OPTIMIZED SEGMENTATION METHOD
Patent Information
- Application Number
- DE502018015188
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-08-07
- Filing Date
- 2018-08-02
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2038-08-02
AI Technical Summary
Additive manufacturing processes face challenges in achieving homogeneity at the boundaries between different solidification areas due to varying energy input parameters, leading to potential weaknesses and distortions in the finished object.
A method and device that generate control data for additive manufacturing by defining sub-areas with different energy input parameters, allowing the energy beam to move continuously across the boundary while adjusting parameters within a specific region to ensure homogeneous solidification, avoiding abrupt changes and potential weak points.
This approach ensures more uniform and homogeneous solidification, reducing mechanical parameter jumps and enhancing the strength and quality of the manufactured objects by gradually changing energy input parameters during the transition between sub-areas.
Description
[0001] The invention relates to a method and a device for providing control data for an additive manufacturing device, a correspondingly adapted additive manufacturing method, a correspondingly adapted additive manufacturing device and a correspondingly adapted computer program.
[0002] Additive manufacturing devices and associated processes are generally characterized by the fact that they produce objects by solidifying a formless build material layer by layer. Solidification can be achieved, for example, by supplying thermal energy to the build material, by irradiating it with electromagnetic radiation or particle radiation (e.g., laser sintering (SLS or DMLS) or laser melting or electron beam melting), or by inducing a crosslinking reaction in the build material (e.g., stereolithography).
[0003] WO 2015 / 000854 A1 describes a method for the layer-by-layer production of a three-dimensional object, in which a powdered or liquid building material that can be solidified by exposure to electromagnetic or particle radiation is applied in layers with a layer thickness d, and in each layer, the locations corresponding to a cross-section of the object assigned to that layer are solidified. Each cross-section consists of a contour region and an interior region, and the method includes the following sub-step: In a sequence of N consecutive cross-sections, where N is an integer greater than 1, a sub-region in each cross-section is defined as a critical region and the remainder of the cross-section is defined as a non-critical region. In particular, a number of N layers are applied successively without solidification of the non-critical regions.Only after the application of the Nth layer does the non-critical areas of all N layers become solidified.
[0004] EP 3 127 635 A1 describes a radiation-based additive manufacturing process in which an object is produced that has a lateral overhang. To prevent a change in the shape of the overhang, as it is surrounded by unsolidified powder, the radiation energy to be introduced into the build material is reduced in the overhang. The energy to be introduced is reduced most significantly at those points of the overhang that protrude the furthest from the object.
[0005] US 2016 / 263832 describes a component of a CAM system that instructs a 3D printer to apply material from a print head in a spiral pattern in one layer.
[0006] CN 103 231 055 A describes a differential 3D printing process in which each layer is divided into an outer, middle and inner region, in which the laser is moved at different speeds in the outer, middle and inner regions.
[0007] The article DD Gu et al: "Laser additive manufacturing of metallic components: materials, processes and mechanisms" in INTERNATIONAL MATERIALS REVIEWS, Vol. 57, No. 3, pp. 133-164 gives an overview of laser-based additive manufacturing processes.
[0008] European patent application EP 2 565 018 A1 addresses the problem that, when components are built layer by layer using additive manufacturing processes, stresses arise during the cooling or curing of the building materials, which lead to component distortion. To solve this problem, it is proposed to divide the component to be manufactured into 3D volume regions, each of which is realized by solidifying the building material. The goal is to optimize the size and shape of the volume regions, and in particular the contours of the outer surfaces of the volume regions, so that the stresses resulting after completion of the component are minimal. In this case, it is proposed to either leave a gap between two volume regions or to allow volume regions to overlap with one another.
[0009] The inventors have discovered that the introduction of volume regions in the object to be manufactured, each of which is solidified separately and possibly with different material solidification parameters, can lead to problems with homogeneity, particularly strength, at the points where volume regions adjoin one another. The object of the present invention is therefore to provide a method and a device by means of which the homogeneity of objects manufactured by an additive manufacturing process can be improved.
[0010] The object is achieved by a computer-aided method according to claim 1, an additive manufacturing method according to claim 10, a device according to claim 11, a computer program according to claim 12, and an additive manufacturing device according to claim 13. Further developments of the invention are claimed in the dependent claims. In particular, a device according to the invention can also be further developed by features of the methods according to the invention set out below or in the dependent claims, and vice versa. Furthermore, the features described in connection with a device can also be used to further develop another device according to the invention, even if this is not explicitly stated.
[0011] A computer-aided method according to the invention for providing control data for an additive manufacturing device for producing a three-dimensional object, wherein the object is produced by means of the additive manufacturing device by applying a building material layer upon layer and solidifying the building material by supplying radiant energy to locations in each layer that are associated with the cross-section of the object in this layer, by an energy input device for introducing energy into the building material scanning these locations with at least one energy beam according to a set of energy input parameters, comprises: a first step of accessing computer-based model data of at least one section of the object to be produced, a second step of defining a first sub-area and a second sub-area within the at least one object section, which adjoin one another at a boundary, a third step of generating at least one data model of a region of a building material layer to be selectively solidified for producing the at least one object section, in which a first sub-area cross-section intersects the first sub-area and a second sub-area cross-section intersects the second sub-area, wherein the data model specifies,that in the first partial area cross-section at least one energy input parameter has on average a different value than in the second partial area cross-section and during the introduction of energy into the building material by the at least one energy beam, the at least one energy beam is moved several times across the boundary and a fourth step in which control data corresponding to the at least one data model generated in the third step are provided for the generation of a control data set for the additive manufacturing device, wherein in the third step data models of n+1 consecutive building material layers are generated, where n is a natural number, wherein in the data models of n consecutive building material layers a scanning of the building material with the at least one energy beam only in the first partial area cross-section,but not specified in the second partial area cross-section and in the data model of the subsequent n+1 -th building material layer a sampling of the building material in the first partial area cross-section and in the second partial area cross-section is specified, wherein in the third step the value of at least one energy input parameter is changed within a boundary region, which is a region in the building material layer described by the data model on at least one side of the boundary, in which the locations to be solidified have a maximum distance of 2000 µm, more preferably 1500 µm, even more preferably 1000 µm, even more preferably 100 µm, most preferably 50 µm from the boundary.
[0012] With such a procedure, hardening in both sub-area cross-sections is only specified in the n+1th layer with at least one energy input parameter that differs on average. During hardening of the second sub-area cross-section in the n+1th layer, the energy input parameters are then selected such that when the n+1th layer is scanned in the second sub-area cross-section, the build-up material in the n preceding layers in the second sub-area cross-section is also hardened. This means, however, that different energy input parameters must be selected in the second sub-area cross-section than in the first sub-area cross-section. By moving the energy beam across the boundary during the introduction of energy (i.e., in one pass), homogeneous hardening can still be ensured at the boundary between the two sub-areas.
[0013] This approach allows for structures to be created with higher resolution in the first sub-area than in the second sub-area. For example, if the first sub-area contains surface areas of the object to be manufactured that are difficult to rework, these can be built with greater precision than the interior of the object, where high detail resolution is not essential. The interior of the object can be solidified, for example, by solidifying several layers at once with high energy density and / or high speed and / or a large diameter of the radiation impact area on the layer.
[0014] If an energy beam crosses the boundary between the first and second sub-regions (s-cross-section) in one go, the value of an energy input parameter must be changed at some point, since in the second sub-region (s-cross-section) the value of at least one energy input parameter is on average different than in the first sub-region (s-cross-section). This change of at least one energy input parameter value preferably takes place in a boundary region close to the boundary. The extent of the boundary region, within which the parameter is expediently changed, depends, among other things, on the system inertia of the energy input device used in the individual case. For a high traversing speed of the energy beam, for example, a larger extent of the boundary region perpendicular to the boundary will generally be selected.Since the boundary between the first sub-area cross-section and the second sub-area cross-section does not necessarily have to be a straight line in plan view, the spatial distance or maximum spatial distance to the boundary is conveniently determined along a perpendicular from a point to be strengthened to the boundary. If the boundary region is selected so that it has a relatively large extent perpendicular to the boundary, then the energy input parameter values can be modified at different points within the boundary region (i.e., with varying distances from the boundary). This creates a mixture of areas that were strengthened with different energy input parameter values. The advantage of this is that the energy input parameter values are not modified at an exact boundary line, which could potentially prove to be a weak point (predetermined fracture line) after the object is completed.
[0015] Additive manufacturing devices and methods to which the present invention relates are, in particular, those in which energy is selectively supplied to a layer of the build material in the form of electromagnetic radiation or particle radiation. The working plane is a plane in which the upper side of the layer to which the energy is supplied lies. In this case, the energy input device can comprise, for example, a laser or an electron beam source; however, a UV light source, as is used in particular in stereolithography, would also be conceivable. While in stereolithography, solidification of the build material is brought about by the radiation acting on the build material causing a crosslinking reaction therein, in other methods, in particular laser sintering, laser melting or electron beam melting, heat is supplied to the build material.The build-up material is partially or completely melted using the energy introduced by the radiation, causing the components of the build-up material (e.g., powder grains) to bond together. After cooling, the build-up material then exists as a solid. Since the transitions between surface melting (sintering) and complete melting (melting) are fluid, the terms sintering and melting are used synonymously in this application, and no distinction is made between sintering and melting.
[0016] When this application refers to layers located below or above an object's cross-section, this direction refers to a direction that is essentially perpendicular to the layer planes or perpendicular to the construction plane. The term "essentially" here expresses that the layer thickness may not be uniform in some cases, e.g., the layer thickness may vary monotonically across the object's cross-section. In this context, it is assumed that underlying layers are applied before the overlying layers and are therefore arranged below the overlying layers.
[0017] It should also be noted at this point that using an additive manufacturing device according to the invention, not only one object but also multiple objects can be manufactured simultaneously. Whenever the present application refers to the manufacture of one object, it is understood that the respective description is equally applicable to additive manufacturing methods and devices in which multiple objects are manufactured simultaneously.
[0018] A control data set (often also referred to as a control command set) is considered here to be a sequence of instructions to apply layers of the build material one after the other and to scan areas of the respective layers, which correspond to the cross-section of an object to be manufactured, with energy radiation in order to solidify the build material.
[0019] In detail, a control data set is based on a computer-based model of the object(s) to be manufactured, preferably a CAD model. For each build material layer during production, the control data set specifies, in particular, the thickness of the layer application and the locations at which the build material is to be solidified by radiation. Furthermore, a control data set often also contains production-specific information, for example regarding the position and orientation of the objects in the additive manufacturing device or regarding the diameter of the energy beam (bundle) when it hits the build material. As a rule, the control data set contains all the data required to control the energy input device, which specifies, among other things, the energy density of the energy radiation or the travel speed of the beam bundle over the build material and / or an irradiation pattern.
[0020] The control data set can thus be viewed as the totality of all control data specified for controlling the manufacturing process in an additive manufacturing device. The control data related to an individual layer is also referred to below as a layer data set. In the present application, it is particularly assumed that a layer data set contains a data model of the locations of an object cross-section to be solidified during the manufacturing process. Such a data model is generally generated by dividing a CAD model of the object to be manufactured into layers (referred to in technical jargon as slicing). However, it is also conceivable to extract a two-dimensional representation of the object cross-section to be solidified in a layer using one or more beams from the computer-based CAD model of the object in another way.The layer data set specifies locations corresponding to an object cross-section that are to be solidified in the associated build-up material layer. Furthermore, further information regarding the production of the object cross-section can be included, in particular the chronological sequence in which locations corresponding to an object cross-section are to be solidified, i.e., a scan line or scanning track along which solidification is to take place, or, for example, the layer thickness or irradiation parameter values such as the diameter or travel speed of a beam impinging on the build-up material, etc. It should be emphasized that there are also special cases in which a layer data set does not refer to a complete object cross-section, but only to a part of it.
[0021] The computer-based model data can, for example, be a CAD model of the object section to be manufactured, which is available in STL format, for example, and does not yet contain any information about the decomposition into layers for layer-by-layer production, or a number of layer data sets. It should be noted here that in the present application, the term "number" is always to be understood as "one or more." Furthermore, it should be noted that the object section does not necessarily refer to a part of the object to be manufactured, but can also encompass the entire object to be manufactured.
[0022] Access to the model data can be achieved by reading the model data from a memory or receiving it over a network. The model data for the entire object section does not necessarily have to be read in at once. It is also possible to have a longer time interval between accesses to parts of the model data, for example, parts of the model data are read in as needed during a production process for the object section, and a generated data model is then integrated into the control data set during the production process.
[0023] If energy input parameter values are already specified in the model data of the object section, then in the second step, the first and second sub-areas are preferably defined such that at least one energy input parameter in the first sub-area has a different average value than in the second sub-area. Each sub-area preferably extends over a plurality of build-up material layers to be applied during its manufacture.
[0024] If energy input parameters already specified in the model data have a multitude of values or fluctuate significantly within the object section, i.e., they change particularly over small areas, the second step preferably does not specify an arbitrary number of sub-areas, but rather only a limited number of sub-areas that differ in that the value of at least one energy input parameter differs, at least on average. In practice, for example, a sub-area can be defined by the fact that the energy input parameter values within it do not exceed a specified degree of fluctuation.
[0025] If the model data of the object section already contains a number of layer data sets, the generation of at least one data model in the third step can consist of modifying a data model of a building material layer already present in the model data. Otherwise, a data model of a building material layer can be generated for the first time in the third step, in which case a different value is specified on average for at least one energy input parameter in the first sub-area cross-section than in the second sub-area cross-section.
[0026] Furthermore, it should be emphasized that in the third step, a data model of a building material layer is created in which the boundary between the first and second partial areas lies at least partially inside the object section. In other words, a data model of a building material layer is created in which the boundary between the first and second partial areas is at least partially not above unconsolidated building material and is not covered by unconsolidated building material during the construction process. In other words, in the third step, a data model of a building material layer is created in which the boundary between the first and second partial areas runs at least partially, preferably completely, above points to be consolidated in the underlying layer and below points to be consolidated in the underlying layer.This is achieved by the first sub-area cross-section intersecting the first sub-area, and the second sub-area cross-section intersecting the second sub-area. The term "intersect" here expresses that in the generated data model, neither the first sub-area cross-section nor the second sub-area cross-section coincide with a floor or top surface of the first sub-area or second sub-area, respectively. This specification automatically places the boundary between the first and second sub-areas at least partially within the object section.
[0027] In a data model generated in the third step, it is not specified that each partial area cross-section is first completely scanned with an energy beam before an adjacent partial area cross-section is scanned with the energy beam. Rather, it is specified that an energy beam is moved essentially continuously, i.e. without stopping, across the boundary between the first and second partial areas or first and second partial area cross-sections. The energy beam therefore first scans locations in the first partial area cross-section and, while scanning the build-up material, i.e. essentially without interrupting the energy supply to the build-up material, crosses the boundary to the second partial area cross-section, in order to then scan locations in the second partial area cross-section based on a changed value of at least one energy input parameter.
[0028] If the energy beam has a flat impact area on the build-up material or the working plane, i.e. does not impact essentially in a point-like manner, moving the energy beam across the boundary means in particular that the impact area of the energy beam on the build-up material completely crosses the boundary. Preferably, the energy beam is therefore moved so far into the other partial area (s-cross section) that the build-up material in the other partial area (s-cross section) is not only scanned close to the boundary. In other words, the first partial area cross section and the second partial area cross section are scanned with the energy beam in one go, i.e. essentially without any interruption in movement at the boundary. A scan line, i.e. the scanning path on the build-up material orIn the working plane, the second partial area cross-section is traversed immediately after a scan line in the first partial area cross-section. Preferably, the entire first and second partial area cross-section are scanned in this way.
[0029] It should be noted that the control data provided for the generation of a control data record can, on the one hand, consist of the at least one data model itself generated in the third step, but, on the other hand, the at least one data model can also be further prepared by the control command set according to the format requirements.
[0030] The procedure according to the invention allows the energy to be introduced into the construction material as homogeneously as possible, despite different values of an energy input parameter in two adjacent sub-regions. This makes it possible to avoid abrupt changes in property parameters in the finished object at the boundary between the sub-regions in different sub-regions of an object cross-section in which energy is introduced with different values of at least one energy input parameter. The more homogeneous solidification caused by such a procedure can, in particular, ensure smooth changes in the property parameters of the object. The present application defines greater homogeneity of the manufactured object at a transition within the object as, in particular, smaller jumps in a property of the object at this transition.The described procedure can reduce or prevent jumps in mechanical parameters, such as elongation at break, and thus, for example, ensure greater strength of the manufactured objects. For example, a more uniform quality of the crystalline structure of an object produced using a metal-based additive manufacturing process can be achieved. Of course, the inventive procedure is not limited to two adjacent sub-regions with different energy input parameter values, but is applicable to all adjacent sub-regions in an object, each with different energy input parameter values.
[0031] In practice, minor disturbances may occur during the movement of an energy beam, particularly a laser or electron beam, due to delayed reactions in the mechanics or electronics of the energy input device. These effects can also be tolerated with the procedure according to the invention. In any case, the method just described aims to move an energy beam as continuously as possible across the boundary between two sub-regions. Brief interruptions of the energy beam, e.g., when changing an energy input parameter, must be tolerated, but are not intended according to the invention. As long as such interruptions are less than one or more microseconds, preferably less than ten microseconds, they are tolerable within the scope of the invention. Even interruptions of several tens of microseconds are still acceptable in some cases.
[0032] In a variant of the procedure, in the first step, model data is accessed which comprises a number of layer data sets, each layer data set comprising a data model of a region of a build-up material layer which is to be selectively solidified during production and which corresponds to a cross-section of the object section.
[0033] This previously mentioned variant of the approach simplifies the process because existing shift data sets can be used, which are simply modified. Particularly if energy input parameter values are already specified in the shift data sets, the first and second sub-areas can preferably be defined in the second step such that at least one energy input parameter in the first sub-area has a different average value than in the second sub-area.
[0034] If an energy beam crosses the boundary between the first and second sub-regions (s-cross-section) in one go, the value of an energy input parameter must be changed at some point, since in the second sub-region (s-cross-section) the value of at least one energy input parameter is on average different than in the first sub-region (s-cross-section). This change of at least one energy input parameter value preferably takes place in a boundary region close to the boundary. The extent of the boundary region, within which the parameter is expediently changed, depends, among other things, on the system inertia of the energy input device used in the individual case. For a high traversing speed of the energy beam, for example, a larger extent of the boundary region perpendicular to the boundary will generally be selected.Since the boundary between the first sub-area cross-section and the second sub-area cross-section does not necessarily have to be a straight line in plan view, the spatial distance or maximum spatial distance to the boundary is conveniently determined along a perpendicular from a location to be consolidated to the boundary. If the boundary region is selected such that it has a relatively large extension perpendicular to the boundary, then the energy input parameter values can be modified at different locations within the boundary region (i.e., at varying distances from the boundary). This creates a mixture of areas that were consolidated with different energy input parameter values.
[0035] The advantage of this is that the energy input parameter values are not changed at an exact boundary line, which could possibly turn out to be a weak point (predetermined fracture line) after completion of the object.
[0036] Further preferably, the value of at least one energy input parameter is changed immediately upon crossing the limit.
[0037] If different values of energy input parameters are specified for different sub-areas of the object to be manufactured, it is advisable to change the energy input parameter values directly at the boundary between sub-areas, even if an energy beam is traversed across the boundary without interruption. How quickly the energy input parameter can actually be changed depends on the equipment conditions. In this case, a change at the boundary between two sub-areas is targeted in the control data. If necessary, equipment delays are taken into account by specifying a changed value of an energy input parameter for the energy beam before the energy beam has yet reached the boundary.Due to any delays in the equipment, the energy input parameter is then changed as close as possible to the boundary, i.e., when the energy beam moves across the boundary (when crossing the boundary). Even if the impact area of an energy beam on the build-up material is not point-like but has a surface area, a change in the value of an energy input parameter when crossing the boundary can be specified in such a way that the value of the energy input parameter is changed while the impact area moves across the boundary. In any case, the method relates to the specification of the control data for the energy input device, i.e., in particular, to the location or coordinate information provided to the energy input device by the control data.
[0038] As an alternative to the procedure just described, the value of at least one energy input parameter can be gradually changed within the boundary region.
[0039] Although it is naturally desirable that the exact value of an energy input parameter be specified at all locations in the sub-regions with different values of this energy input parameter, it may be easier in practice if the value of an energy input parameter within a boundary region is changed gradually rather than abruptly. This may mean, on the one hand, that the value of an energy input parameter is changed in several stages from the value within the first sub-region (s-section) to the value within the second sub-region (cross-section), or it may be changed essentially continuously from the value within the first sub-region (cross-section) to the value within the second sub-region (cross-section).
[0040] Here, we speak of an "essentially continuous" change, since in practice, a continuous change (which implies an infinite number of steps) is not possible. In practice, there is always a maximum speed at which the value of an energy input parameter can be changed. Since the value of an energy input parameter is essentially changed during the movement of the energy beam, the impact area of the energy beam already moves a bit further during the change of the energy input parameter value. In practice, therefore, even with an intended continuous change in the value of an energy input parameter, the energy input will always change in steps. It should be noted in passing that the control data cannot specify different values of an energy input parameter with arbitrarily fine granularity. In practice, discrete value specifications will always be present.
[0041] Further preferably, the at least one energy beam bundle scans the build material in the first partial area cross-section along first scan lines and the build material in the second partial area cross-section along second scan lines, wherein first scan lines within the first partial area cross-section in the boundary region, in particular at the boundary, run in the same direction as second scan lines within the second partial area cross-section.
[0042] The locations within an object's cross-section are normally solidified by moving at least one energy beam bundle over the build-up material in essentially parallel, preferably parallel, scanning lines. The scan lines are spaced apart so that the build-up material is solidified as homogeneously as possible in the area scanned by the scan lines. A distance between two adjacent scan lines is defined, for example, as the distance between the line centers in a direction perpendicular to the line path. To ensure that there are as few jumps in the material properties or mechanical parameters of the solidified object at the boundary between the two sub-areas as possible, the direction in which the scan lines run is maintained at the boundary or in the boundary region in the procedure just described, i.e. it is not changed.Preferably, this applies not just to one scan line, but to all scan lines that intersect the boundary. In the context of this application, "direction" refers to the position within the plane of the object's cross-section, not the direction of movement of the energy beam along a scan line. It should be noted here that, for the sake of clarity, those scan lines located in the first partial cross-section are referred to as first scan lines, and those scan lines located in the second partial cross-section are referred to as second scan lines, regardless of changes in the direction of the scan lines or changes in an energy input parameter during the movement of the impact area of the energy beam along the scan line, i.e., along the specified scanning path.
[0043] Alternatively, the at least one energy beam scans the build-up material in the first partial area cross-section along first scan lines and scans the build-up material in the second partial area cross-section along second scan lines, wherein the first scan lines and the second scan lines in the boundary region, in particular at the boundary, have an angle to one another that is different from 0°.
[0044] When scanning areas of an object's cross-section along scan lines, in practice, the same amount of energy per unit area is sometimes not applied at all points along a scan line. Rather, the amount of energy applied per unit area also depends on the shape of the respective sub-area. There may also be preferred scan line directions depending on the shape of an area.
[0045] In particular, the first scan lines and second scan lines in the boundary region, in particular at the boundary, may have an angle to each other that is less than 30°, preferably less than 10°, even more preferably less than 1°.
[0046] In order to achieve the greatest possible homogeneity at the boundaries between sub-areas, there is preferably a maximum angle between the directions of the first scan lines in the first sub-area cross-section and the second scan lines in the second sub-area cross-section.
[0047] In particular, the directions of the first scan lines and / or the second scan lines may gradually change within the boundary region.
[0048] In order to achieve the most homogeneous solidification of the material during the transition from the first sub-area to the second sub-area, it is advantageous if the direction in which an energy beam is moved along a first scan line in the first sub-area cross-section is successively changed, so that the energy beam is moved in the second sub-area cross-section along a second scan line with a different direction. In other words, the direction in which an energy beam is moved changes successively when the energy beam is moved from the first sub-area cross-section to the second sub-area cross-section. On the one hand, it is conceivable that a two-, three-, or multiple-time change in the direction of movement of the energy beam occurs in the boundary region. However, it is also conceivable that the direction of movement of the energy beam changes almost continuously, i.e.in many steps and therefore almost continuously, within the boundary region. This makes it possible for an energy beam to be moved along first scan lines within the first partial cross-section, along second scan lines within the second partial cross-section, and gradually change the direction of the scan lines during the transition from the first to the second partial cross-section in the boundary region. By avoiding an abrupt change in the direction of movement of the energy beam, a more homogeneous solidification of the build-up material within the boundary region is ensured. Furthermore, such an approach can also result in a speed or time gain when using energy input devices where, due to the mechanical inertia of the beam deflection device, abrupt changes in direction are only possible by means of time-consuming braking and acceleration.Again, the described procedure is preferably followed for all first scan lines in the first partial area cross-section which intersect the boundary.
[0049] In particular, the at least one energy beam can scan the build material in the first partial area cross-section along first scan lines and scan the build material in the second partial area cross-section along second scan lines, wherein within the boundary region, in particular directly at the boundary, an offset of first and / or second scan lines takes place by an amount which is less than half the distance between the first scan lines or second scan lines.
[0050] Especially when the scan line spacing between the first scan lines in the first partial area cross-section is different from the scan line spacing between the second scan lines in the second partial area cross-section, it can happen that a first and a second scan line meet exactly at the boundary, but the first and second scan lines adjacent to them do not meet at the boundary. Likewise, if the scan line spacings in the first partial area cross-section and in the second partial area cross-section are the same, but the directions of the first scan lines in the first partial area cross-section are different from the directions of the second scan lines in the second partial area cross-section, it can happen that not all scan line pairs from the first scan line and the second scan line intersect at the boundary or in the boundary region. This then results inwithin the boundary region, an offset of first and second scan lines, which means the distance between the intersection point of a first scan line with the boundary and the intersection point of a second scan line with the boundary or with an edge of the boundary region. An intersection point of a scan line with the boundary is, for example, the point at which the center of the scan line intersects the boundary in a direction perpendicular to the line path of the scan line. For sufficient homogeneity during the solidification of the build-up material, however, it is sufficient if such an offset of a first scan line compared to a second scan line is less than half the distance between the first or second scan lines. A scan line spacing is defined here as the distance between the line centers of two adjacent scan lines in a direction perpendicular to the direction of the two scan lines.Although in some cases it may be sufficient if sufficient homogeneity in the solidification is ensured only locally at the boundary between the first sub-area cross-section and the second sub-area cross-section, it is nevertheless advantageous if the above condition applies to all first and second scan lines whose direction of travel has an intersection with the boundary.
[0051] In particular, the at least one energy beam bundle can scan the build material in the first partial area cross-section along first scan lines and scan the build material in the second partial area cross-section along second scan lines, wherein the distance between first scan lines in the first partial area cross-section is equal to the distance between second scan lines in the second partial area cross-section.
[0052] Again, with a view to achieving the most homogeneous hardening possible, the same scan line density is selected for the second sub-area cross-section as for the first sub-area cross-section. If the first and second scan lines are parallel to each other, this is easily achieved. In other cases, for example, by gradually changing the scan line directions in the boundary region, an equal scan line spacing can be ensured in the first sub-area cross-section and the second sub-area cross-section.
[0053] Optionally, the distance between the first scan lines in the first partial area cross-section can be different from the distance between the second scan lines in the second partial area cross-section. This preferably applies to all scan lines in the first and second partial area cross-section that intersect the boundary. In particular, the build-up material in the second partial area cross-section can be specifically consolidated with a different scan line spacing. This can be motivated, for example, by the fact that different values of energy input parameters are desired in the second partial area cross-section.
[0054] In an additive manufacturing method according to the invention for producing a three-dimensional object, wherein the object is produced by applying a building material layer upon layer and solidifying the building material by supplying radiant energy to locations in each layer that are associated with the cross-section of the object in this layer, by scanning these locations with at least one energy beam according to a set of energy input parameters to introduce energy into the building material, the sequence of the additive manufacturing method is controlled by a control data set that was generated using a method according to the invention for providing control data.
[0055] If control data provided according to the invention are used in a control data set that was generated for the control of an additive manufacturing process, in particular the control of a layer-by-layer additive manufacturing process, such as a layer-by-layer powder melting or sintering process, such as SLS or DMLS, then objects with the most homogeneous properties possible, ie without local jumps in property parameters of the object, such as elongation at break, surface roughness, color, etc., can be produced.
[0056] A device according to the invention for providing control data for an additive manufacturing device for producing a three-dimensional object, wherein the object is produced by means of the additive manufacturing device by applying a building material layer upon layer and solidifying the building material by supplying radiant energy to locations in each layer that are associated with the cross-section of the object in this layer, by an energy input device scanning these locations for introducing energy into the building material with at least one energy beam according to a set of energy input parameters, comprises: a data access unit designed to access computer-based model data of at least one section of the object to be produced, a segmentation unit designed to define a first sub-area and a second sub-area within the at least one object section, which adjoin one another at a boundary, a data model generation unit designed to generate at least one data model of a region of a building material layer to be selectively solidified for producing the at least one object section, in which a first sub-area cross-section intersects the first sub-area and a second sub-area cross-section intersects the second sub-area, wherein the data model specifies,that in the first partial area cross-section at least one energy input parameter has on average a different value than in the second partial area cross-section and during the introduction of energy into the building material by the at least one energy beam, the at least one energy beam is moved several times across the boundary, and a control data provision unit which is designed to provide control data corresponding to the at least one data model generated by the data model generation unit for the generation of a control data set for the additive manufacturing device, wherein in the third step data models of n+1 consecutive building material layers are generated, where n is a natural number, wherein in the data models of n consecutive building material layers a scanning of the building material with the at least one energy beam only in the first partial area cross-section,but not specified in the second partial area cross-section and in the data model of the subsequent n+1 -th building material layer a sampling of the building material in the first partial area cross-section and in the second partial area cross-section is specified, wherein in the third step the value of at least one energy input parameter is changed within a boundary region, which is a region in the building material layer described by the data model on at least one side of the boundary, in which the locations to be solidified have a maximum distance of 2000 µm, more preferably 1500 µm, even more preferably 1000 µm, even more preferably 100 µm, most preferably 50 µm from the boundary.
[0057] The provision of the data model generated in the third step for generating a control data set can be done by the control data provision unit itself by integrating the generated data model into a control data set for the additive manufacturing device. However, provision also includes forwarding the data model to a data processing device, which integrates the data model into a control data set, or forwarding it directly to an additive manufacturing device. In particular, it is possible to dynamically provide data models for object cross-sections yet to be manufactured in the additive manufacturing device during a manufacturing process. In particular, data models generated in the third step do not have to be provided individually for an additive manufacturing process.Rather, several generated data models can first be collected and then made available in their entirety for integration into a tax data set.
[0058] A computer program according to the invention has program code means for executing all steps of a method according to a method according to the invention for providing control data when the computer program is executed by means of a data processor, in particular a data processor cooperating with an additive manufacturing device.
[0059] "Interaction" here means that the data processor is either integrated into the additive manufacturing device or can exchange data with it. Implementing the inventive method for providing control data and the associated device using software enables easy installation on various IT systems at different locations (for example, at the creator of the object's design or at the operator of the additive manufacturing device).
[0060] An additive manufacturing device according to the invention for producing a three-dimensional object, wherein in the additive manufacturing device the object is produced by applying a building material layer upon layer and solidifying the building material by supplying radiant energy to locations in each layer that are associated with the cross-section of the object in this layer, by scanning these locations for introducing energy into the building material with at least one energy beam according to a set of energy introduction parameters, comprises: a layer application device suitable for applying a layer of a building material to an already existing, preferably already selectively solidified, building material layer, an energy input device suitable for scanning the locations assigned to the cross-section of the object in a layer with at least one energy beam, and a control unit configured to execute a computer program according to the invention for controlling the production of the object.
[0061] Further features and advantages of the invention will become apparent from the description of embodiments with reference to the accompanying figures. Fig. 1 shows a schematic, partially sectioned view of an exemplary device for the generative production of a three-dimensional object according to an embodiment of the invention, Fig. 2 shows schematically an exemplary decomposition of an object to be manufactured into sub-areas according to the invention, Fig. 3 shows schematically a horizontal section through the Fig. 2 depicted object, Fig. 4 shows schematically a horizontal section similar to Fig. 3 to illustrate an alternative approach, Fig. 5 shows schematically a horizontal section similar to Fig. 3 to illustrate a variant of the inventive procedure, Fig. 6 bis 8 schematically show different possible procedures in the case that scan lines in a first and second partial area cross-section run in different directions, Fig. 9 shows schematically the procedure for a scan line offset, Fig. 10 illustrates the process of providing tax data, Fig. 11 shows the schematic structure of a device for providing control data, Fig. 12 shows an exemplary procedure for avoiding a sudden scan line offset directly at the border and Fig. 13 shows a specific embodiment of the invention.
[0062] For a description of the invention, an additive manufacturing device according to the invention will first be described below using the example of a laser sintering or melting device with reference to Fig. 1 be described.
[0063] For constructing an object 2, the laser sintering or laser melting device 1 contains a process chamber or build chamber 3 with a chamber wall 4. Arranged within the process chamber 3 is a build container 5 open at the top and with a container wall 6. A work plane 7 is defined by the upper opening of the build container 5, with the area of the work plane 7 located within the opening, which can be used to construct the object 2, being referred to as the build field 8.
[0064] Arranged within the construction container 5 is a carrier 10 movable in a vertical direction V, to which a base plate 11 is attached, which closes off the container 5 at the bottom and thus forms its base. The base plate 11 can be a plate formed separately from the carrier 10 and fastened to the carrier 10, or it can be formed integrally with the carrier 10. Depending on the powder and process used, a construction platform 12 can also be attached to the base plate 11 as a construction base, on which the object 2 is built. However, the object 2 can also be built on the base plate 11 itself, which then serves as the construction base. Fig. 1 the object 2 to be formed in the container 5 on the construction platform 12 is shown below the working level 7 in an intermediate state with several solidified layers, surrounded by unsolidified building material 13.
[0065] The laser sintering or melting device 1 further includes a reservoir 14 for a build material 15, in this example a powder that can be solidified by electromagnetic radiation, and a coater 16 movable in a horizontal direction H for applying the build material 15 within the build field 8. Optionally, a heating device, e.g., a radiant heater 17, can be arranged in the process chamber 3. An infrared radiator, for example, can be provided as the radiant heater 17.
[0066] The exemplary additive manufacturing device 1 further includes an energy input device 20 with a laser 21, which generates a laser beam 22, which is deflected via a deflection device 23 and is focused onto the working plane 7 by a focusing device 24 via a coupling window 25, which is attached to the top of the process chamber 3 in the chamber wall 4.
[0067] In laser sintering or laser melting, an energy input device can comprise, for example, one or more gas or solid-state lasers or any other type of laser such as laser diodes, in particular VCSEL (Vertical Cavity Surface Emitting Laser) or VECSEL (Vertical External Cavity Surface Emitting Laser), or a row of these lasers. Fig. 1 The specific structure of a laser sintering or melting device shown is therefore only exemplary for the present invention and can, of course, also be modified, particularly when using a different energy input device than the one shown. To emphasize that the shape of the radiation impact area on the construction material is not necessarily approximately point-shaped, but can also be planar, the term "beam bundle" is often used in this application as a synonym for "beam."
[0068] The laser sintering device 1 further includes a control device 29, via which the individual components of the device 1 are controlled in a coordinated manner to carry out the construction process. Alternatively, the control device can also be mounted partially or entirely outside the additive manufacturing device. The control device can include a CPU whose operation is controlled by a computer program (software). The computer program can be stored separately from the additive manufacturing device in a storage device, from where it can be loaded (e.g., via a network) into the additive manufacturing device, in particular into the control device.
[0069] During operation, the control device 29 lowers the carrier 10 layer by layer, controls the coater 16 to apply a new powder layer, and controls the deflection device 23 and, if appropriate, also the laser 21 and / or the focusing device 24 to solidify the respective layer at the locations corresponding to the respective object by means of the laser by scanning these locations with the laser.
[0070] All statements made below apply not only to laser sintering or melting devices, but also to other types of generative layer building devices in which thermal energy is introduced into the build-up material in the form of radiation.
[0071] In the generative layered construction device just described as an example, a manufacturing process takes place in such a way that the control unit 29 processes a control data set (often also referred to as a control command set).
[0072] The control data set specifies to an energy input device, in the case of the above laser sintering or laser melting device specifically the deflection device 23, at each point in time during the solidification process the point on the working plane 7 to which energy radiation is to be directed. Of course, in practice, the deflection device 23 will exhibit inertia, so that if the point of impact or area of the laser beam 22 on the working plane 7 is changed by means of the deflection device 23, the point of impact or area cannot be moved across the working plane 7 at an arbitrarily high speed. Even if, for example, due to the inertia of the deflection device 23, the point of impact of the laser beam 22 cannot be moved across the working plane 7 with arbitrarily small curve radii, this has no impact on the idea of the present invention. The invention aims to modify the control data.Measures that are additionally necessary due to the inertia of, for example, a beam deflection device can be taken independently of the procedure according to the present invention.
[0073] As in Fig. 11 As shown, a device 100 for providing control data for an additive manufacturing device includes a data access unit 101, a segmentation unit 102, a data model generation unit 103 and a control data provision unit 104. The operation of the device 100 for providing control data is explained with reference to Fig. 10 described.
[0074] In the Fig. 11 In the device 100 shown for providing control data for an additive manufacturing device, the data access unit 101 first accesses a number, i.e. one or more, of layer data sets, each of which has a data model of a region of a building material layer to be selectively solidified during production, preferably of the entire region of a building material layer to be solidified, which corresponds to a cross-section of an object section. In the device shown in Fig. 10 In the process sequence shown, this is the first step S1.
[0075] In a Fig. 10 In the second step S2 shown, the segmentation unit 102 determines subregions of an object or object section for which different values of at least one energy input parameter are specified during the solidification of the construction material. In Fig. 2 A schematic representation of a decomposition of the object 2 to be manufactured into a first sub-area 51 and a second sub-area 52 is shown. The reason for selecting different energy input parameters in different sub-areas can be due, for example, to the geometry of the sub-areas or to changed build material parameters at different locations on the build field 7. In this exemplary embodiment, it is assumed that the information about the energy input parameters is already present in the layer data sets accessed by the data access unit 101.
[0076] In the Fig. 10 In the third step S3 shown, the data model generation unit 103 now specifies in at least one data model, in which at least one first partial area cross-section 51a and a second partial area cross-section 52a, which adjoin one another, are present, how at least one energy beam is to be moved across the two partial area cross-sections 51a and 52a. In other words, a temporal sequence for scanning the individual locations of the first partial area cross-section 51a and the second partial area cross-section 52a with energy radiation is determined. Here, it is specified that an energy beam does not reverse its direction of movement at the boundary 55 between the first partial area cross-section 51a and the second partial area cross-section 52a, but is moved across the boundary 55 in one go while energy radiation is being supplied to the building material. The procedure is exemplified in Fig. 3 shown.
[0077] Fig. 3 shows schematically a horizontal section through the Fig. 2 object shown. Accordingly, one sees in Fig. 3 a plan view of a first partial area cross-section 51a and a second partial area cross-section 52a, which have a rectangular shape and adjoin one another at a boundary 55. Furthermore, scan lines 81 can be seen in the first partial area cross-section 51a and scan lines 82 in the second partial area cross-section 52a. The scan lines are paths along which the impact area of an energy beam on a building material layer is moved across the layer. The arrows in Fig. 3 indicate the direction of movement of the energy beam, whereby in the example it is assumed that the same energy beam is used for solidification for the first partial area cross-section 51a as for the second partial area cross-section 52a, which, however, does not necessarily have to be the case. In this case, a first scan line 81 merges seamlessly into a second scan line 82. The distinction between first scan lines 81 and second scan lines 82 is made here only to emphasize in which of the two partial area cross-sections 51a and 52a the impact area of the energy beam is located. If it is assumed that the impact area of the energy beam has a certain extent, it can be specified, for example, that the impact area of the energy beam is located in that partial area cross-section in which the larger area portion of the impact area lies at a certain point in time.
[0078] Since at least one energy input parameter is specified differently in the two partial area cross-sections 51a and 52a, the data model generation unit 103 specifies a modification of this at least one energy input parameter, for example the laser power, when crossing the boundary 55.
[0079] The modification can take place directly at the boundary 55, i.e. while the impact area of the energy beam is moved across the boundary 55. However, it will usually be sufficient if energy input parameters are within a region close to the boundary, i.e. a boundary region 57, as shown in Fig. 4 The width of this boundary region 57, i.e. the maximum distance between the edges 571 and 572 of the boundary region 57 perpendicular to the boundary 55, depends on the size of the partial cross-sections 51a and 52a and on the type of changing energy input parameter. The layer thickness and the type of build-up material also play a role. A practical guideline for the maximum distance is 1000 µm. In some cases, however, a smaller maximum distance of just 100 µm may be appropriate, while there may also be cases in which the maximum distance can have a value of up to 10,000 µm.
[0080] In order to achieve the most homogeneous solidification of the build-up material during the transition from the first sub-area 51 to the second sub-area 52, it is advisable to change changing energy input parameters gradually rather than abruptly during the transition from one sub-area to the other. Such a gradual change can be achieved by changing an energy input parameter in at least two discrete steps or by changing it almost continuously in a large number of steps. Of course, a completely continuous change is desirable. In practice, however, due to the inertia or reaction time of the mechanical and electrical components of the energy input device, there will always be discrete minimum time steps within which a change can take place.
[0081] Fig. 5 shows a more detailed illustration of the procedure just described. Fig. 5 represents an excerpt from Fig. 4 in which a region within the border region 57 is shown enlarged. In Fig. 5 For the sake of a more intuitive representation, the values of an energy input parameter that is modified are denoted by E1, E1', E1", E1‴, E2‴, E2", E2', and E2. Outside the boundary region, the energy input parameter has the value E1 in the first sub-area cross-section 51a and the value E2 in the second sub-area cross-section 52a. Within the boundary region, which is horizontally limited by the edges 571 and 572 in the figure, the value of the energy input parameter is changed in steps, whereby at the transition from E1 to E1', E1' to E1", E1" to E1‴, E1‴ to E2‴, E2‴ to E2", E2" to E2' and E2' to E2, the value of the energy input parameter approaches the value E2. In the Fig. 5 The scan lines pointing from right to left represent a gradual transition from the value E2 of the energy input parameter to the value E1 of the energy input parameter. However, for the sake of clarity, a detailed illustration of the respective energy input parameter values for the scan lines running from right to left has been omitted.
[0082] One recognizes in Fig. 5 Dashed lines parallel to the edges 571 and 572 of the boundary region serve to illustrate a specific embodiment of the invention. In this specific embodiment of the invention, two subregions 51 and 52, in which the value of at least one energy input parameter is different, are not arranged directly next to each other, but rather, additional intermediate subregion cross-sections are introduced into the respective cross-sections. Fig. 5 These are the intermediate sub-area cross-sections 51a', 51a", 51a‴, 52a‴, 52a" and 52a'. If one again assumes that an energy input parameter in the sub-area cross-section 51a has the value E1 and in the sub-area cross-section 52a has the value E2, then intermediate values between E1 and E2 can be assigned to these energy input parameters in the intermediate sub-area cross-sections. As a result, the value of the energy input parameter is then changed when the energy beam moves across a boundary between two (intermediate) sub-area cross-sections, for example when the energy beam moves across the dashed boundary between the intermediate sub-area cross-sections 51a" and 51a‴ from the value E1" to the value E1‴.Of course, not only can intermediate sub-area cross-sections be defined with respect to a cross-section, but in step S2 the segmentation unit 102 can define intermediate sub-areas in order to ensure a smoother transition between the first sub-area 51a and the second sub-area 52a.
[0083] While in the examples of Figuren 3 bis 5 the first scan lines 81 and the second scan lines 82 run in the same direction, Fig. 6 An example in which, in the two partial area cross-sections 51a and 52a, the scan lines in the first partial area cross-section 51a run in a different direction than in the second partial area cross-section 52a. To account for this circumstance, a change in the direction of movement of the energy beam occurs when the impact area of an energy beam crosses the boundary 55. The change in direction can occur during the energy input into the building material by the energy beam, i.e., without interrupting the movement of the energy beam across the building material layer.
[0084] Especially with a curved boundary 55, it can sometimes be difficult to change the direction of movement of the scan line(s) without having to accept fluctuations in the mutual distance between the scan lines (hatch distance). Especially in such a case, it is advisable to change the direction of the scan lines not directly at the boundary 55, but in a boundary region 57, as already described in connection with the examples of Fig. 4 and 5 introduced. Fig. 7 shows an example of such an approach.
[0085] To ensure the most homogeneous solidification of the build-up material, it is advantageous to change the direction of the scan lines gradually rather than abruptly. This can be done in at least two discrete steps within a boundary region, and in particular in a large number of small steps to achieve a continuous change in the direction of movement. Fig. 8 shows here, as an example, a two-fold change in the direction of the scan lines. In this case, a change of direction occurs within the boundary region 57 between the boundary region edge 571 and the boundary 55, and a change of direction occurs between the boundary region edge 572 and the boundary 55. The first scan lines 81 in the first partial area cross-section 51a have a distance of d outside the boundary region 57, and the second scan lines 82 in the second partial area cross-section 52a have a distance of d outside the boundary region 57. The scan line distance between the two changes of direction in the boundary region 57 is d'. Changing the direction of the scan lines in several steps also has the particular advantage that the angle by which the direction of movement changes is small and does not exceed a predetermined maximum value, for example, 30°, 10°, 5°, or 1°. In particular, such a maximum angle can be predetermined by the inertia of the deflection device 23.
[0086] If the direction of movement of the energy beam changes, the mutual distance between adjacent, parallel scan lines also changes for geometric reasons, as can be seen in Fig. 6 detects where the scan line spacing d in the first partial area cross-section (51a) is different from the scan line spacing d' in the second partial area cross-section (52a). When an energy beam is moved across a boundary 55 between a first partial area cross-section 51a and a second partial area cross-section 52a, a scan line offset at the boundary should preferably not exceed a predetermined maximum value. The situation is described in Fig. 9 For simplicity, Fig. 9 The first scan lines 81 are parallel to the second scan lines 82. It can be seen that the scan line spacing d between the scan lines 81 is equal to the scan line spacing between the second scan lines 82, and a scan line offset x is present directly at the boundary 55. Preferably, the maximum offset of scan lines should be less than half the distance between the first scan lines or the second scan lines. In particular, the maximum offset can be selected taking into account the inertia of the beam deflection device.
[0087] In the Fig. 12 In the example shown, a sudden scan line offset directly at the boundary 55 is avoided by gradually, ie in several steps, a scan line offset within the boundary region 57. In Fig. 12 The position of the scan lines in the vertical direction in the drawing plane is continuously changed.
[0088] In the following, an embodiment is described in which the advantages of the inventive approach become particularly clear. Fig. 13 The upper half shows a horizontal cross-section through a cylindrical object 2 to be manufactured, which has two cylindrical recesses 2a and 2b. In such an object 2, the walls of the cylindrical recesses must be manufactured with particular precision, since reworking these walls after completion of the object 2 is difficult. Since the rest of the object does not need to be manufactured with such high precision, in order to provide control data for the additive manufacturing device, a CAD model of the object 2 is first divided into a first sub-region 511, which has the wall of the cylindrical recess 2a, a second sub-region 512, which has the wall of the cylindrical recess 2b, and a third sub-region 513, which has the remainder of the object 2. In Fig. 13 The decomposition is reflected in the sub-area cross-sections 511a, 512a and 513a.
[0089] In sub-areas 511 and 512, a layer thickness of, for example, 20 µm is specified for the build material layers to achieve high precision, whereas in sub-area 513, which does not need to be manufactured with such high precision, a layer thickness of, for example, 40 µm is specified. For the production of object 2, this means that the build material layers are applied with the lower layer thickness of 20 µm. In sub-areas 511 and 512, the build material is solidified after each layer application, but in sub-area 513, only after every second layer application. In sub-area 513, sufficient energy must be introduced into the build material during solidification so that the build material of two layers of 20 µm each is solidified during scanning.
[0090] For the provision of control data, this means that in the data models of half of the layer data sets, hardening is only specified in sub-areas 511 and 512, but not in sub-area 513. In the data models of the other half of layer data sets, hardening is specified in all sub-areas 511, 512 and 513, but in sub-area 513 with an average different energy input per unit area than in sub-areas 511 and 512. In those data models in which hardening is specified in all sub-areas 511, 512 and 513, it is specified that when the boundary 55 between sub-areas 511 and 513 or 512 and 513 is crossed with the energy beam, e.g. B. a laser, the energy to be applied per unit area is changed in order to meet the requirements in the other sub-area.Nevertheless, when crossing the boundary, there is essentially no interruption in the energy supply from the energy beam to the build-up material. To illustrate the process, the lower half of . Fig. 13 an enlarged view of the square section of the upper half of Fig. 13 shown object cross-section.
[0091] In the case of Figur 13 The hatched lines represent the scan lines when scanning the object cross-section. It can be seen that, for example, the scan line that intersects the boundary 55 at the cross markings is traversed in one pass, first in the partial area cross-section 513a, then in the partial area cross-section 511a, and then again in the partial area cross-section 513a.
[0092] In the embodiment shown, despite different layer thicknesses in the different sub-areas of the object, it is still possible to ensure the most homogeneous solidification possible at the transition between sub-areas.
[0093] Finally, it should be mentioned that a device 100 according to the invention for providing control data for an additive manufacturing device can be implemented not only solely by software components, but also solely by hardware components or combinations of hardware and software. In particular, interfaces mentioned in the present application do not necessarily have to be designed as hardware components, but can also be implemented as software modules, for example, if the input or output data can be taken over by other components already implemented on the same device, or only need to be transferred to another component via software. Likewise, the interfaces could consist of hardware and software components, such as a standard hardware interface that is specifically configured by software for the specific application.In addition, several interfaces can also be combined into a common interface, for example an input-output interface.
Claims
1. A computer-based method of providing control data for an additive manufacturing apparatus for manufacturing a three-dimensional object, wherein by means of the additive manufacturing apparatus the object is manufactured by applying a building material layer by layer and by solidifying the building material by supplying radiant energy to positions in each layer that are assigned to the cross-section of the object in that layer in that by an energy input unit these positions are scanned with at least one energy beam so that energy is input into the building material according to a set of energy input parameters, wherein the method of providing control data comprises: a first step (S1) of accessing computer-based model data of at least one portion of the object to be manufactured, a second step (S2) of determining a first partial region (51) and a second partial region (52) inside of the at least one object portion, which are abutting each other at a border (55), a third step (S3) of generating at least one data model of a region of a building material layer to be selectively solidified in order to manufacture the at least one object portion, in which a first partial region cross-section (51a) intersects the first partial region (51) and a second partial region cross-section (52a) intersects the second partial region (52), wherein it is specified in the data model that in said first partial region cross-section (51a) at least one energy input parameter on average has a different value than in said second partial region cross-section (52a) and that the at least one energy beam is moved across the border (55) several times while inputting energy into the building material by the at least one energy beam, and a fourth step (S4), in which control data are provided for the generation of a control dataset for the additive manufacturing apparatus, said control data corresponding to the at least one data model generated in the third step (S3), wherein in the third step data models of n+1 consecutive building material layers are generated, n being a natural number, wherein in the data models of n consecutive building material layers a scanning of the building material with the at least one energy beam is specified only in the first partial region cross-section (51a) but not in the second partial region cross-section (52a) and in the data model of the following (n+1)-th building material layer a scanning of the building material in the first partial region cross-section (51a) and in the second partial region cross-section (52a) is specified, wherein in the third step the value of at least one energy input parameter is changed inside of a border region (57), said border region being a region on at least one side of the border (55) in said building material layer described by the data model, the positions to be solidified in said region having a maximum distance of 2000 µm, more preferably 1500 µm, even more preferably 1000 µm, even further preferably 100 µm, most preferably 50 µm, to the border (55).
2. The method of claim 1, wherein in the first step (S1) model data are accessed that comprise a number of layer datasets, wherein each layer dataset comprises a data model of a region of a building material layer to be selectively solidified during the manufacturing, said region corresponding to a cross-section of the object portion.
3. The method of claim 1 or 2, wherein the value of at least one energy input parameter is changed immediately when crossing the border (55).
4. The method of claim 1 or 2, wherein the value of at least one energy input parameter is gradually changed inside of said border region (57).
5. The method of one of claims 1 to 4, wherein the at least one energy beam scans the building material in said first partial region cross-section (51a) along first scan lines (81) and scans the building material in said second partial region cross-section (52a) along second scan lines (82), wherein in said border region (57), in particular at the border (55), first scan lines (81) in the first partial region cross-section (51a) extend in the same direction as second scan lines (82) in the second partial region cross-section (52a).
6. The method of one of claims 1 to 4, wherein the at least one energy beam scans the building material in said first partial region cross-section (51a) along first scan lines (81) and scans the building material in said second partial region cross-section (52a) along second scan lines (82), wherein in said border region, in particular at the border (55), said first scan lines (81) and said second scan lines (82) are at an angle relative to one another that is different from 0°.
7. The method of claim 6, wherein the extension directions of the first scan lines (81) and / or of the second scan lines (82) are gradually changed inside of the border region (57).
8. The method of one of claims 1 to 7, wherein the at least one energy beam scans the building material in said first partial region cross-section (51a) along first scan lines (81) and scans the building material in said second partial region cross-section (52a) along second scan lines (82), wherein in said border region (57), in particular immediately at the border (55), said first scan lines and / or said second scan lines are displaced by an amount that is smaller than half the pitch of the first scan lines (81) or the second scan lines (82).
9. The method of one of claims 1 to 8, wherein the at least one energy beam scans the building material in said first partial region cross-section (51a) along first scan lines (81) and scans the building material in said second partial region cross-section (52a) along second scan lines (82), wherein the pitch of the first scan lines (81) in the first partial region cross-section (51a) equals the pitch of the second scan lines (82) in the second partial region cross-section (52a).
10. An additive manufacturing method of manufacturing a three-dimensional object, wherein the object is manufactured by applying a building material layer by layer and by solidifying the building material by supplying radiant energy to positions in each layer that are assigned to the cross-section of the object in that layer in that these positions are scanned with at least one energy beam so that energy is input into the building material according to a set of energy input parameters, wherein the process of the additive manufacturing method is controlled by a control dataset generated using a method of one of claims 1 to 9.
11. A device of providing control data for an additive manufacturing apparatus for manufacturing a three-dimensional object, wherein the object is manufactured by means of the additive manufacturing apparatus by applying a building material layer by layer and by solidifying the building material by supplying radiant energy to positions in each layer that are assigned to the cross-section of the object in that layer in that by an energy input unit these positions are scanned with at least one energy beam so that energy is input into the building material according to a set of energy input parameters, wherein the device of providing control data comprises: a data access unit (101) configured to access computer-based model data of at least one portion of the object to be manufactured, a segmentation unit (102) configured to determine a first partial region (51) and a second partial region (52) inside of the at least one object portion, which are abutting each other at a border (55), a data model generation unit (103) that is configured to generate at least one data model of a region of a building material layer to be selectively solidified in order to manufacture the at least one object portion, in which a first partial region cross-section (51a) intersects the first partial region (51) and a second partial region cross-section (52a) intersects the second partial region (52), wherein it is specified in the data model that in said first partial region cross-section (51a) at least one energy input parameter on average has a different value than in said second partial region cross-section (52a) and that the at least one energy beam is moved across the border (55) several times while inputting energy into the building material by the at least one energy beam, and a control data provision unit (104) that is configured to provide control data for the generation of a control dataset for the additive manufacturing apparatus, said control data corresponding to the at least one data model generated by the data model generation unit (103), wherein the data model generation unit (103) is configured to generate data models of n+1 consecutive building material layers, n being a natural number, wherein in the data models of n consecutive building material layers a scanning of the building material with the at least one energy beam is specified only in the first partial region cross-section (51a) but not in the second partial region cross-section (52a) and in the data model of the following (n+1)-th building material layer a scanning of the building material in the first partial region cross-section (51a) and in the second partial region cross-section (52a) is specified, wherein the data model generation unit (103) is configured to change the value of at least one energy input parameter inside of a border region (57), said border region being a region on at least one side of the border (55) in said building material layer described by the data model, the positions to be solidified in said region having a maximum distance of 2000 µm, more preferably 1500 µm, even more preferably 1000 µm, even further preferably 100 µm, most preferably 50 µm, to the border (55).
12. A computer program having program code means to perform all steps of a method according to one of claims 1 to 9 when the computer program is executed by a data processor, in particular a data processor interacting with an additive manufacturing apparatus.
13. An additive manufacturing apparatus for manufacturing a three-dimensional object, wherein the object is manufactured in the additive manufacturing apparatus by applying a building material layer by layer and by solidifying the building material by supplying radiant energy to positions in each layer that are assigned to the cross-section of the object in that layer in that these positions are scanned with at least one energy beam so that energy is input into the building material according to a set of energy input parameters, wherein said additive manufacturing apparatus comprises: a layer application unit configured to apply a layer of a building material onto a building material layer that already exists and preferably has already been selectively solidified, an energy input unit configured to scan with at least one energy beam the positions in a layer assigned to the cross-section of the object, and a control unit configured to execute a computer program of claim 12 in order to control the manufacture of the object.