MEMBRAN ELECTRODE ARRANGEMENT AND FUEL CELL

DE502020009435D1Active Publication Date: 2024-10-31GREENERITY GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009435
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-26
Filing Date
2020-07-10
Publication Date
2024-10-31
Estimated Expiration
2040-07-10

AI Technical Summary

Technical Problem

Membrane electrode arrangements for fuel cells have low tolerance to carbon monoxide, which acts as a catalyst poison, reducing their performance and power density.

Method used

A membrane electrode arrangement with a cathode and an anode separated by a proton-conductive membrane, where the cathode includes a first metal-containing catalyst for oxygen reduction and the anode includes a second and third catalyst for hydrogen oxidation and CO oxidation, respectively, with a specific mass ratio of platinum to other metals that ensures high catalytic activity and CO tolerance.

Benefits of technology

The arrangement achieves high long-term stability of power density and improved CO tolerance by effectively oxidizing CO to CO2, preventing it from inhibiting catalyst performance and maintaining high catalytic activity with minimal platinum usage.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a membrane electrode assembly having high catalytic activity with improved tolerance to carbon monoxide (CO) and to a fuel cell comprising this membrane electrode assembly.

[0002] Membrane electrode assemblies for fuel cell applications are known from the prior art. These comprise a proton-conducting membrane coated with an anode on one side and a cathode on the other. The anode usually contains platinum as a catalyst, which catalyzes the conversion of hydrogen supplied to the fuel cell into protons. Platinum is also usually used as a catalyst for the reduction of oxygen on the cathode side. A disadvantage of previous membrane electrode assemblies is their low tolerance to CO, which acts as a catalyst poison and secondarily reduces the performance of the membrane electrode assembly and thus also of the fuel cell.

[0003] EP 0736921 A1 describes an electrode comprising a first catalytic component active at reaction sites in the gas phase and a second catalytic component active at electrochemical reaction sites, each catalytic component being present either as a separate layer, as a single mixed layer, or as a combination of a separate layer and a mixed layer. The electrode exhibits improved tolerance to poisons such as carbon monoxide and carbon dioxide.

[0004] JPH10270055 A describes the creation of a local battery between catalysts and an acceleration of the electrochemical catalytic reaction by arranging ion-permeable material in which ions can move and electron-permeable material in which electrons can move between multiple catalysts. In detail, JPH10270055 A describes a catalyst A1 and catalyst B2, whose natural potentials are different, arranged to contact each other via the electron-permeable material and the ion-permeable material. On catalyst B2, whose natural potential is low and close to the hydrogen production potential, a reactant is oxidized to produce a product.Produced ions and electrons reach catalyst A1 through the electron-permeable material and the ion-permeable material, and another reactant is reduced on catalyst A1 to produce another product. A poly-based catalyst containing platinum and a first metal other than platinum, and a poly-based catalyst containing platinum and a second metal other than platinum, are used as catalysts. Phosphoric acid, sulfuric acid, solid high-molecular-weight electrolytes, or mixtures thereof are used as ion-permeable materials. The catalyst is contained in an electron-permeable material.

[0005] US 2006 / 099489 A1 teaches a fuel cell electrode comprising a catalyst layer and an electrode substrate supporting the catalyst layer and comprising a conductive substrate. The catalyst layer comprises a first catalyst supported on a carbon support and a second catalyst supported on an inorganic oxide support. The first catalyst comprises an alloy of Pt and a metal selected from the group consisting of Co, Ni, and a mixture thereof, and the second catalyst comprises an alloy of Pt and a metal selected from the group consisting of Co, Ni, and a mixture thereof.

[0006] The object of the invention is to provide a membrane electrode assembly characterized by high catalytic activity and high CO tolerance. Furthermore, the object of the invention is to provide a fuel cell with a consistently high power density.

[0007] This problem is solved by the features of the independent claims. The dependent claims contain advantageous developments of the invention.

[0008] Thus, the problem is solved by a membrane electrode assembly comprising a cathode, an anode, and a proton-conducting membrane. The membrane is arranged between the cathode and the anode. The cathode comprises a first metal-containing catalyst and a proton-conducting ionomer. The first catalyst is preferably homogeneously distributed in the ionomer, resulting in high catalytic activity across the entire cathode and effective oxygen conversion. The first catalyst is specifically limited to catalyzing the cathode reaction, i.e., the reduction of oxygen.

[0009] The anode also comprises a proton-conducting ionomer and, next to it, a second metal-containing catalyst that catalyzes the oxidation of hydrogen to protons. In other words, the second catalyst catalyzes the anode reaction, i.e., the conversion (oxidation) of hydrogen to protons. The protons then migrate through the proton-conducting membrane and subsequently react with the reduced oxygen.

[0010] The anode also comprises a third metal-containing catalyst that catalyzes the reaction of CO to CO2, i.e. the oxidation of CO. CO, which acts as a catalyst poison and reduces the performance of the electrodes, can be introduced, for example, by the hydrogen-containing fuel gas. If it is not removed quickly, it blocks the active sites of the catalysts and significantly reduces the power density of the membrane electrode assembly. By providing the third catalyst, any existing CO is oxidized to CO2 and thus rendered harmless. CO2 does not inhibit the performance of the catalysts, so the third catalyst increases tolerance to CO. The total mass ratio of platinum in the second catalyst and platinum in the third catalyst to the total mass ratio of metals in the second catalyst and the third catalyst, with the exception of platinum, is greater than 3:1.Only through this mass ratio is a high long-term stability of the power density and at the same time a high CO tolerance achieved in the membrane electrode arrangement according to the invention.

[0011] Any metal-containing catalysts that catalyze the desired reaction and contain at least one metal are suitable as metal-containing first, second and third catalysts. The metal can be present in different forms. Example catalysts include (pure, i.e. elemental) metals, such as noble metals, including Ir, Ru and Pt, but also metal oxides and alloys of two or more metals. The second catalyst and the third catalyst can contain the same metal, but are then present in different forms. For example, the second catalyst is a (pure) metal and the third catalyst is an alloy. Or the second catalyst is a (pure) metal and the third catalyst is a metal oxide. Or the second catalyst is a metal oxide and the third catalyst is an alloy.Any combination of metal-containing catalysts in the second and third catalysts is possible.

[0012] The mass ratio is determined based on the respective mass of the metal (or metals) of the corresponding metal-containing catalyst. The second catalyst or the third catalyst, or both the second catalyst and the third catalyst, may contain platinum. It is not necessary for both the second catalyst and the third catalyst to contain platinum, as long as the mass ratio of the total mass of platinum in the second and third catalysts to the total mass of the other metals in the second catalyst and the third catalyst—that is, all metals except platinum—is greater than 3:1.

[0013] According to the invention, the total area weight of platinum of the second catalyst and of platinum of the third catalyst is less than 0.4 mg / cm 2< , whereby very good catalytic properties can be obtained at minimal financial expense.

[0014] The CO tolerance will be improved while maintaining a very good power density of the membrane electrode assembly by ensuring that the total mass ratio of platinum of the second catalyst and platinum of the third catalyst to the total mass ratio of metals of the second catalyst and the third catalyst, with the exception of platinum, is less than or equal to 9:1.

[0015] According to an advantageous development, the second catalyst and the third catalyst are each arranged on an electrically conductive support. The electrically conductive support on which the second catalyst and the third catalyst are arranged can be the same electrically conductive support, or different electrically conductive supports can be used. This improves the electrical conductivity of the anode, which is beneficial to the power density of the membrane electrode assembly. The second catalyst and / or the third catalyst can be present in discrete electrode layers or homogeneously distributed in a common electrode layer. In the first case, the membrane electrode assembly has the following layer sequence: cathode / membrane / anode layer 1 / anode layer 2. In the second case, the membrane electrode assembly has the following layer sequence: cathode / membrane / anode.

[0016] Due to their very high reactivity and thus their good catalytic properties, the second catalyst and the third catalyst are selected from: an alloy, a metal, a metal oxide, or a mixture of these compounds. At least one of these metal-containing compounds of the second and / or third catalyst contains platinum in order to adjust the ratio of the total mass of platinum in the second catalyst and platinum in the third catalyst to the total mass ratio of metals in the second catalyst and the third catalyst, with the exception of platinum, to greater than 3:1. The second catalyst is preferably platinum. The third catalyst is also advantageously a platinum alloy, since platinum alloys can be very well selected in light of their CO binding and conversion activity.

[0017] Particularly advantageously, the alloy comprises platinum and at least one element selected from the group consisting of Ru, Rh, Ni, Cu and Ir. Among the above-mentioned alloying elements, Ru is particularly preferred because it binds CO very quickly and thus effectively and also accelerates the conversion to CO2.

[0018] Furthermore, the electrically conductive carrier(s) is / are selected from conductive carbon, inorganic oxides, and mixtures thereof. Due to the ease of processing, it is particularly advantageous to use either electrically conductive carbon or one or more oxides.

[0019] It is further advantageous if the electrically conductive support(s) have a specific surface area of ​​50 to 1000 m² / g, as this allows the second catalyst and the third catalyst to be distributed particularly finely and evenly within the anode. This improves the activity of the anode by increasing the number of bonding sites on the catalyst for carrying out the catalytic reaction. The specific surface area is determined using nitrogen adsorption (BET method) in accordance with DIN ISO 9277:2003-05 "Determination of the specific surface area of ​​solids by gas adsorption using the BET method."

[0020] A further advantageous development provides for the platinum weight per unit area of ​​the second catalyst to be less than 0.3 mg / cm². The platinum weight per unit area is understood to be the weight of platinum in the second catalyst relative to the geometric surface of the anode facing the membrane. A platinum weight per unit area of ​​the second catalyst of less than 0.3 mg / cm² allows costs to be kept as low as possible while maintaining very high catalytic activity of the anode.

[0021] In order to achieve particularly good catalytic properties, the total area weight of platinum of the second catalyst and of platinum of the third catalyst is advantageously more than 0.015 mg / cm 2< and in particular more than 0.03 mg / cm 2< .

[0022] For the above reasons, it is further preferred if the area weight of platinum of the second catalyst is more than 0.015 mg / cm 2< and in particular more than 0.03 mg / cm 2<.

[0023] To achieve particularly high long-term stability of the membrane electrode assembly's performance, i.e., high catalytic activity in the conversion of the fuels used, with very good CO tolerance, the mass ratio of platinum in the first catalyst to the total mass ratio of metals in the second catalyst and the third catalyst, with the exception of platinum, is preferably greater than 12:1 and in particular greater than 35:1. This ratio allows for a sustained high power density even if an alloy metal, such as ruthenium, transfers from the anode to the cathode during operation. This process can lead to a reduction in the catalytic activity of the cathode and is then less pronounced if the aforementioned catalyst ratios are maintained.

[0024] Due to the very good catalytic activity in the conversion of oxygen with protons to water, the first catalyst is advantageously selected from platinum, platinum alloys, transition metals, transition metal alloys and mixtures thereof.

[0025] In order to achieve the most uniform distribution possible with a low catalyst concentration and thus a very high catalytic activity of the cathode, according to a further advantageous development, the first catalyst is arranged on an electrically conductive support. The electrically conductive support used can be an electrically conductive support such as that described above as advantageous for supporting the second catalyst and the third catalyst.

[0026] If a transition metal alloy is used as the first catalyst, it is preferably selected from platinum and cobalt. Platinum-cobalt alloys have proven to be readily available and exhibit high catalytic activity.

[0027] The invention also describes a fuel cell comprising the membrane electrode assembly disclosed above. The use of the membrane electrode assembly according to the invention results in a fuel cell with a permanently high power density that is tolerant to CO.

[0028] The advantages, advantageous effects and further developments described for the membrane electrode arrangement according to the invention also apply to the fuel cell according to the invention.

[0029] Further details, advantages, and features of the present invention will become apparent from the following description of exemplary embodiments with reference to the drawings. It shows: Fig. 1 a membrane electrode arrangement according to an embodiment in section, Fig. 2 a graph illustrating test results on performance stability and CO stability, Fig. 3 a table illustrating the test results from Figure 2 for performance stability and Fig. 4 a table illustrating the test results from Figure 2 on CO stability.

[0030] In Figure 1 Only the essential features of the membrane electrode assembly are shown. All other features are omitted for clarity.

[0031] Figure 1 shows a membrane electrode assembly 1 comprising a cathode 2 and an anode 3, which have a proton-conductive membrane 4 between them. The anode 3 is the electrode at which hydrogen is oxidized to protons, which then react further to form water. The cathode 2 is the electrode at which oxygen is reduced.

[0032] The cathode 2 comprises a first catalyst 5 and a proton-conductive ionomer 6, wherein the first catalyst 5 catalyzes the reduction of oxygen and comprises, in particular, platinum, a platinum alloy, one or more transition metals, or mixtures thereof. The first catalyst is preferably arranged on an electrically conductive support 7.

[0033] The anode 3 also comprises a proton-conductive ionomer 8, a second catalyst 9 catalyzing the reaction of hydrogen to protons, and a third catalyst 10 catalyzing the reaction of CO to CO 2 . Both the second catalyst 9 and the third catalyst 10 are supported on an electrically conductive carrier 11.

[0034] The second catalyst 9 is platinum, and the third catalyst 10 is a platinum alloy. In the platinum alloy, platinum is the main component by mass, and at least one element selected from the group consisting of Ru, Rh, Ni, Cu, and Ir serves as a doping element.

[0035] The total mass ratio of platinum of the second catalyst 9 and platinum of the third catalyst 10 to the total mass ratio of metals of the second catalyst 9 and the third catalyst 10 with the exception of platinum is more than 3:1 and less than or equal to 9:1.

[0036] The membrane electrode assembly 1 is characterized by high long-term stability of the power density and very high tolerance to CO.

[0037] Furthermore, the following experiments were conducted. Membrane electrode assemblies were fabricated with a cathode comprising platinum as the first metal-containing catalyst with a surface weight of 0.40 mg Pt / cm2 in the form of a platinum-cobalt alloy on a high-surface-area carbon layer, and a proton-conductive ionomer with an ion exchange capacity of approximately 1.27 meq / g. The cathode also comprised a proton-conductive ionomer with an ion exchange capacity of approximately 1.27 meq / g, a second metal-containing catalyst catalyzing the reaction of hydrogen to protons, and a third metal-containing catalyst catalyzing the reaction of CO to CO2. Platinum was used as the second catalyst, and a platinum-ruthenium alloy as the third catalyst.

[0038] In the membrane electrode assemblies produced, the total mass ratio of platinum of the second catalyst and platinum of the third catalyst (here 57.4 mass%) to the total mass ratio of metals of the second catalyst (here 0 mass%) and the third catalyst (here 42.6 mass%) with the exception of platinum (Ru) was varied.

[0039] The fabrication of the membrane electrode assembly was generally as follows: First, separate dispersions ("inks") were prepared to produce the anode and cathode catalyst layers. The respective catalysts, proton-conductive ionomer, and suitable solvents—selected from water and organic solvents—were dispersed using a suitable dispersion unit. The second and third catalysts were used to prepare the anode catalyst dispersion, and their compositions were varied to achieve different ratios of platinum to non-platinum metals. The anode and cathode inks were then coated onto PTFE carrier foils and dried to produce anode and cathode layers with the desired platinum metal loading per unit area.A proton-conductive membrane was then placed between the anode and cathode layers on the carrier foils and pressed under pressure and heat to transfer the previously prepared electrode layers to the membrane. Perfluorinated or hydrocarbon-based polymers functionalized with acid groups (e.g., sulfonic acids or carboxylic acids) can be used as ionomers. The acid groups are typically arranged in a side chain, the chain length of which can vary and which can be either linear or branched. Alcohols, ketones, aldehydes, carboxylic acids, carboxylic acid esters, ethers, or amides, each with varying chain lengths and cyclic structures, or mixtures thereof, can be used as organic solvents.

[0040] Anode 1 (Pt : Ru = 9 : 1): 7.00 g of a pure platinum catalyst consisting of 19.9 mass% platinum and 80.1 mass% carbon support, and 0.77 g of a platinum-ruthenium alloy catalyst consisting of 30.5 mass% platinum, 23.6 mass% ruthenium and 45.9 mass% carbon support, were dispersed together with 19.20 g of an ionomer dispersion consisting of 24.9% proton-conductive ionomer and 75.1 mass% water, as well as 73.03 g of other solvents for 1 h in a suitable dispersion unit. The catalyst ink thus obtained was coated on a PTFE carrier film and the wet film thickness was adjusted to obtain a basis weight in terms of platinum between 0.015 mg / cm 2 and 0.2 mg / cm 2 .

[0041] Anode 2 (Pt:Ru = 6:1): 6.64 g of a pure platinum catalyst, consisting of 19.9 mass% platinum and 80.1 mass% carbon support, and 1.19 g of a platinum-ruthenium alloy catalyst, consisting of 30.5 mass% platinum, 23.6 mass% ruthenium and 45.9 mass% carbon support, were dispersed together with 18.88 g of an ionomer dispersion, consisting of 24.9% proton-conductive ionomer and 75.1 mass% water, as well as 73.29 g of other solvents for 1 h in a suitable dispersion unit. The catalyst ink thus obtained was coated on a PTFE carrier film and the wet film thickness was adjusted to obtain a basis weight in terms of platinum between 0.015 mg / cm 2 and 0.2 mg / cm 2 .

[0042] Anode 3 (Pt:Ru = 3:1): 4.76 g of a pure platinum catalyst, consisting of 19.9 mass% platinum and 80.1 mass% carbon support, and 2.34 g of a platinum-ruthenium alloy catalyst, consisting of 30.5 mass% platinum, 23.6 mass% ruthenium and 45.9 mass% carbon support, were dispersed together with 15.62 g of an ionomer dispersion, consisting of 24.9% proton-conductive ionomer and 75.1 mass% water, as well as 77.27 g of other solvents for 1 h in a suitable dispersion unit. The catalyst ink thus obtained was coated on a PTFE carrier film and the wet film thickness was adjusted to obtain a basis weight in terms of platinum between 0.015 mg / cm 2 and 0.2 mg / cm 2 .

[0043] Cathode: 6.67 g of a platinum-cobalt alloy catalyst consisting of 48.5 mass% platinum, 4.9 mass% cobalt, and 46.6 mass% carbon support, and 93.33 g of an ionomer dispersion consisting of 3.60 mass% proton-conductive ionomer, 96.4 mass% water, and other solvents were dispersed for 1 h in a stirred ball mill. The resulting catalyst ink was coated onto a PTFE carrier film, and the wet film thickness was adjusted to achieve a platinum weight of 0.4 mg / cm².

[0044] Preparation of the electrode-membrane composite: Supported anode and cathode catalyst layers were arranged congruently on opposite sides of a proton-conductive membrane and then pressed under pressure in a press at a temperature of 160°C for 5 minutes, so that a bond was formed between the electrodes and the membrane and the electrodes could be removed from the corresponding PTFE carrier films without leaving any residue. The measurement parameters were as follows: Power density and CO tolerance:

[0045] First, the cell potential of the catalyst-coated membranes without CO contamination was investigated using a polarization curve. The cell temperature was 80°C, the gas temperature was 64°C, and the humidification was 50% RH. The inlet pressure was 1.5 bar.

[0046] Subsequently, the hydrogen gas stream was enriched with 0.2 ppm CO on the anode side and supplied to the anode at a nitrogen dilution of 30 vol%. The power density was again investigated. The reduction in cell voltage at a current density of 1.2 A cm -2 is an indicator of the CO tolerance of the catalyst-coated membrane. Start-up / shut down -Cycle Test (SUSD)

[0047] SUSD cycles were conducted in a gas-switching test with a precisely defined residence time of the hydrogen / air interface. The anode side was equipped with a three-way valve that enabled switching from dry air to humidified hydrogen and vice versa. To facilitate start-up ( Start-up ), the anode flow field was first filled with dry air. Subsequently, it was switched to humidified hydrogen, which led to the formation of a hydrogen-air boundary. Conversely, during the shutdown process ( Shut down ), the hydrogen-filled anode flow field was purged with air, which led to the formation of an air-hydrogen boundary. The operating conditions were kept constant in both chambers (anode and cathode) of the cell during the SUSD test (1.5 bar abs., inlet, cell temperature 35°C, gas temperature 30°C and 75% RH). The residence time of the hydrogen-air boundary in the cell was defined by the volume of the flow field and the volume flow of the supplied gases and was 0.3 s. The time between Start-up and Shut down was set to 120 s. A total of 500 SUSD cycles were repeated. Power density and CO tolerance after SUSD cycles:

[0048] Following the SUSD cycles, a polarization curve was measured again. The reduction in cell voltage was examined in relation to the first measurement. Subsequently, CO tolerance was again examined using the method described above.

[0049] As can be seen from the graphic in Figure 2As can be seen, the total mass ratio of platinum in the second catalyst and platinum in the third catalyst to the total mass ratio of metals in the second catalyst and the third catalyst, with the exception of platinum (Ru), was varied in a range from approximately 10:1 to approximately 2:1. With regard to the performance stability and CO stability of the membrane electrode assemblies, five ranges could be distinguished: In range A, i.e. with a mass ratio of Pt:Ru of more than 9:1 and a low loading of the anode in relation to the basis weight of the platinum, the CO tolerance was significantly reduced. In range E, i.e. with a mass ratio of Pt:Ru of less than 3:1 and a high loading of the anode in relation to the basis weight of the platinum, the long-term stability of the (catalytic) performance of the membrane electrode assemblies was significantly reduced.Good results were achieved in areas B and D for both long-term stability of the (catalytic) performance and CO tolerance, with the best results being obtained in area C.

[0050] The table in Figure 3 illustrates the test results from Figure 2 The table shows the long-term stability of the (catalytic) performance of the membrane electrode assembly, or rather the loss of cell voltage after 500 SUSD cycles at a current density of 1.2 A cm -2< , whereby a significant reduction of the cell voltage of more than 50 mV was observed, particularly for high Ru contents, ie for a high anode loading of 0.2 mg cm -2< in combination with a Pt : Ru mass ratio of 3 : 1.

[0051] The table in Figure 4 also illustrates the test results from Figure 2The table shows that good CO tolerances and performance of the membrane electrode assembly are achieved with a Pt:Ru mass ratio in a range of 9:1 to 3:1. However, at the limit of low Ru contents, i.e., at very low anode loading and a Pt:Ru mass ratio of 9:1, the values ​​deteriorate significantly. By further varying the Pt weight per unit area in the anode, the CO tolerance and performance of the membrane electrode assembly could be further improved.

[0052] In addition to the above written description of the invention, reference is hereby explicitly made to the graphic representation of the invention in the figures for its supplementary disclosure. List of reference symbols

[0053] 1Membrane electrode assembly 2Cathode 3Anode 4Proton-conductive membrane 5First catalyst 6Proton-conductive ionomer 7Electrically conductive support 8Proton-conductive ionomer 9Second catalyst 10Third catalyst 11Electrically conductive support

Claims

1. Membrane electrode assembly (1) comprising a cathode (2), an anode (3), and a proton-conductive membrane (4), wherein - the cathode (2) comprises a first metal-containing catalyst (5) and a proton-conductive ionomer (6), wherein - the anode (3) comprises a proton-conductive ionomer (8), a second metal-containing catalyst (9), which catalyzes the reaction of hydrogen to protons, and a third metal-containing catalyst (10), which catalyzes the reaction of CO to CO2, and wherein the total mass ratio of platinum of the second catalyst (9) and platinum of the third catalyst (10) to the total mass ratio of metals of the second catalyst (9) and the third catalyst (10), with the exception of platinum, is greater than 3:1 and smaller than or equal to 9:1, wherein the total mass per unit area of platinum of the second catalyst (9) and of platinum of the third catalyst (10) is less than 0.4 mg / cm2.

2. Membrane electrode assembly (1) according to claim 1, wherein the second catalyst (9) and the third catalyst (10) are each arranged on an electrically conductive support (11).

3. Membrane electrode assembly (1) according to one of the preceding claims, wherein the second catalyst (9) is platinum and the third catalyst (10) is selected from: an alloy, a metal, a metal oxide, or a mixture of these compounds, wherein the alloy comprises in particular platinum and at least one element selected from the group consisting of Ru, Rh, Ni, Cu and Ir.

4. Membrane electrode assembly (1) according to claim 2, wherein the electrically conductive support (11) is selected from electrically conductive carbon, inorganic oxides and mixtures thereof and / or wherein the electrically conductive support (11) has a specific surface area of 50 to 1000 m2 / g.

5. Membrane electrode assembly (1) according to one of the preceding claims, wherein the mass per unit area of platinum of the second catalyst (9) is less than 0.3 mg / cm2 and / or wherein the total mass per unit area of platinum of the second catalyst (9) and of platinum of the third catalyst (10) is more than 0.015 mg / cm2 and in particular more than 0.03 mg / cm2 and / or wherein the mass per unit area of platinum of the second catalyst (9) is more than 0.015 mg / cm2 and in particular more than 0.03 mg / cm2.

6. Membrane electrode assembly (1) according to one of the preceding claims, wherein the mass ratio of platinum of the first catalyst (5) to the total mass ratio of metals of the second catalyst (9) and the third catalyst (10), with the exception of platinum, is greater than 12:1, in particular greater than 35:1.

7. Membrane electrode assembly (1) according to one of the preceding claims, wherein the first catalyst (5) is selected from platinum, platinum alloys, transition metals, transition metal alloys and mixtures thereof, wherein the transition metal is in particular cobalt or nickel and / or wherein the first catalyst (5) is arranged on an electrically conductive support (7).

8. Membrane electrode assembly (1) according to one of the preceding claims, wherein the membrane is selected from the group of perfluorinated, partially fluorinated or non-fluorinated materials and / or wherein the layer thickness of the membrane is 3 to 20 µm.

9. A fuel cell comprising a membrane electrode assembly (1) according to one of the preceding claims.