METHOD FOR MANUFACTURED DENSITE INORGANIC LAYERS, USABLE AS ELECTRODES AND / OR ELECTROLYTES FOR LI-ION MICROBATTERIES, AND DENSITE INORGANIC LAYERS THUS OBTAINED
By using non-agglomerated nanoparticles with specific size distributions and low-temperature processing, the method addresses inefficiencies in existing lithium ion battery manufacturing, achieving dense, stable, and efficient microbattery components.
Patent Information
- Application Number
- FR2020003104
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-03-30
AI Technical Summary
Existing methods for manufacturing lithium ion battery electrodes and electrolytes are inefficient, costly, and difficult to scale for microbatteries due to high porosity, which affects energy density and diffusion rates, and require high-temperature processes that degrade battery materials.
A method involving the use of non-agglomerated nanoparticles with specific size distributions, deposited via electrophoretic or coating techniques, followed by mechanical compression and low-temperature heat treatment to create dense, compact layers with minimal porosity and defects.
The method produces dense electrodes and electrolytes with high ionic conductivity, stable mechanical structure, good thermal stability, and long lifespan, suitable for microbatteries, while being cost-effective and scalable.
Abstract
Description
Title of the invention: METHOD FOR PRODUCING DENSE INORGANIC LAYERS, USABLE AS ELECTRODES AND / OR ELECTROLYTES FOR MICRO LI-ION BATTERIES, AND DENSE INORGANIC LAYERS OBTAINED THEREBY Technical field of the invention
[0001] The present invention relates to the manufacture of dense inorganic layers, usable in electrochemical devices, in particular as electrode or electrolyte layers. These layers can be used in particular in multi-layer batteries, such as lithium ion microbatteries. The invention also relates to a new method for manufacturing these dense layers. It also relates to the layers obtained by this method, and to multi-layer microbatteries incorporating at least one layer obtained by this method. State of the art
[0002] Lithium ion batteries have the best energy density among the various electrochemical technologies for storing electrical energy available. There are different electrode architectures and chemical compositions for producing lithium ion batteries. The manufacturing processes for lithium ion batteries are presented in numerous articles and patents, and the book "Advances in Lithium-Ion Batteries" (ed. W. van Schalkwijk and B. Scrosati), published in 2002 (Kluever Academie / Plénum Publishers) provides a good overview.
[0003] There is a growing need for microbatteries, i.e. very small rechargeable batteries, capable of being integrated on electronic cards; these electronic circuits can be used in many fields, for example in cards for securing transactions, in electronic labels, in implantable medical devices, in various micromechanical systems.
[0004] According to the state of the art, the electrodes of lithium ion batteries can be manufactured using coating techniques (in particular: roll coating, doctor blade coating, tape casting, slot-die coating). With these methods, the active materials used to produce the electrodes are in the form of powders whose average particle size is between 5 and 15 μm in diameter. These particles are integrated into an ink which is made up of these particles and deposited on the surface of a substrate.
[0005] These techniques make it possible to produce layers with a thickness of between approximately 50 μm and approximately 400 μm. Depending on the thickness of the layers, their porosity and the size of the active particles, the power and energy of the battery can be modulated. To produce microbatteries, a smaller thickness would be desirable.
[0006] The inks (or pastes) deposited to form the electrodes contain particles of active materials, but also (organic) binders, carbon powder to ensure electrical contact between the particles, and solvents which are evaporated during the electrode drying step. To improve the quality of the electrical contacts between the particles and to compact the deposited layers, a calendering step is carried out on the electrodes. After this compression step, the active particles of the electrodes occupy approximately 60% of the volume of the deposit, which means that generally 40% of porosities remain between the particles.
[0007] The contact between each of the particles is essentially punctual and the structure of the electrode is porous. The porosities are filled with an electrolyte, which can be liquid (aprotic solvent in which a lithium salt is dissolved) or in the form of a more or less polymerized gel impregnated with a lithium salt. The thickness of the electrodes of lithium ion batteries being generally between 50 μm and 400 μm, the transport of lithium ions in the thickness of the electrode is carried out via the porosities which are filled with electrolyte (containing lithium salts). Depending on the quantity and size of the porosities, the diffusion rate of lithium in the thickness of the electrode varies.
[0008] To ensure proper battery operation, lithium ions must diffuse both within the particle thickness and within the electrode thickness. Diffusion within the active material particle is slower than within the electrolyte with which the porous electrode is impregnated: this electrolyte is liquid or gelled. The slow diffusion within the electrode particles contributes to the series resistance of the battery. Also, to achieve good battery power, the particle size must be reduced; in standard lithium ion batteries it is typically between 5 pm and 15 pm.
[0009] On the other hand, depending on the thickness of the layers, the size and density of active particles contained in the ink, the power and energy of the battery can be modulated. Increasing the energy density necessarily comes at the expense of the power density. High-power battery cells must use electrodes and separators of low thickness and high porosity, whereas increasing the energy density requires, on the contrary, increasing these same thicknesses and reducing the porosity rate. The article “Optimization of Porosity and Thickness of a Battery Electrode by Means of a Reaction-Zone Model” by John Newman, published in J. Electrochem. Soc., Vol. 142, No. 1 in January 1995, demonstrates the respective effects of electrode thicknesses and porosity on their discharge rate (power) and energy density.
[0010] However, increasing the porosity in the electrodes tends to deteriorate the energy density of the battery: to increase the energy density of the electrodes, it is necessary to reduce the porosity. In current lithium ion batteries, it is essentially the electrolyte-filled porosities located between the active particles that ensure the diffusion of lithium ions in the electrode. In the absence of electrolyte-filled porosities, the transport of lithium ions from one particle to another takes place only at the contacts between the particles, this contact being substantially point-like. Thus, the resistance to the transport of lithium ions is such that the battery cannot operate.
[0011] Furthermore, to function properly, the porosities of the electrodes must be filled with electrolyte. This filling is only possible if these porosities are open. Furthermore, depending on the size of the porosities and their tortuosity, impregnation of the electrode with the electrolyte can become very difficult, or even impossible. When the porosity rate, impregnated with electrolyte, decreases, the electrical resistance of the layer decreases and its ionic resistance increases. When the porosity drops below 30% or even 20%, the ionic resistance increases sharply because certain porosities are then likely to close, which prevents the wetting of the electrode by the electrolyte.
[0012] Consequently, when it is sought to produce electrode films without porosity to increase the energy density, it is appropriate to limit the thickness of these films to less than 50 μm, and preferably to less than 25 μm, in order to allow the rapid diffusion of lithium ions in the solid, without loss of power.
[0013] To produce dense films, the main method used consists of depositing a film of lithium-inserted electrode material by a vacuum process. This technique makes it possible to obtain dense films, without porosity or binders, and consequently having excellent energy densities and good temperature resistance.
[0014] The absence of porosities makes it possible to ensure the transport of lithium ions by diffusion through the film, without resorting to the use of organic electrolytes based on polymers or solvents containing lithium salts.
[0015] Such totally inorganic films provide excellent performance in aging, safety and temperature resistance.
[0016] PVD (Physical Vapor Deposition) is the most widely used technology currently used for the manufacture of thin-film microbatteries. Indeed, these products require films free of porosities and other point defects to ensure low electrical resistivity, and good ionic conduction necessary for the proper functioning of electrochemical devices.
[0017] The deposition rate obtained with such technologies is of the order of 0.1 pm to 1 pm per hour. PVD deposition techniques make it possible to obtain films of very good quality, containing almost no point defects, and make it possible to carry out depositions at relatively low temperatures. However, due to the difference in evaporation rate between the different elements, it is difficult to deposit complex compounds with such techniques, and to control the stoichiometry of the layer. This technique is perfectly suited to the production of thin layers of simple chemical composition, but as soon as one seeks to increase the deposit thickness, the deposition time becomes too long to envisage industrial use in the field of low-cost products.
[0018] Furthermore, the vacuum deposition techniques used to produce such films are very expensive and difficult to implement industrially over large surfaces, with high productivity.
[0019] Other technologies currently available for producing dense ceramic films include embodiments based on the densification of compact particle deposits or obtaining films using sol-gel techniques. Sol-gel techniques consist of depositing a polymer network obtained after hydrolysis, polymerization and condensation steps on the surface of a substrate. The sol-gel transition occurs during the evaporation of the solvent, which accelerates the reaction processes on the surface. This technique makes it possible to produce compact deposits of very low thickness. The films thus obtained have a thickness of around a hundred nanometers. These thicknesses are then too low to allow reasonable energy storage in battery applications.
[0020] To increase the thickness of the deposit without inducing the risk of cracks or crazing, it is advisable to proceed in successive stages. However, this reduces the industrial productivity of this technique, as soon as one seeks to increase the thickness of the layers.
[0021] It is also possible to produce ceramic electrode and / or electrolyte films for batteries by powder sintering. For this, a paste containing ceramic particles and organic binders is formed into a film to obtain a precursor strip commonly called a “green-sheet”.
[0022] This precursor strip is then calcined to remove the organic matter and sintered at high temperature to obtain a plate of ceramic material.
[0023] In this case, the metal films used for collecting current on these electrodes are also deposited by inking techniques. The metal powders will also be sintered at the same time as the "green-sheet". Indeed, during the step of sintering, the porosities between the ceramic material particles will be filled, which will lead to a narrowing of the strip.
[0024] Sintering the current collectors with the ceramic films makes it possible to accommodate the dimensional variations of the ceramic films and metal collectors and to avoid the occurrence of cracks.
[0025] These processes operate at very high temperatures. However, battery materials are most often sensitive to temperature and deteriorate rapidly when they undergo such heat treatments.
[0026] In order to reduce this sintering temperature, the use of nanoparticles has been proposed. In this case, it is a question of producing compact deposits of non-agglomerated nanoparticles. These deposits can be easily sintered at relatively low temperatures. This low temperature makes it possible to envisage carrying out sintering directly on metal substrates.
[0027] However, it is observed that these deposits, when they are made on metallic substrates, are conducive, depending on the thickness of the deposit, its compactness, the size of the particles, to the appearance of cracks during the drying and / or sintering steps.
[0028] Electrophoretic deposition techniques of nanoparticles have been used to increase the compactness of the deposits and thus facilitate low-temperature sintering with fewer cracks; this is described in WO 2013 / 064 773 (Fabien Gaben). Thermal coalescence occurs at a lower temperature the smaller the size of the nanoparticles, and in practice preferably less than 100 nm.
[0029] The present invention seeks to remedy at least in part the drawbacks of the prior art mentioned above.
[0030] More specifically, the problem that the present invention seeks to solve is to provide a method for manufacturing dense ceramic layers, directly on a metal substrate and which is simple, safe, fast, easy to implement, and inexpensive.
[0031] The present invention also aims to produce dense solid (ceramic) layers, usable in lithium ion microbatteries, containing no or very little defects and porosity.
[0032] The present invention also aims to provide dense electrodes and dense electrolytes having high ionic conductivity, a stable mechanical structure, good thermal stability and a long service life.
[0033] Another aim of the invention is to provide a method for manufacturing an electronic, electrical or electrotechnical device such as a microbattery, a capacitor, a supercapacitor, a photovoltaic cell comprising a dense electrode or a dense electrolyte according to the invention. Subject of the invention
[0034] According to the invention, the problem is solved by a method of manufacturing a dense layer, comprising the steps of:
[0035] - supplying a substrate and a suspension of non-agglomerated nanoparticles of a material P, - depositing a layer, on said substrate, from the suspension of primary nanoparticles of a material P; - drying of the layer thus obtained, - densification of the dried layer by mechanical compression and / or heat treatment,
[0036] knowing that the drying step and the densification step can be done at least partially at the same time, or during a temperature ramp.
[0037] Said method, which forms a first object of the present invention, is characterized in that the suspension of non-agglomerated nanoparticles of material P comprises nanoparticles of material P having a particular size distribution, making it possible to obtain after deposition a density greater than 75%. Said size is characterized by its D50 value.
[0038] This particular size distribution can be obtained either:
[0039] - continuously: In this case, the standard deviation / average size ratio of the nanoparticles of material P must be greater than 0.6, and the average size of the primary nanoparticles of material P less than or equal to 50 nm; or - discontinuously: in this case the size distribution of the nanoparticles of material P comprises nanoparticles of a first size DI between 50 nm and 20 nm, and nanoparticles of a second size D2 at least five times smaller than that of DI. Very advantageously, the particles of size DI represent between 50 and 75% of the total mass of nanoparticles.
[0040] Said suspension of non-agglomerated nanoparticles of material P can be obtained using a suspension of monodisperse nanoparticles of size DI, and / or said suspension of nanoparticles of size D2 can be obtained using a monodisperse suspension.
[0041] According to the invention, the deposition of the dense solid and ceramic layer is carried out electrophoretically, by the dip coating process, by the inkjet printing process, by roller coating, by coating through a slot-shaped die, by curtain coating, or by scraping.
[0042] A second object of the invention is a dense layer capable of being obtained by the method according to the first object. It can in particular be chosen from an anode, a cathode or an electrolyte.
[0043] A final object is an electrochemical device, and in particular a microbattery, and in particular a lithium ion microbattery, comprising at least one dense layer according to the second object of the invention.
[0044] In one embodiment, said lithium ion microbattery comprises an anode and a cathode which are dense layers according to the invention. This anode and / or this cathode may have a thickness of between approximately 1 μm and approximately 50 μm.
[0045] In a first variant, its electrolyte layer may also be a dense layer according to the invention. In a second variant, said microbattery comprises a liquid electrolyte infiltrated into a porous separator which separates said anode and said cathode. This electrolyte layer or this separator advantageously has a thickness of between approximately 1 μm and approximately 20 μm, and preferably between approximately 3 μm and approximately 10 μm.
[0046] In another embodiment, it is only its electrolyte layer which is a dense layer according to the invention. Detailed description
[0047] In the context of this document, the size of a particle is defined by its largest dimension. By "nanoparticle" is meant any particle or object of nanometric size having at least one of its dimensions less than or equal to 100 nm. This size D is expressed here as size D50.
[0048] The term "nanoparticle" is used herein to refer to primary particles, as opposed to particles formed by the aggregation or agglomeration of several primary particles. Such agglomerates may be reduced to nanoparticles (as used herein) by a deagglomeration operation, for example by grinding or ultrasonic treatment.
[0049] The density of a layer is here expressed as a relative value (for example in percent), which is obtained by comparing the actual density of the layer (here designated as dlayer) and the theoretical density of the bulk material which constitutes it (here designated as dtheorical) - Thus, the porosity of the layer, expressed in percent, is determined in the following manner: Porosity [%] = [(doric - dlayer) / dtheorical] x 100.
[0050] According to the invention, the problem is solved by a method of depositing a layer from a suspension of nanoparticles, in which the size of the nanoparticles has a particle size distribution of a particular type.
[0051] According to one of the essential aspects of the invention, a suspension of nanoparticles is used which represents a particular nanoparticle size distribution, so as to significantly increase the density of the nanoparticle deposit before sintering.
[0052] Obtaining the most compact deposit possible before sintering will reduce shrinkage and the risk of cracking. In order to obtain the most compact deposit possible, it is not only necessary to perfectly control the size distribution of the nanoparticles but also to have the most compact deposit possible of these nanoparticles, without agglomeration.
[0053] To obtain such compact deposits, one can either use electrophoretic deposition techniques of dilute suspensions, or techniques of deposition of concentrated, non-agglomerated suspensions of these polydisperse nanoparticles, by inking, dip-coating, curtain coating, doctor blade, slot-die etc. Obtaining such concentrated suspensions requires the use of stabilizers, which are organic ligands (for example of the PVP type), in order to avoid agglomeration phenomena between nanoparticles. These ligands will be eliminated at the start of the sintering heat treatment: typically, an intermediate thermal ramp is carried out in order to eliminate all these organic compounds before sintering.
[0054] The viscosity of the suspension used for the deposition depends essentially on the nature of the liquid phase (solvent), the size of the particles and their concentration (expressed by the dry extract). The viscosity of the suspension, as well as the parameters of the deposition process (in particular the running speed or the speed of passage through the liquid) determine the thickness of the deposit. Depending on these parameters specific to the deposition technique, the viscosity generally used for dip coating, curtain coating or slot die can vary widely and is between approximately 20 cP and approximately 2000 cP, measured at 20 °C. A colloidal suspension intended to produce a deposit is often called an “ink”, regardless of its viscosity.
[0055] Once these organic compounds have been eliminated, the nanoparticles will come into contact and begin the consolidation process. The surfaces of the nanoparticles will weld at the contact points; this phenomenon is known as "necking". During sintering, these contact points, which have become welding zones, will grow by diffusion until they fill the empty spaces left by the initial porosity of the deposit. It is the filling of these voids that is the origin of the shrinkage.
[0056] Also, to obtain a final porosity rate of less than 15%, preferably less than 10%, on thick deposits made on metallic substrates and without cracks, it is necessary to maximize the compactness of the initial nanoparticle deposit, while retaining the nanometric effect which makes it possible to reduce the consolidation temperatures and keep them compatible with the use of metallic substrates.
[0057] According to the invention, colloidal suspensions of nanoparticles are used, the average size of which does not exceed 100 nm. These nanoparticles also have a fairly spread size distribution. When this size distribution follows an approximately Gaussian distribution, then the ratio (sigma / Ravg) of the standard deviation to the mean radius of the nanoparticles must be greater than 0.6.
[0058] To increase this compactness of the initial deposit before sintering, it is also possible to use a mixture of two populations of nanoparticle sizes. In this case, the average diameter of the largest distribution should not exceed 100 nm, and preferably not exceed 50 nm. This first population of larger nanoparticles may have a narrower size distribution and with a sigma / R avg ratio of less than 0.6. This population of “large” nanoparticles should represent between 50% and 75% of the dry extract of the deposit (expressed as a mass percentage relative to the total mass of nanoparticles in the deposit). The second population of nanoparticles will therefore represent between 50% and 25% of the dry extract of the deposit (expressed as a mass percentage relative to the total mass of nanoparticles in the deposit).The average particle diameter of this second population must be at least 5 times smaller than that of the largest nanoparticle population. As with the largest nanoparticles, the size distribution of this second population may be narrower and potentially with a sigrna / Rmoy ratio of less than 0.6.
[0059] In all cases, the two populations must not present any agglomeration in the ink produced. Also, these nanoparticles can be advantageously synthesized in the presence of ligands or organic stabilizers so as to avoid aggregation, or even agglomeration of the nanoparticles.
[0060] The preparation of colloidal suspensions by wet nanogrinding makes it possible to obtain fairly broad size distributions. However, depending on the nature of the ground material, its "fragility" and the reduction rate applied, the primary nanoparticles may be damaged or amorphized.
[0061] The materials used in the manufacture of lithium ion batteries are particularly sensitive; the slightest change in their crystalline state or chemical composition results in degraded electrochemical performance. Also, for this type of application, it is preferable to use nanoparticles prepared in suspension directly by precipitation, using solvothermal or hydrothermal processes, at the desired primary nanoparticle size.
[0062] These nanoparticle synthesis processes by precipitation make it possible to obtain primary nanoparticles of homogeneous size with a reduced size distribution, good crystallinity and purity. It is also possible to obtain with these processes very small particle sizes, which can be less than 10 nm, and in a non-aggregated state. For this, it is appropriate to add a ligand directly into the synthesis reactor so as to avoid the formation of agglomerates, aggregates during the synthesis. For example, PVP can be used to ensure this function.
[0063] Since the size distribution of the non-agglomerated nanoparticles obtained by precipitation is quite narrow, it is advisable to favor a colloidal suspension development strategy mixing two size distributions following the rules described previously in order to maximize the compactness of the deposit before sintering. This will allow, after sintering, relatively thick deposits to be produced directly on metal substrates with little or no risk of cracking during the sintering heat treatment, which will be maintained at a relatively low temperature due to the small size of the nanoparticles used.
[0064] This bimodal nanoparticle suspension is then used to deposit the compact layers, which will then be densified by a low-temperature heat treatment and used in particular as electrodes or electrolyte in electrochemical devices such as lithium-ion batteries. Different processes can be used to deposit these layers, including electrophoresis, ink-jet printing, doctor blade, roll coating, curtain coating, dip-coating, and slot-die deposition. These are simple, safe processes that are easy to implement and industrialize and which make it possible to obtain a homogeneous final dense layer.
[0065] Electrophoresis allows a uniform layer to be deposited over large areas at a high deposition speed. Coating techniques, including dipping, roller, curtain or scraper coatings, simplify bath management compared to electrophoresis, because the composition of the bath remains constant during coating deposition. Inkjet printing deposition allows localized deposits to be made.
[0066] Thick-layer dense electrodes and electrolytes produced in a single step can be obtained by the aforementioned methods from a suspension of bimodal or polydisperse nanoparticles.
[0067] The production of a dense electrode according to the invention is now described by way of non-limiting example.
[0068] Nature of the current collector
[0069] The substrate serving as a current collector within the batteries employing dense electrodes according to the invention is metallic, for example a metal foil. It must be selected so as to withstand the temperature of any heat or thermomechanical treatment which will be applied to the layer deposited on this substrate, and this temperature will depend on the chemical nature of said layer. The substrate is preferably chosen from foils made of titanium, molybdenum, chromium, tungsten, copper, nickel or stainless steel or any alloy containing at least one of the preceding elements.
[0070] The metal sheet may be coated with a layer of noble metal, notably chosen from gold, platinum, palladium, titanium, molybdenum, tungsten, chromium or alloys containing predominantly at least one or more of these metals, or with a layer of conductive material of the ITO type (which has the advantage of also acting as a diffusion barrier).
[0071] In this example, we will use a 10 micron thick 316L type stainless steel sheet.
[0072] Deposition of a dense electrode layer by dipping (dip-coating)
[0073] Bimodal nanoparticles can be deposited by the dip coating process, regardless of the chemical nature of the nanoparticles used. For example, to produce a dense ceramic deposit of Li4Ti50i2, we can produce an ink composed of nanoparticles of two different sizes; in the case of a Li4Ti50i2 anode, Li4Ti50i2 nanoparticles of approximately 5 nm in diameter are synthesized by glycothermal routes (see the article “Impact of the Synthesis Parameters on the microstructure of nano-structured LTO prepared by glycothermal routes and 7 Li NMR structural investigations”, M. Odziomek, F. Chaput et al., published in J Sol-Gel Sci Technol 89, 225-233 (2019)). Ligands are added to this synthesis to limit the agglomeration of the nanoparticles. These 5 nm diameter nanoparticles are combined with Li4Ti50i2 nanoparticles obtained by hydrothermal synthesis with particle sizes of 30 nm.
[0074] These nanoparticles are mixed, deagglomerated by ultrasound, with 70% by mass of 30 nm particles and 30% by mass of 5 nm nanoparticles in an ink with 15% of total dry extract, in ethanol and containing PVP as stabilizer. Each dipping pass produces only a layer of fairly limited thickness; the wet layer must be dried. In order to obtain a layer of a desired final thickness, the step of deposition by dipping followed by the step of drying the layer can be repeated as many times as necessary.
[0075] Although this succession of coating steps by dipping / drying is time-consuming, the dip-coating deposition process is a simple, safe, easy to implement and industrialize process that allows a homogeneous and compact final layer to be obtained.
[0076] Treatment and properties of deposited layers
[0077] The layers deposited by dipping must be dried. Once dried, a two-step heat treatment is carried out. First, the deposit is maintained for 10 minutes at 400°C in order to calcine all the organic compounds it contains. Then the treatment temperature is increased to 550°C and maintained for one hour at this temperature in order to obtain consolidation of the deposit.
[0078] The selection of nanoparticle materials depends of course on the function of the layers thus deposited in the electrochemical, electrical or electronic device in question.
[0079] If the layer according to the invention is to function as the cathode of a battery, especially a lithium ion battery, it can be made for example from a material P which is a cathode material chosen from:
[0080] - the oxides LiMn2O4, Lii+xMn2xO4 with 0 < x < 0.15, LiCoO2, LiNiO2, LiMnM Ni0>5O4, LiMnij5Nioj5-xXx04 where X is selected from Al, Fe, Cr, Co, Rh, Nd, other rare earths such as Sc, Y, Lu, La, Ce, Pr, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and where 0 < x < 0.1, LiMn2 xMxO4 with M = Er, Dy, Gd, Tb, Yb, Al, Y, Ni, Co, Ti, Sn, As, Mg or a mixture of these compounds and where 0 < x < 0.4, LiFeO2, LiMni / 3Nii / 3Coi / 3O2, ,LiNio8Coo i5A1q()5O2, Li Alxl\4n2xO4 with 0 < x < 0.15, LiNii / xCoi / yMni / zO2 with x+y+z =10; - phosphates LiFePO4, LiMnPO4, LiCoPO4, LiNiPO4, Li3V2(PO4)3; phosphates of formula LiMM'P04, with M and M' (M M') selected from Fe, Mn, Ni, Co, V; - all lithiated forms of the following chalcogenides: V2O5, V3O8, TiS2, titanium oxysulfides (TiOySz with z=2-y and 0.3 < y < 1), tungsten oxysulfides (WOySz with 0.6 < y < 3 and 0.1 < z < 2), CuS, CuS2, preferably LixV2O5 with 0 < x < 2, LixV3O8 with 0 < x < 1.7, LixTiS2 with 0 < x < 1, titanium and lithium oxysulfides LixTiOySz with z = 2-y, 0.3 < y < 1, LixW0 ySz, LixCuS, LixCuS2.
[0081] If the layer according to the invention is to function as the anode of a battery, especially a lithium ion battery, it can be made for example from a material P which is an anode material chosen from:
[0082] - carbon nanotubes, graphene, graphite; - lithium iron phosphate (typical formula LiFePO4); - mixed silicon and tin oxynitrides (typical formula SiaSnbOyNz with a>0, b>0, a+b<2, 0 <y<4, 0<z<3) (appelés aussi SiTON), et en particulier le SiSn0,8701,2Ni,72 ; ainsi que les oxynitrures-carbures de formule typique SiaSnbCcOyNz avec a > 0, b > 0, a+b <2, 0 < c < 10, 0 < y < 24, 0 < z < 17; - nitrides of the type SixNy (in particular with x=3 and y=4), SnxNy (in particular with x=3 and y=4), ZnxNy (in particular with x=3 and y=2), Li3 xMxN (with 0 < x < 0.5 for M=Co, 0 < x < 0.6 for M=Ni, 0 < x < 0.3 for M=Cu); Si3 xMxN4 with M=Co or Fe and 0 < x < 3. - the oxides SnO2, SnO, Li2SnO3, SnSiO3, LixSiOy (x >= 0 and 2 > y > 0), Li4Ti5O i2, TiNb2O7, Co3O4, SnB0,6Po,402j9 and TiO2, - TiNb2O7 composite oxides comprising between 0% and 10% by mass of carbon, preferably the carbon being chosen from graphene and carbon nanotubes, - compounds of general formula LiwTii_xM1xNb2_yM2yO7_zM3z in which M 1 and M2 are each at least one element selected from the group consisting of Nb, V, Ta, Fe, Co, Ti, Bi, Sb, As, P, Cr, Mo, W, B, Na, Mg, Ca, Ba, Pb, Al, Zr, Si, Sr, K, Cs and Sn, M1 and M2 being able to be identical or different from each other, and in which M3 is at least one halogen, and in which 0 < w < 5, 0 <x<l,0<y<2et0<z< 0.3.
[0083] If the layer according to the invention is to function as an electrolyte in a battery, especially a lithium ion battery, it can be made for example from a material P which is an electrolyte material chosen from:
[0084] - garnets of formula LidA'xA2y(TO4)z where A1 represents a cation of oxidation state +11, preferably Ca, Mg, Sr, Ba, Fe, Mn, Zn, Y, Gd; and where A2 represents a cation of oxidation state +III, preferably Al, Fe, Cr, Ga, Ti, La; and where (TO4) represents an anion in which T is an atom of oxidation state +IV, located at the center of a tetrahedron formed by oxygen atoms, and in which TO4 advantageously represents the silicate or zirconate anion, knowing that all or part of the elements T of an oxidation state +IV can be replaced by atoms of an oxidation state +III or +V, such as Al, Fe, As, V, Nb, In, Ta; knowing that: d is between 2 and 10, preferably between 3 and 9, and even more preferably between 4 and 8; x is between 2.6 and 3.4 (preferably between 2.8 and 3.2); y is between 1.7 and 2.3 (preferably between 1.9 and 2.1) and z is between 2.9 and 3.1; - garnets, preferably chosen from: Li7La3Zr20i2; Li6La2BaTa20i2; Li5j5La3Nbij75lno.250i2; Li5La3M20i2 with M = Nb or Ta or a mixture of the two compounds; Li7 xBaxLa3 xM20i2 with 0 <x<letM = Nb ou Ta ou un mélange des deux composés ; le Li7 xLa3Zr2 xMxOi2avec 0<x<2etM = Al, Ga ou Ta ou un mélange de deux ou trois de ces composés ; - lithium phosphates, preferably chosen from: lithium phosphates of the NaSICON type, Li3PO4; LiPO3; Li3Al0j4Scij6(PO4)3 called “LASP”; Lii>2Zri çCa0ji(PO4)3; LiZr2(PO4)3; Lii+3xZr2(Pi_xSixO4)3 with 1.8 < x < 2.3; Lii+6xZr2(Pi XBXO4)3 with 0 < x < 0.25; Li3(Sc2 xMx)(PO4)3 with M=A1 or Y and 0 < x < 1; Lii+xMx(Sc)2 x(PO4)3 with M = Al, Y, Ga or a mixture of the three compounds and 0 < x < 0.8; Lii+xMx(Gai yScy)2 x(PO4)3 with 0 < x < 0.8; 0 < y < 1 and M= Al or Y or a mixture of the two compounds; Lii+xMx(Ga)2 x(PO4)3 with M = Al, Y or a mixture of the two compounds and 0 < x < 0.8; Lii+xAlxTi2 x(PO4)3 with 0 < x < 1 called “LATP”; or Lii+XA1 xGe2 X(PO4)3 with 0 < x < 1 called “LAGP”; or Lii+x+zMx(Gei_yTiy)2_xSizP 3 ZO[2 with 0 < x < 0.8 and 0 < y < 1.0 and 0 < z < 0.6 and M = Al, Ga or Y or a mixture of two or three of these compounds; Li3+y(Sc2 xMx)QyP3 yO[2 with M = Al and / or Y and Q = Si and / or Se, 0 < x < 0.8 and 0 < y < 1; or Lii+x+yMxSc2 x QyP3yO12 with M = Al, Y, Ga or a mixture of the three compounds and Q = Si and / or Se, 0 < x < 0.8 and 0 < y < 1; or the Lii+x+y+zMx(Gai_yScy)2_xQzP3_zOi2with 0 < x < 0,8,0 <y<l,0<z< 0,6 avec M = Al ou Y ou un mélange des deux composés et Q= Si et / ou Se ; ou le LiUxZr2 XBX(PO4)3 avec 0 < x < 0,25 ; ou le Lii+xZr2 xCax(PO4)3 avec 0 < x < 0,25 ; ou LiUxM3xM2 xP30i2 avec 0 < x < 1 et M3= Cr, V, Ca, B, Mg, Bi et / ou Mo, M = Sc, Sn, Zr, Hf, Se ou Si, ou un mélange de ces composés ; le Lii+2xCaxZr2 x(PO4)3 avec 0 < x < 0,25 ; lithium borates, preferably chosen from: Li3(Sc2 xMx)(BO3)3 with M=A1 or Y and 0 < x < 1; Lii+xMx(Sc)2_x(BO3)3 with M = Al, Y, Ga or a mixture of the three compounds and 0 < x < 0.8; Lii+xMx(Gai_yScy)2_x(BO3)3 with 0 < x < 0.8, 0 < y < 1 and M= Al or Y; Lii+xMx(Ga)2 x(BO3)3 with M = Al, Y or a mixture of the two compounds and 0 < x < 0.8; Li3BO3, Li3BO3-Li2 SO4, Li3BO3-Li2SiO4, Li3BO3-Li2SiO4-Li2SO4; oxynitrides, preferably chosen from Li3PO4 xN2x / 3, Li4SiO4 xN2x / 3, Li4 GeO4 xN2x / 3 with 0 < x < 4 or Li3BO3 xN2x / 3 with 0 < x < 3; lithium compounds based on lithium and phosphorus oxynitride, called "LiPON", in the form of LixPOyNz with x ~ 2.8 and 2y+3z ~ 7.8 and 0.16 < z < 0.4, and in particular Li2>9PO3.3N0.46, but also the compounds LiwPOxNy Sz with 2x+3y+2z = 5 = w or the compounds LiwPOxNySz with 3.2 < x < 3.8, 0.13 < y < 0.4, 0 < z < 0.2,2.9 < w < 3.3 or the compounds in the form of Lit PxAlyOuNvSw with 5x+3y=5, 2u+3v+2w=5+t, 2.9 <t<3,3, 0,84<x<0,94, 0,094<y<0,26, 3,2<u<3,8, 0,13<v<0,46, 0<w<0,2 ; materials based on lithium phosphorus or boron oxynitrides, called respectively “LiPON” and “LIBON”, which may also contain silicon, sulfur, zirconium, aluminum, or a combination of aluminum, boron, sulfur and / or silicon, and boron for materials based on lithium phosphorus oxynitrides; lithium compounds based on lithium, phosphorus and silicon oxynitride called “LiSiPON”, and in particular Lii çSio.^Pi.oOi.iNi.o; lithium oxynitrides of the types LiBON, LiBSO, LiSiPON, LiSON, thio-LiSiCON, LiPONB (where B, P and S represent boron, phosphorus and sulfur respectively); lithium oxynitrides of LiBSO type such as (lx)LiBO2-xLi2SO4 with 0.4 < x < 0.8; - lithiated oxides, preferably chosen from Li7La3Zr2Oi2 or Li5+xLa3 (Zrx,A2x)O12 with A = Sc, Y, Al, Ga and 1.4 < x < 2 or Li0j35La0j55TiO3 or Li3xLa2 / 3 xTiO3 with 0 < x < 0.16 (LLTO); - silicates, preferably chosen from Li2Si2O5, Li2SiO3, Li2Si2O6, LiAlSiO4, Li4SiO4, LiAlSi2O6; - solid electrolytes of anti-perovskite type chosen from: Li3OA with A a halide or a mixture of halides, preferably at least one of the elements chosen from F, Cl, Br, I or a mixture of two or three or four of these elements; Li(3 x)Mx / 2OA with 0 < x < 3, M a divalent metal, preferably at least one of the elements chosen from Mg, Ca, Ba, Sr or a mixture of two or three or four of these elements, A a halide or a mixture of halides, preferably at least one of the elements chosen from F, Cl, Br, I or a mixture of two or three or four of these elements; Li(3 x)M 3x / 3OA with 0 < x < 3, M3 a trivalent metal, A a halide or a mixture of halides, preferably at least one of the elements chosen from F, Cl, Br, I or a mixture of two or three or four of these elements; or LiCOXzY(iz), with X and Y halides as mentioned above in relation to A, and 0 < z < 1, - the compounds Lao,5iLio>34Ti2,94, Li3j4Voj4Geo>604, Li2O-Nb2O5, LiAlGaSPO4; - formulations based on Li2CO3, B2O3, Li2O, Al(PO3)3LiF, P2S3, Li2S, Li3N, Li14Zn(GeO4)4, Li3>6Ge0,6Vo,404, LiTi2(PO4)3, Li3 25Geoj25Po>25S4, Li13Aloj3Ti17(PO 4)3, Lii+xAlxM2 x(PO4)3 (where M = Ge, Ti, and / or Hf, and where 0 < x < 1), Lii+x+yAlxTi2 x SiyP3 yO[2 (where 0 < x < 1 and 0 < y < 1).
[0085] The nanoparticles used in the inks used to make these deposits for the electrodes can also have a core-shell structure. Indeed, the performance of the dense electrodes thus obtained will depend on their ionic and electronic conduction properties. Also, on the surface of the nanoparticles of active material, it may be important to apply a “shell” of an inorganic material, with good electronic and / or ionic conduction properties.
[0086] Thus, in an advantageous embodiment the core is formed from an electrode material (anode or cathode), and the shell is formed from a material which is both electronically conductive and which does not prevent the passage of lithium ions. For example, the shell may be formed by a layer of a metal, which is sufficiently thin to allow lithium ions to pass through, or by a sufficiently thin layer of graphite, or by a layer of an ionic conductor which is also a good electronic conductor.
[0087] Example of manufacturing a lithium ion microbattery
[0088] A method of manufacturing lithium ion microbatteries using the layers according to the invention.
[0089] a) Preparation of the electrodes by the deposition process according to the invention
[0090] A first dense electrode of Li4Ti50i2 was deposited, obtained by the method described above in the chapter “Deposition of a dense electrode layer by dipping (dip-coating)”. A second dense electrode of LiMn2O4 was also deposited by a similar method.
[0091] On each of these two electrodes, a mesoporous thin film of Li3PO4 agglomerates was then deposited, which acts as a separator film in the battery, and which was prepared as described below.
[0092] b) Deposition of the separator layer
[0093] A suspension of Li3PO4 nanoparticles was prepared from the two solutions presented below: First, 45.76 g of CH3COOLi, 2H2O were dissolved in 448 ml of water, then 224 ml of ethanol were added with vigorous stirring to the medium in order to obtain a solution A. Second, 16.24 g of H3PO4 (85 wt% in water) were diluted in 422.4 ml of water, then 182.4 ml of ethanol were added to this solution in order to obtain a second solution hereinafter called solution B. Solution B was then added, under vacuum stirring, to solution A.
[0094] The solution obtained, perfectly clear after the disappearance of the bubbles formed during mixing, was added to 4.8 liters of acetone under the action of an Ultraturrax™ type homogenizer in order to homogenize the medium. A white precipitation suspended in the liquid phase was immediately observed.
[0095] The reaction medium was homogenized for 5 minutes and then kept for 10 minutes under magnetic stirring. It was left to settle for 1 to 2 hours. The supernatant was discarded and the remaining suspension was centrifuged for 10 minutes at 6000 g. Then 1.2 l of water was added to resuspend the precipitate (using a sonotrode, magnetic stirring). Two additional washes of this type were then carried out with ethanol. With vigorous stirring, 15 ml of a 1 g / ml solution of Bis(2-(methacryloyoloxy)ethyl)phosphate was added to the colloidal suspension in ethanol thus obtained. The suspension thus became more stable. The suspension was then sonicated using a sonotrode. The suspension was then centrifuged for 10 minutes at 6000 g. The pellet was then redispersed in 1.2 L of ethanol and centrifuged for 10 minutes at 6000 g.The pellets thus obtained are redispersed in 900 ml of ethanol in order to obtain a 15 g / l suspension suitable for carrying out electrophoretic deposition.
[0096] Agglomerates of approximately 200 nm consisting of primary Li3PO4 particles of 10 nm were thus obtained in suspension in ethanol.
[0097] Thin porous layers of Li3PO4 were then deposited by electrophoresis on the surface of the anodes and cathodes previously prepared by applying a field 20V / cm electric current to the previously obtained suspension of Li3PO4 nanoparticles, for 90 seconds to obtain a layer of approximately 2 pm. The layer was then air-dried at 120°C and then a calcination treatment at 350°C for 120 minutes was carried out on this previously dried layer in order to eliminate any trace of organic residues.
[0098] c) Assembly of the electrodes and the separator
[0099] After depositing 2 pm of porous Li3PO4 on each of the electrodes (Lii+xMn2 yO4 and Li4Ti50i2) previously developed, the two subsystems were stacked so that the Li3PO4 films were in contact. This stack was then hot-pressed under vacuum between two flat plates. To do this, the stack was first placed under a pressure of 5 MPa and then dried under vacuum for 30 minutes at 103 bar. The press plates were then heated to 550°C with a speed of 0.4°C / second. At 550°C, the stack was then thermo-compressed under a pressure of 45 MPa for 20 minutes, then the system was cooled to room temperature. The assembly was then dried at 120°C for 48 hours under vacuum (10 mbar).
[0100] d) Impregnation of the separator with a liquid electrolyte
[0101] This assembly was then impregnated, under anhydrous atmosphere, by dipping in an electrolytic solution comprising PYR14TFSI, and LiTFSI at 0.7 M. PYR14TFSI is the common abbreviation for 1-butyl-l-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide. LITFSI is the common abbreviation for lithium bis-trifluoromethanesulfonimide (CAS No.: 90076-65-6). The ionic liquid enters instantly by capillarity into the pores of the separator. Each of the two ends of the system was kept immersed for 5 minutes in a drop of the electrolytic mixture.
[0102] It is noted that in an industrial manufacturing process, the impregnation is carried out after the encapsulation of the battery, and followed by the production of the electrical contact members.
[0103] The battery according to the invention may be a lithium ion microbattery. In particular, it may be designed and sized so as to have a capacity less than or equal to approximately 1 mA h (commonly called a “microbattery”). Typically, microbatteries are designed so as to be compatible with microelectronics manufacturing processes.
[0104] These micro-batteries can be made:
[0105] - either only with layers according to the invention, of the “all solid” type, i.e. provided with impregnated liquid or pasty phases (said liquid or pasty phases may be a conductive medium for lithium ions, capable of acting as an electrolyte),
[0106] - either with electrodes according to the invention and “all-solid” type separators mesoporous, impregnated with a liquid or pasty phase, typically a lithium ion-conducting medium, which spontaneously enters the layer and no longer comes out of this layer, so that this layer can be considered quasi-solid,
[0107] - either with electrodes according to the invention and impregnated porous separators (i.e. layers having a network of open pores which can be impregnated with a liquid or pasty phase, and which gives these layers wet properties).
Claims
Claims
1. A method of manufacturing a dense layer, comprising the steps of: i. Providing a substrate and a suspension of non-agglomerated nanoparticles of a material P; ii. Depositing a layer, on said substrate, from the suspension of primary nanoparticles of a material P; iii. Drying the layer thus obtained; iv.Densification of the dried layer by mechanical compression and / or heat treatment, knowing that steps (iii) and (iv) can be carried out at least partially at the same time, or during a temperature ramp; said method being characterized in that the suspension of non-agglomerated nanoparticles of material P comprises nanoparticles of material P having a size distribution, said size being characterized by its D50 value, such that: - the distribution comprises nanoparticles of material P of a first size DI between 20 nm and 50 nm, and nanoparticles of material P of a second size D2 characterized by a D50 value at least five times lower than that of DI; or - the distribution has an average size of the nanoparticles of material P of less than 50 nm, and a standard deviation to average size ratio greater than 0.
6.
2. Method according to claim 1, wherein said suspension of non-agglomerated nanoparticles of material P comprises nanoparticles of material P of a first size DI between 20 nm and 50 nm, and nanoparticles of material P of a second size D2 characterized by a value D50 at least five times lower than that of D1, and said particles of size D1 represent between 50 and 75% of the total mass of nanoparticles.
3. Method according to claim 1 or 2, characterized in that said suspension of non-agglomerated nanoparticles of material P is obtained using a suspension of monodisperse nanoparticles of size Dl.
4. Method according to one of claims 1 to 3, characterized in that the suspension of nanoparticles of size D2 is obtained using a
5.
6.
7. monodisperse suspension. Method according to any one of claims 1 to 4, characterized in that the deposition of the dense thin layer is carried out electrophoretically, by the dip coating process, by the inkjet printing process, by roller coating, by curtain coating or by scraping. Method according to any one of claims 1 to 5, characterized in that said suspension has a viscosity, measured at 20°C, between 20 cP and 2000 cP. Method according to any one of claims 1 to 6, characterized in that said material P is an inorganic material, preferably selected from the group formed by: - the oxides LiMn2O4, Lii+xMn2xO4 with 0 < x < 0.15, LiCoO2, LiNiO2, LiMnij5Nio>504, LiMni>5Nio,5-xXx04 where X is selected from Al, Fe, Cr, Co, Rh, Nd, other rare earths such as Sc, Y, Lu, La, Ce, Pr, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and where 0 < x < 0.1, LiMn2 xMxO4 with M = Er, Dy, Gd, Tb, Yb, Al, Y, Ni, Co, Ti, Sn, As, Mg or a mixture of these compounds and where 0 < x < 0.4, LiFeO2, LiMni / 3Nii / 3Coi / 3O2, ,LiNio.8Coo.15AI0.05 O2, LiAlxMn2 XO4 with 0 < x < 0.15, LiNii / xCoi / yMni / zO2 with x+y+z =10; - phosphates LiFePO4, LiMnPO4, LiCoPO4, LiNiPO4, Li3V2 (PO4)3; phosphates of formula LiMM'P04, with M and M' (M M') selected from Fe, Mn, Ni, Co, V; - all lithiated forms of the following chalcogenides: V2O5, V3O8, TiS2, titanium oxysulfides (TiOySz with z=2-y and 0.3 < y < 1), tungsten oxysulfides (WOySz with 0.6 < y < 3 and 0.1 < z < 2), CuS, CuS2, preferably LixV2O5 with 0 < x < 2, LixV3O8 with 0 < x < 1.7, LixTiS2 with 0 < x < 1, titanium and lithium oxysulfides LixTiOySz with z = 2-y, 0.3 < y < 1, LixWOySz, LixCuS, LixCuS2; - carbon nanotubes, graphene, graphite; - lithium iron phosphate (typical formula LiFePO4); - mixed silicon and tin oxynitrides (typical formula SiaSnbOyNz with a>0, b>0, a+b<2, 0 <y<4, 0<z<3) (appelés aussi SiTON), et en particulier le SiSn0,87Oi,2Ni,72 ; ainsi que les oxynitrures-carbures de formule typique SiaSnbCcOyNz avec a > 0, b > 0, a+b <2, 0 < c < 10, 0 < y < 24, 0 < z < 17; nitrides of type SixNy (in particular with x=3 and y=4), Snx Ny (in particular with x=3 and y=4), ZnxNy (in particular with x=3 and y=2), Li3 xMxN (with 0 < x < 0.5 for M=Co, 0 < x < 0.6 for M=Ni, 0 < x < 0.3 for M=Cu); Si3 xMxN4 with M=Co or Fe and 0 < x < 3. the oxides SnO2, SnO, Li2SnO3, SnSiO3, LixSiOy (x >= 0 and 2 > y > 0), Li4Ti50i2, TiNb2O7, Co3O4, SnB0j6Po,402>9 and TiO2, the composite oxides TiNb2O7 comprising between 0% and 10% by mass of carbon, preferably the carbon being chosen from graphene and carbon nanotubes; garnets of formula LidA'xA2y(TO4)z where A1 represents a cation with oxidation number +11, preferably Ca, Mg, Sr, Ba, Fe, Mn, Zn, Y, Gd; and where A2 represents a cation with oxidation number +III, preferably Al, Fe, Cr, Ga, Ti, La; and where (TO4) represents an anion in which T is an atom with oxidation number +IV, located at the center of a tetrahedron formed by oxygen atoms, and in which TO4 advantageously represents a silicate or zirconate anion, knowing that all or part of the T elements with oxidation number +IV can be replaced by atoms with oxidation number +III or +V, such as Al, Fe, As, V, Nb, In, Ta; knowing that: d is between 2 and 10, preferably between 3 and 9, and even more preferably between 4 and 8; x is between 2.6 and 3.4 (preferably between 2.8 and 3.2); y is between 1.7 and 2.3 (preferably between 1.9 and 2.1) and z is between 2.9 and 3.1; garnets, preferably chosen from: Li7La3Zr20i2; Li6 La2BaTa2O[2; Li33La3Nb| 73Ini)23O|2; Li3La3M2O|2 with M = Nb or Ta or a mixture of the two compounds; Li7 xBaxLa 3xM2O12 with 0 < x < andM = Nb or Ta or a mixture of the two compounds; Li7 xLa3Zr2xMxOi2with 0 <x<2etm = al, ga ou ta un mélange de deux trois ces composés ;lithium phosphates, preferably chosen from: lithium phosphates of the NaSICON type, Li3PO4; LiPO3; Li3Al0j4Scij6(PO4)3 called “LASP”; Liij2ZrijQCa0ji(PO4)3; LiZr2(PO4)3; Li|+3xZr2(P| XSixO4)3 with 1.8 < x < 2.3; Li i+6xZr2(Pi_xBxO4)3 with 0 < x < 0.25; Liî(Sc2 XM j(PO4)î with M=A1 or Y and 0 < x < 1; Lii+xMx(Sc)2_x(PO4)3 with M = Al, Y, Ga or a mixture of the three compounds and 0 < x < 0.8; Li i+xMx(Gai yScy)2_x(PO4)3 with 0 < x < 0.8; 0 < y < 1 and M= Al or Y or a mixture of the two compounds; Li[+xMx(Ga)2 X(PO4 )3 with M = Al, Y or a mixture of the two compounds and 0 < x < 0.8; Lii+xAlxTi2 x(PO4)3 with 0 < x < 1 called “LATP”; or Lii+xAlxGe2 X(PO4)3 with 0 < x < 1 called “LAGP”; or Li1+x+zMx(Ge! yTiy)2 xSizP3 ZO12 with 0 < x < 0.8 and 0 < y < 1.0 and 0 < z < 0.6 and M= Al, Ga or Y or a mixture of two or three of these compounds; Li3+y(Sc2 xMx)Qy P3 yO[2 with M = Al and / or Y and Q = Si and / or Se, 0 < x < 0.8 and 0 < y < 1; or Lii+x+yMxSc2 xQyP3 yO[2 with M = Al, Y, Ga or a mixture of the three compounds and Q = Si and / or Se, 0 < x < 0.8 and 0 < y < 1; or the Li1+x+y+zMx(Gal yScy)2 xQzP3 zOi2with 0 < x < 0,8,0 <y<l,0<z< 0,6 avec m="Sc," ou y un mélange des deux composés et q="Si" se ; le lii+xzr2 x bx(po4)3 0 < x < 0,25 xcax(po4)3 lii+xm3xm2 xp30i2 < 1 m3="Cr," v, ca, b, mg, bi mo, sn, zr, hf, si, de ces lii+2xcaxzr2 x(po4)3 ;lithium borates, preferably chosen from: Li3(Sc2_xMx )(BO3)3 with M=A1 or Y and 0 < x < 1; Lii+xMx(Sc)2 x(BO3)3 with M = Al, Y, Ga or a mixture of the three compounds and 0 < x < 0.8; Lii+xMx(GaiyScy)2x(BO3)3 with 0 <x<0,8,0<y< 1 et m="Al," ou y ; le lii+xmx(ga)2 x(bo3)3 avec un mélange des deux composés 0 < x < 0,8 li3bo3, li3bo3-li2so4, li3bo3-li2sio4, li3bo3-li2sio4-li2so4 les oxynitrures, de préférence choisis parmi li3po4 xn2x 3, li4 sio4_xn2x li4gco4 3 < 4 li3bo3 xn2s 0<x<3;lithium compounds based on lithium and phosphorus oxynitride, called "LiPON", in the form of LixPOyNz with x ~ 2.8 and 2y+3z ~ 7.8 and 0.16 < z < 0.4, and in particular Li2Q PO3j3N0j46, but also the compounds LiwPOxNySz with 2x+3y+2z = 5 = w or the compounds LiwPOxNySz with 3.2 < x < 3.8, 0.13 < y < 0.4, 0 < z < 0.2,2.9 < w < 3.3 or the compounds in the form of LitPxAlyOuNvSw with 5x+3y=5, 2u+3v+2w=5+t, 2.9 <t<3,3, 0,84<x<0,94, 0,094<y<0,26, 3,2<u<3,8, 0,13<v<0,46, 0<w<0,2 ;materials based on lithium phosphorus or boron oxynitrides, called respectively “LiPON” and “LIBON”, which may also contain silicon, sulfur, zirconium, aluminum, or a combination of aluminum, boron, sulfur and / or silicon, and boron for materials based on lithium phosphorus oxynitrides; lithium compounds based on lithium, phosphorus and silicon oxynitride called “LiSiPON”, and in particular Li1.9Si0.28Pi.oOi.iNi.o; lithium oxynitrides of the types LiBON, LiBSO, LiSiPON, LiSON, thio-LiSiCON, LiPONB (where B, P and S represent boron, phosphorus and sulfur respectively); lithium oxynitrides of LiBSO type such as (lx)LiBO2 -xLi2SO4 with 0.4 < x < 0.8; lithiated oxides, preferably chosen from Li7La3Zr20i2 or Li5+xLa3(Zrx,A2 x)Oi2 with A = Sc, Y, Al, Ga and 1.4 < x < 2 or Lioj35La0j55Ti03 or Li3xLa2 / 3 xTiO3 with 0 < x < 0.16 (LLTO); silicates, preferably chosen from Li2Si2O5, Li2SiO3, Li2 Si2O6, LiAlSiO4, Li4SiO4, LiAlSi2O6; solid electrolytes of anti-perovskite type chosen from: Li3OA with A a halide or a mixture of halides, preferably at least one of the elements chosen from F, Cl, Br, I or a mixture of two or three or four of these elements; Li (3 x)Mx / 20A with 0 < x < 3, M a divalent metal, preferably at least one of the elements chosen from Mg, Ca, Ba, Sr or a mixture of two or three or four of these elements, A a halide or a mixture of halides, preferably at least one of the elements chosen from F, Cl, Br, I or a mixture of two or three or four of these elements; Li(3 x)M3x / 3OA with 0 < x < 3, M3 a trivalent metal, A a halide or a mixture of halides, preferably at least one of the elements chosen from F, Cl, Br, I or a mixture of two or three or four of these elements; or LiCOXzY(iz), with X and Y halides as mentioned above in relation to A, and 0 < z < 1, - the compounds Lao.51Lio.34Ti3.94, Li34Vo.4Geo.6O4, Li2O-Nb2O5, LiAlGaSPO4; - formulations based on Li2CO3, B2O3, Li2O, Al(PO3)3LiF, P2 S3, Li2S, LUN, Lii4Zn(GeO4)4, Li3.5Geo.6Vo.4O4, LiTi2(PO4)3, Li 3.25Geo.25Po.25S4, Lii.3Alo.3Tii.7(P04)3, Lii+XA1XM2_X(PO4)3 (where M = Ge, Ti, and / or Hf, and where 0 < x < 1), Lii+x+yAlxTi2.xSiyP3-yOi2 (where 0 < x < 1 and 0 < y < 1).
8. Method according to any one of claims 1 to 7, characterized in that said nanoparticles of a material P comprise nanoparticles composed of a core and a shell, said shell being formed of a material which is an electronic conductor.
9. Dense layer obtainable by the method according to any one of claims 1 to 8.
10. Dense layer according to claim 9, characterized in that it is chosen from an anode, a cathode or an electrolyte.
11. Electrochemical device, comprising at least one dense layer according to claim 9 or 10.
12. Electrochemical device according to claim 11, characterized in that it is a battery with a capacity not exceeding 1 mA h, and in particular a lithium ion battery.
13. Lithium ion battery according to claim 12, characterized in that it comprises an anode and a cathode which are dense layers according to one of claims 9 or 10.
14. Lithium ion battery according to claim 12 or 13, characterized in that it comprises an electrolyte layer which is a dense layer according to one of claims 9 or 10.
15. Lithium ion battery according to claim 13, characterized in that it comprises a liquid electrolyte infiltrated into a porous separator which separates said anode and said cathode.