Multi-layered plastic sleeve with a porous food contact side, suitable for transferring food additives

DE502022002171D1Active Publication Date: 2024-12-05KALLE & CO AKTIENGESELLSCHAFT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502022002171
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-04
Filing Date
2022-09-28
Publication Date
2024-12-05
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Existing food casings with non-polar polyolefinic layers face issues with adhesion to polar media, inefficient absorption and transfer of polar food additives, and uneven coating due to low affinity and permeability, leading to poor absorption and desorption efficiency and a blotchy appearance.

Method used

A coextruded, tubular, seamless food casing with at least three layers, including a porous layer composed of aliphatic copolyamides and hydrophilic polymers, using chemical blowing agents to create porosity and biaxial stretching for enhanced mechanical strength and absorption capabilities, ensuring efficient absorption, storage, and transfer of food additives.

Benefits of technology

The solution enables rapid, uniform, and efficient absorption and transfer of food additives, improving the mechanical strength and appearance of the casing, with high porosity and effective water vapor barrier properties, resulting in a more even and effective coating of food additives.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a coextruded, multilayer, water vapor-impermeable, tubular, and seamless food casing with one or more porous layers, which is capable of efficiently absorbing, storing, and transferring food additives to a product in contact with the inner surface. It also relates to a method for producing the casing and its use as food packaging.

[0002] A multilayer food casing with at least one porous layer is known in the prior art. WO 2017 / 148682 A1 describes a tubular, coextruded film consisting of three "layer stacks." The inner "layer stack" consists of several adjacent layers, each consisting of a foamed polymer of the polyolefin type. The inner layers are always based on polyolefin, specifically at least one olefinic polymer, copolymer, or terpolymer, in particular from the group consisting of LDPE, LLDPE, VLDPE, and mixtures thereof, especially copolymers and terpolymers with C3-C10 alpha-olefins or alkyl (meth)acrylates. The outer stack consists of several layers, each of the polyamide type. An adhesion-promoting layer is located between these layer stacks. The cavities, open cells, or pores in the layers of the "inner stack" are created during coextrusion by adding a foaming agent.Chemical foaming agents, especially alkali (bi)carbonates and citric acid, are preferred. The inner side of the film is capable of releasing or transferring food additives.

[0003] EP 3 014 997 A1 discloses a multilayer food casing with a porous layer. The prior art describes a coextruded food casing with at least the following three layers: at least one inner porous layer, at least one barrier layer (ie a layer with a barrier effect for water vapor and / or oxygen), at least one adhesive layer, wherein the porosity of the first-mentioned layer is created by (co)extruding a polymer composition and a supercritical pore former. The porous layer is capable of absorbing, retaining, desorbing, and transferring at least one functional (food) additive to the encased food. Various gases in the supercritical state are defined as supercritical pore formers. Preferred are carbon dioxide (CO 2 ) and nitrogen (N 2 The porous layer itself preferably contains an organic polymer, particularly preferably a polymer from the groups (co)polyamides, polyolefins, vinyl copolymers, vinylidene copolymers, and (co)polyesters. The supercritical pore former is introduced into the layer-forming polymer via one or more inlet openings on the extruder; preferably via an extruder section with a plurality of radially distributed injection nozzles. Also preferred is a process embodiment with the inlet opening(s) arranged above a mixing section of the extruder, where its screw contains multiply perforated screw blades.

[0004] EP 1 911 352 A1 describes a coextruded, multilayer stretched casing with a porous inner layer. The inner layer preferably contains at least one plastic component and at least one agent that supports the formation of pores or pore channels during stretching. Preferably, the inner layer additionally contains a (liquid) emulsifier and a fine-grained organic and / or inorganic filler. Furthermore, a mineral oil is preferred as a component of the inner layer. The plastic component is typically an organic thermoplastic polymer; this is preferably selected from the group consisting of aliphatic or partially aromatic (co)polyamides, polyolefins, polyurethanes, vinyl polymers, vinylidene chloride (co)polymers, and (co)polyesters. The porous layer is also capable of absorbing, retaining, desorbing, and transferring at least one functional (food) additive to the encased food.

[0005] DE 10 2008 017920 A1 similarly describes a casing capable of retaining a liquid containing coloring and / or flavoring on the inside. The inner layer is not porous, but rather has a relief-like design. The relief elements are specified in terms of length and volume. Example 6 describes a 5-layer casing in which a combination of polyamide 6 and a blowing agent superconcentrate (a masterbatch with substances that release gases when heated) was used for the inner layer.

[0006] Finally, WO 2005 / 097461 A1 discloses a coextruded, at least two-layer casing with an outer layer having a porosity of at least 5 vol.% and a roughness depth R z of at least 5.0 µm. The surface of the outer layer has open pores and / or pores with crater-like protruding edges. These pores create a matte appearance on the outside of the casing, which can be designed very similar to that of hide fiber casing, fiber-reinforced cellulose casing, or natural casing. In one embodiment, the surface structure of the outer layer is produced by physical or chemical foaming of a plastic melt. Chemical foaming using substances that release gas when heated (e.g., sodium bicarbonate) is preferred.

[0007] The polymers known from WO 2017 / 148682 A1 are consistently very nonpolar or hydrophobic and therefore exhibit very low affinity for polar media such as a protein-containing meat emulsion. When such emulsions are heated in casings, no adhesion develops between the coagulated meat surface and the casing. Consequently, water contained in the emulsion can separate at the interface between the meat and casing (so-called "purge" or jelly deposit).

[0008] A further disadvantage caused by the nonpolarity of polyolefin layer materials is their low permeability to polar media. During the absorption and desorption of typical, water-containing, polar food additives (liquid smoke, dyes, and flavors) or their formulations, transport between the cavities can only occur to the extent that the cavities communicate with each other (i.e., through channels or similar) and are connected to each other. The migration of water or polar substances between isolated cavities, i.e., through the matrix, occurs extremely slowly. Therefore, of the cavities in the "layer package," only those located directly on the inner surface of the shell or connected via "channels" to cavities on the inner surface are used for absorption and desorption. The transfer function of the shell is therefore inefficient.

[0009] Finally, the non-polarity of the polyolefin layer surface is detrimental to the uniform absorption of polar or aqueous food additives. The latter tend to bead up or spontaneously coalesce into droplets. With shorter contact times with the food additive between coating and drying, the surface is not evenly covered and the additive is not fully absorbed, at least not in the open pores of the foam structure. In the case of colored additives, this can result in a spotty, pale color appearance on the surface of the filled food.

[0010] The subject of DE 10 2004 017 350 A1 is a multilayer, coextruded, seamless food casing made of thermoplastic material. The outer layer has a porosity of at least 5 vol.% and a surface roughness of at least 5 µm. The casing thus has a matte appearance, similar to that of natural casings or casings based on regenerated cellulose. To create the porosity, a blowing agent, such as sodium bicarbonate, and / or a blowing gas is added to the outer layer material prior to extrusion. This creates pores or bubbles in the material upon pressure release.

[0011] EP 3 014 997 A1 discloses a multilayer, coextruded, seamless tubular food casing with at least one porous inner layer. According to EP 3 014 997 A1, the porosity of the inner layer(s) is created by a supercritical pore former added immediately before extrusion. "Supercritical pore former" implies that a medium that is gaseous under normal conditions (e.g., CO 2 or N 2 ) is provided, converted to a supercritical state by exposure to high pressure and low temperature, and introduced into a plastic melt in such a way that it forms pores there through expansion. This principle is known as physical foaming of plastics.

[0012] A disadvantage of the physical foaming process is the unusually high process complexity. Generating the supercritical state requires compression and temperature control of the foaming medium. For the precise distribution of the supercritical medium in the melt, a special, complex extruder with various radially arranged feed nozzles and a mixing segment along the extruder screw with multiple perforated elements ("flights") is required.

[0013] According to EP 3 014 997 A1, suitable materials for the porous inner layer are (co)polyamides, polyolefins, vinyl copolymers (such as polyvinyl alcohol, ethylene / vinyl alcohol copolymers, polyvinylpyrrolidone, polystyrene, polyvinyl chloride, and / or polyvinyl fluoride), vinylidene chloride copolymers, or (co)polyesters (such as polylactides, polycaprolactone, polycarbonate, or copolymers of diols with aliphatic or aromatic dicarboxylic acids). Ethylene and propylene copolymers, as well as polyolefins grafted with maleic anhydride, are described as particularly suitable. It may also contain a nucleating agent. The proportion of any nucleating agent present is not specified. Among others, carbonates, such as sodium bicarbonate, and azo compounds, such as azodicarbonamides, are also disclosed as nucleating agents.Furthermore, the multilayer casing according to EP 3 014 997 A1 can comprise layers that consist essentially of aliphatic and / or partially aromatic (co)polyamide. However, the examples specifically disclose only multilayer casings with a foamed inner layer made of an ethylene / butylene copolymer (C4-LLDPE) and a filler masterbatch made of talc and LLDPE—without nucleating agents or other additives.

[0014] EP 1 911 352 A1 describes an emulsifier and an oil as components of the coextruded, inner layer. These substances are very fluid at extrusion temperatures, or significantly less fluid than the matrix-forming organic polymer. It is known that mixtures of viscous and low-viscosity media tend to separate under the shear gradient present in the die gap of an extrusion die. Specifically, the less fluid medium migrates in the direction of the greatest shear gradient, i.e., toward the gap surfaces (in the case of coextrusion, toward the inner gap surface). The consequence is an enrichment of the medium on the inner surface of the coextrudate, followed by successive deposition at the die edge. The deposits must be removed regularly to avoid disruptions during tube forming. This impairs the efficiency of the manufacturing process.

[0015] The casing according to DE 10 2008 017 290 A1 contains no cavities or pores, but merely a relief-like formation of the inner layer. This layer thus has a slightly enlarged "outer surface," but not the much larger "inner surface" and no internal volume as is the case with porous structures. Consequently, the casing's ability to absorb and transfer food additives is limited.

[0016] WO 2005 / 097461 A1 describes a multilayer casing with a porous outer layer. The porosity results in a matte appearance of the exterior. A food transfer function is not possible and not intended due to the position of the porous layer.

[0017] It is therefore an object of the present invention to provide a (barrier) casing based on thermoplastics that does not have the above-described disadvantages of the prior art. In particular, the casing should have the ability to rapidly, evenly, and highly absorb food additives, store them, and efficiently transfer them to a product packaged in the casing.

[0018] This problem was solved by a coextruded, tubular, water vapor-impermeable, and seamless casing with at least three layers. At least one layer is porous and forms a surface layer facing the food. At least one porous layer comprises an aliphatic (co)polyamide and a hydrophilic (co)polymer with an average molecular weight Mw of at least 8,000 Da (determined by GPC = gel permeation chromatography), with the proportion of the hydrophilic (co)polymer in the porous layer being between 3 and 40 wt.%, based on the total weight of the respective porous layer. The at least one porous layer is capable of efficient absorption, storage, and transfer of food additives.

[0019] The invention also includes a corresponding manufacturing process in which the porosity of said layer(s) is achieved through the use of one or more chemical blowing agents. Chemical blowing agents are organic or inorganic substances (e.g. citric acid, azodicarbonamide, sodium bicarbonate) which, at elevated temperature, release one or more substances that are gaseous under normal conditions (e.g. CO2 or N2). Optionally, the manufacturing process also includes biaxial stretching of the shell, preferably in a so-called double-bubble or triple-bubble process. The biaxial stretching significantly increases the mechanical strength and elasticity of the shell. Supercritical pore formers, such as supercritical CO2 or supercritical nitrogen, are not used in the present invention. They are significantly more difficult to dose and mix with the other components of the inner layer than chemical blowing agents.

[0020] In one embodiment, the casing has a porous layer arranged on the surface of the casing facing the food. However, preferred embodiments include two, three, or more adjacent porous layers, one of which forms the surface facing the food.

[0021] In the context of the present invention, "water vapor impermeable" is understood to mean a casing that has a water vapor permeability of less than 30 g / m 2 < d, preferably less than 15 g / m 2 < d, determined according to DIN 53 122, Part 1 at 23 °C and 85% RH. For this purpose, a casing section, which is stretched sealingly over a small dish containing a desiccant, is exposed on one side to air with a relative humidity of 85% at 23 °C in a climatic chamber with stagnant air. The weight of the entire dish, including the casing, desiccant, and sealing wax, is determined before and after exposure to the climatic chamber.

[0022] The term "porous layer" in the sense of the invention refers to a plurality of interconnected cavities (so-called openings), in particular pores, which are capable of efficiently absorbing, storing and transferring the food additives.

[0023] The total porosity of a single porous layer is generally in the range of 5 to 80 vol.%, determined according to the method described below ("volumetric porosity determination"). In the case of several adjacent porous layers, their porosity is preferably also in the range of 5 to 80 vol.%, or the porosity averaged over the several porous layers is in the range of 5 to 80%. Corresponding porosity values ​​are preferably in the range of 10 to 75 vol.%, particularly preferably in the range of 20 to 70 vol.%, and particularly preferably in the range of 30 to 65 vol.%.

[0024] The main component of the at least one porous layer is at least one aliphatic (co)polyamide.

[0025] In the context of the present invention, the term "(co)polyamide" is used as a shorthand for "polyamide or copolyamide." The term "copolyamide" also includes polyamides with three or more different monomer units.

[0026] Among the aliphatic (co)polyamides, preferred are poly(ε-caprolactam), also known as PA 6, copolymers of ε-caprolactam and ω-laurolactam (= PA 6 / 12), copolymers of ε-caprolactam, hexamethylenediamine, and adipic acid (= PA 6 / 66), and terpolymers of ε-caprolactam, 3-aminomethyl-3,5,5-trimethylcyclohexylamine (isophoronediamine), and isophthalic acid. Heterofunctional polyamides, particularly polyetheramides, polyesteramides, polyetheresteramides, and polyamideurethanes, are also considered (co)polyamides. Among these polymers, those with a block-like distribution of the various functionalities, i.e., block copolymers, are preferred. Particularly preferred block copolymers are poly(ether-block-amides).

[0027] The proportion of the aliphatic (co)polyamide is generally 50 to 95 wt.%, preferably 60 to 85 wt.%, particularly preferably 70 to 80 wt.%, in each case based on the total weight of the respective porous layer.

[0028] Another component of the at least one porous layer is at least one hydrophilic (co)polymer with an average molecular weight M w of at least 8,000 Da. Preferred among these are: a) Polyvinyl alcohol (PVAL), as obtainable by partial or complete saponification of polyvinyl acetate (PVAC), or a copolymer with vinyl alcohol units (for example a copolymer with units of vinyl alcohol and propen-1-ol), b) Polyvinylpyrrolidone (homopolymer of N-vinyl-2-pyrrolidone), c) Copolymers with N-vinyl-2-pyrrolidone units and units of at least one α,β-olefinically unsaturated monomer, preferably vinyl ester, particularly preferably vinyl acetate, d) Copolymers of N-vinyl-2-pyrrolidone and one or more α,β-unsaturated carboxylic acids and / or one or more esters or amides of α,β-unsaturated carboxylic acids, preferably methyl acrylate and acrylamide e) Copolymers of N-vinyl-2-pyrrolidone and N-vinylimidazole

[0029] Of these groups, b) and d) are particularly preferred. Polyvinylpyrrolidone with an average molecular weight M w in the range of 8,500 to 400,000 Da and a K value (according to Fickentscher) in the range of 15 to 60 is especially preferred. The average molecular weight M w of the polyvinylpyrrolidone is preferably 9,700 to 200,000 Da, particularly preferably 24,000 to 70,000 Da.

[0030] The proportion of the hydrophilic (co)polymer in the mixture is generally 3 to 40 wt.%, preferably 8 to 25 wt.%, particularly preferably 10 to 20 wt.%, based on the total weight of the respective porous layer.

[0031] To foam the at least one porous layer, at least one chemical blowing agent is added as an additional component during extrusion. Citric acid and / or sodium bicarbonate are preferred. At extrusion temperatures, the chemical blowing agents decompose partially or completely into smaller molecules, at least one of which is gaseous under normal conditions. The finished casing therefore no longer contains the added blowing agent(s) in its original state (possibly in a reduced concentration), but rather in the form of its decomposition products. These can be detected in the finished casing in corresponding quantities. Under normal conditions, these substances are gaseous, but also liquid and / or solid. The gaseous decomposition products cause foaming. This means that they lead to the formation of bubbles or foam cells in the melt.Liquid decomposition products may also be gaseous at extrusion temperature and contribute to foaming. In the case of sodium bicarbonate, CO2 is formed as a gas. Sodium carbonate and water remain as further decomposition products. Citric acid gradually releases water and CO2. Itaconic anhydride and citaconic anhydride remain. The amount of chemical blowing agent is selected to achieve the above-mentioned porosity of the inner layer(s).

[0032] Optionally, the at least one porous layer contains inorganic or organic additives in a proportion of 0.2 to 5 wt.% based on the total weight of the respective layer. Examples include nucleating agents (e.g., CaCO 3 , BaSO 4 , or talc), plasticizers, plasticizers, including diols (e.g., polyethylene glycol) and / or polyols (e.g., glycerin), as well as additives typical for plastics, such as antiblocking and slip agents, pigments, and stabilizers.

[0033] The term "polyol" refers to an aliphatic compound with three or more free hydroxy groups, for example, glycerin, diglycerin, 1,1,1-trimethylolpropane, 2,2-bis-hydroxymethyl-1,3-propanediol (pentaerythritol), and sugar alcohols such as erythritol, sorbitol, and mannitol. Glycerol is preferred.

[0034] The hydrophilic polymer with a molecular weight M w of at least 8,000 Da has two positive effects when mixed with aliphatic (co)polyamide: 1. An increase in the water swelling capacity of the foam matrix; this allows water applied to the foam surface, as well as substances dissolved in water, to diffuse more rapidly through the cell walls of the bubbles and rapidly distribute within the foam structure. The advantage is rapid "drying" or immobilization of a layer of aqueous food additives applied to the shell surface. 2. Compared to pure (co)polyamide (with a molecular weight in the typical extrusion range), it significantly increases melt strength. In this context, melt strength refers to the progressive resistance of a melt to rapid deformation. The deformation resistance is mathematically described as the so-called extensional viscosity v ε and can be measured with special rheometers. The higher these values, the "firmer" the melt.High melt strength results in a slower, controlled expansion of the gas bubbles formed during foaming and an increase in the strength of the "cell walls" between adjacent bubbles. Under these conditions, it is possible to obtain particularly fine foam structures with bubbles or pores of relatively uniform size.

[0035] There are basically several ways to determine the porosity of foamed layer(s). For example, pore areas can be determined from microscopic images of cross-sections (taken using a microtome) of the shell by statistically measuring the cavity edges, preferably using a grid of reference lines superimposed over the microscopic image. By combining the area values ​​of cross-sections taken in several directions, the total porosity can be calculated as the ratio of the cavity volume to the total volume (geometric volume).

[0036] Porosity in the sense of the present invention is the sum of "open porosity" (represented by pores connected to each other and to the environment via channels) and "closed porosity" (represented by closed, unconnected pores). For smaller pore sizes, the mercury infiltration method is suitable for determining open porosity. However, for larger pores, such as those found in the casing according to the present invention, the aforementioned methods are inaccurate or unsuitable. A method known as "volumetric porosity determination" according to the following definition has proven suitable for determining the total porosity Φ: ϕ = V H / V × 100 % = V − V F / V × 100 % with VH = void volume, VF = clean volume and V = total volume of the specimen

[0037] To determine Φ, VF and V are determined as follows. VF corresponds to the volume of a "pore-free" extruded layer made of solid raw materials. This volume can be determined based on the density of the (unfoamed) extrudate and the speed of the extruder used or the speed of the melt pump downstream of the extruder, provided that the extruder or pump has been calibrated for throughput to the raw material mixture. Alternatively, VF can also be determined on the finished shell by selectively removing its foamed layer with a suitable solvent (e.g., formic acid), evaporating the resulting solution, and weighing the dry residue. The total volume V of the foamed layer is determined from its average thickness, obtained by measuring shell cross-sections produced with a microtome, by converting the thickness value to a volume. This method is referred to in the present application as "volumetric porosity determination."

[0038] The shell contains at least one layer based on at least one aliphatic and / or partially aromatic (co)polyamide. Among the aliphatic (co)polyamides, preferred are poly(ε-caprolactam), also referred to as PA 6, copolymers of ε-caprolactam and ω-laurolactam (= PA 6 / 12), copolymers of ε-caprolactam, hexamethylenediamine, and adipic acid (= PA6 / 66), and terpolymers of ε-caprolactam, 3-aminomethyl-3,5,5-trimethylcyclohexylamine (isophoronediamine), and isophthalic acid. Among the partially aromatic (co)polyamides, preferred are copolymers of hexamethylenediamine, isophthalic acid, and terephthalic acid (PA 6-I / 6-T), as well as the homopolymer of m-xylylenediamine and adipic acid (Nylon-MXD6). The layer optionally contains small amounts of additives typical for plastics. The proportion of additives is from 0.1 to 5 wt.%, preferably 0.2 to 4 wt.%, particularly preferably 0.7 to 3 wt.%, particularly preferably 1 to 2 wt.%, based on the total weight of the respective layer.The preferred additives are antiblocking and / or slip agents, stabilizers and color pigments.

[0039] The shell contains at least one layer with a water vapor barrier (water vapor impermeable) character. The layer preferably comprises predominantly olefinic (co)polymer, e.g., polyethylene (HDPE, LDPE, or LLDPE), ethylene-α-olefin copolymers, polypropylene, ethylene-propylene copolymers, or terpolymers of various olefins. Heterofunctional olefin copolymers may also be present in proportion. Examples include copolymers of ethylene and vinyl acetate or ethylene and (meth)acrylic acid, as well as corresponding functional terpolymers. This layer also optionally contains small amounts of additives typical of plastics, including antiblocking and / or slip agents, stabilizers, and color pigments.

[0040] The shell contains at least one layer, which is arranged to adjacent polyamide-based layers and is capable of developing chemical and / or physical adhesive properties (so-called adhesive layer). This layer preferably comprises predominantly olefin-containing polymer modified with polar functional groups. Examples include polyethylene (or ethylene-α-olefin copolymer) grafted with anhydride of an α,β-unsaturated dicarboxylic acid (preferably maleic anhydride), ethylene / vinyl acetate copolymers, ethylene / (meth)acrylic acid copolymers and their Na or Zn salts, ethylene / (meth)acrylic acid ester copolymers, and corresponding terpolymers. Non-functionalized olefin (co)polymers may be included as admixtures.

[0041] One or more of the layer(s) with water vapor barrier properties and the layer(s) with adhesive properties comprising an adhesion-promoting component can also be combined into a single layer. The adhesion-promoting component is therefore contained in one or more of the water vapor-impermeable layer(s). In this case, the polymers mentioned in the previous paragraph are again preferred as components of the layer. Optionally, one or more of the polymers mentioned in the paragraph regarding the water vapor barrier layer can be added. Optionally, the layer can also contain additives as mentioned above.

[0042] The casing according to the invention generally has 3, 4, 5, 6, 7, 8, or 9 layers. Casings with 5 or 7 layers are preferred.

[0043] The invention also relates to a process for producing the food casing according to the invention. Production is generally carried out by extrusion processes known per se to those skilled in the art.

[0044] First, a compound is produced from at least one aliphatic (co)polyamide and at least one hydrophilic (co)polymer, and optionally additives. For this purpose, the components are melted together in a suitable device, preferably a twin-screw extruder (also called a twin-screw extruder) with a connected perforated die, air cooling section, and granulator, plasticized, homogenized, and extruded through the die. The resulting granulate is mixed at room temperature with at least one blowing agent—optionally in the form of a granular masterbatch—and optionally further additives, and then remelted in another extruder. As the temperature rises in the extruder, the formation of the gaseous medium from the blowing agent begins. Due to the pressure applied in the extruder, the gas initially remains partially or completely dissolved in the melt.

[0045] Preferably, the extrusion of the latter mixture is not carried out in a single extruder, but rather divided between two or more similar extruders. The composition of the mixture may vary slightly for each extruder.

[0046] In addition to this extruder(s), the process involves two or more additional extruders. The components of the subsequent layers described above are fed to each of these extruders.

[0047] All extruders are connected to a temperature-controlled coextrusion ring die with a number of melt channels corresponding to the number of extruders. If the blowing agent-containing mixture is distributed across multiple extruders, the melt streams from these extruders enter adjacent melt channels and form adjacent layers. A ring-shaped, multilayer melt film emerges from the annular gap of this die. During the pressure drop shortly before exiting the die, gas bubbles form and expand in the blowing agent-laden layer(s). Cooling of the melt film forms a primary tube with a relatively thick wall, in which the bubble or foam structure is solidified. The primary tube is then rapidly cooled to freeze the amorphous state of the polymers. It is then reheated to the temperature required for stretching, for example, to approximately 80°C.The tube is then stretched longitudinally and transversely, preferably in a single operation. Longitudinal stretching is typically performed using two pairs of squeeze rollers with increasing drive speeds. Transverse stretching is achieved by gas pressure acting on the walls of the tube from the inside. The areal stretch ratio (the product of the longitudinal and transverse stretch ratios) is generally about 6 to 18, preferably 7 to 15, and particularly preferably about 8 to 11.

[0048] After stretching, the tube is preferably heat-set. The degree of heat-set allows the desired shrinkage properties to be precisely adjusted. Finally, the tube is cooled, flattened, and wound up. The wall thickness (total thickness) of the casing, determined by microscopic measurement of casing cross-sections, after stretching and heat-set is generally about 40 to 120 µm, preferably about 60 to 100 µm. The proportion of the foamed layer(s) on the inside of the casing is generally 30 to 85%, preferably 50 to 75%, based on the wall thickness. The diameter of the casing is generally in the range of 60 to 220 mm, preferably 80 to 170 mm.

[0049] The foamed layer(s) can be arranged either on the outer or inner surface of the tubular structure. In the former case, the food additive(s) are applied to the casing from the outside, e.g., by spraying, rolling, or printing. The surface can then be dried, e.g., with hot air. The casing must then be turned over to bring the coated side to the inside, allowing the additive(s) to be transferred to the food after it has been filled.

[0050] Once the foamed layer(s) is / are positioned on the inner surface of the casing, the food additive(s) are applied to the inside, preferably by so-called "slug impregnation." A liquid preparation of the substance(s) is poured into the casing and held in contact with it for a few seconds. The casing is then passed through a pair of squeeze rollers to remove any excess liquid that has not been absorbed. The thus impregnated casing is rewound. The process can be operated continuously or discontinuously. In any case, turning the casing is unnecessary. It can be used directly for filling the food product. The food casing according to the invention is particularly suitable as an artificial sausage casing, especially for wrapping cooked or scalded sausage. Examples:

[0051] The following examples serve to illustrate the scope of the invention without limiting it. Percentages are by weight unless otherwise stated or apparent from the context. The following starting materials were used: (Co)Polyamides:

[0052] PA1 Polyamide 6 / 66 with a relative viscosity of 3.4 (measured in 96% sulfuric acid) and a crystallite melting temperature of 192°C (measured by DSC) (Ultramid ®< C33 N, BASF SE) PA2 Polyamide 6 with a relative viscosity of 4 (measured in 96% sulfuric acid) and a crystallite melting temperature of 220°C (measured by DSC) (Ultramid ®< B40 N, BASF SE) PA3 Dryblend of polyamide (approx. 88%), polyamide 6-I / 6-T (approx. 10%) and calcium carbonate (approx. 2%) (Grilon ®< FG40 NL, Ems-Chemie) Hydrophilic polymers:

[0053] PVP1 Polyvinylpyrrolidone with a K value of 25 and an average molecular weight M w of 34,000 Dalton (Kollidon ®< 25, BASF SE) PVP2 Polyvinylpyrrolidone with a K value of 12 and an average molecular weight M w of 5,000 Dalton (PVP K-12, Ashland Industries Europe GmbH) Plasticizers:

[0054] Glycerin 96% purity according to DAB (German Pharmacopoeia) Chemical blowing agent:

[0055] TR-MB Wax-based blowing agent masterbatch containing sodium bicarbonate, citric acid and nucleating agent (Corducel ®< ETS 9610, Nemetz Additive Plastic GmbH) Polyamide antiblocking agent:

[0056] PA-AB Masterbatch based on polyamide 6 and calcium carbonate (5015-FT72, PolyOne Colour and Additives Germany GmbH) Polyolefin / polymer with water vapor barrier properties:

[0057] PO1 Low-density polyethylene (LDPE) with a density of 0.923 g / cm3 and an MFI (melt flow index) of 2.0 g / 10 min, measured at 2.16 kg load and 190°C (LD100 BW, ExxonMobil) Olefin copolymer:

[0058] PO2 Ethylene-methacrylic acid copolymer (9.5 wt% methacrylic acid) with an MFI of 1.3 g / 10 min, measured at 2.16 kg load and 190°C (Nucrel™< 31001, DOW) Polyolefin antiblocking agent:

[0059] PO-AB Masterbatch based on polyethylene LLDPE and calcium carbonate (CESA Block 1101 from Clariant Masterbatches Deutschland GmbH) Adhesion promoter / polymer with adhesive properties to polyamide:

[0060] PO-HV Linear low density polyethylene (LLDPE) grafted with maleic anhydride (MSA) with a density of 0.928 g / cm 3 and an MFI of 3.0 g / 10 min, measured at 2.16 kg load and 190°C (Yparex™ 9403, The Compound Company BV). Measurement parameters for characterizing the shells:

[0061] porosity

[0062] The total porosity was determined using the “Volumetric Porosity Determination” method described above. Visual assessment

[0063] For the visual assessment, wound casing material was coated on the side of layer 1 (outside) using a gravure printing process.

[0064] For coating purposes, for example, formulations of paints as well as mixtures of preferably polar liquid smoke types can be used.

[0065] A mixture of liquid smoke types was used for the coating. The coating was applied to the casing surface while lying flat, one-sided, using a screened gravure cylinder. Immediately after coating, the casing was passed through a drying tunnel through which conditioned air at a temperature of approximately 60°C flowed. The dried casing was then coated in the same way on the reverse side, dried, and then rewound. Samples cut at intervals of several meters were used for evaluation.

[0066] The assessment was based on (a) the visual appearance of the coated surface and (b) an image analysis of the brown-colored surface fraction compared to the total surface. A high proportion of colored surface indicates both a high degree of absorption of the food additive and a relatively uniform coverage of the surface.

[0067] For image analysis (b), microscopic top-down images of the coated surface were first taken from four sample sections per sample. An Olympus BX60 light microscope with a Hitachi HV-C20 digital camera was used. All images were taken under uniform incident light illumination of the samples and with uniform camera settings. A section measuring 1400 x 1200 µm was analyzed from each image.

[0068] The image analysis was carried out using the ColorAnalysis software from Datinf ®< GmbH, Tübingen. After preselecting color values ​​for an object and for the object's surroundings, this software allows the object area to be calculated in relation to the total area of ​​objects and object surroundings. The software first converts the RGB values ​​of each pixel of the camera image into HSV coordinates. (For an understanding of the HSV color space, see: https: / / de.wikipedia.org / wiki / HSV-Farbraum. The value H designates the angle in a color wheel, S defines the color saturation, and V the brightness of the hue.) The preselected colors for the object and surroundings are also converted into HSV values. The HSV values ​​are then converted to Cartesian coordinates. The software then determines the smaller squared distance (divided by a 0.01% weighting) to the object color or the surrounding area for each image pixel.to the surrounding color and outputs the number of pixels assigned to each of these colors as percentages.

[0069] The following selection colors were used consistently for all image analyses: Object color H = 32 Ambient color H = 180 S = 98 (medium brown) S = 94 (white) V = 52 V = 100

[0070] Table 5 shows the averaged area shares from 4 images per example. Example 1 (according to the invention) and Example V1 (comparison): Production of compounds from aliphatic copolyamide and hydrophilic polymer

[0071] In a twin-screw extruder (manufacturer: Coperion, screw diameter 25 mm) with a single-hole outlet nozzle, the components listed in Table 1 were fed sequentially through three discretely arranged metering devices. The metering rates [mass per unit time] were related to each other according to the percentages given in the table. The extruder was heated to 180°C at the polyamide feed point. In the subsequent barrel zones, the temperature was gradually increased to a maximum of 230°C. The screw speed was approximately 200 rpm. In this way, the polyamide was melted and plasticized with the powdered PVP and the glycerol to form a homogeneous mixture. The mixture exited the extruder through the perforated die as a water-clear, uniform strand. The strand was passed through a water bath for cooling and then reduced to granules using a strand chopper.The granules were dried in a circulating air dryer at approximately 100°C. Table 1: Components of the compounds Example Name Compound aliphatic polyamide hydrophilic polymer Plasticizers 1 Comp1 PA1 75.5 wt.% PVP1 21 wt%. Glycerin 2.7% w / w V1 Comp2 PA1 75.5 wt.% PVP2 21 wt%. Glycerin 2.7% w / w Examples 2 and 3: Production of biaxially stretched tubular casings with foamed layers

[0072] A state-of-the-art coextrusion line was used to produce the casings. The coextrusion line is equipped with seven extruders, each downstream of a melt pump calibrated for mass throughput, a seven-layer ring die with a 60 mm ring diameter, a pipe calibration system, a downstream stretching zone for biaxial bubble stretching, a subsequent heat-setting zone, and finally a tube winding system (a so-called double-bubble system).

[0073] The seven extruders were connected to the nozzle in such a way that the melt stream exiting extruder 1 was directed to the channel forming the outer layer, and the stream from extruder 7 was directed to the inner layer of the channel forming the seven-layer tube. The remaining extruders were connected to the nozzle channels according to the extruder numbering.

[0074] The granules or granule premixes according to Table 2 were fed to the seven extruders via conventional metering devices, melted, plasticized, and conveyed toward the die. The extruder temperatures ranged between 100 and 240°C (increasing downstream). The die was heated to 235°C. The blowing agent fed proportionally to extruders 1 to 3 gradually released gas due to the elevated temperatures in the melt streams. During the pressure drop as the melt film emerged from the die, the corresponding layers 1, 2, and 3 foamed. The melt film was formed into a pre-tube with a diameter of 32 mm via the pipe calibration system and solidified. In the stretching zone, the tube was then biaxially stretched by a factor of 8.05, subsequently passed through the thermosetting zone, flattened, and wound up.The resulting casings had a caliber of 104 mm and a shrinkage (measured after 15 minutes of immersion in 80°C water) of 6 to 10%, both in the longitudinal and transverse directions. Due to their foamed, porous surfaces, the total thickness of the casings could not be precisely measured mechanically. The gravimetrically calculated thicknesses of the layers ("net thicknesses") and the resulting total net thicknesses of the casings (expansion due to foaming not taken into account) are given. Table 2: Structure of the casings according to Examples 2 and 3 (according to the invention) Example No. layer Composition [wt%] Net thickness of single layer 1)< [um / %] Net thickness of the entire structure 1)< [µm] 2 1 Comp1

[87] , PA-AB [9], TR-MB [4] 4,2 / 7,2 58,4 2 Comp1

[87] , PA-AB [9], TR-MB [4] 4,3 / 7,4 3 Comp1

[87] , PA-AB [9], TR-MB [4] 15,1 / 25,8 4 PO-HV ​​

[100] 2,4 / 4,1 5 PA1

[30] , PA2

[70] 22,6 / 38,7 6 PO-HV ​​

[100] 2,4 / 4,1 7 PA3

[100] 7,4 / 12,7 3 1 Comp1

[87] , PA-AB [9], TR-MB [4] 4,0 / 6,9 58,2 2 Comp1

[87] , PA-AB [9], TR-MB [4] 4,5 / 7,7 3 Comp1

[87] , PA-AB [9], TR-MB [4] 14,8 / 25,4 4 PO-HV ​​

[100] 2,5 / 4,3 5 PA1

[30] , PA2

[70] 22,1 / 38,0 6 PA1

[30] , PA2

[70] 3,5 / 6,0 7 PA3

[100] 6,8 / 11,7 1) Effect of foaming not taken into account Comparison examples V2 to V5:

[0075] Using the described coextrusion system, multilayer, biaxially stretched casings were produced under the same conditions as in Examples 2 to 3. The composition of the layers and casing structures are shown in Table 3. Table 3: Structure of the casings according to comparative examples V2 to V5. (not according to the invention) Example No. layer Composition [wt%] Net thickness of single layer 1)< [µm / %] Net thickness of the entire structure 1)< [µm] V2 1 Comp2

[87] , PA-AB [9], TR-MB [4] 4,0 / 6,9 58,1 2 Comp2

[87] , PA-AB [9], TR-MB [4] 4,2 / 7,2 3 Comp2

[87] , PA-AB [9], TR-MB [4] 14,2 / 24,4 4 PO-HV ​​

[100] 2,6 / 4,5 5 PA1

[30] , PA2

[70] 22,8 / 39,3 6 PO-HV ​​

[100] 2,6 / 4,5 7 PA3

[100] 7,7 / 13,2 V3 1 PO1

[87] , PO-AB [9], TR-MB [4] 3,8 / 6,3 60,0 2 PO1

[87] , PO-AB [9], TR-MB [4] 3,5 / 5,8 3 PO1

[87] , PO-AB [9], TR-MB [4] 12,5 / 20,8 4 PO-HV ​​

[100] 2,7 / 4,5 5 PA1

[30] , PA2

[70] 26,7 / 44,5 6 PO-HV ​​

[100] 2,3 / 3,8 7 PA3

[100] 8,5 / 14,2 V4 1 PA3

[87] , PA-AB [9], TR-MB [4] 4,5 / 7,5 59,9 2 PA3

[87] , PA-AB [9], TR-MB [4] 4,6 / 7,7 3 PA3

[87] , PA-AB [9], TR-MB [4] 15,2 / 25,4 4 PO-HV ​​

[100] 2,8 / 4,7 5 PA1

[30] , PA2

[70] 23,1 / 38,6 6 PO-HV ​​

[100] 2,5 / 4,2 7 PA3

[100] 7,2 / 12,0 V5 1 PO2

[87] , PO-AB [9], TR-MB [4] 4,4 / 7,5 58,8 2 PO2

[87] , PO-AB [9], TR-MB [4] 4,3 / 7,3 3 PO2

[87] , PO-AB [9], TR-MB [4] 15,1 / 25,7 4 PO-HV ​​

[100] 2,6 / 4,4 5 PA1

[30] , PA2

[70] 22,8 / 38,8 6 PO-HV ​​

[100] 2,4 / 4,1 7 PA3

[100] 7,2 / 12,2 1) Effect of foaming not taken into account

[0076] All casings according to examples were coated with the food additive under uniform conditions as described above.

[0077] The properties determined on samples from the examples are listed in Tables 4 and 5 below. Table 4: Porosity values ​​of the casings according to the invention and the casings from comparative examples Example Total net volumes of layers 1 to 3 per unit area 1)< VR 1-3 [µm 3< / µm 2< ] Volume sum of layers 1 to 3 per unit area 2)< V 1-3 [µm 3< / µm 2< ] Average total porosity of layers 1 to 3 3)< Φ 1-3 [%] 2 23,6 67 65 3 23,3 61 62 V2 22,4 42 47 V3 19,8 30 34 V4 24,3 35 39 V5 23,8 59 60 1) Value corresponds to the sum of the net thicknesses of layers 1, 2 and 3 (see Table 3); 2) Value corresponds to the sum of the thicknesses of the foamed layers, determined by measuring microscopic images of shell cross-sections; 3) Calculated according to the described method "Volumetric porosity determination". Table 5: Visual evaluation of the surfaces of casings according to the invention coated with food additive and coated casings from comparative examples Example Visual appearance Area proportion of object color (brown) [%] Area proportion of ambient color (white) [%] 2 Surface and cavities completely colored, homogeneous color impression 83,9 16,1 3 Surface and cavities completely colored, homogeneous color impression 79,2 19,8 V2 Surface and cavities colored, cavities large and uneven, somewhat "unrestful" color impression 50,5 49,5 V3 dark round color dots, strongly "speckled" color impression 17,2 82,8 V4 Cavities colored, intermediate areas white, slightly inhomogeneous color impression 21,3 78,7 V5 Cavities partially colored, intermediate areas white, clearly inhomogeneous color impression 19,9 80,1

[0078] The high values ​​of total porosity, the homogeneity of the visual appearance and the high area proportion of the object color in Examples 2 and 3 demonstrate the superiority of the casing according to the invention over the prior art.

Claims

1. Coextruded, water vapour-impermeable, tubular, seamless food casing having at least three layers, comprising: at least one porous layer, wherein one of the porous layers forms a surface layer that faces toward a food, at least one carrier layer based on at least one aliphatic and / or partially aromatic (co-)polyamide, and at least one water vapour-impermeable layer, wherein either at least one adhesive layer comprising an adhesion-promoting component is arranged between the adjoining layers or the adhesion-promoting component is contained in one or more of the water vapour-impermeable layer(s), characterized in that at least one porous layer comprises an aliphatic (co)polyamide and a hydrophilic (co-)polymer having a mean molar mass Mw of at least 8000 Da, wherein the proportion of the hydrophilic (co-)polymer in the porous layer is 3 to 40 wt.%, in relation to the total weight of the respective porous layer.

2. Food casing according to Claim 1, characterized in that at least one porous layer has a total porosity φ in the range of 5 to 80 vol.%, preferably 10 to 75 vol.%, particularly preferably 20 to 70 vol.%, particularly preferably in the range of 30 to 65 vol.%, wherein φ is ascertained according to the described method "volumetric porosity determination".

3. Food casing according to Claim 1 or 2, characterized in that the aliphatic (co-)polyamide of the at least one porous layer and / or the at least one carrier layer comprises poly(ε-caprolactam) (PA 6), copolymers of ε-caprolactam and ω-laurin lactam (PA 6 / 12), copolymers of ε-caprolactam, hexamethylene diamine, and adipic acid (PA6 / 66), and terpolymers of ε-caprolactam, 3-aminomethyl-3,5,5-trimethylcyclohexylamine (isophorone diamine) and / or isophthalic acid.

4. Food casing according to Claim 1, characterized in that the partially aromatic (co-)polyamide of the at least one carrier layer is a copolymer of hexamethylene diamine, isophthalic acid, and terephthalic acid (PA 6-1 / 6-1) or a homopolymer of meta-xylylene diamine and adipic acid (nylon-MXD6) .

5. Food casing according to one or more of Claims 1 to 4, characterized in that the proportion of the aliphatic (co-)polyamide(s) in the at least one porous layer is 50 to 95 wt.%, preferably 60 to 85 wt.%, particularly preferably 70 to 80 wt.%, each in relation to the total weight of the respective layer.

6. Food casing according to one or more of Claims 1 to 5, characterized in that the hydrophilic (co-)polymer is - polyvinyl alcohol (PVAL), a copolymer having vinyl alcohol units, preferably a copolymer having units made up of vinyl alcohol and propen-1-ol; - polyvinyl pyrrolidone, preferably a homopolymer made up of N-vinyl-2-pyrrolidone units; - a copolymer made up of or having N-vinyl-2-pyrrolidone units and units of at least one α,β-olefinically unsaturated monomer, preferably vinyl ester, particularly preferably vinyl acetate; - a copolymer made up of units of N-vinyl-2-pyrrolidone and one or more α,β-unsaturated carboxylic acids and / or one or more esters or amides of α,β-unsaturated carboxylic acids, preferably methyl acrylate and acrylamides; or - a copolymer made up of units of N-vinyl-2-pyrrolidone and N-vinylimidazole.

7. Food casing according to one or more of Claims 1 to 6, characterized in that the proportion of the hydrophilic (co-)polymer in the porous layer is 8 to 25 wt.%, preferably 10 to 20 wt.%, in relation to the total weight of the respective porous layer.

8. Food casing according to one or more of Claims 1 to 7, characterized in that the casing comprises at least one chemical propellant, preferably citric acid and / or sodium hydrogen carbonate, and / or thermal degradation products of at least one chemical propellant.

9. Food casing according to one or more of Claims 1 to 8, characterized in that at least one porous layer contains inorganic or organic additives.

10. Food casing according to one or more of Claims 1 to 9, characterized in that the water vapour-impermeable layer comprises an olefinic (co-)polymer, preferably polyethylene (HDPE, LDPE, or LLDPE), ethylene-α-olefin copolymers, polypropylene, an ethylene-propylene copolymer, or a terpolymer made up of various olefins.

11. Food casing according to one or more of Claims 1 to 10, characterized in that the adhesive layer comprises an olefin-containing polymer, preferably polyethylene (or ethylene-α-olefin-copolymer) grafted with the anhydride of an α,β-unsaturated dicarboxylic acid, particularly preferably maleic acid anhydride; an ethylene / vinyl acetate copolymer, an ethylene / (meth)acrylic acid copolymer or their Na or Zn salt, an ethylene / (meth)acrylic acid ester copolymer, or a corresponding terpolymer.

12. Food casing according to one or more of Claims 1 to 11, characterized in that at least one of the further (nonporous) layers contains plastic-typical additives in a proportion of 0.2 to 5 wt.% in relation to the total weight of the respective layer.

13. Method for producing a food casing according to one or more of Claims 1 to 12, comprising the following steps: - providing a granulated material comprising at least one aliphatic (co-)polyamide, at least one hydrophilic (co-)polymer, and possibly additive(s), - producing one or more mixtures of the obtained granulated material with at least one propellant or at least one propellant masterbatch and possibly further additives; - melting, plasticizing, and homogenizing the mixture or the mixtures in one or more extruder(s); - melting, plasticizing, and homogenizing one or more granulated materials / granulated material mixtures for the carrier layer(s) in one or more further extruder(s); - melting, plasticizing, and homogenizing one or more granulated materials / granulated material mixtures for the water vapour-impermeable layer(s) in one or more further extruder(s); - possibly melting, plasticizing, and homogenizing one or more granulated materials / granulated material mixtures for the adhesive layer (s) in one or more further extruder(s); - bringing together the melt flows in a coextrusion annular die and forming them into a seamless multi-layered primary tube; - rapidly cooling the primary tube; - heating the primary tube to approximately 80 °C with subsequent stretching of the primary tube in the longitudinal and transverse directions.

14. Use of the food casing according to one or more of Claims 1 to 13 as an artificial sausage casing, in particular for encasing cooked or boiled sausage.