MAGNETKUGEL

DE602021022602T2Active Publication Date: 2024-11-27SAINT GOBAIN CENT DE RES & DEVS & DETUD EUROEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602021022602
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-22
Filing Date
2021-12-17
Publication Date
2024-11-27
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

Zirconia balls used in microgrinding for food materials face issues of wear and contamination, with existing stabilization methods like Y2O3 being ineffective, leading to degradation in wear resistance and contamination of the ground material.

Method used

Sintered balls with specific crystallized phases, including stabilized zirconia, monoclinic zirconia, and a magnetic constituent such as magnetic spinels, garnets, or hexagonal ferrites, where the zirconia is stabilized with CeO2 and optionally Y2O3, allowing for magnetic separation of wear fragments while maintaining wear resistance.

Benefits of technology

The solution effectively reduces contamination and maintains good wear resistance by using CeO2 stabilization and magnetic separation, improving the durability and purity of the ground material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Technical field

[0001] The invention relates to sintered balls, in particular for grinding food materials. Prior art

[0002] Various industries use balls for fine grinding of materials, or “microgrinding”.

[0003] All these balls typically have a size of 0.03 mm to 10 mm.

[0004] Zirconia balls, at least partially stabilized, are commonly used: they offer a good compromise between wear resistance, density and chemical inertness. During microgrinding, some of these balls can nevertheless wear out, or even break, and contaminate the ground material.

[0005] Such contamination is particularly detrimental in the agri-food sector.

[0006] There is a constant need for zirconia balls with good wear resistance and to limit contamination of the ground material.

[0007] An aim of the invention is to solve, at least partially, this problem. Document US 2002 / 047058 A1 describes magnetic materials for sintered balls, for example Sr or Ba ferrite, and materials based on stabilized zirconia comprising CeO 2 . Summary of the invention

[0008] According to the invention, this aim is achieved by means of a sintered ball having the following crystallized phases, in percentages by mass based on the crystallized phases and for a total of 100%: stabilized zirconia: complement 100%; monoclinic zirconia: ≤ 20%; 4% ≤ magnetic constituent ≤ 22%; crystallized phases other than stabilized zirconia, monoclinic zirconia and magnetic constituent: < 10%; the magnetic constituent being chosen from magnetic spinels, magnetic garnets, magnetic hexagonal ferrites and mixtures thereof; the sintered ball comprising, apart from the magnetic constituent, CeO 2 and optionally Y 2 O 3 , in contents such that, in molar percentages based on the sum of ZrO 2 , CeO 2 and Y 2 O 3 , 1.5% ≤ CeO 2 ≤ 17.5% and 1.5% ≤ Y 2 O 3 + (CeO 2 ) / 3.5 ≤ 5%.

[0009] The addition of such a magnetic constituent, in the quantities mentioned, makes it possible to magnetically separate the fragments resulting from wear, while maintaining good wear resistance. The inventors discovered that it was however necessary for the stabilization of the zirconia to be at least partially obtained with CeO 2 , Y 2 O 3 being optionally only able to be present in addition to CeO 2 . In particular, they found that the wear resistance is degraded if the stabilized zirconia is entirely stabilized with Y 2 O 3 .

[0010] Y 2 O 3 is the most widely used zirconia stabilizer in the intended application. Observing its ineffectiveness, it is the inventors' merit to have tested other zirconia stabilizers to discover the specific and unexpected effect of CeO 2 . Without being bound by this theory, the inventors believe that the presence of a magnetic constituent could lead to destabilization of a portion of said zirconia stabilized with Y 2 O 3 .

[0011] Furthermore, excluding the magnetic constituent, the molar content of Y 2 O 3 must be adapted to the molar content of CeO 2 and the molar contents of these two oxides must be linked by the relationship 1.5% ≤ Y 2 O 3 + (CeO 2 ) / 3.5 ≤ 5%.

[0012] A sintered ball according to the invention may also comprise one or more of the following optional and preferred characteristics: excluding magnetic constituent, 3% ≤ CeO 2 , preferably 5% ≤ CeO 2 , and / or CeO 2 ≤ 16%, preferably CeO 2 ≤ 15%, in molar percentages based on the sum of ZrO 2 , CeO 2 and Y 2 O 3 ; excluding magnetic constituent, Y 2 O 3 + (CeO 2 ) / 3.5 is greater than or equal to 2% and less than or equal to 4%; the zirconia is stabilized entirely with CeO 2 , or in which the stabilized zirconia is stabilized entirely with CeO 2 and Y 2 O 3 ; the stabilized zirconia is present, for more than 90%, in the form of quadratic zirconia, in mass percentage based on the stabilized zirconia; the ball has a monoclinic zirconia content, in percentage by mass based on the total quantity of crystallized phases, of less than or equal to 10%; the ball has a magnetic constituent content of greater than or equal to 5% and less than or equal to 18%, in percentages by mass based on the crystallized phases;the ball has a magnetic constituent content greater than or equal to 7% and less than or equal to 15%, in percentages by mass based on the crystallized phases; said magnetic spinel is made up, excluding oxygen and for more than 90% of its mass, of iron and zinc and copper, iron and copper and aluminum, iron and nickel, iron and cobalt, iron and copper, iron and zinc, iron and magnesium, iron and manganese, iron and nickel and zinc, iron and nickel and zinc and copper, iron and manganese and zinc, iron and manganese and zinc and aluminum, iron and lithium and zinc and nickel and manganese, iron and zinc and lithium, iron and zinc and copper and aluminum and calcium, and mixtures thereof; said magnetic garnet is chosen from garnets containing iron;the magnetic hexagonal ferrite is selected from an M-type hexagonal ferrite, a W-type hexagonal ferrite and mixtures thereof; 0.2% ≤ Al 2 O 3 ≤ 2%, Al 2 O 3 being expressed excluding the magnetic constituent; CaO ≤ 1.5%, CaO being expressed excluding the magnetic constituent; the ball has: a size less than 10 mm and greater than 0.01 mm, and a sphericity greater than 0.85.;

[0013] The invention also relates to a sintered bead powder comprising more than 90%, preferably more than 95%, preferably substantially 100%, in mass percentages, of sintered beads according to the invention.

[0014] The invention also relates to a method for manufacturing sintered balls according to the invention, said method comprising the following successive steps: a) preparation of a particulate mixture having a median size of less than 2 µm and a composition suitable for obtaining, at the end of step g), sintered balls according to the invention, b) optionally, drying said particulate mixture, c) preparation of a starting charge from said particulate mixture, optionally dried, d) shaping the starting charge in the form of raw balls, e) optionally, washing, f) optionally, drying, g) sintering at a sintering temperature above 1100°C so as to obtain sintered balls.

[0015] The invention also relates to a method for extracting beads and / or bead fragments according to the invention, said method comprising the following step: 2) applying a magnetic field to said beads and / or said bead fragments, so as to attract said beads and / or said bead fragments.

[0016] The magnetic nature of the material of the beads according to the invention advantageously makes it possible to extract the fragments of the beads and / or the beads from a load, solid or liquid, in particular to purify a load or prepare it for a subsequent step, or to recover fragments of beads and / or beads in order to recycle or reuse them. The method can be implemented in particular to purify a load resulting from a grinding, dispersion, homogenization or projection operation on a surface.

[0017] In one embodiment, step 2) is preceded by a following step 1): 1) mixing a material to be ground, dispersed, homogenized, or separated, with beads according to the invention and / or fragments of beads according to the invention, then if a material to be ground, dispersed, or homogenized has been mixed with said beads and / or with said fragments of beads, grinding, dispersing or homogenizing said mixture, respectively, so as to obtain a charge, the magnetic field being applied to said charge in step 2).

[0018] The mixture can be advantageously purified due to the extraction of the beads and / or bead fragments according to the invention. Step 2) is then a step of purification of the charge by extraction according to the invention, the magnetic field being applied to said charge.

[0019] A material is "to be separated" when, after having been mixed with beads and / or fragments of beads according to the invention, it is necessary to separate it from said beads and / or said fragments of beads. The mixture may in particular be a set of particles resulting from a projection of beads according to the invention onto a surface.

[0020] The magnetic nature of the bead material also allows said beads and / or fragments of said beads to be isolated from a substrate on the surface of which said beads and / or fragments of said beads rest.

[0021] The substrate may in particular be a part onto which balls according to the invention have been projected or an apparatus used for said projection.

[0022] In one embodiment, step 2) is preceded by a following step 1'): 1') projection of balls and / or fragments of balls according to the invention onto a surface to be treated, for example a metal surface, by means of a projection apparatus, the magnetic field being applied to said metal surface or to said projection apparatus in step 2).

[0023] Step 2) is then a step of recovering said beads or said bead fragments by extraction according to the invention, the magnetic field being applied to said substrate surface, the substrate surface being able to be in particular the surface to be treated and / or a surface of said projection apparatus.

[0024] In step 2), the magnetic field can be applied in particular to a surface of the projection device in contact with the balls during the projection operation. It thus makes it possible to recover unprojected balls, particularly those lodged in places that are difficult to access.

[0025] It can also be applied to the treated surface in order to clean it and recover the beads and bead fragments that are on this surface. The method is particularly effective when the surface has cavities in which the beads and bead fragments can lodge. The invention also relates to the use of a sintered bead powder according to the invention, as a grinding medium, dispersion medium, homogenization medium, or media for surface treatment, as well as a device chosen from a suspension, a grinder, a surface treatment apparatus, a cell lysis apparatus, said device comprising a sintered bead powder according to the invention, in particular manufactured according to a method according to the invention. Definitions

[0026] The term "particle" means a solid product individualized in a powder. "Powder" and "particulate mixture" are conventionally synonyms. For the sake of clarity, in this description, the term "particulate mixture" refers to the powder that is manufactured in step a) of a method for manufacturing sintered balls according to the invention. The term "sintering" is conventionally used to refer to the consolidation by heat treatment at more than 1100°C of a raw particle (granular agglomerate), with possibly partial or total fusion of some of its constituents (but not all of its constituents). The "grains" of a sintered ball are made up of the particles of the particulate mixture agglomerated by sintering. A sintered ball according to the invention is thus made up of an agglomerate of grains bonded by sintering. It may also comprise an amorphous phase.By "ball" is meant a particle having a sphericity, that is to say a ratio between its smallest Ferret diameter and its largest Ferret diameter, greater than 0.6, regardless of the way in which this sphericity was obtained. Preferably, the balls according to the invention have a sphericity greater than 0.7. The term "size" of a ball refers to its smallest Ferret diameter. The term "percentiles" 10 (noted D 10 ), 50 (noted D 50 ) and 90 (noted D 90 ) of a powder or particulate mixture are used, the particle sizes corresponding to the percentages equal to 10%, 50% and 90%, respectively, by mass, on the cumulative particle size distribution curve of the particle sizes of the powder or particulate mixture respectively, said particle sizes being classified in ascending order.According to this definition, 10% by mass of the particles of the powder or particulate mixture thus have a size less than D 10 and 90% of the particles, by mass, have a size greater than or equal to D 10 . The percentiles can for example be determined using a laser diffraction granulometer. The "median size" of a powder of particles or of a particulate mixture is called the 50th percentile, D 50 . The median size therefore divides the particles of the powder or of the particulate mixture into first and second populations equal in mass, these first and second populations comprising only particles having a size greater than or equal to, or less than, respectively, the median size. By "sintered ball" is meant a solid ball obtained by sintering a green ball. In the context of this application, HfO 2 is considered not to be chemically dissociable from ZrO 2 .Furthermore, according to the present invention, HfO 2 is not intentionally added to the starting charge and is only present in trace amounts, this oxide always being naturally present in zirconia sources. In a ball according to the invention, HfO 2 < 4%. In the chemical composition of a product comprising zirconia, "ZrO 2" therefore designates the total content of these two oxides, i.e. "ZrO 2 +HfO 2".

[0027] The magnetic component may also include a small amount of zirconium. Unless otherwise indicated, ZrO 2 refers to the zirconium oxide (and hafnium oxide) content in the beads. In this description and in the claims, "zirconia" refers to the total content of zirconia and hafnia. “Stabilized zirconia” means the assembly consisting of quadratic zirconia and cubic zirconia. “Powder of a compound” means a powder comprising more than 95% by mass of particles comprising more than 90% by mass of said compound. Thus, a corundum powder comprises more than 95% by mass of particles comprising more than 90% by mass of corundum. A “quadratic zirconia powder” comprises more than 95% by mass of particles comprising more than 90% by mass of quadratic zirconia. A “stabilized zirconia powder” comprises more than 95% by mass of particles comprising more than 90% by mass of stabilized zirconia. “Precursor” of a constituent means one or more ingredients capable of providing said constituent during a sintering step of a manufacturing method according to the invention. For example, aluminum hydroxides are precursors of alumina.An amount of a precursor of an oxide is said to be "equivalent" to an amount of said oxide when, upon sintering, it leads to said amount of said oxide. By "spinel" is conventionally meant the cubic crystallographic structure corresponding to a particular arrangement of elements A and elements B in sites conventionally called "octahedral sites" and "tetrahedral sites". Compounds having a spinel crystallographic structure include compounds of formula AB 2 O 4 called "direct spinels", in which the elements A occupy a tetrahedral site and the elements B occupy an octahedral site. In compounds of formula B(A,B)O 4 , called "inverse spinels", the elements B occupy tetrahedral and octahedral sites and the elements A occupy an octahedral site.An example of a magnetic spinel is the inverse spinel NiFe 2 O 4 , where A is nickel arranged on octahedral sites, and B is iron arranged on octahedral sites and tetrahedral sites. The term "garnet" is conventionally understood to mean a compound with a cubic crystallographic structure corresponding to a particular arrangement of C elements and D elements of the formula C 3 D 5 O 12 . An example of a magnetic garnet is the garnet Y 3 Fe 5 O 12 , where element C is yttrium and element D is iron.By "hexagonal ferrite" is conventionally meant a compound of hexagonal crystallographic structure corresponding to a particular arrangement of elements E and elements F of formula EF 12 O 19 , conventionally called hexagonal ferrite of type M, such as for example BaFe 12 O 19 ; or of formula E 3 F 16 O 27 , conventionally called hexagonal ferrite of type W, such as for example BaCo 2 Fe 16 O 27 ; or of formula E 4 F 28 O 46 , conventionally called hexagonal ferrite of type X, such as for example Ba 2 Co 2 Fe 28 O 46 ; or of formula E 4 F 12 O 22 , conventionally called hexagonal ferrite of type Y, such as for example Ba 2 Zn 2 Fe 12 O 22 ; or of formula E 5 F 24 O 41 , classically called hexagonal ferrite of type Z, such as for example Ba 3 Co 2 Fe 24 O 41 ; or of formula E 6 F 36 O 60 , classically called hexagonal ferrite of type U, such as for example Ba 4 Zn 2 Fe 36 O 60 .Conventionally, in a hexagonal ferrite, the iron element can be partially or even totally substituted by another element. A constituent is said to be "magnetic" when it has a mass magnetization greater than 2 Am 2< .kg -1< measured at an excitation magnetic field equal to 100 kA / m. Thus, a magnetic constituent can be attracted by a magnet. The magnetic magnetization of a constituent or a bead is conventionally measured using a vibrating sample magnetometer, by subjecting it to an excitation magnetic field of 100 kA / m, at room temperature (20°C).

[0028] Some magnetic constituents, such as hexagonal ferrite, may exhibit hysteresis. The magnetic field is then increased until it exceeds the saturation mass magnetization, for example beyond 2500 kA / m, then decreased to 100 kA / m to perform the measurement.

[0029] Magnetic spinels, magnetic garnets, and magnetic hexagonal ferrites are well known. If in doubt, a simple measurement of the mass magnetization, as shown above, can verify whether a spinel, garnet, or ferrite is magnetic.

[0030] Magnetic spinels, magnetic garnets, and magnetic hexagonal ferrites may contain cerium and / or yttrium. This cerium and / or yttrium are, however, not taken into account when determining the "non-magnetic" contents. In other words, "non-magnetic" means that the contents of ZrO 2 and / or CeO 2 and / or Y 2 O 3 referred to do not take into account any ZrO 2 and / or CeO 2 and / or Y 2 O 3 that may be present in the magnetic component. Unless otherwise stated, CeO 2 and Y 2 O 3 are molar percentages excluding the magnetic component based on the sum of ZrO 2 , CeO 2 and Y 2 O 3 excluding the magnetic component.

[0031] Similarly, Al 2 O 3 or CaO contents expressed “excluding magnetic constituent” are determined without taking into account the Al 2 O 3 or CaO possibly present in the magnetic constituent; For the sake of clarity, the terms "ZrO 2 ", "CeO 2 ", "Y 2 O 3 ", "Al 2 O 3 ", "Fe 2 O 3 ", "ZnO", "CuO" and "La 2 O 3" are used to designate the contents of these oxides in the composition, and "zirconia", "cerina", "yttrium", "corundum", "iron oxide", "zinc oxide", "copper oxide" and "lanthanum oxide" are used to designate crystallized phases of these oxides consisting of ZrO 2 , CeO 2 , Y 2 O 3 , Al 2 O 3 , Fe 2 O 3 , ZnO, CuO and La 2 O 3 respectively. These oxides may, however, also be present in other phases. In a preferred embodiment, ZrO 2 , Y 2 O 3 and CeO 2 are present, or even exclusively present in the form of stabilized zirconia. The term "zirconia" conventionally includes the small amount of hafnia phase, not distinguishable by X-ray diffraction.A "non-oxygen" mass content of a constituent in a product is the mass percentage of that constituent based on the mass of the product without taking oxygen into account. For example, when a product is "consisting, excluding oxygen and for more than 80% of its mass, of iron", the iron represents more than 80% of the mass of the product without taking into account the oxygen present in the product. The specific surface area is calculated by the BET (Brunauer Emmet Teller) method as described in Journal of American Chemical Society 60 (1938), pages 309 to 316. Unless otherwise stated, all averages are arithmetic averages. Unless otherwise stated, all percentages are mass percentages based on the oxides. A mass content of an element is expressed in the form of the most stable oxide. In particular, each element of the magnetic constituent is converted to the form of the most stable oxide of that element.“Behave” or “include” or “exhibit” should be interpreted in a non-limiting manner. All characteristics of the beads can be measured in accordance with the protocols described for the examples. Detailed description Sintered ball

[0032] A sintered ball according to the invention preferably consists of oxides for more than 98%, preferably for more than 99%, preferably for more than 99.5%, preferably for more than 99.9%, of its mass. Preferably, the sintered ball according to the invention consists substantially entirely of oxides.

[0033] Preferably, in the sintered ball according to the invention, the mass quantity of amorphous phase, i.e. vitreous, as a percentage by mass relative to the mass of said ball, is less than 7%, preferably less than 5%, preferably substantially zero.

[0034] The sintered ball according to the invention is remarkable for the stabilization of the stabilized zirconia: the zirconia is in fact specifically stabilized with CeO 2 and optionally Y 2 O 3 .

[0035] Preferably, in a sintered ball according to the invention, the zirconia is stabilized only by CeO 2 , and optionally Y 2 O 3 .

[0036] Preferably, in the sintered ball according to the invention, excluding the magnetic constituent, the CeO 2 content, in molar percentages based on the sum of ZrO 2 , CeO 2 and Y 2 O 3 , is greater than or equal to 2%, preferably greater than or equal to 3%, preferably greater than or equal to 5%, and preferably less than or equal to 16%, preferably less than or equal to 15%.

[0037] Preferably, in the sintered ball according to the invention, excluding the magnetic constituent, the contents of CeO 2 and Y 2 O 3 , in molar percentages based on the sum of ZrO 2 , CeO 2 and Y 2 O 3 , are such that the sum Y 2 O 3 + (CeO 2 ) / 3.5 is greater than or equal to 2%, preferably greater than or equal to 2.5%, and preferably less than or equal to 4%.

[0038] In one embodiment, the stabilized zirconia is stabilized entirely with CeO 2 (no Y 2 O 3 stabilizer) and the CeO 2 content, excluding magnetic constituent, is greater than or equal to 2%, preferably greater than or equal to 3%, preferably greater than or equal to 5%, and less than or equal to 17.5%, preferably less than or equal to 16%, preferably less than or equal to 15%, in molar percentages based on the sum of ZrO 2 and CeO 2 .

[0039] In one embodiment, the stabilized zirconia is stabilized with CeO 2 and Y 2 O 3 , and the contents of CeO 2 and Y 2 O 3 excluding the magnetic component are such that, in molar percentages based on the sum of ZrO 2 , CeO 2 and Y 2 O 3 : CeO 2 is greater than or equal to 2%, preferably greater than or equal to 3%, preferably greater than or equal to 5%, and preferably less than or equal to 16%, preferably less than or equal to 15%, and Y 2 O 3 + (CeO 2 ) / 3.5 is greater than or equal to 2%, preferably greater than or equal to 2.5%, and less than or equal to 4%.

[0040] Preferably, in this embodiment, excluding the magnetic constituent, the Y 2 O 3 content in molar percentages based on the sum of ZrO 2 , CeO 2 and Y 2 O 3 is greater than or equal to 0.5%, preferably greater than or equal to 0.8%, and preferably less than or equal to 2%, preferably less than or equal to 1.5%.

[0041] Preferably, the stabilized zirconia is present, for more than 90%, more than 95%, more than 98%, preferably substantially 100%, in the form of quadratic zirconia, in mass percentage based on the stabilized zirconia. The limitation of the CeO 2 content advantageously makes it possible to limit the quantity of cubic zirconia.

[0042] The sintered ball according to the invention has a monoclinic zirconia content, as a percentage by mass based on the total quantity of crystallized phases, of less than or equal to 20%, preferably less than or equal to 15%, preferably less than or equal to 10%, preferably less than or equal to 7%, preferably less than or equal to 5%.

[0043] The sintered ball according to the invention is also remarkable for the presence of a magnetic constituent, specifically chosen from magnetic spinels, magnetic garnets, magnetic hexagonal ferrites and their mixtures.

[0044] Preferably, the magnetic constituent has a mass magnetization greater than 5 Am 2< .kg -1< , preferably greater than 10 Am 2< .kg -1< , preferably greater than 15 Am 2< .kg -1< , preferably greater than 20 Am 2< .kg -1< , measured at an excitation magnetic field equal to 100 kA / m.

[0045] Preferably, the magnetic constituent is selected from magnetic spinels, magnetic hexagonal ferrites and mixtures thereof. More preferably, the magnetic constituent is selected from magnetic spinels.

[0046] Preferably, said magnetic spinel is chosen from spinels comprising iron, preferably from spinels comprising iron on the one hand, and manganese and / or zinc and / or nickel and / or copper and / or cobalt and / or chromium and / or lithium and / or titanium and / or tin and / or magnesium and / or aluminum and / or cerium and / or calcium on the other hand, and mixtures thereof.

[0047] Preferably, said magnetic spinel is selected from spinels comprising iron and zinc and copper, iron and copper and aluminum, iron and nickel, iron and cobalt, iron and copper, iron and zinc, iron and magnesium, iron and manganese, iron and nickel and zinc, iron and nickel and zinc and copper, iron and manganese and zinc, iron and manganese and zinc and aluminum, iron and lithium and zinc and nickel and manganese, iron and zinc and lithium, iron and zinc and copper and aluminum and calcium, and mixtures thereof. Preferably, said magnetic spinel is selected from spinels comprising iron and zinc and copper, iron and manganese and zinc, and mixtures thereof.

[0048] Preferably, said magnetic spinel is chosen from spinels consisting, excluding oxygen and for more than 80%, preferably for more than 90%, preferably for more than 95%, preferably for more than 98% of their mass, of iron and zinc and copper, iron and copper and aluminum, iron and nickel, iron and cobalt, iron and copper, iron and zinc, iron and magnesium, iron and manganese, iron and nickel and zinc, iron and nickel and zinc and copper, iron and manganese and zinc, iron and manganese and zinc and aluminum, iron and lithium and zinc and nickel and manganese, iron and zinc and lithium, iron and zinc and copper and aluminum and calcium, and mixtures thereof.

[0049] Preferably, said magnetic spinel is chosen from spinels consisting, excluding oxygen and for more than 80%, preferably for more than 90%, preferably for more than 95%, preferably for more than 98% of their mass, of iron and zinc and copper, iron and manganese and zinc, or a mixture of these elements.

[0050] Preferably, said magnetic garnet is chosen from garnets comprising iron, preferably from garnets comprising iron on the one hand, and yttrium and / or ytterbium and / or erbium and / or dysprosium and / or samarium and / or gadolinium on the other hand, and mixtures thereof.

[0051] Preferably, said magnetic garnet is chosen from garnets comprising iron and yttrium, iron and ytterbium, and mixtures thereof.

[0052] Preferably, said magnetic garnet is chosen from garnets consisting, excluding oxygen and for more than 80%, preferably for more than 90%, preferably for more than 95%, preferably for more than 98% of their mass, of iron and yttrium, iron and ytterbium, and their mixtures.

[0053] Preferably, the magnetic hexagonal ferrite is selected from M-type hexagonal ferrite, W-type hexagonal ferrite and mixtures thereof. Preferably, the magnetic hexagonal ferrite is M-type hexagonal ferrite.

[0054] Preferably, said magnetic hexagonal ferrite, preferably of type M, is chosen from hexagonal ferrites comprising iron, preferably from hexagonal ferrites comprising iron on the one hand, and barium and / or strontium and / or lanthanum and / or calcium and / or cerium and / or aluminum and / or cobalt and / or titanium and / or gallium and / or indium and / or manganese and / or zinc and / or nickel and / or copper and / or chromium and / or magnesium on the other hand, and mixtures thereof.

[0055] Preferably, said hexagonal ferrite, preferably of type M, is chosen from hexagonal ferrites comprising iron and barium, iron and strontium, iron and barium and cobalt and titanium, iron and strontium and cobalt and titanium, iron and barium and cobalt, iron and lanthanum and aluminum, iron and barium and aluminum, iron and strontium and aluminum, iron and barium and aluminum and calcium, iron and barium and aluminum and calcium, and mixtures thereof.

[0056] Preferably, said hexagonal ferrite, preferably of type M, is chosen from hexagonal ferrites consisting, excluding oxygen and for more than 80%, preferably for more than 90%, preferably for more than 95%, preferably for more than 98% of their mass, of iron and barium, iron and strontium, iron and barium and cobalt and titanium, iron and strontium and cobalt and titanium, iron and barium and cobalt, iron and lanthanum and aluminum, iron and barium and aluminum, iron and strontium and aluminum, iron and barium and aluminum and calcium, iron and barium and aluminum and calcium, and mixtures thereof.

[0057] More preferably, said hexagonal ferrite, preferably of type M, is chosen from hexagonal ferrites consisting, excluding oxygen and for more than 80%, preferably for more than 90%, preferably for more than 95%, preferably for more than 98% of their mass, of iron and lanthanum and aluminum, iron and barium, iron and strontium, iron and barium and aluminum, iron and barium and strontium, and mixtures thereof.

[0058] Preferably, the ball according to the invention has a magnetic constituent content greater than or equal to 5%, preferably greater than or equal to 6%, preferably greater than or equal to 7%, preferably greater than or equal to 8%, and preferably less than or equal to 21%, preferably less than or equal to 20%, preferably less than or equal to 18%, preferably less than or equal to 15%, in percentages by mass on the basis of the crystallized phases and for a total of 100%.

[0059] Preferably, the ball according to the invention has a mass magnetization greater than 1 Am 2< .kg -1< , preferably greater than 2 Am 2< .kg -1< , preferably greater than 3 Am 2< .kg -1< , preferably greater than 4 Am 2< .kg -1< , measured at an excitation magnetic field equal to 100 kA / m.

[0060] The sintered ball according to the invention preferably has a total content of crystallized phases other than stabilized zirconia, monoclinic zirconia and magnetic constituent, in percentage by mass based on the total quantity of crystallized phases, of less than 6%, preferably less than 5%, or even less than 4%.

[0061] In a preferred embodiment, the sintered ball according to the invention has the following crystallized phases, in percentages by mass based on the crystallized phases and for a total of 100%: stabilized zirconia: complement to 100%; monoclinic zirconia: ≤ 20%, preferably less than or equal to 15%, preferably less than or equal to 10%, preferably less than or equal to 7%, preferably less than or equal to 5%, preferably substantially zero; magnetic constituent: content greater than or equal to 4%, preferably greater than or equal to 5%, preferably greater than or equal to 6%, preferably greater than or equal to 7%, preferably greater than or equal to 8%, and preferably less than or equal to 21%, preferably less than or equal to 20%, preferably less than or equal to 18%, preferably less than or equal to 15%; crystallized phases other than stabilized zirconia, monoclinic zirconia, and magnetic constituent: < 7%, preferably less than 6%, preferably less than 5%, or even less than 4%; the magnetic constituent being chosen from spinels comprising iron and zinc and copper, iron and copper and aluminum, iron and nickel, iron and cobalt, iron and copper, iron and zinc, iron and magnesium, iron and manganese, iron and nickel and zinc, iron and nickel and zinc and copper, iron and manganese and zinc, iron and manganese and zinc and aluminum, iron and lithium and zinc and nickel and manganese, iron and zinc and lithium, iron and zinc and copper and aluminum and calcium, and mixtures thereof, and among the hexagonal ferrites, preferably of type M, chosen from the hexagonal ferrites comprising iron and barium, iron and strontium, iron and barium and cobalt and titanium, iron and strontium and cobalt and titanium, iron and barium and cobalt, iron and lanthanum and aluminum, iron and barium and aluminum, iron and strontium and aluminum, iron and barium and aluminum and calcium, iron and barium and aluminum and calcium, and mixtures thereof, and mixtures thereof, said stabilized zirconia being stabilized with CeO 2 and optionally with Y 2 O 3 , CeO contents 2 and Y 2 O 3 , excluding magnetic constituent, in molar percentages based on the sum of ZrO 2 , from CeO 2 and Y 2 O 3 , being such that: CeO 2 is greater than or equal to 2%, preferably greater than or equal to 3%, preferably greater than or equal to 5%, and preferably less than or equal to 16%, preferably less than or equal to 15%, and Y 2 O 3 + (CeO 2 ) / 3.5 is greater than or equal to 2%, preferably greater than or equal to 2.5%, and less than or equal to 4%, said sintered ball having a mass quantity of amorphous phase, as a percentage by mass relative to the mass of said sintered ball, of less than 7%, preferably less than 5%, preferably substantially zero.

[0062] The composition of the sintered ball is mainly made up of ZrO 2 , CeO 2 , Y 2 O 2 and the oxides of the elements of the magnetic constituent.

[0063] In one embodiment, the sintered ball according to the invention has an Al 2 O 3 content greater than or equal to 0.2%, preferably greater than or equal to 0.25% and preferably less than 3%, preferably less than or equal to 2.5%, preferably less than or equal to 2%, preferably less than or equal to 1.2%, preferably less than or equal to 1%, preferably less than or equal to 0.8%, preferably less than or equal to 0.5%, in percentages by mass based on the oxides, said Al 2 O 3 content not taking into account the aluminum content, expressed in the form Al 2 O 3 , possibly present in the magnetic constituent.

[0064] The sintered ball according to the invention preferably has a CaO content of less than 1.5%, preferably less than 1.0%, in percentages by mass based on the oxides, said CaO content not taking into account the calcium content, expressed in the form of CaO, possibly present in the magnetic constituent.

[0065] In one embodiment, the sintered ball according to the invention has a CaO content greater than 0.1%, preferably greater than 0.2%, preferably greater than 0.3%, as a percentage by mass based on the oxides, said CaO content not taking into account the calcium content, expressed in the form of CaO, possibly present in the magnetic constituent.

[0066] Preferably, the sintered ball according to the invention has a surface density of pores, measured on images taken by Scanning Electron Microscopy, of less than 5%, preferably less than 4%, preferably less than 2%, preferably less than 1%.

[0067] The sintered ball according to the invention preferably has a size less than 10 mm, preferably less than 8 mm, and / or greater than 0.01 mm, preferably greater than 0.02 mm, preferably greater than 0.03 mm. In one embodiment, the sintered ball according to the invention preferably has a size less than 8 mm, preferably less than 7 mm and greater than 2 mm, preferably greater than 3 mm.

[0068] A sintered ball according to the invention preferably has a sphericity greater than 0.7, preferably greater than 0.8, preferably greater than 0.85, or even greater than 0.9. Sintered ball manufacturing process

[0069] To manufacture sintered balls according to the invention, steps a) to g) described above and detailed below can be carried out.

[0070] In step a), a particulate mixture having a median size of less than 2 µm is prepared. The composition of the particulate mixture is adapted, in a manner known per se, so that the sintered balls have a composition in accordance with the invention.

[0071] The raw material powders are mixed thoroughly.

[0072] The raw material powders may be individually ground or, preferably, co-ground so that the resulting particle mixture has a median size of less than 2 µm, preferably less than 1.5 µm, preferably less than 1 µm, preferably less than 0.8 µm, preferably less than 0.6 µm, preferably less than 0.5 µm, preferably less than 0.4 µm, preferably less than 0.3 µm and / or preferably greater than 0.05 µm. This grinding may be wet grinding. Grinding or co-grinding may also be used to obtain an intimate mixture.

[0073] Y 2 O 3 and CeO 2 are known stabilizers of zirconia. In the particulate mixture, they may or may not stabilize the zirconia. According to the invention, however, the particulate mixture must lead to a sintered ball according to the invention.

[0074] Ceria and / or a ceria precursor and / or yttria and / or a yttria precursor may, partially or completely, be incorporated into the particulate mixture in a form separate from the zirconia, so that after sintering, the zirconia is at least partly stabilized. In this embodiment, the median size of the yttria powder and / or the yttria precursor and / or ceria and / or the ceria precursor is preferably less than 1 µm, preferably less than 0.5 µm, more preferably less than 0.3 µm. The effectiveness of the stabilization of the zirconia is thereby advantageously improved during sintering.

[0075] In one embodiment, the particulate mixture comprises a monoclinic zirconia powder as the sole source of zirconia, and a ceria powder as the sole source of CeO 2 . The zirconia is only stabilized with CeO 2 at the end of step g).

[0076] In one embodiment, the particulate mixture comprises a ceria powder as the sole source of CeO 2 and a zirconia powder at least partly stabilized with Y 2 O 3 as the sole source of zirconia. The zirconia only becomes stabilized with CeO 2 and Y 2 O 3 at the end of step g). Preferably, the zirconia powder at least partly stabilized with Y 2 O 3 has a specific surface area, calculated by the BET method, greater than 0.5 m 2 < / g, preferably greater than 1 m 2 < / g, preferably greater than 1.5 m 2 < / g, and / or less than 20 m 2 < / g, preferably less than 18 m 2 < / g, preferably less than 15 m 2 < / g. Advantageously, the optional grinding, generally in suspension, is facilitated.

[0077] In one embodiment, the particulate mixture comprises particles in which zirconia, stabilized or not, and ceria and / or yttria are intimately mixed. Such an intimate mixture can for example be obtained by co-precipitation or atomization, and optionally consolidated by a heat treatment. In such a particulate mixture, ceria and / or yttria can be replaced by an equivalent quantity of precursor(s).

[0078] Preferably, the particulate mixture does not include a yttrium precursor.

[0079] Preferably, the particulate mixture does not include a ceria precursor.

[0080] Preferably, the particulate mixture does not include a zirconia precursor.

[0081] Preferably, when the sintered ball comprises zirconia stabilized with CeO 2 and Y 2 O 3 at the end of step g), the particulate mixture does not comprise monoclinic zirconia powder.

[0082] In one embodiment, in particular when the magnetic constituent comprises substantially no ZrO 2 , nor CeO 2 , nor Y 2 O 3 , and when the sintered ball comprises zirconia only stabilized with CeO 2 at the end of step g), the CeO 2 content in the particulate mixture is greater than or equal to 3%, preferably greater than or equal to 5%, preferably greater than or equal to 7% and / or less than 17.5%, preferably less than 14%, preferably less than 12%, in molar percentages based on the sum of ZrO 2 , Y 2 O 3 and CeO 2 present in said particulate mixture.

[0083] In one embodiment, in particular when the magnetic constituent comprises substantially no ZrO 2 , no CeO 2 , no Y 2 O 3 , and when the sintered ball comprises zirconia stabilized with CeO 2 and Y 2 O 3 at the end of step g), the CeO 2 content in the particulate mixture is greater than or equal to 1.5%, preferably greater than or equal to 2%, preferably greater than or equal to 3% and / or preferably less than or equal to 17.5%, preferably less than or equal to 16%, preferably less than or equal to 15%, and the Y 2 O 3 content is such that Y 2 O 3 + (CeO 2 ) / 3.5 is greater than or equal to 1.5%, preferably greater than or equal to 2%, preferably greater than or equal to 2.5%, and preferably less than or equal to 5%, preferably less than or equal to 4%, in molar percentages based on the sum of ZrO 2 , Y 2 O 3 and CeO 2 present in said particulate mixture.

[0084] The particulate mixture also comprises a powder of the magnetic constituent and / or precursor(s) of the magnetic constituent introduced in equivalent quantities. The precursors of the magnetic constituent may be raw materials providing the oxides constituting the magnetic constituent in the sintered ball at the end of step g).

[0085] Preferably, the particulate mixture does not comprise magnetic constituent powder, but magnetic constituent precursor powders each having a median size of less than 5 µm, less than 3 µm, less than 2 µm, less than 1 µm, less than 0.7 µm, preferably less than 0.6 µm, preferably less than 0.5 µm. A person skilled in the art knows how to adapt the quantities of these powders to obtain the desired quantity of magnetic constituent in the sintered ball. Some of the precursor powders may not combine to form magnetic constituent.

[0086] In one embodiment, the particulate mixture comprises an alumina powder in an amount greater than or equal to 0.2%, preferably greater than or equal to 0.25% and preferably less than 3%, preferably less than or equal to 2.5%, preferably less than or equal to 2%, preferably less than or equal to 1.2%, preferably less than or equal to 1%, preferably less than or equal to 0.8%, in percentages by mass based on the mass of the particulate mixture. Advantageously, the sinterability of the particulate mixture is improved. The alumina may be replaced, in part or in whole, by an equivalent amount of alumina precursor. Preferably, the particulate mixture does not comprise an alumina precursor. More preferably, the alumina is substantially exclusively present in the form of corundum.The corundum powder preferably has a median size of less than 5 µm, preferably less than 3 µm, preferably less than 1 µm.

[0087] Preferably, the powders used in the particulate mixture each have a median size of less than 5 µm, preferably less than 3 µm, preferably less than 2 µm, preferably less than 1 µm, preferably less than 0.7 µm, preferably less than 0.6 µm, preferably less than 0.5 µm, preferably less than 0.4 µm, or even less than 0.3 µm.

[0088] Whatever the embodiment, one or more of the powders of the particulate mixture described above can be replaced, at least partially, by equivalent precursor powders, that is to say by powders which, during the manufacture of a ball according to the invention, lead, in said ball, to the same constituents (same composition, same crystallographic phase), in the same quantities.

[0089] In step b), optionally, the particulate mixture may be dried, for example in an oven or by spray drying, in particular if it has been obtained by wet grinding or if at least one raw material powder has been obtained by wet grinding. Preferably, the temperature and / or the duration of the drying step are adapted so that the residual moisture of the particulate mixture is less than 2%, or even less than 1.5%.

[0090] At step c),a starting charge is prepared, preferably at room temperature, comprising the particulate mixture obtained at the end of step a) or at the end of step b) and, optionally, a solvent, preferably water.

[0091] As is well known to those skilled in the art, the starting charge is adapted to the shaping process of step d).

[0092] The shaping may in particular result from a gelling process. For this purpose, a solvent, preferably water, is preferably added to the starting charge so as to produce a suspension.

[0093] The suspension preferably has a dry matter mass content of between 50% and 70%.

[0094] The suspension may also contain one or more of the following constituents: a dispersant, in an amount of 0 to 10%, in mass percentage on a dry matter basis; a surface tension modifier, in an amount of 0 to 3%, in mass percentage on a dry matter basis; a gelling agent, or “gelling agent”, in an amount of 0 to 2%, in mass percentage on a dry matter basis.

[0095] Dispersants, surface tension modifiers and gelling agents are well known to those skilled in the art.

[0096] Examples include, as dispersants, the family of sodium or ammonium polymethacrylates, the family of sodium or ammonium polyacrylates, the family of citrates, for example ammonium, the family of sodium phosphates, and the family of carbonic acid esters; as surface tension modifiers, organic solvents such as aliphatic alcohols; as gelling agents, natural polysaccharides.

[0097] The particulate mixture is preferably added to a mixture of water and dispersants / deflocculants in a micro-mill. After stirring, water is added in which a gelling agent has been previously dissolved to obtain a suspension.

[0098] If the shaping results from extrusion, thermoplastic polymers or thermosetting polymers may be added to the feedstock, said feedstock preferably not containing a solvent.

[0099] At step d), any conventional shaping process known for the manufacture of sintered beads can be implemented.

[0100] Among these processes, we can cite: granulation processes, for example using granulators, fluidized bed granulators, or granulation discs, gelation processes, injection or extrusion molding processes, and pressing processes.

[0101] In a gelling process, drops of the suspension described above are obtained by flowing the suspension through a calibrated orifice. The drops emerging from the orifice fall into a bath of a gelling solution (electrolyte adapted to react with the gelling agent) where they harden after recovering a substantially spherical shape.

[0102] In step e), optionally, the raw balls obtained during the previous step are washed, for example with water.

[0103] At step f), optionally, the raw balls, possibly washed, are dried, for example in an oven.

[0104] In step g), the raw beads, optionally washed and / or dried, are sintered. Preferably, sintering is carried out in air, preferably in an electric furnace, preferably at atmospheric pressure.

[0105] The sintering in step g) is carried out at a temperature preferably above 1200°C, preferably above 1250°C, and preferably below 1600°C, preferably below 1550°C, preferably below 1500°C, preferably below 1450°C, preferably below 1400°C.

[0106] The holding time at the temperature level is preferably greater than 1 hour and / or preferably less than 10 hours, preferably less than 7 hours, preferably less than 5 hours, preferably less than 3 hours. Preferably, the sintering time is between 1 and 3 hours.

[0107] The sintered balls obtained preferably have a size greater than 0.01 mm and less than 10 mm. Process of grinding, dispersing, homogenizing or separating

[0108] The sintered balls according to the invention can be used in a process comprising steps 1) and 2).

[0109] In step 1),beads according to the invention are mixed with a material to be ground, dispersed, homogenized, or separated, which may be in the form of a powder or a suspension or a mass, for example animal tissue, in particular to extract DNA therefrom.

[0110] All known mixing processes can be considered.

[0111] Agitation of the balls, conventionally by rotating the mixture obtained, can lead to grinding, dispersion or homogenization of the solid part of the material to be ground, dispersed or homogenized.

[0112] The material to be ground, dispersed, homogenized, or separated may be an organic material, for example a food material, for example cocoa.

[0113] The material to be dispersed or homogenized can be, for example, paint.

[0114] The material to be separated may be, for example, a powder of non-magnetic particles. The mixture may thus be, for example, a particulate mixture resulting from a surface treatment operation by projection. This mixture may comprise beads and fragments of beads according to the invention projected onto a surface, but also non-magnetic particles projected onto the surface and / or fragments of such magnetic particles, and / or fragments of a coating detached from the surface during projection. The invention thus makes it possible to separate the beads and fragments of beads according to the invention from the mixture.

[0115] At the end of step 1), a charge is obtained in which balls, ball fragments and the ground, dispersed, homogenized or separated material are mixed.

[0116] Conventionally, the beads are then extracted from the load. According to the invention, the bead fragments, and even the beads, can be advantageously extracted magnetically in step 2).

[0117] In step 2), a magnetic field is applied to the charge obtained at the end of step 1), and therefore to the beads and fragments of beads that it contains. This magnetic field exclusively attracts the “magnetic” constituents, which allows their extraction.

[0118] By adjusting the strength of the magnetic field, it is possible to adjust the size of the objects (sintered beads and / or fragments of sintered beads) that are extracted: the higher the strength of the applied magnetic field, the larger the size of these objects.

[0119] This method advantageously makes it possible to substantially completely separate the sintered balls according to the invention and the fragments of said sintered balls according to the invention.

[0120] The magnetic field can be applied by any technique known to those skilled in the art, including magnets, in particular hard ferrite permanent magnets, AlNiCo alloy permanent magnets, electromagnets, or superconducting coils. Method for cleaning a surface treated by projection of beads according to the invention

[0121] At step 1'), beads according to the invention can be projected, by means of a projection apparatus, alone or in mixture with other media, onto a surface of a part to modify its characteristics, for example to modify its appearance or remove a coating. The surface to be treated can be for example a metal surface.

[0122] After projection, a magnetic field is applied to the projected media so as to extract fragments of the beads according to the invention and / or beads according to the invention.

[0123] After projection, a magnetic field can also be applied to at least part of the surface of the treated part so as to extract fragments of the balls according to the invention and / or balls according to the invention, which could for example have remained in a blind hole of the part. Method for cleaning a ball projection device according to the invention

[0124] Cleaning a projection device requires recovering any balls that remain inside the device, particularly in corners or cavities. Mechanical cleaning can be difficult.

[0125] Applying a magnetic field to a surface of the projection device makes it very easy to recover these balls. Examples

[0126] The following non-limiting examples are given for the purpose of illustrating the invention. Measurement protocols

[0127] The following methods were used to determine some properties of different sintered ball mixtures. They provide an excellent simulation of actual in-service behavior in microgrinding applications.

[0128] To determine the sphericity of a ball, the smallest and largest Ferret diameters are measured with a Camsizer XT marketed by the Horiba company.

[0129] To determine the so-called “planetary” wear resistance», 20 ml (volume measured using a graduated cylinder) of test beads, between 0.9 and 1.2 mm in size, are weighed (mass m 0 ) and introduced into one of the 4 bowls coated with dense sintered alumina, with a capacity of 125 ml, of a fast planetary mill of the PM400 type of RETSCH brand. 2.2 g of silicon carbide of the Presi brand (having a median size D 50 of 23 µm) and 40 ml of water are added to the same bowl already containing the beads. The bowl is closed and set in rotation (planetary movement) at 400 rpm with reversal of the direction of rotation every minute for 1 hour 30 minutes. The contents of the bowl are then washed on a 100 µm sieve to remove residual silicon carbide and material tears due to wear during grinding. After sieving on a 100 µm sieve, the balls are dried in an oven at 100 °C for 3 hours and then weighed (mass m 1 ).Said balls (mass m 1 ) are again introduced into one of the bowls with a SiC suspension (same concentration and quantity as previously) and undergo a new grinding cycle, identical to the previous one. The contents of the bowl are then washed on a 100 µm sieve so as to remove the residual silicon carbide as well as the material tears due to wear during grinding. After sieving on a 100 µm sieve, the balls are dried in an oven at 100 °C for 3 hours and then weighed (mass m 2 ). Said balls (mass m 2 ) are again introduced into one of the bowls with a SiC suspension (same concentration and quantity as previously) and undergo a new grinding cycle, identical to the previous one. The contents of the bowl are then washed on a 100 µm sieve to remove residual silicon carbide as well as material tears due to wear during grinding.After sieving through a 100 µm sieve, the beads are dried in an oven at 100°C for 3 hours and then weighed (mass m 3 ).

[0130] Planetary wear (UP) is expressed as a percentage (%) and is equal to the loss of mass of the balls reduced to the initial mass of the balls, i.e.: 100.(m 0 -m 3 ) / (m 0 ); the UP result is given in table 1.

[0131] The results are considered particularly satisfactory if the products have a planetary wear resistance (UP) which degrades by less than 5% compared to that of Example 1, the reference example. Such degradation is acceptable because the balls can advantageously be easily recovered magnetically.

[0132] The preferred products exhibit improved planetary wear (UP) resistance of at least 5% compared to that of Example 1.

[0133] Quantification of crystallized phasespresent in the sintered beads according to the invention is carried out from samples of polished beads prepared according to the following method: for each of the examples, a substantially continuous monolayer of beads having a size between 0.9 and 1.2 mm, is partially embedded in acrylic resin, at a temperature equal to 180°C. After hardening and returning to room temperature, a block of resin is obtained.

[0134] The outer diameter of the resin block containing the balls is 25.4 mm.

[0135] The block is polished using abrasive paper with a grain size of 65 µm, until the center of the balls can be clearly seen. The block is then polished more finely, the penultimate polishing step being carried out with a 1µm DiaPro Nap B diamond preparation marketed by Struers, and the last polishing step being carried out using a 0.04 µm colloidal silica solution.

[0136] The acquisition of the diffraction pattern is carried out with a D8 Endeavor device from Bruker, over an angular range 2θ between 5° and 100°, with a step of 0.01°, and a counting time of 0.34 s / step. The front optics have a primary slit of 0.3° and a Soller slit of 2.5°. The polished resin block containing the balls is rotating on itself at a speed equal to 5 rpm, with use of the automatic knife.

[0137] The rear optics feature a 2.5° Soller slit, a 0.0125 mm nickel filter, and a 1D detector with an aperture equal to 4°.

[0138] The diffraction patterns are then qualitatively analyzed using EVA software and the ICDD2016 database.

[0139] Once the present phases have been highlighted, the diffraction diagrams are quantitatively analyzed with the High Score Plus software by Rietveld refinement according to the following strategy: A refinement of the background signal is carried out using the function "treatment", "determine background" with the following choices: "bending factor" equal to 0 and "granularity" equal to 40. Note that if a halo induced by the resin is observed, it is possible to manually draw the baseline point by point; Conventionally, the ICDD sheets of the highlighted and quantifiable phases present are selected, and therefore taken into account in the refinement; An automatic refinement is then carried out by selecting the background signal previously determined "use available background" and by selecting the mode "automatic: option phase fit-default Rietveld"; A manual refinement of the parameter "B overall" of all the selected phases is then carried out simultaneously.

[0140] There amount of amorphous phasepresent in the sintered balls of the examples is measured by X-ray diffraction, using a D8 Endeavor type device from Bruker. The acquisition of the diffraction pattern is carried out using this equipment, in the same way as for the determination of the crystallized phases present in the balls, the analyzed sample being in the form of a powder. The method applied consists of adding a known quantity of a fully crystallized standard, in this case a zinc oxide powder, ZnO in an amount equal to 20%, based on the mass of zinc oxide and sample of sintered balls ground according to the invention. The maximum size of the zinc oxide powder is equal to 1 µm and the balls according to the invention are ground so as to obtain a powder having a maximum size of less than 40 µm.

[0141] After performing the Rietveld refinement, the maximum size of the ZnO particles was entered into the High Score Plus software to limit micro-absorption effects. The mass quantity of the ZnO particles was also entered into the High Score Plus software.

[0142] The mass quantity of each phase present, in percentage, is taken equal to the “as received weight %” value given by the High Score Plus software.

[0143] The mass quantity of amorphous phase, in percentage based on the mass of the sample, is equal to the complement to 100 of the sum of the mass quantities of the phases present.

[0144] Typically, if zinc oxide is present among the crystallized phases of the sample to be characterized (which is not the case in the examples below), another oxide not detected as a crystallized phase in the sample to be characterized will be used as a standard.

[0145] There pore surface density of sintered balls is measured by the following method. Images of polished surfaces of sections of the sintered balls are made using a Scanning Electron Microscope, so that each image is a rectangular image with a length between 40 and 60 µm and a width between 35 µm and 50 µm. For each example, 10 images are thus made.

[0146] For each example, using the image processing software ImageJ, the observed surface area SO i , and the surface area covered by pores SP i are calculated for each of the images i. The total observed surface area SOT is equal to the sum of the total observed surface area, SO i , on each of the images i. The total surface area covered by pores SPT is equal to the sum of the surface area covered by pores SP i , on each of the images i. The surface density of pores, expressed as a percentage, is equal to SPT / SOT.

[0147] L chemical analysissintered beads is determined by X-ray fluorescence on a bead made by melting said beads.

[0148] There apparent density of the sintered beads of the examples, in g / cm 3< , is measured using a helium pycnometer (AccuPyc 1330 from the company Micromeritics ®< ), according to a method based on the measurement of the volume of gas displaced (in this case helium).

[0149] There quantity of marbles attracted by a magnetis evaluated by the following method. 100 g of balls of each example, having a size between 0.9 and 1.2 mm, are placed in a container. A ceramic magnet with a nickel-plated steel casing of external diameter 22 mm, internal diameter 16 mm, height 6 mm, having an attraction of 3 kg, marketed by the company Wilmart, is then immersed for 10 seconds in the balls. The magnet is then removed and the balls remaining stuck to the magnet are recovered and then weighed. This mass M allows a rapid comparison between the balls of the different examples. A high value of said mass M is sought.

[0150] Mass magnetizationof the sintered balls of the examples is determined at room temperature using a vibrating sample magnetometer marketed by the company Lake Shore Cryotronics, said balls being subjected to an excitation magnetic field equal to 2500 kA / m, said magnetic field being reduced to a value equal to 100 kA / m, this latter value being that at which the mass magnetization measurement is carried out. Manufacturing protocol

[0151] Sintered beads were prepared from: of a yttria-containing zirconia powder containing a molar content of Y 2 O 3 equal to 1%, having a specific surface area of ​​the order of 7 m 2 < / g and a median size equal to 1.1 µm for examples 3, 8 and 9; of a yttria-containing zirconia powder containing a molar content of Y 2 O 3 equal to 3%, having a specific surface area of ​​the order of 13 m 2 < / g and a median size equal to 0.2 µm for examples 7, 8 and 9; of a ceria powder of purity greater than 99% and having a median size equal to 4.6 µm for examples 2 to 6, and 8 to 9; of an alumina powder with a purity greater than 99.5% and a median size equal to 0.4 µm for examples 4 to 6, and 8 to 9; of an unstabilized zirconia powder CZ-5, marketed by Saint-Gobain ZirPro, in monoclinic crystallographic form, having a specific surface area of ​​the order of 6 m 2 < / g and a median size equal to 4.5 µm for examples 2, and 4 to 6;of a zinc oxide powder having a mass purity of ZnO greater than 99% and a median size equal to 0.3 µm for examples 2 to 5, and 7 to 9; of a copper oxide powder having a mass purity of CuO greater than 96% and a median size equal to 1.3 µm for examples 2 to 5, and 7 to 9; of an iron oxide powder Fe 2 O 3 having a mass purity of Fe 2 O 3 greater than 97% and a median size equal to 0.34 µm for examples 2 to 9; of a lanthanum oxide powder La 2 O 3 having a mass purity of La 2 O 3 greater than 99.5% and a median size equal to 7 µm for example 6. ;

[0152] The sintered bead powder of example 1, outside the invention, is a Zirmil-Ce bead powder marketed by the company Saint-Gobain Zirpro, having a size between 0.9 and 1.2 mm.

[0153] Table 1 summarizes the characteristics of the particulate mixtures of the examples.

[0154] These powders were mixed and then co-ground in a wet environment until a particulate mixture with a median size of less than 0.4 µm was obtained. The particulate mixture was then dried.

[0155] A starting charge consisting of an aqueous suspension comprising, in percentages by mass based on dry matter, 2% of a carboxylic acid type dispersant and 2% of a gelling agent, namely a polysaccharide of the alginate family, was then prepared from this particulate mixture.

[0156] A micro-mill was used for this preparation in order to obtain good homogeneity of the starting charge: A solution containing the gelling agent was first formed. The particulate mixture and the dispersants were successively added to water. The solution containing the gelling agent was then added. The mixture thus obtained was stirred for 8 hours. The particle size was controlled using a Partica LA-950 laser diffraction granulometer marketed by Horiba Scientific (median size < 0.4µm), and water was added in a determined quantity to obtain an aqueous suspension at 68% dry matter and a viscosity, measured with a Brookfield viscometer using the LV3 spindle at a speed of 20 rpm, of less than 5000 centipoise. The pH of the suspension was then approximately 9 after adjustment using a strong base.

[0157] The suspension was forced through a calibrated hole and at a flow rate allowing to obtain after sintering beads having a size of approximately 1 mm. The drops of suspension fell into a gelling bath based on an electrolyte (divalent cation salt), reacting with the gelling agent. The green beads were collected, washed, then dried at 80°C to remove moisture. The beads were then transferred to a sintering furnace where they were brought, at a rate of 100°C / h, to the temperature equal to 1250°C for examples 2 and 4 to 9 and to 1275°C for example 3. At the end of a 4-hour hold at this temperature, the temperature decrease was carried out by natural cooling. Results

[0158] The results obtained are summarized in Tables 2 to 4 below. [Table 1] Examples 1(*) 2 3 4 5(*) 6 7(*) 8(*) 9 Composition of the particulate mixture (mass percentages) Yttria zirconia powder containing a molar content of Y 2 O 3 equal to 1% - - 81,87 - - - - 11,62 36,24 Cerine powder - 14,78 9,10 13,08 11,86 14,80 - 1,27 6,64 Unstabilized zirconia powder CZ-5 - 75,16 - 66,56 60,79 75,20 - - Yttria zirconia powder containing a molar content of Y 2 O 3 equal to 3% - - - - - - 90,00 76,86 46,80 Alumina powder - - - 0,33 0,30 0,71 - 0,30 0,30 Zinc oxide powder - 1,71 1,53 3,40 4,59 - 1,69 1,69 1,70 Copper oxide powder - 1,67 1,50 3,32 4,48 - 1,66 1,65 1,66 Iron oxide powder - 6,68 6,00 13,31 17,98 7,78 6,65 6,61 6,66 Lanthanum oxide powder - - - - - 1,51 - - - (*): excluding invention [Table 2] Examples 1 (*) 2 3 4 5(*) 6 7(*) 8(*) 9 Chemical analysis, in mass percentages based on oxides unless otherwise stated ZrO 2 (%) 82 74,7 79,7 68,1 59,4 75,4 83,8 83,8 79,1 CeO 2 (%) 16 14,8 9,6 12,7 11 14,2 - 1,3 6,5 Y 2 O 3 (%) - - 1,7 - - - 5,0 4,6 3,2 ZnO (%) - 1,2 1,2 2,3 5,1 - 1,8 1,2 1,7 CuO (%) - 1,4 1,1 3 4,4 - 1,6 1,5 1,4 Fe 2 O 3 (%) - 6,3 6,1 13 19,2 7,3 6,5 6,3 6,8 The 2 O 3 (%) - - - - - 1,2 - - Al 2 O 3 (%) 0,5 0,4 - 0,3 0,4 1,2 0,5 0,6 0,6 CaO (%) 0,3 0,7 0,3 0,3 0,3 0,3 0,4 0,1 0,3 Oxides other than ZrO 2 , CeO 2 , Y 2 O 3 , ZnO, CuO, Fe 2 O 3 , La 2 O 3 , Al 2 O 3 , and CaO (%) 1,2 0,5 0,3 0,3 0,2 0,4 0,4 0,6 0,4 CeO 2 in mol% based on the sum of ZrO 2 , HfO 2 , CeO 2 and Y 2 O 3 12,2 12,4 7,8 11,8 11,7 11,9 0 1,1 5,4 Y 2 O 3 in mol% based on the sum of ZrO 2 , HfO 2 , CeO 2 and Y 2 O 3 0 0 1,1 0 0 0 3,1 2,9 2 Y 2 O 3 + CeO 2 / 3.5, in mol% 3,5 3,5 3,3 3,4 3,3 3,4 3,1 3,2 3,5 (*): excluding invention [Table 3] Examples 1(*) 2 3 4 5(*) 6 7(*) 8(*) 9 Crystallized phases, in mass percentage based on the mass of the crystallized phases Zirconia stabilized with CeO 2 and optionally Y 2 O 3 95 87 89 79 68 92 46 48 86 Monoclinic zirconia 5 5 5 5 7 Complement to 100 46 42 6 Magnetic spinel - 8 6 16 25 - 8 10 8 Nature of said spinel - Spinel containing iron, zinc, and copper Spinel containing iron, zinc, and copper Spinel containing iron, zinc, and copper Spinel containing iron, zinc, and copper - Spinel containing iron, zinc, and copper Spinel containing iron, zinc, and copper Spinel containing iron, zinc, and copper Magnetic M-type hexagonal ferrite - - - - - 6 - - - Nature of said hexagonal ferrite - - - - - Type M hexagonal ferrite containing iron and lanthanum and aluminum - - - (*): excluding invention [Table 4] Examples 1(*) 2 3 4 5(*) 6 7(*) 8(*) 9 Features Apparent density of the beads (g / cm 3< ) 6,20 6,10 6,05 6,00 5,93 6,00 5,79 5,81 6,01 Planetary wear UP (in %) 2,3 2 1,9 2,1 3 1,8 3,3 2,5 1,6 Improvement UP% / example 1 - 13% 17,4% 8,7% -30% 21,7% -43,5% -8,7% 30,4% Mass M of balls attracted by a magnet (in g) 0 10 9,1 13,6 15,5 1,3 8,2 9,3 9,2 Mass magnetization (Am 2< .kg -1< ) nd 4,5 nd nd 13 1,7 nd nd nd (*): excluding invention nd: not determined

[0159] The bead powders of the examples have an average sphericity greater than 0.9.

[0160] The beads of Examples 2 to 9 have a substantially zero quantity of amorphous phase and a surface density of pigs of less than 1%.

[0161] Before performing the quantification of the crystallized phases by X-ray diffraction, spotting carried out using an electron microprobe revealed the presence of a phase comprising iron and copper and zinc in the beads of examples 2 to 5 and 7 to 9, and a phase comprising iron and lanthanum and aluminum in the beads of example 6.

[0162] A comparison of the reference example 1 outside the invention, and of example 2 according to the invention, shows that the balls according to example 2, comprising zirconia stabilized with CeO 2 , a molar content of CeO 2 equal to 12.4%, and having a spinel content comprising iron and zinc and copper equal to 8% based on the mass of the crystallized phases, are attracted by a magnet, unlike the balls of reference example 1, the ball powder of example 2 having a UP% wear equal to 2%, i.e. 13% lower than the UP% wear of the ball powder of reference example 1 outside the invention.

[0163] A comparison of the reference example 1 outside the invention, and of example 3 according to the invention, shows that the balls according to example 3, comprising zirconia stabilized with CeO 2 and Y 2 O 3 , the molar contents of CeO 2 and Y 2 O 3 being equal to 7.8% and 1.1%, respectively, and having a spinel content comprising iron and zinc and copper equal to 6% based on the mass of the crystallized phases, are attracted by a magnet, unlike the balls of reference example 1, the ball powder of example 3 having a UP% wear equal to 1.9%, i.e. 17.4% lower than the UP% wear of the ball powder of reference example 1 outside the invention.

[0164] A comparison of the reference example 1 outside the invention, and of example 4 according to the invention, shows that the balls according to example 4, comprising zirconia stabilized with CeO 2 , a molar content of CeO 2 equal to 11.8% and having a spinel content comprising iron, zinc and copper equal to 16% based on the mass of the crystallized phases, are attracted by a magnet, unlike the balls of reference example 1, the ball powder of example 4 having a UP% wear equal to 2.1%, i.e. 8.7% lower than the UP% wear of the ball powder of reference example 1 outside the invention.

[0165] A comparison of the reference example 1 outside the invention, and of the example 5 outside the invention, shows that the balls according to said example 5, comprising stabilized zirconia CeO 2 , a molar content of CeO 2 equal to 11.7%, and having a spinel content comprising iron, zinc and copper equal to 25% based on the mass of the crystallized phases, are attracted by a magnet, unlike the balls of the reference example 1, the ball powder of example 5 also having a UP% wear equal to 3%, i.e. 30% higher than the UP% wear of the ball powder of the reference example 1 outside the invention.

[0166] A comparison of the reference example 1 outside the invention, and of example 6 according to the invention, shows that the balls according to example 6, comprising zirconia stabilized with CeO 2 , a molar content of CeO 2 equal to 11.9%, and having a content of hexagonal ferrite of type M comprising iron, lanthanum and aluminum equal to 6% based on the mass of the crystallized phases, are attracted by a magnet, unlike the balls of the reference example 1, the ball powder of example 6 having a UP% wear equal to 1.8%, i.e. 21.7% lower than the UP% wear of the ball powder of the reference example 1 outside the invention.

[0167] A comparison of Reference Example 1 outside the invention, Example 2 according to the invention and Example 7 outside the invention, shows that the balls according to Example 7, comprising zirconia stabilized with Y 2 O 3 , a molar content of Y 2 O 3 equal to 3.1%, and having a spinel content comprising iron, zinc and copper equal to 8% based on the mass of the crystallized phases, surprisingly exhibits a UP% wear equal to 3.3%, i.e. 43.5% higher than the UP% wear of the balls of Example 1 and 65% higher than the UP% wear of the balls of Example 2. Although the balls of Example 7 are attracted by a magnet, they exhibit a UP% wear much higher than that of Reference Example 1, which demonstrates that the presence of CeO 2 as a zirconia stabilizer is necessary.

[0168] A comparison of the reference example 1 outside the invention, of example 3 according to the invention and of example 8 outside the invention, shows that the balls according to example 8, comprising zirconia stabilized with CeO 2 and Y 2 O 3 , the molar contents of CeO 2 and Y 2 O 3 being equal to 1.1% and 2.9%, respectively, and having a content of spinel comprising iron, zinc and copper equal to 10% based on the mass of the crystallized phases, exhibits a UP% wear equal to 2.5%, i.e. 8.7% higher than the UP% wear of the balls of example 1 and 31.6% higher than the UP% wear of the balls of example 3. Although the balls of example 8 are attracted by a magnet, they exhibit a UP% wear higher than that of examples 1 and 3, which demonstrates that the presence of CeO 2 in an amount greater than 1.5 mol% is required.

[0169] A comparison of the reference example 1 outside the invention, and of example 9 according to the invention, shows that the balls according to example 9, comprising zirconia stabilized with CeO 2 and Y 2 O 3 , the molar contents of CeO 2 and Y 2 O 3 being equal to 5.4% and 2%, respectively, and having a spinel content comprising iron and zinc and copper equal to 8% based on the mass of the crystallized phases, are attracted by a magnet, unlike the balls of reference example 1, the ball powder of example 9 having a UP% wear equal to 1.6%, i.e. 30.4% lower than the UP% wear of the ball powder of reference example 1 outside the invention.

[0170] The sintered balls according to the invention, as well as fragments of said balls, can thus easily be separated from a liquid or solid constituent ground using said balls, by simple application of a magnetic field.

[0171] As is now clearly apparent, the invention therefore makes it possible to provide a zirconia ball powder having good wear resistance and making it possible to limit contamination of the ground material.

[0172] Of course, the invention is not limited to the examples and embodiments described above.

Claims

1. A sintered bead having the following crystalline phases, as percentages by weight on the basis of the crystalline phases and for a total of 100%: stabilized zirconia: complement to 100%; monoclinic zirconia: ≤ 20%; 4% ≤ magnetic constituent ≤ 22%; crystalline phases other than stabilized zirconia, monoclinic zirconia and magnetic constituent: < 10%; the magnetic constituent being selected from magnetic spinels, magnetic garnets, magnetic hexagonal ferrites and their mixtures; excluding the magnetic constituent, the sintered bead comprising CeO2 and optionally Y2O3 in contents such that 3% ≤ CeO2 ≤ 17.5% and 1.5% ≤ Y2O3 + (CeO2) / 3.5 ≤ 5%, as molar percentages on the basis of the sum of ZrO2, CeO2 and Y2O3.

2. The sintered bead as claimed in the preceding claim in which, excluding the magnetic constituent, CeO2 ≤ 16%, as molar percentages on the basis of the sum of ZrO2, CeO2 and Y2O3.

3. The sintered bead as claimed in the preceding claim, in which 5% ≤ CeO2 and CeO2 ≤ 15%, as molar percentages on the basis of the sum of ZrO2, CeO2 and Y2O3.

4. The sintered bead as claimed in any one of the preceding claims in which, excluding the magnetic constituent, Y2O3 + (CeO2) / 3.5 is more than or equal to 2% and less than or equal to 4%.

5. The sintered bead as claimed in any one of the preceding claims, in which the zirconia is entirely stabilized with CeO2, or in which the stabilized zirconia is entirely stabilized with CeO2 and Y2O3.

6. The sintered bead as claimed in any one of the preceding claims, in which more than 90% of the stabilized zirconia is present in the form of quadratic zirconia, as a percentage by weight on the basis of the stabilized zirconia, and / or having a monoclinic zirconia content, as a percentage by weight on the basis of the total quantity of the crystalline phases, of less than or equal to 10%.

7. The sintered bead as claimed in any one of the preceding claims, having a magnetic constituent content of more than or equal to 5% and less than or equal to 18%, as percentages by weight on the basis of the crystalline phases.

8. The sintered bead as claimed in the immediately preceding claim, having a magnetic constituent content of more than or equal to 7% and less than or equal to 15%, as percentages by weight on the basis of the crystalline phases.

9. The sintered bead as claimed in any one of the preceding claims, in which - excluding oxygen and for more than 90% of its mass, said magnetic spinel is constituted by iron and zinc and copper, by iron and copper and aluminum, by iron and nickel, by iron and cobalt, by iron and copper, by iron and zinc, by iron and magnesium, by iron and manganese, by iron and nickel and zinc, by iron and nickel and zinc and copper, by iron and manganese and zinc, by iron and manganese and zinc and aluminum, by iron and lithium and zinc and by nickel and manganese, by iron and zinc and lithium, by iron and zinc and copper and aluminum and calcium, and their mixtures; and / or - the magnetic hexagonal ferrite is selected from a M-type hexagonal ferrite, a W-type hexagonal ferrite and their mixtures, and / or - the magnetic constituent is selected from magnetic spinels, magnetic hexagonal ferrites and their mixtures, or.said magnetic garnet is selected from garnets comprising iron.

10. The sintered bead as claimed in any one of the preceding claims, in which 0.2% ≤ Al2O3 <_ 2%, Al2O3 being expressed as excluding the magnetic constituent; and / or CaO ≤ 1.5%, CaO being expressed as excluding the magnetic constituent.

11. Powdered sintered beads comprising more than 90%, as percentages by weight, of sintered beads in accordance with any one of the preceding claims.

12. A method for extracting beads and / or fragments of beads in accordance with any one of claims 1 to 10, said method comprising the following step: 2) applying a magnetic field to said beads and / or said fragments of beads, in a manner such as to attract said beads or said fragments of beads.

13. A method for grinding, dispersing, homogenizing a material, said method comprising the following steps: 1) mixing a material to be ground, to be dispersed, to be homogenized, with beads and / or fragments of beads in accordance with any one of claims 1 to 10, in order to obtain a charge; 2) purifying the charge by extraction in accordance with the method of claim 14, the magnetic field being applied to said charge.

14. The method for extracting beads or fragments of beads in accordance with any one of claims 1 to 10 from a surface of a substrate on which said beads or said fragments of beads are lying, said method comprising the following steps: 1') projecting beads and / or fragments of beads in accordance with any one of claims 1 to 10 onto a surface to be treated by means of a projection apparatus; 2) recovering said beads or said fragments of beads by extraction in accordance with the method of claim 12, the magnetic field being applied to said substrate surface, the substrate surface possibly in particular being the surface to be treated and / or a surface of said projection apparatus.

15. A method comprising the use of powdered sintered beads in accordance with claim 11, as a grinding medium, dispersion medium, homogenizing medium or medium for the treatment of surfaces.