Carbon fiber reinforced carbide ceramic composite component

ES3084071T3Undetermined Publication Date: 2026-11-10SGL CARBON SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
ES2016791346T
Authority / Receiving Office
ES · ES
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-10-28
Filing Date
2016-10-26
Publication Date
2026-11-10
Estimated Expiration
2036-10-26

AI Technical Summary

Technical Problem

Existing carbon fiber reinforced carbon (CFC) charging racks are susceptible to oxidation, have high open porosity, and are inefficiently manufactured, leading to increased process costs and material degradation.

Method used

A ceramic component comprising a stack of directly adjacent unidirectional carbon fiber fabrics embedded in a ceramic matrix of silicon carbide and elemental silicon, allowing complete infiltration with liquid silicon and resulting in a dense, oxidation-resistant structure.

Benefits of technology

The solution provides a lightweight, high-strength, and low-porosity component suitable for high-temperature applications, reducing energy costs and material degradation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a ceramic component comprising at least one stack of at least two layers of unidirectional non-wavy carbon fiber fabrics embedded in a ceramic matrix containing silicon carbide and elemental silicon, characterized in that all adjacent layers within the at least one stack are directly contiguous with each other, the at least one stack has a minimum thickness of 1.5 mm perpendicular to the plane of the layers, and the ceramic matrix penetrates essentially throughout the component.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a ceramic component containing unidirectional layers of carbon fibers, wherein the layers are arranged directly on top of each other or stacked within the component and form a layer stack with a height or thickness of at least 1.5 mm. The present invention further relates to a method for manufacturing this component and the use of the component as a charging rack for the high-temperature treatment of goods.

[0002] Curing racks are needed, for example, to harden goods such as machine components or automotive parts by exposing them to high temperatures while they rest on the rack. The material requirements for such curing racks include high mechanical strength (stiffness and rigidity), high temperature resistance, and low weight. Carbon fiber reinforced carbon is an excellent material that meets these criteria. These curing racks are typically manufactured by laminating unidirectional, resin-impregnated carbon fiber fabrics (e.g., prepregs) on top of each other, curing them under increased pressure and temperature, and then subjecting them to pyrolysis, during which the cured resin is converted into carbon.

[0003] The unidirectional carbon fiber fabrics consist (and also within the scope of the present invention) of a continuous band of closely spaced, parallel, continuous carbon fibers. After laminating several layers of the pre-impregnated carbon fiber fabrics and curing the resin, a carbon fiber reinforced plastic (CFRP) is obtained, with the cured resin forming the matrix of the CFRP. During the pyrolysis of the CFRP, which typically takes place at approximately 800°C, the polymer matrix decomposes and the volatile components contained therein are released. What remains is carbon fiber reinforced carbon (CFC).

[0004] A disadvantage of CFC charging racks, however, is their susceptibility to oxidation and their high open porosity. Therefore, high-temperature treatment with such racks must be carried out in the absence of oxygen. This is typically the case when used in industrial hardening furnaces under a protective gas atmosphere or vacuum, where the workpieces, such as gears, are hardened. The workpieces to be hardened are usually first soft-machined; for example, the teeth of gears are milled. Afterwards, the workpieces must be cleaned of residues such as cooling lubricants or washing solutions and dried. For this purpose, the entire batch is heated to up to 500°C using a gas flame under normal atmospheric conditions, thereby burning off the aforementioned impurities. The workpieces then enter the actual heat treatment system or the hardening furnace.Preferably, the goods to be charged are placed on the same charging rack in both heat treatment processes, because changing the charging rack means a significant increase in process costs, as the batch has to cool down to a certain extent between the two processes, be transferred and then reheated.

[0005] However, the continuous use of CFC charging racks during pre-oxidation and subsequent heat treatment or hardening is disadvantageous due to the aforementioned oxidation sensitivity of CFC.

[0006] During the cooling of the charging rack and its contents at the end of the heat treatment, they are sometimes placed in cooling baths containing liquids (e.g., oil). Faster cooling rates are possible there compared to air cooling. However, the cooling medium penetrates the open porosity of the charging rack material. This medium evaporates again during the next hardening cycle, thus exerting a destructive effect on the material.

[0007] It is therefore the object of the present invention to provide an improved component that can be used as a charging rack and has high oxidation resistance, while simultaneously offering high mechanical strength (stiffness and rigidity), high temperature resistance, low weight and low open porosity.

[0008] Silicon carbide (SiC) ceramic components are a well-known example of oxidation-resistant components. These can typically be produced by liquid siliconization of a CFC molded body, i.e., by infiltrating CFC with liquid silicon. In this process, some of the carbon reacts with the elemental silicon to form SiC. EP 1 340 733 B1, for example, describes SiC ceramic composites with unidirectional orientation of the reinforcing fibers (especially carbon fibers). Here, the unidirectional reinforcing fibers are in the form of individual roving bundles spaced a certain distance apart.The pore structure that develops during the carbonization of the CFRP to form the CFC body is crucial for the subsequent siliconization and formation of the SiC matrix. Only a suitable pore structure ensures that the liquid silicon penetrates the CFC body uniformly and in sufficient quantity (see EP 1 340 733 B1, paragraph 6). If the reinforcing fiber rovings are aligned parallel and unfixed in the plane, the carbonization of the binder resins leads to unimpeded contraction perpendicular to the fiber orientation. This causes the rovings in the CFC to shrink very tightly against each other, lying side by side with minimal open porosity. This complicates the liquid siliconization process because the pore volume and the distribution of capillaries (microchannels) within the material are adversely affected compared to CFC preforms reinforced with short fibers or fabrics.Using conventional techniques, it is therefore not yet possible to achieve satisfactory properties in C / SiC materials reinforced with unidirectional fibers ("UD fibers") (see EP 1 340 733 B1, paragraph 8). The spacing of the roving bundles in EP 1 340 733 B1 is therefore necessary to allow the liquid silicon to completely infiltrate or impregnate the CFC molded body.

[0009] German patent DE 10 2007 007 410 A1 also describes a SiC ceramic composite material with unidirectional carbon fiber orientation. Similar to the CFC charging racks described above, unidirectional carbon fiber fabrics are used. However, to enable the final liquid siliconization to be carried out completely, due to the difficulties mentioned in EP 1 340 733 B1, a spacer in the form of a coating or a transverse thread system is provided between the unidirectional carbon fiber fabrics. This spacer preferably evaporates completely during pyrolysis, thus ensuring the pore structure required for liquid siliconization.

[0010] However, a disadvantage of the solutions of EP 1 340 733 B1 and DE 10 2007 007 410 A1 is that the spacing of the rovings or the fabrics proposed in both solutions results in areas that are not reinforced with carbon fiber, which means that the component has to be designed to be correspondingly thicker, i.e. heavier.

[0011] The object of the present invention is also to provide an improved component.

[0012] Within the scope of the present invention, it has been found that, under certain conditions, a carbide ceramic component with unidirectional carbon fiber fabrics can be produced for the first time, in which the fiber fabrics can be stacked directly on top of each other without any predetermined spacing, and the stack can have practically any thickness. Despite the densely packed unidirectional carbon fibers, the CFC preform can be completely infiltrated with liquid silicon.

[0013] The object of the present invention was therefore solved by providing a ceramic component comprising at least one stack of at least two layers of unidirectional carbon fiber fabric embedded in a ceramic matrix containing silicon carbide and elemental silicon, characterized in that all adjacent layers within the at least one stack are directly adjacent to each other, that the at least one stack has a thickness perpendicular to the plane of the layers of at least 1.5 mm and that the ceramic matrix penetrates substantially the entire component.

[0014] The phrase "all adjacent layers within the at least one stack are directly adjacent to one another" in the context of the present invention means that the layers are not deliberately kept at a distance, as is the case, for example, with the methods described in patent documents EP 1 340 733 B1 and DE 10 2007 007 410 A1. However, the present invention encompasses the presence, or potential presence, of a matrix film between the layers or between the fibers of the adjacent layers, which is practically always present when pre-impregnated fiber layers are directly laminated together.

[0015] Due to its closely spaced layers, the component according to the invention is characterized by increased strength. This allows the component to be designed thinner and therefore lighter overall for the respective application, for example as a charging rack. This facilitates handling and reduces the costs of using the charging rack, as it requires less energy for heating due to its lower mass.

[0016] The thickness, or height, of the stack of directly superimposed unidirectional carbon fiber fabrics is not limited. In contrast to DE 10 2007 007 410 A1, according to which the layers of carbon fiber fabrics separated by spacers each have a thickness of only about 0.1 mm (see figures of DE 10 2007 007 410 A1), the thickness of the corresponding layers, or of the layer stack, according to the present invention is at least 1.5 mm. This cannot be achieved with known methods. Preferably, the aforementioned thickness is at least 2.0 mm and more preferably at least 2.5 mm. Most preferably, the layer stack within the component is as thick as the entire component according to the invention itself, i.e., the component preferably consists exclusively of a stack of directly adjacent layers of unidirectional carbon fiber fabrics embedded in the ceramic matrix.

[0017] The thickness of individual layers of unidirectional carbon fiber fabrics is not particularly limited. It is possible for a layer to be so thin that it consists of only a single monofilament layer, meaning that the layer thickness is practically equal to the diameter of a carbon fiber, which is typically in the range of 6 to 9 µm. When using such monofilament layers, the number of layers stacked directly on top of each other according to the invention is correspondingly large, so that the layer stack has a height of at least 1.5 mm. In the case of particularly thick layers, for example, thicker than 0.75 mm, it is possible that there are actually only two layers stacked directly on top of each other in the component, so that the stack thickness is at least 1.5 mm.

[0018] Unidirectional carbon fiber fabrics are typically obtained by spreading one or more carbon fiber rovings to a certain width. Carbon fiber rovings are bundles of continuous, parallel, untwisted, and untwisted carbon fiber filaments. Typically, one or more 50K rovings are used. A 50K roving consists of approximately 50,000 individual filaments. These spread fiber tapes are available, among other things, pre-impregnated with a resin as prepregs. They typically have a thickness of around 0.25 mm. Starting from such prepregs, for example, the inventive process described below can be carried out.

[0019] For the suitability of the component in high-temperature applications in oxidative atmospheres, it is crucial that the ceramic matrix essentially permeates the entire component. This means, as further explained below in the context of the inventive process, that the CFC preform is completely infiltrated by the liquid silicon during siliconization, and that the carbon matrix of the CFC preform is at least partially converted into SiC. This makes the component according to the invention significantly more resistant to oxidation than, for example, CFC components siliconized only on the surface. In the latter, atmospheric oxygen penetrates the interior over time and gradually destroys the integrity and stability of the component.

[0020] Preferably, the matrix has a homogeneous composition across the entire component. However, this does not preclude the possibility that the component may have a certain surface treatment, which may penetrate from the surface into the matrix to a certain depth. The composition of the matrix's structural components, i.e., those responsible for its strength, is preferably homogeneous. This results in equally homogeneous component properties, such as strength and oxidation resistance.

[0021] According to a preferred embodiment of the component according to the invention, successive layers within the at least one stack vary in their fiber orientation relative to one another. For example, the layers can be arranged alternately in 0° and 90° fiber orientations, which is preferred because this variation leads to a significant improvement in the component's stability perpendicular to the 0° direction, compared to a component in which all unidirectional fiber layers are oriented in only one direction, the 0° direction, while requiring only a slightly higher manufacturing effort. A 0° / 60° / 120° sequence of successive layers is also possible. The type of variation in the fiber orientations of individual layers is not particularly restricted and can be designed according to the load profile of the component in the subsequent application.

[0022] Preferably, the component according to the invention has an open porosity of a maximum of 3.5%, more preferably a maximum of 3.0%. The lower the open porosity of the component, the fewer attack surfaces are offered for oxidative attacks. The open porosity can be reduced, for example, by re-compacting the CFC body one or more times with a liquid carbon source. This process is described in more detail below in the context of a preferred embodiment of the method according to the invention.

[0023] Preferably, the component according to the invention has a fiber volume fraction in the range of 50-65%. The fiber volume fraction can be determined geometrically or optically, for example, using micrographs. A high fiber volume fraction ensures a correspondingly high modulus of elasticity of the component. Such a high fiber volume fraction of carbon fibers in SiC ceramic components, as in the preferred embodiment where the thickness of the stack according to the invention corresponds to the thickness of the entire component, cannot be produced using known methods. Even with densely pressed carbon fiber fabrics, the fiber volume fraction is lower than with non-woven fabrics, since gaps inevitably exist within a fabric that are not filled with fibers.

[0024] A simple embodiment of the component according to the invention is a plate in whose plane the fiber lay-ups are oriented. More complex embodiments of the present invention are preferably assembled from individual such plate-shaped components. This assembly takes place before siliconization, as described below in the context of a preferred method according to the invention. The component, assembled in a form-fit manner in the graphitized CFC state, is then siliconized as a whole. In this process, the components are bonded together at the connection points in a material-bonded and irreversible manner. Therefore, in a preferred embodiment, the present invention relates to a ceramic component comprising at least two material-bonded components, wherein each of the at least two components is also designed as a ceramic component according to the invention.

[0025] Preferably, the material-bonded connection between the interfaces of the interconnected components of the ceramic component consists of elemental silicon. However, the form-fitted CFC components can also be additionally bonded with an adhesive. The adhesive is preferably carbonizable and can thus be converted into carbon during the siliconization of the assembled component upon heating. This carbon, through its porosity, conducts the liquid silicon from one of the two connected components to the other. The resulting ceramic component therefore exhibits not only elemental silicon but also SiC at the material-bonded connection between the interfaces of the interconnected components. This bonding and joining technique for materials undergoing siliconization is known and is described, for example, in DE 10 2011 007 815 A1.The type of adhesive and any fillers it may contain are not particularly restricted.

[0026] The component according to the invention preferably exhibits an oxidative weight loss of a maximum of 0.05%, more preferably 0.03%, in an oxidation test in air at 400°C within 1 hour.

[0027] The component according to the invention preferably has a Young's modulus of at least 60 GPa. The component according to the invention preferably has a strength of at least 190 MPa. Young's modulus and strength are known to be determined in the 3-point bending test according to the current test standard EN 658-3. In the case of composite components, these parameters naturally only apply to the individual, homogeneous components that are not interrupted by joints.

[0028] The component according to the invention preferably has a density of no more than 2.0 g / cm³. This low density results from the relatively high carbon content, which in turn is due to the high fiber volume fraction. The carbon fibers in the component are therefore still almost intact and have only been minimally attacked by silicon and converted to SiC. The low density is particularly advantageous for use in charging racks, because a lower density also results in a lower heat capacity, which reduces energy costs in the application.

[0029] Another aspect of the present invention relates to a method for manufacturing a ceramic component comprising the following steps: a) direct layering of at least two unidirectional carbon fiber fabrics impregnated with a polymer or a polymer precursor, b) consolidation of the layered carbon fiber fabrics under increased pressure and temperature to obtain a carbon fiber reinforced plastic, c) carbonization of the carbon fiber reinforced plastic at a temperature between 600°C and 1000°C to obtain carbon fiber reinforced carbon, d) graphitization of the carbon fiber reinforced carbon at a temperature of at least 1800°C, e) siliconization of the graphitized carbon fiber reinforced carbon in step d), wherein the siliconization is carried out in such a way that at least a portion of the carbon fibers of at least one of the carbon fiber fabrics face the end face of a surface of the graphitized carbon fiber reinforced carbon in contact with liquid silicon.

[0030] The component according to the invention described above is preferably manufactured using the method according to the invention. All features mentioned in connection with the component according to the invention therefore also apply accordingly to the method and vice versa.

[0031] Direct layering means that the impregnated, unidirectional carbon fiber fabrics are placed directly on top of each other, without anything between them. As described above in connection with patent documents EP 1 340 733 B1 and DE 10 2007 007 410 A1, liquid siliconizing of CFC bodies containing unidirectional carbon fiber fabrics is not readily possible because the densely packed carbon fibers in the fabric do not have a sufficiently large pore structure through which the liquid silicon can penetrate the body. Within the scope of the present invention, measures have been found that enable complete penetration of the body with liquid silicon.

[0032] A crucial factor influencing the formation of a suitable pore system in the CFC body is the graphitization of the CFC body described in step d). At graphitization temperatures of 1800°C and above, the carbon fiber undergoes a specific change in its geometry: it becomes shorter and simultaneously thicker; that is, the carbon fiber shrinks in the fiber direction while expanding perpendicular to it. This expansion leads to the formation of channels along the carbon fibers after cooling, which are suitable for siliconization. Conveniently, graphitization can also take place in a single step with the preceding carbonization, without the need for intermediate cooling. This means that the body to be carbonized and graphitized can be brought to the selected graphitization temperature in one step.

[0033] To allow the silicon to enter these channels, the invention provides that during liquid siliconization, the graphitized CFC body is brought into contact with liquid silicon in such a way that at least a portion of the carbon fibers of the graphitized, carbon fiber-reinforced carbon faces the contact surface with the liquid silicon. The exact angle at which these carbon fibers face the contact surface is not particularly restricted; that is, they can also face the contact surface obliquely. To illustrate this more clearly, for example, in plate-shaped components according to the invention with 0° / 90° fiber orientation of the layups, the siliconization can be carried out via any edge surface of the corresponding CFC plate. It has been shown that once the silicon has found its way into the interior of the preform, it is completely impregnated.Silicification becomes more difficult, however, when the exemplary, plate-shaped preform is to be silicified over its large surface area, which lies parallel to the layers, for example by placing it on wicks.

[0034] The polymer or polymer precursor mentioned in step a) is not particularly restricted. It can be a solution, a melt, or a powder of synthetic resins, thermoplastics, or their precursors, with synthetic resins being preferred because these can usually be converted into dimensionally stable thermosets. Suitable and therefore preferred synthetic resins are phenolic resin, furan resin, and cyanate esters. According to a preferred embodiment, the polymer or polymer precursor therefore comprises a synthetic resin selected from the group consisting of phenolic resin, furan resin, and cyanate esters. A carbonizable thermoplastic is used as a preferred thermoplastic.A "carbonizable thermoplastic" is defined as a thermoplastic which, when heated to a temperature of at least 800°C in the absence of oxidizing substances, forms a carbon residue whose mass is at least 20% of the mass (in the case of solutions, the dry mass) of the thermoplastic used.

[0035] Consolidation according to step b) means that the superimposed, impregnated carbon fiber layups are solidified to form a CFRP body. In the case of thermoset precursors, such as phenolic resins, furan resins, or cyanate esters, the consolidation step includes the curing of the resin. In the case of thermoplastics, the consolidation step includes bonding the layers together by melting the thermoplastic.

[0036] According to a preferred embodiment of the present invention, the carbon fiber reinforced carbon is subjected to at least one post-treatment after step c), which comprises the following steps: c1) Impregnating the carbon fiber reinforced carbon with a liquid carbon supplier and c2) Carbonizing the impregnated carbon fiber reinforced carbon according to step c).

[0037] A carbon source is defined as any liquid substance that leaves carbon after pyrolysis or carbonization. Furthermore, within the scope of the present invention, the terms pyrolysis and carbonization are to be understood as synonyms. Preferred carbon sources are pitch, phenolic resin, and furfuryl alcohol, as these exhibit a high carbon yield.

[0038] According to a preferred embodiment of the present invention, the unidirectional carbon fiber fabric impregnated with a polymer or a polymer precursor is a prepreg selected from the group consisting of phenolic resin prepreg, furan resin prepreg, and cyanate ester prepreg. These are characterized by advantageous handling during lamination and form dimensionally stable CFRP bodies.

[0039] In the case of using a synthetic resin, and in particular a prepreg, the consolidation of the superimposed carbon fiber fabrics includes the curing of the synthetic resin.

[0040] According to a preferred embodiment of the present invention, the graphitized, carbon fiber-reinforced carbon is mechanically machined according to the desired shape of the ceramic component, thereby obtaining a shaped body. Within the scope of the present invention, the shaped body is understood to be the mechanically machined graphitized CFC body before siliconization. The mechanical machining of a CFC body is significantly less complex than that of the considerably harder siliconized component.

[0041] According to a preferred embodiment of the present invention, at least two molded parts are positively connected to one another in such a way that at the respective contacting interfaces of the connected molded parts, at least a portion of the carbon fibers of at least one of the carbon fiber fabrics on both molded parts face these interfaces. This contributes to a better transfer of silicon from one component to the other. The term "face" here has the same meaning as defined above in connection with the component according to the invention. Components joined in this way are monolithic and therefore do not need to be connected by additional, complex connecting elements, such as springs, clamps, etc. In a preferred variant of this embodiment, grooves are incorporated into individual elongated plates along one of the two long edges, the width of which corresponds to the thickness of a plate.These joints extend inwards from the edge of the panel at a right angle towards the center, or rather, the longitudinal axis of the panel. The panels, thus jointed, are then assembled into a checkerboard-like grid, analogous to log house construction. This grid can then be siliconized as a whole. This example shows that it is not necessary to provide end-terminating fibers on the entire interface of one component in contact with another. Rather, it is sufficient to provide end-terminating fibers only in certain areas of the interface, whereby the corresponding areas of the components to be joined must be at least partially in contact with each other.

[0042] Another aspect of the present invention is the use of the ceramic component according to the invention as a charging rack, preferably as a charging rack in high-temperature applications (at least 500°C) and more preferably in the presence of atmospheric oxygen. With regard to this advantageous use, the present invention, or rather the component according to the invention, has already been described in detail above, to which reference is hereby made to avoid repetition.

[0043] The present invention will be illustrated below by means of specific examples. Examples

[0044] Twenty layers of a unidirectional (UD) prepreg were laid directly on top of each other, alternating between 0° and 90° orientations. The UD prepreg consists of parallel carbon fibers impregnated with uncured phenolic resin. According to the invention, the prepreg contains no auxiliary threads or other components perpendicular to the fiber direction of the carbon fibers. Each layer of this prepreg has a height (thickness) of approximately 0.25 mm and a width of approximately 1.20 m. The laminate is cured in a shallow mold at 140 °C for 8 hours at a pressure of 1 bar. The resulting CFRP sheet is cleaned of excess resin on the surface and cut into smaller test specimens measuring 10 cm x 10 cm.

[0045] The CFRP plates are carbonized at 900°C under protective gas (nitrogen).

[0046] One test specimen of the carbonized plate was subjected to the following post-compaction procedure twice (Example 1), another three times (Example 2): Impregnation with pitch and recarbonization (900°C).

[0047] Subsequently, the specimens from Examples 1 and 2 underwent a 24-hour graphitization process at approximately 2000°C. The graphitized CFC specimens were then placed in a siliconization chamber and siliconized at approximately 1700°C. During this process, the specimens were mounted in a graphite frame, which stood within a graphite crucible containing a sufficient quantity of silicon powder for siliconization. The graphite frame ensured the component was aligned with the silicon bath surface according to the invention, meaning that during siliconization, one edge of the plates was in contact with the molten silicon, as some of the carbon fibers terminated at the edges. Candidate Example 1 Candidate Example 2 AD (g / cm 3< ) 1,90 1,80 Open porosity 2% 3% Si content 10% 8% C content 66% 71% SiC content 24% 21% E-modulus (GPa) 60 65 AD: Density determined using water according to Archimedes' principle. Open porosity: Also determined and measured according to Archimedes' principle. Si content: Free silicon, not bound to carbon. C content: Free carbon, not bound to silicon.

[0048] An oxidation test was performed on the specimen according to Example 2. At 400°C in air, a weight loss of approximately 0.15% was determined over 8 hours, which corresponds to a weight loss of about 0.02% per hour.

[0049] In both samples, the exceptionally high proportion of free carbon is striking, resulting from the high fiber volume fraction. This ultimately leads to a high modulus of elasticity and a low density, which, combined with the low susceptibility to oxidation, surpasses that of known ceramic materials. Furthermore, it is evident that additional densification, as in Example 2, results in a higher modulus of elasticity. This is presumably because the carbon fibers are even better protected, thus preserving more of the fiber. The carbon (C) and silicon carbide (SiC) content of Example 2 also point to this.

Claims

1. Ceramic component comprising at least one stack of at least two layers of unidirectional carbon fiber fabric embedded in a ceramic matrix containing silicon carbide and elemental silicon, characterized in that all adjacent layers within the at least one stack directly adjoin one another, wherein the at least one stack has, perpendicularly to the plane of the layers, a thickness of at least 1.5 mm, wherein the ceramic matrix substantially infiltrates the entire component, and wherein the component has a density of at most 2.0 g / cm3 and a fiber volume content in the range of 50-65%.

2. Ceramic component according to claim 1, characterized in that the matrix has a homogeneous composition across the entire component.

3. Ceramic component according to claim 1, characterized in that successive layers within the at least one stack vary in their fiber orientation relative to one another.

4. Ceramic component according to claim 1, characterized in that the component has an open porosity of at most 3.5%.

5. Ceramic component according to claim 1, characterized in that the component comprises at least two bonded components, wherein the at least two components are each likewise configured as ceramic components according to claim 1.

6. Method for producing a ceramic component according to any of the preceding claims, comprising the following steps: a) directly placing at least two unidirectional carbon fiber fabrics impregnated with a polymer or a polymer precursor one on top of the other, b) consolidating the carbon fiber fabrics placed one on top of the other under increased pressure and increased temperature and obtaining a carbon fiber-reinforced plastic material, c) carbonizing the carbon fiber-reinforced plastic material at a temperature between 600°C and 1000°C and obtaining a carbon fiber-reinforced carbon, d) graphitizing the carbon fiber-reinforced carbon at a temperature of at least 1800°C, e) siliconizing the graphitized, carbon fiber-reinforced carbon from step d), wherein the siliconization is carried out in such a manner that, at a surface of the graphitized, carbon fiber-reinforced carbon that is in contact with liquid silicon, at least a portion of the carbon fibers of at least one of the carbon fiber fabrics points with its end face toward said surface.

7. Method according to claim 6, characterized in that the carbon fiber-reinforced carbon according to step c) is subjected, at least once to a posttreatment comprising the following steps: c1) impregnating the carbon fiber-reinforced carbon with a liquid carbon source and c2) carbonizing the impregnated carbon fiber-reinforced carbon according to step c).

8. Method according to claim 6, characterized in that the polymer or polymer precursor comprises a synthetic resin selected from the group consisting of phenolic resin, furan resin and cyanate ester.

9. Method according to claim 6, characterized in that the unidirectional carbon fiber fabric impregnated with a polymer or a polymer precursor is a prepreg selected from the group consisting of phenol resin prepreg, furan resin prepreg and cyanate ester prepreg.

10. Method according to claim 6, characterized in that the consolidation of the carbon fiber fabrics placed one on top of the other comprises curing the synthetic resin.

11. Method according to claim 6, characterized in that the graphitized, carbon fiber-reinforced carbon is mechanically machined according to the desired shape of the ceramic component, resulting in a shaped body.

12. Method according to claim 11, characterized in that at least two shaped bodies are form-fittingly connected to one another such that, at the respective boundary surfaces of the connected shaped bodes that are in contact with one another, at least a portion of the carbon fibers of the respective shaped bodies points with its end face toward said boundary surfaces.

13. Use of the ceramic component according to claim 1 as a charging rack.