METHOD FOR PRODUCING A HOLLOW CORE FIBER AND FOR PRODUCING A PREFORM FOR A HOLLOW CORE FIBER

DE502019012473D1Active Publication Date: 2024-11-28HERAEUS QUARZGLAS GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502019012473
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-07-17
Publication Date
2024-11-28
Estimated Expiration
2039-07-17

AI Technical Summary

Technical Problem

Antiresonant hollow core fibers have complex internal geometries, making them difficult to produce accurately and reproducibly, especially with conventional 'stack and draw' techniques, which struggle to maintain precise dimensional tolerances and uniform wall thickness of antiresonance elements.

Method used

A positioning template with locking means is used within the cladding tube to accurately position and fix antiresonance element preforms, combined with advanced machining techniques like drilling, milling, and polishing to create a stable and precise preform structure, and a SiO2-based sealing compound for fixation and compaction.

Benefits of technology

This method enables the cost-effective production of antiresonant hollow core fibers with high precision and reproducibility, ensuring exact positioning of antiresonance elements and maintaining low optical attenuation and broad transmission spectra.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Technical background

[0001] The invention relates to a method for producing an anti-resonant hollow core fiber, which has a hollow core extending along a fiber longitudinal axis and a cladding region surrounding the hollow core, which comprises a plurality of anti-resonance elements, with the method steps: (a) Providing a cladding tube having a cladding tube inner bore and a cladding tube longitudinal axis along which a cladding tube wall bounded by an inner side and an outer side extends, (b) Providing a number of anti-resonance element preforms, (c) Arranging the anti-resonance element preforms at desired positions on the inner side of the cladding tube wall to form a primary preform for the hollow core fiber having a hollow core region and a cladding region, and (d) Elongating the primary preform to form the hollow core fiber or further processing the primary preform to form a secondary preform from which the hollow core fiber is drawn, wherein the further processing comprises a single or repeated execution of one or more of the following hot forming processes: (i) Elongation, (ii) Collapse, (iii) Collapse and simultaneous elongation, (iv) Collapsing additional cladding material,(v) Collapse of additional mantle material and subsequent elongation, (vi) Collapse of additional mantle material and simultaneous elongation. ,

[0002] Furthermore, the invention relates to the production of a preform for an anti-resonant hollow core fiber, which has a hollow core extending along a fiber longitudinal axis and a cladding region surrounding the hollow core, which comprises a plurality of anti-resonance elements, with the method steps: (a) Providing a cladding tube having a cladding tube inner bore and a cladding tube longitudinal axis along which a cladding tube wall bounded by an inner side and an outer side extends, (b) Providing a number of anti-resonance element preforms, (c) Arranging the anti-resonance element preforms at desired positions on the inner side of the cladding tube wall to form a primary preform for the hollow core fiber having a hollow core region and a cladding region, and (d) Optionally further processing the primary preform into a secondary preform for the hollow core fiber, wherein the further processing comprises a single or repeated execution of one or more of the following hot forming processes: (i) elongation, (ii) collapse, (iii) collapse and simultaneous elongation, (iv) collapsing additional cladding material, (v) collapsing additional cladding material and subsequent elongation,(vi) Collapse of additional mantle material and simultaneous elongation,

[0003] Conventional single-mode optical fibers made of solid material have a glass core surrounded by a glass cladding region with a lower refractive index. Light transmission is based on total internal reflection between the core and cladding regions. However, the interactions of the guided light with the solid material are associated with increased latency in data transmission and relatively low damage thresholds for high-energy radiation.

[0004] These disadvantages are avoided or reduced by hollow-core fibers, in which the core contains an evacuated cavity filled with gas or liquid. In hollow-core fibers, the interaction of light with the glass is less than in solid-core fibers. The refractive index of the core is lower than that of the cladding, so light transmission by total internal reflection is not possible, and the light would normally escape from the core into the cladding. Depending on the physical mechanism of light transmission, hollow-core fibers are divided into photonic bandgap fibers and antiresonance reflection fibers.

[0005] In "photonic bandgap fibers," the hollow core region is surrounded by a cladding in which small hollow channels are periodically arranged. The periodic structure of the hollow channels in the cladding causes the effect referred to in semiconductor technology as the "photonic bandgap," whereby light of certain wavelength ranges scattered by the cladding structures experiences constructive interference in the central cavity due to Bragg reflection and cannot propagate transversely in the cladding.

[0006] In the design known as "antiresonant hollow-core fibers" (AR-HCF), the hollow core region is surrounded by an inner cladding region in which so-called "antiresonant elements" (or "antiresonant elements"; abbreviated to "AREs") are arranged. The walls of the antiresonant elements, evenly distributed around the hollow core, can act as Fabry-Perot cavities operating in antiresonance, reflecting the incident light and guiding it through the fiber core.

[0007] This fiber technology promises low optical attenuation, a very broad transmission spectrum (including in the UV or IR wavelength range) and low latency in data transmission.

[0008] Potential applications of hollow core fibers are in the field of data transmission, high-performance beam guidance, for example for material processing, modal filtering, nonlinear optics, in particular for supercontinuum generation, from the ultraviolet to the infrared wavelength range. State of the art

[0009] A disadvantage of antiresonant hollow core fibers is that higher order modes are not necessarily suppressed, so that over long transmission lengths they are often not purely single-mode and the quality of the output beam deteriorates.

[0010] In the paper by Francesco Poletti, "Nested antiresonant nodeless hollow core fiber"; Optics Express, Vol. 22, No. 20 (2014); DOI: 10.1364 / OE 22.023807, a fiber design is proposed in which antiresonant elements are not formed as a simple, singular structural element, but are composed of multiple, nested structural elements. The nested antiresonant elements are designed such that higher-order core modes are phase-matched to the cladding modes and are suppressed, but not the fundamental core mode. This ensures the propagation of the fundamental core mode at all times, and the hollow-core fiber can be effectively made single-mode over a limited wavelength range.

[0011] The effective mode suppression depends on the center wavelength of the transmitted light and on structural parameters of the fiber design, such as the radius of the hollow core and the diameter difference of nested ring structures in the antiresonance elements.

[0012] EP 3 136 143 A1 discloses an antiresonant hollow-core fiber (referred to therein as a "hollow-core fiber with no band gap") in which the core can conduct additional modes in addition to the fundamental mode. For this purpose, it is surrounded by an inner cladding with "non-resonant elements" that provide phase matching of antiresonant modes with the higher modes. The hollow-core fiber is manufactured using a so-called "stack-and-draw" technique, in which the starting elements are arranged in an axis-parallel ensemble and fixed to a preform, which is then elongated. A cladding tube with a hexagonal inner cross-section is used, and six so-called "ARE preforms" (anti-resonance element preforms) are fixed in the inner edges of the cladding tube. This preform is drawn into a hollow-core fiber in two stages.

[0013] WO 2018 / 169487 A1 discloses a method for producing a preform for anti-resonant hollow-core fibers, in which a first cladding region comprises a plurality of rods and a second cladding region comprises a plurality of tubes surrounded by an outer cladding tube. The rods, tubes, and cladding tube are assembled using a "stack and draw" technique to form a preform. Before the preform is elongated, the preform end is sealed by applying a sealing compound. A UV adhesive, for example, is used as the sealing compound.

[0014] AF Kosolapov et al.: "Hollow-core revolver fiber with a double-capillary reflective cladding", Quantum Electronics, Vol. 46, No. 3, March 29, 2016 (2016-03-29), Pages 267-270, DOI: 10.1070 / QEL15972, describes a method for fabricating an antiresonant hollow-core fiber by providing a cladding tube and a number of antiresonant element preforms, which are assembled as a double tube consisting of an ARE outer tube and an ARE inner tube welded to its inner wall. The double tube is elongated and then exhibits an oval cross-section. Five of the oval double tubes are mounted on the inside of the cladding tube. A custom-made quartz glass plate with a thickness of 1.27 mm is positioned between each adjacent double tube. The double tubes are then welded to the inside of the cladding tube. The resulting primary preform is elongated into a secondary preform, from which the hollow-core fiber is drawn.

[0015] In US 2005 / 226578 A1, a tubular assembly of tubular and rod-shaped elements is created to manufacture a photonic optical fiber, with the voids between the elements being filled with a filler. The filler is deposited from the gas phase or generated from the liquid phase, for example, using a colloidal sol containing SiO2 particles. The voids are filled with the filler starting from the inner bore of the assembly. The filler serves to secure the elements and can also be used to attach an inner capillary. Technical task

[0016] Antiresonant hollow-core fibers, especially those with nested structural elements, have complex internal geometries, making their precise and reproducible manufacturing difficult. This is all the more true because, in order to maintain resonance or antiresonance conditions, even small dimensional deviations on the order of magnitude of the operating wavelength of the guided light are intolerable. Deviations from the target geometry can be caused by the configuration of the fiber preform, and they can also occur due to unintentional off-scale deformations during the fiber drawing process.

[0017] With the well-known "stack-and-draw" technique, many elements must be assembled with precise positioning. For example, to produce the hollow-core fiber in the "NANF" design known from the paper mentioned above, six antiresonance element preforms, each consisting of an ARE outer tube and an ARE inner tube welded to one side of the ARE outer tube's inner surface, must be attached to the inside of a cladding tube.

[0018] To achieve low attenuation values ​​and wide transmission ranges, in addition to a uniform wall thickness of the antiresonance elements, the azimuthal positioning of the antiresonance elements within the cladding tube is also important. This cannot be easily achieved using the "stack-and-draw" technique. The aim of the invention is to provide a method for the cost-effective production of an antiresonant hollow-core fiber that avoids the limitations of conventional manufacturing processes.

[0019] In particular, it is an object of the invention to provide a method for producing an antiresonant hollow core fiber and a preform for antiresonant hollow core fibers, with which a high precision of the structural elements and an exact positioning of the antiresonant elements in the fiber can be achieved in a sufficiently stable and reproducible manner.

[0020] In addition, disadvantages of the classic "stack and draw" technique, with which the required structural accuracies, in particular a uniform wall thickness of the anti-resonance elements and exact positioning at specified azimuthal positions, are not easy to achieve, should be avoided as far as possible. Summary of the invention

[0021] With regard to the method for producing the anti-resonant hollow core fiber, this object is achieved according to the invention, starting from a method of the type mentioned at the outset, in that for arranging the anti-resonance element preforms according to method step (c) a positioning template is inserted into the cladding tube inner bore, which has holding elements for positioning the anti-resonance element preforms at the desired positions, and in that the positioning template has at least one locking means which interacts with a locking means counterpart in the cladding tube wall to form a force-fitting and / or form-fitting connection.

[0022] The starting point for the production of the antiresonant hollow-core fiber is a preform, also referred to here as a "cane" or "primary preform." It comprises a cladding tube in which or on which precursors or preforms for forming antiresonant elements in the hollow-core fibers (referred to here briefly as "antiresonant elements") are contained. The primary preform can be elongated to form the hollow-core fiber; however, additional cladding material is usually added to the primary preform to create a preform referred to here as a "secondary preform." If necessary, the hollow-core fiber is created by elongating the secondary preform. Alternatively, the primary preform or the secondary preform are surrounded by one or more overwrapped cylinders to form a coaxial assembly of components, and the coaxial assembly is elongated directly to form the hollow-core fiber.The general term "preform" is understood here to refer to the component or coaxial ensemble of components from which the hollow core fiber is ultimately drawn.

[0023] The addition of sheath material is achieved, for example, by collapsing a casing cylinder onto the primary preform. The coaxial arrangement of primary preform and casing cylinder is either elongated or not elongated when the casing cylinder collapses. In this process, the shape or arrangement of the antiresonance element preforms is either changed or not changed.

[0024] The accuracy of positioning the preforms on the inner surface of the cladding tube is improved by using a positioning template to arrange the anti-resonance element preforms.

[0025] To fix the positioning template to the cladding tube, it has at least one locking means which interacts with a locking means counterpart in the cladding tube wall to form a force-locking and / or form-locking connection.

[0026] The locking means and the counterpart are, for example, a system of hook / eyelet, spring / groove or the like, preferably a plug connection which is as easy as possible to attach to the cladding tube wall or to insert into the cladding tube wall.

[0027] For example, it has proven advantageous if the locking means counterpart is arranged in the front side of the cladding tube wall and the locking means can be completely retracted therein.

[0028] The end face of the cladding tube thus retains its flatness, which facilitates the connection to other components, such as the adhesive connection to a tubular holder.

[0029] It is advantageous if the locking element counterpart does not reach the outside of the cladding tube and does not break through it.

[0030] The positioning template has, for example, a shaft projecting into the inner bore of the cladding tube, which is provided with holding elements in the form of several radially outward-pointing holding arms.

[0031] The design-specific star-shaped arrangement of the holding elements facilitates the exact positioning of the anti-resonance element preforms at the respective target positions and their fixation.

[0032] In a preferred procedure, the anti-resonance element preforms are tubular with a tubular outer surface, wherein each holding element has at least two contact points with the tubular outer surface of the anti-resonance element preform to be held.

[0033] Two contact points are sufficient for a defined and stable positioning of the anti-resonance element preform, so that any deflection of the anti-resonance element preform during fixation to the inner surface can be prevented.

[0034] The positioning template is preferably used exclusively in the area of ​​the cladding tube end faces, preferably in the area of ​​both cladding tube end faces.

[0035] This limits the surface contact of the positioning template with the anti-resonance element preforms to what is absolutely necessary. Furthermore, the positioning template can remain in the inner bore of the cladding tube during further handling and processing of the primary preform, ensuring the stable position of the anti-resonance element preforms.

[0036] Positioning templates made of graphite or glass, preferably quartz glass, have proven particularly useful.

[0037] Positioning templates made of these materials can be machined with high purity and high accuracy, with a dimensional tolerance of less than + / -0.1 mm. They exhibit high temperature stability and are inert to the hollow-core fiber material, especially glass.

[0038] The accuracy of positioning the preforms on the inner surface of the cladding tube is improved by machining the inner surface of the cladding tube, in particular by drilling, milling, grinding, honing and / or polishing.

[0039] Compared to other known forming techniques using heat and pressure, these processing techniques produce more precise and delicate structures and avoid surface contamination by forming tools such as nozzles, presses or melt molds.

[0040] The machining preferably also includes structuring the cladding tube interior in the region of the target positions of the anti-resonance element preforms by providing them with a longitudinal structure extending in the direction of the cladding tube's longitudinal axis. This longitudinal structure comprises, for example, longitudinal slots and / or longitudinal grooves in the cladding tube's interior wall, which run parallel to the cladding tube's longitudinal axis and are preferably created by drilling, sawing, milling, cutting, or grinding.

[0041] The longitudinal structure extending along the cladding tube's longitudinal axis serves as a positioning aid for the anti-resonance element preforms. It facilitates the anti-resonance element preforms' adoption of predefined positions on the inside of the cladding tube.

[0042] Particularly in the case of continuous longitudinal slots, it is advantageous if the cladding tube has front ends, with the longitudinal slots ending before the front ends. Longitudinal grooves that do not penetrate the cladding tube wall, on the other hand, preferably extend to the front ends.

[0043] In a preferred method variant, the longitudinal structure has longitudinal slots distributed around the circumference of the cladding tube wall, wherein the anti-resonance element preforms are arranged at a longitudinal slot.

[0044] The longitudinal slots penetrate the cladding tube wall from the inside out, with the exception of the two end regions of the cladding tube. They have parallel longitudinal edges and a maximum slot width SB, with the anti-resonance element preforms preferably being connected to the longitudinal edges. The anti-resonance element preforms have a width dimension that is greater than the maximum width Se, so that they do not fully penetrate the longitudinal slots. The area below the longitudinal edges forms a cavity into which a gas can be introduced or from which a gas can be extracted.

[0045] In a preferred process variant, the arrangement of the anti-resonance element preforms at desired positions on the inside of the cladding tube wall and / or the drawing of the hollow core fiber according to process step (c) comprises a fixing measure and / or a sealing measure using a sealing or bonding compound containing amorphous SiO 2 particles.

[0046] The sealing or bonding compound used for sealing or fixing contains amorphous SiO2 particles, which are, for example, suspended in a dispersion liquid. This compound is applied between the surfaces to be bonded or sealed and is usually pasty during use. Upon drying at low temperature, the dispersion liquid is partially or completely removed and the compound solidifies. The sealing or bonding compound, and in particular the solidified SiO2-containing sealing or bonding compound obtained after drying, meets the requirements for fixing and compaction. The temperature required for drying is below 300°C, which promotes compliance with the dimensional stability of the preform and avoids thermal impairments.Heating to higher temperatures around 800 °C, for example, during elongation of the preform into a hollow-core fiber, leads to further thermal strengthening of the sealing or bonding compound, which is also suitable for forming opaque or transparent glass. This occurs through sintering or vitrification, whereby sintering to opaque glass requires comparatively lower temperatures and / or shorter heating times than vitrification to complete transparency. The sealing or bonding compound can thus be fully densified by heating and vitrified by heating during the hot-forming process. The sealing or bonding compound behaves like quartz glass; it becomes viscous and malleable.

[0047] During the hot-forming process, the sealing or bonding compound does not decompose and releases few impurities. It is thus characterized by thermal stability and purity during the hot-forming process and avoids deformation due to different thermal expansion coefficients.

[0048] In a preferred process variant, the arrangement of the anti-resonance element preforms at desired positions on the inside of the cladding tube wall and / or the elongation or further processing of the primary preform according to process step (d) comprises a fixing measure and / or a sealing measure using a sealing or bonding compound containing amorphous SiO 2 particles.

[0049] The sealing or bonding compound used for sealing or fixing contains amorphous SiO2 particles, which are, for example, suspended in a dispersion liquid. This compound is applied between the surfaces to be bonded or sealed and is usually pasty during use. Upon drying at low temperature, the dispersion liquid is partially or completely removed and the compound solidifies. The sealing or bonding compound, and in particular the solidified SiO2-containing sealing or bonding compound obtained after drying, meets the requirements for fixing and compaction. The low temperature required for this, below 300°C, promotes compliance with the dimensional stability of the preform and avoids thermal impairments.By heating to higher temperatures, for example, during the elongation of the preform into a hollow-core fiber, the sealing or bonding compound is also suitable for forming opaque or transparent glass. This is achieved by sintering or vitrification, whereby sintering to opaque glass requires comparatively lower temperatures and / or shorter heating times than vitrification to complete transparency. The sealing or bonding compound can thus be densified by heating and vitrified by heating during the hot-forming process.

[0050] During the hot-forming process, the sealing or bonding compound does not decompose and releases few impurities. It is thus characterized by thermal stability and purity during the hot-forming process and avoids deformation due to different thermal expansion coefficients.

[0051] In particular with regard to low optical attenuation and a large optical transmission bandwidth of the hollow core fiber, it has proven particularly advantageous if the antiresonance element preforms are arranged around the hollow core with an odd symmetry.

[0052] With regard to the production of the preform for the hollow core fiber, the above-mentioned technical problem is solved according to the invention on the basis of a method of the type mentioned at the outset in that the arrangement of the anti-resonance element preform according to method step (c) is carried out by means of a positioning template inserted into the cladding tube inner bore, which has holding elements for positioning the anti-resonance element preforms at the desired positions, and in that the positioning template has at least one locking means which interacts with a locking means counterpart in the cladding tube wall to form a force-fitting and / or form-fitting connection.

[0053] The preform is the starting point for the production of the antiresonant hollow-core fiber. By elongating the primary preform, the antiresonant hollow-core fiber is either drawn directly, or the primary preform is further processed to create another semi-finished product, also referred to here as the "secondary preform," from which the antiresonant hollow-core fiber can be drawn.

[0054] In each case, preform manufacturing involves installing and bonding anti-resonance element preforms to a cladding tube. Preform positioning accuracy is improved by using a positioning template to arrange the anti-resonance element preforms. Further improvement is achieved by pre-structuring the cladding tube.

[0055] Measures for producing the preform are explained above in the context of the production of the hollow core fiber and these explanations are hereby incorporated. Definitions

[0056] Individual process steps and terms from the above description are defined in more detail below. These definitions are part of the description of the invention. In the event of a factual contradiction between one of the following definitions and the rest of the description, the statement in the description shall prevail. Anti-resonance elements

[0057] The antiresonance elements can be simple or nested structural elements of the hollow-core fiber. They have at least two walls that, viewed from the direction of the hollow core, have a negative curvature (convex) or no curvature (flat, straight). They are typically made of a material that is transparent to the working light, for example, glass, particularly doped or undoped SiO2, a plastic, particularly a polymer, a composite material, or a crystalline material. Anti-resonance element preform / anti-resonance element precursor

[0058] Anti-resonance element preforms are components or parts of the preform that essentially become anti-resonance elements in the hollow core fiber through simple elongation during the fiber drawing process. Anti-resonance element precursors are components or parts of the preform that only become anti-resonance element preforms through forming or directly become anti-resonance elements. The anti-resonance element preforms can be simple or nested components, to which additional positioning aids can be attached. They are originally present in the primary preform (cane).

[0059] Further processing of the primary preform, particularly through hot forming steps, can produce intermediate products in which the original anti-resonance element preforms are present in a modified form compared to the original. This modified form is also referred to here as an anti-resonance element preform or anti-resonance element precursor. Preform / primary preform / secondary preform

[0060] The preform is the component from which the antiresonant hollow-core fiber is drawn. It is a primary preform or a secondary preform created by further processing the primary preform. Further processing of the primary preform into a secondary preform from which the hollow-core fiber is drawn may involve a single or repeated execution of one or more of the following hot-forming processes: (i) elongation, (ii) collapse, (iii) collapse and simultaneous elongation, (iv) collapse of additional mantle material, (v) collapse of additional mantle material and subsequent elongation, (vi) collapse of additional mantle material and simultaneous elongation. Elongation / Collapse

[0061] During elongation, the primary preform is elongated. Elongation can occur without simultaneous collapse. Elongation can be performed to scale, so that, for example, the shape and arrangement of components or parts of the primary preform are reflected in the elongated final product. During elongation, the primary preform can also be drawn out of scale, and its geometry can be altered.

[0062] During collapse, an internal bore is narrowed or annular gaps between tubular components are closed or narrowed. Collapse is usually accompanied by elongation. Hollow core / Inner shell area / Outer shell area / Cane

[0063] The assembly consisting of at least one cladding tube and loosely or firmly fixed preforms or precursors for anti-resonance elements is also referred to here as the "primary preform" or "cane." The primary preform (cane) comprises the hollow core and a cladding region. This cladding region is also referred to as the "inner cladding region" if there is also an "outer cladding region," created, for example, by collapsing onto the cane, and if a distinction is to be made between these cladding regions. The terms "inner cladding region" and "outer cladding region" are also used for the corresponding regions in the hollow core fiber or in intermediate products obtained by further processing the primary preform.

[0064] The term "pipe inside" is also used as a synonym for "pipe inner surface," and the term "pipe outside" is also used as a synonym for "pipe outer surface." The term "internal bore" in connection with a pipe does not imply that the internal bore was created by a drilling process. Machining

[0065] This refers to mechanical manufacturing processes for the separation of a workpiece, in particular turning, cutting, drilling, sawing, milling, and grinding. This machining creates a longitudinal structure extending along the longitudinal axis of the cladding tube, which serves as a positioning aid for the anti-resonance element preforms. The longitudinal structure is accessible from the inside of the cladding tube; it can also extend through the entire cladding tube wall to the outside. Particle size and particle size distribution

[0066] The particle size and particle size distribution of the SiO2 particles are characterized using the D50 values. These values ​​are taken from particle size distribution curves, which show the cumulative volume of the SiO2 particles as a function of the particle size. The particle size distributions are often characterized using the respective D10, D50, and D90 values. The D10 value indicates the particle size not reached by 10% of the cumulative volume of the SiO2 particles, and accordingly the D50 and D90 values ​​indicate the particle sizes not reached by 50% and 90% of the cumulative volume of the SiO2 particles, respectively. The particle size distribution is determined by light scattering and laser diffraction spectroscopy according to ISO 13320. Example

[0067] The invention is explained in more detail below with reference to an embodiment and a drawing. In detail, a schematic representation Figure 1 Embodiments of positioning templates in a top view, Figure 2 Process steps for positioning anti-resonance element preforms on the inner surface of a cladding tube using a positioning template, Figure 3 a longitudinal section along the section line S1 through the cladding tube of Figure 2(a) with a groove on the front side to accommodate a positioning template, Figure 4 a longitudinal section along the section line S2 through the cladding tube of Figure 2(b) with inserted positioning template, and Figure 5 Embodiments of cladding tubes with additional longitudinal structures for positioning anti-resonance element preforms.

[0068] Figure 1 and Figure 5 are as such outside the scope of the claims.

[0069] During the production of the hollow core fiber or the preform for the hollow core fiber, a large number of components must be joined together. In addition, it can be helpful to seal existing gaps or channels in the preform during hot forming processes. For joining or sealing, an SiO 2 -based sealing or bonding compound is used, as known from DE 10 2004 054 392 A1. In this process, an aqueous slurry is produced by wet grinding quartz glass grains. This slurry contains amorphous SiO 2 particles with a particle size distribution characterized by a D 50 value of approximately 5 µm and a D 90 value of approximately 23 µm. Additional amorphous SiO 2 grains with an average grain size of approximately 5 µm are mixed into the base slurry. The slip used as a bonding compound has a solids content of 90%, which consists of at least 99.9 wt.% SiO2.

[0070] Figure 1 schematically shows several star-shaped embodiments of the positioning template 1 for use in the method according to the invention. Each positioning template 1 has a central area (shaft 2) from which radially outward-pointing - more or less pronounced - holding arms 3 extend.

[0071] Figure 2 shows process steps for installing the positioning template into a cladding tube 4 and for positioning anti-resonance element preforms 5 using the positioning template 1. The inner and outer surfaces of the cladding tube 4 are machined by grinding, honing, and polishing and brought to their final dimensions. At the same time, the cladding tube interior was structured in the area of ​​the target positions of the anti-resonance element preforms 5, which will be explained in more detail below.

[0072] Figure 2(a) and the corresponding longitudinal section of Figure 3 show that grooves 6 are milled into the end faces of the cladding tube 4, starting from the inner surface. The grooves 6 have a width and a depth of 2 mm each. They do not penetrate the outer surface of the cladding tube 4. They serve to hold the arms 3 of a positioning template 1, which is inserted into the inner bore 9 in the area of ​​the end face of the cladding tube 4. The grooves 6 are adapted to the dimensions of the holding arms 3 and thus act as counter-locking means for the holding arms 3 to be held (spring). This is shown schematically in Figure 2(b) and in the corresponding longitudinal section of Figure 4 shown. The ends of the holding arms 3 are completely received in the grooves 6, so that they do not protrude beyond the end face of the cladding tube and thus do not impair its flatness.

[0073] In Figure 2(c)It is shown that anti-resonance element preforms 5 are positioned between the holding arms 3. The anti-resonance element preforms 5 rest against both the holding arms 3 and the shaft 2, so that they are secured against slipping in both the peripheral and radial directions.

[0074] The anti-resonance element preforms 4 are fixed to the inner wall of the cladding tube 4 using the SiO 2 -based bonding compound described above. The bonding compound is applied locally in the area of ​​the front ends of the anti-resonance element preform 5, and the anti-resonance element preforms are placed thereon using the positioning template 1. The positioning template 1 is limited to the area around the two front ends of the cladding tube.

[0075] This method creates a precise and reproducible connection between the cladding tube 4 and the anti-resonance element preforms 5. For fixation, solidification of the bonding compound at a low temperature below 300 °C is sufficient, thus avoiding excessive heating of the surrounding areas and thus deformation of the anti-resonance element preforms 5.

[0076] The cladding tube 4 is made of quartz glass. It has a length of 500 mm, an outer diameter of 73 mm, and an inner diameter of 24 mm. The assembly 7, consisting of the cladding tube 4 and the antiresonance element preforms 5 positioned within it, is referred to here as the "primary preform" and often also as the "cane."

[0077] Figure 5shows further embodiments of cladding tubes 4 in a view of the cladding tube end face. The cladding tubes 4 each have longitudinal grooves 8 on the inner surface of the cladding tube wall. The longitudinal grooves 8 are evenly distributed around the inner circumference of the respective cladding tube 4 in sixfold symmetry. They serve as additional positioning aids for the anti-resonance element preforms 5.

[0078] Figure 5(a) shows flat, wide, bowl-shaped longitudinal grooves 8 in cross-section, which are produced by milling. Figure 5(b) shows flat, narrow and in cross-section semicircular longitudinal grooves 8, which are also produced by milling. Figure 5(c) shows deep, narrow, and in cross-section almost closed circular longitudinal grooves 8, created by drilling. The maximum depth is 3 mm and the inner diameter is 4 mm.

[0079] To produce the antiresonant hollow core fiber, the primary preform 7 is over-cased with an over-case cylinder to add additional cladding material and to adjust the core-cladding diameter ratio specified for the hollow core fiber in the final, secondary preform.

Claims

1. A method for producing an anti-resonant hollow-core fiber which comprises a hollow core extending along a longitudinal axis of the fiber and an inner casing region that surrounds the hollow core and comprises a plurality of anti-resonant elements, comprising the method steps of: (a) providing a cladding tube (4), which comprises a cladding tube inner bore and a cladding tube longitudinal axis, along which a cladding tube wall extends, which wall is delimited by an inner face and an outer face, (b) providing a number of anti-resonant element preforms (5), (c) arranging the anti-resonant element preforms (5) at desired positions on the inner face of the cladding tube wall to form a primary preform (7) for the hollow-core fiber, which primary preform comprises a hollow core region and a casing region, and (d) elongating the primary preform (7) to form the hollow-core fiber or further processing the primary preform (7) to form a secondary preform from which the hollow-core fiber is drawn, the further processing comprising carrying out one or more of the following hot-forming processes once or repeatedly: (i) elongation, (ii) collapse, (iii) collapse and simultaneous elongation, (iv) collapse of additional casing material, (v) collapse of additional casing material and subsequent elongation, (vi) collapse of additional casing material and simultaneous elongation, characterized in that, in order to arrange the anti-resonant element preforms (5) according to method step (c), a positioning template (1) is inserted into the cladding tube inner bore, which template comprises holding elements (3) for positioning the anti-resonant element preforms (5) in the desired positions, and in that the positioning template (1) comprises at least one latching means which interacts with a latching means counterpart (6) in the cladding tube wall to form a force-fitting and / or form-fitting connection.

2. The method according to claim 1, characterized in that a positioning template (1) having a shaft (2) that projects into the cladding tube inner bore is inserted, which shaft is provided with holding elements (3) in the form of a plurality of holding arms pointing radially outward.

3. The method according to either claim 1 or claim 2, characterized in that the anti-resonant element preforms (5) are tubular having a tube outer lateral surface, and in that each holding element (3) has at least two contact points with the tube outer lateral surface of the antiresonant element preform (5) to be held.

4. The method according to any of the preceding claims, characterized in that the positioning template (1) is inserted in the region of a cladding tube end face, preferably in the region of both cladding tube end faces.

5. The method according to claim 1, characterized in that the latching means counterpart (6) is arranged in the end face of the cladding tube wall and the latching means is completely retractable therein.

6. The method according to either claim 1 or claim 5, characterized in that the latching means counterpart (6) does not reach the outer face of the cladding tube.

7. The method according to any of the preceding claims, characterized in that the positioning template (1) is made of graphite or glass, preferably quartz glass.

8. The method according to any of the preceding claims, characterized in that the positioning template (1) is machined with a dimensional deviation of less than + / - 0.1 mm.

9. The method according to any of the preceding claims, characterized in that a cladding tube (5) having a circular inner cross section is provided, which comprises a longitudinal structure (8) on the inner face of the cladding tube wall, which structure is designed as a longitudinal groove or as a longitudinal slot.

10. The method according to any of the preceding claims, characterized in that the inner face of the cladding tube is produced by machining, in particular by drilling, milling, grinding, honing and / or polishing.

11. The method according to any of the preceding claims, characterized in that arranging the antiresonant element preforms (5) at desired positions on the inner face of the cladding tube wall and / or elongating or further processing the primary preform (7) according to method step (d) includes a fixing measure and / or a sealing measure using an amorphous SiOz particle-containing sealing or bonding compound.

12. A method for producing a preform for an anti-resonant hollow-core fiber which comprises a hollow core extending along a longitudinal axis of the fiber and an inner casing region that surrounds the hollow core and comprises a plurality of anti-resonant elements, comprising the method steps of: (a) providing a cladding tube (4), which comprises a cladding tube inner bore and a cladding tube longitudinal axis, along which a cladding tube wall extends, which wall is delimited by an inner face and an outer face, (b) providing a number of anti-resonant element preforms (5), (c) arranging the anti-resonant element preforms (5) at desired positions on the inner face of the cladding tube wall to form a primary preform (7) for the hollow-core fiber, which primary preform comprises a hollow core region and a casing region, and (d) optionally further processing the primary preform to form a secondary preform for the hollow-core fiber, the further processing comprising carrying out one or more of the following hot-forming processes once or repeatedly: (i) elongation, (ii) collapse, (iii) collapse and simultaneous elongation, (iv) collapse of additional casing material, (v) collapse of additional casing material and subsequent elongation, (vi) collapse of additional casing material and simultaneous elongation, characterized in that, in order to arrange the anti-resonant element preforms (5) according to method step (c), a positioning template (1) is inserted into the cladding tube inner bore, which template comprises holding elements (3) for positioning the anti-resonant element preforms (5) in the desired positions, and in that the positioning template (1) comprises at least one latching means which interacts with a latching means counterpart (6) in the cladding tube wall to form a force-fitting and / or form-fitting connection.