METHOD FOR PRODUCE A HOT OR COLD STRIP AND / OR A FLEXIBLY ROLLED STEEL FLAT PRODUCT FROM A HIGH-STRENGTH MANGANESE STEEL AND STEEL FLAT PRODUCT ACCORDING TO THESE

DE502017016548D1Active Publication Date: 2024-11-28SALZGITTER FLASHSTAHL GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502017016548
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-09-16
Filing Date
2017-09-12
Publication Date
2024-11-28
Estimated Expiration
2037-09-12

AI Technical Summary

Technical Problem

High-strength manganese-containing steel products exhibit a strong tendency to work hardening during flexible rolling, limiting the maximum degree of forming and requiring expensive annealing to restore formability, while also being prone to hydrogen-induced delayed cracking and embrittlement.

Method used

A method for producing flexibly rolled flat steel products with a high degree of forming capacity, combining TRIP and/or TWIP effects, involving specific alloy compositions and processing steps such as preheating, hot rolling, pickling, annealing, and flexible rolling at controlled temperatures to optimize strength, elongation, and resistance to hydrogen-induced issues.

Benefits of technology

The method achieves a high maximum degree of forming, improved strength and formability, and increased resistance to hydrogen-induced delayed cracking and embrittlement, reducing the need for subsequent annealing and enhancing the steel's mechanical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for producing a flexibly rolled steel flat product from a high-strength manganese-containing steel with TRIP and / or TWIP effects, as well as with increased resistance to hydrogen-induced delayed fracture and hydrogen embrittlement. Flexibly rolled steel flat products can be in the form of, for example, steel strips or steel sheets, with hot-rolled or cold-rolled strip being used as the semi-finished product for flexible rolling. The manganese content of these steels is between > 5 and < 10 wt%. The invention also relates to a method for producing hot-rolled or cold-rolled strip from a high-strength manganese-containing steel and to a steel flat product flexibly rolled according to the method.

[0002] In the context of the present invention, flexible rolling is understood to be a method for producing flat steel products in which a flat steel product with varying thicknesses is produced in virtually any sequence in the rolling direction via an adjustable roll gap. Thickness differences of up to 50% can be achieved within a flexibly rolled flat steel product; the advantage is the homogeneous transition between two constant thicknesses. The flat steel product produced by flexible rolling is preferably used as a semi-finished product for subsequent forming into a desired component, for example, by deep drawing or roll forming. The formed components are widely used in the automotive industry, for example, for the production of vehicle bodies.Flexible rolling advantageously achieves a thickness gradient in the flexibly rolled steel flat product that is adapted to the load-bearing capacity of the component to be subsequently formed from it. This results in material and weight savings and, optionally, allows multiple components to be integrated without additional joining processes, leading to lower manufacturing costs. This is particularly suitable for components that are subjected to varying stresses along their length.

[0003] European patent application EP 2 383 353 A2 discloses a high-strength manganese-containing steel, a flat steel product made from this steel, and a process for producing this flat steel product. The steel consists of the following elements (contents in wt.% based on the steel melt): C: up to 0.5; Mn: 4 to 12.0; Si: up to 1.0; Al: up to 3.0; Cr: 0.1 to 4.0; Cu: up to 4.0; Ni: up to 2.0; N: up to 0.05; P: up to 0.05; S: up to 0.01; as well as iron and unavoidable impurities. Optionally, one or more elements from the group "V, Nb, Ti" are included, the sum of the contents of these elements not exceeding 0.5. This steel is said to be characterized by being more cost-effective to produce than high-manganese steels, while simultaneously possessing high elongation at break values ​​and thus significantly improved formability.A process for producing a flat steel product from the aforementioned high-strength manganese-containing steel comprises the following steps: - Melting the aforementioned molten steel, - Producing a starting product for subsequent hot rolling by casting the molten steel into a strand, from which at least one slab or thin slab is cut as the starting product for hot rolling, or into a cast strip that is fed to the hot rolling process as the starting product, - Heat treating the starting product to bring it to a hot rolling start temperature of 1150 to 1000 °C, - Hot rolling the starting product into a hot strip with a thickness of at most 2.5 mm, with the hot rolling being terminated at a hot rolling end temperature of 1050 to 800 °C, - Coiling the hot strip into a coil at a coiling temperature of ≤ 700 °C.Optionally, the hot-rolled strip can be annealed at 250 to 950°C, then cold-rolled and annealed again at 450 to 950°C. The possibility of flexible rolling is not mentioned.

[0004] Furthermore, a method for manufacturing a product from flexibly rolled strip material is known from German patent DE 10 2012 110 972 B3. The flexible rolling is carried out as a cold rolling process. By means of flexible rolling, a flexibly rolled strip material with a variable thickness along its length is produced from a strip material with a largely constant thickness. An alloy composition for the flexibly rolled strip material is not mentioned.

[0005] Patent application US 2015 / 0147589 A1 also describes the flexible rolling of steel strips to produce strip material with at least two different thicknesses along the steel strip. The flexible rolling is carried out as flexible cold rolling. An excerpt of the alloy composition for the flexibly rolled strip material contains (contents in wt.%): C: ≤0.1; Mn: 0.5 to 7; Al: ≤0.1; P: ≤0.03; S: ≤0.005; N: ≤0.008; as well as the remainder being iron and process-related impurities.

[0006] European patent EP 1 238 727 B1 discloses a method for producing metallic strips with sections exhibiting different material properties. The metallic strips are produced in a two-roll casting machine, and strip-shaped sections with varying material properties are achieved by applying different cooling rates. This method can be used with low-alloy or micro-alloy steel alloys, which typically contain the following composition (contents in wt.%): C: 0.01 to 0.8; Mn: 0.3 to 5; Al: ≤0.1, plus the remainder being iron and unavoidable impurities. A strip produced by this method can be used as a feedstock for flexible rolling.

[0007] Furthermore, so-called TRIP steels are already described in German patent application DE 10 2012 013 113 A1. These steels have a predominantly ferritic microstructure with retained austenite, which can transform to martensite during forming (TRIP effect). Due to their high work hardening properties, TRIP steels achieve high values ​​for uniform elongation and tensile strength. TRIP steels are used, among other things, in structural, chassis, and crash-relevant components of vehicles, as sheet blanks, tailored blanks (welded blanks), and as flexible cold-rolled strips, so-called tailored rolled blanks (TRBs). The flexible cold-rolled strips enable a significant weight reduction through load-adapted sheet thickness along the component length. The steel has a manganese content of 1 to 2.25 wt%.

[0008] A method for producing a TWIP steel strip is also known from international patent application WO 2009 / 095264A1, wherein molten steel with a composition comprising 0.05–0.78% C, 11–23% Mn, at most 5% Al, at most 5% Cr, at most 2.5% Ni, at most 5% Si, at most 0.5% V, the remainder being iron and unavoidable impurities, is continuously cast into a slab with a thickness of at least 30 mm and at most 120 mm. The slab is then hot-rolled into a steel strip of the desired final thickness. In one embodiment, the hot-rolled steel strip is subsequently flexibly cold-rolled. The temperature of the steel strip before flexible rolling is limited to a maximum of 400 °C, preferably 200 °C. These temperature values ​​are also maintained during the rolling process. Following flexible rolling, the strip can be coated with zinc.

[0009] Furthermore, a process for manufacturing components from a metastable austenitic lightweight steel by rolling a sheet, exhibiting a temperature-dependent TRIP and / or TWIP effect during forming, is already known from international patent application WO 2014 / 180456 A1. To achieve high toughness of the component, rolling is carried out at a temperature above room temperature (40 to 160°C) to avoid the TRIP / TWIP effect, and to achieve high component strength, rolling is carried out at a temperature below room temperature (-65 to 0°C) to enhance the TRIP / TWIP effect.

[0010] The international patent application WO 2016 / 067624 A1 and the corresponding European patent application EP 3 214 193 A1 describe a process for producing a high-strength hot-rolled steel flat product with good formability, a high yield strength, and high tensile strength. The composition of the steel flat product comprises (in wt.%): C: 0.03 to 0.25; Mn: 4.2 to 6; P: 0.001 to 0.1; S: 0.0001 to 0.02; N: 0.0005 to 0.01; Si: 0.01 to 3; Ti: 0.005 to 0.2; and one or more of (in wt.%): Al: 0.01 to 2; Cr: 0.005 to 1; Nb: 0.005 to 2. V: 0.005 to 0.5; Sn: 0.002 to 0.2; Cu: 0.005 to 1; Ta: 0.001 to 0.01; B: 0.0003 to 0.005; Ni: 0.005 to 1; Mo: 0.005 to 1; Sb: 0.002 to 0.2; Ca: 0.0005 to 0.005; Mg: 0.0005 to 0.005; REM: 0.0005 to 0.005. A corresponding steel slab is heated to a temperature of 1100°C to 1300°C and then hot-rolled, with the final rolling temperature being between 750°C and 1000°C.The hot-rolled strip is then coiled and pickled at a temperature of 300°C to 750°C. Before subsequent cold rolling, the steel strip is annealed at a temperature of Ac1+20°C to Ac1+120°C for 600 to 21,600 seconds. Cold rolling is followed by another annealing at a temperature of Ac1 to Ac1+100°C for 20 to 900 seconds. The steel sheet is then either zinc-plated or zinc-plated followed by an alloy treatment at 450°C to 600°C, hot-dip galvanized, or electrolytically zinc-plated.

[0011] A problem in the production of flexible cold-rolled flat steel products from high-strength manganese-containing steel is the strong tendency for work hardening during flexible rolling, which significantly increases the forming forces and thus limits the maximum degree of deformation. Furthermore, the known manganese-containing steel exhibits a limited maximum rolling deformation due to the faster onset of martensite formation when formed at room temperature. Additionally, the residual formability of the resulting flat steel product is significantly reduced, so that, in some cases, costly annealing is required to restore formability before further forming processes.

[0012] Based on this, the present invention aims to provide a method for producing a flexibly rolled steel flat product from a high-strength manganese-containing steel with TRIP and / or TWIP effects, in particular for producing a flexibly rolled steel flat product which achieves a high maximum degree of deformation during flexible rolling and offers a good combination of strength and formability properties as well as high residual formability of the flexibly rolled steel flat product. The steel flat product produced in this way should also exhibit high resistance to hydrogen-induced delayed cracking, hydrogen embrittlement, and liquid metal embrittlement during welding.

[0013] This problem is solved by a method for producing a flexibly rolled steel flat product from a high-strength manganese-containing TRIP and / or TWIP steel with the features of claim 1. Advantageous embodiments of the invention are specified in the dependent claims. A steel flat product according to the invention is specified with the features of claim 10. A use of the steel flat product produced in this way is specified with the features of claim 12.

[0014] According to the invention, a method for producing a flexibly rolled steel flat product with a sectionally required final thickness from a high-strength manganese-containing steel having a tensile strength Rm of more than 1000 MPa to 2000 MPa and an elongation at break A50 of more than 3% to 45% in the most deformed areas of the steel flat product comprises the steps: Melting of a steel melt containing (in wt.%): C: 0.05 to 0.35; Mn: > 5 to < 10; Al: 0.05 to 5; P: < 0.1; S: < 0.1; N: < 0.1; balance iron including unavoidable steel-associated elements, with optional addition of one or more of the following elements (in wt.%): Si: up to 6; Cr: up to 6; Nb: up to 1; V: up to 1.5; Ti: up to 1.5; Mo: up to 3; Sn: up to 0.5; Cu: up to 3; W: up to 5; Co: up to 8; Zr: up to 0.5; Ta: up to 0.5; Te: up to 0.5; B: up to 0.15, via the process route blast furnace-steelworks or electric arc furnace-steelworks with optional vacuum treatment of the melt; casting of the molten steel into a strip using a near-net-shape horizontal or vertical strip casting process or casting of the molten steel into a slab or thin slab using a horizontal or vertical slab or thin slab casting process,Heating the roughing strip or slab or thin slab to a temperature of 1050 to 1250°C or inline rolling from casting heat, hot rolling to a uniform final thickness of 20 to 0.8 mm at a rolling temperature of 1050 to 800°C, coiling the hot strip at a coiling temperature of more than 100 to 800°C, pickling the hot strip, annealing the hot strip at a temperature of 500 to 840°C for a time of 1 min to 24 h in a continuous or hood annealing furnace, optional cold rolling of the hot strip to a uniform final thickness at room temperature or elevated temperature in one or more passes, optional annealing of the cold-rolled hot strip at a temperature of 500 to 840°C for 1 min to 24 h in a continuous or hood annealing furnace Flexible rolling of hot or cold strip in one or more rolling steps to the required final thicknesses in each section, with a temperature of the hot or cold strip from 60 °C to below Ac3.preferably from 60 °C to 450 °C, before the first rolling step, wherein this feature is understood to mean that the desired temperature is already reached before the first rolling step and is not only generated by the rolling itself, optional electrolytic zinc plating or hot-dip zinc plating of the hot or cold strip or application of another metallic, organic or inorganic coating before or after flexible rolling, , a steel flat product which achieves a high maximum degree of deformation during flexible rolling and offers a good combination of strength and forming properties as well as a high residual formability of the flexibly rolled steel flat product, and increased resistance to delayed cracking, hydrogen embrittlement and liquid metal embrittlement, which also exhibits a TRIP and / or TWIP effect under mechanical stress.

[0015] Particularly preferably, the hot or cold strip is preheated before the first rolling step to a temperature of 60 °C to below Ac3, preferably from 60 °C to 450 °C.

[0016] It is also advantageously provided that, with the exception of the first rolling step, the hot or cold strip is flexibly rolled in the subsequent rolling steps at the same or different temperatures of the hot or cold strip, from room temperature, which is in the range between 15 and 25 °C, down to below Ac3, advantageously at room temperature down to below 450 °C. In a special method, it is provided that the hot or cold strip is flexibly rolled in the first rolling step and the subsequent rolling steps at the same temperature of the hot or cold strip, from 60 °C down to below Ac3, advantageously from 60 °C down to below 450 °C.

[0017] In connection with the present invention, room temperature is defined as lying in the range between 15 and 25 °C.

[0018] Connected to the semi-warm rolling process with preheating, the final rolling step or steps can optionally be carried out at temperatures, optionally locally limited, from -100 to 60 °C, thereby selectively converting metastable austenite into martensite. This allows for a targeted increase in the strength of the finished semi-finished product or finished product.

[0019] Using the described manganese-containing steel, the following is now possible with the method according to the invention: Increasing the maximum degree of deformation of flexibly rolled medium manganese steel by reducing work hardening during flexible rolling. Targeted adjustment of strength and elongation properties by varying the forming temperature.

[0020] In an advantageous embodiment of the invention, cold rolling is carried out at a temperature before the first rolling step of 60 °C to below the Ac3 temperature, preferably from 60 to 450 °C, and heating or cooling between the rolling passes to 60 °C to below the Ac3 temperature, preferably from 60 to 450 °C. Cold rolling at an elevated temperature is advantageous in order to reduce the rolling forces and to promote the formation of deformation twins (TWIP effect).

[0021] Furthermore, it is planned that the cold-rolled strip will subsequently be annealed at a temperature of 500 to 840 °C for 1 min to 24 h in a continuous or hood annealing furnace to restore sufficient forming properties.

[0022] In connection with the aforementioned method according to the invention, a pre-strip produced near-net-shape by the two-roll casting process, with a thickness of less than or equal to 3 mm, preferably 1 mm to 3 mm, is already considered a hot-rolled strip with a uniform thickness. Due to the deformation introduced by the two counter-rotating rolls, the pre-strip produced in this way as a hot-rolled strip with a uniform thickness does not exhibit any original cast structure. Hot rolling thus takes place inline during the two-roll casting process, so that separate hot rolling is unnecessary.

[0023] The annealing of hot-rolled strip takes place at an annealing temperature of 500 to 840 °C and for a duration of 1 minute to 24 hours. Higher temperatures correspond to shorter treatment times, and vice versa. Annealing can be carried out, for example, in a bell annealing furnace (longer annealing times) or in a continuous annealing furnace (shorter annealing times). Annealing allows for the establishment of nearly homogeneous mechanical properties across the different thickness ranges of the flexibly rolled steel flat product, ensuring good machinability in subsequent forming processes.

[0024] According to the invention, the flexible rolling of hot or cold strip takes place after initial deformation in the range of 60 °C to below Ac3, preferably 60 °C to 450 °C, in one or more passes or rolling steps. This completely or partially suppresses the transformation of metastable austenite into martensite (TRIP effect) during the rolling process, and allows deformation twins (TWIP effect) to form in the austenite, which significantly increases the formability. This effect advantageously reduces the rolling forces and increases the overall formability.

[0025] Furthermore, the end product flexibly rolled at elevated temperature exhibits at least the same or higher strength properties (yield strength and / or tensile strength) than the end product flexibly rolled at room temperature, with the elongation at break being at least 5% or even 10% higher compared to flexible rolling at room temperature. Similarly, it is possible to set comparable values ​​for elongation at break, with the strength value (yield strength and / or tensile strength) being 10% higher than the values ​​for flexible rolling at room temperature.

[0026] After flexible rolling at elevated temperature, one or more final rolling steps can be carried out at temperatures, which can also be locally limited, from -100 to 60 °C, whereby metastable austenite is specifically converted into martensite and the strength in the affected area is significantly increased.

[0027] The inventive method for the flexible rolling of this material at elevated temperatures, through the optimization of the metallurgy, hot rolling conditions, and temperature-time parameters at the annealing furnace, results in a cold-rolled or hot-rolled strip that is particularly well-suited for subsequent flexible rolling. In particular, the rolling forces during flexible rolling are reduced, and the maximum degree of deformation is increased. The flexibly rolled steel flat product also exhibits increased residual formability, thus eliminating the need for annealing, such as...

[0028] This eliminates the need for recrystallization annealing of the material after flexible rolling.

[0029] According to the invention, strengths and residual elongations can be locally adjusted by local heating / cooling during flexible rolling, whereby higher strengths are achieved primarily through targeted cooling and higher residual elongations through local heating.

[0030] Due to the elevated temperature before rolling, deformation twins (TWIP effect) can be deliberately introduced. These twins further transform into martensite at room temperature, thereby increasing energy absorption capacity and allowing for a higher degree of deformation. Flat steel products manufactured in this way exhibit increased resistance to hydrogen-induced embrittlement and delayed cracking, as the TRIP effect is at least partially suppressed.

[0031] Preferably, the flexibly rolled steel flat product is hot-dip or electrolytically zinc-plated or coated with a metallic, inorganic, or organic material. If already galvanized hot- or cold-rolled strips are to be flexibly rolled, the heating temperature before rolling is advantageously limited to 60 to 450 °C to largely prevent zinc liquefaction. Furthermore, the zinc coating is subjected to only minimal thermal stress during semi-hot forming below 450 °C, thus ensuring cathodic corrosion protection of the coating even after the forming process.

[0032] It also exhibits good weldability. Furthermore, the production of this medium manganese steel according to the invention, based on the alloying elements carbon and manganese, is very cost-effective.

[0033] The steel according to the invention is an alloy exhibiting a TRIP and / or TWIP effect, which improves formability and tensile strength. Furthermore, component failure is mitigated in the case of overloads by locally deforming the component, thereby reducing stresses and thus mitigating sudden failure, for example, due to component breakage.

[0034] A flexibly rolled steel flat product produced according to the inventive method has a tensile strength Rm of more than 1000 MPa and an elongation at break A50 of more than 3% to 45% in the most deformed areas of the steel flat product.

[0035] Regarding the alloy composition for achieving the desired effects, the following element contents have proven to be particularly advantageous: C: 0.05 to 0.35 Mn: > 5 to < 10 Al: > 0.5 to 3 optionally in combination with Si: 0 - 6, preferably 0.05 - 3, particularly preferably 0.1 - 1.5 Cr: 0 - 6, preferably 0.1 - 4, particularly preferably > 0.5 - 2.5 Nb: 0 - 1, preferably 0.005 - 0.4, particularly preferably 0.01 - 0.1 V: 0 - 1.5, preferably 0.005 - 0.6, particularly preferably 0.01 - 0.3 Ti: 0 - 1.5, preferably 0.005 - 0.6, particularly preferably 0.01 - 0.3 Mo: 0 - 3, preferably 0.005 - 1.5, particularly preferably 0.01 - 0.6 Sn: 0 - 0.5, preferably < 0.2, particularly preferably < 0.05 Cu: 0 - 3, preferably < 0.5, particularly preferably < 0.1 W: 0 - 5, preferably 0.01 - 3, particularly preferably 0.2 - 1.5 Co: 0 - 8, preferably 0.01 - 5, particularly preferably 0.3 - 2 Zr: 0 - 0.5, preferably 0.005 - 0.3, particularly preferably 0.01 - 0.2 Ta: 0 - 0.5, preferably 0.005 - 0.3, particularly preferably 0.01 - 0.1 Te: 0 - 0.5, preferably 0.005 - 0.3, particularly preferably 0.01 - 0.1 B: 0 - 0.15,preferably 0.001 - 0.08, particularly preferably 0.002 - 0.01 ,

[0036] Alloying elements are generally added to steel to selectively influence specific properties. However, a single alloying element can affect different properties in different steels. The effect and interaction generally depend strongly on the quantity, the presence of other alloying elements, and the solution state within the material. The relationships are multifaceted and complex. The following section will discuss the effect of the alloying elements in the steel according to the invention in more detail. The positive effects of the alloying elements used according to the invention are described below.

[0037] The use of the term "to" in the definition of salary ranges, such as 0.005 to 0.6 weight %, means that the end values ​​- in the example 0.005 and 0.6 - are included.

[0038] Carbon (C): Carbon is required for the formation of carbides, stabilizes the austenite, and increases strength. Higher carbon contents impair weldability and, in the steels according to the invention, lead to a deterioration of elongation and toughness properties; therefore, a maximum content of 0.35 wt% is specified. To achieve the desired strength and minimum elongation at break values ​​in combination, a minimum addition of 0.05 wt% is provided. Contents of 0.05 to 0.35 wt% are provided.

[0039] Manganese (Mn): Mn stabilizes the austenite, increases strength and toughness, and enables deformation-induced martensite and / or twinning formation in the alloy according to the invention. Contents of 5 wt% or less are insufficient for stabilizing the austenite and thus impair the elongation properties, while at contents of 10 wt% or more, the austenite is stabilized too strongly, thereby reducing the strength properties, particularly the yield strength. For the manganese steel according to the invention with medium manganese contents, a range of more than 5 and less than 10 wt% is defined.

[0040] Phosphorus (P): Phosphorus is a trace element, originating predominantly from iron ore and dissolved in the iron lattice as a substitution atom. Through solid solution strengthening, phosphorus increases strength and hardness and improves hardenability. However, it is generally desirable to reduce the phosphorus content as much as possible, since, among other things, its low diffusion rate makes it highly susceptible to segregation and it significantly reduces toughness. Phosphorus deposition at the grain boundaries can lead to cracking along the grain boundaries during hot rolling. Furthermore, phosphorus raises the transition temperature from tough to brittle behavior by up to 300 °C. For the aforementioned reasons, the phosphorus content is limited to less than 0.1 wt%, preferably less than 0.04 wt%.

[0041] Sulfur (S): Like phosphorus, sulfur is present as a trace element in iron ore, but especially in the production route via the blast furnace process, it is bound in coke. It is generally undesirable in steel because it tends to segregate excessively and is highly embrittlement-causing. Therefore, every effort is made to minimize the amount of sulfur in the melt (e.g., through deep vacuum treatment). For the aforementioned reasons, the sulfur content is limited to less than 0.1 wt%, preferably less than 0.02 wt%.

[0042] Nitrogen (N): N is also an accompanying element in steel production. In its dissolved state, it improves the strength and toughness properties of steels with a higher manganese content of 4 wt% Mn or greater. Steels with a lower manganese content of less than 4 wt% Mn tend to exhibit a strong aging effect in the presence of free nitrogen. Even at low temperatures, the nitrogen diffuses across dislocations and blocks them. This results in an increase in strength coupled with a decrease in toughness. The nitrogen can be bound in the form of nitrides by adding alloying elements such as aluminum, vanadium, niobium, or titanium. For the aforementioned reasons, the nitrogen content is limited to less than 0.1 wt%, preferably less than 0.05 wt%.

[0043] Aluminum (Al): Al is added in amounts of 0.05 to 5 wt%. Al is used for the deoxidation of steels. Furthermore, the addition of Al advantageously improves the strength and elongation properties and positively influences the transformation behavior of the alloy according to the invention. An improvement in cold rollability has also been observed through the addition of Al. Al contents of up to 10 wt% significantly reduce the specific gravity of the steel and thus contribute to reducing fuel consumption in motor vehicles. However, higher Al contents significantly impair the casting properties in continuous casting.

[0044] This results in increased effort during casting. Furthermore, aluminum contents exceeding 5 wt% impair the elongation properties. Therefore, a maximum content of 5 wt% is specified. Preferably, an alloy addition in the range of greater than 0.05 wt% to 5 wt% is specified. A minimum aluminum content of > 0.5 wt% and a maximum content of 3 wt% are particularly preferred.

[0045] Silicon (Si): Si inhibits carbon diffusion, reduces specific density, and increases strength, elongation, and toughness. Furthermore, an improvement in cold rollability has been observed through the addition of Si. In alloys according to the invention, contents exceeding 6 wt% lead to embrittlement of the material and negatively affect hot and cold rollability as well as coating properties, for example, by zinc plating. Therefore, a maximum content of 6 wt% is specified. An alloying content in the range of 0.05 to 3 wt% is preferred, particularly in the range of 0.1 to 1.5 wt%.

[0046] Chromium (Cr): Cr improves strength and reduces the corrosion rate, delays ferrite and pearlite formation, and forms carbides. The maximum content is optionally set at less than 6 wt%, as higher contents result in a deterioration of the elongation properties. A Cr content of 0.1 to 4 wt% is preferred, and more preferably more than 0.5 to 2.5 wt%.

[0047] Microalloying elements are typically added in very small quantities (< 0.1 wt% per element). Unlike alloying elements, they primarily exert their effects through precipitation, but can also influence properties in the dissolved state. Even small additions of microalloying elements significantly affect processing and final properties. Particularly during hot forming, microalloying elements favorably influence recrystallization behavior and result in grain refinement.

[0048] Typical microalloying elements are vanadium, niobium, and titanium. These elements can be dissolved in the iron lattice and form carbides, nitrides, or carbonitrides with carbon and nitrogen.

[0049] Vanadium (V) and niobium (Nb): These minerals have a grain-refining effect, particularly through the formation of carbides, which simultaneously improves strength, toughness, and elongation properties. Contents above 1 wt% for Nb and 1.5 wt% for V offer no further advantages. Contents of 0.005 to 0.4 wt% for Nb, preferably 0.01 to 0.1 wt%, and 0.005 to 0.6 wt% for V, preferably 0.01 to 0.3 wt%, can be added optionally.

[0050] Titanium (Ti): As a carbide former, Ti acts to refine the grain structure, thereby simultaneously improving strength, toughness, and elongation properties, and reducing intergranular corrosion. Ti contents exceeding 1.5 wt% impair the elongation and forming properties in the alloys according to the invention; therefore, a maximum content of 1.5 wt% is optionally specified. Minimum contents of 0.005 to 0.6 wt%, preferably 0.01 to 0.3 wt%, can optionally be added.

[0051] Molybdenum (Mo): Mo acts as a strong carbide former, increasing strength and resistance to delayed cracking and hydrogen embrittlement. Mo contents above 3 wt% impair elongation properties; therefore, a maximum content of 3 wt% and a minimum content of 0.005 to 1.5 wt%, preferably 0.01 to 0.6 wt%, are optionally specified.

[0052] Tin (Sn): Sn increases strength, but, similar to copper, it accumulates at higher temperatures under the scale layer and at the grain boundaries. Its penetration into the grain boundaries leads to the formation of low-melting phases, resulting in cracks in the microstructure and solder brittleness. Therefore, a maximum content of up to 0.5, preferably less than 0.2, and particularly preferably less than 0.05 wt% is optionally specified.

[0053] Copper (Cu): Cu reduces the corrosion rate and increases strength. Contents above 3 wt% impair manufacturability due to the formation of low-melting phases during casting and hot rolling; therefore, a maximum content of 3 wt%, preferably less than 0.5 wt%, and particularly preferably less than 0.1 wt%, is optionally specified.

[0054] Tungsten (W): W acts as a carbide former and increases strength and high-temperature strength. W contents above 5 wt% impair elongation properties, therefore a content of 0.01 to 3 wt%, preferably 0.2 to 1.5 wt%, is optionally specified.

[0055] Cobalt (Co): Co increases the strength of the steel, stabilizes the austenite, and improves its high-temperature strength. Contents above 8 wt% impair the elongation properties in the alloys according to the invention; therefore, a content of 0.01 to 5 wt%, preferably 0.3 to 2 wt%, is optionally specified.

[0056] Zirconium Zr: Zr acts as a carbide former and improves strength. Zr contents above 0.5 wt% impair elongation properties, therefore an optional content of 0.3 wt% and a minimum content of 0.005 wt% are specified. A content of 0.01 to 0.2 wt% is particularly preferred.

[0057] Tantalum (Ta): Similar to niobium, Ta acts as a carbide former, refining the grain and thereby simultaneously improving strength, toughness, and elongation properties. Contents above 0.5 wt% do not result in any further improvement of these properties. Therefore, a maximum content of 0.5 wt% is optionally specified. Preferably, a minimum content of 0.005 wt% and a maximum content of 0.3 wt% are specified, within which grain refinement can be advantageously achieved. To improve cost-effectiveness and optimize grain refinement, a content of 0.01 wt% to 0.1 wt% is particularly preferred.

[0058] Tellurium (Te): Te improves corrosion resistance, mechanical properties, and machinability. Furthermore, Te increases the strength of MnS, resulting in less elongation in the rolling direction during hot and cold rolling. Contents above 0.5 wt% impair elongation and toughness properties, therefore a maximum content of 0.5 wt% is specified. Optionally, a minimum content of 0.005 wt% and a maximum content of 0.3 wt% are specified, which advantageously improve mechanical properties and increase the strength of existing MnS. Furthermore, a minimum content of 0.01 wt% and a maximum content of 0.1 wt% are preferred, which allow for optimization of mechanical properties while simultaneously reducing alloying costs.

[0059] Boron (B): B improves strength and stabilizes the austenite. Contents exceeding 0.15 wt% lead to embrittlement of the material. Therefore, in the steel according to the invention, B is optionally added in the range of 0.001 wt% to 0.08 wt%. A content of 0.002 to 0.01 wt% is particularly preferred.

[0060] The steel flat product described above according to the invention is particularly suitable for the production of flexibly rolled steel flat products, which, due to the adapted sheet thickness profile, enable weight reduction and thus lower production costs and increased efficiency. Flexibly rolled steel flat products are used, for example, in the automotive industry (vehicle bodies), agricultural technology, railway vehicle construction, transportation technology, and household appliance technology. Furthermore, the steel flat product according to the invention is particularly suitable for use in tailored welded blanks.

[0061] To investigate the mechanical properties of steel strips produced according to the invention from an exemplary alloy 1, tests were carried out. In addition to iron and impurities resulting from the melting process, alloy 1 contains, in particular, the following elements in the listed amounts in weight percent: alloy C Mn Al Si Leg. 1 0,2 7,0 0,9 0,5

[0062] The steel strips produced from the aforementioned alloy 1 were cold-rolled for comparison, i.e., at room temperature and thus below 50°C, and also rolled according to the invention at 250°C. The specified properties depend on the degree of deformation e. The degree of deformation e is defined as the quotient of the thickness change Δd of the investigated steel strip divided by the initial thickness d0 of the investigated steel strip. As is customary in flexible rolling, several cross-sections were used. The different degrees of deformation correspond to different thicknesses in flexible rolling. The characteristic values ​​can be obtained using both hot-rolled strip (characteristic values ​​determined on hot-rolled strip) and annealed cold-rolled strip. All characteristic values ​​are given for alloy 1: Rolling temperature Rp0.2 [MPa] Rm [MPa] A50 [%] Degree of deformation (e=Δd / d0) [%] RT (approx. 25 °C) 601 904 29,5 0 RT (approx. 25 °C) 1222 1317 2,5 44 250 °C 819 1070 27,9 17 250 °C 1017 1141 22,2 32 250 °C 1047 1296 20,3 44 250 °C 1119 1418 17,6 54

Claims

1. A method for producing a flexibly rolled flat steel product having a final thickness required in sections from a high-strength steel containing manganese with a tensile strength Rm of more than 1000 MPa to 2000 MPa and an elongation at break A50 of more than 3% to 45% in the most deformed areas of the flat steel product, comprising the steps of: - melting of a steel melt with an alloy composition containing (in wt.%): C: 0.05 to 0.35; Mn: > 5 to < 10; Al: 0.05 to 5; P: < 0.1; S: < 0.1; N: < 0.1; balance iron including unavoidable steel accompanying elements, with optional alloying of one or more of the following elements (in wt.%): Si: up to 6; Cr: up to 6; Nb: up to 1; V: up to 1.5; Ti: up to 1.5; Mo: up to 3; Sn: up to 0.5; Cu: up to 3; W: up to 5; Co: up to 8; Zr: up to 0.5; Ta: up to 0.5; Te: up to 0.5: B: up to 0.15, via the blast furnace steelworks or electric arc furnace steelworks process route with optional vacuum treatment of the melt, - casting the molten steel to form a pre-strip by means of a near-net-shape horizontal or vertical strip casting method or casting the steel melt to form a slab or thin slab by means of a horizontal or vertical slab or thin slab casting process, - heating the pre-strip or the slab or thin slab to a temperature of 1050 to 1250°C or inline rolling from the casting heat (first heat), - hot rolling to a uniform final thickness of 20 to 0.8 mm at a final rolling temperature of 1050 to 800°C, - coiling the hot strip at a coiling temperature of more than 100 to 800°C, - pickling the hot strip - annealing of the hot strip at a temperature of 500 to 840°C for a time of 1 min to 24 h in a continuous or bell annealer, - optional cold rolling of the hot strip to a uniform final thickness at room temperature or at an elevated temperature in one or more rolling passes, - optional annealing of the cold-rolled hot strip at a temperature of 500 to 840°C for 1 min to 24 h in a continuous or bell annealer - flexible rolling of the hot or cold strip in one or more rolling steps to the final thicknesses required in sections with a temperature of the hot or cold strip of 60°C to below Ac3, preferably of 60°C to 450°C, before the first rolling step, - optional electrolytic galvanizing or hot-dip galvanizing of the hot or cold rolled strip or application of another metallic, organic or inorganic coating before or after flexible rolling.

2. The method according to claim 1, wherein the hot or cold strip is preheated to a temperature of 60°C to below Ac3, preferably of 60°C to 450°C, before the first rolling step.

3. The method according to claim 1 or 2, wherein the hot or cold strip, with the exception of the first rolling step, is flexibly rolled in the following rolling steps at the same or different temperatures of the hot or cold strip from room temperature to below Ac3, advantageously at room temperature, which is in the area between 15 and 25°C, to below 450°C.

4. The method according to claim 1 or 2, wherein the hot or cold strip is flexibly rolled in the first rolling step and the following rolling steps at the same temperatures of the hot or cold strip of 60°C to below Ac3, advantageously at 60°C to below 450°C.

5. The method according to any one of claims 1 to 4, wherein a plurality of required rolling steps after the first rolling step with preheating, optionally the last rolling step or a plurality of last rolling steps are done at temperatures of -100 to 60°C.

6. The method according to claim 5, wherein the temperature effect on the flat steel product is locally limited.

7. The method according to at least any of claims 1 to 6, wherein the flat steel product is produced with the following alloy composition in % by weight: Al: > 0.5 to 38. The method according to at least any of claims 1 to 7, wherein the flat steel product is produced with the following alloy composition in % by weight: Si: 0.05 - 3, preferably 0.1 - 1.5 Cr: 0.1 - 4, preferably > 0.5 - 2.5 Nb: 0.005 - 0.4, preferably 0.01 - 0.1 V: 0.005 - 0.6, preferably 0.01 - 0.3 Ti: 0.005 - 0.6, preferably 0.01 - 0.3 Mo: 0.005 - 1.5, preferably 0.01 - 0.6 Sn: < 0.2, preferably < 0.05 Cu: < 0.5, preferably < 0.1 W: 0 - 5, 0.01 - 3, preferably 0.2 - 1.5 Co: 0.01 - 5, preferably 0.3 - 2 Zr: 0.005 - 0.3, preferably 0.01 - 0.2 Ta: 0.005 - 0.3, preferably 0.01 - 0.1 Te: 0.005 - 0.3, preferably 0.01 - 0.1 B: 0.001 - 0.08, preferably 0.002 - 0.

019. The method according to claim 1, wherein the cold rolling is done at a temperature before the first rolling step of 60°C to below the Ac3 temperature, preferably of 60 to 450°C, and heating or cooling between the rolling passes to 60°C to below the Ac3 temperature, preferably to 60 to 450°C, takes place.

10. A flexible rolled flat steel product produced by the method according to at least any of claims 1 to 9, wherein the tensile strength Rm of the flat steel product is more than 1000 MPa to 2000 MPa and the elongation at break A50 is more than 3% to 45% in the most deformed areas.

11. The flexible rolled flat steel product according to claim 10, wherein the flat steel product is hot-dip or electrolytically galvanized or metallically, inorganically or organically coated.

12. Use of a flat steel product according to claims 10 and 11 for use in the automotive industry, agricultural engineering, rail vehicle construction, transportation technology, household appliance technology or as welded blanks (tailored welded blanks).