COMPOSITE DISC WITH IMPROVED COLOR EFFECT

DE502022002079D1Active Publication Date: 2024-11-28SAINT GOBAIN SEKURIT FRANCE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502022002079
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-28
Filing Date
2022-01-12
Publication Date
2024-11-28
Estimated Expiration
2042-01-12

AI Technical Summary

Technical Problem

Existing composite panes for vehicles face challenges in achieving optimal transparency and color neutrality in reflection, particularly with the use of conductive coatings that can reduce transmission and introduce undesirable color tones, while also being cost-intensive and limited in adjustability.

Method used

A composite pane design featuring a thermoplastic intermediate layer with refractive index-lowering agents, reducing the refractive index by at least 0.05, combined with a functional film containing metal layers, which maintains transparency and mechanical properties while improving the color impression in reflection.

Benefits of technology

The solution achieves an improved aesthetic appearance with reduced undesirable color tones in reflection, maintaining or enhancing transparency and mechanical properties, and allowing for better adjustability of the color effect without increasing costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a composite pane with improved optical properties, in particular an improved color effect in reflection, and to a method for producing such a composite pane and its use.

[0002] Laminated glass panes consist of two or more individual panes, bonded together using one or more interlayers under heat and pressure. The interlayers are usually made of thermoplastics such as polyvinyl butyral (PVB) or ethylene vinyl acetate (EVA).

[0003] High demands are placed on the glazing of motor vehicles. The following legal regulations apply to the size of the viewing area and the structural stability of the windows: ECE R 43: "Uniform provisions concerning the approval of safety glass and laminated glass materials" as well as technical requirements for vehicle components in type approval § 22a StVZO, "Safety glass".

[0004] These regulations are generally met by laminated glass panes. Thermoplastic films, particularly polyvinyl butyral (PVB) films, have been used in the manufacture of laminated glass panes. These films have a refractive index as close as possible to that of the outer and inner panes. The refractive index of the PVB films used to date is typically approximately 1.48 in the visible range, which is usually specified at a fixed value, for example, 500 or 550 nm. (DC Miller, Optical Engineering 50(1), 013003, 2011).

[0005] It is known to provide windshields with transparent, functional films, for example, with electrically conductive coatings. These coatings can, for example, act as IR-reflective coatings to reduce heating of the vehicle interior and thereby improve thermal comfort. However, the coatings can also fulfill other functions and, for example, be used as heatable coatings by connecting them to a voltage source so that a current flows through the coating. Suitable coatings include, for example, conductive, metallic layers based on silver. Since these layers are susceptible to corrosion, it is common practice to apply them to the surface of the outer pane or the inner pane facing the intermediate layer, so that they have no contact with the atmosphere. So-called low-E coatings are also applied to the inner surface of the inner pane.Silver-containing transparent coatings are known, for example, from WO 03 / 024155, US2007 / 0082219 A1, US2007 / 0020465 A1, WO2013 / 104438 or WO2013 / 14439.

[0006] WO2019 / 206493 A1 describes a composite pane with an electrically conductive coating and an anti-reflection coating as a projection surface for a head-up display.

[0007] WO2012 / 052315 describes a transparent composite pane with an electrically heatable coating, in which at least one electrically heatable coating comprises at least four functional layers arranged one above the other. Each functional layer comprises at least one layer of optically highly refractive material with a refractive index ≥ 2.1. The functional layer comprises several silver-containing layers and matching and smoothing layers arranged between them. The transparent pane has a total transmittance of > 70%.

[0008] DE 202019102388 U1 describes a composite pane comprising a transparent, electrically conductive coating that additionally has a dielectric superlattice. The superlattice is preferably formed from alternating layers with different refractive indices and consists of a plurality of individual layers, with layers with a high refractive index (preferably greater than 1.8 at a wavelength of 550 nm) and layers with a low refractive index (preferably less than 1.8 at a wavelength of 550 nm) being arranged alternately one above the other. The superlattice reduces transmission in the spectral range from 400 nm to 500 nm. The region with the superlattice is located outside the central viewing area of ​​the composite pane, so that the reduction in transmission has no negative effects on the vehicle occupants, particularly with regard to overall transmission and any color cast.

[0009] When using functional films in laminated glass, the specialist must consider a wide range of requirements when designing the coatings, particularly in vehicle construction. The conductive layers of the functional films, which typically contain metal, reduce transmission in the visible spectral range. A higher amount of conductive material in the individual layers can also result in a reduction in the transparency of the laminated glass. Since a windshield, for example, must meet strict minimum transparency requirements (at least 70% transmission in the visible spectral range according to Regulation 43 of the United Nations Economic Commission for Europe (ECE R 43)), there are limits to the amount of conductive material and the number of layers for the functional films.

[0010] In addition to transparency, the reflection spectrum of the laminated pane and other boundary conditions must also be considered. This particularly applies to the color effect of the laminated pane, as generally only panes with a green-blue color are desirable, not yellow or red (relative to the reflection color).

[0011] The higher the number of conductive layers, the better the coating can usually be optimized with regard to the desired transmittance, color, or sheet resistance. However, coatings as functional films, especially with multiple precious metal layers, are comparatively expensive and limited in their adjustability to the desired color impression in combination with the necessary transparency. Therefore, alternatives are being sought to optimize the color effect of a composite pane designed with one or more functional films.

[0012] The object of the present invention is therefore to provide a transparent composite pane with at least one functional film, wherein, at the same time as the function provided by this film, an improved aesthetic appearance can be achieved, in particular as free as possible from undesirable color tones in the reflection of the composite pane.

[0013] The object of the present invention is achieved by a composite pane according to claim 1. Preferred embodiments are evident from the subclaims.

[0014] According to the invention, a composite pane is provided, comprising an outer pane and an inner pane which are connected to one another via a thermoplastic intermediate layer, wherein the composite pane has at least one functional film which contains at least one metal layer, in particular a transparent metal layer, and the thermoplastic intermediate layer is formed with at least one thermoplastic film which contains refractive index-lowering agents and by means of these refractive index-lowering agents the refractive index of the thermoplastic film in the optically visible range between 380 nm - 780 nm is reduced by at least 0.05 (n Δ -0.05).

[0015] In other words, according to the invention, the intermediate layer of the composite pane is formed from at least one thermoplastic film whose refractive index is reduced by at least 0.05 (n Δ -0.05) by refractive index-lowering agents compared to the refractive index n of a thermoplastic film with a comparable composition but without the refractive index-lowering agents used according to the invention. At the same time, the other properties, for example optical or mechanical properties of the films and the resulting composite pane, such as the required transparency, light transmission, breaking strength / pummel value or processability, are essentially retained. As a result, the composite pane according to the invention surprisingly has an improved color impression in reflection without any other properties of the composite pane being negatively affected.

[0016] The composite pane according to the invention comprises an outer pane and an inner pane, which are connected to one another via a thermoplastic intermediate layer. The composite pane is intended to separate the interior space from the exterior environment in a window opening, in particular the window opening of a vehicle. For the purposes of the invention, the "inner pane" refers to the pane of the composite pane facing the interior space (in particular the vehicle interior). The "outer pane" refers to the pane of the composite pane facing the exterior environment. The composite pane is preferably a vehicle windshield (in particular the windshield of a motor vehicle, for example a passenger car or truck), a side window, or a roof window.

[0017] As a windshield, the composite pane has an upper edge and a lower edge as well as two side edges running in between. The upper edge is the edge that is intended to point upwards when installed. The lower edge is the edge that is intended to point downwards when installed. The upper edge is often referred to as the roof edge and the lower edge as the engine edge. The outer pane and the inner pane each have an outside surface and an inside surface and a circumferential side edge running in between. For the purposes of the invention, the outside surface refers to the main surface that is intended to face the outside environment when installed. For the purposes of the invention, the inside surface refers to the main surface that is intended to face the interior when installed.The interior surface of the outer pane and the exterior surface of the inner pane face each other and are connected by the thermoplastic intermediate layer.

[0018] The surfaces of the panes are typically designated as follows: The outside of the outer pane is designated as Side I. The inside of the outer pane is designated as Side II. The outside of the inner pane is designated as Side III. The inside of the inner pane is designated as Side IV.

[0019] The outer pane and the inner pane are preferably formed independently of one another from glass or plastic, preferably soda-lime glass, alkali aluminosilicate glass, polycarbonate, or polymethyl methacrylate. In a particularly preferred embodiment, the outer pane and the inner pane are made of glass.

[0020] The outer pane and the inner pane are preferably not mechanically prestressed, but in further embodiments they can be thermally prestressed or partially prestressed or chemically prestressed.

[0021] Suitable glass sheets include glass sheets known under the trade names Planiclear ®< and Planilux ®< (each clear glass), VG 10, VG 20, VG 40 or TSANx, TSA3+, TSA4+ from Saint-Gobain, where the VG series are grey tinted glasses and the TSA series are green tinted glasses.

[0022] The outer and / or the inner pane preferably has, independently of one another, a thickness of 0.1 to 4 mm, preferably of 1 to 4 mm, particularly preferably of 1.6 mm to about 2.1 mm.

[0023] The composite pane according to the invention also comprises at least one functional film, preferably a transparent functional film, containing at least one metal layer. According to the invention, this functional film contains at least one metal or metal alloy, for example, silver, aluminum, copper, palladium, platinum, or gold, and is preferably based on the metal or metal alloy, i.e., it consists essentially of the metal or metal alloy, excluding any doping or impurities.

[0024] The functional film is applied, for example, to the outer surface of the inner pane facing the intermediate layer (side III) or to the interior surface of the outer pane facing the intermediate layer (side II). Alternatively, the functional film can be arranged as a coating within the intermediate layer. For this purpose, the functional film can also be applied to a carrier film, for example made of polyethylene terephthalate (PET) with a thickness of approximately 20 µm to 100 µm, for example 50 µm, which is arranged between two layers of thermoplastic material, for example between two polymer films, such as PVB films.

[0025] A transparent functional film is understood to be a layer or layer system (coating) that has an average transmission in the visible spectral range of at least 70%, preferably at least 75%, which therefore does not significantly restrict visibility through the window and yet provides or enables functions such as reflection for a HUD display or IR radiation reflection for a sun protection coating. The functional film can also be designed as a heatable coating that is electrically contacted and heats up when a current flows through it. The transmission in the visible spectral range is determined according to the method for testing the light transmittance of motor vehicle windows specified in ECE-R 43, Annex 3, Section 9.1.

[0026] In a further embodiment of the composite pane according to the invention, the functional film comprises, as a transparent metal layer, at least one silver layer, one aluminum layer, one copper layer, one palladium layer, one platinum layer, or one gold layer. According to the invention, the at least one metal layer is preferably a silver layer. Silver has emerged as a preferred metal for the metallic layer because it has a relatively neutral color effect and, for example, when used as a sun protection layer, selectively reflects infrared radiation outside the visible range of solar radiation.

[0027] In another preferred embodiment of the composite pane, the functional film comprises two to four metal layers, preferably two, three, or four silver layers. For example, layer systems for sun protection layers with two silver functional layers, but also three or four silver functional layers, are used, since their efficiency—i.e., the reflection of infrared radiation outside the visible range relative to the transmission of visible radiation—is greater. Furthermore, the adjustability of certain properties, such as the color effect, is more variable with a larger number of layers.

[0028] The metallic layers, preferably silver layers, are typically embedded between dielectric layers in the functional films. In other words, the metal layers are sandwiched between dielectric layers.

[0029] The dielectric layers of the functional film may contain suitable materials known to those skilled in the art, for example at least one metal oxide such as ZnO, ZnSnOx, or a metal nitride such as Si 3 N 4 , or SiZrNx, or NiCr. The dielectric materials may also contain dopants such as aluminum.

[0030] Each metal layer, for example a silver layer, is preferably arranged between two dielectric layers. The metal layers and the dielectric layers are arranged such that, for example, at least one dielectric layer, preferably two or more dielectric layers, is arranged between each two adjacent silver layers between which no further silver layer is arranged, and that at least one further dielectric layer is arranged above the uppermost metal layer, which faces the outer pane in the installed position, and that at least one further dielectric layer is arranged below the lowermost metal layer, which faces the inner pane. According to the invention, the dielectric layers preferably have a thickness of 0.1 nm to 100 nm, particularly preferably of 0.2 nm to 50 nm, for example between 0.3 nm and 45 nm.

[0031] The functional film according to the invention can be applied, for example, as a coating by physical vapor deposition (PVD) by cathode sputtering, particularly preferably by magnetic field-assisted cathode sputtering, for example, to the inner pane. The functional films are preferably applied to the panes as coatings prior to lamination. Instead of applying the coating to a pane surface, it can in principle also be provided on a carrier film arranged in the intermediate layer.This can be achieved, for example, by positioning the functional film between at least two thermoplastic polymer films during the production of the laminated pane. The polymer films are then fused together by the action of heat, for example, during lamination, and the thermoplastic material of the films surrounds and encloses the IR-reflecting film. This protects the functional film from environmental influences.

[0032] In a further embodiment of the composite pane, the refractive index of the thermoplastic film is reduced by the refractive index-lowering agents contained therein to between 0.05 and 0.15 in the optically visible range (380 nm - 780 nm). By reducing the refractive index of the thermoplastic film, an improved aesthetic appearance of the composite pane can be achieved according to the invention, in particular one that is as free as possible from undesirable color tones in reflection. It has been shown that with a greater reduction in the refractive index of the thermoplastic film, the color effect can also be influenced more strongly toward the desired color neutrality, or toward the reduction or avoidance of undesirable yellow and red tones of the composite pane.

[0033] In a preferred embodiment of the invention, the refractive index-lowering agents are nanoparticles that have a refractive index of <1.4, preferably <1.3, in the optically visible range at a wavelength of 550 nm. This means that the stated refractive index values ​​are measured at a wavelength of 550 nm. The refractive index can be determined, for example, using ellipsometry. Ellipsometers are commercially available.

[0034] In a further preferred embodiment, the refractive index-lowering agents are, contain, or comprise metal fluoride nanoparticles, in particular MgF 2 , CaF 2 , or hollow SiO 2 nanoparticles. Alkali metal fluorides with a refractive index < 1.4 and methods for producing alkali metal fluorides, for example, the aforementioned MgF 2 and CaF 2 , are described, for example, in K. Scheurell, Inorganics 6, 128, 2018. The alternatively mentioned hollow SiO 2 nanoparticles are disclosed, for example, in M. Gorsd, Procedia Materials Science 8, 567-576, 2015 and in T. Gao, Appl. Phys. A 110, 65-70, 2013.

[0035] In a further embodiment of the invention, the thermoplastic film contains at least 1 wt.% of refractive index-lowering agents, in particular nanoparticles, based on the total weight of the film in the volume of the thermoplastic film. Preferably, 0.5-50 wt.%; preferably 1 to 25 wt.%, 1-10 wt.%, for example up to 5 wt.% of refractive index-lowering agents, in particular nanoparticles, based on the total weight of the film, are contained in the volume of the thermoplastic film.

[0036] According to the invention, the refractive index-lowering agents are preferably nanoparticles with an average diameter of 5 nm to 200 nm. The particles have an average particle diameter of 5 nm to 200 nm, preferably <150 nm, particularly preferably <100 nm, for example <90 nm, <80 nm, <70 nm, or <50 nm. The particle size distribution is preferably as homogeneous as possible, i.e., the particles used have as nearly the same diameter as possible. For the purposes of the invention, particles with an average diameter of less than or equal to 500 nm are referred to as nanoparticles. Nanoparticle sizes can be measured using dynamic light scattering (DLS).

[0037] In a further embodiment of the composite pane according to the invention, the thermoplastic film is a polyvinyl butyral (PVB) film, an ethylene-vinyl acetate (EVA) film, or a polyurethane (PU) film, preferably a PVB film. In other words, the thermoplastic films according to the invention are designed as thermoplastic polymer films containing polyvinyl butyral (PVB), ethylene-vinyl acetate (EVA), or polyurethane, and / or mixtures and / or copolymers thereof. Polyvinyl butyral is particularly preferred. The thermoplastic films are preferably based on the materials mentioned, but may contain further components, for example, plasticizers. The polymer film types mentioned are particularly well suited for the automotive sector.

[0038] Advantageously, it is possible to incorporate the refractive index-lowering agents, in particular nanoscale particles, into such polymer films without negatively affecting the films' other properties, such as mechanical ones. The thermoplastic films can be standard films with a refractive index reduced by at least 0.05 in the optically visible range between 380 nm and 780 nm due to the refractive index-lowering agents. The thermoplastic films can be clear, colored / tinted (for example, in the case of a roof panel), with a colored band, or can be configured individually or in combination with other special properties or functions. The thermoplastic films can, for example, be wedge films for use as a projection surface for a head-up display or acoustic films.

[0039] The thermoplastic film of the laminated glass pane according to the invention preferably has a thickness of at least 0.1 mm to a maximum of 2 mm, preferably 0.2 mm to 1 mm, particularly preferably 0.3 mm to 0.8 mm. Polymer films of the intermediate layer, in particular the PVB films, have, for example, a thickness of 0.38 mm, 0.76 mm, or 0.81 mm. Further properties of the laminated glass pane can be influenced by the thickness of the films. For example, thicker PVB films result in improved sound absorption, especially if they contain an acoustically effective core, increased burglary resistance of the laminated glass pane, and also increased protection against ultraviolet radiation (UV protection).

[0040] In another preferred embodiment of the composite pane, the intermediate layer is formed from two or more thermoplastic films that have different refractive indices. The optical properties, in particular the color effect in the reflection from the outside and inside, can thereby be further advantageously influenced and optimized to the desired values ​​for the composite pane.

[0041] Furthermore, the invention comprises a method for producing a composite pane according to the invention as described above in various embodiments, comprising the steps: S1: Providing a thermoplastic film containing refractive index-lowering agents; S2: Providing a functional film on the outer pane, the inner pane, the thermoplastic film, and / or on a carrier film; S3: Forming a stacking sequence of outer pane, inner pane, and the thermoplastic film, as well as optionally the carrier film; S4: Connecting the stacking sequence under the influence of pressure, heat, and / or vacuum.

[0042] The thermoplastic films can be produced in step 1 using methods known per se. In a preferred embodiment, the films are manufactured with the refractive index-lowering nanoparticles, which have a refractive index of <1.4, preferably <1.3, in the optically visible range. In other words, the nanoparticles are dispersed throughout the volume of the films. The films with the nanoparticles dispersed therein can be manufactured, for example, in a manner analogous to the methods described in JP 2002326846 A, US2003 / 0054160 A1, or EP1227070 B1.

[0043] Advantageously, it is possible to incorporate refractive index-lowering agents, particularly nanoscale particles, into such polymer films without negatively affecting the films' other properties, such as mechanical ones. The thermoplastic films can be standard films, for example, PVB films, supplemented with the refractive index-lowering agents according to the invention, which reduce the film's refractive index by at least 0.05 in the optically visible range (380 nm - 780 nm). The thermoplastic films can be clear, colored / tinted, with a color band, or can also be designed with other special properties or functions, individually or in combination. The thermoplastic films can be, for example, wedge films for use as a projection surface for a head-up display or acoustic films.

[0044] In a further preferred embodiment, it is provided that the refractive index-lowering agents contain or comprise metal fluoride nanoparticles, in particular MgF 2 , CaF 2 , or hollow SiO 2 nanoparticles.

[0045] In step S2, the functional film can be applied to the inner pane or the outer pane, for example, by physical vapor deposition (PVD), sputtering, or magnetic field-assisted sputtering. The functional films are preferably applied to the inner side II of the outer pane or the outer side III of the inner pane. The coatings are preferably applied to the panes before lamination.

[0046] Preferably, at least 80% of the pane surface is coated with the functional film. In particular, the laminated pane is coated over its entire surface, with the exception of a peripheral edge area and, optionally, a local area serving as communication, sensor, or camera windows intended to ensure the transmission of electromagnetic radiation through the laminated pane and therefore not coated. The peripheral uncoated edge area can, for example, have a width of up to 20 cm. This prevents direct contact of the coating with the surrounding atmosphere, thus advantageously protecting the coating inside the laminated pane from corrosion and damage.

[0047] Instead of applying the functional films as a coating to a pane surface, they can also be provided on a carrier film, for example made of polyethylene terephthalate (PET), which is arranged in the intermediate layer. This can be achieved, for example, by positioning the functional film between at least two thermoplastic polymer films in step S3 of the composite pane.

[0048] In step S3, the outer pane, inner pane and the thermoplastic film as well as, if applicable, the carrier film are arranged flat on top of each other in the usual way.

[0049] If the composite pane is to be bent, the outer pane and the inner pane are preferably subjected to a bending process before step S4 and preferably after any coating processes in step S2. Preferably, the outer pane and the inner pane are bent congruently together (i.e., simultaneously and using the same tool), as this ensures that the shape of the panes is optimally matched for subsequent lamination. Typical temperatures for glass bending processes are, for example, 500°C to 700°C.

[0050] The bonding of the outer pane and the inner pane via the thermoplastic intermediate layer from the stacking sequence to form the composite pane in step S4 is preferably carried out by lamination under the influence of heat, vacuum, and / or pressure. Known methods for producing a composite pane can be used. During lamination, the heated, flowable thermoplastic material flows around the functional film, creating a stable composite. The solar control coating is encapsulated in the intermediate layer and protected from damage and environmental influences.

[0051] For example, so-called autoclave processes can be carried out at an elevated pressure of approximately 10 to 15 bar and temperatures of 130°C to 145°C for approximately 2 hours. Conventional vacuum bag or vacuum ring processes, for example, operate at approximately 200 mbar and temperatures of 80°C to 110°C. The outer pane, the thermoplastic intermediate layer, and the inner pane can also be pressed into a pane in a calender between at least one pair of rollers. Systems of this type are known for the production of panes and usually have at least one heating tunnel upstream of a pressing unit. The temperature during the pressing process can range, for example, from 40°C to 150°C. Combinations of calender and autoclave processes have proven particularly successful in practice. Alternatively, vacuum laminators can be used.These consist of one or more heatable and evacuatable chambers in which the panes are laminated within, for example, about 60 minutes at reduced pressures of 0.01 mbar to 800 mbar and temperatures of 80°C to 170°C.

[0052] In a preferred embodiment of the method, the thermoplastic film (4B) provided in step S1 is formed with metal fluoride nanoparticles, in particular MgF2, CaF2, or hollow SiO2 nanoparticles, as refractive index-lowering agents. Nanoparticles can be integrated into the films using conventional methods without adversely affecting other properties.

[0053] In another embodiment of the method, two or more thermoplastic films (4B, 4, 4A) with different refractive indices are used in step S1. In other words, an intermediate layer is formed from two or more thermoplastic films with different refractive indices. The optical properties, in particular the color effect in the reflection from the outer and inner sides of the composite pane, can thereby be further advantageously influenced and optimized to the desired values ​​for the composite pane.

[0054] The invention further comprises the use of the composite pane according to the invention in means of transport for traffic on land, in the air or on water, in particular in motor vehicles, for example as a windscreen, rear window, side window and / or roof window.

[0055] All standards mentioned refer to the version valid on the date of filing.

[0056] The various embodiments of the invention can be implemented individually or in any combination. In particular, the features mentioned above and those to be explained below can be used not only in the specified combinations, but also in other combinations or on their own, without departing from the scope of the invention. Unless embodiments and / or their features are explicitly mentioned only as alternatives or are mutually exclusive.

[0057] The invention is presented in more detail below with reference to the examples and figures. It should be noted that different aspects are described, each of which can be used individually or in combination. This means that any aspect can be used with different embodiments of the invention, unless explicitly presented as a mere alternative.

[0058] The drawings are simplified, schematic representations and not to scale. The drawings do not limit the invention in any way. Examples

[0059] Table 1 ClimaCoat ®< with 4 silver layers laminate Standard PVB1 refractive index 1.48 PVB2 With low refractive index (Δ -0.05) PVB3 with ultra-low refractive index (Δ-0.13) TL (A) 71.7% 71.6% 71.4% a* 8° -7.6 -7.7 -7.7 b* 8° -10.7 -9.4 -7.8 a* 60° +0.9 -0.2 -1.4 b* 60° -5.3 -4.3 -3.2

[0060] Table 1 compares the integral values ​​for a laminated pane with a sheet resistance of approximately 0.7 ohms, using a standard PVB available under the trade name ClimaCoat® from Saint Gobain, with the values ​​for identically constructed and comparable laminated panes, but with a PVB with a low refractive index (0.05 lower than the standard PVB) and a PVB with an ultra-low refractive index (0.13 lower than the standard PVB). The reflection values ​​are determined by simulations using a common optical simulation program.

[0061] The specified color values ​​describe the reflection color of the respective laminated pane and are related to the L* a* b* color space (also: Lab color space), which is standardized in EN ISO 11664-4 "Colorimetry -- Part 4: CIE 1976 L* a* b* Color space" and the more recent DIN EN 410. The specified color values ​​a* , b* refer at least to the external reflection color under irradiation with the light source D65 and angles of incidence of 8° and 60° (angle to the surface normal), measured when the outer pane is irradiated with radiation of mixed polarization (50% s, 50% p) and measurement conditions specified in the aforementioned standards as D65 / 10.

[0062] It can be seen that the external reflection at 8° becomes less blue with the increasing reduction in the refractive index and less red at 60°. The difference compared to the color values ​​of the laminated pane with the standard PVB film is more than one point in each case and can therefore be considered a significant improvement. The observable trend toward color neutrality with the reduction in the refractive index of the PVB film suggests that a further reduction in the refractive index of the PVB film used could further enhance this effect of the improved color effect in the reflection of the laminated pane. Table 1-1 Layer structure for the composite panes from Table 1 with 4 metal layers Composite pane with functional film with 4 silver layers Layer thickness Outer pane1 Clear glass pane Planiclear ®< PLC 2.1 mm Thermoplastic film 4 Standard PVB1 4A (state of the art) or 0.737 mm PVB2 with reduced refractive index n(Δ -0.05) 4B (according to the invention) or Thermoplastic film 4 PVB3 with reduced refractive index n(Δ -0.13) 4B (according to the invention) Si3N4 15.8 nm SiZrNx 8.1 nm Functional Film 5 ZnO 13 nm NiCr 0.2 nm Ag [metal layer 6] 10.9 nm ZnO 12.0 nm ZnSnOx 10.0 nm SiZrNx 21.1 nm Si3N4 20.9 nm ZnO 16.0 nm NiCr 0.2 nm Ag [metal layer 6] 14.2 nm ZnO 14.0 nm ZnSnOx 11.0 nm SiZrNx 18.4 nm Si3N4 17.2 nm ZnO 15.0 nm NiCr 0.3 nm Ag [metal layer 6] 13.5 nm ZnO 16.0 nm ZnSnOx 10.0 nm SiZrNx 35.5 nm ZnO 16 nm NiCr 0.2 nm Ag [metal layer 6] 11.5 nm ZnO 11.0 nm ZnSnOx 8.0 nm SiZrNx 13.7 nm Inner pane 2 Clear glass pane Planiclear ®< PLC 1.6 mm

[0063] Table 1-1 shows the layer structures for the three composite panes with four silver layers, the values ​​of which were determined by simulation, whereby the layer sequence and the layer thicknesses are retained and the difference lies only in the different refractive index of the PVB1 (standard / reference n at 500 nm 1.48) and the PVB2 (n (Δ -0.05) and the PVB3 (n (Δ -0.13)) used for the composite pane. Table 2 ClimaCoat ®< with 3 silver layers laminate Standard PVB1 PVB2. With low refractive index (n Δ -0.05) TL (A) 72.4% 72.7% a* 8° -2.5 -1,3 b* 8° -2.9 -3,1 a* 60° +0.1 -0.2 b* 60° 5.0 5.0

[0064] Table 2 compares the integral values ​​for a laminated pane with a sheet resistance of approximately 0.9 ohms, using a standard PVB available under the trade name ClimaCoat® from Saint Gobain, and for similarly constructed and comparable laminated panes, but with a PVB with a low refractive index (0.05 lower than the standard PVB). The simulation shows the same trends in the reflection values ​​as in the simulation measurements shown in Table 1, although less pronounced. Table 2-1 Layer structure for the composite panes from Table 2 Composite pane with functional film with 3 silver layers Layer thickness Outer pane1 Clear glass pane Planiclear ®< PLC 2.1 mm Standard PVB1 4A (state of the art) or Thermoplastic film 4 PVB2 with reduced refractive index n (Δ -0.05) 4B (according to the invention) 0.76 mm Functional Film 5 SiZrNx 9.6 nm Si3N4 9.9 nm ZnO 13 nm NiCr 0.2 nm Ag [metal layer 6] 9.0 nm ZnO 14.0 nm ZnSnOx 7.0 nm SiZrNx 21.5 nm Functional Film 5 Si3N4 25.5 nm ZnO 10.0 nm NiCr 0.3 nm Ag [metal layer 6] 9.5 nm ZnO 9.0 nm ZnSnOx 8.0 nm SiZrNx 42.1 nm ZnO 13 nm NiCr 0.2 nm Ag [metal layer 6] 9.5 nm ZnO 13 nm ZnSnOx 7.0 nm SiZrNx 10.9 nm Inner pane 2 Clear glass pane Planiclear ®< PLC 1.6 mm

[0065] Table 2-1 shows the layer structures for the two composite panes with three silver layers, whereby the layer sequence and the layer thicknesses are retained and the difference lies only in the different refractive index of the PVB1 (standard / reference n at 500 nm 1.48) and the PVB2 (n (Δ -0.05)) used for the composite pane. Table 3 Layer structure of the HUD composite window laminate HUD composite laminate Standard PVB1 refractive index n 1.48 at 500 nm PVB2 with low refractive index (Δ -0.05) TL (A) 71.9% 71.5% at -1,5 -1.3 b*t 0.6 0.9 RL(A) 22.9 23.4 a* 8° -0.5 -1.1 b* 8° 1.8 1.0 RL(A) 60° 28.0 28.1 a* 60° -0.6 -1.1 b* 60° 1.1 0.5 RL(A) p-pol 20.1 20.1 a* p-pol 0.6 0.4 b* p-pol 1.1 0.3 TTS 59.7 59.7 Polarization ratio 1.405 1.412

[0066] Table 3 compares the integral values ​​for a HUD-compatible laminated glass (HUD laminated glass) with a silver layer (with a standard PVB (PVB1)) to a similarly constructed and comparable laminated glass, but with a PVB with a low refractive index n. In PVB2, n is lower by 0.05 compared to PVB1 (n Δ -0.05).

[0067] The layer structure for the composite glazing laminates, which was investigated using a simulation with an optical simulation program, is shown in Figure 1 and the corresponding description.

[0068] This simulation also shows a significant effect on the color effect of the laminated pane in reflection, with almost constant light transmission TL(A) and an identical TTS value (total transmission of solar energy). The reflection color at 8° and 60° is shifted into the green range by the PVB film with the reduced refractive index. The HUD p-pol reflection color also becomes more color-neutral with the PVB with the reduced refractive index. This means that a disturbing color shift can be reduced or avoided during HUD projection. The closer the color values ​​a* and b* are to zero, the more color-neutral the color effect in reflection. Surprisingly, when comparing the two HUD laminated panes with the PVB with the reduced refractive index, a 0.007 increase in the polarization ratio (p-polarization / s-polarization) was also observed.This ratio should be as high as possible for the functionality of camera systems integrated in the windshield.

[0069] The values ​​shown in Tables 1 to 3 were obtained by simulation using an optical simulation program.

[0070] They mean: RL(A) Visible external reflection [%] External reflectivity describes the reflected portion of the visible radiation incident from the external environment. TL(A) Visible light transmission [%] of the laminated panes TTS Total transmitted thermal radiation [%] RL(A) 60° visible reflection at a viewing angle of 60° [%] RL(A) p-pole visible p-pole reflection [%] L*, a*, b* Color coordinates (CIE color space, International Commission on Illumination) The values ​​for light transmission (TL) and reflection (RL) refer to light type A, i.e. the visible part of sunlight at a wavelength of 380 nm to 780 nm.

[0071] They show: Figure 1 a schematic cross-section through a layer structure for a composite pane according to the invention using the example of a HUD-compatible composite pane laminate (HUD composite pane / HUD laminate); Figure 2 a diagram of the refractive index n and wavelength for PVB films with different reduced refractive index Figure 3 the colour values ​​a* b* of the laminated panes from Table 1 with the thermoplastic films PVB1, PVB 2 and PVB 3 in a colour diagram.

[0072] Figure 1shows a schematic cross-section through a layer structure 10 for a composite pane 100 according to the invention, using the example of a HUD laminate, as investigated with the optical simulation program. The values ​​for the comparative optically simulated measurements, once for a composite pane 100 with a clear standard PVB film 4A (prior art) and once with a clear PVB film 4B with a reduced refractive index n according to the invention, are shown in Table 3. The layer structure 10 for the composite pane 100 comprises an outer pane 1, an inner pane 2, and an intermediate layer 3.In the example used as the basis for the optical simulation (Table 3), the inner pane 2 and the outer pane 1 are 2.1 mm thick clear glass panes that are available, for example, under the trade name Planiclear®. The intermediate layer 3 comprises a thermoplastic film 4 (4A prior art / 4B according to the invention with reduced refractive index n); in the comparative examples from Table 3, a PVB film 4A (PVB1 standard / state of the art) and PVB film 4B (PVB2 / with reduced refractive index) with a thickness of 0.76 mm. On the outer side III of the inner pane 2, facing the thermoplastic film 4 (4A / 4B), a multilayer, functional film 5 with a transparent silver layer 6 is arranged in the intermediate layer 3. The functional film 5 of the example composite wafers 100 comprises a silver layer 6 with a thickness of 12.5 nm and further dielectric layers (5a, 5b, 5c, 5d, 5e, 5f).The layer structure for the optical simulations from Table 3 is shown in detail in Table 4. The functional film 5 can be applied to the inner pane, for example, by conventional methods such as sputtering. It has been shown that the composite panes 100 according to the invention exhibit a significant, positive effect on the color effect in reflection at virtually identical transmission values ​​TL(A). The reflection color of the composite pane 100 is shifted into the green range by the PVB film 4B according to the invention (Table 3, PVB2) with the reduced refractive index n. The HUD p-pol reflection color also becomes more color-neutral with the PVB film 4B (PVB2) with the reduced refractive index n.This means that with the composite pane 100 manufactured according to the invention using the PVB film 4B with the reduced refractive index n, a disturbing color shift in a HUD projection can be reduced or avoided compared to the prior art (use of the standard PVB film 4A). The closer the color values ​​a* and b* are to zero, the more color-neutral the color effect is in reflection. Surprisingly, when comparing the two HUD composite pane laminates 100 using the PVB2 4B with the reduced refractive index, a polarization ratio (p-polarization) increased by 0.007 was also observed. Table 4 Structure of a composite pane 100 using the example of a HUD composite pane with a silver layer compared with a PVB1 (4A) and a PVB2 (4B) as thermoplastic film 4 (4A / 4B) HUD composite window Layer thickness Outer pane1 Clear glass pane Planiclear ®< PLC 2.1 mm Thermoplastic film 4 Standard PVB1 4A (state of the art) or 0.76 mm PVB2 with reduced refractive index 4B (according to the invention) Functional Film 5 Si3N4 50 nm SiZrNx 10 nm ZnO 10 nm NiCr 0.3 nm Ag [metal layer 6] 12.5 nm ZnO 10.0 nm SiZrNx 10.0 nm Si3N4 10.0 nm Inner pane 2 Clear glass pane Planiclear ®< PLC 2.1 mm

[0073] Figure 2shows a diagram of the refractive index n and wavelength for four PVB films with different reduced refractive indices. Simulations were performed with PVB1 (standard / reference refractive index at 500 nm approximately 1.48), PVB 2 (refractive index at 500 nm approximately 1.43; Δ -0.05), and PVB 3 (refractive index at 500 nm approximately 1.35; Δ -0.13), which yielded the values ​​presented in Tables 1 to 3. PVB 4, another PVB film with a refractive index at 500 nm of approximately 1.39, is graphically represented.

[0074] Figure 3 shows the color values ​​a* and b* of the laminated panes 100 from Table 1 determined with the optical simulation program with the different thermoplastic films PVB1 (standard / reference), PVB 2 (refractive index Δ -0.05) and PVB 3 (refractive index at 500 nm n Δ -0.13) in a color coordinate diagram a*b*.

[0075] It can be seen that the external reflection at 8° is less blue with the increasing reduction of the refractive index and less red at 60°. The trend toward color neutrality with the reduction of the refractive index of the PVB film 4, represented by the arrows X (reflection values ​​at 8°) and Y (reflection values ​​at 60°), suggests that a further reduction in the refractive index n of the PVB film used could further enhance this effect of improved color in the reflection of the laminated pane 100.

[0076] The composite pane according to the invention has surprisingly good optical and aesthetic properties, whereby in particular undesirable color tones in the reflection of the composite pane can be minimized or even avoided.

[0077] This is possible according to the invention without negatively affecting other properties of the composite pane.

[0078] According to the invention, laminated panes with an improved color impression in reflection are provided. Advantageously, the improved color effect and the resulting improved aesthetic visual impression can be achieved without negatively affecting other properties of the laminated pane. List of reference symbols

[0079] 100Laminated pane 10Layer structure 1Outer pane 2Inner pane 3Intermediate layer 4Thermoplastic film 4AStandard PVB film (state of the art) 4BPVB film 4B (PVB2 / with reduced refractive index according to the invention) 5Functional film 5a, 5b, 5c, 5d, 5e, 5fDielectric layers 6Metal layer IOuter surface of outer pane 1 IIInner surface of outer pane 1 IIIOuter surface of inner pane 2 IVInner surface of inner pane 2 XTendency of reflection values ​​at 8° with decreasing refractive index of the PVB YTendency of reflection values ​​at 60° with decreasing refractive index of the PVB

Claims

1. Laminated pane (100) comprising an outer pane (1) and an inner pane (2) which are connected to one another via a thermoplastic intermediate layer (3), characterized in that the laminated pane (100) has at least one functional film (5) which contains at least one metal layer (6), and the thermoplastic intermediate layer (3) has at least one thermoplastic film (4B) which contains refractive index-reducing media and the refractive index of the thermoplastic film (4B) is reduced by at least 0.05 in the optically visible range between 380 nm - 780 nm by means of these refractive index-reducing media.

2. Laminated pane according to claim 1, characterized in that the functional film (5) comprises, as a metal layer (6), at least one silver layer, aluminum layer, copper layer, palladium layer, platinum layer or a gold layer.

3. Laminated pane according to either claim 1 or 2, characterized in that the functional film (5) has two to four metal layers (6), preferably 2, 3 or 4 silver layers.

4. Laminated pane according to any of claims 1 to 3, characterized in that the functional film (5) comprises at least two dielectric layers (5a, 5b, 5c, 5d, 5d, 5e) which embed the metal layers (6) in a sandwich-like manner.

5. Laminated pane according to any of claims 1 to 4, characterized in that the refractive index of the thermoplastic film (4B) is reduced in the optically visible range between 0.05 and 0.15 by means of the refractive index-reducing media contained therein.

6. Laminated pane according to any of claims 1 to 5, characterized in that the refractive index-reducing media are nanoparticles which have a refractive index n <1.4, preferably <1.3, in the optically visible range.

7. Laminated pane according to any of claims 1 to 6, characterized in that the refractive index-reducing media are, contain or comprise metal fluoride nanoparticles, in particular MgF2, CaF2, or hollow SiO2 nanoparticles.

8. Laminated pane according to any of claims 1 to 7, characterized in that the thermoplastic film (4B) contains at least 1 wt.% refractive index-reducing media, in particular nanoparticles, based on the total weight in the volume of the thermoplastic film.

9. Laminated pane according to any of claims 1 to 8, characterized in that the refractive index-reducing media are nanoparticles with an average diameter of 5 nm to 200 nm.

10. Laminated pane according to any of claims 1 to 9, characterized in that the thermoplastic film (4B) is a polyvinyl butyral (PVB) film, an ethylene vinyl acetate (EVA) film or a polyurethane (PU) film, preferably a PVB film.

11. Laminated pane according to any of claims 1 to 10, characterized in that the thermoplastic film (4B) has a thickness of at least 0.1 mm to a maximum of 2 mm, preferably 0.2 mm to 1 mm, particularly preferably 0.3 mm to 0.8 mm.

12. Laminated pane according to any of claims 1 to 11, characterized in that the intermediate layer (3) is formed from two or more thermoplastic films (4B) which have a different refractive index from each other.

13. Method for producing a laminated pane (100) according to any of claims 1 to 12, comprising the steps of: S1: providing at least one thermoplastic film (4B) containing refractive index-reducing media; S2: providing a functional film (5) on the outer pane (1), the inner pane (2), on the thermoplastic film (4B) and / or on a carrier film; S3: forming a stacking sequence from the outer pane (1), inner pane (2) and the thermoplastic film (4B) and, if applicable, the carrier film; S4: connecting the stacking sequence under the influence of pressure, heat and / or vacuum.

14. Method according to claim 13, characterized in that in step S1, the thermoplastic film (4B) contains metal fluoride nanoparticles, in particular MgF2, CaF2, or hollow SiO2 nanoparticles, as refractive index-reducing media.

15. Method according to either claim 13 or 14, characterized in that in step S1, two or more thermoplastic films (4B,4) are used which have a different refractive index.