Thermoplastic polymer powder for 3D printing
Patent Information
- Application Number
- FR2021007386
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-07-08
Abstract
Description
Title of the invention: Thermoplastic polymer powder for construction of 3D articles FIELD OF THE INVENTION
[0001] The present invention relates to a polymer powder suitable for 3D printing by sintering. More particularly, the present invention relates to a powder comprising a thermoplastic polymer composition (component (a)) making it possible to obtain articles manufactured by 3D printing having improved mechanical properties. The invention also relates to its manufacturing method and its use for manufacturing articles by 3D printing (also called "printed parts"). TECHNICAL BACKGROUND
[0002] There are different techniques for 3D printing using polymer powder. The principle is generally based on the agglomeration of powder, layer by layer by melting it (hereinafter "sintering") caused by a source of electromagnetic energy, for example a laser beam, infrared radiation, UV radiation, or any source of electromagnetic radiation allowing the powder to be melted layer by layer to manufacture three-dimensional objects.
[0003] Mention may be made of selective laser beam sintering (SLS) technology. Mention may also be made of sintering technologies using an absorber, for example the technologies known as “High Speed Sintering” in English (HSS) and “Multi-Jet Fusion” in English (MJF).
[0004] To carry out the printing, the polymer powder, preheated in a reservoir tank, is introduced into the construction enclosure, spread in a thin layer (called the “bed”) on a horizontal plate then heated to the temperature of the bed.
[0005] The bed temperature is generally located in the interval between the crystallization temperature (Te) and the melting temperature (Tf) of the polymer.
[0006] Generally, for polymers having sharp melting temperatures, in particular when the enthalpy of fusion is high (eg > 60 J / g), the bed temperature can be adjusted between Tf-5°C and Tf-20°C.
[0007] However, in the case of elastomers and polymers having spread melting temperatures, in particular when the enthalpy of fusion is low (eg < 60 J / g), the temperature of the bed is generally set to a lower temperature, for example at Tf-30°C, to avoid the caking phenomenon.
[0008] During printing, the thin layer of polymer powder is selectively and briefly irradiated by an electromagnetic energy source, for example, a laser beam in an SLS process, or infrared radiation in an MJF process.
[0009] The result is that the impacted powder particles melt to form material points of the article to be printed. When the printing of the layer is finished, the plate is lowered, and the bed is covered with a new thin layer of powder. The steps are repeated with a succession of layers of powder until the solid part is obtained.
[0010] Undesirable porosity has often been observed in printed parts. This porosity is due in whole or in part to poor coalescence of the melted powder grains during the printing process.
[0011] Too much porosity is detrimental to mechanical properties. For example, a significantly lower elongation at break can be observed for a 3D printed part compared to a part of the same composition but obtained by an injection process.
[0012] Poor coalescence of the powder can also create surface defects.
[0013] To solve this coalescence problem, different solutions have been proposed. in the past.
[0014] For example, document US 10,596,728 B2 proposes a powder suitable for PBF to coat the powder with a hydrophobic substance to lower the surface energy thereof to less than 35 mN / m.
[0015] A prior preparation step to coat the powder with a hydrophobic substance is therefore required.
[0016] Or again, it is proposed, for 3D printing in MJF, to use a fusion agent including an energy absorber making it possible to absorb the electromagnetic radiation to coalesce the powders, as described in:
[0017] - document WO 19245518 describing a kit a thermoplastic elastomer having an avalanche angle of 49 to 59°C, a cut-off energy of 55 to 78 kJ / kg, and an avalanche energy of 10 to 27 kJ / kg, and a melting agent, - document WO 19182614 describing a kit comprising a polyether block and polyamide block polymer having a relative viscosity in solution of 1.55 to 1.80, and a melting agent, - document WO 19245517 describing a kit comprising a thermoplastic elastomer in which at least 70% of the individuals have an aspect ratio of 0.75 to 1 and a melting agent.
[0018] There is therefore a need to be able to manufacture parts, from a thermoplastic powder, by 3D printing by sintering, with good mechanical properties and without the aforementioned constraints.
[0019] The present invention makes it possible to meet this need. Summary of the invention
[0020] According to a first aspect, the invention relates to a polymer powder suitable for 3D printing by sintering, comprising: (a) a thermoplastic polymer composition; and optionally, (b) one or more fillers or reinforcements, (c) one or more additives, where the ratio G"2 / G"1 of said powder is less than or equal to 3.00, preferably less than or equal to 2.90, G"1 being the loss modulus at the melting temperature (Tf) of the powder, when the powder is heated to Tf+40°C for 2 minutes and is then cooled to Tf at a rate of -5°C / min, G"2 being the loss modulus at - 30°C of the Tf of the powder, when the powder is heated to Tf+ 40°C for 2 minutes and is then cooled to Tf-30°C at a rate of -5°C / min,, the values of G"2, G"1 being measured according to ISO 6721-10: part 10, at an angular frequency of 6.28 rad / sec.
[0021] Preferably, the ratio G"2 / G"1 is less than or equal to 2.80.
[0022] Generally, the ratio G"2 / G"1 is greater than or equal to 2.00, preferably greater or equal to 2.10.
[0023] According to one embodiment, G"1 is less than or equal to 100,000 Pa, preferably less than or equal to 50,000 Pa.
[0024] According to one embodiment, G"2 is less than or equal to 200,000 Pa, preferably less than or equal to 100,000 Pa.
[0025] It was observed that when the ratio G"2 / G"1 was less than 3.00, the coalescence of the powders could take place sufficiently, during its cooling from the molten state. The printed parts then have a better elongation at break, comparable with the printed parts obtained by injection.
[0026] When the ratio G"2 / G"1 is greater than 3.00, the molten powders solidify too quickly, preventing sufficient coalescence between them, creating undesirable porosity in the printed part, which leads to poor elongation at break.
[0027] This is particularly suitable for elastomers and polymers having spread melting temperatures, in particular when the enthalpy of fusion is low (eg < 60 J / g), namely, in the case where the bed temperature is set relatively far from the Tf, typically at Tf-30°C.
[0028] The present invention therefore provides a thermoplastic powder making it possible to obtain good quality printed parts, having improved coalescence, as well as improved mechanical properties.
[0029] Advantageously, the powder has a diameter Dv50 as measured according to standard ISO 9276 - parts 1 to 6, of 40 to 150 pm.
[0030] Advantageously, the powder has an inherent viscosity greater than or equal to 1.0, preferably greater than or equal to 1.1, or 1.2, and less than or equal to 1.8, preferably less than or equal to 1.7, or 1.6, or 1.5.
[0031] The powder having an inherent viscosity in the range described above makes it possible to advantageously improve the mechanical properties of the printed parts. Indeed, it has been observed that when the inherent viscosity is too low, namely, less than 1.0, the mechanical properties of the printed parts become insufficient for certain end uses. When the inherent viscosity is greater than 1.8, the coalescence of the powders can be impacted, thus creating porosities in the final parts and poor mechanical properties.
[0032] Preferably, the polymer composition (a) has an enthalpy of fusion less than or equal to 60 J / g, preferably less than or equal to 55 J / g.
[0033] Preferably, composition (a) has an enthalpy of fusion of 10 to 15 J / g; or 15 to 20 J / g; or 20 to 25 J / g; or 25 to 30 J / g; or 30 to 35 J / g; or 35 to 40 J / g; or 40 to 45 J / g; or 45 to 50 J / g; or 50 to 55 J / g; or 55 to 60 J / g.
[0034] According to one embodiment, the polymer composition (a) comprises at least one thermoplastic polymer chosen from polypropylene (PP), polyolefin, polyamide (PA), polyester, polyarylether ketone (PAEK), polyphenylene sulfide, polyacetal, polyimide, vinylidene fluoride polymer and / or their mixture, preferably chosen from PP, PA, and / or PAEK.
[0035] According to a particularly interesting embodiment, the polymer composition (a) comprises at least one thermoplastic elastomer.
[0036] Preferably, the polymer composition (a) comprises a thermoplastic elastomer selected from the group consisting of SBS, SIS, SEBS, TPU, COPE and PEBA block copolymers and their blends and alloys, and in particular, it comprises a PEBA. Alternatively, the polymer composition (a) may comprise a thermoplastic elastomer selected from TPO, PP / NBR, PO / CPE-VD, EVA / VC and PVC / NBR blends.
[0037] The present invention thus provides a particular thermoplastic powder for printing which makes it possible to improve the coalescence of the powders, by reducing the porosity of the printed part, thus improving the mechanical property thereof, in particular in terms of elongation at break.
[0038] According to a second aspect, the invention relates to a process for preparing such a powder, comprising the steps of: (i) grinding a polymer composition (a) into a powder with a volume average diameter Dv50 of 40 to 150 pm, before or after, (ii) introduction of at least one or more fillers and / or one or more additives, where applicable.
[0039] According to another aspect, the invention aims at the use of such a powder for 3D printing by sintering, in particular chosen from the selective laser sintering (SLS) process, the MJF (Multi Jet Fusion) type sintering process and the HSS (High Speed Sintering) type sintering process.
[0040] According to another aspect, the invention finally relates to an article obtained by 3D printing by sintering such a powder. Description of the invention Definition
[0041] In the present description of the invention, including in the examples below: - the term "thermoplastic polymer" is understood to denote a polymer having the property of softening when it is heated sufficiently, and which, upon cooling, becomes hard again;
[0042] - the term “thermoplastic elastomer” means a polymer comprising flexible segments and rigid segments, for example in the form of a block copolymer, in which the rigid segments disappear when the temperature increases. Alternatively, these may be mixtures combining the presence of a flexible elastomer phase, crosslinked or not, dispersed in a rigid thermoplastic continuous phase. The mixtures may in particular be mixtures of a thermoplastic polymer with an elastomer;
[0043] - The term "copolymer" means a polymer resulting from the copolymer rization of at least two chemically different types of monomer, called comonomers. A copolymer is therefore formed from at least two repeating units. It can also be formed from three or more repeating units. More specifically, the term "block copolymer" or "block copolymer" is understood to mean copolymers in the above sense, in which at least two distinct monomer blocks are covalently linked. The length of the blocks can be variable. Preferably, the blocks are composed of 1 to 1000, preferably 1 to 100, and in particular 1 to 50 repeating units, respectively. The link between the two monomer blocks may sometimes require an intermediate non-repeating unit called a connecting block.
[0044] - The term "melting temperature" means the temperature at at which a partially crystalline polymer passes into the viscous liquid state, as measured during the first heating (Tfl) by differential scanning calorimetry (DSC) according to standard NF EN ISO 11 357-3 using a heating rate of 20°C / min.
[0045] - The term "crystallization temperature" means the temperature at which a partially crystalline polymer changes from a viscous liquid state to a solid state, as measured by differential scanning calorimetry (DSC) according to standard NF EN ISO 11 357-3 using a cooling rate of 20°C / min.
[0046] - the term "glass transition temperature" means the temperature temperature at which a polymer changes from a rubbery state to a glassy state, or vice versa, as measured by differential scanning calorimetry (DSC) according to standard NF EN ISO 11 357-2 using a heating rate of 20°C / min;
[0047] - the term "enthalpy of fusion" means the heat consumed during the solid / liquid transition of the thermoplastic elastomer, as measured by differential scanning calorimetry, according to ISO 11257-3:1999;
[0048] - the term “volume average diameter” or “Dv” also means the volume mean diameter of a powdery material, as measured according to ISO 9276 - parts 1 to 6: "Representation of data obtained by particle size analysis". Different diameters are distinguished. More specifically, Dv50 designates the volume median diameter, and Dv10 and Dv90 designate respectively the volume mean diameters below which 10 or 90% by volume of the particles are located. The volume mean diameter can be measured in particular by means of a laser granulometer, for example a laser granulometer (Sympatec Helos) and software (Fraunhofer) making it possible to obtain the volumetric distribution of a powder and to deduce the Dv10, Dv50 and Dv90;
[0049] - The term "inherent viscosity" means the viscosity such that measured according to the following steps: - Taking polymer samples between 0.07 and 0.10 g and preferably 0.15 g maximum, - Addition of a sufficient quantity of m-cresol solvent by weighing in order to obtain a concentration (C) of 0.5 g / L, - Heating the mixture with stirring on a hot plate, regulated at 100°C ± 5°C, until the polymer is completely dissolved; - Cooling the solution to room temperature, preferably for at least 30 minutes; - Measurement of the flow time tO of the pure solvent and the flow time t of the solution using a micro-Ubbelohde tube viscometer in a thermostatically controlled bath regulated at 20°C ± 0.05°C, - Calculation of viscosity according to the formula 1 / C x Ln (t / tO), where C represents the concentration and Ln the natural logarithm, For each sample, three measurements are made on different solutions and then the average is calculated.
[0050] - the term "loss modulus" means the modulus measured in a oscillatory rheometer according to ISO 6721-10:2015 - Part 10 under the following conditions: Device used: ARES G2 (TA Instruments) Geometry: parallel planes of 25mm diameter Angular frequency: 1Hz (6.28 rad / sec) Deformation: 2% Atmosphere: Nitrogen flushing
[0051] - The nomenclature used to designate the polyamides according to the present invention follows the ISO 1874-1 standard.
[0052] - The molar mass in number Mn of the polymers described, and of the constituent blocks thermoplastic elastomers, can be measured before copolymerization by size exclusion chromatography (SEC) according to ISO 16014-1:2012 using hexafluoroisopropanol (HFIP) as eluent. Thermoplastic polymer composition (a)
[0053] The thermoplastic polymer composition can in principle be of any nature, provided that it has the properties, in particular thermal properties, suitable for 3D printing by sintering.
[0054] The polymer composition (a) may comprise at least one polymer chosen from polyolefin, polyamide, polyester, polyarylether ketone (PAEK), polyphenylene sulfide, polyacetal, polyimide, vinylidene fluoride polymer and / or their mixture.
[0055] According to one embodiment, the polymer composition (a) comprises a polyarylether ketone (PAEK), selected from polyetherketoneketone (PEKK), polyetheretherketone (PEEK), polyetherketone(PEK), polyetheretherketoneketone (PEEKK), a polyetheretheretherketone (PEEEK), polyetherdiphenyletherketone (PEDEK), their mixtures and / or their copolymers.
[0056] More specifically: the PEKK comprises one or more units of formula: -Ph-O-Ph-C(O)-Ph-C(O)-; the PEEK comprises one or more units of formula: -Ph-O-Ph-O-Ph-C(O)-; PEK comprises one or more units of formula: -Ph-O-Ph-C(O)-; the PEEKK comprises one or more units of formula: -Ph-O-Ph-O-Ph-C(O)- Ph-C(O)-; the PEEEK comprises one or more units of formula: -Ph-O-Ph-O-Ph-O- Ph-C(O)-; PEDEK comprises one or more units of formula -Ph-O-Ph-Ph-O-Ph-C(O)-; in which: Ph represents a phenylene group and -C(O)- a carbonyl group, each of the phenylenes being able independently to be of ortho (1-2), meta (1-3) or para (1-4) type, preferentially being of meta or para type.
[0057] According to one embodiment, the polymer composition (a) comprises a vinylidene fluoride polymer which may be a homopolymer or a copolymer obtained by polymerization of the VDF monomer with at least one other comonomer, The at least one other comonomer may be a halogenated alkene, and more preferably a fluorinated alkene. Examples include halogenated propenes or ethylenes, and more particularly fluoroethylene (or vinyl fluoride), chlorofluoroethylenes (1-chloro-1-fluoroethylene and 1-chloro-2-fluoroethylene), trifluoroethylene, chlorodifluoroethylenes (especially 1-chloro-2,2-difluoroethylene), 1-bromo-2,2-difluoroethylene, bromotrifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, trifluoropropenes (especially 3,3,3-trifluoropropene), tetrafluoropropenes (especially 2,3,3,3-tetrafluoropropene), chlorotrifluoropropenes (especially 2-chloro-3,3,3-trifluoropropene), pentafluoropropenes (especially 1,1,3,3,3-pentafluoropropene or 1,2,3,3,3-pentafluoropropene) and hexafluoropropene also called hexafluoropropylene.It may also be a perfluoroalkylvinylether, of general formula RrO-CF-CF2, Rf being an alkyl group, preferably C1 to C4. Preferred examples are PP VE (perfluoropropylvinylether) and PMVE (perfluoromethylvinylether).
[0058] Such polymers are commercially available, for example the products marketed by Arkema under the names Dyflor®, Kynar®, Solef®.
[0059] According to one embodiment, the polymer composition (a) comprises a polyamide.
[0060] The polyamide may be a homopolyamide, a copolyamide, or mixtures thereof.
[0061] According to one embodiment, the polyamide comes from the condensation of one or more monomers of α,β-aminocarboxylic acid type or one or more monomers of lactam type (type “Z”).
[0062] Examples of α,α-amino carboxylic acids include alpha-omega amino acids, such as aminocaproic, amino-7-heptanoic, amino-11-undecanoic, n-heptyl-11-aminoundecanoic and amino-12-dodecanoic acids.
[0063] Examples of lactams include those having 3 to 12 carbon atoms on the main ring and which may be substituted. Examples include P,[3-dimethylpropriolactam, α,α-dimethylpropriolactam, amylolactam, ca-prolactam, capryllactam, oenantholactam, 2-pyrrolidone and lauryllactam.
[0064] As examples of this type of preferred polyamides, mention may be made of PA 6, PA 11 and PA 12, as well as their mixtures.
[0065] According to one embodiment, the polyamide comes from the condensation of a dicarboxylic acid with an aliphatic, cycloaliphatic or aromatic diamine (type “XY”, X representing the number of carbon atoms of the diamine and Y representing the number of carbon atoms of the dicarboxylic acid).
[0066] As an example of a diamine, mention may be made of aliphatic diamines having from 6 to 12 atoms, diamine X also being able to be aryl and / or saturated cyclic. As Examples include hexamethylenediamine, piperazine, tetramethylenediamine, octamethylenediamine, decamethylenediamine, dodecamethylenediamine, 1,5 diaminohexane, 2,2,4-trimethyl-1,6-diaminohexane, diamine polyols, isophorone diamine (IPD), methyl pentamethylenediamine (MPDM), bis(aminocyclohexyl)methane (BACM), bis(3-methyl-4 aminocyclohexyl)methane (BMACM), methaxylyenediamine, trimethylhexamethylenediamine.
[0067] As an example of a dicarboxylic acid, mention may be made of acids Y having between 4 and 18 carbon atoms, preferably from 9 to 12 carbon atoms. Mention may be made, for example, of adipic acid, sebacic acid, azelaic acid, suberic acid, isophthalic acid, butanedioic acid, 1,4 cyclohexyldicarboxylic acid, terephthalic acid, the sodium or lithium salt of sulfoisophthalic acid, dimerized fatty acids (in particular those having a dimer content of at least 98% and / or hydrogenated) and 1,2-dodecanedioic acid HOOC-(CH2)i0-COOH.
[0068] As an example of this type of preferred polyamides, PA 612 resulting from the condensation of hexamethylenediamine and 1,12-dodecanedioic acid; PA 613 resulting from the condensation of hexamethylenediamine and brassylic acid; PA 912 resulting from the condensation of 1,9-nonanediamine and 1,12-dodecanedioic acid; PA 1010 resulting from the condensation of 1,10-decanediamine and sebacic acid; PA 1012 resulting from the condensation of 1,10-decanediamine and 1,12-dodecanedioic acid.
[0069] According to one embodiment, the polyamide is a copolyamide resulting from the polycondensation: - at least two different monomers chosen from different α,α-amino carboxylic acids or two different lactams or a lactam and an α,α-amino carboxylic acid of different carbon numbers; or -at least one α,α-amino carboxylic acid (or a lactam), at least one diamine and at least one dicarboxylic acid, or - an aliphatic diamine with an aliphatic dicarboxylic acid and at least one other monomer chosen from aliphatic diamines different from the previous one and aliphatic diacids different from the previous one.
[0070] The notation PA Z / XY, PA Z / Z', PA Z / XY / X'Y', PA Z / Z7XY, PA Z / Z7XY / X'Y', etc. refers to copolyamides in which XY, Z, X'Y', Z' etc. represent homopolyamide monomers XY, Z as described above, X'Y' being the same as or different from XY, Z' being the same as or different from Z.
[0071] According to one embodiment, one of the monomers constituting a copolyamide may represent more than 50%, preferably more than 60% by mass of the total mixture of monomers.
[0072] According to one embodiment, one of the monomers constituting a copolyamide may represent less than 90%, preferably less than 80% by mass of the total monomer mixture.
[0073] Examples of particularly preferred copolyamides are the blocks PA 6 / 11, PA 6 / 12, PA 11 / 12, PA 6 / 11 / 12, PA 6 / 66 / 12, PA 6 / 1010, PA 6 / 1012, PA 6 / 1010 / 1012, PA 6 / 1012 / 12, PA 6 / 66 / 11 / 12, PA 6 / 1010 / 1012 / 1014, as well as mixtures thereof.
[0074] It is also possible to use mixtures of polyamides, which may be mixtures of aliphatic polyamides and semi-aromatic polyamides and mixtures of aliphatic polyamides and cycloaliphatic polyamides. Thermoplastic elastomer
[0075] According to one embodiment, the polymer composition (a) according to the invention comprises at least one thermoplastic elastomer.
[0076] The thermoplastic elastomer can in principle be of any nature, provided that it has the properties, particularly thermal properties, suitable for 3D printing by sintering.
[0077] The thermoplastic elastomer may in particular be a sty-block copolymer polystyrene (TPS), in particular polystyrene and polybutadiene blocks (SBS), a polystyrene and polyisoprene block copolymer (SIS), a polystyrene and poly(ethylene / butylene) block copolymer (SEBS), an isocyanate and ether or ester block copolymer (TPU), a polyester and polyester or polyether block copolymer (COPE), or a polyamide and polyether block copolymer (PEBA).
[0078] Such thermoplastic elastomers are commercially available, for example products under the names CAWITON®, THERMOLAST K®, THERMOLAST M®, Sofprene®, Dryflex® and Laprene ® (TPS), Desmopan® or Elastollan® (TPU), Santoprene®, Termoton®, Solprene®, THERMOLAST V®, Vegaprene®, or Forprene® (TPV), and For-Tec E® or Engage. Ninjaflex® (TPO).
[0079] According to a particularly interesting embodiment, the thermoplastic elastomer is a “PEBA” copolymer. These copolymers are notably marketed by Arkema France under the name Pebax®, by Evonik® under the name Vestamid®, by EMS under the name Grilamid®, and by Sanyo under the name Pelestat®.
[0080] Alternatively, it may be a mixture of a flexible polymer phase dispersed in a continuous rigid polymer phase. Examples of such mixtures include EPDM dispersed in a polyolefin (TPO) or a thermoplastic vulcanizate (TPV), a copolymer of butadiene and acrylonitrile (NBR), vulcanized or not, dispersed in a polypropylene (PP / NBR), a chlorinated polyethylene dispersed in a polyolefin (PO / CPE-VD), an EVA dispersed in vinylidene chloride (EVA / VC), or a copolymer of butadiene and acrylonitrile (NBR), vulcanized or not, dispersed in a polyvinyl chloride (PVC / NBR).
[0081] The elastomer present in component (a) of the powder of the invention has preferably a melting temperature (Tm) ranging from 100 to 300°C, and preferably from 120 to 200°C.
[0082] Furthermore, the thermoplastic elastomer preferably has a crystallization temperature (Te) ranging from 40 to 250°C, and preferably from 45 to 200°C, for example from 45 to 150°C.
[0083] Typically, the Tf and Te are determined directly from the polymer powder. When dealing with a polymer blend, the Tf retained is the lowest Tf in the polymer blend, and the Te retained will be the highest Te in the polymer blend.
[0084] Finally, the difference between the Te and the Tf of the thermoplastic elastomer is preferably greater than or equal to 20°C, preferably greater than or equal to 30°C, more preferably greater than or equal to 40°C, or 50°C, or 60°C, or 70°C, or 80°C.
[0085] Component (a) may comprise one or more thermoplastic polymers as described above.
[0086] According to one embodiment, component (a) may further comprise up to 50% by weight of one or more additional thermoplastic polymers. Preferably, however, component (a) consists only of thermoplastic elastomer.
[0087] The thermoplastic elastomer may in particular have a fusion enthalpy of between 10 and 45 J / g. In particular, it may be 10 to 15 J / g; or 15 to 20 J / g; or 20 to 25 J / g; or 25 to 30 J / g; or 30 to 35 J / g; or 35 to 40 J / g, or 40 to 45 J / g.
[0088] Copolymer with polyamide blocks and polyether blocks (PEBA)
[0089] The polyamide block and polyether block copolymer of the present invention may preferably be a linear (non-crosslinked) copolymer.
[0090] PEBA copolymers can result from the polycondensation of polyamide (PA) blocks with reactive ends with polyether (PE) blocks with reactive ends, such as: 1) polyamide blocks with diamine chain ends with polyoxyalkylene blocks with dicarboxylic chain ends; 2) polyamide blocks with dicarboxylic chain ends with polyoxyalkylene blocks with diamine chain ends; 3) polyamide blocks with dicarboxylic chain ends with polyetherdiols, the products obtained being, in this particular case, polyetheresteramides.
[0091] The polyamide blocks with dicarboxylic chain ends originate, for example, from the condensation of polyamide precursors in the presence of a chain-limiting carboxylic diacid. The polyamide blocks with diamine chain ends originate, for example, from the condensation of polyamide precursors in the presence of a chain-limiting diamine.
[0092] Two types of polyamide blocks can be advantageously used.
[0093] According to a first type (variant I), the polyamide blocks are copolyamide blocks.
[0094] The copolymer blocks (COPA) may be a copolyamide as described in the “polyamide” section above.
[0095] According to this variant I, the number-average molar mass (Mn) of the polyamide blocks in the PEBA copolymer is from 400 to 20,000 g / mol, more preferably from 500 to 10,000 g / mol, preferably from 500 to 4,000 g / mol, and even more preferably from 600 to 2,000 g / mol. For example, the number average molar mass of the polyamide blocks in the PEBA copolymer may be 400 to 1000 g / mol, or 1000 to 1500 g / mol, or 1500 to 2000 g / mol, or 2000 to 2500 g / mol, or 2500 to 3000 g / mol, or 3000 to 3500 g / mol, or 3500 to 4000 g / mol, or 4000 to 5000 g / mol, or 5000 to 6000 g / mol, or 6000 to 7000 g / mol, or 7000 to 8000 g / mol, or 8000 to 9000 g / mol, or 9000 to 10000 g / mol, or from 10000 to 11000 g / mol, or from 11000 to 12000 g / mol, or 12000 to 13000 g / mol, or 13000 to 14000 g / mol, or 14000 to 15000 g / mol, or 15000 to 16000 g / mol, or 16000 to 17000 g / mol, or 17000 to 18000 g / mol, or 18000 to 19000 g / mol, or 19000 to 20000 g / mol.
[0096] According to this variant I, the number-average molar mass (Mn) of the polyether blocks is from 100 to 6000 g / mol, more preferably from 200 to 3000 g / mol, and even more preferably from 200 to 2000 g / mol. The number average molar mass of the polyether blocks may be 100 to 200 g / mol, or 200 to 500 g / mol, or 500 to 800 g / mol, or 800 to 1000 g / mol, or 1000 to 1500 g / mol, or 1500 to 2000 g / mol, or 2000 to 2500 g / mol, or 2500 to 3000 g / mol, or 3000 to 3500 g / mol, or 3500 to 4000 g / mol, or 4000 to 4500 g / mol, or 4500 to 5000 g / mol, or 5000 to 5500 g / mol, or 5500 to 6000 g / mol.
[0097] According to one embodiment, the preferred PEBA copolymers are copolymers comprising copolyamide blocks as defined above (variant I) and blocks derived from PTMG, for example: PA 6 / 11 and derived from PTMG, PA 6 / 12 and derived from PTMG, PA 11 / 12 and derived from PTMG, PA 6 / 11 / 12 and derived from PTMG, PA 6 / 66 / 12 and derived from PTMG, PA 6 / 1010 and derived from PTMG, PA 6 / 1012 and derived from PTMG, PA 6 / 1010 / 1012 and derived from PTMG, PA 6 / 1012 / 12 and derived from PTMG.
[0098] According to a second type (variant II), the polyamide blocks result from the condensation of an α,α-aminocarboxylic acid or a lactam and the number-average molar mass (Mn) of the polyamide blocks in the PEBA is preferably from 400 to 1500 g / mol, more preferably from 500 to 1200 g / mol, preferably from 500 to 1000 g / mol.
[0099] The polyamide blocks according to this variant are polyamides of the “Z” type such as described in the “polyamide” section below.
[0100] For example, the number average molar mass (Mn) of the polyamide blocks in the PEBA copolymer may be 400 to 600 g / mol, or 600 to 900 g / mol, or 900 to 1000 g / mol, or 1000 to 1200 g / mol, or 1200 to 1300 g / mol, or 1300 to 1400 g / mol, or 1400 to 1500 g / mol.
[0101] According to this embodiment, the number-average molar mass (Mn) of the polyether blocks is preferably from 400 to 1500 g / mol, more preferably from 500 to 1200 g / mol, and even more preferably from 500 to 1000 g / mol.
[0102] For example, the number average molar mass of the polyether blocks may be 400 to 600 g / mol, or 600 to 900 g / mol, or 900 to 1000 g / mol, or 1000 to 1200 g / mol, or 1200 to 1300 g / mol, or 1300 to 1400 g / mol, or 1400 to 1500 g / mol.
[0103] According to this embodiment, the preferred PEBA copolymers are PA 11, PA 12, PA 6, and their mixtures.
[0104] The polyether blocks of PEBA essentially comprise or consist of alkylene oxide units. The polyether blocks may be derived from alkylene glycols such as PEG (polyethylene glycol), PPG (propylene glycol), PO3G (polytrimethylene glycol) or PTMG (polytetramethylene glycol), preferably PTMG.
[0105] They can also be derived from copolyethers comprising different alkylene oxides distributed in the chain in a regular manner, in particular by blocks, or in a statistical manner.
[0106] Polyether blocks can also be obtained by oxyethylation of bisphenols, such as bisphenol A. These products are described in particular in document EP 613919 AL
[0107] The polyether blocks can also be ethoxylated primary amines, such as the products of formula:
[0108] [Chem.l] H--(OŒ2CH2)m —N—(CH2CH2O)n— H (CHA Eye
[0109] in which m and n are integers between 1 and 20 and x an integer between 8 and 18.
[0110] These products are, for example, commercially available under the brand NORAMOX® from the company CECA and under the brand GENAMIN® from the company CLARIANT.
[0111] The polyether blocks may finally comprise or consist of polyoxyalkylene blocks with NH2 chain ends. Such blocks may be obtained by cyanoace- tylation of polyether diols. Such polyethers are sold by Huntsman Company under the name Jeffamine® or Elastamine® (e.g. Jeffamine® D400, D2000, ED 2003, XTJ 542).
[0112] A two-step method for preparing PEBAs having ester bonds between PA blocks and PE blocks is described in FR 2846332 A1. A method for preparing PEBAs having amide bonds between PA blocks and PE blocks is described in EP 1482011 A1. The polyether blocks can also be mixed with polyamide precursors and a diacid chain limiter to prepare PEBAs by a one-step process.
[0113] If PEBAs generally comprise a polyamide block and a polyether block, they can also comprise two, three, four or even more different blocks chosen from those described.
[0114] The number-average molar masses (Mn) in the present invention are fixed by the chain limiter content. They can be calculated according to the relationship:
[0115] hî-n H monomer X hdw repeating unit / H chain limiter 4" hî-w chain limiter
[0116] In this formula, nmonomer represents the number of moles of monomer, n limiter of chain represents the number of moles of limiter (e.g. diacid) in excess, Mwrepeat unit represents the molar mass of the repeat unit, and Mwichain limiter represents the molar mass of the limiter (e.g. diacid) in excess.
[0117] According to one embodiment, the mass proportion of polyether blocks in the copolymer is at least 50% relative to the total weight of the copolymer.
[0118] Preferably, the mass proportion of polyether blocks is from 55 to 85% relative to the total weight of the copolymer, and more preferably from 60 to 80%, relative to the total weight of the copolymer.
[0119] The mass proportions of blocks in the copolymer can be determined from the number-average molar masses of the blocks.
[0120] Copolymer with polyester blocks and polyether blocks (COPE)
[0121] According to another embodiment, the thermoplastic elastomer is a copoly-etherester (COPE).
[0122] COPEs comprise at least one polyether (PE) block, and at least one PES polyester (homopolyester or copolyester) block.
[0123] COPEs comprise flexible PE blocks derived from polyetherdiols and rigid polyester blocks which result from the reaction of at least one dicarboxylic acid with at least one short diol. The PES blocks and the PE blocks are linked by ester bonds resulting from the reaction of the acid functions of the dicarboxylic acid with the OH functions of the polyetherdiol.
[0124] The chain of polyethers and diacids forms the flexible blocks while the chain of the short diol with the diacids forms the rigid blocks of the copoly-etherester.
[0125] Advantageously, the diacids are aromatic dicarboxylic acids having from 8 to 14 carbon atoms. Up to 50 mol% of the aromatic dicarboxylic acid may be replaced by at least one other aromatic dicarboxylic acid having from 8 to 14 carbon atoms, and / or up to 20 mol% may be replaced by an aliphatic dicarboxylic acid having from 2 to 14 carbon atoms. Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, bibenzoic acid, naphthalene dicarboxylic acid, 4,4'-diphenylenedicarboxylic acid, bis(p-carboxyphenyl)methane acid, ethylene bis(p-benzoic acid), 1,4-tetramethylene bis(p-oxybenzoic acid), ethylene bis(p-oxybenzoic acid), 1,3-trimethylene bis(p-oxybenzoic acid).
[0126] The short diol may in particular be an aliphatic glycol of formula HO(CH2)nOH in which n is an integer ranging from 2 to 10, in particular ethylene glycol, 1,3-trimethylene glycol, 1,4-tetramethylene glycol, 1,6-hexamethylene glycol, 1,3 propylene glycol, 1,8 octamethylene glycol and 1,10-decamethylene glycol, or neopentyl glycol.
[0127] The preferred PES units are derived from the reaction of an aromatic dicarboxylic acid, in particular terephthalic acid, with a glycol, in particular ethanediol or 1,4-butanediol. Such copolyetheresters are described in patents EP 402883 A1 and EP 405227 A1
[0128] The PE units may be derived from polyetherdiols as defined above, for example polyethylene glycol (PEG), polypropylene glycol (PPG), polytrimethylene glycol (PO3G) or polytetramethylene glycol (PTMG). The PES units may be derived from the reaction of a dicarboxylic acid such as terephthalic acid with a glycol such as in particular ethanediol or 1,4-butanediol. Such copolyetheresters are described in patents EP 402883 A1 and EP 405227 A1.
[0129] The number-average molar mass (Mn) of the polyester blocks is preferably from 400 to 1500 g / mol, more preferably from 500 to 1200 g / mol, preferably from 500 to 1000 g / mol. For example, the number-average molar mass (Mn) of the polyester blocks may be from 400 to 600 g / mol, or from 600 to 900 g / mol, or from 900 to 1000 g / mol, or from 1000 to 1200 g / mol, or from 1200 to 1300 g / mol, or from 1300 to 1400 g / mol, or from 1400 to 1500 g / mol.
[0130] The number-average molar mass (Mn) of the polyether blocks is as described above for PEBAs.
[0131] The mass ratio of the polyester blocks relative to the polyether blocks of the COPE may in particular be from 0.1 to 20. The mass ratio may in particular be from 0.1 to 0.2; or from 0.2 to 0.3; or from 0.3 to 0.4; or from 0.4 to 0.5; or from 0.5 to 1; or from 1 to 2; or from 2 to 3; or from 3 to 4; or from 4 to 5; or from 5 to 7; or from 7 to 10; or from 10 to 13; or from 13 to 16; or from 16 to 19; or from 19 to 20. A mass ratio of 2 to 19, and more specifically of 4 to 10 is particularly preferred. Thermoplastic polyurethane (TPU)
[0132] According to another embodiment, the thermoplastic elastomer is a TPU, i.e. a copolymer with polyurethane (PU) blocks and polyether (PE) blocks, also called polyether-urethane, or a copolymer with polyurethane (PU) blocks and polyester (PES) blocks, also called polyesterurethane.
[0133] TPUs of the first type mentioned above result from the condensation of polyetherdiols with polyurethanes. The rigid PU blocks and the flexible PE blocks are connected by bonds resulting from the reaction of the isocyanate functions of the polyurethane with the -OH functions of the polyetherdiol.
[0134] The PU blocks may be derived from the reaction of at least one diisocyanate which may be chosen from aromatic diisocyanates (e.g.: MDI, TDI) and / or aliphatic diisocyanates (e.g.: HDI or hexamethylenediisocyanate) with at least one short diol. This short diol may be chosen from the glycols mentioned previously in the description of the copolyetheresters, in particular polyethylene glycol (PEG), poly(1,2-propylene glycol) (PPG), poly(1,3-propylene glycol) (PO3G), or polytetramethylene glycol (PTMG).
[0135] TPUs of the second type mentioned above result from the condensation of flexible polyesters with polyisocyanates. The rigid PU blocks and the flexible PES blocks are connected by bonds resulting from the reaction of the isocyanate functions of the polyurethane with the terminal functions of the polyester.
[0136] The PU blocks may be as described above for the TPUs of the first type. The flexible PES blocks may be derived from the reaction of an aliphatic dicarboxylic acid having 4 to 12 carbon atoms, in particular adipic acid, with a glycol, such as ethanediol or 1,4-butanediol. Such copolyetheresters are described in patents EP 402883 A1 and EP 405227 A1.
[0137] The number-average molar mass (Mn) of the PU blocks in the TPUs is preferably 400 to 1500 g / mol, more preferably 500 to 1200 g / mol, preferably 500 to 1000 g / mol. For example, the number-average molar mass (Mn) of the PU blocks may be 400 to 600 g / mol, or 600 to 900 g / mol, or 900 to 1000 g / mol, or 1000 to 1200 g / mol, or 1200 to 1300 g / mol, or 1300 to 1400 g / mol, or 1400 to 1500 g / mol. That of the polyether blocks is as described above for the PEBAs.
[0138] The mass ratio of the polyurethane blocks relative to the polyether blocks of the TPU may in particular be from 0.1 to 20. In particular, it may be from 0.1 to 0.2; or from 0.2 to 0.3; or from 0.3 to 0.4; or from 0.4 to 0.5; or from 0.5 to 1; or from 1 to 2; or from 2 to 3; or from 3 to 4; or from 4 to 5; or from 5 to 7; or from 7 to 10; or from 10 to 13; or from 13 to 16; or from 16 to 19; or from 19 to 20. A mass ratio of 2 to 19, and more specifically of 4 to 10 is particularly preferred.
[0139] The thermoplastic elastomers according to the invention can be obtained at least partially from bio-resourced raw materials.
[0140] By raw materials of renewable origin or bio-resourced raw materials is meant materials which comprise bio-resourced carbon or carbon of renewable origin. Indeed, unlike materials derived from fossil materials, materials composed of renewable raw materials contain 14 C. The “renewable carbon content” or “bio-resourced carbon content” is determined in accordance with the standards ASTM D 6866 (ASTM D 6866-06) and ASTM D 7026 (ASTM D 7026-04). For example, the PEBAs comprising PA 11 blocks come at least in part from bio-resourced raw materials and have a bio-resourced carbon content of at least 1%, which corresponds to a 12C / 14C isotopic ratio of at least 1.2 x 10 14. Preferably, the PEBAs comprise at least 50% by mass of bio-resourced carbon on the total mass of carbon, which corresponds to a 12C / 14C isotopic ratio of at least 0.6.10 12.This content is advantageously higher, in particular up to 100%, which corresponds to a 12C / 14C isotopic ratio of 1.2 x 10 12, in the case for example of PEBA with PA 11 blocks and PE blocks comprising PTMG from raw materials of renewable origin. Loads and reinforcements (b)
[0141] The polymer powder according to the invention may also optionally comprise fillers or reinforcements, in particular in order to ensure that the printed article has sufficient mechanical properties, in particular in terms of modulus. These fillers may in particular be carbonate minerals, in particular calcium carbonate, magnesium carbonate, dolomite, calcite, barium sulfate, calcium sulfate, dolomite, alumina hydrate, wollastonite, montmorillonite, zeolite, perlite, nanofillers (fillers having a dimension of the order of a nanometer) such as nano-clays, calcium silicates, magnesium silicates, such as talc, mica, kaolin, attapulgite and mixtures thereof. As reinforcements, mention may in particular be made of carbon nanotubes, glass fibers and carbon fibers as well as glass beads optionally coated with silane.Component (c) may comprise one or more fillers and / or reinforcements. Advantageously, the fillers and reinforcements do not comprise pigments as defined below for the pigment composition.
[0142] More specifically, the powder of the invention may comprise 0 to 60%; or 5 to 50%; or 10 to 40%; or 10 to 30% by weight of component (c). According to one embodiment of realization, the polymer powder is free of fillers and reinforcements. Additives (c)
[0143] The polymer powder may optionally comprise additives usual in polymer powders used in 3D printing by sintering.
[0144] These may include additives, in powder form or not, which contribute to improving the behavior of the powder in 3D printing by sintering and those making it possible to improve the properties of the printed articles, in particular the mechanical properties, and in particular the elongation at break and the impact resistance.
[0145] These usual additives can in particular be chosen from flow agents, fire-resistant agents, flame retardants, anti-UV agents, anti-oxidant agents, anti-abrasion agents, light stabilizers, impact modifiers, anti-static agents, pigments and waxes.
[0146] By way of example, the flow agent may be chosen, for example, from silicas, in particular hydrophobic fumed silica, such as the product sold under the name Cab-o-Sil® TS610 by Cabot Corporation, precipitated silica, hydrated silica, vitreous silica, fumed silica, vitreous oxides, in particular vitreous phosphates, vitreous borates, alumina, such as amorphous alumina.
[0147] The antioxidant agent may comprise a phenolic compound, such as 3,3'-Bis(3,5-di-tert-butyl-4-hydroxyphenyl)-N,N'-hexamethylenedipropionamide marketed in particular under the name Palmarole® AO.OH.98 by Palmarole, (4,4'-Butylidenebis(2-t-butyl-5-methylphenol) marketed in particular under the name Lowinox® 44B25 by Addivant, Pentaerythritol tetrakis(3-(3,5-di-tertbutyl-4-hydroxyphenyl)propionate) marketed in particular under the name Irganox® 1010 by BASF, N,N'-hexane-1,6-diylbis(3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)) marketed in particular under the name Irganox® 1098 by BASF, 3,3',3',5,5',5'-hexa-tert-butyl-a,a',a'-(mesitylene-2,4,6-triyl) tri-p-cresol marketed in particular under the name Irganox® 1330 by BASF, Ethylenebis(oxyethylene)bis-(3-(5-tert-butyl-4-hydroxy-m- tolyl)propionate) marketed in particular under the name Irganox® 245 by BASF, l,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-l,3,5-triazine-2,4,6(lH,3H,5H)-trione marketed in particular under the name Irganox® 3114 by BASF, N'N'-(2 ethyl-2'ethoxyphenyl)oxanilide marketed in particular under the name Tinuvin® 312 by BASF, Phenol 4,4',4"-trimethyl- 1,3,5-benzenetriyl) tris-(methylene)] tris 2,6-bis(l,l-dimethylethyl) marketed in particular under the name Alvinox® 1330 by 3V, Hostanox® 245 FF, Hostanox® 245 Pwd, marketed by Clariant, Pentaerythritol Tetrakis (3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) marketed in particular under the names Evernox® 10, Evernox® 10GF, by Everspring Chemical, Company Limited, Octadecyl-3-(3,5-di-tert-4-hydroxyphenyl)-propionate marketed in particular under the names Evemox® 76, Evernox® 76GF by Everspring Chemical Company Limited, Tetrakis [Methylene-3(3',5'-di-tert-butyl-4-hydroxyphenyl) propionate] methane marketed in particular under the name BNX® 1010 by Mayzo, Thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] marketed in particular under the name BNX® 1035 by Mayzo, Tetrakis [Methylene-3 (3',5'-di-tert-butyl-4-hydroxyphenyl)propionate] methane, Octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate marketed in particular under the name BNX® 2086 by Mayzo, l,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-l,3,5-triazine-2,4,6(lH,3H,5H)trione marketed in particular under the name BNX® 3114 by Mayzo.
[0148] The antioxidant agent may also comprise a phosphate compound, such as the product Hostanox® P-EPQ® marketed by Clariant.
[0149] The pigment may be a pigment having an absorbance of light with a wavelength of 1000 nm, as measured according to ASTM E1790, of less than 40%, for example selected from metal and transition metal oxides and their corresponding mixtures, mixed oxides, and doped oxides. For example, an oxide selected from titanium, tin, magnesium, copper, zinc, iron, manganese, cobalt, nickel, aluminum, antimony, chromium, titanium, silicon or a corresponding mixture, mixed oxide, or doped oxide.
[0150] The wax may comprise a wax of polyethylene and polypropylene, polytetrafluoroethylene, ketones, acid, partially esterified acid, acid anhydride, ester, aldehydes, amides, their derivatives as well as their mixtures. The wax may in particular comprise a product marketed under the name Crayvallac® WN1135, WN 1495 or WN1265 by ARKEMA or a product marketed under the name Ceridust® 9615A or 8020 marketed by CLARIANT.
[0151] According to a particular embodiment, the wax is present in the powder in the form of a coating at least partially covering the polymer composition. Polymer powder
[0152] The powder according to the invention comprises a polymer composition (a) comprising at least one thermoplastic polymer, preferably a thermoplastic elastomer, and optionally fillers or reinforcements (component (b)) and / or one or more additives (component (c)).
[0153] According to one embodiment, the powder according to the invention comprises: (a) 30 to 99%, preferably 40 to 95%, in particular 50 to 90% and most particularly 70 to 85% by weight of a thermoplastic polymer composition; (b) 0 to 70%, preferably 10 to 50%, and in particular 20 to 30% by weight of one or more fillers or reinforcements; and (c) 0 to 10%, preferably 0.1 to 7.5%, in particular 1 to 5% by weight of one or more additives, the respective proportions of components (a), (b) and (c) adding up to 100%.
[0154] According to one embodiment, the polymer composition (a) comprises at least one thermoplastic elastomer as described above.
[0155]
[0156] The powder according to the invention, to be suitable for 3D printing by sintering, will have a suitable particle size distribution.
[0157] Typically, the polymer powder according to the invention has a diameter Dv50 of 40 to 150 pm, and preferably of 50 to 100 pm. For example, the diameter Dv50 of the polymer powder may be 40 to 45 pm; or 45 to 50 pm; or 50 to 55 pm; or 55 to 60 pm; or 60 to 65 pm; or 65 to 70 pm; or 70 to 75 pm; or 75 to 80 pm; 80 to 85 pm; or 85 to 90 pm; or 90 to 95 pm; or 95 to 100 pm; or 100 to 105 pm; or 105 to 110 pm; or from 110 to 115 pm; or from 115 to 120 pm; or from 120 to 125 pm; or from 125 to 130 pm; or from 130 to 135 pm; or from 135 to 140 pm; or from 140 to 145 pm; or from 145 to 150 pm.
[0158] The polymer powder according to the invention may have a Tm of 100 to 300°C, and preferably of 120 to 200°C.
[0159] The powder may have a Te of 40 to 250°C, and preferably of 45 to 200°C, for example of 45 to 150°C.
[0160] When composition (a) comprises several polymers, we consider as Tf, the lowest Tf in the mixture, and as Te, the highest Te in the mixture.
[0161] The difference between the Te and the Tf of the powder is preferably greater than or equal to 20°C, or more preferably greater than or equal to 30°C. Process for preparing the powder
[0162] The polymer powder can be manufactured according to the usual methods.
[0163] The polymer compositions useful in the present invention are commercially available, in particular in the form of granules, flakes or powder. If necessary, component (a) can be transformed into powder, by means of known methods, in particular by grinding.
[0164] Preferably, the grinding is cryogenic grinding. In this method, the material to be ground is cooled below the thermoplastic polymer glass transition temperature, for example by means of liquid nitrogen, liquid carbon dioxide or liquid helium. The grinding can be carried out for example in a counter-rotating pin mill, a hammer mill or in a grinder whirl mill.
[0165] The grinding can be carried out before and / or after bringing the polymer into contact with the various additives, namely components (b), and (c).
[0166] Components (b) and (c) are mostly available in powder form.
[0167] One or more additives (component (c)) may be added to the composition of polymer (component (a)) before grinding, in particular by adding one or more additives to the molten polymer, for example in an extruder (compounding).
[0168] Alternatively or in addition, one or more additives and fillers and reinforcements may be added after grinding, for example by dry blending. Furthermore, it is possible to mix the components by means of coprecipitation of the polymer composition from a solution in the presence of the component(s) (dissolution / precipitation).
[0169] The powder thus obtained can then be sieved or subjected to a selection step to obtain the desired particle size profile.
[0170] Before use, the polymer powder can then be subjected to different treatments, in particular thermal or hydraulic treatments, so that it is better suited to 3D printing by sintering. Powder sintering process
[0171] The polymer powder as described above is useful in particular for use in a 3D printing process by sintering. The powder of the invention can be used in a selective laser sintering (SLS) process, a sintering process of the MJF (Multi Jet Fusion) type or a sintering process of the HSS (High Speed Sintering) type.
[0172] The SLS process is widely known. In this context, reference may be made in particular to documents US 6,136,948 and WO 96 / 06881.
[0173] In this type of process, a thin layer of powder is deposited on a horizontal plate held in an enclosure heated to a temperature called the build temperature. The build temperature refers to the temperature to which the powder bed, of a constituent layer of a three-dimensional article under construction, is heated during the layer-by-layer sintering process of the powder. Electromagnetic radiation, for example in the form of a laser, subsequently provides the energy necessary to sinter the powder particles at different points of the powder layer according to a geometry corresponding to an object, for example using a computer having in memory the shape of an object and restoring the latter in the form of slices. Then, the horizontal plate is lowered by a height corresponding to the thickness of a layer of powder, and a new layer of powder is spread, heated and then sintered in the same way.The procedure is repeated until the object is manufactured.
[0174] The layer of powder deposited on a horizontal plate may have, before sintering, for example a thickness of 50 to 300 μm, and preferably 80 to 220 μm. After sintering, the thickness of the layer of agglomerated material is a little lower, and may have for example a thickness of 20 to 200 μm, and preferably 30 to 150 μm.
[0175] For the MJF and HSS process, the entire layer of the build material is exposed to radiation, but only a portion covered with a fusing agent is melted to become a layer of a 3D part. The fusing agent is selectively applied in the selected region of the build material. The fusing agent is able to penetrate the layer of the build material and transmits the absorbed energy to the neighboring build material, thereby causing it to melt or be sintered. By melting, bonding, and subsequent hardening of each layer of the build material, the object is formed.
[0176] Advantageously, the use of the polymer powder of the invention in these processes does not require any particular modification of the equipment.
[0177] The powder composition according to the invention makes it possible to manufacture good quality printed parts, having good mechanical properties and precise and well-defined dimensions and contours.
[0178] The polymer powder according to the invention can be recycled and reused in several successive constructions. It can, for example, be used as it is or in a mixture with other recycled or non-recycled powders.
[0179] The following examples illustrate the invention without limiting it. EXAMPLE
[0180] Each polymer used (with the exception of Example C) was obtained by grinding the corresponding granules in a cryogenic mill with counter-rotating spindles.
[0181] A polymer powder is obtained having a particle size distribution measured according to the ISO 13320 standard, characterized by a DvlO of 30 pm, a Dv50 of 90 pm and a Dv90 of 175 pm.
[0182] In a Henschel IAM 6L mixer, the polymer powder prepared with different additives is introduced by dry mixing.
[0183] The different powders have been presented below.
[0184] [Tables 1] Example Polymer composition Hydrophobic fumed silica Amide wax Tf (°C) A (comparative) 97.7% PA12-PTMG 1000 g / mol-1000 g / mol 0.3% 2.0% 147 B (comparative) 97.7% PA 11-PTMG 1000 g / mol-1000 g / mol 0.3% 2.0% 157 B' (comparative) 97% PA 11-PTMG 1000 g / mol-1000 g / mol 1.0% 2.0% 157 C (comparative) A thermoplastic polyurethane powder, marketed under the name Ultrasint® TPU 88A (BASF) at 100% 168 D 97.7% PA 11 / 12 (mass concentration 90% / 10%) -PTMG 1000 g / mol - 1000 g / mol 0.3% 2.0% 149 E 97.7% PA 11 / 12 (mass concentration 70% / 30%) -PTMG 1000 g / mol - 1000 g / mol 0.3% 2.0% 134 E' 97% PA 11 / 12 (mass concentration 70% / 30%) -PTMG 1000 g / mol - 1000 g / mol 1.0% 2.0% 134 F 97.7% PA 11-PTMG 650 g / mol - 650 g / mol 0.3% 2.0% 144
[0185] The polymer powder thus obtained is then used to print by laser sintering an IB XY specimen according to the ISO 527-1B standard on a Prodways P1000 machine at a powder bed temperature equal to Tf - 30°C by 3D printing by laser sintering.
[0186] The laser conditions used are the same for all prints.
[0187] During construction, the temperature of the powder on the surface of the construction tray is imposed, and measured at the surface by means of an infrared thermal sensor.
[0188] The specimens thus obtained are then characterized in terms of their mechanical properties. More specifically, the elongation at break of the specimens is measured on an INSTRON 5966 machine according to the ISO 527-2 standard. The elongation at break indicated corresponds to the average of the elongation at break measured for 5 printed IB XY specimens.
[0189] [Tables2] Examples G"1 (Pa) G"2 (Pa) G"2 / G"1 Elongation at break in XY (%) 3D Elongation at break in XY (%) Injection A (comparative) 19159 57604 3.01 300 >400 B (comparative) 11362 34254 3.01 240 >400 B' (comparative) 11362 34254 3.01 240 >400 C (comparative) 1820 5933 3.26 270 >400 D 27826 72469 2.60 >400 >400 E 54210 126659 2.34 >400 >400 E' 54210 126659 2.34 >400 >400 F 13411 37520 2.80 >400 >400
[0190] It is observed in the table that the powders having a G"2 / G"1 value lower than 3.00, have a better result in XY elongation at break test, comparable with the results obtained on the parts prepared, from the same powder, by injection in standard conditions in injections in ISO 527 - IB test molds, all these parts have elongations at break higher than 400%.
Claims
Claims
1. A polymer powder suitable for 3D printing by sintering, comprising: (a) a thermoplastic polymer composition; and optionally, (b) one or more fillers or reinforcements, (c) one or more additives, wherein the ratio G"2 / G"1 of said powder is less than or equal to 3.00, preferably less than or equal to 2.90, G" 1 being the loss modulus at the melting temperature (Tf) of the powder, when the powder is heated to Tf+40°C for 2 minutes and is then cooled to the Tf at a rate of -5°C / min, G"2 being the loss modulus at -30°C of the Tf of the powder, when the powder is heated to Tf+40°C for 2 minutes and is then cooled to the Tf-30°C at a rate of -5°C / min,, the values of G"2, G"1 being measured according to ISO 6721-10: part 10, at an angular frequency of 6.28 rad / sec.
2. Powder according to claim 1, in which the ratio G"2 / G"1 is less than or equal to 2.
80.
3. Powder according to claim 1 or 2, having a G"1 less than or equal to 100,000 Pa, preferably less than or equal to 50,000 Pa.
4. Powder according to one of claims 1 to 3, in which the polymer composition (a) has an enthalpy of fusion less than or equal to 60 J / g, preferably less than or equal to 55 J / g.
5. Powder according to one of claims 1 to 4, wherein the polymer composition (a) comprises at least one thermoplastic polymer selected from polypropylene (PP), polyolefin, polyamide (PA), polyester, polyarylether ketone (PAEK), polyphenylene sulfide, polyacetal, polyimide, vinylidene fluoride polymer and / or their mixture, preferably selected from PP, PA, and / or PAEK.
6. The powder of claim 5, wherein the polymer composition (a) comprises a polyarylether ketone (PAEK), selected from polyether ketone ketone (PEKK), polyether ether ketone (PEEK), polyether ketone (PEK), polyether ether ketone ketone (PEEKK), polyether ether ether ketone (PEEEK), polyether diphenyl ether ketone (PEDEK), mixtures thereof and / or copolymers thereof.
7. Powder according to one of claims 1 to 4, in which the com- polymer position (a) comprises a thermoplastic elastomer selected from the group consisting of SBS, SIS, SEBS, TPU, COPE and PEBA block copolymers and their blends and alloys.
8. The powder of claim 7, wherein the polymer composition (a) comprises a PEBA.
9. Powder according to claim 7 or 8, in which the polyamide blocks of the PEBA are copolyamide blocks, preferably chosen from the blocks PA 6 / 11, PA 6 / 12, PA 11 / 12, PA 6 / 11 / 12, PA 6 / 66 / 12, PA 6 / 1010, PA 6 / 1012, PA 6 / 1010 / 1012, PA 6 / 1012 / 12, PA 6 / 66 / 11 / 12, PA 6 / 1010 / 1012 / 1014, as well as their mixtures.
10. Powder according to claim 9, in which one of the monomers constituting the copolyamide represents more than 50%, preferably more than 60% by mass of the total mixture of monomers and / or less than 90%, preferably less than 80% by mass of the total mixture of monomers.
11. Powder according to claim 7 or 8, wherein the polyamide blocks in the PEBA result from the condensation of an α,α-aminocarboxylic acid or a lactam and the number-average molar mass (Mn) of the polyamide blocks in the PEBA is preferably 400 to 1500 g / mol, more preferably 500 to 1200 g / mol, preferably 500 to 1000 g / mol.
12. Powder according to claim 7, wherein the number average molar mass (Mn) of the polyester blocks in the COPE is 400 to 1500 g / mol, more preferably 500 to 1200 g / mol.
13. Powder according to claim 7, wherein the number average molar mass (Mn) of the PU blocks in the TPU is 400 to 1500 g / mol, more preferably 500 to 1200 g / mol.
14. Powder according to claim 1, having a diameter Dv50 as measured according to ISO 9276 - parts 1 to 6, of 40 to 150 pm.
15. A powder according to claim 1, comprising: (a) 30 to 99% by weight of a thermoplastic polymer composition; (b) 0 to 70% by weight of one or more fillers or reinforcements; and (c) 0 to 10% by weight of one or more additives, the respective proportions of components (a), (b) and (c) adding up to 100%.
16. A process for preparing a powder according to one of claims 1 to 15, comprising the steps of: (i) grinding a polymer composition (a) into a powder of a volume average diameter Dv50 of 40 to 150 pm, before or after, (ii) introduction of at least one or more fillers or reinforcements and / or one or more additives, where appropriate.
17. Use of a powder according to one of claims 1 to 15 for 3D printing by sintering, preferably chosen from the selective laser sintering (SLS) process, the MJF (Multi Jet Fusion) type sintering process and the HSS (High Speed Sintering) type sintering process.
18. Article obtained by 3D printing by sintering a powder as defined in claims 1 to 15.