CARBON FIBER AND METHOD FOR PRODUCING SUCH CARBON FIBER FROM CELLULOSE

DE602019061582T2Active Publication Date: 2024-11-06FAURECIA SERVICES GRP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602019061582
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-09
Filing Date
2019-07-08
Publication Date
2024-11-06
Estimated Expiration
2039-07-08

AI Technical Summary

Technical Problem

Current processes for manufacturing carbon fibers from cellulose fail to achieve high mechanical properties and low hydrostatic density, and often require high carbonization temperatures, making them costly and inefficient.

Method used

A process involving cellulose fibers subjected to a two-phase heat treatment with stretching ratios between 1.25 and 3 in the first phase at 500-700°C, and 0.7-1.1 in the second phase at 900-1500°C, resulting in carbon fibers with Young's modulus greater than 85 GPa and tensile breaking stress greater than 1500 MPa, while maintaining low hydrostatic density and being cost-effective.

Benefits of technology

The process yields carbon fibers with superior mechanical properties and low density, suitable for composite materials, and can be completed at low carbonization temperatures, reducing energy and investment costs, and enabling their use in various applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention falls within the field of manufacturing carbon fibers from bio-based raw materials, and more specifically from cellulose.

[0002] More specifically, the present invention relates to a cellulose-based carbon fiber, as well as a method for preparing such a carbon fiber from a cellulose fiber. The present invention also relates to the use of such a carbon fiber for the manufacture of a composite material, and a composite material comprising such a carbon fiber.

[0003] Carbon fibers are used in many fields, taking advantage of their mechanical, electrical, and thermal properties. For example, they are frequently used as reinforcing fibers in composite materials, where they are distributed within a polymer resin matrix.

[0004] The production of carbon fibers from renewable bio-based materials, in order to overcome the problem of the projected depletion of fossil resources, has been the subject of much research in recent decades. Prior art, in particular, has proposed manufacturing such fibers from cellulose, a high-carbon biopolymer that is the main constituent of plant cell walls. Cellulose is estimated to make up 35 to 50% of terrestrial biomass, making its utilization highly desirable.

[0005] Cellulose can notably be shaped by spinning to form fibers, which can be used as precursors to carbon fibers, and which have the advantage of being obtainable at low cost.

[0006] In the context of natural resource valorization, various processes for manufacturing carbon fibers from cellulose fibers have been proposed in the prior art. As an example, document WO 01 / 42541 describes a continuous or batch carbonization process for cellulosic fibrous materials in the presence of at least one organosilicon compound. However, the carbon fibers obtained by such a process exhibit average mechanical properties, and in particular, based on the examples cited in this document, a tensile strength of 1100 to 1200 MPa and a Young's modulus of 40 to 45 GPa.

[0007] Document WO 2014 / 029748 describes carbon fibers obtained from cellulose fibers. These carbon fibers are said to have a Young's modulus of 155 GPa, a tensile strength of 1500 MPa, and an elongation at break of 2.1%. However, such a combination of values ​​for these three parameters is not technically possible, so the carbon fibers described in this document cannot be considered to actually possess the stated mechanical properties. Furthermore, the density of these carbon fibers is not specified in this document.

[0008] Carbon fiber density is an important parameter, particularly in the context of composite material manufacturing. Lower density carbon fibers allow for the production of lighter or stronger materials for the same weight, which is especially advantageous for many applications.

[0009] There remains at present a need for a process for preparing carbon fibers from cellulose fibers that makes it possible to obtain carbon fibers with good tensile mechanical properties and low hydrostatic density.

[0010] The present invention aims to propose such a process, as well as carbon fibers that can be obtained by such a process and that exhibit both high performance in terms of mechanical resistance and low hydrostatic density.

[0011] The invention also aims to enable such carbon fibers to be prepared at low cost.

[0012] The present inventors have now discovered that such objectives can be achieved, and that carbon fibers exhibiting both low density and good mechanical properties can be obtained from cellulose fibers, moreover by means of a process employing relatively low carbonization temperatures, less than or equal to 1500 °C. Such a result is all the more surprising given that it is known from the literature that the tensile mechanical properties of carbon fibers are directly proportional to the greater the stretching of the fibers during the carbonization process, and that significant fiber stretching is only possible at high temperatures, on the order of 2500 °C and above.The inventors have discovered that, quite unexpectedly, by implementing specific operating conditions, cellulose fibers can be stretched significantly during a carbonization heat treatment carried out at a moderate temperature, resulting in carbon fibers that exhibit particularly high tensile strength while simultaneously displaying a low hydrostatic density. Indeed, the hydrostatic density of a carbon fiber is directly proportional to the lower the treatment temperatures at which the fiber has been subjected.

[0013] Furthermore, precisely because of the use of low carbonization temperatures, as well as the low cost of the raw material, the carbon fibers obtained by this process can advantageously be produced at low cost.

[0014] Thus, according to a first aspect, the present invention proposes a non-graphitized carbon fiber prepared from cellulose, comprising one or more filaments, having a Young's modulus in tension (E) (measured according to ISO 11566:1997, method B) greater than or equal to 85 GPa and a tensile breaking strength (σH) (measured according to ISO 11566:1997, method B) greater than or equal to 1500 MPa, preferably greater than or equal to 1600 MPa and preferably greater than or equal to 1800 MPa, and in which the filament(s) each have a hydrostatic density (measured according to ISO 10119:2002, method B2) between 1.3 and 1.65 g / m³.

[0015] In this description, non-graphitized carbon fiber means a carbon fiber obtained through a carbonization process and not subsequently subjected to heat treatment, known as graphitization treatment, carried out at very high temperature, more particularly at a temperature between 1800 °C and 3000 °C, allowing the transformation of amorphous carbon into graphite.

[0016] For convenience, such an ungraphitized carbon fiber will be referred to in this description as "carbon fiber". The term "graphitized carbon fiber" will be used to designate the fiber obtained after graphitization, that is, heat treatment at very high temperature, greater than or equal to 1800 °C, of ​​the ungraphitized carbon fiber according to the invention.

[0017] The carbon fiber according to the invention can, for example, comprise between 500 and 48,000 filaments, in particular about 12,000 filaments, or between 500 and 2,000 filaments, in particular about 1,000 filaments.

[0018] As stated above, the carbon fiber according to the invention advantageously exhibits high performance in terms of tensile mechanical strength, as well as low hydrostatic density.

[0019] The hydrostatic density of the filaments constituting the fiber can be measured by any method which is conventional in itself for a person skilled in the art, in particular by a method described in the ISO 10119:2002 - B2 standard, for example the gravimetric method, which consists of immersing a sample of finely cut carbon fibers in different solvents and / or mixtures of solvents of different densities, listed in the standard, and deducing the density of the fibers according to whether they sink or not.

[0020] These properties prove particularly advantageous, notably for the use of carbon fiber according to the invention as reinforcement in composite materials. Indeed, a lower density of reinforcing fibers in a composite material results in either better mechanical properties, as it can contain more reinforcing fibers for an equivalent material weight, or greater lightness, for the same percentage of reinforcing fibers.

[0021] The carbon fiber according to the invention, obtained from a cellulose-based precursor fiber, and which may comprise one or more filaments, can have any length.

[0022] It can be formed from any type of cellulose-based precursor fiber, this precursor fiber typically being formed by a coagulation spinning process.

[0023] The cellulose-based precursor fiber can therefore be of the viscose type or of the Lyocell type, these types of cellulose fibers being well known to those skilled in the art, or of the type obtained by a process of dissolving cellulose in phosphoric acid H3PO4, as described for example in document WO 85 / 05115, or a process of dissolving cellulose in an ionic liquid.

[0024] The cellulose-based precursor fiber, from which the carbon fiber according to the invention is formed, may have been prepared by a process involving the addition to the cellulose, prior to spinning or during spinning, of: one or more polymer additives, preferably in a quantity by weight between 10 and 30%. Preferably, however, lignin is avoided in the context of the invention; one or more substances facilitating the impregnation of cellulose by the solvent, such as the products marketed under the names NOPCO ESA 120, EMULAN ®< ES 9880 or BEROCELL VISCO 388; and / or fillers selected from among nanometric carbon fillers, such as carbon nanotubes and graphene, and / or cellulose nanocrystals; these fillers being preferably added in a total quantity by weight less than or equal to 20%, and preferably between 0.005 and 5%.

[0025] In this description, the term "carbon nanofiller" refers to a filler comprising an element from the group consisting of carbon nanotubes, carbon nanofibers, graphene, fullerenes, and carbon black, or any mixture of such elements. Preferably, the carbon nanofillers used in the invention are carbon nanotubes, either alone or in a mixture with graphene. Carbon nanotubes are, for example, marketed by ARKEMA under the name Graphistrength®.

[0026] Carbon nanofillers can have a small dimension ranging from 0.1 to 200 nm, preferably between 0.1 and 160 nm, and preferably between 0.1 and 50 nm. This dimension can, for example, be measured by light scattering.

[0027] In this description, "graphene" refers to a flat, isolated, and individual sheet of graphite, but also, by extension, to an assembly comprising between one and several dozen sheets and exhibiting a planar or more or less undulating structure. This definition thus encompasses FLGs (Few Layer Graphene, i.e., loosely stacked graphene), NGPs (Nanosized Graphene Plates, i.e., graphene plates of nanometric dimensions), CNSs (Carbon NanoSheets, i.e., graphene nanosheets), and GNRs (Graphene NanoRibbons, i.e., graphene nanoribbons). It excludes, however, carbon nanotubes and carbon nanofibers, which are respectively composed of the coaxial winding of one or more graphene sheets and the turbostratically stacking of these sheets.

[0028] The carbon fiber according to the invention can be formed from a cellulose fiber which, prior to the implementation of a carbonization process, has been impregnated with one or more additives.

[0029] Examples of such impregnation additives, used alone or in mixtures, include: Brønsted acid compounds or compounds that release Brønsted acids upon heating, such as: o hydrogen halides o halides having any counterion such as sodium, potassium, ammonium, etc. o sulfuric acid o sulfates having any counterion such as sodium, potassium, ammonium, etc. o organic sulfonic acids bearing an alkyl group, such as methylsulfonic acid, or an aryl group, such as para-toluenesulfonic acid, or any other organic group o organic sulfonates corresponding to the above sulfonic acids and having any counterion such as sodium, potassium, ammonium, etc. o phosphoric acid and polyphosphoric acids o and / or phosphates and polyphosphates having any counterion such as sodium, potassium, ammonium, etc.Lewis acid compounds, such as: o boric acid o and / or metal halides such as aluminium chloride AlCl 3 or iron chloride FeCl 2; urea; nanometric carbon fillers; and / or formulations based on silicone polymers, for example based on polydimethylsiloxane combined with a crosslinking agent.

[0030] Such a list is of course in no way exhaustive of the invention.

[0031] Impregnation additives based on silicone polymers are particularly preferred in the context of the present invention, as they allow for further improvement of the mechanical properties of the carbon fiber according to the invention.

[0032] Silicone-type impregnation additives are preferably used at a rate, defined as the mass percentage of additive deposited relative to the total weight of the cellulosic fiber and the additive, of between 0.01 and 20%, preferably between 0.5 and 10%, and preferably still between 1 and 5%.

[0033] The cellulose-based precursor fiber preferably has a count between 700 and 80000 dtex.

[0034] Preferably, the carbon fiber according to the invention meets one or more, preferably all, of the following characteristics: It has a Young's modulus in tension greater than or equal to 90 GPa, a tensile strength at break greater than or equal to 2000 MPa, and a carbon content greater than or equal to 85%, preferably greater than or equal to 90%. The filament constituting it has a diameter between 3 and 10 µm, preferably between 3 and 8 µm, and preferably between 3 and 6 µm, or the filaments constituting it have an average diameter between 3 and 10 µm, preferably between 3 and 8 µm, and preferably between 3 and 6 µm. This average diameter may, for example, be between 3 and 4 µm. The diameter of the filament(s) is measured according to ISO 11567:2018, method C.

[0035] Such a small diameter is evidence of particularly good mechanical properties of the fiber.

[0036] The carbon content of carbon fiber can be measured using any method known to those skilled in the art, including elemental analysis. In a conventional manner, a sample of the fiber to be analyzed is placed in the combustion chamber of an elemental analyzer with a high oxygen flow, causing the carbon to oxidize to carbon dioxide, which is then detected and quantified, particularly by a thermal conductivity detector. For example, one or more of the following parameters can be used: combustion furnace temperature 925 °C; gas flow rate: helium 140 ml / min, oxygen 90 ml / min; analysis duration 600 seconds.

[0037] The carbon fiber according to the invention further preferably contains a bio-based carbon content, measured according to ASTM D 6866-18 or EN 16640, greater than 5%, and preferably greater than 95%, relative to the total amount of carbon.

[0038] ASTM D 6866-18 and EN 16640, standards relating to the analysis of the bio-based (i.e., renewable) content of solid, liquid, or gaseous samples using radioactive carbon dating techniques, are well known to those skilled in the art and allow, in particular, the determination of the bio-based carbon content of materials. Biomass contains a characteristic amount of carbon-14, which is easily distinguished from other materials, such as fossil fuels, which contain only trace amounts of carbon-14.

[0039] Carbon fibers prepared from raw material derived from biomass, particularly cellulose as is the case according to the present invention, therefore contain a significant amount of carbon 14. Carbon fibers obtained from raw material derived from fossil resources, on the other hand, contain only traces of it.

[0040] In another aspect, the present invention relates to a method for preparing a carbon fiber according to the invention. According to this method, a cellulose-based fiber, preferably lignin-free, is subjected to a heat treatment, known as carbonization, comprising: a first phase comprising a temperature ramp-up step to a temperature between 500 and 700 °C, preferably between 500 and 550 °C, and holding at this temperature for a period between 30 seconds and 180 minutes, in particular between 30 seconds and 15 minutes, preferably between 30 seconds and 5 minutes, or between 15 and 180 minutes, this holding being referred to in this description as the "main stage of the first phase"; the cellulose-based fiber being stretched at a stretch ratio between 1.25 and 3, preferably between 1.3 and 3, and for example between 1.3 and 2, during this first phase;and a second phase comprising a temperature ramp-up step to a temperature between 900 and 1500 °C, preferably between 1000 and 1200 °C, and holding at this temperature for a period of between 1 and 40 minutes, in particular between 1 and 10 minutes, preferably between 5 and 10 minutes, or between 10 and 40 minutes, preferably between 10 and 20 minutes, this holding being referred to in this description as the "main plateau of the second phase"; the fiber being stretched at a stretch ratio between 0.7 and 1.1, preferably between 0.9 and 1.1, during this second phase.

[0041] Such a specific combination of fiber stretch ratio parameters during its heat treatment and temperature to be applied as a function of time, advantageously allows obtaining the particularly good properties stated above for carbon fiber, in particular its good tensile mechanical properties and its low density.

[0042] This combination of operating parameters results in a very significant stretching of the fibers, which at the end of the carbonization treatment have a length 23% greater, and can even go up to more than 50%, compared to the length of the cellulose-based precursor fiber initially used.

[0043] Furthermore, due to the use of such low carbonization temperatures—the maximum heat treatment temperature not exceeding 1500 °C, and preferably 1200 °C—the process according to the invention is energy-efficient, economical, and environmentally friendly. The savings in investment costs, as well as in energy and environmental terms, are particularly significant compared to prior art carbon fiber preparation processes using much higher carbonization temperatures.

[0044] Advantageously, the process according to the invention also does not require a prior step of thermal stabilization of the cellulose-based precursor fiber.

[0045] The process according to the invention thus advantageously makes it possible to obtain, at a temperature not exceeding 1500 °C, carbon fibers exhibiting low hydrostatic density and particularly high mechanical properties. These carbon fibers, which can therefore be obtained at low cost, are suitable for direct use in a large number of applications not requiring very high fiber strength, applications for which they prove to be much more economical than carbon fibers available in the prior art.Alternatively, they can be used as a base material for the formation of graphitized carbon fibers, by heat treatment at a temperature between 1800 and 3000 °C, typically between 2000 and 3000 °C, these graphitized carbon fibers exhibiting even better mechanical strength properties, and being particularly well suited for many other applications requiring greater mechanical strength of the fibers.

[0046] The process according to the invention may also meet one or more of the characteristics described below, implemented individually or in each of their technically operative combinations.

[0047] The heat treatment of the process according to the invention is preferably carried out continuously.

[0048] Preferably, for this heat treatment, the cellulose-based fiber is driven in a scrolling motion, preferably at a speed between 0.05 and 10 m / min, and preferably between 0.1 and 5 m / min, in a thermal device in which it is subjected to said heat treatment.

[0049] In this description, the term "thermal device" includes any device for heating the fiber to different temperatures, including devices comprising multiple ovens.

[0050] Thus, according to the invention, the thermal device can consist of a single oven or a plurality of ovens in which the fiber passes successively.

[0051] This oven, or these ovens, can be of any conventional type. Each can contain several distinct temperature zones, for example, 2 to 8 such independent temperature zones.

[0052] The fiber feed speed may be the same in all ovens, or differ from oven to oven.

[0053] The thermal device used is preferably of the type allowing the simultaneous carbonization of several fibers moving in parallel. Thus, in specific implementations, the process according to the invention achieves the simultaneous carbonization of several carbon fibers, each of these fibers being, for example, composed of 500 to 48,000 filaments.

[0054] Preferably, the first phase of the heat treatment is carried out in a first oven, called a low-temperature oven, and the second phase is carried out in a second oven, called a high-temperature oven.

[0055] The atmosphere in each of the furnaces used can be either air or an inert atmosphere, for example nitrogen or argon.

[0056] Each of the phases of the heat treatment of the process according to the invention can be carried out by establishing a plasma, in particular microwaves, in the device used.

[0057] For each phase of the heat treatment process according to the invention, the temperature ramp-up step may include several temperature ramp-up substeps, one or more temperature plateaus, and even one or more temperature drops, before reaching the main plateau of the phase. Each phase, in particular the first phase, may also include, after its main plateau, one or more temperature ramp-ups, temperature plateaus, and / or temperature drops, while not exceeding, for the first phase, a temperature of 700 °C, and for the second phase, a temperature of 1500 °C, preferably 1200 °C.

[0058] In preferred embodiments of the invention, the overall stretch ratio to which the fiber is subjected during heat treatment is greater than 1.2. This overall stretch ratio may also, for example, be less than or equal to 3.

[0059] The variation in fiber length during the process is preferably greater than or equal to 20%.

[0060] The process according to the invention can be implemented from any type of cellulose fiber, in particular viscose cellulose or Lyocell, or generated by a process comprising dissolving the cellulose in phosphoric acid or in an ionic liquid, with the possible incorporation of additives, as described above.

[0061] This cellulose-based precursor fiber can be any length.

[0062] Prior to the heat treatment, the process according to the invention may include a step of impregnating the cellulose-based fiber with an impregnation additive, for example, a silicone-based impregnation additive. This preliminary step can be carried out using any conventional method that is itself applicable to those skilled in the art. Non-limiting examples of impregnation additives that can be used in the context of the invention are listed above in this description.

[0063] The impregnation of cellulose fibers with silicone-type impregnation additives can also be preceded by a step of impregnating the fibers with sulfate and / or sulfonate-type additives.

[0064] At the end of the impregnation step(s), the cellulose-based fiber is preferably dried, in particular under air, before being subjected to the heat treatment of the process according to the invention.

[0065] In particular embodiments of the invention, the second phase of the heat treatment of the carbon fiber preparation process comprises: a temperature increase at a rate between 1 and 1000 °C / min, in particular between 1 and 200 °C.min -1, for example between 4 and 20 °C.min -1, or between 200 and 1000 °C / min, up to a temperature between 900 °C and 1500 °C, preferably between 1000 °C and 1300 °C, and preferably between 1000 and 1200 °C; and a plateau at this temperature, for a duration of between 1 and 40 minutes, in particular between 1 and 10 minutes, for example between 3 and 8 minutes or between 5 and 10 minutes, or between 10 and 40 minutes, preferably between 10 and 20 minutes.

[0066] The process according to the invention may further include one or more conventional final steps in themselves, such as surface treatment, dimensioning, drying, winding, etc.

[0067] In particular embodiments of the invention, the process includes a surface treatment step of the carbon fiber obtained after heat treatment, this step being carried out according to any conventional method in itself for the treatment of carbon fibers, for example: by exposure to acids in liquid or gaseous form, for example nitric acid HNO3, sulfuric acid H2SO4, etc.; by exposure to oxidants in liquid or gaseous form, for example oxygen O2, water H2O, carbon dioxide CO2, potassium permanganate KMnO4, sodium hypochlorite NaCl, etc.; by electrochemical treatment, in particular by anodic oxidation of the fiber immersed in an electrolytic solution, for example an aqueous solution of sodium chloride NaCl, ammonium sulfate (NH4)2SO4, sodium hydroxide NaOH, etc.; by treatment by exposure to a plasma, for example a plasma of air, oxygen, ammonia, argon, etc.

[0068] Carbon fiber can also be subjected to a sizing step, by impregnation with a conventional formulation in itself.

[0069] For their subsequent use, a plurality of carbon fibers according to the invention can be assembled, for example in the form of a non-woven fabric, or woven.

[0070] According to another aspect, the present invention relates to the use of a carbon fiber according to the invention for the manufacture of a composite material, in which a plurality of mechanically resistant fibers, called reinforcing fibers, are distributed in a matrix of organic polymer resin.

[0071] In particular embodiments of the invention, prior to their use for the manufacture of a composite material, the carbon fibers according to the invention are subjected to a graphitization step, carried out in a conventional manner in itself, preferably by heat treatment at a temperature between 1800 and 3000 °C.

[0072] After the graphitization stage, the fibers can undergo any subsequent conventional stage in itself, for example surface treatment, in particular as described above, sizing, drying, winding, etc.

[0073] Thus, the reinforcing fibers of the composite material can advantageously be made up of carbon fibers according to the invention, or of fibers obtained by graphitization of these carbon fibers.

[0074] A composite material is defined in this description in the classical sense, that is, as consisting of the assembly of several different materials or elementary components bonded together, more specifically mechanically resistant fibers distributed in a polymer organic resin matrix. The term resin here defines a polymer compound, which may be thermoplastic or thermosetting, that acts as a structural adhesive in which the fibers are dispersed in a more or less organized manner.

[0075] Within the composite material, the carbon fibers according to the invention, or the graphitized carbon fibers which may be derived from it, can be arranged into fabrics of different weights and weaves, for example in taffeta, twill, satin, etc., used alone or in combination, or in non-wovens, in which the fibers are all oriented in the same direction.

[0076] Any conventional organic polymer resin in itself can be used within the framework of the present invention, whether it is a thermosetting type resin, for example an epoxy resin or a phenolic resin, or a mixture of such resins; or a thermoplastic type resin, for example a polyamide resin or an acrylic resin, or a mixture of such resins.

[0077] The product thus described is a graphitized carbon fiber obtained by graphitization, that is, heat treatment at a temperature between 1800 and 3000 °C, of ​​a carbon fiber according to the invention. This graphitized carbon fiber has a tensile Young's modulus greater than or equal to 150 GPa, preferably greater than or equal to 200 GPa, and a tensile strength greater than or equal to 1500 MPa, preferably greater than or equal to 1800 MPa, and preferably greater than or equal to 2000 MPa. Its hydrostatic density is also advantageously low.

[0078] An additional aspect of the invention is a composite material in which a plurality of carbon fibers according to the invention are distributed in a polymer organic resin matrix.

[0079] This composite material can meet one or more of the characteristics described above. It advantageously takes advantage of the low cost, low density, and good mechanical properties of carbon fibers or graphitized carbon fibers according to the invention.

[0080] Such a composite material is, for example, particularly well suited for use in the automotive sector.

[0081] The features and advantages of the invention will become clearer in light of the following implementation examples, provided by way of illustration only and in no way limiting the invention, with the support of the figures 1 to 2 , in which: there figure 1shows a graph representing temperature profiles as a function of time for different processes according to the invention (temperature profiles P1, P2, P3 and P4); and the figure 2 represents an image, obtained by scanning electron microscopy, of isolated filaments of a carbon fiber obtained by a process according to the invention.

[0082] Examples of carbon fiber preparation processes according to the invention, implemented from cellulose-based fibers of the high-tenacity viscose process type, are described in detail below.

[0083] The cellulose-based fibers were obtained using a conventional high-tenacity viscose process, which involves dissolving the cellulose in a solution of sodium hydroxide and carbon disulfide. Each cellulose-based fiber contains approximately 1000 filaments, with an average filament diameter of 12.5 µm. Their density is 1840 dtex and their tenacity is 4.78 cN / dtex.

[0084] Cellulose-based fibers are impregnated with a silicone additive based on polydimethylsiloxane combined with a crosslinking agent, at a content of less than 10% by weight, by soaking the fibers in a silicone solution.

[0085] These cellulose-based fibers are fed successively, at a speed of 0.1 m / min, through two ovens, each with several independently adjustable temperature zones. The device used is conventional in itself.

[0086] In the first oven, called the low temperature oven, the cellulose-based fiber is subjected to a first stretching ratio of between 1.25 and 1.6, the exact value of which is indicated in Table 1 below, and to a first heat treatment phase including a temperature rise step up to a temperature of 550 °C, followed by a plateau of 15 to 180 min at this temperature.

[0087] In the second oven, called the high-temperature oven, the cellulose-based fiber is subjected to a second stretching ratio of between 0.95 and 1, the exact value of which is indicated in Table 1 below, and to a second heat treatment phase comprising a temperature ramp-up to a temperature of 1200 °C, followed by a plateau of 1 to 10 min at this temperature.

[0088] The exact temperature-time profiles applied according to the present invention and designated by the abbreviations P1, P2, P3, and P4 are shown on the figure 1 .

[0089] For comparison purposes, a similar process is also implemented, but in which the stretch ratios applied to the cellulose-based fibers do not conform to the present invention (comparative example Comp1).

[0090] As a result of these experiments, carbon fibers are obtained, each containing approximately 1000 filaments.

[0091] These carbon fibers are characterized as follows: The average filament diameter is calculated from the average of the diameter measurements of 15 individual filaments. These measurements are obtained from scanning electron microscopy images. The filament density is obtained as described in ISO 10119-2002-B2, using the gravimetric method. The Young's modulus and tensile strength are measured by tensile mechanical testing of specimens consisting of a carbon fiber monofilament bonded to a paper frame, as described in ISO 11566. The tests are performed on a machine equipped with a 5 N force sensor. The test speed is set at 1 mm / min. The initial tested length of the monofilament is 10 mm. The displacement and the generated force are measured. The Young's modulus (E) and tensile strength (σH) values ​​are calculated from these data and the previously obtained average diameter.8 test tubes are tested and the values ​​obtained are averaged.

[0092] All the carbon fibers obtained from the processes according to the invention have a Young's modulus in tension E greater than or equal to 85 GPa, a tensile breaking strength σ H greater than 1500 MPa, a hydrostatic density between 1.3 and 1.65 and a diameter between 3 and 4 µm.

[0093] Specific examples of the results obtained are shown in Table 1 below. In this table, experiments 1, 2 and 3 conform to the invention, and experiment Comp1 does not conform. Table 1 - properties of carbon fibers obtained by processes according to the invention and a comparative process Exp. Temperature profile 1st stretch ratio 2nd stretch ratio Overall stretch ratio Fiber length variation (%) E (GPa) σ H (MPa) 1 P1 1,268 0,955 1,231 23,1 85,0 1892 2 P1 1,566 0.965 1,510 51,0 108 2138 3 P4 1,300 0,963 1,270 27,0 91,9 2051 Comp1 P1 1,235 0,965 1,192 19,2 68,5 1419

[0094] As can be seen, the processes according to the invention (experiments 1, 2 and 3) all lead to carbon fibers with particularly good tensile mechanical properties, and superior to those obtained for the comparative process (experiment Comp1).

[0095] In particular, processes using a stretch ratio greater than or equal to 1.3 in the low temperature furnace (1st < stretch ratio) exhibit the best performance in terms of tensile mechanical properties of the formed fibers.

[0096] As an example, it is shown on the figure 2 An image obtained by scanning electron microscopy, at x9000 magnification, of 3 filaments constituting a carbon fiber obtained at the end of experiment 3, these 3 filaments having been separated from the rest of the fiber. The diameter of each of these filaments, indicated in the figure, is between 3.3 and 3.8 µm.

[0097] Carbon fibers obtained according to the invention are particularly well suited, where appropriate after further processing steps, for example graphitization, for use as reinforcing fibers in composite materials, for example intended for the automotive field.

Claims

1. Non-graphitised carbon fibre prepared from cellulose, comprising one or several filaments, characterised by: - a tensile Young's modulus, as determined according to the standard ISO 11566, which is greater than or equal to 85 GPa, - and a tensile breaking stress, as determined according to the standard ISO 11566, which is greater than or equal to 1800 MPa, and wherein said filament or said filaments each have a hydrostatic density, as determined according to the standard ISO 10119, comprised between 1.3 and 1.65 g / m3.

2. Carbon fibre according to claim 1, having a tensile Young's modulus which is greater than or equal to 90 GPa.

3. Carbon fibre according to any one of claims 1 to 2, comprising a carbon content, as measured by elemental analysis in a combustion chamber at a temperature of 925°C under a helium flow rate of 140 ml / min and an oxygen flow rate of 90 ml / min for 600 seconds, which is greater than or equal to 85%.

4. Carbon fibre according to any one of claims 1 to 3, containing a biobased carbon content, measured according to the ASTM D 6866-18 standard, which is greater than 95% relative to the amount of total carbon.

5. Carbon fibre according to any one of claims 1 to 4, wherein said filaments have an average diameter comprised between 3 and 10 µm.

6. Method for preparing a carbon fibre according to any one of claims 1 to 5, wherein a cellulose-based fibre is subjected to a heat treatment comprising: - a first phase comprising a step of rising the temperature to a temperature comprised between 500 and 700°C, and maintaining it at said temperature for a period comprised between 30 seconds and 180 minutes, said cellulose-based fibre being stretched at a stretch ratio comprised between 1.25 and 3 during said first phase; - and a second phase comprising a step of rising the temperature to a temperature comprised between 900 and 1500°C, and maintaining it at said temperature for a period comprised between 1 seconds and 40 minutes, said cellulose-based fibre being stretched at a stretch ratio comprised between 0.7 and 1.1 during said second phase.

7. Method according to claim 6, wherein the cellulose-based fibre is scroll driven at a speed comprised between 0.05 and 10 m / min in a thermal device wherein it is subjected to said heat treatment.

8. Method according to any one of claims 6 to 7, wherein the second phase of said heat treatment comprises: - a temperature rise at a rate comprised between 1 and 1000°C.min-1, up to a temperature comprised between 900°C and 1500°C; - and a plateau at said temperature, of a duration comprised between 1 and 40 minutes.

9. Method according to any one of claims 6 to 8, comprising a step of impregnating the cellulose-based fibre with an additive before said heat treatment.

10. Use of a carbon fibre according to any one of claims 1 to 5, for the manufacture of a composite material wherein a plurality of fibres are distributed in a matrix of organic polymer resin.

11. Use according to claim 10, wherein said carbon fibre is previously subjected to a graphitisation step, preferably at a temperature comprised between 1800 and 3000°C.

12. A composite material wherein a plurality of carbon fibres according to any one of claims 1 to 5, are distributed in a matrix of organic polymer resin.