METHOD FOR MANUFACTURING LITHIUM ION BATTERIES

By employing non-agglomerated nanoparticles with controlled size distributions and low-temperature processing, dense ceramic layers for lithium ion batteries are produced, addressing industrial scalability and performance challenges.

FR3108792B1Inactive Publication Date: 2024-10-25I TEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2020003108
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-30
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current lithium ion battery manufacturing processes face challenges in producing dense, defect-free layers with high ionic conductivity and thermal stability, while maintaining industrial feasibility and cost-effectiveness, as existing methods are either expensive, time-consuming, or result in cracks and porosity issues.

Method used

A method involving the deposition of non-agglomerated nanoparticles with specific size distributions, followed by mechanical compression and low-temperature heat treatment, using electrophoretic or coating techniques, to create dense ceramic layers on metal substrates, ensuring high density and minimal porosity.

Benefits of technology

This approach enables the production of dense electrodes and electrolytes with enhanced ionic conductivity, mechanical stability, and long lifespan, suitable for lithium ion batteries, while being cost-effective and scalable.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A method for manufacturing a lithium-ion battery with a capacity greater than 1 mA h, comprising the deposition of at least one dense layer, which may be an anode and / or a cathode and / or an electrolyte, by a dense layer deposition process comprising the following steps: supplying a substrate and a suspension of non-agglomerated nanoparticles of a material P; deposition of a layer, on said substrate, from said suspension; drying of the layer thus obtained; densification of the dried layer by mechanical compression and / or heat treatment;said deposition process being characterized in that the suspension of non-agglomerated nanoparticles of material P comprises nanoparticles of material P having a size distribution, said size being characterized by its D50 value, such that: - the distribution comprises nanoparticles of material P of a first size D1 between 20 nm and 50 nm, and nanoparticles of material P of a second size D2 characterized by a D50 value at least five times smaller than that of D1; or - the distribution has an average size of the nanoparticles of material P less than 50 nm, and a standard deviation to average size ratio greater than 0.6.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: METHOD FOR MANUFACTURING LITHIUM ION BATTERIES Technical field of the invention

[0001] The present invention relates to the manufacture of dense inorganic layers, usable as electrode or electrolyte layers in multilayer batteries, such as lithium-ion batteries. More specifically, the invention relates to a new method for manufacturing these dense layers. It also relates to multilayer batteries incorporating at least one layer obtained by this method, this layer being able, in particular, to act as an electrode in a lithium-ion battery. State of the art

[0002] The ideal battery for powering autonomous electrical devices (such as: phones and laptops, handheld tools, autonomous sensors) or for traction of electric vehicles would have a long lifespan, be capable of storing both large quantities of energy and power, and would not present a risk of overheating or even explosion.

[0003] Currently, these electrical devices are primarily powered by lithium-ion batteries, which offer the highest energy density among the various storage technologies available. Different electrode architectures and chemical compositions exist for manufacturing lithium-ion batteries. The manufacturing processes for lithium-ion batteries are described in numerous articles and patents, and the book "Advances in Lithium-Ion Batteries" (ed. W. van Schalkwijk and B. Scrosati), published in 2002 (Kluever Academie / Plenum Publishers), provides a good overview.

[0004] Lithium-ion battery electrodes can be manufactured using coating techniques (in particular: roll coating, doctor blade coating, tape casting, slot-die coating). With these processes, the active materials used to make the electrodes are in powder form with an average particle size between 5 and 15 µm in diameter. These particles are incorporated into an ink made up of these particles and deposited on the surface of a substrate.

[0005] These techniques make it possible to produce layers with a thickness ranging from approximately 50 pm to approximately 400 pm. Depending on the thickness of the layers, their porosity, and the size of the active particles, the power and energy of the battery can be adjusted.

[0006] The inks (or pastes) deposited to form the electrodes contain particles of active materials, as well as (organic) binders, carbon powder to ensure electrical contact between the particles, and solvents that evaporate during the electrode drying stage. To improve the quality of electrical contact between the particles and to compact the deposited layers, a calendering step is performed on the electrodes. After this compression step, the active particles of the electrodes occupy approximately 60% of the deposit volume, which means that generally 40% of the porosity between the particles remains.

[0007] The contact between each of the particles is essentially point contact, and the electrode structure is porous. The pores are filled with an electrolyte, which can be liquid (an aprotic solvent in which a lithium salt is dissolved) or in the form of a more or less polymerized gel impregnated with a lithium salt. Since the thickness of lithium-ion battery electrodes is generally between 50 µm and 400 µm, the transport of lithium ions through the electrode thickness occurs via the pores, which are filled with electrolyte (containing lithium salts). Depending on the quantity and size of the pores, the rate of lithium diffusion through the electrode thickness varies.

[0008] To ensure proper battery operation, lithium ions must diffuse both within the particle and the electrode. Diffusion within the active material particle is slower than within the electrolyte with which the porous electrode is impregnated; this electrolyte is liquid or gel. The slow diffusion within the electrode particles contributes to the battery's series resistance. Therefore, to achieve sufficient battery power, the particle size must be reduced; in standard lithium-ion batteries, it is typically between 5 µm and 15 µm.

[0009] On the other hand, depending on the thickness of the layers and the size and density of active particles contained in the ink, the power and energy of the battery can be modulated. Increasing the energy density necessarily comes at the expense of the power density. High-power battery cells must use thin electrodes and separators with high porosity, while increasing the energy density requires, on the contrary, increasing these same thicknesses and reducing the porosity. The article “Optimization of Porosity and Thickness of a Battery Electrode by Means of a Reaction-Zone Model” by John Newman, published in J. Electrochem. Soc., Vol. 142, No. 1 in January 1995, demonstrates the respective effects of electrode thickness and porosity on their discharge rate (power) and energy density.

[0010] However, the increase in porosity in the electrodes tends to deteriorate the Battery energy density: To increase the energy density of the electrodes, it is necessary to reduce porosity. In current lithium-ion batteries, it is primarily the electrolyte-filled pores located between the active particles that ensure the diffusion of lithium ions into the electrode. In the absence of electrolyte-filled pores, the transport of lithium ions from one particle to another occurs only at the points of contact between the particles, and this contact is essentially point-like. Thus, the resistance to lithium ion transport is so great that the battery cannot function.

[0011] Furthermore, for proper operation, the electrode pores must be filled with electrolyte. This filling is only possible if these pores are open. Moreover, depending on the size and tortuosity of the pores, impregnation of the electrode with the electrolyte can become very difficult, or even impossible. When the electrolyte-saturated porosity decreases, the electrical resistance of the layer decreases and its ionic resistance increases. When the porosity falls below 30% or even 20%, the ionic resistance increases sharply because some pores are then likely to close, preventing the electrode from being wetted by the electrolyte.

[0012] Therefore, when seeking to produce electrode films without porosity to increase energy density, it is necessary to limit the thickness of these films to less than 50 pm, and preferably to less than 25 pm, in order to allow the rapid diffusion of lithium ions in the solid, without loss of power.

[0013] To produce dense films, the main method used consists of depositing a film of lithium insertion electrode material using a vacuum process. This technique makes it possible to obtain dense films, without porosity or binders, and consequently having excellent energy densities and good temperature resistance.

[0014] The absence of porosity allows the transport of lithium ions by diffusion through the film, without the need for the use of organic electrolytes based on polymers or solvents containing lithium salts.

[0015] Such totally inorganic films provide excellent performance in aging, safety and temperature resistance.

[0016] Physical Vapor Deposition (PVD) is currently the most widely used technology for manufacturing thin-film microbatteries. These products require films free from porosity and other point defects to ensure low electrical resistivity and the good ionic conductivity necessary for the proper functioning of electrochemical devices.

[0017] The deposition rate obtained with such technologies is on the order of 0.1 pm to 1 pm per hour. PVD deposition techniques make it possible to obtain very thin films. These materials offer good quality, contain virtually no point defects, and allow for deposition at relatively low temperatures. However, due to the difference in evaporation rates between the various elements, it is difficult to deposit complex compounds using such techniques and to control the stoichiometry of the layer. This technique is perfectly suited to the production of thin films with simple chemical compositions, but as soon as one attempts to increase the deposition thickness, the deposition time becomes too long for industrial use in the field of low-cost products.

[0018] Moreover, the vacuum deposition techniques used to produce such films are very expensive and difficult to implement industrially over large areas, with high productivity.

[0019] Other currently available technologies for producing dense ceramic films include embodiments based on the densification of compact particle deposits or on obtaining films using sol-gel techniques. Sol-gel techniques consist of depositing a polymer network onto the surface of a substrate after hydrolysis, polymerization, and condensation steps. The sol-gel transition occurs during solvent evaporation, which accelerates the surface reaction processes. This technique allows for the production of very thin, compact deposits. The films thus obtained have a thickness on the order of hundreds of nanometers. These thicknesses are therefore too small to allow for reasonable energy storage in battery applications.

[0020] To increase the thickness of the deposit without inducing the risk of cracks or fissures, it is necessary to proceed in successive stages. However, this reduces the industrial productivity of this technique, since the aim is to increase the thickness of the layers.

[0021] It is also possible to produce ceramic films of electrodes and / or electrolyte for batteries by powder sintering. For this, a paste containing ceramic particles and organic binders is formed into a film to obtain a precursor strip commonly called a "green sheet".

[0022] This precursor strip is then calcined to remove organic matter and sintered at high temperature to obtain a plate of ceramic material.

[0023] In this case, the metallic films used to collect the current on these electrodes are also deposited using inking techniques. The metallic powders will also be sintered at the same time as the green sheet. Indeed, during the sintering step, the pores between the ceramic material particles will be filled, which will lead to a narrowing of the strip.

[0024] Sintering the current collectors with the ceramic films makes it possible to accommodate the dimensional variations of the ceramic films and collectors. to prevent the appearance of cracks.

[0025] These processes operate at very high temperatures. However, battery materials are most often sensitive to temperature and deteriorate rapidly when subjected to such heat treatments.

[0026] To reduce this sintering temperature, the use of nanoparticles has been proposed. This involves creating compact deposits of non-agglomerated nanoparticles. These deposits can be easily sintered at relatively low temperatures. This low temperature makes it possible to consider performing sintering directly on metallic substrates.

[0027] However, it is observed that these deposits, when made on metallic substrates, are prone, depending on the thickness of the deposit, its compactness, the size of the particles, to the appearance of cracks during the drying and / or sintering stages.

[0028] Electrophoretic nanoparticle deposition techniques have been used to increase the compactness of the deposits and thus facilitate low-temperature sintering with fewer cracks; this is described in WO 2013 / 064 773 (Fabien Gaben). Thermal coalescence occurs at a lower temperature the smaller the size of the nanoparticles, and in practice preferably below 100 nm.

[0029] The present invention seeks to remedy at least in part the disadvantages of the prior art mentioned above.

[0030] More specifically, the problem that the present invention seeks to solve is to provide a method for manufacturing dense ceramic layers directly on a metallic substrate that is simple, safe, fast, easy to implement, and inexpensive.

[0031] The present invention also aims to produce dense solid (ceramic) layers, usable in lithium ion batteries, containing no or very few defects and porosity.

[0032] The present invention also aims to provide dense electrodes and dense electrolytes having high ionic conductivity, a stable mechanical structure, good thermal stability and a long service life.

[0033] Another object of the invention is to provide a method for manufacturing an electronic, electrical or electrotechnical device such as a battery, a capacitor, a supercapacitor, a photovoltaic cell comprising a dense electrode or a dense electrolyte according to the invention. Object of the invention

[0034] According to the invention, the problem is solved by a method for manufacturing a lithium-ion battery with a capacity greater than 1 mA h, said method comprising the deposition of at least one dense layer, which may be an anode and / or a cathode and / or a electrolyte, by a dense layer deposition process comprising the steps of:

[0035] - supplying a substrate and a suspension of non-agglomerated nanoparticles of a material P, - deposition of a layer, on said substrate, from the suspension of primary nanoparticles of a material P; - drying of the layer thus obtained, - densification of the dried layer by mechanical compression and / or heat treatment,

[0036] knowing that the drying step and the densification step can be carried out at least partially at the same time, or during a temperature ramp.

[0037] The said process, which forms a first object of the present invention, is characterized in that the suspension of non-agglomerated nanoparticles of material P comprises nanoparticles of material P having a particular size distribution, making it possible to obtain, after deposition, a density greater than 75%. Said size is characterized by its value of D50.

[0038] This particular size distribution can be obtained either:

[0039] - continuously: In this case, the standard deviation / average size ratio of the nanoparticles of material P must be greater than 0.6, and the average size of the primary nanoparticles of material P less than or equal to 50 nm; or - discontinuously: in this case, the size distribution of the nanoparticles of material P includes nanoparticles with a first size DI between 50 nm and 20 nm, and nanoparticles with a second size D2 at least five times smaller than that of DI. Very advantageously, the particles of size DI represent between 50 and 75% of the total mass of nanoparticles.

[0040] Said suspension of non-agglomerated nanoparticles of material P can be obtained using a monodisperse DI size nanoparticle suspension, and / or said D2 size nanoparticle suspension can be obtained using a monodisperse suspension.

[0041] According to the invention, the deposition of the solid and dense ceramic layer is carried out by electrophoretic means, by the dip coating process, by the inkjet printing process, by roller coating, by coating through a slotted die, by curtain coating, or by scraping.

[0042] A second object of the invention is a lithium-ion battery with a capacity greater than 1 mA h, which can be obtained by this process. Said battery therefore comprises at least one dense layer, which may be an anode layer and / or a cathode layer and / or an electrolyte layer.

[0043] This dense anode layer and / or this dense cathode layer may exhibit a thickness of between approximately 1 pm and approximately 50 pm.

[0044] In one embodiment, said lithium ion battery comprises an anode and a cathode which are dense layers according to the invention.

[0045] In a first embodiment, the electrolyte layer may also be a dense layer according to the invention. In a second embodiment, said battery comprises a porous separator that separates said anode and said cathode; this porous separator is infiltrated by a liquid electrolyte. This electrolyte layer or this separator advantageously has a thickness of between approximately 1 µm and approximately 25 µm, and preferably between approximately 3 µm and approximately 10 µm.

[0046] In another embodiment, only its electrolyte layer is a dense layer according to the invention. Detailed description

[0047] In the context of this document, the size of a particle is defined by its largest dimension. The term "nanoparticle" means any particle or object of nanometric size having at least one dimension less than or equal to 100 nm. This size D is expressed here as size D50.

[0048] The term "nanoparticle" is used here to refer to primary particles, as opposed to particles formed by the aggregation or agglomeration of several primary particles. Such agglomerates can be reduced to nanoparticles (as we understand them here) by a deagglomeration operation, for example by grinding or ultrasonic treatment.

[0049] The density of a layer is here expressed as a relative value (for example as a percentage), which is obtained by comparing the actual density of the layer (denoted here as dlayer) and the theoretical density of the bulk material which constitutes it (denoted here as dtheoriqUe)- Thus, the porosity of the layer, expressed as a percentage, is determined as follows: Porosity [%] = [(doric - dlayer) / dtheoric] x 100.

[0050] According to the invention, the problem is solved by a method of depositing a layer from a suspension of nanoparticles, in which the size of the nanoparticles has a particle size distribution of a particular type.

[0051] According to one of the essential aspects of the invention, a suspension of nanoparticles is used which represents a particular nanoparticle size distribution, so as to significantly increase the density of the nanoparticle deposit before sintering.

[0052] Obtaining the most compact deposit possible before sintering will reduce shrinkage and the risk of cracking. In order to obtain the most compact deposit possible, it is necessary not only to perfectly control the size distribution of the nanoparticles but also to have the most compact deposit possible of these nano- particles, without agglomeration.

[0053] To obtain such compact deposits, one can either use electrophoretic deposition techniques for dilute suspensions, or techniques for depositioning concentrated, non-agglomerated suspensions of these polydisperse nanoparticles, by inking, dip-coating, curtain coating, doctor blade, slot-die, etc. Obtaining such concentrated suspensions requires the use of stabilizers, which are organic ligands (for example, of the PVP type), in order to prevent agglomeration between nanoparticles. These ligands will be removed at the beginning of the sintering heat treatment: typically, an intermediate thermal ramp is carried out to eliminate all these organic compounds before sintering.

[0054] The viscosity of the suspension used for deposition depends essentially on the nature of the liquid phase (solvent), the particle size, and their concentration (expressed as dry extract). The viscosity of the suspension, as well as the parameters of the deposition process (in particular the flow rate or the flow rate through the liquid), determine the thickness of the deposit. Depending on these parameters specific to the deposition technique, the viscosity generally used for dip coating, curtain coating, or slot die can vary widely and ranges from approximately 20 cP to approximately 2000 cP, measured at 20 °C. A colloidal suspension intended for deposition is often called an "ink," regardless of its viscosity.

[0055] Once these organic compounds are eliminated, the nanoparticles will come into contact and begin the consolidation process. The surfaces of the nanoparticles will weld together at the points of contact; this phenomenon is known as "necking." During sintering, these contact points, now weld zones, will grow by diffusion until they fill the voids left by the initial porosity of the deposit. It is the filling of these voids that causes the shrinkage.

[0056] Also, to obtain a final porosity rate of less than 15%, preferably less than 10%, on thick deposits made on metallic substrates and without cracks, it is necessary to maximize the compactness of the initial nanoparticle deposit, while retaining the nanometric effect which makes it possible to reduce consolidation temperatures and keep them compatible with the use of metallic substrates.

[0057] According to the invention, colloidal suspensions of nanoparticles are used, the average size of which does not exceed 100 nm. These nanoparticles also exhibit a fairly wide size distribution. When this size distribution follows an approximately Gaussian distribution, then the ratio (sigma / Ravg) of the standard deviation to the average radius of the nanoparticles must be greater than 0.6.

[0058] To increase the compactness of the initial deposit before sintering, it is also possible to use a mixture of two populations with different nanoparticle sizes. In this case, the The average diameter of the largest distribution should not exceed 100 nm, and preferably not exceed 50 nm. This first population of larger nanoparticles may have a more compact size distribution and an average sigma / R ratio of less than 0.6. This population of "large" nanoparticles should represent between 50% and 75% of the dry extract of the deposit (expressed as a mass percentage relative to the total mass of nanoparticles in the deposit). The second population of nanoparticles will therefore represent between 50% and 25% of the dry extract of the deposit (expressed as a mass percentage relative to the total mass of nanoparticles in the deposit). The average diameter of the particles in this second population should be at least five times smaller than that of the population of larger nanoparticles.As with the larger nanoparticles, the size distribution of this second population may be more compact and potentially with a sigma / Rmean ratio of less than 0.6.

[0059] In all cases, the two populations must not exhibit agglomeration in the resulting ink. Therefore, these nanoparticles can advantageously be synthesized in the presence of ligands or organic stabilizers in order to prevent aggregation, or even agglomeration, of the nanoparticles.

[0060] The preparation of colloidal suspensions by wet nanomilling makes it possible to obtain fairly wide size distributions. However, depending on the nature of the milled material, its "fragility," and the applied reduction ratio, the primary nanoparticles can be damaged or amorphized.

[0061] The materials used in the manufacture of lithium-ion batteries are particularly sensitive; the slightest change in their crystalline state or chemical composition results in degraded electrochemical performance. Therefore, for this type of application, it is preferable to use nanoparticles prepared in suspension directly by precipitation, using solvothermal or hydrothermal processes, at the desired primary nanoparticle size.

[0062] These precipitation-based nanoparticle synthesis processes allow for the production of primary nanoparticles of homogeneous size with a reduced size distribution, good crystallinity, and purity. It is also possible to obtain very small particle sizes, down to less than 10 nm, in a non-aggregated state using these processes. To achieve this, a ligand must be added directly to the synthesis reactor to prevent the formation of agglomerates or aggregates during synthesis. For example, PVP can be used to perform this function.

[0063] Since the size distribution of the non-agglomerated nanoparticles obtained by precipitation is quite narrow, it is advisable to favor a colloidal suspension preparation strategy mixing two size distributions, following the rules described above, in order to maximize the compactness of the deposit before sintering. This will allow, after sintering, the creation of relatively thick deposits directly onto metallic substrates with little or no risk of cracking during the sintering heat treatment, which will be maintained at a relatively low temperature due to the small size of the nanoparticles used.

[0064] This bimodal nanoparticle suspension is then used to deposit compact layers, which are subsequently densified by low-temperature heat treatment and can be used, in particular, as electrodes or electrolytes in electrochemical devices such as lithium-ion batteries. Various processes can be used to deposit these layers, including electrophoresis, inkjet printing, doctor blade deposition, roll coating, curtain coating, dip coating, and slot-die deposition. These are simple, safe, easy-to-implement and industrialize processes that produce a homogeneous, dense final layer.

[0065] Electrophoresis allows for the deposition of a uniform layer over large surfaces at a high deposition rate. Coating techniques, particularly dipping, roller coating, curtain coating, or squeegee coating, simplify bath management compared to electrophoresis, as the bath composition remains constant during coating deposition. Inkjet printing allows for localized deposition.

[0066] Dense thick-film electrodes and electrolytes produced in a single step can be obtained by the aforementioned processes from suspensions of bimodal or polydisperse nanoparticles.

[0067] The realization of a dense electrode according to the invention is now described by way of non-limiting example.

[0068] Nature of the current collector

[0069] The substrate serving as a current collector within batteries employing dense electrodes according to the invention is metallic, for example, a metal foil. It must be selected so as to withstand the temperature of any heat or thermomechanical treatment that will be applied to the layer deposited on this substrate, and this temperature will depend on the chemical nature of said layer. The substrate is preferably chosen from strips of titanium, molybdenum, chromium, tungsten, copper, nickel, or stainless steel, or any alloy containing at least one of the preceding elements.

[0070] The metal foil can be coated with a layer of noble metal, in particular chosen from gold, platinum, palladium, titanium, molybdenum, tungsten, chromium or alloys containing predominantly at least one or more of these metals, or with a layer of conductive material of the ITO type (which has the advantage of acting (also as a diffusion barrier).

[0071] In this example, we will use a 10-micron thick sheet of 316L type stainless steel.

[0072] Deposition of a dense electrode layer by dip-coating

[0073] Bimodal nanoparticles can be deposited by the dipping coating process, regardless of the chemical nature of the nanoparticles used. For example, to achieve a dense ceramic deposit of Li4Ti50i2, we can create an ink composed of nanoparticles of two different sizes. In the case of a Li4Ti50i2 anode, Li4Ti50i2 nanoparticles approximately 5 nm in diameter are synthesized via a glycothermal route (see the article "Impact of the Synthesis Parameters on the microstructure of nano-structured LTO prepared by glycothermal routes and 7 Li NMR structural investigations," M. Odziomek, F. Chaput et al., published in J Sol-Gel Sci Technol 89, 225-233 (2019)). Ligands are added to this synthesis to limit the agglomeration of the nanoparticles. These 5 nm diameter nanoparticles are combined with Li4Ti50i2 nanoparticles obtained by hydrothermal synthesis with particle sizes of 30 nm.

[0074] These nanoparticles are mixed and deagglomerated by ultrasound, with 70% by mass of 30 nm particles and 30% by mass of 5 nm nanoparticles in an ink with 15% total solids content, in ethanol, and containing PVP as a stabilizer. Each dip pass produces only a layer of limited thickness; the wet layer must be dried. To obtain a layer of the desired final thickness, the dip deposition step followed by the layer drying step can be repeated as many times as necessary.

[0075] Although this succession of dip-coating / drying steps is time-consuming, the dip-coating process is a simple, safe, easy-to-implement, and easy-to-industrialize process that allows for obtaining a homogeneous and compact final layer.

[0076] Treatment and properties of the deposited layers

[0077] The coatings deposited by dipping must be dried. Once dried, they undergo a two-stage heat treatment. First, the coating is held at 400°C for 10 minutes to calcine all the organic compounds it contains. Then, the treatment temperature is raised to 550°C and maintained at this temperature for one hour to consolidate the coating.

[0078] The selection of nanoparticle materials depends of course on the function of the layers thus deposited in the electrochemical, electrical or electronic device intended.

[0079] If the layer according to the invention is to function as the cathode of a battery, especially a lithium-ion battery, it can be made, for example, from a material P which is a cathode material chosen from:

[0080] - the oxides LiMn2O4, LiMn2O4 with 0 < x < 0.15, LiCoO2, LiNiO2, LiMnMn2O4, Li ... i5A1q()5O2, Li Alxl\4n2xO4 with 0 < x < 0.15, LiNii / xCoi / yMni / zO2 with x+y+z =10; - the phosphates LiFePO4, LiMnPO4, LiCoPO4, LiNiPO4, Li3V2(PO4)3; the phosphates of formula LiMM'PO4, with M and M' (M M') selected from Fe, Mn, Ni, Co, V; - all the lithia forms of the following chalcogenides: V2O5, V3O8, TiS2, titanium oxysulfides (TiOySz with z=2-y and 0.3 < y < 1), tungsten oxysulfides (WOySz with 0.6 < y < 3 and 0.1 < z < 2), CuS, CuS2, preferably LixV2O5 with 0 < x < 2, LixV3O8 with 0 < x < 1.7, LixTiS2 with 0 < x < 1, titanium and lithium oxysulfides LixTiOySz with z = 2-y, 0.3 < y < 1, LixW0 ySz, LixCuS, LixCuS2.

[0081] If the layer according to the invention is to function as the anode of a battery, especially a lithium-ion battery, it can be made, for example, from a material P which is an anode material selected from:

[0082] - carbon nanotubes, graphene, graphite; - lithium iron phosphate (typically formulated as LiFePO4); - mixed silicon and tin oxynitrides (typical formula SiaSnbOyNz with a>0, b>0, a+b<2, 0 <y<4, 0<z<3) (appelés aussi SiTON), et en particulier le SiSn0,8701,2Ni,72 ; ainsi que les oxynitrures-carbures de formule typique SiaSnbCcOyNz avec a > 0, b > 0, a+b <2, 0 < c < 10, 0 < y < 24, 0 < z < 17; - nitrides of type SixNy (in particular with x=3 and y=4), SnxNy (in particular with x=3 and y=4), ZnxNy (in particular with x=3 and y=2), Li3 xMxN (with 0 < x < 0.5 for M=Co, 0 < x < 0.6 for M=Ni, 0 < x < 0.3 for M=Cu); Si3 xMxN4 with M=Co or Fe and 0 < x < 3. - the oxides SnO2, SnO, Li2SnO3, SnSiO3, LiSiO3 (x >= 0 and 2 > y > 0), Li4Ti5O12, TiNb2O7, Co3O4, SnBo2bPO4O2 and TiO2, - TiNb2O7 composite oxides comprising between 0% and 10% by mass of carbon, preferably the carbon being chosen from graphene and carbon nanotubes, - compounds of general formula LiwTii xM1xNb2_yM2y07 zM3z in which M1 and M2 are each at least one element chosen from the group consisting of Nb, V, Ta, Fe, Co, Ti, Bi, Sb, As, P, Cr, Mo, W, B, Na, Mg, Ca, Ba, Pb, Al, Zr, Si, Sr, K, Cs and Sn, M1 and M2 being able to be identical or different from each other, and in which M3 is at least one halogen, and in which 0 < w < 5, 0 <x<l,0<y<2et0<z< 0.3.

[0083] If the layer according to the invention is to function as an electrolyte in a battery, especially a lithium-ion battery, it can be made, for example, from a material P which is an electrolyte material selected from:

[0084] - garnets of formula LidA1xA2y(TO4)z where A1 represents a cation of oxidation state +11, preferably Ca, Mg, Sr, Ba, Fe, Mn, Zn, Y, Gd; and where A2 represents a cation of oxidation state +III, preferably Al, Fe, Cr, Ga, Ti, La; and where (TO4) represents an anion in which T is an atom of oxidation state +IV, located at the center of a tetrahedron formed by the oxygen atoms, and in which TO4 advantageously represents the silicate or zirconate anion, knowing that all or part of the elements T of an oxidation state +IV can be replaced by atoms of an oxidation state +III or +V, such as Al, Fe, As, V, Nb, In, Ta; knowing that: d is between 2 and 10, preferably between 3 and 9, and even more preferably between 4 and 8; x is between 2.6 and 3.4 (preferably between 2.8 and 3.2); y is between 1.7 and 2.3 (preferably between 1.9 and 2.1) and z is between 2.9 and 3.1; - garnets, preferably chosen from: Li7La3Zr20i2; Li6La2BaTa20i2; Li5>5La3Nbi>75lno.250i2; Li5La3M20i2 with M = Nb or Ta or a mixture of the two compounds; Li7 xBaxLa3 XM2O[2 with 0 <x<letM = Nb ou Ta ou un mélange des deux composés ; le Li7 xLa3Zr2 xMxOi2avec 0<x<2etM = Al, Ga ou Ta ou un mélange de deux ou trois de ces composés ; - Lithified phosphates, preferably chosen from: NaSICON type lithified phosphates, Li3PO4; LiPO3; Li3Al0j4Scij6(PO4)3 called "LASP"; Lii>2Zri çCaOji(PO4)3; LiZr2(PO4)3; Lii+3xZr2(Pi_xSixO4)3 with 1.8 < x < 2.3; Lii+6xZr2(Pi XBXO4)3 with 0 < x < 0.25; Li3(Sc2 xMx)(PO4)3 with M=A1 or Y and 0 < x < 1; Lii+xMx(Sc)2 x(PO4)3 with M = Al, Y, Ga or a mixture of the three compounds and 0 < x < 0.8; Lii+xMx(Gai yScy)2 x(PO4)3 with 0 < x < 0.8 ; 0 < y < 1 and M= Al or Y or a mixture of the two compounds; Lii+xMx(Ga)2 x(PO4)3 with M = Al, Y or a mixture of the two compounds and 0 < x < 0.8; Lii+xAlxTi2 x(PO4)3 with 0 < x < 1 called “LATP”; or Lii+XA1 xGe2 X(PO4)3 with 0 < x < 1 called “LAGP”; or Lii+x+zMx(Gei.yTiy)2.xSizP 3 ZO[2 with 0 < x < 0.8 and 0 < y < 1.0 and 0 < z < 0.6 and M= Al, Ga or Y or a mixture of two or three of these compounds; the Li3+y(Sc2 xMx)QyP3 yOi2 with M = Al and / or Y and Q = Si and / or Se, 0 < x < 0.8 and 0 < y < 1; or the Lii+x+yMxSc2 x . QyP3yO12 with M = Al, Y, Ga or a mixture of the three compounds and Q = Si and / or Se, 0 < x < 0.8 and 0 < y < 1; or the Lii+x+y+zMx(Gai_yScy)2_xQzP3_zOi2 with 0 < x < 0.8,0 <y<l,0<z< 0,6 avec M = Al ou Y ou un mélange des deux composés et Q= Si et / ou Se ; ou le Lii+xZr2 XBX(PO4)3 avec 0 < x < 0,25 ; ou le Lii+xZr2xCax(PO4)3 avec 0 < x < 0,25 ; ou Lii+XM3XM2 xP30i2 avec 0 < x < 1 et M3= Cr, V, Ca, B, Mg, Bi et / ou Mo, M = Sc, Sn, Zr, Hf, Se ou Si, ou un mélange de ces composés ; ou le Lii+2xCaxZr2 x(PO4)3 avec 0 < x < 0,25 ; lithia borates, preferably chosen from: Li3(Sc2xMx)(BO3)3 with M=A1 or Y and 0 < x < 1; Li1+xMx(Sc)2.x(BO3)3 with M = Al, Y, Ga or a mixture of the three compounds and 0 < x < 0.8; Li1+xMx(Gal yScy)2 x(BO3)3 with 0 < x < 0.8, 0 < y < 1 and M= Al or Y; Li1+xMx(Ga)2 x(BO3)3 with M = Al, Y or a mixture of the two compounds and 0 < x < 0.8; Li3BO3, Li3BO3-Li2SO4, Li3BO3-Li2SiO4, Li3BO3-Li2SiO4-Li2SO4; oxynitrides, preferably chosen from Li3PO4 xN2x / 3, Li4SiO4 xN2x / 3, Li4 GeO4 xN2x / 3 with 0 < x < 4 or Li3BO3 xN2x / 3 with 0 < x < 3; Lithium compounds based on lithium oxynitride and phosphorus, called "LiPON", in the form of LixPOyNz with x ~ 2.8 and 2y+3z ~ 7.8 and 0.16 < z < 0.4, and in particular Li2.9PO3.3No.46, but also the compounds LiwPOxNySz with 2x+3y+2z = 5 = w or the compounds LiwPOxNySz with 3.2 < x < 3.8, 0.13 < y < 0.4, 0 < z < 0.2, 2.9 < w < 3.3 or the compounds in the form of Li PxAlyOuNvSw with 5x+3y=5, 2u+3v+2w=5+t, 2.9 <t<3,3, 0,84<x<0,94, 0,094<y<0,26, 3,2<u<3,8, 0,13<v<0,46, 0<w<0,2 ; materials based on lithium phosphorus or boron oxynitrides, respectively called "LiPON" and "LIBON", may also contain silicon, sulfur, zirconium, aluminum, or a combination of aluminum, boron, sulfur and / or silicon, and boron for materials based on lithium phosphorus oxynitrides; lithium compounds based on lithium oxynitride, phosphorus and silicon called "LiSiPON", and in particular Li19Si0.28P1.0O1.1N10; lithium oxynitrides of the types LiBON, LiBSO, LiSiPON, LiSON, thio-LiSiCON, LiPONB (where B, P and S represent boron, phosphorus and sulfur respectively); lithium oxynitrides of the LiBSO type such as (lx)LiBO2-xLi2SO4 with 0.4 < x < 0.8; the lithia oxides, preferably chosen from Li7La3Zr2Oi2 or Li5+xLa3 (Zrx,A2 x)Oi2 with A = Sc, Y, Al, Ga and 1.4 < x < 2 or Li3xLa2 / 3 xTiO3 or Li3xLa2 / 3 xTiO3 with 0 < x < 0.16 (LLTO); silicates, preferably chosen from Li2Si2O5, Li2SiO3, Li2Si2O6, LiAlSiO4 , Li4SiO4, LiAlSi2O6; - solid anti-perovskite type electrolytes selected from: Li3OA with A a halide or a mixture of halides, preferably at least one of the elements selected from F, Cl, Br, I or a mixture of two, three or four of these elements; Li(3_x)Mx / 2OA with 0 < x < 3, M a divalent metal, preferably at least one of the elements selected from Mg, Ca, Ba, Sr or a mixture of two, three or four of these elements, A a halide or a mixture of halides, preferably at least one of the elements selected from F, Cl, Br, I or a mixture of two, three or four of these elements; Li(3 x)M 3x / 3OA with 0 < x < 3, M3 a trivalent metal, A a halide or a mixture of halides, preferably at least one of the elements selected from F, Cl, Br, I or a mixture of two, three or four of these elements; or LiCOXzY(iz), with X and Y being halides as mentioned above in relation to A, and 0 < z < 1, - the compounds Lao,5iLio>34Ti2,94, Li3j4Voj4Geo>604, Li2O-Nb2O5, LiAlGaSPO4; - formulations based on Li2CO3, B2O3, Li2O, Al(PO3)3LiF, P2S3, Li2S, Li3N, Lii4Zn(GeO4)4, Li3.6Geo,6Vo,4O4, LiTi2(PO4)3, Li3j25Geo>25Po,25S4, Liij3Aloj3Tii 7(PO 4)3, Lii+xAlxM2 x(PO4)3 (where M = Ge, Ti, and / or Hf, and where 0 < x < 1), Lii+x+yAlxTi2 x SiyP3 yOi2 (where 0 < x < 1 and 0 < y < 1).

[0085] The nanoparticles used in the inks for depositing these electrodes can also have a core-shell structure. Indeed, the performance of the dense electrodes thus obtained will depend on their ionic and electronic conductivity. Therefore, it may be important to apply a "shell" of an inorganic material with good electronic and / or ionic conductivity properties to the surface of the active material nanoparticles.

[0086] Thus, in an advantageous embodiment, the core is formed of an electrode material (anode or cathode), and the shell is formed of a material that is both electronically conductive and does not impede the passage of lithium ions. By way of example, the shell may be formed by a layer of a metal that is thin enough to allow lithium ions to pass through, or by a sufficiently thin layer of graphite, or by a layer of an ionic conductor that is also a good electronic conductor.

[0087] Example of manufacturing a lithium-ion battery

[0088] A method for manufacturing lithium ion batteries using the layers according to the invention is described here.

[0089] a) Preparation of the electrodes by the deposition process according to the invention

[0090] A first dense Li4Ti50i2 electrode was deposited, obtained by the process described above in the chapter "Deposition of a dense electrode layer by dipping" (dip-coating). A second dense LiMn2O4 electrode was also deposited using a similar process.

[0091] On each of these two electrodes, a thin mesoporous film of Li3PO4 agglomerates was then deposited, which acts in the battery as a separator film, and which was prepared as described below.

[0092] b) Deposition of the separator layer

[0093] A suspension of Li3PO4 nanoparticles was prepared from the two solutions shown below: First, 45.76 g of CH3COOLi, 2H2O were dissolved in 448 ml of water, and then 224 ml of ethanol were added with vigorous stirring to obtain solution A. Second, 16.24 g of H3PO4 (85 wt% in water) were diluted in 422.4 ml of water, and then 182.4 ml of ethanol were added to this solution to obtain a second solution, hereafter referred to as solution B. Solution B was then added, under vacuum and stirring, to solution A.

[0094] The resulting solution, perfectly clear after the disappearance of the bubbles formed during mixing, was added to 4.8 liters of acetone using an Ultraturrax™ type homogenizer to homogenize the medium. A white precipitate was immediately observed in suspension in the liquid phase.

[0095] The reaction mixture was homogenized for 5 minutes and then maintained under magnetic stirring for 10 minutes. It was allowed to settle for 1 to 2 hours. The supernatant was discarded, and the remaining suspension was centrifuged for 10 minutes at 6000 g. Then, 1.2 L of water was added to resuspend the precipitate (using a sonotrode and magnetic stirring). Two further washes of this type were then performed with ethanol. Under vigorous stirring, 15 mL of a 1 g / mL Bis(2-(methacryloyoloxy)ethyl)phosphate solution was added to the resulting colloidal suspension in ethanol. This made the suspension more stable. The suspension was then sonicated using a sonotrode. The suspension was then centrifuged for 10 minutes at 6000 g. The pellet was then redispersed in 1.2 L of ethanol and then centrifuged for 10 minutes at 6000 g.The pellets thus obtained are redispersed in 900 ml of ethanol to obtain a 15 g / l suspension suitable for electrophoretic deposition.

[0096] Agglomerates of approximately 200 nm consisting of primary Li3PO4 particles of 10 nm were thus obtained in suspension in ethanol.

[0097] Thin porous films of Li3PO4 were then deposited by electrophoresis onto the surface of the previously prepared anodes and cathodes by applying an electric field of 20 V / cm² to the previously obtained Li3PO4 nanoparticle suspension for 90 seconds to obtain a layer of approximately 2 µm. The layer was then air-dried at 120°C and subsequently calcined at 350°C for 120 minutes to eliminate any traces of organic residues.

[0098] c) Assembly of the electrodes and the separator

[0099] After depositing 2 µm of porous Li3PO4 onto each of the previously fabricated electrodes (Li2+xMn2yO4 and Li4Ti5O2i2), the two subsystems were stacked so that the Li3PO4 films were in contact. This stack was then hot-pressed under vacuum between two flat plates. To do this, the stack was first placed under a pressure of 5 MPa and then dried under vacuum for 30 minutes at 103 bar. The press plates were then heated to 550°C at a rate of 0.4°C / second. At 550°C, the stack was then thermo-compressed under a pressure of 45 MPa for 20 minutes, and the system was then cooled to room temperature. The assembly was then dried at 120°C for 48 hours under vacuum (10 mbar).

[0100] d) Impregnation of the separator with a liquid electrolyte

[0101] This assembly was then impregnated, under an anhydrous atmosphere, by immersion in an electrolytic solution comprising PYR14TFSI and 0.7 M LiTFSI. PYR14TFSI is the common abbreviation for 1-butyl-1-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide. LITFSI is the common abbreviation for lithium bis-trifluoromethanesulfonimide (CAS No. 90076-65-6). The ionic liquid instantly entered the pores of the separator by capillary action. Each of the two ends of the system was kept immersed for 5 minutes in a drop of the electrolytic mixture.

[0102] It is noted that in an industrial manufacturing process, impregnation is carried out after the encapsulation of the battery, and followed by the production of the electrical contact elements.

[0103] The battery according to the invention can be a mini-battery, with a capacity greater than 1 mAh and up to about 1 Ah, or a battery with a capacity greater than 1 Ah. Indeed, the process according to the invention is particularly well suited to producing layers with a thickness greater than 1 µm, or even greater than 5 µm, while ensuring a low series resistance of the battery.

[0104] These batteries and mini-batteries can be made:

[0105] - either solely with "all-solid" type layers, i.e., devoid of phases

[0106] impregnated liquids or pastes (said liquid or paste phases being a lithium ion conductive medium, capable of acting as an electrolyte),

[0107] - either with electrodes according to the invention and mesoporous "all-solid" type separators, impregnated by a liquid or paste-like phase, typically a lithium ion-conducting medium, which spontaneously enters the layer and does not exit this layer, so that This layer can be considered quasi-solid. or again with an electrode according to the invention and impregnated porous separators (i.e. layers having a network of open pores which can be impregnated with a liquid or pasty phase, and which gives these layers wet properties.

Claims

Claims

1. A method of manufacturing a lithium ion battery with a capacity greater than 1 mA h, comprising depositing at least one dense layer, which may be an anode and / or a cathode and / or an electrolyte, by a method of depositing a dense layer which comprises the steps of: i. Providing a substrate and a suspension of non-agglomerated nanoparticles of a material P; ii. Depositing a layer, on said substrate, from the suspension of primary nanoparticles of a material P; iii. Drying the layer thus obtained; iv.Densification of the dried layer by mechanical compression and / or heat treatment, knowing that steps (iii) and (iv) can be carried out at least partially at the same time, or during a temperature ramp; said method being characterized in that the suspension of non-agglomerated nanoparticles of material P comprises nanoparticles of material P having a size distribution, said size being characterized by its D50 value, such that: - the distribution comprises nanoparticles of material P of a first size DI between 20 nm and 50 nm, and nanoparticles of material P of a second size D2 characterized by a D50 value at least five times lower than that of DI; or - the distribution has an average size of the nanoparticles of material P of less than 50 nm, and a standard deviation to average size ratio greater than 0.

6.

2. Method according to claim 1, wherein said suspension of non-agglomerated nanoparticles of material P comprises nanoparticles of material P of a first size DI between 20 nm and 50 nm, and nanoparticles of material P of a second size D2 characterized by a value D50 at least five times lower than that of D1, and said particles of size D1 represent between 50 and 75% of the total mass of nanoparticles.

3. Method according to claim 1 or 2, characterized in that said suspension of non-agglomerated nanoparticles of material P is obtained using a suspension of nanoparticles of size Dl mo- nodisperse.

4. Method according to one of claims 1 to 3, characterized in that the suspension of nanoparticles of size D2 is obtained using a monodisperse suspension.

5. A method according to any one of claims 1 to 4, characterized in that the deposition of the dense thin layer is carried out electrophoretically, by the dip coating method, by the inkjet printing method, by roller coating, by curtain coating or by scraping.

6. Method according to any one of claims 1 to 5, characterized in that said suspension has a viscosity, measured at 20°C, between 20 cP and 2000 cP.

7. Method according to any one of claims 1 to 6, characterized in that said material P is an inorganic material, preferably selected from the group formed by: - ​​the oxides LiMn2O4, Lii+xMn2xO4 with 0 < x < 0.15, LiCoO2, LiNiO2, LiMni.5Nio,504, LiMni,5Nio,5-xXx04 where X is selected from Al, Fe, Cr, Co, Rh, Nd, other rare earths such as Sc, Y, Lu, La, Ce, Pr, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and where 0 < x < 0.1, LiMn2xMxO4 with M = Er, Dy, Gd, Tb, Yb, Al, Y, Ni, Co, Ti, Sn, As, Mg or a mixture of these compounds and or 0 < x < 0.4, LiFeO2, Lihdni / 3Nii / 3Coi / 3O2, ,LiNio ^Coq.15AI005 O2, LiAlxMn2 XO4 with 0 < x < 0.15, LiNii / xCoi / yMni / zO2 with x+y+z =10; - phosphates LiFePO4, LiMnPO4, LiCoPO4, LiNiPO4, Li3V2 (PO4)3; phosphates of formula LiMM'P04, with M and M' (M M') selected from Fe, Mn, Ni, Co, V; - all lithiated forms of the following chalcogenides: V2O5, V3O8, TiS2, titanium oxysulfides (TiOySz with z=2-y and 0.3 < y < 1), tungsten oxysulfides (WOySz with 0.6 < y < 3 and 0.1 < z < 2), CuS, CuS2, preferably LixV2O5 with 0 < x < 2, LixV3O8 with 0 < x < 1.7, LixTiS2 with 0 < x < 1, titanium and lithium oxysulfides LixTiOySz with z = 2-y, 0.3 < y < 1, LixWOySz, LixCuS, LixCuS2; - carbon nanotubes, graphene, graphite; - lithium iron phosphate (typical formula LiFePO4); - mixed oxynitrides of silicon and tin (typical formula. SiaSnbOyNz with a>0, b>0, a+b<2, 0 <y<4, 0<z<3) (appelés aussi SiTON), et en particulier le SiSno,870i,2Ni,72 ; ainsi que les oxynitrures-carbures de formule typique SiaSnbCcOyNz avec a > 0, b > 0, a+b <2, 0 < c < 10, 0 < y < 24, 0 < z < 17; nitrides of type SixNy (in particular with x=3 and y=4), Snx Ny (in particular with x=3 and y=4), ZnxNy (in particular with x=3 and y=2), Li3 xMxN (with 0 < x < 0.5 for M=Co, 0 < x < 0.6 for M=Ni, 0 < x < 0.3 for M=Cu); Si3 xMxN4 with M=Co or Fe and 0 < x < 3. the oxides SnO2, SnO, Li2SnO3, SnSiO3, LixSiOy (x >= 0 and 2 > y > 0), Li4Ti50i2, TiNb2O7, Co3O4, SnB0j6Po,402>9 and TiO2, the composite oxides TiNb2O7 comprising between 0% and 10% by mass of carbon, preferably the carbon being chosen from graphene and carbon nanotubes; compounds of general formula LiwTii xM1xNb2 yM2y07 zM3z in which M1 and M2 are each at least one element selected from the group consisting of Nb, V, Ta, Fe, Co, Ti, Bi, Sb, As, P, Cr, Mo, W, B, Na, Mg, Ca, Ba, Pb, Al, Zr, Si, Sr, K, Cs and Sn, M1 and M2 being able to be the same or different from each other, and in which M3 is at least one halogen, and in which 0 <w<5, 0<x<l,0<y<2et0<z< 0.

3. garnets of formula LidA'xA2y(TO4)z where A1 represents a cation with oxidation number +11, preferably Ca, Mg, Sr, Ba, Fe, Mn, Zn, Y, Gd; and where A2 represents a cation with oxidation number +III, preferably Al, Fe, Cr, Ga, Ti, La; and where (TO4) represents an anion in which T is an atom with oxidation number +IV, located at the center of a tetrahedron formed by oxygen atoms, and in which TO4 advantageously represents a silicate or zirconate anion, knowing that all or part of the T elements with oxidation number +IV can be replaced by atoms with oxidation number +III or +V, such as Al, Fe, As, V, Nb, In, Ta; knowing that: d is between 2 and 10, preferably between 3 and 9, and even more preferably between 4 and 8; x is between 2.6 and 3.4 (preferably between 2.8 and 3.2); y is between 1.7 and 2.3 (preferably between 1.9 and 2.1) and z is between 2.9 and 3.1; garnets, preferably chosen from: Li7La3Zr20i2; Li6 La2BaTa20i2; Li5.5La3Nbi.75lno.250i2; Li5La3M20i2 with M = Nb or Ta or a mixture of the two compounds; Li7 xBaxLa 3xM20i2 with 0 < x < andM = Nb or Ta or a mixture of the two compounds; Li7 xLa3Zr2xMxOi2with 0 <x<2etM = Al, Ga ou Ta ou un mélange de deux ou trois de ces composés ; lithium phosphates, preferably chosen from: lithium phosphates of the NaSICON type, Li3PO4; LiPO3; Li3Al0j4Sci>6(PO4)3 called “LASP”; Liij2ZrijQCa0ji(PO4)3; LiZr2(PO4)3; Lii+3xZr2(Pi_xSixO4)3 with 1.8 < x < 2.3; Li i+6xZr2(Pl xBxO4)3 with 0 < x < 0.25; Li3(Sc2 xMx)(PO4)3 with M=A1 or Y and 0 < x < 1; Lii+xMx(Sc)2 x(PO4)3 with M = Al, Y, Ga or a mixture of the three compounds and 0 < x < 0.8; Li i+xMx(Gai yScy)2 x(PO4)3 with 0 < x < 0.8; 0 < y < 1 and M= Al or Y or a mixture of the two compounds; Lii+xMx(Ga)2 X(PO4 )3 with M = Al, Y or a mixture of the two compounds and 0 < x < 0.8; Lii+xAlxTi2 x(PO4)3 with 0 < x < 1 called “LATP”; or Lii+xAlxGe2 X(PO4)3 with 0 < x < 1 called “LAGP”; or Li1+x+zMx(Gej yTiy)2xSizP3 ZO12 with 0 < x < 0.8 and 0 < y < 1.0 and 0 < z < 0.6 and M = Al, Ga or Y or a mixture of two or three of these compounds; Li3+y(Sc2 xMx)Qy P3 yOi2 with M = Al and / or Y and Q = Si and / or Se, 0 < x < 0.8 and 0 < y < 1; or Lii+x+yMxSc2 xQyP3 yOi2 with M = Al, Y, Ga or a mixture of the three compounds and Q = Si and / or Se, 0 < x < 0.8 and 0 < y < 1; or the Lii+x+y+zMx(Gai_yScy)2_xQzP3_zOi2with 0 < x < 0,8,0 <y<l,0<z< 0,6 avec M = Al ou Y ou un mélange des deux composés et Q= Si et / ou Se ; ou le Lii+xZr2 x Bx(PO4)3 avec 0 < x < 0,25 ; ou le Lii+xZr2 xCax(PO4)3 avec 0 < x < 0,25 ; ou Lii+xM3xM2 xP30i2 avec 0 < x < 1 et M3= Cr, V, Ca, B, Mg, Bi et / ou Mo, M = Sc, Sn, Zr, Hf, Se ou Si, ou un mélange de ces composés ; ou le Lii+2xCaxZr2 x(PO4)3 avec 0 < x < 0,25 ; lithium borates, preferably chosen from: Li3(Sc2_xMx )(BO3)3 with M=A1 or Y and 0 < x < 1; Lii+xMx(Sc)2 x(BO3)3 with M = Al, Y, Ga or a mixture of the three compounds and 0 < x < 0.8; Lii+xMx(GaiyScy)2x(BO3)3 with 0 <x<0,8,0<y< 1 et M= Al ou Y ; le Lii+xMx(Ga)2 x(BO3)3 avec M = Al, Y ou un mélange des deux composés et 0 < x < 0,8 ; le Li3BO3, le Li3BO3-Li2SO4, Li3BO3-Li2SiO4, Li3BO3-Li2SiO4-Li2SO4; oxynitrides, preferably selected from Li3PO4_xN2x / 3, Li4 SiO4_xN2x / 3, Li4GeO4-xN2x / 3 with 0 < x < 4 or Li3BO3 xN2x / 3 with 0 <x<3; lithium compounds based on lithium and phosphorus oxynitride, called "LiPON", in the form of LixPOyNz with x ~ 2.8 and 2y+3z ~ 7.8 and 0.16 < z < 0.4, and in particular Li2.9 PO3.3N0.46, but also the compounds LiwPOxNySz with 2x+3y+2z = 5 = w or the compounds LiwPOxNySz with 3.2 < x < 3.8, 0.13 < y < 0.4, 0 < z < 0.2,2.9 < w < 3.3 or the compounds in the form of LitPxAlyOuNvSw with 5x+3y=5, 2u+3v+2w=5+t, 2.9 <t<3,3, 0,84<x<0,94, 0,094<y<0,26, 3,2<u<3,8, 0,13<v<0,46, 0<w<0,2 ; materials based on lithium phosphorus or boron oxynitrides, called respectively “LiPON” and “LIBON”, which may also contain silicon, sulfur, zirconium, aluminum, or a combination of aluminum, boron, sulfur and / or silicon, and boron for materials based on lithium phosphorus oxynitrides; lithium compounds based on lithium, phosphorus and silicon oxynitride called “LiSiPON”, and in particular Lii.9Sio.28Pi.oOi.iNi.o; lithium oxynitrides of the types LiBON, LiBSO, LiSiPON, LiSON, thio-LiSiCON, LiPONB (where B, P and S represent boron, phosphorus and sulfur respectively); lithium oxynitrides of LiBSO type such as (lx)LiBO2 -xLi2SO4 with 0.4 < x < 0.8; lithiated oxides, preferably chosen from Li7La3Zr20i2 or Li5+xLa3(Zrx,A2 x)Oi2 with A = Sc, Y, Al, Ga and 1.4 < x < 2 or Lio.35Lao.55Ti03 or Li3xLa2 / 3 xTiO3 with 0 < x < 0.16 (LLTO); silicates, preferably chosen from Li2Si2O5, Li2SiO3, Li2 Si2O6, LiAlSiO4, Li4SiO4, LiAlSi2O6; solid electrolytes of anti-perovskite type chosen from: Li3OA with A a halide or a mixture of halides, preferably at least one of the elements chosen from F, Cl, Br, I or a mixture of two or three or four of these elements; Li (3 x)Mx / 20A with 0 < x < 3, M a divalent metal, preferably at least one of the elements selected from Mg, Ca, Ba, Sr or a mixture of two or three or four of these elements, A a halide or a mixture of halides, preferably at least one of the elements selected from F, Cl, Br, I or a mixture of two or three or four of these elements; Li(3 x)M3x / 3OA with 0 < x < 3, M3 a trivalent metal, A a halide or a mixture of halides, preferably at least one of the elements selected from F, Cl, Br, I or a mixture of two or three or four of these elements; or LiCOXzY(iz), with X and Y halides as mentioned above in relation to A, and 0 < z < 1, - the compounds LaOj5iLioj34Ti2j94, Li3j4Voj4Ge0j604, Li2O-Nb2O5, LiAlGaSPO4; - formulations based on Li2CO3, B2O3, Li2O, Al(PO3)3LiF, P2 S3, Li2S, Li3N, Lii4Zn(GeO4)4, Li3>6Geo,6Vo,404, LiTi2(PO4)3, Li 3,25Geoj25Poj25S4, Lilj3Aloj3Tilj7(P04)3, Li1+XA1XM2_X(PO4)3 (where M = Ge, Ti, and / or Hf, and where 0 < x < 1), Lii+x+yAlxTi2_xSiyP3_yOi2 (where 0 < x < 1 and 0 < y < 1).

8. Lithium ion battery with a capacity greater than 1 mA h, obtainable by a method according to any one of claims 1 to 7.

9. Lithium ion battery according to claim 8, characterized in that said dense layer is an anode layer.

10. A lithium ion battery according to any one of claims 8 or 9, characterized in that said dense layer is a cathode layer.

11. A lithium ion battery according to any one of claims 8 to 10, characterized in that said dense layer is an electrolyte layer.

12. Lithium ion battery according to any one of claims 8 to 10, characterized in that it comprises an anode and a cathode each of which is one of said dense layers, in that it further comprises a porous separator which separates said anode and said cathode, and a liquid electrolyte infiltrated into said porous separator.