GSF" for total acid according to Fischer, "GS" for total acid and "S-value" for acid value.

[0046] These parameters are determined as follows: Free acid (FA):

[0047] To determine the free acid, 10 ml of the phosphating composition is pipetted into a suitable container, for example, a 300 ml Erlenmeyer flask. If the phosphating composition contains complex fluorides, 2-3 g of potassium chloride are added to the sample. Then, using a pH meter and an electrode, titrate with 0.1 M NaOH to a pH of 3.6. The amount of 0.1 M NaOH consumed in ml per 10 ml of the phosphating composition gives the free acid (FA) value in points. Free acid (diluted) (FS (dil.)):

[0048] To determine the free acid (diluted), 10 ml of the phosphating composition is pipetted into a suitable container, for example a 300 ml Erlenmeyer flask. Then, 150 ml of deionized water is added. Using a pH meter and an electrode, the solution is titrated with 0.1 M NaOH to a pH of 4.7. The amount of 0.1 M NaOH used in ml per 10 ml of the diluted phosphating composition gives the free acid (diluted) value (FS (dil.)) in points. The complex fluoride content can be determined from the difference to the free acid (FS). If this difference is multiplied by a factor of 0.36, the complex fluoride content is obtained as SiF 6 2-< in g / l. Total acidity according to Fischer (GSF):

[0049] Following determination of the free acid (diluted), the diluted phosphate composition is titrated to a pH of 8.9 after adding potassium oxalate solution using a pH meter and an electrode with 0.1 M NaOH. The consumption of 0.1 M NaOH in ml per 10 ml of the diluted phosphate composition yields the total acidity according to Fischer (GSF) in points. Multiplying this value by 0.71 yields the total phosphate ion content, calculated as P 2 O 5 (see W. Rausch: "Die Phosphatierung von Metallen" (The Phosphatization of Metals). Eugen G. Leuze-Verlag 2005, 3rd edition, pp. 332 ff.). Total acid (GS):

[0050] Total acidity (TA) is the sum of the divalent cations present, as well as free and bound phosphoric acids (the latter are phosphates). It is determined by the consumption of 0.1 M NaOH using a pH meter and an electrode. To do this, 10 ml of the phosphating composition is pipetted into a suitable container, such as a 300 ml Erlenmeyer flask, and diluted with 25 ml of deionized water. The solution is then titrated with 0.1 M NaOH to a pH of 9. The consumption in ml per 10 ml of the diluted phosphating composition corresponds to the total acidity (TA) score. Acid value (S-value):

[0051] The so-called acid value (S-value) stands for the ratio FS : GSF and is obtained by dividing the value of the free acid (FS) by the value of the total acid according to Fischer (GSF).

[0052] Surprisingly, the further improvement in paint adhesion, especially on hot-dip galvanized surfaces, was achieved by setting an acid value in the range of 0.03 to 0.065, especially in the range of 0.04 to 0.06.

[0053] It has surprisingly been found that, particularly in the case of steel or hot-dip galvanized metallic surfaces, a temperature of the phosphating composition of less than 45 °C, preferably in the range between 35 and 45 °C, leads to further improved corrosion and paint adhesion values.

[0054] The phosphating composition is essentially nickel-free. It preferably contains less than 0.1 g / l, and more preferably less than 0.01 g / l, of nickel ions.

[0055] The treatment of the metallic surface with the phosphating composition is preferably carried out for 30 to 480, particularly preferably for 60 to 300 and most particularly preferably for 90 to 240 seconds, preferably by dipping or spraying.

[0056] By treating the metallic surface with the phosphating composition, the following preferred and particularly preferred zinc phosphate layer weights are achieved on the metallic surface, depending on the treated surface (determined by X-ray fluorescence analysis (XRF)): Treated surface Zinc phosphate layer weight (g / m 2< ) Steel 0.5 to 6 1 to 5 Hot-dip galvanizing 1.0 to 6 1.5 to 5 electrolytic galvanizing 1.0 to 6 1.5 to 5 aluminum 0.5 to 6 1 to 5

[0057] Preferably, the metallic surface is rinsed after treatment with the phosphating composition, more preferably with demineralized water or tap water. Optionally, the metallic surface is dried before treatment with the post-rinse composition.

[0058] According to the method according to the invention, the metallic surface already treated with the phosphating composition, i.e. phosphate-coated, is further treated with an aqueous rinsing composition as defined in claim 1.

[0059] The rinse composition can be obtained from a concentrate by diluting with a suitable solvent, preferably with water, by a factor between 1 and 1000, preferably between 5 and 500, and if necessary adding a pH-modifying substance.

[0060] According to one embodiment, the rinse composition contains at least one type of metal ion selected from the group consisting of the ions of the following metals in the following preferred, particularly preferred and most particularly preferred concentration ranges (all calculated as the corresponding metal): Mon 10 to 500 mg / l 20 to 225 mg / l Cu 1 to 1000 mg / l 100 to 500 mg / l 150 to 225 mg / l Ag 1 to 500 mg / l 5 to 300 mg / l 20 to 150 mg / l Au 1 to 500 mg / l 10 to 300 mg / l 20 to 200 mg / l Pd 1 to 200 mg / l 5 to 100 mg / l 15 to 60 mg / l Sn 1 to 500 mg / l 2 to 200 mg / l 3 to 100 mg / l Sb 1 to 500 mg / l 2 to 200 mg / l 3 to 100 mg / l Ti 20 to 500 mg / l 50 to 300 mg / l 50 to 150 mg / l Zr 20 to 500 mg / l 50 to 300 mg / l 50 to 150 mg / l Hf 20 to 500 mg / l 50 to 300 mg / l 50 to 150 mg / l

[0061] The metal ions contained in the rinsing solution are deposited either in the form of a salt containing the corresponding metal cation (e.g. molybdenum or tin) preferably in at least two oxidation states - in particular in the form of an oxide-hydroxide, a hydroxide, a spinel or a defect spinel - or in elemental form on the surface to be treated (e.g. copper, silver, gold or palladium).

[0062] Molybdenum ions are necessarily present as metal ions in the rinse solution. These are deposited as molybdate, preferably as

[0063] Ammonium heptamolybdate, and particularly preferably as ammonium heptamolybdate x 7 H 2 O, is added to the rinse composition. The molybdenum ions can also be added as sodium molybdate.

[0064] However, molybdenum ions can also be added to the rinse composition, for example, in the form of at least one salt containing molybdenum cations, such as molybdenum chloride, and then oxidized to molybdate by a suitable oxidizing agent, for example, the accelerators described above. In such a case, the rinse composition itself contains a corresponding oxidizing agent.

[0065] More preferably, the rinse composition contains molybdenum ions in combination with copper ions, tin ions or zirconium ions, with zirconium ions being mandatory.

[0066] The rinsing solution contains molybdenum ions in combination with zirconium ions and optionally a polymer or copolymer, in particular selected from the group consisting of the polymer classes of polyamines, polyethyleneamines, polyanilines, polyimines, polyethyleneimines, polythiophenes and polypyrroles as well as their mixtures and copolymers and polyacrylic acid, wherein the content of molybdenum ions is mandatory and the content of zirconium ions is preferably in the range of 10 to 500 mg / l (calculated as metal).

[0067] The content of molybdenum ions is preferably in the range from 20 to 225 mg / l, particularly preferably from 50 to 225 mg / l and very particularly preferably from 100 to 225 mg / l and the content of zirconium ions is in the range from 50 to 300 mg / l, particularly preferably from 50 to 150 mg / l.

[0068] According to a further preferred embodiment, the metal ions are copper ions. The rinse solution preferably contains these at a concentration of 100 to 500 mg / l, more preferably 150 to 225 mg / l.

[0069] According to a further embodiment, the rinse composition according to the invention contains at least one polymer selected from the group consisting of the polymer classes of polyamines, polyethyleneamines, polyanilines, polyimines, polyethyleneimines, polythiophenes and polypyrroles as well as mixtures and copolymers thereof.

[0070] The at least one polymer is preferably present in a concentration in the range from 0.1 to 5 g / l, more preferably from 0.1 to 3 g / l, more preferably from 0.3 to 2 g / l and particularly preferably in the range from 0.5 to 1.5 g / l (calculated as pure polymer).

[0071] Cationic polymers, especially polyamines, polyethyleneamines, polyimines, and / or polyethyleneimines, are preferred as polymers. Particular preference is given to using a polyamine and / or polyimine, and most preferably a polyamine.

[0072] According to one embodiment, the rinse composition disclosed herein contains at least one type of metal ion selected from the group consisting of the ions of molybdenum, copper, silver, gold, palladium, tin, antimony, titanium, zirconium and hafnium and at least one polymer selected from the group consisting of the polymer classes of polyamines, polyethyleneamines, polyanilines, polyimines, polyethyleneimines, polythiophenes and polypyrroles as well as mixtures and copolymers thereof, in each case in the following preferred, particularly preferred and very particularly preferred concentration ranges (polymer calculated as pure polymer and metal ions calculated as corresponding metal). Mon 1 to 1000 mg / l 10 to 500 mg / l 20 to 225 mg / l Cu 1 to 1000 mg / l 100 to 500 mg / l 150 to 225 mg / l Ag 1 to 500 mg / l 5 to 300 mg / l 20 to 150 mg / l Au 1 to 500 mg / l 10 to 300 mg / l 20 to 200 mg / l Pd 1 to 200 mg / l 5 to 100 mg / l 15 to 60 mg / l Sn 1 to 500 mg / l 2 to 200 mg / l 3 to 100 mg / l Sb 1 to 500 mg / l 2 to 200 mg / l 3 to 100 mg / l Ti 20 to 500 mg / l 50 to 300 mg / l 50 to 150 mg / l Zr 20 to 500 mg / l 50 to 300 mg / l 50 to 150 mg / l Hf 20 to 500 mg / l 50 to 300 mg / l 50 to 150 mg / l polymer 0.1 g / l to 3 g / l 0.3 g / l to 2 g / l 0.5 to 1.5 g / l

[0073] According to a preferred embodiment, the at least one polymer is a cationic polymer, in particular a polyamine and / or polyimine, and the metal ions are copper ions, molybdenum ions and / or zirconium ions, each in the following preferred, particularly preferred and very particularly preferred concentration ranges (polymer calculated as pure polymer and metal ions calculated as corresponding metal). Mon 1 to 1000 mg / l 10 to 500 mg / l 20 to 225 mg / l Cu 1 to 1000 mg / l 100 to 500 mg / l 150 to 225 mg / l Zr 20 to 500 mg / l 50 to 300 mg / l 50 to 150 mg / l cat. polymer 0.1 g / l to 3 g / l 0.3 g / l to 2 g / l 0.5 g / l to 1.5 g / l

[0074] The rinse composition preferably additionally comprises – particularly when the metallic surface is aluminum or an aluminum alloy – 20 to 500 mg / l, more preferably 50 to 300 mg / l, and particularly preferably 50 to 150 mg / l of Ti, Zr, and / or Hf in complexed form (calculated as metal). These are preferably fluorocomplexes. Furthermore, the rinse composition preferably comprises 10 to 500 mg / l, more preferably 15 to 100 mg / l, and particularly preferably 15 to 50 mg / l of free fluoride.

[0075] Particularly preferably, the rinsing composition contains Zr in complexed form (calculated as metal) and at least one type of metal ion selected from the group consisting of the ions of molybdenum, copper, silver, gold, palladium, tin and antimony, wherein the presence of ions of molybdenum is mandatory.

[0076] A rinse composition comprising Ti, Zr and / or Hf in complexed form preferably additionally contains at least one organosilane and / or at least one hydrolysis product thereof, i.e. an organosilanol, and / or at least one condensation product thereof, i.e. an organosiloxane / polyorganosiloxane, in a concentration range of 5 to 200 mg / l, more preferably of 10 to 100 mg / l and particularly preferably of 20 to 80 mg / l (calculated as Si).

[0077] The at least one organosilane preferably has at least one amino group. It is particularly preferably one that can be hydrolyzed to an aminopropylsilanol and / or to 2-aminoethyl-3-aminopropylsilanol and / or a bis(trimethoxysilylpropyl)amine.

[0078] The pH of the rinse composition is preferably in the acidic range, more preferably in the range of 3 to 5, particularly preferably in the range of 3.5 to 5.

[0079] Surprisingly, it was found that lowering the pH promotes the deposition of molybdenum ions on the phosphate-coated metallic surface. Therefore, for a rinsing solution containing molybdenum ions, the pH is preferably 3.5 to 4.5, and particularly preferably 3.5 to 4.0.

[0080] The rinse composition is essentially nickel-free. Preferably, it contains less than 0.1 g / l and more preferably less than 0.01 g / l of nickel ions.

[0081] The rinse composition preferably has a temperature in the range of 15 to 40 °C. The treatment of the metallic surface with the rinse composition is preferably carried out for 10 to 180 seconds, particularly preferably for 20 to 150 seconds, and most particularly preferably for 30 to 120 seconds, preferably by immersion or spraying.

[0082] The invention further relates to a phosphate-coated metallic surface which is obtainable by the process according to the invention.

[0083] The method according to the invention allows the electrical conductivity of the phosphate-coated metal surface to be specifically adjusted by creating defined pores in the phosphate layer. The conductivity can be either greater, equal to, or lower than that of a corresponding metal surface coated with a nickel-containing phosphate coating.

[0084] The electrical conductivity of the phosphate-coated metal surface adjusted by the method according to the invention can be influenced by varying the concentration of a given metal ion or polymer in the rinsing solution.

[0085] An electrocoating paint can then be cathodically deposited and a paint build-up applied to the phosphate-coated metallic surface treated with the rinsing composition.

[0086] If necessary, the metallic surface is first rinsed after treatment with the rinsing composition, preferably with demineralized water, and dried if necessary.

[0087] In the following, the present invention will be explained by non-limiting embodiments and comparative examples. Comparison example 1

[0088] A test plate made of electrolytically galvanized steel (ZE) was coated with a phosphating solution containing 1.3 g / l Zn, 1 g / l Mn, 13 g / l PO 4 3-< (calculated as P 2 O 5 ), 3 g / l NO 3 -< and 1 g / l nickel at 53 °C. No rinsing was performed. Subsequently, the current density i in A / cm 2< was measured across the applied voltage E in V vs. a silver / silver chloride (Ag / AgCl) electrode (see Fig. 1 : ZE_Variation11_2: Curve 3). The measurement was performed using linear sweep voltammetry (potential range: -1.1 to -0.2 V ref ; scan rate: 1 mV / s).

[0089] In all examples and comparative examples, the measured current density i depends on the electrical conductivity of the conversion coating. The following applies: The higher the measured current density i, the higher the electrical conductivity of the conversion coating. A direct measurement of the electrical conductivity in µS / cm, as is possible in liquid media, cannot be performed with conversion coatings.

[0090] In this case, the current density i measured for a nickel-containing conversion coating always serves as a reference point for statements about the electrical conductivity of a given conversion coating.

[0091] The indication "1E" in the Figures 1 to 4 always stands for "10." For example, "1E-4" means "10 -4<". Comparison example 2

[0092] A test plate according to Comparative Example 1 was coated using a nickel-free phosphating solution containing 1.3 g / l Zn, 1 g / l Mn, 16 g / l PO 4 3-< (calculated as P 2 O 5 ) and 2 g / l NO 3 -< at 53 °C without rinsing and then the current density i was measured against the voltage E according to Comparative Example 1 (see Fig. 1 . ZE_Variation1_1: Curve 1; ZE_Variation1_3: Curve 2).

[0093] How Fig. 1 As can be seen, the resting potential of the nickel-free system (Comparative Example 2) is shifted to the left compared to that of the nickel-containing system (Comparative Example 1). The electrical conductivity is also lower: the "arms" of curves 1 and 2 are each located below curve 3, i.e., toward lower current densities. Comparison example 3

[0094] A test plate according to Comparative Example 1 was coated using a nickel-free phosphating solution according to Comparative Example 2. The coated test plate was then treated with a rinsing solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and having a pH value of approximately 4. The current density i versus the voltage E was measured according to Comparative Example 1 (see Fig. 2 . ZE_Variation6_1: Curve 1; ZE_Variation6_2: Curve 2). Comparison is made with comparative example 1 ( Fig. 2 : ZE_Variation11_2: Curve 3) How Fig. 2 As can be seen, the resting potential of the nickel-free system is shifted to the left when using a rinsing solution containing ZrF 6 2-< (Comparative Example 3) compared to that of the nickel-containing system (Comparative Example 1). The electrical conductivity is also lower in the nickel-free system (see the comments on Comparative Example 2). Example 1 (not according to the invention)

[0095] A test plate according to Comparative Example 1 was coated using a nickel-free phosphating solution according to Comparative Example 2. The coated test plate was then treated with a rinsing solution containing approximately 220 mg / l copper ions and having a pH value of approximately 4. The current density i versus the voltage E was measured according to Comparative Example 1 (see Fig. 3 . ZE_Variation2_1: Curve 1; ZE_Variation2_2: Curve 2). Comparison is again made with comparative example 1 ( Fig. 3 : ZE_Variation11_2: Curve 3).

[0096] How Fig. 3 As can be seen, the resting potential of the nickel-free system when using a rinsing solution containing copper ions (Example 1) corresponds to that of the nickel-containing system (Comparative Example 1). The conductivity of this nickel-free system is slightly higher than that of the nickel-containing system. Example 2 (not according to the invention)

[0097] A test plate according to Comparative Example 1 was coated using a nickel-free phosphating solution according to Comparative Example 2. The coated test plate was then treated with a rinsing solution containing approximately 1 g / l (calculated on the pure polymer) of electrically conductive polyamine (Lupamin ®< 9030, manufacturer BASF) and having a pH value of approximately 4. The current density i versus the voltage E was measured according to Comparative Example 1 (see Fig. 4 . ZE_Variation3_1: Curve 1; ZE_Variation3_2: Curve 2). Comparison is made with comparative example 1 ( Fig. 4 : ZE_Variation11_2: Curve 3).

[0098] How Fig. 4As can be seen, the resting potential of the nickel-free system when using a rinsing solution containing an electrically conductive polymer (Example 2) corresponds to that of the nickel-containing system (Comparative Example 1). The electrical conductivity of the nickel-free system is slightly lower than that of the nickel-containing system. Comparison example 4

[0099] A test plate made of hot-dip galvanized steel (EA) was coated using a phosphating solution containing 1 g / l nickel according to Comparative Example 1. The coated test plate was then treated with a rinsing solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) with a pH value of approximately 4, and then the current density i in A / cm 2< was measured across the voltage E in V applied to a silver / silver chloride (Ag / AgCl) electrode (see Fig. 5 : EA 173: Curve 1). The measurement was performed using linear sweep voltammetry. Comparison example 5

[0100] A test plate according to Comparative Example 4 was coated using a nickel- and nitrate-free phosphating solution containing 1.2 g / l Zn, 1 g / l Mn and 16 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C without rinsing and then the current density i was measured against the voltage E according to Comparative Example 3 (see Fig. 5 . EA 167: Curve 3; EA 167 2: Curve 2).

[0101] How Fig. 5 As can be seen, the resting potential of the nickel-free system (Comparative Example 5) is shifted to the right compared to that of the nickel-containing system (Comparative Example 4). The electrical conductivity of the nickel-containing system is significantly lower, which is due to the passivation by the rinsing solution containing ZrF 6 2-<. Example 3 (not according to the invention)

[0102] A test plate according to Comparative Example 4 was coated using a nickel-free phosphating solution according to Comparative Example 2. The coated test plate was then treated with a rinsing solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions with a pH value of approximately 4. The current density i versus the voltage E was measured according to Comparative Example 1 (see Fig. 6 . EA 178: Curve 3; EA 178 2: Curve 2). Comparison is made with comparative example 3 ( Fig. 6 : EA 173: Curve 1).

[0103] How Fig. 6As can be seen, the resting potential of the nickel-free system when using a rinsing solution containing ZrF 6 2-< and molybdenum ions (Example 3) corresponds to that of the nickel-containing system (Comparative Example 4). By adding molybdenum ions (Example 3) to the rinsing solution containing ZrF 6 2-< (Comparative Example 4), the conductivity at the substrate surface could be significantly increased.

[0104] Test panels according to comparative examples 1 to 3 (VB1 to VB3) and examples 1 and 2 (B1 and B2) were coated with a cathodic electrocoat and a standard automotive paint system (filler, basecoat, clearcoat) after phosphating and then subjected to a cross-cut test according to DIN EN ISO 2409. Three panels each were tested before and after exposure to condensation water for 240 hours (DIN EN ISO 6270-2 CH). The corresponding results can be found in Table 1.A cross-cut score of 0 is the best, and a score of 5 is the worst. Values ​​of 0 and 1 are comparably good. Table 1 (Comparison) example Cross-hatch before exercise (0-5) after load (0-5) VB1 0 / 0 / 0 1 / 1 / 0 VB2 1 / 0 / 0 3 / 1 / 0 VB3 0 / 0 / 1 1 / 5 / 4 B1 1 / 0 / 0 0 / 0 / 1 B2 1 / 1 / 1 1 / 1 / 1

[0105] Table 1 reveals the poor results of VB2 and especially VB3 after loading, while B1 (copper ions) and B2 (electrically conductive polyamine) provide good results - VB1 (nickel-containing phosphate) at least comparable results. Comparison example 6

[0106] A test plate made of hot-dip galvanized steel (EA) was coated with a nitrite-accelerated phosphating solution (approximately 90 mg / l nitrite) containing 1.1 g / l Zn, 1 g / l Mn, 13.5 g / l PO 4 3-< (calculated as P 2 O 5 ), 3 g / l NO 3 -<, and 1 g / l nickel at 53 °C. The coated test plate was then treated with a rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and a pH of approximately 4. Comparison example 7

[0107] A test plate according to Comparative Example 6 was coated with a nickel-free, 35°C phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, 17 g / l PO 4 3-< (calculated as P 2 O 5 ), and 0.5 g / l NO 3 -<, with a nitrite-accelerated coating (approx. 90 mg / l nitrite). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4. Example 4

[0108] A test plate according to Comparative Example 6 was coated with a nickel- and nitrate-free phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, and 17 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C with a nitrite-accelerated coating (approx. 90 mg / l nitrite). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions at a pH of approximately 4. Comparison example 8

[0109] A test plate according to Comparative Example 6 was coated with a nickel-free, 35°C phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, 17 g / l PO 4 3-< (calculated as P 2 O 5 ), and 0.5 g / l NO 3 -<, accelerated by peroxide (approx. 80 mg / l H 2 O 2 ). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4. Example 5

[0110] A test plate according to Comparative Example 6 was coated with a nickel- and nitrate-free phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, and 17 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C, accelerated by peroxide (approx. 80 mg / l H 2 O 2 ). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4.

[0111] Test panels according to comparative examples 6 to 8 (VB6 to VB8) and examples 4 and 5 (B4 and B5) were coated with a cathodic electrocoat and a standard automotive paint system (filler, basecoat, clearcoat) after phosphating and then subjected to a cross-cut test according to DIN EN ISO 2409. Three panels each were tested before and after exposure to condensation water for 240 hours (DIN EN ISO 6270-2 CH). The corresponding results can be found in Table 2. Table 2 (Comparison) example Cross-hatch before exercise (0-5) after load (0-5) VB6 0 / 0 / 0 0 / 0 / 0 VB7 5 / 5 / 5 5 / 5 / 5 B4 1 / 0 / 0 1 / 0 / 1 VB8 5 / 4 / 5 5 / 5 / 5 B5 0 / 1 / 0 1 / 1 / 1

[0112] Table 2 shows the poor results of VB7 (nitrite-accelerated) and VB8 (peroxide-accelerated) compared to VB6, while B4 (nitrite-accelerated) and B5 (peroxide-accelerated) deliver good results comparable to VB6 (nickel-containing phosphating). Comparison example 9

[0113] A test plate made of hot-dip galvanized steel (EA) was coated with a nitrite-accelerated phosphating solution (approximately 90 mg / l nitrite) containing 1.1 g / l Zn, 1 g / l Mn, 13.5 g / l PO 4 3-< (calculated as P 2 O 5 ), 3 g / l NO 3 -<, and 1 g / l nickel at 53 °C. The coated test plate was then treated with a rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and a pH of approximately 4. Example 6

[0114] A test plate according to Comparative Example 9 was coated with a nickel- and nitrate-free phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, and 17 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C, accelerated by peroxide (approx. 80 mg / l H 2 O 2 ). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4. Comparison example 10

[0115] A blank steel test plate was coated with a nitrite-accelerated phosphating solution (approximately 90 mg / l nitrite) at 53 °C containing 1.1 g / l Zn, 1 g / l Mn, 13.5 g / l PO 4 3-< (calculated as P 2 O 5 ), 3 g / l NO 3 -<, and 1 g / l nickel. The coated test plate was then treated with a rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and a pH of approximately 4. Example 7

[0116] A test plate according to Comparative Example 10 was coated with a nickel- and nitrate-free phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, and 17 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C, accelerated by peroxide (approx. 80 mg / l H 2 O 2 ). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4. Comparison example 11

[0117] A test plate made of electrolytically galvanized steel (ZE) was coated with a nitrite-accelerated phosphating solution (approximately 90 mg / l nitrite) containing 1.1 g / l Zn, 1 g / l Mn, 13.5 g / l PO 4 3-< (calculated as P 2 O 5 ), 3 g / l NO 3 -<, and 1 g / l nickel at 53 °C. The coated test plate was then treated with a rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and a pH of approximately 4. Example 8

[0118] A test plate according to Comparative Example 11 was coated with a nickel- and nitrate-free phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, and 17 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C, accelerated by peroxide (approx. 80 mg / l H 2 O 2 ). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4.

[0119] After phosphating, test panels according to Comparative Examples 9 to 11 (VB9 to VB11) and Examples 6 to 8 (B6 to B8) were coated with a cathodic electrocoat and a standard automotive paint system (primer, basecoat, clearcoat) and subjected to the cross-cut test described above for VB6 to VB8, B4, and B5. The results are summarized in Table 3.

[0120] In addition, the test panels were subjected to a VDA test (VDA 621-415), in which the paint penetration (U) in mm was determined, as well as the paint detachment after stone impact (DIN EN ISO 20567-1, Procedure C). A result of 0 is the best, and a result of 5 the worst after stone impact. A value of up to 1.5 is considered a good value. The results are also in Table 3 summarized. Table 3 (Comparison) example Cross-hatch VDA before exercise (0-5) after load (0-5) U in mm Rockfall VB9 0 / 0 / 0 0 / 0 / 0 0,3 / 0,3 / 0,5 0,5 / 0 ,5 / 0,5 B6 0 / 0 / 1 1 / 1 / 1 0,8 / 1 / 1,3 1 / 1 / 0,5 VB10 0 / 0 / 0 0 / 0 / 0 0,5 / 0,5 / 0,3 1 / 1 / 1 B7 0 / 0 / 0 0 / 0 / 0 0,8 / 0,8 / 0,8 1 / 0,5 / 1 VB11 0 / 0 / 0 0 / 0 / 0 0,8 / 0,8 / 0,5 0,5 / 0,5 / 0,5 B8 0 / 0 / 0 1 / 0 / 1 1,5 / 1,8 / 1,3 1 / 1 / 1

[0121] Table 3 The good results achieved with the nickel-free process according to the invention on hot-dip galvanized steel (B6), bright steel (B7), and electrolytically galvanized steel (B8) can be seen. These results are comparable to the nickel-containing process (cf. B6 with VB9, B7 with VB10, and B8 with VB11). Comparison example 12

[0122] A test plate made of hot-dip galvanized steel (EA) was coated with a nitrite-accelerated phosphating solution (approximately 90 mg / l nitrite) containing 1.1 g / l Zn, 1 g / l Mn, 13.5 g / l PO 4 3-< (calculated as P 2 O 5 ), 3 g / l NO 3 -<, and 1 g / l nickel at 53 °C. The coated test plate was then treated with a rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and a pH of approximately 4. Example 9

[0123] A test plate according to Comparative Example 12 was coated with a nickel- and nitrate-free phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, and 17 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C, accelerated by peroxide (approx. 80 mg / l H 2 O 2 ). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4. Example 10

[0124] A test plate according to Comparative Example 12 was coated with a nickel- and nitrate-free phosphating solution containing 1.2 g / l Zn, 1 g / l Mn, and 13 g / l PO 4 3-< (calculated as P 2 O 5 ) at 45 °C, accelerated by peroxide (approx. 50 mg / l H 2 O 2 ). The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4. Comparison example 13

[0125] A blank steel test plate was coated with a nitrite-accelerated phosphating solution (approximately 90 mg / l nitrite) according to Comparative Example 12. The coated test plate was then treated with a rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and a pH of approximately 4. Example 11

[0126] A test plate according to Comparative Example 13 was coated using a peroxide-accelerated phosphating solution according to Example 9 (approx. 80 mg / l H 2 O 2 ). Subsequently, the coated test plate was treated with a rinsing solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions with a pH of approximately 4. Example 12

[0127] A test plate according to Comparative Example 13 was coated using a peroxide-accelerated phosphating solution according to Example 10 (approx. 50 mg / l H 2 O 2 ). Subsequently, the coated test plate was treated with a rinsing solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions with a pH of approximately 4. Comparison example 14

[0128] A test plate made of AA6014 S was coated with a nitrite-accelerated phosphating solution (approximately 90 mg / l nitrite) according to Comparative Example 12. The coated test plate was then treated with a rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and a pH of approximately 4. Example 13

[0129] A test plate according to Comparative Example 14 was coated using a peroxide-accelerated phosphating solution according to Example 9 (approx. 80 mg / l H 2 O 2 ). Subsequently, the coated test plate was treated with a rinsing solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions with a pH of approximately 4. Example 14

[0130] A test plate according to Comparative Example 14 was coated using a peroxide-accelerated phosphating solution according to Example 10 (approx. 50 mg / l H 2 O 2 ). Subsequently, the coated test plate was treated with a rinsing solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions with a pH of approximately 4.

[0131] Test panels according to comparative examples 12 to 14 (VB12 to VB14) and examples 9 to 14 (B9 to B14) were coated with a cathodic electrocoat and a standard automotive paint system (filler, basecoat, clearcoat) after phosphating.

[0132] The test panels of comparative examples 12 and 13 (VB12 and VB13) as well as examples 9 to 12 (B9 to B12) were subjected to the VDA test described above. The results are shown in Table 4 summarized.

[0133] The test panels of comparative example 14 (VB14) and examples 13 and 14 (B13 and B14) were subjected to a 240-hour CASS test according to DIN EN ISO 9227. The results are shown in Table 5 summarized. Table 4 (Comparison) example VDA U in mm Rockfall VB12 0,1 / 0,1 / 0,3 0,5 / 0,5 / 0,5 B9 0,8 / 0,8 / 0,3 1,5 / 1,5 / 1,5 B10 0,3 / 0,3 / 0,3 1 / 1 / 1 VB13 0,3 / 0,5 / 0,5 0,5 / 0,5 / 0,5 B11 1 / 0,5 / 1,3 1 / 1,5 / 1,5 B12 1,3 / 1,3 / 1 1 / 1 / 1 Table 5 (Comparison) example CASS VB14 0,8 / 0,8 / 0,8 B13 1,5 / 1,5 / 1,5 B14 1,5 / 1,5 / 1,3 Example 15

[0134] A test plate made of hot-dip galvanized steel (EA) was coated with a nickel- and nitrate-free phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, and 17 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C, accelerated by peroxide (approx. 80 mg / l H 2 O 2 ). The acid value of the phosphating solution was adjusted to 0.07. The coated test plate was then treated with a rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4. Example 16

[0135] A test plate made of hot-dip galvanized steel (EA) was coated with a nickel- and nitrate-free phosphating solution containing 1.1 g / l Zn, 1 g / l Mn, and 17 g / l PO 4 3-< (calculated as P 2 O 5 ) at 35 °C, accelerated by peroxide (approx. 80 mg / l H 2 O 2 ). The acid value of the phosphating solution was adjusted to 0.05. The coated test plate was then treated with a post-rinse solution containing approximately 120 mg / l ZrF 6 2-< (calculated as Zr) and 220 mg / l molybdenum ions, with a pH of approximately 4.

[0136] Test panels according to Examples 15 and 16 (B15 and B16) were coated with a cathodic electrocoat and a standard automotive paint system (primer, basecoat, clearcoat) after phosphating and then subjected to a cross-cut test before and after exposure to condensation for 240 hours as described above. The results are shown in Table 6 summarized. Example Cross-hatch before exercise (0-5) after load (0-5) B15 0 / 0 / 1 3 / 2 / 1 B16 0 / 1 / 0 1 / 1 / 1

[0137] Table 6 It can be seen that the cross-cut results after exposure to condensation water can be significantly improved by lowering the acid value (B16).

Claims

1. A method for substantially nickel-free phosphating of a metallic surface, wherein a metallic surface, optionally after cleaning and / or activation, is first treated with an acidic aqueous phosphating composition which comprises zinc ions, manganese ions, and phosphate ions, is optionally rinsed and / or dried, and is thereafter treated with an aqueous after-rinse composition which comprises from 10 to 500 mg / l (calculated as metal) of molybdenum ions as molybdate and zirconium ions and has a pH in the range from 3 to 5, wherein both the phosphating composition and the after-rinse composition comprise less than 0.3 g / l of nickel ions and wherein the phosphating composition comprises less than 0.5 g / l of nitrate.

2. The method according to claim 1, wherein the metallic surface is at least partially galvanized.

3. The method according to either of the preceding claims, wherein the phosphating composition comprises 0.5 to 3 g / l of complex fluoride and wherein the complex fluoride is tetrafluoroborate (BF4-) and / or hexafluorosilicate (SiF62-).

4. The method according to any of the preceding claims, wherein the phosphating composition comprises H2O2 as an accelerator.

5. The method according to any of the preceding claims, wherein the phosphating composition has a free acid in the range from 0.3 to 2.0, a free acid (diluted) in the range from 0.5 to 8, a total acid according to Fischer in the range from 12 to 28, a total acid in the range from 12 to 45 and an acid value in the range from 0.01 to 0.2.

6. The method according to any of the preceding claims, wherein the phosphating composition has an acid value in the range from 0.03 to 0.065.

7. The method according to any of the preceding claims, wherein the phosphating composition has a temperature in the range from 30 to 50°C, preferably in the range between 35 and 45°C.

8. The method according to claim 1, wherein the after-rinse composition comprises 20 to 225 mg / l of molybdenum ions and 50 to 300 mg / l of zirconium ions.

9. The method according to either of claims 1 and 8, wherein the pH of the after-rinse composition is 3.5 to 4.5, preferably 3.5 to 4.0.

10. The method according to any of the preceding claims, wherein the after-rinse composition comprises copper ions.

11. The method according to claim 10, wherein the after-rinse composition comprises 100 to 500 mg / l of copper ions.

12. The method according to any of the preceding claims, wherein the after-rinse composition comprises a polyamine and / or polyimine.

13. A phosphate-coated metallic surface, wherein it is obtainable by a method according to any of claims 1 to 12.