AI Technical Summary
The challenge in producing wood-based materials lies in balancing system speed and raw material efficiency, as excessive binder usage is required for optimal performance, leading to increased costs and potential binder diffusion into the wood, which affects binding effectiveness and manufacturing efficiency.
A binder composition comprising a polymer adhesive, a phase transfer catalyst, and a hydrophilizing agent, specifically a silane compound, is used to control curing speed and prevent binder penetration into the wood, ensuring uniform hardening and reduced binder usage.
This approach allows for targeted and efficient binder application, minimizing diffusion and optimizing manufacturing processes while maintaining product quality, thereby reducing costs and improving production efficiency.
Description
[0001] The invention relates to a binder composition for producing a wood-based material, in particular a board-shaped wood-based material, such as chipboards or wood fiber boards, in particular OSB, HDF or MDF boards, as well as plywood and glued laminated timber, a process for producing such a binder composition, a process for producing such a wood-based material and such a wood-based material.
[0002] A variety of binder compositions, especially glues, are used in the production of wood-based materials. Depending on the application, different binder compositions are favored or particularly suitable. For wood-based panels intended for later use in furniture production or interior design, binder compositions based on urea / formaldehyde have proven particularly suitable.
[0003] For applications where increased air humidity or moisture penetration from adjacent components is to be expected, such as floor coverings, urea-formaldehyde glues, possibly reinforced with melamine, are usually used, whereby the increased requirements are taken into account by an increased amount of the binder compositions.
[0004] For wood-based panels used in areas with high humidity or in direct contact with water, melamine resin-reinforced urea-formaldehyde glues, phenolic resins, or polymeric diphenylmethane diisocyanate (PMDI) have proven suitable. Plywood, particleboard, and OSB (Oriented Strand Board) are particularly suitable for the various applications. Although any binder that is not hydrolyzed by moisture or water can generally be used for the wood-based panels described above, polymeric diphenylmethane diisocyanate (PMDI) has proven particularly suitable for OSB.
[0005] In the production of wood-based materials, the fundamental objectives are not only the most effective use of equipment but also the most effective use of raw materials. These two objectives are often in conflict with one another. For example, in order to achieve the highest possible line speed, a larger amount of binder must be used. However, with an operation that is optimized with regard to the amount of binder, compromises in line speed must be accepted. The general limiting factor is the heat transfer from the press heating plates to the center of the particle or fiber cake. Depending on the operation mode, this conflict of objectives leads to higher fixed costs for the equipment used or to higher material costs. This problem can be somewhat alleviated by using hardeners or aggregates that enable the accelerated introduction of heat into the particle or fiber cake.
[0006] However, it should be noted that, for example, while hardeners allow for faster curing, they can lead to pre-curing of the binder during plant downtime. This is particularly problematic when using polymeric diphenylmethane diisocyanate. This polymer adhesive reacts with many catalysts even at room temperature, which can lead to pre-curing. Accordingly, it is advantageous to use a catalyst that allows for easy curing control and minimizes pre-curing.
[0007] With an appropriate catalyst, the binder composition cures precisely at the desired time. However, this has the disadvantage that the uncured binder remains in contact with the wood material to be bonded for longer during the process and increasingly penetrates it. Studies have shown that absorption or diffusion of the binder into the wood is particularly pronounced when gluing wood material, e.g. with PMDI, and in particular strands for OSB made from softwood. One reason for this is that the hydrophobic PMDI binder in particular is absorbed by the wood surface, which contains more or less fatty acids depending on the season. This means that only part of the binder is available for gluing the strands across the surface, so a large amount of binder is necessary to achieve sufficient bonding.This leads to increased production costs and, in some cases, suboptimal application of the binder. Furthermore, the penetration of the binder into the wood material imposes technological limitations on the equipment to be used and the possible process management.
[0008] US 10 189 178 B2 already discloses a method for producing wood-based panels, in particular OSB wood-based panels, in which wood strands are first provided and then at least one adhesive system is applied to the wood strands, wherein the adhesive system comprises at least one polymer adhesive and at least one nanoparticle smaller than 500 nm. Subsequently, the wood strands mixed with the adhesive system are pressed to form OSB wood-based panels. The nanoparticles are modified with a silane compound to improve the wetting of the strand surface with glue and to improve the adhesion of the glue to the surface. Furthermore, the adhesive system can be produced using an acid or an ammonium salt as a catalyst.
[0009] US 10 119 051 B2 already discloses a binder composition, particularly for wood-based panels, producible from at least one polymer adhesive, at least one polyalcoholic compound, and at least one silane compound specifically modified such that the molecule resulting from the silane compound and the polyalcohol possesses reactive groups that can react with the polymer adhesive or with the OH groups of the wood. These new compounds and the macromolecules formed by condensation with the glue are no longer able to pass through the hydrophobic fatty acid layer of the strands due to the hydrophilic residues. As a result, the present binder composition remains on the surface of the strands or fibers and does not diffuse into the wood matrix.
[0010] The invention is therefore based on the object of providing a binder composition for producing a wood-based material, in particular a board-shaped wood-based material, a method for producing such a wood-based material and such a wood-based material, in which the speed of curing of the binder can be specifically controlled and at the same time diffusion of the binder into the wood material to be bound is prevented as best as possible, thereby enabling a safe, fast and cost-effective production process with the lowest possible binder use without a reduction in product quality.
[0011] The object is achieved according to the invention by a binder composition for producing a wood-based material according to claim 1, by a method for producing a wood-based material according to claim 10, and by a wood-based material according to claim 15. Advantageous developments of the invention are specified in the dependent claims.
[0012] The binder composition according to the invention for producing a wood-based material, in particular a board-shaped wood-based material, such as particle boards or wood fiber boards, in particular OSB, HDF or MDF boards, as well as plywood and glued laminated timber, comprises an organic phase comprising at least one polymer adhesive, an aqueous phase, at least one phase transfer catalyst for accelerating the curing of the polymer adhesive and a hydrophilizing agent comprising or formed from at least one silane compound for increasing the hydrophilicity of the polymer adhesive and / or for reducing the penetration of the polymer adhesive into the material to be bonded, in particular into the particle material to be bonded, of the wood-based material.
[0013] The invention further relates to a process for producing a binder composition according to the invention, comprising at least the steps of providing at least one silane compound, preferably at least two different silane compounds, in particular of the general formulas (I) and / or (II), adding at least one polyalcoholic compound to the at least one silane compound, and preferably adding at least one catalyst, in particular an acid, to the mixture of at least one silane compound and at least one polyalcoholic compound. This is followed by precipitation and / or separation of the reaction mixture comprising the at least one silane compound and the at least one polyalcoholic compound, and adding the phase transfer catalyst.At the same time, or preferably subsequently, at least one polymer adhesive system is then added to the phase-transfer catalyst and / or the separated reaction mixture of the at least one silane compound and the at least one polyalcohol compound. Furthermore, a binder composition according to the invention can also be produced exclusively using a silane compound without a polyalcohol as a reactant, so that no corresponding catalyst is required. In this case, only at least one silane compound as a hydrophilizing agent, a phase-transfer catalyst, and at least one polymer adhesive are mixed together.
[0014] The invention also relates to a method for producing a wood-based material, in particular a board-shaped wood-based material, such as particle boards or wood fiber boards, in particular OSB, HDF or MDF boards, as well as plywood and glued laminated timber, wherein firstly a chip material is produced and / or provided and subsequently a binder composition is added to the chip material, wherein the binder composition has an organic phase comprising at least one polymer adhesive and a second aqueous phase immiscible with the organic phase, a phase transfer catalyst for accelerating the curing of the polymer adhesive and a hydrophilizing agent comprising at least one silane compound for increasing the hydrophilicity of the polymer adhesive and / or for reducing the penetration of the polymer adhesive into the chip material of the wood-based material to be bonded.Finally, the wood-based material is formed from the glued chip material, in particular by pressing it into a panel-shaped wood-based material.
[0015] The wood-based material according to the invention, in particular produced by the process according to the invention, comprises at least one chip material and at least one cured binder composition in at least one layer of the wood-based material, in particular a binder composition according to the invention, wherein the binder composition comprises at least one cured polymer adhesive, a phase transfer catalyst for accelerating the curing of the polymer adhesive and a hydrophilizing agent comprising at least one silane compound for increasing the hydrophilicity of the polymer adhesive and / or for reducing the penetration of the polymer adhesive into the chip material of the wood-based material to be bonded.
[0016] Finally, the invention relates to the use of a binder composition according to this invention with a phase transfer catalyst for producing a wood-based material and preferably in the production of wood chipboards or wood fiber boards, in particular OSB, HDF or MDF boards, as well as plywood and glued laminated timber.
[0017] The inventors have recognized that the use of a phase transfer catalyst in combination with a hydrophilizing agent in a binder composition of a wood-based material makes it possible to specifically control the reactivity and thus the speed of curing and at the same time successfully minimize or even substantially prevent absorption of the binder or penetration of the binder to a greater extent into the wood, so that at the same time the use of a small amount of the binder is possible and a particularly uniform and targeted curing can be achieved.
[0018] In addition, the combination of the hydrophilizing agent with the phase transfer catalyst has the advantage that the heat required for setting or curing reaches the binder particularly evenly, since at least the majority of the binder is located between the chip material and not inside the wood, so that a particularly uniform effect of the catalyst can be achieved.
[0019] A binder composition is understood to be a composition intended for the addition and bonding of wood, and in particular, particle material, to a wood-based material. The binder composition is preferably formed such that a wood-based material can be produced exclusively from the particle material and the binder composition. In principle, however, it is also possible to add additional components to the wood-based material, such as auxiliary materials and fillers. The binder composition can be ready-to-use and / or formed from a single component.
[0020] Alternatively, the binder composition can also be formed from several separately provided components, in particular from two components, which are only brought together and mixed before or during use. In particular, the organic phase can be one component and the aqueous phase the other component, with the phase transfer catalyst and / or the hydrophilizing agent preferably being contained in the aqueous phase. Furthermore, however, it is also conceivable for the hydrophilizing agent and / or the phase transfer catalyst to be provided as a salt or dissolved as a further, in particular third and / or fourth component and / or to be added only upon use. Both the phase transfer catalyst and the hydrophilizing agent can also be produced in situ.The ready-to-use binder composition consisting of one or more already mixed components is often also referred to as glue or resin, and accordingly the application of the binder to the chip material is referred to as gluing.
[0021] Furthermore, it is particularly conceivable that the multiple components of the binder composition only come together on the surface of the wood to be bonded, in particular the chip material, wherein preferably first a first component, in particular an aqueous phase, the phase transfer catalyst and / or the hydrophilizing agent is brought onto the chip material and / or to the chip material and then the organic phase with the at least one polymer adhesive, in particular an isocyanate binder, is added.
[0022] The wood-based material can, in principle, be any material that is predominantly composed, preferably at least 90% apart from the binder composition, of wood, plant fibers, and / or a material made therefrom by bonding several pieces of this material with a binder composition. This is preferably at least one particle material. The wood-based material can, in principle, have any desired shape, with panel-shaped wood-based materials, in particular lignocellulose and / or fiber-containing boards, particle boards, and / or coarse particle boards, being preferred.
[0023] The chip material can in principle comprise any desired plant chips and / or fibers and is preferably formed essentially from plant chips. The chip material is particularly preferably made from wood. Most preferably, the chip material consists of long chips (strands) and / or coarse chips, in particular for producing a coarse chipboard, also known as OSB (oriented strand boards). The wood chips produced or provided for producing a coarse chipboard can have a length between 50 and 200 mm, preferably 70 to 180 mm, particularly preferably 90 to 150 mm; a width between 5 and 50 mm, preferably 10 to 30 mm, particularly preferably 15 to 20 mm; and a thickness between 0.1 and 2 mm, preferably between 0.3 and 1.5 mm, particularly preferably between 0.4 and 1 mm. For chipboards, the chip sizes for the top and / or middle layer are preferably in the range from <1 mm to approximately 30 mm.
[0024] Although the shaping of the wood-based material can in principle be carried out in any desired manner, it is preferably carried out as a continuous process, in particular by scattering the glued chip material onto a conveying device, in particular onto a conveyor belt, and / or by pressing the glued chip material into the wood-based material. The shaping of the wood-based material and in particular the pressing preferably takes place under high pressure and / or at a high temperature, preferably of at least 150°C, more preferably between 170°C and 220°C, and most preferably between 180°C and 220°C.
[0025] Particularly preferably, the glued particle material for producing a coarse particle board is scattered in scattering devices alternately longitudinally and transversely to the production direction, so that the particle material is arranged crosswise, particularly preferably in at least three layers, in particular a lower cover layer, a middle layer, and an upper cover layer. The scattering direction of the lower and upper cover layers is preferably the same and / or differs from the scattering direction of the middle layer.
[0026] The chip material is preferably produced by stripping debarked round wood, preferably softwood, in the longitudinal direction and / or using rotating knives. Furthermore, the produced chip material is preferably dried before adding the binder, in particular to reduce the natural moisture content of the chip material at high temperatures. The moisture content of the chip material after drying is particularly preferably below 10%, and most preferably below 7%, in order to avoid cracks during subsequent pressing and / or to avoid excessive steam formation during pressing.
[0027] The addition of the binder composition to the chip material preferably involves gluing at least a portion, and preferably all, of the chip material as the starting material for the wood-based material. Furthermore, the binder composition is preferably applied in finely distributed form to the chip material. Alternatively, it is conceivable to first apply a first component of the binder composition or to soak the chip material therein and only then apply the second component. The amount of the binder composition, particularly when PMDI is used as the binder, is preferably 1 to 10 wt.%, more preferably 1.5 to 5 wt.%, most preferably 2 to 5 wt.%, and especially preferably 2 to 3 wt.%, based on the total amount of chip material.
[0028] In the wood-based material according to the invention, the binder composition is preferably fully cured after its production, with an isocyanate binder particularly preferably reacting with the water of the aqueous phase to form carbamic acids and / or further to the corresponding amines and / or polyureas. The cured binder composition preferably consists essentially of polyureas, the phase transfer catalyst, and / or other constituents of the organic and / or aqueous phase.
[0029] According to the invention, the binder composition comprises at least one polymer adhesive and preferably at least one isocyanate binder. In this case, the binder composition can in principle, in particular depending on the desired properties of the wood-based material produced, comprise only a single polymer adhesive or a mixture of several polymer adhesives, wherein particularly preferably all polymer adhesives are polyurethane adhesives and / or each comprise at least one isocyanate binder or are based on at least one diisocyanate. The proportion of all binders in the binder composition is preferably between 60% and 100%, particularly preferably at least 85% and very particularly preferably at least 95%. The polymer adhesive and in particular polymeric diphenylmethane diisocyanate is preferably used as a pure binder and / or without further addition of water in the organic phase. The water proportion orthe proportion of the aqueous phase in the binder composition is preferably between 0 and 15%, particularly preferably between 0.01 and 10% and very particularly preferably between 0.5 and 8%.
[0030] According to the invention, the binder composition comprises at least one, preferably precisely one, phase transfer catalyst, although it is also conceivable in principle to use several chemically different phase transfer catalysts simultaneously. The phase transfer catalyst according to the invention fundamentally enables the entry of constituents of the aqueous phase, in particular water itself, into the non-aqueous or organic phase, in particular to the polymer adhesive and / or an isocyanate binder, with water then very particularly preferably being the reactant for curing the binder. Accordingly, the phase transfer catalyst preferably transfers water from the aqueous phase into the organic phase, where a reaction with the polymer adhesive and in particular the isocyanate can take place, and the phase transfer catalyst is subsequently released again.
[0031] Thus, the phase-transfer catalyst accelerates the curing reaction of the binder, but is not itself directly involved in the reaction. Particularly preferably, the phase-transfer catalyst is selected such that it is not involved in activating the isocyanate group of the binder. The phase-transfer catalyst leads to a lower required reaction temperature and / or a shorter reaction time and also enables good control of the reaction kinetics. There is preferably a linear relationship between the gel time or curing time and the amount of phase-transfer catalyst used.
[0032] The hydrophilizing agent is essentially a substance or a mixture of substances that influences the hydrophilic properties of the binder, particularly increasing its hydrophilicity. For this purpose, the hydrophilizing agent preferably has at least one hydrophilic region and at least one hydrophobic region, with the hydrophobic region furthermore preferably interacting directly with the binder composition and / or with the polymer adhesive contained therein.
[0033] The hydrophilizing agent can be a pure single substance or a mixture of substances, whereby the hydrophilizing agent can in particular be a mixture of various substances formed by a reaction. The reaction of at least one silane compound and at least one polyalcohol initially produces a compound or reaction mixture which is highly hydrophilic due to the large number of OH groups in the polyalcohol on one side of the molecule. On the other hand, the molecule produced from the silane compound and the polyalcohol has reactive groups due to the specifically modified silane, which can react with the polymer adhesive, such as PMDI glue, or with the OH groups of the wood. These new compounds and the macromolecules formed by condensation with the polymer adhesive or glue are no longer able to pass through the hydrophobic fatty acid layer of the chip material due to the hydrophilic residues.As a result, the binder composition remains on the surface of the particle material or fibers and does not diffuse into the wood matrix. Accordingly, the hydrophilizing agent acts preferentially by providing the polymer adhesive with a hydrophilic anchor. However, as an alternative to a reaction product, a silane or a silane compound, and especially a suitably modified silane compound, can also be used as the hydrophilizing agent.
[0034] To control the reaction of the at least one silane compound with the at least one polyalcohol, a catalyst is preferably added. Particularly suitable catalysts are inorganic and / or organic acids, which are particularly preferably selected from a group consisting of phosphoric acid, acetic acid, p-toluenesulfonic acid, hydrochloric acid, formic acid, or sulfuric acid. Ammonium salts such as ammonium sulfate, which react as weak acids, are also suitable. However, p-toluenesulfonic acid is particularly preferred.
[0035] The use of sodium glycerophosphate has proven particularly suitable for precipitating the reaction mixture from at least one silane compound, and in particular at least one compound of formula (I) and / or (II), and at least one polyalcoholic compound. Other suitable precipitating agents include alkalis such as NaOH, KOH, or ammonium hydroxide solutions. The precipitating agent is preferably added to the reaction mixture together with water. In this way, the reaction product is concentrated in the aqueous phase and separated from the hydrolysis products, such as ethanol.
[0036] Although in principle at least any phase-transfer catalyst can be used, in an advantageous embodiment of the binder composition, the phase-transfer catalyst comprises an onium ion and preferably an ammonium, phosphonium, and / or sulfonium ion, and is particularly preferably triethylbenzylammonium chloride. In addition, at least one phase-transfer catalyst can also be a crown ether, in particular 12-crown-4.
[0037] In a preferred embodiment of the binder composition according to the invention, the polymer adhesive is exclusively a polyurethane adhesive based on an isocyanate binder, preferably based on aromatic polyisocyanates, in particular polydiphenylmethane diisocyanate (PMDI), tolylene diisocyanate (TDI), and / or diphenylmethane diisocyanate (MDI). A polymeric diphenylmethane diisocyanate is particularly preferred. The sole polymer adhesive is particularly preferably a polyurethane adhesive based on a polymeric diphenylmethane diisocyanate. In general, the content of polymer adhesive in the binder composition is preferably at least 70% by weight, more preferably at least 80% by weight, and most preferably at least 95% by weight.
[0038] In a likewise preferred embodiment of the binder composition according to the invention, it is also possible to use more than one polymer adhesive. Thus, in principle, several polyaddition adhesives, such as an epoxy resin, polycyanurate, and / or polyurethane adhesive, in particular a polyurethane adhesive based on polydiphenylmethane diisocyanate (PMDI), can be used, with all polymer adhesives particularly preferably being based on at least one diisocyanate.
[0039] The hydrophilizing agent preferably comprises at least one polyalcohol, and in particular, the hydrophilizing agent is formed by a reaction of the at least one silane compound with at least one polyalcohol. The at least one polyalcohol of the hydrophilizing agent is preferably selected from a group comprising tetravalent, pentavalent, hexavalent alditols, or a higher-valent alcohol with more than six hydroxyl groups as a polyalcoholic compound. The use of n-polyglycols and n-polyvinyl alcohols as the polyalcohol is also conceivable in principle. The amount of the polyalcoholic compound in the binder composition is preferably between 5 and 50 wt.%, particularly preferably between 10 and 30 wt.%, and most particularly preferably between 5 and 10 wt.%, based on the total amount of the binder composition.
[0040] A particularly preferred embodiment of the binder composition according to the invention further provides that at least one alditol is selected from a group containing threitol, erythritol, and pentaerythritol as tetrahydric alcohols; arabitol, adonitol, and xylitol as pentahydric alcohols; and sorbitol, mannitol, dulcitol, and dipentaerythritol as hexahydric alcohols. Alditols are also known as reduced sugars. Higher-valent alcohols with more than six hydroxyl groups, such as seven or eight hydroxyl groups, can also be used. Suitable polyglycols include polyethylene or polypropylene glycols. However, the use of sorbitol has proven particularly advantageous.
[0041] A particularly preferred embodiment of the binder composition according to the invention provides that the at least one silane compound is a compound of the general formula (I) R a SiX (4-a) (I), or of the general formula (II) O b X c (OH) d R e SiO(4-bcde) / 2 (II), where X is H, OH or a hydrolyzable radical selected from the group comprising halogen, alkoxy, carboxy, amino, monoalkylamino or dialkylamino, aryloxy, acyloxy, alkylcarbonyl, R is a non-hydrolyzable organic radical R is selected from the group comprising substituted and unsubstituted alkyl, substituted and unsubstituted aryl, substituted and unsubstituted alkenyl, substituted and unsubstituted alkynyl, substituted and unsubstituted cycloalkyl, which may be interrupted by -O- or -NH-, and wherein R may have at least one functional group Q which is selected from a group containing an epoxide, hydroxyl, ether, amino, monoalkylamino, dialkylamino, substituted and unsubstituted anilino, amide, carboxy, alkynyl, acryloyl, acryloyloxy, Methacrylic, methacryloxy, mercapto, cyano, alkoxy, isocyanato, aldehyde, alkylcarbonyl, acid anhydride and / or phosphoric acid group,R and X may each be the same or different from each other, and a = 0, 1, 2, 3, in particular 0 or 1, b, c, d = 0 or 1, and e = 1, 2, 3. ,
[0042] The silane-containing compounds of general formula (II) are derived directly as hydrolysis and / or condensation products from the silane compounds of general formula (I). The hydrolysis and / or condensation of the compounds of general formula (I) is determined and influenced in particular by the reaction conditions, especially acidic reaction conditions, during binder production.
[0043] In the silane compounds of formula (I), the radical X is advantageously selected from a group containing fluorine, chlorine, bromine, iodine, C 1-6 alkoxy, in particular methoxy, ethoxy, n-propoxy and butoxy, C 6 -C 10 aryloxy, in particular phenoxy, C 2 -C 7 acyloxy, in particular acetoxy or propionoxy, C 2 -C 7 alkylcarbonyl, in particular acetyl, monoalkylamino or dialkylamino with C 1 -C 12 , in particular C 1 -C 6 . Particularly preferred hydrolyzable groups are C 1 -C 4 alkoxy groups, in particular methoxy and ethoxy.
[0044] The silane compound preferably has a non-hydrolyzable organic radical R. The term "non-hydrolyzable organic radical" in the context of the present invention refers to an organic radical which, in the presence of water, does not lead to the formation of an OH group or NH2 group linked to the Si atom. The non-hydrolyzable radical R is preferably selected from a group comprising substituted and unsubstituted C 1 -C 30 alkyl, in particular C 5 -C 25 alkyl, substituted and unsubstituted C 2 -C 6 alkenyl, substituted and unsubstituted C 2 -C 6 alkynyl, and substituted and unsubstituted C 6 -C 10 aryl. Preferably, the non-hydrolyzable radical R is selected from the group containing methyl, ethyl, n-propyl, isopropyl, n-butyl, s-butyl, t-butyl, pentyl, hexyl, cyclohexyl, vinyl, 1-propenyl, 2-propenyl, butenyl, acetylenyl, propargyl, phenyl and naphthyl.
[0045] The non-hydrolyzable radical R can have at least one functional group Q. Furthermore, the radical R can also be substituted by other radicals. In one variant, the at least one functional group Q is selected from a group containing epoxy, hydroxy, ether, acryloyl, acryloxy, methacryloyl, methacryloxy, amino, alkoxy, cyano, and / or isocyano groups. In a further variant, the at least one functional group Q contained in the organic non-hydrolyzable radical R advantageously comprises an epoxy, in particular a glycidyl or glycidyloxy group, an alkoxy, an amino, or an isocyano group.
[0046] The functional groups through which crosslinking between the polymer adhesive and the wood surface is possible include, in particular, polymerizable and / or polycondensable groups, whereby the polymerization reaction also includes polyaddition reactions. The functional groups are preferably selected such that organic crosslinking between the polymer adhesive and the wood surface, and possibly also between different adhesive systems, can be achieved via optionally catalyzed polymerization and / or condensation reactions.
[0047] In a particularly preferred embodiment, tetraethoxysilane, methyltriethoxysilane, gamma-isocyanatopropyltriethoxysilane or a glycidyloxypropyltriethoxysilane are used as silanes.
[0048] The term "substituted", when used with "alkyl", "alkenyl", "aryl", etc., denotes the substitution of one or more atoms, usually H atoms, by one or more of the following substituents, preferably by one or two of the following substituents: halogen, hydroxy, protected hydroxy, oxo, protected oxo, C 3 -C 7 cycloalkyl, bicyclic alkyl, phenyl, naphthyl, amino, protected amino, monosubstituted amino, protected monosubstituted amino, disubstituted amino, guanidino, protected guanidino, a heterocyclic ring, a substituted heterocyclic ring, imidazolyl, indolyl, pyrrolidinyl, C 1 -C 12 alkoxy, C 1 -C 12 acyl, C 1 -C 12 acyloxy, acryloyloxy, nitro, carboxy, protected Carboxy, carbamoyl, cyano, methylsulfonylamino, thiol, C 1 -C 10 alkylthio and C 1 -C 10 alkylsulfonyl.The substituted alkyl groups, aryl groups, alkenyl groups can be substituted once or multiple times, preferably once or twice, with the same or different substituents.
[0049] The term "alkynyl," as used herein, refers to a radical of the formula RC=C-, in particular a "C"-C6-alkynyl." Examples of C2-C6-alkynyls include: ethynyl, propynyl, 2-butynyl, 2-pentynyl, 3-pentynyl, 2-hexynyl, 3-hexynyl, 4-hexynyl, vinyl, and di- and tri-ynes of straight and branched alkyl chains. The term "aryl," as used herein, refers to aromatic hydrocarbons, for example, phenyl, benzyl, naphthyl, or anthryl. Substituted aryl groups are aryl groups which, as defined above, are substituted with one or more substituents as defined above. The term "cycloalkyl" includes the groups cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and cycloheptyl.
[0050] In a preferred embodiment, the present binder composition comprises at least two silane compounds and particularly preferably two different compounds of the general formula (I) and / or (II). A binder composition is preferred in which a first compound corresponds to the formula SiX 4 with X being OH or alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and a second compound corresponds to the formula R a SiX (4-a) with a = 1 or 2, where X is OH or alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, R is methyl, ethyl, n-propyl or n-butyl and Q is a glycidyl or glycidyloxy group, an alkoxy, an amine or an isocyano group. The molar ratio of the first and second compounds can be 0.1 to 1 mol, preferably 0.1 to 0.5 mol, particularly preferably 0.1 to 0.4 mol.
[0051] Furthermore, it is preferred that the amount of reaction mixture comprising at least one silane compound, in particular of formula (I) and / or (II), and the at least one polyalcoholic compound is preferably 1 to 20 wt.%, particularly preferably 2 to 15 wt.%, and very particularly preferably 3 to 10 wt.%, based on the amount of polymer adhesive. The content of the silane compound, the hydrophilizing agent, and / or the phase-transfer catalyst is preferably in each case between 1 to 30 wt.%, particularly preferably 5 to 20 wt.%, and very particularly preferably between 10 to 20 wt.%. However, these figures do not initially take into account the solvent content of the polymer adhesive used.
[0052] A particularly preferred variant of the present binder composition comprises tetraethylorthosilicate, glycidyloxypropyltriethoxysilane, sorbitol, triethylbenzylammonium chloride as phase transfer catalyst and PMDI glue as polymer adhesive.
[0053] An advantageous development of the method according to the invention for producing a wood-based material provides that the binder composition is added to the particle material in the form of two separate components of the binder composition, one component being an organic phase containing the polymer adhesive, and the other component being at least one aqueous phase containing the phase-transfer catalyst and / or the hydrophilizing agent. Alternatively, the phase-transfer catalyst and / or the hydrophilizing agent are preferably added together with paraffin, with particular preference being given to premixing the phase-transfer catalyst and / or the hydrophilizing agent with the paraffin.The application of the aqueous phase and / or the paraffin with the phase transfer catalyst and / or the hydrophilizing agent to the chip material is particularly preferably carried out via nozzles or atomizers in a mixer or is sprayed onto the chip material in the coil.
[0054] In a further preferred embodiment of the method according to the invention for producing a wood-based material, the phase transfer catalyst and / or the hydrophilizing agent is added directly to the chip material to be bonded and / or not first to the organic phase comprising the polymer adhesive, so that, for example, pre-reactions can be particularly effectively avoided during a plant shutdown.
[0055] Although the production of a single-layer wood-based material is also conceivable, the wood-based material is preferably constructed from at least two different layers and / or from a lower cover layer, a middle layer, and an upper cover layer, wherein at least one of the layers, preferably the middle layer, comprises a binder composition with a phase transfer catalyst and a hydrophilizing agent, and at least one further layer comprises a binder composition with no or a lower concentration of the phase transfer catalyst and / or the hydrophilizing agent. The two cover layers preferably have an identical binder composition and / or an identical amount of binder. Particularly preferably, both cover layers are formed identically to one another.Furthermore, the concentration of the phase transfer catalyst and / or the hydrophilizing agent in the cover layer preferably corresponds to between 25% and 75%, preferably between 40% and 60% and particularly preferably between 45% and 55% of the concentration in the middle layer.
[0056] The content of the binder composition in the wood-based panel, in particular an OSB wood-based panel, is preferably between 0.5 and 5.0 wt%, particularly preferably between 1.5 and 4.0 wt%, and very particularly preferably between 2.0 and 3.0 wt%, based on the total amount of wood fibers or chip material. In a preferred embodiment, the binder composition is sprayed onto the wood chips, the chip material, or the wood fibers.
[0057] The invention is explained in more detail below using exemplary embodiments. Example 1:
[0058] In a plant for producing OSB with three layers, a middle layer and two outer skin layers, the strand material for a middle layer in coils was sprayed with a 12.5% solution of Inosil GS 55 as a silane compound and a 20% solution of TEBA (triethylbenzylammonium chloride) as a phase-transfer catalyst. The amount of Inosil GS 55 was 0.04 wt% based on dry wood, and the amount of TEBA was 1.0 wt% based on dry wood.
[0059] Subsequently, the strands of the middle layer were sprayed with 2.0 wt% PMDI (polymeric diphenylmethane diisocyanate) as a polymer adhesive and 1 wt% paraffin. An 18 mm OSB was then produced from the middle layer strands and the top layer strands, which had been sprayed with 2.9 wt% PMDI and 1.0 wt% paraffin in a coil. The ratio of top layer to middle layer was equal.
[0060] The OSB plant was operated at a speed of 450 mm / sec and at typical pressures (200-500 N / cm²) and temperatures (210-250 °C). The OSB produced with the described parameters meets all requirements of the standards applicable to this product.
[0061] However, when OSB was produced without Inosil GS 55 and TEBA under otherwise identical conditions, and in particular, using the same amount of polymer adhesive and at the same speed, cracking occurred, so the product quality had to be assessed as unsatisfactory. When OSB was produced with either Inosil GS 55 or TEBA in the above-mentioned amounts, OSB was obtained, but its transverse tensile strength was inadequate, below 0.3 N / mm². The elastic moduli (longitudinal and transverse) of the boards were also below the standard requirements. Example 2:
[0062] In a plant for producing OSB with three layers, a core layer and two outer skin layers, the strands for a core layer in coils were sprayed with a 12.5% solution of Inosil GS 55 and a 20% solution of TEBA (triethylbenzylammonium chloride). The amount of Inosil GS 55 was 0.04 wt% based on dry wood and 1.0 wt% of TEBA based on dry wood. The strands were further sprayed with 2.0 wt% PMDI and 1 wt% paraffin.
[0063] The strands for the top layer were sprayed in the coil with a 12.5% solution of Inosil GS 55 and a 20% solution of TEBA (triethylbenzylammonium chloride). The amount of Inosil GS 55 was 0.04 wt% based on dry wood and 0.5 wt% of TEBA based on dry wood. The strands were further sprayed with 2.5 wt% PMDI and 1 wt% paraffin.
[0064] An 18 mm OSB was then produced from the core and face layer strands. The ratio of face layer to core layer was equal. The OSB plant was operated at a speed of 470 mm / sec and at typical pressures (200-500 N / cm²) and temperatures (210-250 °C). The OSB produced with the described parameters meets all requirements of the standards applicable to this product.
[0065] When producing OSB without Inosil GS 55 and without TEBA in the top and middle layers under otherwise identical conditions, and in particular, with the same amount of polymer adhesive and at the same speed, cracking again occurred. When producing OSB with either Inosil GS 55 or TEBA in the above-mentioned amounts, OSB was obtained, but again had insufficient transverse tensile strengths below 0.3 N / mm². The elastic moduli (longitudinal and transverse) of the boards were also again below the standard requirements.
[0066] The binder composition according to the invention thus enables effective system utilization, with performance increases of up to approximately 30% possible. Furthermore, the amount of polymer adhesive used can be kept low.
Claims
1. Binder composition for the manufacture of a wood-based material, comprising an organic phase having at least one polymer adhesive, an aqueous phase a phase transfer catalyst to accelerate the curing of the polymer adhesive and a hydrophilizing agent comprising at least one silane compound for increasing the hydrophilicity of the polymer adhesive and / or for reducing the penetration of the polymer adhesive into the material of the wood-based material to be bonded.
2. Binder composition for the manufacture of a wood-based material according to claim 1, characterized in that the phase transfer catalyst has an onium ion and preferably an ammonium, phosphonium and / or sulfonium ion and is particularly preferably triethylbenzyl ammonium chloride.
3. Binder composition for the manufacture of a wood-based material according to claim 1 or 2, characterized in that the phase transfer catalyst is a crown ether, in particular 12-crown-4.
4. Binder composition for the manufacture of a wood-based material according to at least one of the preceding claims, characterized in that all polymer adhesives of the organic phase are exclusively polyurethane adhesives.
5. Binder composition for manufacturing a wood-based material according to at least one of the preceding claims, characterized in that the sole polymer adhesive is a polyurethane adhesive based on a polymeric diphenylmethane diisocyanate.
6. Binder composition for the manufacture of a wood-based material according to at least one of the preceding claims, characterized in that the hydrophilizing agent comprises at least one polyalcohol selected from a group containing tetravalent, pentavalent, hexavalent alditols or a higher-valent alcohol having more than six hydroxy groups as a polyalcoholic compound.
7. Binder composition for the manufacture of a wood-based material according to claim 6, characterized in that at least one alditol is selected from a group comprising as tetravalent alcohols threitol, erythritol, pentaerythritol, as pentavalent alcohols arabitol, adonitol, xylitol and as hexavalent alcohols sorbitol, mannitol, dulcitol, dipentaerythritol.
8. Binder composition for the manufacture of a wood-based material according to at least one of the preceding claims, characterized in that the at least one silane compound is a compound of the general formula (I) Ra SiX(4-a) (I), or the general formula (II) Ob Xc (OH)d Re SiO(4-b-c-d-e) / 2 (II), wherein - X is H, OH or a hydrolyzable group selected from the group consisting of halogen, alkoxy, carboxy, amino, monoalkylamino or dialkylamino, aryloxy, acyloxy, alkylcarbonyl, - R is a non-hydrolyzable organic group R selected from the group consisting of substituted and unsubstituted alkyl, substituted and unsubstituted aryl, substituted and unsubstituted alkenyl, substituted and unsubstituted alkynyl, substituted and unsubstituted cycloalkyl, which may be interrupted by -O- or -NH-, and wherein - R may have at least one functional group Q selected from a group consisting of an epoxide, hydroxy, ether, amino, monoalkylamino, dialkylamino, substituted and unsubstituted anilino, amide, carboxy, alkynyl, acrylic, acryloxy, methacrylic, methacryloxy, mercapto amide, carboxy, alkynyl, acrylic, acryloxy, methacrylic, methacryloxy, mercapto, cyano, alkoxy, isocyanato, aldehyde, alkylcarbonyl, acid anhydride and / or phosphoric acid group, - R and X can be the same or different from each other, and - a = 0, 1, 2, 3, in particular 0 or 1, - b, c, d = 0 or 1, and - e =1,2,3.
9. Method of manufacturing a binder composition according to any one of claims 1 - 8, comprising the steps of: - providing at least one silane compound, - addition of at least one polyalcoholic compound, - preferably addition of at least one catalyst, in particular an acid, to the mixture of at least one silane compound and at least one polyalcoholic compound, - precipitating and / or separating the reaction mixture of the at least one silane compound and the at least one polyalcoholic compound, - addition of the phase transfer catalyst, and - addition of at least one polymer adhesive system to the phase transfer catalyst and / or the separated reaction mixture of the at least one silane compound and the at least one polyalcoholic compound.
10. Method for manufacturing a wood-based material, comprising the steps of: manufacturing and / or providimg a chip material, adding a binder composition to the chip material, the binder composition comprising an organic phase having at least one polymer adhesive and a second aqueous phase immiscible with the organic phase, a phase transfer catalyst for accelerating the curing of the polymer adhesive and a hydrophilizing agent comprising at least one silane compound for increasing the hydrophilicity of the polymer adhesive and / or for reducing the ingress of the polymer adhesive into the chip material of the wood-based material to be bonded, and forming the wood-based material from the glued chip material, in particular pressing it into a board-shaped wood-based material.
11. Method for manufacturing a wood-based material according to claim 10, characterized in that the addition of the binder composition to the chip material is carried out in the form of an addition of two separate components of the binder composition, wherein one component is an organic phase having the polymer adhesive and the other component is at least one aqueous phase containing the phase transfer catalyst and / or the hydrophilizing agent.
12. Method for manufacturing a wood-based material according to claim 10 or 11, characterized in that the phase transfer catalyst and / or the hydrophilizing agent is added directly to the chip material to be bonded and / or is not first added to the organic phase having the polymer adhesive.
13. Method for manufacturing a wood-based material according to at least one of the preceding claims 10 - 13, characterized in that the wood-based material is formed from at least two layers differing from one another and / or from a lower surface layer, a core layer and an upper surface layer, at least one of the layers, preferably the core layer, having a binder composition with a phase transfer catalyst and a hydrophilizing agent and at least one further layer having a binder composition without or with a lower concentration of the phase transfer catalyst and / or the hydrophilizing agent.
14. Method for manufacturing a wood-based material according to claim 13, characterized in that the two surface layers have an identical binder composition and / or an identical amount of binder and / or the concentration of the phase transfer catalyst and / or the hydrophilizing agent in the surface layer corresponds to between 25% and 75%, preferably between 40% and 60% and particularly preferably between 45% and 55% of the concentration in the core layer.
15. A wood-based material, in particular manufactured by a method according to at least one of claims 10 - 14, having at least one chip material and at least one cured binder composition in at least one layer of the wood-based material, in particular a binder composition according to at least one of claims 1-8, wherein the binder composition has at least one cured polymer adhesive, a phase transfer catalyst for accelerating the curing of the polymer adhesive and a hydrophilizing agent comprising at least one silane compound for increasing the hydrophilicity of the polymer adhesive and / or for reducing the penetration of the polymer adhesive into the chip material of the wood-based material to be bonded.