UNHARDENED COMPOSITE STRUCTURES, HARDENED COMPOSITE STRUCTURES AND METHOD FOR HARDENING UNHARDENED COMPOSITE STRUCTURES
Patent Information
- Application Number
- DE602022008114
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-10
- Filing Date
- 2022-07-27
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2042-07-27
AI Technical Summary
It is challenging to maintain a desired distinction between the surface and underlying composite layers during the curing of hybrid composite structures, which affects the structural integrity and environmental protection of the composite structure.
A method involving an uncured composite structure with a structural layer and a surface layer, where the surface resin has a higher viscosity and lower gel point temperature than the structural resin, allowing for initial partial curing of the surface resin while keeping the structural resin uncured, followed by further heating to fully cure both layers at a higher temperature.
This approach results in improved surface quality and reduced defects, with the surface resin protecting the structural layer from environmental factors by maintaining a clear separation and enhancing adhesion between layers.
Description
BACKGROUND
[0001] The present disclosure relates generally uncured composite structures, to cured composite structures, and / or to methods of curing uncured composite structures.
[0002] Composite structures generally include a fiber and a resin material. Chemical and / or physical properties of the fiber and / or of the resin material may have a significant impact on the chemical and / or physical properties of the composite structure that is formed therefrom. As examples, the structural integrity, longevity, chemical resistivity, and / or light stability of the composite structure may be dictated by the chemical and / or physical properties of the fiber and / or of the resin material. With this in mind, a specific fiber and / or resin may be utilized to form a specific composite structure with one or more desired physical and / or chemical properties. In some examples, a composite structure that exhibits one or more desired physical and / or chemical properties also may exhibit one or more undesired physical and / or chemical properties. As a specific example, a composite structure that exhibits a desired structural integrity also may exhibit an undesired chemical resistivity and / or light stability.
[0003] It is known to coat and / or cover a composite structure, such as to protect the composite structure from environmental factors. In some examples, such coating may be accomplished by painting the composite structure. In other examples, it may be desirable to form a hybrid composite structure that includes a surface composite layer and an underlying composite layer. The surface composite layer may be selected to protect the underlying composite layer from the environmental factors, while the underlying composite structure may be selected to provide a desired structural integrity. However, it is difficult to maintain a desired level of distinction between the surface composite layer and the underlying composite layer during curing of the hybrid composite structure. Thus, there exists a need for improved uncured composite structures, cured composite structures, and / or methods of curing uncured composite structures.
[0004] JP 2018 / 202804, in accordance with its abstract, states that there is an aim to provide a molding material that can yield a fiber-reinforced resin molding with excellent surface smoothness and appearance after curing, and a molding method therefor. The proposed solution is to provide, on an outermost layer of a molding material of a fiber-reinforced resin molding, a layer of a second thermosetting resin material with a lower glass transition temperature than that of a first thermosetting resin material contained in an inside CFRP layer as a matrix.SUMMARY
[0005] There is described herein, a method of curing an uncured composite structure that includes a structural layer, which includes an uncured structural resin with a structural resin viscosity, a structural resin gel point temperature, and a structural resin gel time, and a surface layer, which includes an uncured surface resin with a surface resin viscosity that is greater than the structural resin viscosity, a surface resin gel point temperature that is less than the structural resin gel point temperature, and a surface resin gel time that is less than the structural resin gel time, the method comprising: initially heating, for an initial heating time, the uncured composite structure to an initial temperature to generate a partially cured composite structure, wherein the initially heating is sufficient to gel the uncured surface resin but insufficient to gel the uncured structural resin; and subsequently heating, for a subsequent heating time, the partially cured composite structure to a final cure temperature, which is greater than the initial temperature, to generate a cured composite structure, wherein a combination of the initially heating and the subsequently heating is sufficient to fully cure both the uncured surface resin and the uncured structural resin.
[0006] There is also described herein an uncured composite structure, comprising: a structural layer that includes an uncured structural resin, wherein the uncured structural resin has a structural resin viscosity, a structural resin gel point temperature, and a structural resin gel time; and a surface layer that includes an uncured surface resin, wherein the uncured surface resin has a surface resin viscosity that is greater than the structural resin viscosity, a surface resin gel point temperature that is less than the structural resin gel point temperature, and a surface resin gel time that is less than the structural resin gel time.BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Fig. 1 is a flowchart illustrating examples of methods of curing an uncured composite structure. Fig. 2 is a schematic cross-sectional view illustrating examples of an uncured composite structure. Fig. 3 is a schematic cross-sectional view illustrating examples of a cured composite structure. Fig. 4 is a plot illustrating viscosity as a function of cure temperature at a constant ramp rate for two resins that may be utilized with the uncured composite structures, composite structures, and methods. DESCRIPTION
[0008] Figs. 1-4 provide illustrative, non-exclusive examples of uncured composite structures 12, cured composite structures 14, and / or methods 100, according to the present disclosure. Elements that serve a similar, or at least substantially similar, purpose are labeled with like numbers in each of Figs. 1-4, and these elements may not be discussed in detail herein with reference to each of Figs. 1-4. Similarly, all elements may not be labeled in each of Figs. 1-4, but reference numerals associated therewith may be utilized herein for consistency. Elements, components, and / or features that are discussed herein with reference to one or more of Figs. 1-4 may be included in and / or utilized with any of Figs. 1-4 without departing from the scope of the present disclosure.
[0009] In general, elements that are likely to be included in a given (i.e., a particular) example are illustrated in solid lines, while elements that are optional to a given example are illustrated in dashed lines. However, elements that are shown in solid lines are not essential to all examples, and an element shown in solid lines may be omitted from a particular example without departing from the scope of the present disclosure.
[0010] Fig. 1 is a flowchart illustrating examples of methods 100 of curing an uncured composite structure, according to the present disclosure. The uncured composite structure includes a structural layer, which includes an uncured structural resin, and a surface layer, which includes an uncured surface resin. An example of the uncured composite structure is illustrated in Fig. 2. More specifically, Fig. 2 illustrates a composite structure 10 in the form of an uncured composite structure 12. Uncured composite structure 12 includes a structural layer 20, in the form of an uncured structural layer 22, that includes a structural resin 26, in the form of an uncured structural resin 28. Uncured composite structure 12 also includes a surface layer 50, in the form of an uncured surface layer 52, that includes a surface resin 56, in the form of an uncured surface resin 58.
[0011] Methods 100 may include providing an uncured composite structure at 110 and / or applying a pressure at 120. Methods 100 include initially heating at 130 and subsequently heating at 140.
[0012] Providing the uncured composite structure at 110 may include providing any suitable uncured composite structure, which includes the structural layer and the surface layer, in any suitable manner. As an example, the providing at 110 may include laying up, forming, and / or defining the uncured composite structure. In some examples, and as discussed in more detail herein, the providing at 110 includes providing such that the structural resin has a structural resin viscosity, a structural resin gel point temperature, and a structural resin gel time. In some examples, and as also discussed in more detail herein, the providing at 110 includes providing such that the surface resin has a surface resin viscosity, a surface resin gel point temperature, and a surface resin gel time. In some examples, the structural resin viscosity is less than the surface resin viscosity, the surface resin viscosity is greater than the structural resin viscosity, the structural resin gel point temperature is greater than the surface resin gel point temperature, the surface resin gel point temperature is less than the structural resin gel point temperature, the structural resin gel time is greater than the surface resin gel time, and / or the surface resin gel time is less than the structural resin gel time.
[0013] Applying the pressure at 120 may include applying the pressure to the uncured composite structure during the initially heating at 130 and / or applying the pressure to the partially cured composite structure during the subsequently heating at 140. In some examples, the applying the pressure at 120 includes applying an elevated atmospheric pressure to the uncured composite structure and / or to the partially cured composite structure. In some examples, the applying at 120 includes utilizing an autoclave, autoclaving the uncured composite structure during the initially heating at 130, and / or autoclaving the partially cured composite structure during the subsequently heating at 140.
[0014] In some examples of methods 100, the initially heating at 130 includes hardening the surface layer to generate a hardened surface layer. In some such examples, methods 100 further include resisting deformation of the hardened surface layer, which may be caused by the applying at 120, during the subsequently heating at 140. Stated another way, the initially heating at 130 may harden the surface layer such that, during the subsequently heating at 140, the hardened surface layer is more resistant to deformation when compared to the structural layer and / or to the uncured surface layer. Such a configuration may permit the hardened surface layer to function as and / or to be a resin shell for the structural layer during the subsequently heating at 140. Such a configuration may cause composite structures, which are formed utilizing methods 100, to have an improved surface quality and / or to have fewer defects when compared to conventional composite structures that do not include the surface layer and the structural layer disclosed herein.
[0015] Initially heating at 130 may include initially heating the uncured composite structure to an initial temperature, such as to produce and / or generate the partially cured composite structure. As discussed, the uncured surface resin has the surface resin viscosity, the surface resin gel point temperature, and the surface resin gel time. The initially heating at 130 is sufficient to gel the uncured surface resin, such as to generate a cured surface resin, but is insufficient to gel the uncured structural resin. Stated another way, and subsequent to the initially heating at 130, the surface resin may be cured, gelled, and / or hardened; however, the structural resin may be uncured, ungelled, and / or unhardened.
[0016] In some examples, the initially heating at 130 includes initially heating for an initial heating time. In some such examples, the initial heating time includes and / or is a dwell time during which the uncured composite structure is maintained at the initial temperature. Stated another way, the initially heating at 130 may include dwelling at the initial temperature for the initial heating time. In some such examples, the initial heating time also may be referred to herein as an initial dwell time at the initial temperature.
[0017] In some examples, the initial heating time includes and / or is a ramp time during which the uncured composite structure is ramped to the initial temperature. Stated another way, the initially heating at 130 may include ramping the uncured composite structure to the initial temperature during the initial heating time. In some such examples, the initial heating time also may be referred to herein as an initial ramp time to the initial temperature.
[0018] The initial temperature may have any suitable magnitude and / or value, such as may be selected based, at least in part, on one or more desired properties of the surface layer, the surface resin viscosity, the surface resin gel point temperature, and / or the surface resin gel time. Examples of the initial temperature include initial temperatures of at least 60 degrees Celsius (ºC), at least 65 ºC, at least 70 ºC, at least 75 ºC, at least 80 ºC, at least 85 ºC, at least 90 ºC, at least 95 ºC, at least 100 ºC, at least 105 ºC, at least 110 ºC, at most 150 ºC, at most 145 ºC, at most 140 ºC, at most 135 ºC, at most 130 ºC, at most 125 ºC, at most 120 ºC, at most 115 ºC, at most 110 ºC, at most 105 ºC, at most 100 ºC, at most 95 ºC, at most 90 ºC, at most 85 ºC, and / or at most 80 ºC. Stated differently, the initial temperature may be bounded by any of the above temperatures, as appropriate.
[0019] Similarly, the initial heating time may have any suitable magnitude and / or value, such as may be selected based, at least in part, on one or more desired properties of the surface layer, the surface resin viscosity, the surface resin gel point temperature, and / or the surface resin gel time. Examples of the initial heating time include initial heating times of at least 2 minutes, at least 4 minutes, at least 6 minutes, at least 8 minutes, at least 10 minutes, at least 12 minutes, at least 14 minutes, at least 16 minutes, at least 18 minutes, at least 20 minutes, at most 120 minutes, at most 110 minutes, at most 100 minutes, at most 90 minutes, at most 80 minutes, at most 70 minutes, at most 60 minutes, at most 50 minutes, at most 40 minutes, at most 38 minutes, at most 36 minutes, at most 34 minutes, at most 32 minutes, at most 30 minutes, at most 28 minutes, at most 26 minutes, at most 24 minutes, at most 22 minutes, at most 20 minutes, at most 18 minutes, at most 16 minutes, at most 14 minutes, at most 12 minutes, and / or at most 10 minutes. Stated differently, the initial heating time may be bounded by any of the above times, as appropriate.
[0020] Subsequently heating at 140 may include subsequently heating the partially cured composite structure to a final cure temperature, which is greater than the initial temperature, to produce and / or generate a cured composite structure. The subsequently heating at 140 may be performed subsequent to, or after, the initially heating at 130. As discussed, the uncured structural resin has a structural resin viscosity, which is less than the surface resin viscosity, a structural resin gel point temperature, which is greater than the surface resin gel point temperature, and a structural resin gel time, which is greater than the surface resin gel time. Subsequent to the subsequently heating at 140, the uncured surface resin and the uncured structural resin are fully cured. Stated another way, a combination of the initially heating at 130 and the subsequently heating at 140 is sufficient to fully cure both the uncured surface resin and the uncured structural resin, such as to produce and / or generate the cured surface resin an a cured structural resin, respectively.
[0021] An example of the cured composite structure is illustrated in Fig. 3. More specifically, Fig. 3 illustrates a composite structure 10 in the form of a cured composite structure 14. Cured composite structure 14 may be formed from uncured composite structure 12 of Fig. 2, such as by performing methods 100. Cured composite structure 14 includes structural layer 20, in the form of a cured structural layer 24, that includes structural resin 26, in the form of cured structural resin 30. Cured composite structure 14 also includes surface layer 50, in the form of a cured surface layer 54, that includes surface resin 56, in the form of cured surface resin 60.
[0022] In some examples, the subsequently heating at 140 includes subsequently heating for a subsequent heating time. In some such examples, the subsequent heating time includes and / or is a dwell time during which the partially cured composite structure is maintained at the final cure temperature. Stated another way, the subsequently heating at 140 may include dwelling at the final cure temperature for the subsequent heating time. In some such examples, the subsequent heating time also may be referred to herein as a subsequent dwell time at the final cure temperature.
[0023] In some examples, the subsequent heating time includes and / or is a ramp time during which the uncured composite structure is ramped from the initial temperature and / or to the final cure temperature. Stated another way, the subsequently heating at 140 may include ramping the partially cured composite structure to the final cure temperature during the subsequent heating time. In some such examples, the subsequent heating time also may be referred to herein as a subsequent ramp time to the final cure temperature.
[0024] The final cure temperature may have any suitable magnitude and / or value, such as may be selected based, at least in part, on one or more desired properties of the structural layer, the structural resin viscosity, the structural resin gel point temperature, and / or the structural resin gel time. Examples of the final cure temperature include final cure temperatures of at least 110 ºC, at least 115 ºC, at least 120 ºC, at least 125 ºC, at least 130 ºC, at least 135 ºC, at least 140 ºC, at least 145 ºC, at least 150 ºC, at least 155 ºC, at least 160 ºC, at least 165 ºC, at least 170 ºC, at least 175 ºC, at least 180 ºC, at least 185 ºC, at least 190 ºC, at least 195 ºC, at least 200 ºC, at most 260 ºC, at most 250 ºC, at most 240 ºC, at most 230 ºC, at most 220 ºC, at most 210 ºC, at most 200 ºC, at most 195 ºC, at most 190 ºC, at most 185 ºC, at most 180 ºC, at most 175 ºC, at most 170 ºC, at most 165 ºC, at most 160 ºC, at most 155 ºC, at most 150 ºC, at most 145 ºC, at most 140 ºC, at most 135 ºC, and / or at most 130 ºC. Stated differently, the final cure temperature may be bounded by any of the above temperatures, as appropriate.
[0025] In some examples, the final cure temperature differs from, or is greater than, the initial temperature by a threshold temperature difference. As examples, the difference between the final cure temperature and the initial temperature may be at least 20 ºC, at least 25 ºC, at least 30 ºC, at least 35 ºC, at least 40 ºC, at least 45 ºC, at least 50 ºC, at least 55 ºC, at least 60 ºC, at least 65 ºC, at least 70 ºC, at least 75 ºC, at least 80 ºC, at most 120 ºC, at most 110 ºC, at most 100 ºC, at most 90 ºC, at most 80 ºC, at most 70 ºC, at most 60 ºC, and / or at most 50 ºC. Stated differently, the threshold temperature difference may be bounded by any of the above temperature differences, as appropriate.
[0026] Similarly, the subsequent heating time may have any suitable magnitude and / or value, such as may be selected based, at least in part, on one or more desired properties of the structural layer, the structural resin viscosity, the structural resin gel point temperature, and / or the structural resin gel time. Examples of the subsequent heating time include subsequent heating times of at least 15 minutes, at least 20 minutes, at least 25 minutes, at least 30 minutes, at least 35 minutes, at least 40 minutes, at least 45 minutes, at least 50 minutes, at least 55 minutes, at least 60 minutes, at most 150 minutes, at most 140 minutes, at most 130 minutes, at most 120 minutes, at most 115 minutes, at most 110 minutes, at most 105 minutes, at most 100 minutes, at most 95 minutes, at most 90 minutes, at most 85 minutes, at most 80 minutes, at most 75 minutes, at most 70 minutes, at most 65 minutes, and / or at most 60 minutes. Stated differently, the subsequent heating time may be bounded by any of the above heating times, as appropriate.
[0027] In some examples, the subsequent heating time differs from, or is greater than, the initial heating time by a threshold time difference. Examples of the difference between the subsequent heating time and the initial heating time include times of at least 5 minutes, at least 10 minutes, at least 15 minutes, at least 20 minutes, at least 25 minutes, at least 30 minutes, at least 35 minutes, at least 40 minutes, at least 45 minutes, at least 50 minutes, at least 60 minutes, at least 70 minutes, at least 80 minutes, at least 90 minutes, at least 100 minutes, at least 110 minutes, at least 120 minutes, at most 150 minutes, at most 140 minutes, at most 130 minutes, at most 120 minutes, at most 110 minutes, at most 100 minutes, at most 90 minutes, at most 80 minutes, at most 70 minutes, at most 60 minutes, at most 50 minutes, and / or at most 40 minutes. Stated differently, the difference between the subsequent heating time and the initial heating time may be bounded by any of the above time differences, as appropriate.
[0028] Structural layer 20 may, may be designed to, and / or may be selected to provide structural integrity to composite structure 10. Stated another way, a primary function of structural layer 20, within composite structure 10, may be to provide structural integrity, such as via providing a desired level of rigidity, stiffness, and / or flexibility to composite structure 10.
[0029] As illustrated in dashed lines in Figs. 2-3, structural layer 20 may include a plurality of structural fibers 32, which may be at least partially, or even completely, encapsulated within structural resin 26, within uncured structural resin 28, and / or within cured structural resin 30. Examples of the plurality of structural fibers 32 include a plurality of structural carbon fibers, a plurality of structural fiberglass fibers, and / or a plurality of structural aramid fibers. In some examples, structural layer 20 and / or structural fibers 32 include and / or are arranged in a plurality of layered structural plies of composite material, which may include structural resin 26, uncured structural resin 28, and / or cured structural resin 30.
[0030] Structural resin 26 may include and / or be any suitable resin that may have, define, and / or exhibit the structural resin viscosity, the structural resin gel point temperature, and / or the structural resin gel time. Examples of structural resin 26 include a structural epoxy resin, a structural thermoset resin, a structural phenolic resin, and / or a structural polybismaleimide resin.
[0031] Surface layer 50 may, may be designed to, and / or may be selected to provide a desired surface property and / or characteristic to composite structure 10. In some examples, surface layer 50 may define an ultraviolet light-resistant layer of cured composite structure 14. The ultraviolet light-resistant layer may be configured to resist degradation of cured composite structure 14 when exposed to ultraviolet light and / or to protect structural layer 20 from ultraviolet light. In other examples, surface layer 50 may define a sealing layer of cured composite structure 14. The sealing layer may be configured to seal a remainder of cured composite structure 14, such as structural layer 20, from contact with an ambient environment that surrounds cured composite structure 14. In yet other examples, surface layer 50 may define an adhesion layer, a primer layer, and / or an in-mold primer layer of cured composite structure 14. The adhesion layer, the primer layer, and / or the in-mold primer layer may be configured to facilitate adhesion of another layer and / or material, such as paint, to cured composite structure 14.
[0032] As illustrated in dashed lines in Figs. 2-3, surface layer 50 may include a plurality of surface fibers 62, which may be at least partially, or even completely, encapsulated within surface resin 56, within uncured surface resin 58, and / or within cured surface resin 60. Examples of the plurality of surface fibers 62 include a plurality of fiberglass surface fibers, a plurality of polyester surface fibers, and / or a plurality of nylon surface fibers. The plurality of surface fibers 62 may be arranged, within surface layer 50, in any suitable manner. As examples, the plurality of surface fibers may be arranged in a surface weave, a surface mat, and / or a surface scrim mat.
[0033] Surface resin 56 may include and / or be any suitable resin that may have, define, and / or exhibit the surface resin viscosity, the surface resin gel point temperature, and / or the surface resin gel time. Additionally or alternatively, surface resin 56 may include and / or be any suitable resin that may restrict ultraviolet light from being incident upon structural layer 20, such as via reflection and / or absorption of the ultraviolet light. Additionally or alternatively, surface resin 56 may include and / or be any suitable resin that may seal structural layer 20. Additionally or alternatively, surface resin 56 may include and / or be any suitable resin that may improve adhesion, may function as a primer, and / or may function as an in-mold primer for attachment of another layer and / or material to cured composite structure 14. Examples of surface resin 56, of uncured surface resin 58, and / or of cured surface resin 60 include an ultraviolet light-resistant surface resin, an aliphatic epoxy surface resin, and / or a fire-retardant surface resin.
[0034] In some examples, and as illustrated in dashed lines in Figs. 2-3, surface layer 50 includes an additive 64. Additive 64, when present, may be adapted, configured, formulated, synthesized, and / or selected to modify and / or change at least one property of surface layer 50. Some examples of additive 64 include a flow-control additive. The flow-control additive may be selected such that the surface resin viscosity has a desired surface resin viscosity magnitude. Some examples of the flow-control additive include, or are, titanium dioxide.
[0035] As discussed, the surface resin viscosity is greater than the structural resin viscosity. Such a configuration may decrease a potential for the uncured surface resin to diffuse into and / or mix with the uncured structural resin, such as prior to and / or during the initially heating at 130. Subsequent to the initially heating at 130, and as discussed, the uncured surface resin has gelled, has crosslinked, and / or has been converted to the cured surface resin. The gelled uncured surface resin, the crosslinked uncured surface resin, and / or the cured surface resin then defines a unitary and / or cohesive surface layer, which resists mixing and / or diffusion with the uncured structural resin. Such a configuration permits cured composite structures formed via methods 100, according to the present disclosure, to maintain at least partial separation between the cured surface resin and the cured structural resin within the cured composite structure, thereby permitting the cured surface resin to protect the structural layer from environmental factors, as discussed herein.
[0036] The surface resin viscosity may be greater than the structural resin viscosity by any suitable magnitude and / or value. As an example, the surface resin viscosity may be a threshold viscosity multiple of the structural resin viscosity. Stated differently, the structural resin viscosity may be a threshold viscosity fraction of the surface resin viscosity, with the threshold viscosity fraction being defined as an inverse of the threshold viscosity multiple. Examples of the threshold viscosity multiple include multiples of at least 5, at least 7.5, at least 10, at least 20, at least 40, at least 60, at least 80, at least 100, at least 200, at least 400, at least 600, at least 800, at least 1,000, at most 10,000, at most 8,000, at most 6,000, at most 4,000, at most 2,000, at most 1,000, at most 800, at most 600, at most 400, at most 200, and / or at most 100. Stated differently, the threshold viscosity multiple may be bounded by any of the above multiples, as appropriate.
[0037] As also discussed, the surface resin gel point temperature is less than the structural resin gel point temperature. As such, and as discussed, the initial temperature, which is attained during the initially heating at 130, is sufficient to gel the uncured surface resin but insufficient to gel the uncured structural resin. Stated another way, by specifying that the surface resin gel point temperature is less than the structural resin gel point temperature, the composite structures and methods, disclosed herein, may gel the uncured surface resin earlier in the curing process when compared to the uncured structural resin. This earlier gelling of the uncured surface resin may permit and / or facilitate the at least partial separation between the cured surface resin and the cured structural resin within the cured composite structure, thereby permitting the cured surface resin to protect the structural layer from environmental factors, as discussed herein.
[0038] The surface resin gel point temperature may differ from the structural resin gel point temperature by any suitable amount. As an example, the surface resin gel point temperature may be a threshold gel temperature difference less than the structural resin gel point temperature. Stated differently, the structural resin gel point temperature may be the threshold gel temperature difference greater than the surface resin gel point temperature. Examples of the threshold gel temperature difference include temperature differences of at least 20 ºC, at least 25 ºC, at least 30 ºC, at least 35 ºC, at least 40 ºC, at least 45 ºC, at least 50 ºC, at least 55 ºC, at least 60 ºC, at least 65 ºC, at least 70 ºC, at least 75 ºC, at least 80 ºC, at most 120 ºC, at most 110 ºC, at most 100 ºC, at most 90 ºC, at most 80 ºC, at most 70 ºC, at most 60 ºC, and / or at most 50 ºC. Stated differently, the threshold gel temperature difference may be bounded by any of the above temperature differences, as appropriate.
[0039] As also discussed, the surface resin gel time may be less than the structural resin gel time. As such, and as discussed, the uncured surface resin may gel more quickly relative to the uncured structural resin at a given temperature. Stated differently, the cure kinetics of the uncured surface resin may be relatively faster when compared to the cure kinetics of the uncured structural resin. Stated another way, by specifying that the surface resin gel time is less than the structural resin gel time, the composite structures and methods, disclosed herein, may gel the uncured surface resin earlier in the curing process when compared to the uncured structural resin. This earlier gelling of the uncured surface resin may permit and / or facilitate the at least partial separation between the cured surface resin and the cured structural resin within the cured composite structure, thereby permitting the cured surface resin to protect the structural layer from environmental factors, as discussed herein.
[0040] The surface resin gel time may differ from the structural resin gel time by any suitable amount. As an example, the surface resin gel time may be a threshold gel time difference less than the structural resin gel time. Stated differently, the structural resin gel time may be the threshold gel time difference greater than the surface resin gel time. Examples of the threshold gel time difference include time differences of at least 5 minutes, at least 10 minutes, at least 15 minutes, at least 20 minutes, at least 25 minutes, at least 30 minutes, at least 35 minutes, at least 40 minutes, at least 45 minutes, at least 50 minutes, at most 120 minutes, at most 110 minutes, at most 100 minutes, at most 90 minutes, at most 80 minutes, at most 70 minutes, at most 60 minutes, at most 50 minutes, and / or at most 40 minutes. Stated differently, the threshold gel time difference may be bounded by any of the above time differences, as appropriate.
[0041] Fig. 4 is a plot illustrating viscosity as a function of cure temperature at a constant ramp rate for two resins that may be utilized with the uncured composite structures, composite structures, and methods, according to the present disclosure. Fig. 4 graphically illustrates the above-described differences between the surface resin, for which cure kinetics are illustrated in solid lines, and the structural resin, for which cure kinetics are illustrated in dashed lines. As illustrated in Fig. 4, and as the cure temperature is ramped at the constant ramp rate, both the surface resin viscosity and the structural resin viscosity initially will decrease. However, and as also illustrated in Fig. 4, the surface resin and the structural resin are selected such that the surface resin viscosity always remains greater than the structural resin viscosity.
[0042] Fig. 4 further illustrates that both the surface resin and the structural resin exhibit a corresponding viscosity minimum, which corresponds generally to the surface resin gel point temperature and the structural resin gel point temperature, respectively. Both the surface resin and the structural resin then exhibit a pronounced increase in viscosity due to gelling, or crosslinking, of the respective resins. As discussed herein, this increase in viscosity occurs at a lower temperature for the surface resin relative to the structural resin.
[0043] As discussed, uncured composite structures 12, cured composite structures 14, and methods 100, which are disclosed herein, limit mixing, mingling, and / or diffusion between surface layer 50 and structural layer 20. As also discussed, this limiting of the mixing, mingling, and / or diffusion permits the disclosed uncured composite structures 12, cured composite structures 14, and methods 100 to exhibit improved and / or desired characteristics when compared to conventional composite structures formed via conventional methods. More specifically, uncured composite structures 12, cured composite structures 14, and methods 100, according to the present disclosure, permit surface layer 50 to be more uniform relative to conventional surface layers and / or permit surface layer 50 to better protect structural layer 20 from environmental factors when compared to the conventional surface layers.
[0044] Turning to Fig. 3, it is expected that methods 100 and / or cured composite structures 14 formed therefrom may exhibit limited mixing, mingling, and / or diffusion between surface layer 50 and structural layer 20. This limited mixing, mingling, and / or diffusion may be desirable in that it may increase adhesion between surface layer 50 and structural layer 20. However, this mixing, mingling, and / or diffusion between cured surface layer 54 and cured structural layer 24, within cured composite structure 14, may be confined to an interface region 40 between cured surface layer 54 and cured structural layer 24. Stated another way, and as illustrated in Fig. 3, interface region 40 may include both cured surface resin 60 and cured structural resin 30 and / or may be a mixture of cured surface resin 60 and cured structural resin 30. However, interface region 40 may be covered and / or encapsulated by cured surface layer 54, which includes cured surface resin 60 but may not include cured structural resin 30. Stated another way, cured surface layer 54 may define an exposed surface 68, and at least exposed surface 68 may be free of and / or spaced-apart from cured structural resin 30. Additionally or alternatively, cured structural layer 24 may be free of and / or spaced-apart from cured surface resin 60. This is in contrast to conventional cured composite structures formed via conventional methods, within which the conventional structural resin generally extends to the exposed surface of the conventional surface layer, thereby decreasing the ability of the conventional surface layer to protect the conventional structural layer from environmental factors.
[0045] In some examples, and as illustrated in Fig. 3, cured surface layer 54 defines a surface layer thickness 66, or an average surface layer thickness 66. Similarly, and in some such examples, interface region 40 defines an interface region thickness 42, or an average interface region thickness 42. In some such examples, a ratio of average surface layer thickness 66 to average interface region thickness 42 may be at least 0.1, at least 0.25, at least 0.5, at least 0.75, at least 1, at least 1.25, at least 1.5, at least 1.75, at least 2, at most 5, at most 4.5, at most 4, at most 3.5, at most 3, at most 2.5, at most 2, at most 1.75, at most 1.5, at most 1.25, at most 1, at most 0.75, and / or at most 0.5. Such a configuration may provide a desired amount, or distance, of separation between exposed surface 68 and cured structural resin 30 contained within interface region 40. Stated differently, the ratio may be bounded by any of the above ratios, as appropriate.
[0046] In another example according to the present disclosure, an uncured composite structure, comprises: a structural layer that includes an uncured structural resin, wherein the uncured structural resin has a structural resin viscosity, a structural resin gel point temperature, and a structural resin gel time; and a surface layer that includes an uncured surface resin, wherein the uncured surface resin includes a surface resin viscosity that is greater than the structural resin viscosity, a surface resin gel point temperature that is less than the structural resin gel point temperature, and a surface resin gel time that is less than the structural resin gel time.
[0047] In another example, not currently claimed herein, but useful for understanding the claimed method and uncured composite structure, there is provided a cured composite structure, comprises: a cured structural layer that includes a cured structural resin formed from an uncured structural resin, wherein the uncured structural resin has a structural resin viscosity, a structural resin gel point temperature, and a structural resin gel time; a cured surface layer that includes an exposed surface defined by a cured surface resin formed from an uncured surface resin, wherein the uncured surface resin includes a surface resin viscosity that is greater than the structural resin viscosity, a surface resin gel point temperature that is less than the structural resin gel point temperature, and a surface resin gel time that is less than the structural resin gel time; and an interface region between the cured surface layer and the cured structural layer, wherein: (i) the exposed surface is free of the cured structural resin; and (ii) the interface region includes a mixture of the cured surface resin and the cured structural resin.
Claims
1. A method (100) of curing an uncured composite structure (12) that includes a structural layer (20), which includes an uncured structural resin (28) with a structural resin viscosity, a structural resin gel point temperature, and a structural resin gel time, and a surface layer (50), which includes an uncured surface resin (58) with a surface resin viscosity that is greater than the structural resin viscosity, a surface resin gel point temperature that is less than the structural resin gel point temperature, and a surface resin gel time that is less than the structural resin gel time, the method (100) comprising: initially heating (130), for an initial heating time, the uncured composite structure (12) to an initial temperature to generate a partially cured composite structure, wherein the initially heating (130) is sufficient to gel the uncured surface resin (58) but insufficient to gel the uncured structural resin (28); and subsequently heating (140), for a subsequent heating time, the partially cured composite structure to a final cure temperature, which is greater than the initial temperature, to generate a cured composite structure (14), wherein a combination of the initially heating (130) and the subsequently heating (140) is sufficient to fully cure both the uncured surface resin (58) and the uncured structural resin (28).
2. The method (100) of claim 1, wherein: the initial temperature is at least 90 degrees Celsius (ºC) and at most 140 ºC; and / or the final cure temperature is at least 120 ºC and at most 260-ºC.
3. The method (100) of claim 1 or 2, wherein a difference between the final cure temperature and the initial temperature is at least 20 ºC.
4. The method (100) of any one of claims 1-3, wherein: the initial heating time is at least 2 minutes and at most 30 minutes; and / or the subsequent heating time is at least 15 minutes and at most 120 minutes.
5. The method (100) of any one of claims 1-4, wherein a difference between the subsequent heating time and the initial heating time is at least 10 minutes.
6. The method (100) of any one of claims 1-5, wherein the structural layer (20) further includes at least one of: (i) a plurality of structural fibers (32) at least partially encapsulated within the uncured structural resin (28); (ii) a plurality of structural carbon fibers at least partially encapsulated within the uncured structural resin (28); and (iii) a plurality of layered structural plies of composite material that includes the uncured structural resin (28).
7. The method (100) of any one of claims 1-6, wherein the uncured structural resin (28) includes at least one of: (i) a structural epoxy resin; (ii) a structural thermoset resin; (iii) a structural phenolic resin; and (iv) a structural polybismaleimide resin.
8. The method (100) of any one of claims 1-7, wherein the surface layer (50) further includes a plurality of surface fibers (62) at least partially encapsulated within the uncured surface resin (58).
9. The method (100) of any one of claims 1-8, wherein the uncured surface resin (58) includes at least one of: (i) an ultraviolet light-resistant surface resin; (ii) an aliphatic epoxy surface resin; and (iii) a fire-retardant surface resin.
10. The method (100) of any one of claims 1-9, wherein the surface layer (50) is configured to at least one of: (i) define an ultraviolet light-resistant layer of the cured composite structure (14); (ii) define a sealing layer of the cured composite structure (14); (iii) define an adhesion layer of the cured composite structure (14); (iv) define a primer layer of the cured composite structure (14); and (v) define an in-mold primer layer of the cured composite structure (14).
11. The method (100) of claim 10, wherein when the surface layer (50) defines at least one of the adhesion layer, the primer layer, and / or the in-mold primer layer, said adhesion layer, primer layer, and / or in-mold primer being configured to facilitate adhesion of another layer and / or material, such as paint, to the cured composite structure (14).
12. The method (100) of any one of claims 1-11, wherein: the surface resin gel point temperature is less than the structural resin gel point temperature by at least 40 ºC; and / or the surface resin gel time is less than the structural resin gel time by at least 5 minutes.
13. The method (100) of any one of claims 1-12, wherein the method (100) further includes applying a pressure (120) to at least one of: (i) the uncured composite structure (12) and during the initially heating (130); and (ii) the partially cured composite structure and during the subsequently heating (140); and wherein, optionally, the initially heating (130) includes hardening the surface layer (50) to generate a hardened surface layer, and further wherein, during the subsequently heating (140) and also during the applying the pressure (120), the method (100) further includes resisting deformation of the hardened surface layer.
14. The method of any one of claims 1-13, wherein the surface resin viscosity is a threshold viscosity multiple of the structural resin viscosity, wherein the threshold viscosity multiple is at least 10.
15. An uncured composite structure, comprising: a structural layer that includes an uncured structural resin, wherein the uncured structural resin has a structural resin viscosity, a structural resin gel point temperature, and a structural resin gel time; and a surface layer that includes an uncured surface resin, wherein the uncured surface resin includes a surface resin viscosity that is greater than the structural resin viscosity, a surface resin gel point temperature that is less than the structural resin gel point temperature, and a surface resin gel time that is less than the structural resin gel time.