METHOD FOR APPLYING POWDER-FORMED OR WIRE-FORMED MATERIAL TO A WORKPIECE

DE502020009646D1Active Publication Date: 2024-11-21VIENNA UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009646
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-07
Filing Date
2020-09-30
Publication Date
2024-11-21
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing deposition welding methods face issues with nozzle clogging, reduced precision, and increased maintenance costs due to material accumulation, leading to production stoppages and decreased surface quality.

Method used

A method involving a device with a nozzle and working gas region to form a constricted arc between the electrode and workpiece, preventing arc wandering and material accumulation, while using a short nozzle and precise gas control to optimize precision and speed, allowing for dynamic adjustment of arc power and gas flow.

Benefits of technology

This approach ensures precise deposition of material onto the workpiece, extends device longevity, and reduces maintenance costs by preventing nozzle clogging, while enabling precise control over the arc and gas composition for improved surface quality and production efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for the build-up welding of powdered or wire-shaped material onto a workpiece, which is preferably a flat substrate, by means of a device comprising a substantially rod-shaped electrode, wherein the electrode has at least one material feed channel extending in its interior for feeding the powdered or wire-shaped material into the arc (see, for example, US 4 527 039 A).

[0002] In the field of build-up welding, the process of arc welding for applying material to a surface to be machined has been known for some time. Arc welding is a process that involves the localized liquefaction of metals. An arc is ignited between the workpiece and a current-carrying electrode and maintained by the current flowing through the electrode, arc, and workpiece. Since the properties of the arc and the molten metal depend on the atmosphere, specialized gases, usually argon, but also CO2 for the controlled introduction of carbon, are blown around the molten metal to prevent oxidation, allowing welding to take place in a controlled atmosphere.

[0003] Cladding welding introduces fresh material into the arc, which is liquefied and applied to the surface to be welded. This material is usually introduced laterally into the arc as a metal wire or powder. A special form of cladding welding is the MIG / MAG process, in which material is introduced as a wire electrode and melted in the arc, thus depositing it. In this case, the current-carrying wire forms the electrode, so that the arc is formed between the wire and the workpiece.

[0004] In the field of precision metal deposition welding, the Cold Metal Transfer (CMT) process from Fronius is well-known. This is a modification of the MIG / MAG process, which feeds a welding wire as a current-carrying electrode to the welding area, where it is melted by the heat of an arc between the welding wire and the welding area. In the CMT process, this wire is not fed in at a constant rate, but rather is fed in and out depending on the current flow, allowing droplets of the liquefied material to be deposited precisely in the welding area.

[0005] Another common method is tungsten inert gas (TIG) welding, which involves a current-carrying tungsten electrode that is sharpened to a point and continuously purged with argon. In this process, a wire is inserted laterally into the arc.

[0006] A variation of arc welding is plasma welding. In this process, the arc is forced through a nozzle to better control its geometric and thermal properties. The electrode is axially centered behind the nozzle. The nozzle, often made of copper, is often conductive itself to ignite a primary arc between the electrode and nozzle. Once the primary arc has reached the workpiece, the current flow to the nozzle can be cut off, and the arc can be ignited between the electrode and the workpiece instead.

[0007] Like arc welding, plasma cladding can be carried out by feeding material from the side, but since plasma cladding allows much higher temperatures than arc cladding, other types of material liquefaction are also possible.

[0008] In one of these liquefaction methods, plasma spraying, a primary arc between the electrode and nozzle is kept as extended as possible through favorable system parameters. This can be achieved by using a longer nozzle or by working in vacuum chambers. Powder is introduced into the long plasma flame and is transported and accelerated by the hot gas. The powder emerges molten and at high speed from the plasma flame and impacts the surface to be treated. There, the liquid droplets solidify suddenly. Since the droplets are very hot but have a low heat capacity, the thermal energy deposited on the workpiece is low. The quality of the sprayed surface is largely determined by the time the powder spends in the plasma flame. Therefore, the length of the plasma flame is one of the parameters to be maximized.

[0009] The document US 2012193329 A1 discloses a powder microspark deposition system comprising an electrode and a powder feed channel configured within or at least partially around the electrode for feeding powder comprising electrically conductive material into a gap between the electrode and the substrate.

[0010] Furthermore, document EP 264243 A2 discloses a method using the powder micro-spark system from US 2012193329 A1 for repairing a metallic object.

[0011] US 2014008330 A1 also describes a method for repairing a component in which an electrode is positioned over a defect or damage. A first metal powder and a second metal powder can be fed into a discharge gap between the electrode and the component to form a hybrid metal coating.

[0012] The document DE 3110628 A1 discloses a method for producing alloyed surfaces on pipes, wherein alloy material is introduced into an arc through a hollow electrode.

[0013] Although it is known that axial powder feed generally improves surface quality, in practice these processes result in material buildup on the nozzle surrounding the electrode, which subsequently becomes increasingly clogged. On the one hand, if contact is established between the nozzle and the electrode due to deposited material, the build-up welding device can then become permanently unusable and must be replaced, which incurs high costs. On the other hand, even if there is no contact between the electrode and the nozzle due to deposited material over an extended period, not only is the improvement in surface quality de facto prevented by the blockage, but the build-up welding device must also be freed of the material deposited on the nozzle, which entails complex and time-consuming maintenance work.Furthermore, a welding fixture failure results in significant costs due to production downtime. Furthermore, these processes are characterized by reduced precision in applying the material to the surface being machined due to nozzle clogging, as the material accumulated at the nozzle makes it difficult to purge the working gas around the electrode.

[0014] The object of the invention is therefore to provide a method that avoids the disadvantages of the prior art and opens up new manufacturing methods through the resulting precision. This object is achieved by providing a method for the build-up welding of powdered or wire-shaped material with the features of claim 1.

[0015] In the method according to the invention, the device comprises a nozzle surrounding the electrode and a working gas region which is formed between the electrode and the nozzle, the method comprising the following steps: Forming the arc as a transferred arc between the electrode and the workpiece or as a freestanding arc between the electrode and the nozzle, flooding the working gas region with a working gas to constrict the arc towards the workpiece, feeding the powdered or wire-shaped material into the constricted arc and moving the device over the workpiece while feeding the powdered or wire-shaped material into the constricted arc.

[0016] This prevents arc wandering, ensuring a straight arc path and, consequently, the precise feeding of the material in its powder or wire form into the arc, the melting of the material in the arc, and the precise delivery of the molten material to the workpiece. Furthermore, the use of a short nozzle and precise control of the arc by constriction effectively prevents material from accumulating in the nozzle, thereby increasing the longevity of the device. Furthermore, the shape of the arc can be adjusted by selecting the flow rate of the working gas. As a result, the arc power and gas flow rate can be dynamically adjusted to optimize the precision and speed of the process.

[0017] Thus, a working gas zone can advantageously be formed around the electrode, in which the working gas flows around the electrode and the arc to control the gas composition around the working zone, which in turn influences the arc performance. Furthermore, chemical reactions can occur between the atmosphere and the liquid metal. This can be prevented by flushing with working gases such as argon or helium, or utilized for material optimization by suitable active gases such as CO2. During the steps of forming the arc and flowing through the working gas zone, it is irrelevant which of the two steps is started first.

[0018] According to the invention, a radial distance between the nozzle and the electrode is not greater than 1 cm and / or an axial distance between the end of the nozzle facing the workpiece and the end of the electrode facing the workpiece is not greater than 1 cm, wherein the end of the nozzle facing the workpiece is preferably at a smaller distance from the workpiece than the end of the electrode facing the workpiece. The arc between the electrode and the nozzle can thus be formed particularly easily, in particular by selecting a preferred distance between the electrode and the nozzle. Furthermore, this embodiment of the nozzle enables the supply of working gas to the arc attachment of the electrode and, with a suitable feed rate, the constriction of the arc in the direction of the workpiece.The range of suitable flow rates depends on the geometry of the nozzle, the electrode, and the workpiece, as well as on the arc power, and can thus be dynamically adjusted to achieve the highest possible precision. The nozzles known from the prior art for other welding processes are typically longer than 10 cm in length to form a particularly long arc, which, however, is not necessary for the deposition welding process according to the invention.

[0019] Preferably, an additional working gas zone is formed between the nozzle and an atmosphere protection jacket surrounding the nozzle, which is flooded with another working gas before the start of the deposition welding process, thus creating a controlled atmosphere at a deposition point on the workpiece. This advantageously allows for optimal control of the atmosphere at the deposition point of the workpiece to be machined. The gas composition influences the arc performance and must therefore be controlled. Furthermore, chemical reactions can occur between the atmosphere and the liquid metal. This can be prevented by flushing with working gases such as argon or helium, or used for material optimization by suitable active gases such as CO2.

[0020] Alternatively, the device can be used in a controlled atmosphere chamber. This eliminates the need to supply gas through the primary gas stream. A controlled atmosphere chamber avoids turbulence that could occur when gas is flushed around the electrode, thus allowing for particularly precise work. Furthermore, a controlled atmosphere chamber allows for a greater distance between the electrode and the workpiece without loss of precision due to turbulence, allowing for longer arcs. However, since a longer distance inherently reduces precision, this design is particularly suitable for surface finishing.

[0021] The method is preferably used for joint welding, wherein the powdered or wire-shaped material is preferably a metal, or the method is used for surface finishing, wherein the powdered or wire-shaped material is preferably a ceramic powder, a metal, or a carbide powder. Powdered material is particularly preferably used for surface finishing. The method according to the invention can thus be used for two different applications: for joint welding, on the one hand, and for surface finishing, on the other. The same device can be used for both applications, whereby a different material, material feed rate, and / or arc power can be selected in each case.

[0022] According to a further preferred embodiment, the powdered or wire-shaped material is fed in an additional working gas, which is preferably argon, helium, carbon dioxide or nitrogen, wherein the working gas and / or the additional working gas is / are also preferably argon, helium, carbon dioxide or nitrogen. If the same working gases are used, this has the advantage that the atmosphere around the material also remains homogeneous. Different gases initiate chemical reactions, which can also be beneficial for the molten metal. The working gas fed through the nozzle can therefore be identical to that of the controlled atmosphere around the arc, or different from it in order to achieve targeted chemical reactions in the arc. For example, H2 in the arc can react with a CO2 atmosphere to add carbon to the liquid metal.

[0023] Preferably, the distance between the electrode and the workpiece and / or a position of the electrode on the workpiece is controlled by a mechanical guide. On the one hand, structures can be applied to the workpiece by means of the guide and, on the other hand, the distance to the workpiece can be adjusted at any time in order to take account, for example, of unevenness in the workpiece or an inclination of the workpiece, which would not be possible with manual guidance of the device. Furthermore, the guide can be used to functionalise surfaces of workpieces, for example to create abrasion-resistant or high-melting-point surfaces of materials. In particular, the guide makes it possible to machine materials using the method according to the invention that are not themselves driven for the welding process. Workpieces other than, for example, pipes on a lathe can therefore also be machined using the method according to the invention.The guide is preferably a CNC guide or a robot arm.

[0024] According to a further preferred embodiment, the powdered or wire-shaped material is applied layer by layer to the workpiece to form overlapping material layers. For example, the method can therefore comprise the first step of deposition welding on a first location on the workpiece and the second step of repeated deposition welding on the same location on the workpiece. This allows complex, multi-layer structures and shapes to be applied to the workpiece. The shaping can be achieved by repeatedly removing the volume and adding material, which is an additive process for producing a workpiece. In particular, no mechanical shaping is necessary after deposition to produce a desired shape.

[0025] With the aforementioned embodiment, a workpiece can be produced that can be detached from the substrate and used independently, for example, a screw-on joint. On the other hand, the workpiece can remain on the workpiece to fulfill a function there, for example, as a joint socket applied to a metal profile.

[0026] According to a further preferred embodiment, the nozzle has internal channels for receiving cooling fluid, and the electrode has cooling means on its holder. This provides the advantage that, on the one hand, cooling the device increases its service life and, on the other hand, prevents damage to the device caused by overheating, as well as the resulting costly interruption of the work process.

[0027] The opening diameter of the electrode is preferably a maximum of 1 cm, particularly preferably a maximum of 300 µm. Furthermore, the electrode can preferably be tapered at its end facing the workpiece. This makes it easier to ignite an arc.

[0028] According to a further preferred embodiment, the arc power as well as the mixing ratios and / or the flow rates of said gases are adjusted in order to adjust the precision and the speed of application of the powdered or wire-shaped material to the workpiece.

[0029] According to the invention, the powdered or wire-like material is melted in the said arc. Preferably, the arc extends directly between the electrode and the workpiece without arcing into the powdered or wire-like material, which can be achieved by setting a suitable arc power and a suitable feed rate of the powdered or wire-like material. The choice of these parameters can be made by a person skilled in the art, with the arc power usually being high and the feed rate low. Alternatively, the arc can briefly arc into the material, i.e. there is a first arcing between the electrode and the material and a second arcing between the material and the workpiece, with the melting of the material usually occurring in the second arcing.To achieve this variation, the specialist can again select the arc power and feed rate, with the arc power being lower and the feed rate being higher than in the previous variation. However, it should be noted that the latter variation should not be confused with MIG welding, in which current flows through an electrode without an arc into the wire, and the arc only runs between the wire and the workpiece.

[0030] In a further preferred embodiment, the electrode ends in front of the material feed channel in the feed direction of the powdered or wire-shaped material or at the same point as the material feed channel. The first alternative is achieved, for example, by an electrode that has a bore with an internal coating and is tapered at its end. As a result, the material feed channel is longer than the electrode in the direction of the material feed direction, which promotes the flashover of the arc from the electrode directly onto the workpiece or nozzle. The second alternative can be achieved, for example, by the electrode having a bore without an internal coating. Regardless of whether the cathode is tapered at its end or not, the electrode will end in the feed direction of the material at the same point as the material feed channel.

[0031] A particularly advantageous application of this method for build-up welding arises when the workpiece is positioned above the fixture during build-up welding. In this application, the molten material can be transported to the workpiece by the constricted arc against gravity, without the molten material dripping downwards.

[0032] Advantageous and non-limiting embodiments of the invention are explained in more detail below with reference to the drawings. Figure 1 shows an embodiment of the method according to the invention in a schematic cross-sectional view. Figure 2 shows schematically an enlargement of the Figure 1 shown electrode in a cross-sectional view.

[0033] Figure 1shows a device 1 for deposition welding of powdered or wire-shaped material 11 onto a workpiece 10. The device 1 comprises a substantially rod-shaped electrode 6, for example, received in a holder, wherein the electrode 6 has at least one material feed channel 9 extending within its interior for feeding the powdered or wire-shaped material 11 into an arc 8. Preferably, the workpiece 10 is a flat substrate and in particular not a tube, since its curvature impairs the precision of the process.

[0034] The process for build-up welding is explained in more detail below. Up to three different working gases 3, 5, 7 or corresponding working gas streams can be used in the process, with a first working gas being referred to as "working gas 3," a second working gas as "further working gas 5," and a third working gas as "additional working gas 7." The working gases 3, 5, 7 can have different or identical compositions, as explained in more detail below. In particular, all working gases 3, 5, 7 can be shielding gases or active gases.

[0035] To carry out the procedure, as in Figure 1As shown, an electrode 6 made of high-temperature-resistant material, for example, tungsten, preferably for use with inert gas, or, for example, hafnium, preferably for use with active gas, is used. This electrode 6 has the exit of a channel 9 at the point where the arc 10 starts. The channel 9 can be supplied at its end facing away from the workpiece 10 with a flow of an additional working gas 7, which is mixed with a powdered or wire-like material 11.

[0036] This channel 9 can, for example, be present as a central bore through the hafnium insert in a hafnium electrode, which is pressed into a soft metal as a disc. With a tungsten electrode, however, the electrode 6 is usually sharpened. To axially sharpen a cylindrical electrode, the electrode 6 can be clamped in a lathe and ground to the desired sharpening angle with a clamped grinding machine. With tungsten electrodes, a sharpening angle of 10° has proven to be sufficiently sharp, as has also been the case with tungsten electrodes. Figure 2 can be removed. When sharpening, a margin of approximately 10 µm may remain between the channel and the outer diameter to allow for tolerances during clamping.

[0037] Electrodes 6 can also be manufactured with channel 9 already formed, for example, during sintering with an axial obstruction in the cavity. Already manufactured tungsten electrodes can also be machined using the electrode erosion process to create the axial channel 9 axially through the electrode 6. During electrode erosion, drift of the die-sinking wire cannot be avoided, resulting in a bent channel 9. In practice, however, this bending has not proven to be a problem for electrodes shorter than 6 cm.

[0038] As already mentioned above, the channel 9 is supplied with powdered or wire-shaped material 11 at its end facing away from the surface to be treated. For example, to supply the material 11, the additional working gas 7, which flows in a flow direction F3 of the additional working gas 7, can be blown in, which has been mixed with powdered material 11 to be applied.

[0039] Since the electrode 6 can also be flushed externally with a working gas 3 flowing in a flow direction F 2 of the working gas 3, for example with argon, it may be advantageous for some applications to use the same gas to maintain a homogeneous gas mixture around the electrode 6, so that a homogeneous plasma also remains in the arc 8. However, special applications can benefit from separate gas flows, for example, to form free carbon from CO 2 and H 2, which could be introduced into liquid metal for hardening.

[0040] Another method for introducing material is to allow powdered material 11 to trickle through channel 9, whereby this method of introduction is referred to as gravity feeding. Powder feeding is preferably carried out under a controlled atmosphere to avoid the introduction of contaminants or air to the arc.

[0041] Another way to introduce material 11 is to push material in wire or rod form through channel 9. If conductive wire is used, channel 9 is preferably insulated from the wire to prevent current flow through the wire. For this purpose, channel 9 can be vapor-coated internally with ceramics, or a thin ceramic tube can be inserted into channel 9. It should be noted that electrode 6 conducts heat, and the ceramic insert must therefore be comparably heat-resistant to electrode 6. The arc power is usually set such that the wire melts at the level of the electrode opening, but preferably at the latest between the electrode and nozzle.

[0042] The width of the applied welding track depends on the width of channel 9 in electrode 6. The narrower the channel 9 is at the arc initiation point, the narrower the powder or wire material 11 can be applied. The powder grain size can be selected such that the diameter of the powder grains does not exceed half the diameter of channel 9 in electrode 6.

[0043] In order to control the position of the arc 8 and prevent it from wandering, the device comprises a nozzle 2 surrounding the electrode 6 and a working gas region which is formed between the electrode 6 and the nozzle 2. A working gas 3 can be forced through the nozzle 2 or the working gas region at a high gas flow rate at the end of the electrode 6 through the base of the arc 8 in order to form the arc 8. This is referred to as a constricted arc, and the associated process is known as plasma welding. The electrode 6 can be placed axially behind the opening of a nozzle 2, i.e. on the side of the nozzle facing away from the workpiece.

[0044] In plasma welding, higher arc temperatures are possible by minimizing the heat output at the electrode 6 and instead releasing it along the arc 8. Constricting the arc 8 also allows the arc 8 path to be stabilized. While a free arc always exhibits a certain random movement across the workpiece 10, the stationary arc can be fixed by the gas flow, allowing for greater precision. The nozzle 2 has a larger diameter than the electrode 6. To keep the powder flow centered, the gas pressure of the flow through the electrode 6 can be adjusted to match the gas pressure of the arc-forming gas flow.

[0045] The process can be carried out in a chamber filled with an additional working gas 5, or the device 1 can have an additional working gas region, wherein the additional working gas 5 flows in a flow direction F 1 of the additional working gas 5, so that in both cases a controlled atmosphere is generated at a deposition site 12 of the workpiece 10. The additional working gas region can be formed between the nozzle 2 and an atmosphere protection casing 4 surrounding the nozzle 2.

[0046] Material to be applied is fed through channel 9 through electrode 6 to the arc 8 in powder form or as wire. In principle, any material that does not denature at the temperatures in the arc 8 can be processed. However, with materials that evaporate at the temperatures in the arc 8, the sudden increase in volume during evaporation of the powdered or wire-shaped material 11 can lead to turbulence and the gas flow can be deflected, which contributes to the growth of powder residues on the electrode 6 or on the nozzle 2. The process is therefore suitable for materials that melt in the plasma but do not evaporate. For example, steel powder is suitable for joint welding, but the processing of ceramics and carbides in powder form for surface finishing is also possible.

[0047] The temperature of the arc 8 can be controlled by the arc power. Furthermore, in a controlled atmosphere, the gas composition can be selected so that the voltage drop in the arc 8 better corresponds to the desired power. This voltage drop can be derived from the minimum of Paschen's law.

[0048] Higher power levels allow for a higher material flow, while higher electrical currents expand the arc 8, as the current density in the plasma remains constant. To maintain precision at higher power levels, it is necessary to select a suitable gas with a higher voltage drop, for example, nitrogen or hydrogen instead of argon.

[0049] The process is applied by moving the active electrode 6 with a constricted arc 8 over the workpiece 10 while powdered or wire-like material 11 is fed axially. In particular, the speed of movement of the electrode 6 over the workpiece 10 must be taken into account to ensure optimal material deposition.

[0050] If the movement speed is set too low, material can be deposited on the workpiece 10 until it reaches the electrode 6, causing a defect, for example, a short circuit in the case of conductive material. If, on the other hand, the movement speed is set too high, it will be almost impossible to deposit any more powdered or wire-shaped material 11, and the thickness of a layer 13 of a powdered or wire-shaped material 11 applied over the workpiece 10 will become inhomogeneous. The optimal movement speed also depends on the feed rate of the powdered or wire-shaped material 11.

[0051] If insulating material is to be applied, provided the layer 13 is homogeneous and the capacitance of this layer 13 is known, the arc 8 can be maintained by an alternating current source tuned to the capacitance in order to apply several layers 13 one above the other. The more layers 13 are applied one above the other, the smaller the capacitance becomes, which is why higher frequencies of the alternating current source are necessary.

[0052] If, however, conductive material, such as metal or conductive ceramics, is applied, multiple layers 13 can be stacked on top of each other without using an alternating current source tuned to the capacitance. Since the process allows for comparatively high precision, structures can be manufactured additively. In this additive manufacturing process, material is gradually added at selected locations to form a three-dimensional structure.

[0053] If several layers 13 are placed on top of each other, the current of the arc 8 is conducted through all layers 13. This heat load must be taken into account when designing a structure to be manufactured. Furthermore, the width of the arc 8 is determined by the current and must also be minimized for greater precision. Higher heat outputs at lower currents can again be achieved by choosing the right plasma gas; for example, nitrogen allows a voltage drop of approximately 100 V, in contrast to argon, which causes a voltage drop of approximately 10 V across the arc 8. Since the relationship between power P, voltage U, and current flow I is given by P=U*I, the same power P can be achieved with a higher drop in voltage U and a lower current flow I.

[0054] Higher power and larger currents can be used for surface finishing. Electrodes 6 with a wider diameter can also be used to allow for greater material transport. To apply materials with a high melting point, such as refractory metals, the residence time in the arc 8 can be increased. This can be achieved by increasing the distance between electrode 6 and workpiece 10, thus lengthening the arc 8.

[0055] To ensure that the welding device 1 can even better withstand the power losses of the arc 8, active cooling can also be used. Since the nozzle 2 can generally withstand lower temperatures than the electrode 6, the nozzle 2 can be provided with internal channels for coolant. The electrode 6 can be cooled via contact cooling of the electrode holder. This is preferably made of conductive metal, which is also well suited for heat transfer.

[0056] The velocity of the resulting liquid droplets is also relevant for surface finishing. The velocity of the droplets can be controlled by the flow rate of the working gases 3, 7. It should be noted that the gas increases its velocity due to the rapid heating in the arc 8, providing additional acceleration.

[0057] If the material to be deposited is fed in rod or wire form, or gravity-fed as powder, the additional working gas 7 only needs to be conveyed minimally to protect the material from contaminants and air as it is fed into the arc. However, a gas flow with a high flow velocity can also be used to transport powder with the additional working gas 7, which increases the impact speed of the droplets.

[0058] Should the gas escape from the electrode 6 at the speed of sound or supersonic speed, it should be noted that expansion shock waves may occur at the edge of the electrode 6, which may entrain powdered or wire-like material 11 and thus further distribute it, but may also tear it out of the arc 8. This behavior must be avoided if high precision is desired. To avoid expansion shock waves, the ambient pressure and flow velocity of the surrounding working gas or, in a chamber with a controlled atmosphere, the chamber pressure can be adjusted so that a Prandtl-Meyer angle for the flow conditions is 0. This can be achieved by a suitable shape of the electrode 6, for example a tip in the form of an aero-spike nozzle, directly at the arc 8.

[0059] In practice, particularly precise buildup welding was achieved by keeping the distance between electrode 6 and workpiece 10 at a maximum of 1.5 mm. A flow rate of a maximum of 1000 SCCM for the powder-transporting additional working gas 7 proved to be the preferred flow rate. It was also found that limiting the arc current to a maximum of 20 A enabled a particularly precise welding process.

Claims

1. Method for weld cladding of powdery or wire-like material (11) onto a workpiece (10), which is preferably a flat substrate, by means of a device (1) which comprises a substantially rod-shaped electrode (6), the electrode (6) having at least one material feed channel (9) running in its interior for feeding the powdery or wire-like material (11) into the arc (8), characterised in that the device comprises a nozzle (2) surrounding the electrode (6) and a working gas region which is formed between the electrode (6) and the nozzle (2), wherein the method comprises the following steps: - forming the arc (8) as a transferred arc (8) between the electrode (6) and the workpiece (10) or as a free-standing arc (8) between the electrode (6) and the nozzle (2), - flooding the working gas region with a working gas (3) to constrict the arc (8) in the direction of the workpiece (10), - feeding the powdery or wire-like material (11) into the constricted arc (8), wherein the powdery or wire-like material (11) is melted in said arc (8), and - moving the device (1) over the workpiece (10) while the powdery or wire-like material is fed into the constricted arc, wherein a radial distance between the nozzle (2) and the electrode (6) is not greater than 1 cm and / or an axial distance between the end of the nozzle (2) facing the workpiece and the end of the electrode (6) facing the workpiece (10) is not greater than 1 cm, wherein the end of the nozzle (2) facing the workpiece preferably has a smaller distance to the workpiece than the end of the electrode (6) facing the workpiece (10).

2. The method according to claim 1, characterised in that a further working gas region is formed between the nozzle (2) and a protective atmosphere sheathing (4) surrounding the nozzle (2), which is flooded with a further working gas (5) so that a controlled atmosphere is generated on an application point (12) of the workpiece (10), or so that the device (1) is used in a chamber with a controlled atmosphere.

3. The method according to claim 1 or 2, characterised in that the method is used for fusion welding and for this purpose the powdery or wire-like material (11) is preferably a metal, or the method is used for surface finishing and for this purpose the powdery or wire-like material (11) preferably comprises ceramic, metal or carbide.

4. The method according to one of claims 1 to 3, characterised in that the powdery or wire-like material (11) is fed in an additional working gas (7), which is preferably argon, helium, carbon dioxide or nitrogen, wherein the working gas (3) and / or the further working gas (5) is / are also preferably argon, helium, carbon dioxide or nitrogen.

5. The method according to one of claims 1 to 4, characterised in that the distance between the electrode (6) and the workpiece (10) and / or a position of the electrode (6) above the workpiece (10) is controlled by a mechanical guide.

6. The method according to one of claims 1 to 5, characterised in that the powdery or wire-like material (11) is applied to the workpiece (10) in layers to form superimposed layers of material (13).

7. The method according to one of claims 1 to 6, characterised in that the nozzle (2) has internal channels for receiving cooling liquid and / or the electrode (6) has means for cooling on its holder.

8. The method according to one of claims 1 to 7, characterised in that the opening diameter of the electrode (6) is at most 1 cm, preferably essentially at most 300 µm, and the electrode (6) is preferably tapered at its end facing the workpiece.

9. The method according to one of claims 1 to 8, characterised in that the arc power and the mixing ratios and / or the flow rates of said gases (5, 3, 7) are adjusted in order to adjust the precision and the speed of application of the powdery or wire-like material (11) to the workpiece (10).

10. The method according to one of claims 1 to 9, characterised in that the electrode (6) ends before the material feed channel (9) in the feed direction of the powdery or wire-like material (11) or ends at the same point as the material feed channel (9).

11. The method according to one of claims 1 to 10, characterised in that the workpiece (10) is arranged above the device (1) during weld cladding.