Method for Preparing an Enzyme Master Mixture
The described process for preparing enzymized biodegradable plastics by simultaneous introduction and controlled mixing of enzymes, polysaccharides, and low melting point polymers addresses homogeneity and roughness issues, ensuring improved biodegradability and mechanical properties in the final products.
Patent Information
- Application Number
- FR2021007809
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-07-20
AI Technical Summary
Existing processes for preparing enzymized biodegradable plastic materials face issues with homogeneity and roughness, leading to altered physical and mechanical properties due to enzyme aggregation, which affects the aesthetics and performance of the final products.
A process involving the simultaneous introduction of enzymes in solution, polysaccharides, and a low melting point polymer in a mixer, followed by mixing at a temperature where the polymer is partially or completely melted, to enhance enzyme dispersion and maintain mechanical properties while improving biodegradability.
The process ensures homogeneous enzyme distribution, maintains mechanical properties, and enhances biodegradability of the plastic materials without roughness, resulting in improved performance and aesthetics of the final products.
Abstract
Description
Title of the invention: Process for the Preparation of an Enzyme Master Mix FIELD OF THE INVENTION.
[0001] The present invention relates to a method for preparing a masterbatch comprising a polysaccharide, enzymes and a low-melting polymer in a mixer. This masterbatch is used in particular for the manufacture of biodegradable plastic articles. BACKGROUND OF THE INVENTION.
[0002] Processes for preparing plastic materials based on biodegradable and biosourced polyesters have been developed in order to meet ecological challenges. These plastic products, synthesized from starch or starch derivatives and polyester, are used for the manufacture of articles with a short lifespan, such as plastic bags, food packaging, bottles, wrapping films, etc.
[0003] These plastic compositions generally contain polyester and flours from various cereals (US 5,739,244; US 6,176,915; US 2004 / 0167247; WO 2004 / 113433; FR 2 903 042; FR 2 856 405).
[0004] In order to control the degradation of these plastic products, the addition of additive(s) such as mineral fillers (WO 2010 / 041063) and / or biological entities having polyester degradation activity (WO 2013 / 093355; WO 2016 / 198652; WO 2016 / 198650; WO 2016 / 146540; WO 2016 / 062695) has been proposed.
[0005] Biodegradable plastic articles comprising biological entities, more particularly enzymes dispersed in a polymer, thus exhibit better biodegradability compared to plastic products lacking these enzymes.
[0006] Processes for preparing these enzymatic plastics have previously been described, however problems related to homogeneity and roughness may arise and have an impact on the physical properties of the product. For example, the presence of enzyme aggregates results in greater roughness, the aesthetics of the product are reduced and the physical and mechanical properties are altered.
[0007] A first improvement was made by adding the enzyme in liquid form to the support polymer (WO 2019 / 043145, WO 2019 / 043134).
[0008] The object of the invention is to facilitate and secure the industrial implementation of the masterbatch preparation process, in particular by simplifying the tools necessary for its implementation while retaining, or even improving, their performance. in terms of preservation of enzyme activity after formulation, and ability to be used in the preparation of final articles.
[0009] The present invention describes a method for preparing a masterbatch, which used in the manufacture of plastic products comprising enzymes dispersed in a polymer, makes it possible to improve the dispersion of the enzymes in the final compound as well as the rate of biodegradability of the plastic without modifying the mechanical properties of the product. BRIEF DESCRIPTION OF THE INVENTION.
[0010] The present invention relates to a process for preparing a masterbatch comprising a polysaccharide, enzymes and a carrier polymer in a mixer, said process comprising the following steps of: a. separate and simultaneous introduction a1) of the enzymes in solution, a2) of the polysaccharide and a3) of the support polymer b. mixing them at a temperature at which the carrier polymer is partially or completely melted and c. recovery of the master batch.
[0011] The invention also relates to the masterbatches thus obtained and to plastic articles obtained by mixing the masterbatch with a polymer or a mixture of polymers comprising a polymer capable of being degraded by the enzymes of the masterbatch.
[0012] It relates in particular to a process for preparing a plastic article comprising a polymer capable of being degraded by enzymes and enzymes capable of degrading said polymer, comprising a step of mixing the masterbatch according to the invention with said polymer, alone or as a mixture. DETAILED DESCRIPTION OF THE INVENTION.
[0013] The present invention relates to a process for preparing a masterbatch comprising a polysaccharide, enzymes capable of degrading polyesters and a support polymer in a mixer, said process comprising the following steps of: a. separate and simultaneous introduction of a liquid formulation of enzymes, the polysaccharide and the carrier polymer, b. and their mixing at a temperature at which the carrier polymer is partially or completely melted, and c. recovery of the master batch.
[0014] Unless otherwise indicated, the percentages are given by weight relative to the total weight of the composition to which they refer.
[0015] As used herein, the term "polysaccharides" refers to molecules composed of long chains of monosaccharide units linked together by glycosidic bonds. The structure of polysaccharides can be linear to highly branched. Examples include storage polysaccharides such as starch and glycogen, and structural polysaccharides such as cellulose and chitin. Polysaccharides include native polysaccharides or polysaccharides chemically modified by crosslinking, oxidation, acetylation, partial hydrolysis, etc.
[0016] Carbohydrate polymers can be classified according to their source (marine, plant, microbial, or animal), structure (linear, branched), and / or physical behavior (such as the designation as gum or hydrocolloid, which refers to the property that these polysaccharides hydrate in hot or cold water to form viscous solutions or dispersions of low gum or hydrocolloid concentration).
[0017] Within the scope of the invention, the polysaccharides can be classified according to the classification described in “Encapsulation Technologies for Food Active Ingredients and Food Processing - Chapter 3 - Materials for Encapsulation - Christine Wandrey, Artur Bartkowiak and Stephen E. Harding”: - Starch and derivatives, such as amylose, amylopectin, maltodextrin, glucose syrups, dextrin, cyclodextrin - Cellulose and derivatives, such as methylcellulose, hydroxypropylmethylcellulose, ethylcellulose, etc. - Plant exudates and extracts, also known as vegetable gums or natural gums, including, but not limited to, gum arabic (or acacia gum), gum tragacanth, guar gum, locust bean gum, karaya gum, mesquite gum, galactomannans, pectin, soluble soy polysaccharide - Marine extracts such as carrageenan and alginate - Microbial and animal polysaccharides such as gellan, dextran, xanthan, chitosan.
[0018] Polysaccharides can be classified according to their solubility in water. In particular, cellulose is not soluble in water. According to the invention, the polysaccharides have the ability to be soluble in water.
[0019] The polysaccharides used in the formulation of plastic compositions are well known to those skilled in the art. They are in particular chosen from starch derivatives such as amylose, amylopectin, maltodextrins, glucose syrup, dextrins and cyclodextrins, natural gums such as gum arabic, tragacanth gum, guar gum, locust beam gum, karaya gum, mesquite gum, galactomannans, pectin or soluble soy polysaccharides, marine extracts such as carrageenans and alginates, and microbial or animal polysaccharides such as gellans, dextrans, xanthans or chitosan, and mixtures thereof.
[0020] The polysaccharide can also be a mixture of several polysaccharides mentioned above.
[0021] In a preferred embodiment, the polysaccharide used is a natural gum, and more particularly gum arabic.
[0022] The enzymes used are enzymes having polyester degradation activity. Their incorporation into biodegradable plastic products based on polyesters thus makes it possible to improve the biodegradability of the latter.
[0023] Examples of enzymes having polyester degrading activity are well known to those skilled in the art, including depolymerases, esterases, lipases, cutinases, carboxylesterases, proteases or polyesterases.
[0024] Mention will in particular be made of enzymes capable of degrading polyesters so as to improve the biodegradability of the articles prepared with the masterbatch according to the invention. In a particular embodiment of the invention, the enzymes are capable of degrading PLA. Such enzymes and their method of incorporation into thermoplastic articles are known to those skilled in the art, in particular described in patent applications WO 2013 / 093355, WO 2016 / 198652, WO 2016 / 198650, WO 2016 / 146540 and WO 2016 / 062695.
[0025] The enzymes used in the context of the invention are in particular chosen from proteases and serine proteases. Examples of serine proteases are Proteinase K from Tritirachium album, or PLA-degrading enzymes from Amy-colatopsis sp., Actinomadura keratinilytica, Laceyella sacchari LP 175, Thermus sp., or Bacillus licheniformis or reformulated commercial enzymes known to degrade PLA such as Savinase®, Esperase®, Everlase® or any enzyme of the subtilisin family CAS [9014-01-1] or any functional variant.
[0026] The enzymes can be used in their pure or enriched form, and optionally as a mixture with one or more excipient(s).
[0027] In particular, the enzymes are chosen to be capable of degrading at least one polymer of a plastic article which will be obtained by the use of the masterbatch in its manufacturing process.
[0028] The enzymes are used in the method according to the invention in the form of a liquid formulation. A liquid formulation according to the invention is an enzymatic solution and / or a suspension of enzymes in a solvent, in particular a thick suspension, capable of flowing at room temperature. The liquid formulation must be in a form suitable for introduction into the mixer by any usual means for introducing a liquid formula into a mixer. The formulation can thus be introduced via an injector or a peristaltic pump. A person skilled in the art will be able to determine which device is most appropriate for adding the liquid formulation. mulation. In a preferred embodiment, the liquid formulation is introduced via a peristaltic pump. The solvent is a solvent that does not degrade enzymes, and more particularly water. According to one embodiment of the invention, the liquid formulation consists essentially of enzymes and the solvent, in particular water.
[0029] The form of the formulation will depend in particular on the enzyme content. It is understood that if the enzyme content exceeds the solubility threshold of the latter in the solvent, the formulation will comprise enzymes in suspension and will have the appearance of a thick composition, but nevertheless capable of flowing. According to an advantageous embodiment of the invention, the liquid enzyme formulation is an enzyme solution.
[0030] According to one embodiment, the liquid enzyme formulation comprises from 0.01 to 70% by weight of enzymes, in particular from 0.3 to 60% of enzymes, more particularly from 0.5 to 35% of enzymes. In particular, the enzyme formulation, in particular the enzyme solution, may comprise by weight an enzyme content of 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35% or more.
[0031] The support polymer is a low melting point polymer and a polymer which advantageously has a melting temperature below 140°C and / or a glass transition temperature below 70°C. It must also be compatible with the polymer(s) with which the masterbatch will be mixed for the preparation of enzymatic plastic articles.
[0032] Such support polymers are well known to those skilled in the art. These are in particular polycaprolactone (PCL), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), polydioxanone (PDS), polyhdroxyalkanoate (PHA), polylactic acid (PLA), or their copolymers. It may also be a natural polymer such as starch or a polymer that will be described as universal, that is to say compatible with a wide range of polymers such as an EVA-type copolymer.
[0033] Advantageously, the support polymer has a melting temperature of less than 120°C and / or a glass transition temperature of less than 30°C.
[0034] The support polymer is generally a single polymer as defined above. It may also consist of a mixture of these support polymers.
[0035] According to a particular embodiment of the invention, the support polymer is PCL.
[0036] According to a particular embodiment of the invention, the enzymes of the masterbatch are not capable of degrading the support polymer.
[0037] Step a) corresponds to the addition of the polysaccharide, the enzymes in liquid formulation and the support polymer in the mixer. The polysaccharide is in the form powder and is introduced into the mixer via a powder-specific dosing device. Liquid-formulated enzymes are added by any standard means of introducing a solution into a mixer or any other industrial means such as a peristaltic pump or an injector. In one embodiment, the liquid-formulated enzymes are added via a peristaltic pump. The carrier polymer is in the form of granules and is introduced into the mixer via a granule-specific dosing device.
[0038] According to a particular embodiment, the masterbatch is prepared by mixing: - 60-90% carrier polymer, especially PCL - 10-20% of liquid enzyme formulation, in particular of solution in enzyme - 2-15% polysaccharide, especially gum arabic
[0039] In one embodiment of the invention, the composition of the masterbatch comprises at most 5% of enzymes having polyester degradation activity. The content of liquid enzyme formulation, in particular enzyme solution, used in the manufacture of the masterbatch will therefore depend on the content of enzymes in its liquid formulation.
[0040] Advantageously, the liquid enzyme formulation / polysaccharide ratio is calculated so as to have a dry mass (enzymes and polysaccharide) of 30 to 70% of the mixture of the two.
[0041] The polysaccharide / enzymatic solution ratio is determined so as to have a dry mass of at least 30% and at most 55% or even at most 70%.
[0042] A person skilled in the art will know how to adapt the characteristics of the process (temperature and time) necessary for carrying out step a) depending on the components (polysaccharide, enzymes and support polymer) used.
[0043] The mixing of step b) is carried out at a temperature at which the support polymer is partially or completely melted. It is understood that the temperature of step b) will be determined by a person skilled in the art so that it does not alter the enzymes, and more particularly does not substantially reduce their enzymatic activity for degrading the support polymer. According to a particular embodiment, the temperature of step b) is a temperature less than or equal to the melting temperature (Tm) of the support polymer. A person skilled in the art will be able to choose the support polymer according to its melting temperature and the ability of the enzymes chosen to withstand this temperature in the process according to the invention. In a particular embodiment, the temperature of step b) is between the glass transition temperature (Tg) and the melting temperature (Tm) of the support polymer.Alternatively, the temperature of step b) is set at a temperature equal to or above the Tm of the support polymer.
[0044] Generally, the temperature of step b) may be between 40 and 200°C. In one embodiment, the temperature is greater than 40°C, or even greater than 50°C. The temperature is preferably between 55 and 175°C. In a preferred embodiment, the temperature of step b) is adjusted according to the nature of the polymer used. Thus, the temperature of step b) is generally at or corresponds to the melting temperature of the polymer used. Typically, the temperature does not exceed 300°C, more particularly, the temperature does not exceed 250°C.
[0045] It will be sought to maintain a temperature of the mixture in step b) which is as low as possible while allowing mixing and homogeneous dispersion of the enzymes and the polysaccharide in the support polymer.
[0046] In a particular embodiment, the support polymer is PCL and the temperature of the mixing step b) is approximately 60°C, from 55 to 65°C.
[0047] The mixing of the polysaccharide, enzyme and support polymer components in step b) is carried out for a period of 10 to 35 seconds. In a particular embodiment, the mixing lasts between 15 and 35 seconds, in particular about 20 seconds, about 25 seconds or about 30 seconds.
[0048] During the process of producing the masterbatch, the temperature is gradually increased in order to ensure a homogeneous and constant mixture while best preserving the characteristics and properties of each of the components.
[0049] Advantageously, the residence time of the polysaccharide / enzyme composition in the polymer at a temperature above 100°C within the mixer (step b)) is as short as possible. It is preferably between 5 seconds and 10 minutes. However, a residence time of less than 5 minutes is preferred. In a preferred embodiment, this is less than 3 minutes, and optionally less than 2 minutes.
[0050] The masterbatch obtained in step c) is in solid form. It is advantageously recovered in the form of granules. These granules can be stored, transported, and incorporated into the manufacture of plastic products or articles, whatever their form and use, which can be called "final products". These can be films, or flexible or solid parts of shapes and volumes adapted to their uses.
[0051] The masterbatch formulation may include a mineral filler. In this case, the mineral compound is introduced during step a), with the addition of the polysaccharide of the liquid enzyme formulation and the carrier polymer in the mixer.
[0052] Several minerals can be used. Examples are calcite, carbonate salts or carbonate metals such as calcium carbonate, potassium carbonate, magnesium carbonate, aluminum carbonate, zinc carbonate, copper carbonate, chalk, dolomite; silicate salts, such as calcium silicate, potassium silicate, magnesium silicate, aluminum silicate, or a mixture thereof, such as micas, smectites such as montmorillonite, vermiculite, and sepiolite-palygorskite; sulfate salts, such as barium sulfate or calcium sulfate (gypsum), mica; hydroxide salts or hydroxide metals such as calcium hydroxide, potassium hydroxide (potash), magnesium hydroxide, aluminum hydroxide, sodium hydroxide (caustic soda), hydrotalcite; metal oxides or oxide salts such as magnesium oxide, calcium oxide, aluminum oxide, iron oxide, copper oxide, clay, asbestos, silica, graphite, carbon black; metal fibers or metal petals; glass fibers; magnetic fibers; ceramic fibers and derivatives and / or mixtures thereof.
[0053] In a preferred embodiment, the mineral filler used is calcium carbonate.
[0054] Generally, the masterbatch is formulated with: - 60 to 90% of support polymer, in particular PCL, - 10 to 20% of liquid enzymatic formulation, in particular solution in enzyme, - 2 to 15% polysaccharide, in particular gum arabic and - 0 to 20% mineral filler, in particular calcium carbonate.
[0055] The masterbatch may also comprise the presence of one or more compounds. In particular, the masterbatch may comprise one or more additives. Generally, the additives are used to improve specific properties of the final product. For example, the additives may be chosen from plasticizers, coloring agents, processing aids, rheological agents, antistatic agents, anti-UV agents, reinforcing agents, compatibilizers, flame retardants, antioxidants, pro-oxidants, light stabilizers, oxygen scavengers, adhesives, products, excipients, etc.
[0056] Advantageously, the masterbatch comprises less than 20% by weight of additives and preferably less than 10% relative to the total weight of the masterbatch. In general, the composition of the masterbatch comprises from 0% to 10% by weight of additives relative to the total weight of the masterbatch.
[0057] The composition of the masterbatch after formulation comprises between 5% and 30% by weight of liquid enzyme formulation as defined above, relative to the total weight of the masterbatch. In one embodiment, the liquid enzyme formulation represents between 8% and 22% by weight relative to the total weight of the composition. In a preferred embodiment, the masterbatch comprises between 10% and 20% of liquid enzyme formulation, by weight of its composition.
[0058] The process for manufacturing the masterbatch is carried out in a mixer. Those skilled in the art know different types of mixers that can be used for manufacturing these polymer masterbatches.
[0059] In a preferred embodiment, the mixer is an extruder. This can be of the single-screw or twin-screw type. It is preferably of the twin-screw type.
[0060] In particular, the method is implemented in an extruder comprising at least 3 zones, a head zone where the first components are introduced, a mixing zone and an outlet zone through which the masterbatch is recovered, with the following steps a) to c): a. the separate and simultaneous introduction into the head zone of a polysaccharide, a liquid enzymatic formulation and a support polymer, and where appropriate a mineral filler, as defined above, b. mixing the components in the mixing zone at a temperature at which the carrier polymer is partially or completely melted, c. recovery of the master batch at the outlet of the extruder.
[0061] The person skilled in the art will be able to adapt the characteristics of the extruder (i.e. the length and diameter of the screw(s), the screw elements, the degassing zones, etc.) and the residence time of the polysaccharide, the enzymes and the support polymer according to the time and temperature constraints of the different stages of the process of the invention.
[0062] In particular, the temperature in the head zone is lower than the melting temperature of the support polymer and the temperature of the mixing zone is higher than the temperature of the head zone, in particular as defined above for the mixing temperatures.
[0063] The mixing zone may itself comprise several zones and those skilled in the art may, if necessary, adapt the temperatures of each zone, in particular depending on the enzymes and support polymers used.
[0064] The masterbatch can be obtained in the form of granules prepared according to usual techniques. These granules can be stored, transported and used in the manufacture of biodegradable plastic articles, which can be called "final articles".
[0065] When in the form of granules, the masterbatch can be dried for storage. The drying methods are standard methods known to those skilled in the art, in particular with the use of hot air ovens, vacuum ovens, desiccators, microwaves or fluidized beds. The drying temperature and its duration will depend on the one hand on the water content provided by the enzymatic solution in the preparation of the masterbatch, but also on the melting and glass transition temperatures of the support polymer used.
[0066] Once dry, the composition of the masterbatch advantageously comprises: - 60% to 95% of support polymer, - 0.5% to 7% enzyme, - 2% to 27% polysaccharide, and - 0% to 30% mineral charge.
[0067] The humidity level is generally 0.5% or less and preferably less than 0.3%.
[0068] The masterbatch obtained in the form of granules can then be used in the manufacture of biodegradable plastic products or “final articles”. These can be films, or flexible or solid parts of shapes and volumes adapted to their uses.
[0069] The biodegradable plastic article is obtained by mixing the masterbatch comprising the enzymes with at least one polymer capable of being degraded by said enzymes.
[0070] The invention therefore relates to a process for preparing a plastic article or a premix as defined below comprising a polymer capable of being degraded by enzymes and enzymes capable of degrading said polymer, said process comprising the steps of preparing a masterbatch comprising enzymes capable of degrading said polymer, a polysaccharide, and a support polymer, and optionally a mineral filler, the masterbatch being prepared in a mixer by a process comprising the following steps of: a. separate and simultaneous introduction into the mixer of the enzymes in liquid formulation, the polysaccharide and the support polymer, and where appropriate a mineral filler, as defined above b. mixing of components, and c. recovery of the master batch, then mixing said polymer capable of being degraded by enzymes with the masterbatch.
[0071] Advantageously, said polymer capable of being degraded by enzymes is a biodegradable polyester. These polyesters are well known to those skilled in the art, such as polylactic acid (PLA), polyglycolic acid (PGA), polyhydroxyalkanoate (PHA), polycaprolactone (PCL), polybutylene succinate (PBS), polybutylene succinate adipase (PBSA), polybutylene adipate terephthalate (PBAT), plasticized starch and mixtures thereof.
[0072] These polyesters are chosen for their physicochemical properties depending on the final article and the properties that will be sought, in particular its mechanical properties but also their color or their transparency.
[0073] The biodegradable polyesters used for the preparation of the final articles have identical or different physicochemical properties of the polyesters used as support polymers in the masterbatch according to the invention.
[0074] In a preferred embodiment, the enzyme-degradable polyester comprises PLA, alone or in a mixture with another polyester above, in particular a PLA / PBAT mixture.
[0075] The biodegradable plastic article is thus made up of the masterbatch and a biodegradable polymer.
[0076] The composition of the biodegradable plastic article comprises, in addition to the biodegradable polymer, from 0.5% to 20% of enzymatic masterbatch.
[0077] The methods for preparing these final articles are well known to those skilled in the art, including in particular the usual techniques of plastics processing such as extrusion-inflation, extrusion-blowing, cast film extrusion, calendering and thermoforming, injection molding, compression molding, rotational molding, coating, lamination, expansion, pultrusion, compression-granulation. Such operations are well known to those skilled in the art, who will easily adapt the process conditions according to the type of plastic articles intended (for example temperature, residence time, etc.).
[0078] For the preparation of biodegradable plastic articles, the masterbatch can be mixed with the other constituents of the composition for their shaping. It is also possible to prepare a premix or "compound" comprising the masterbatch and at least the biodegradable polymer. This premix in solid form, in particular in the form of granules, can be stored and then transported before being used for shaping the final article, alone or combined with other constituents depending on the final composition of the final article.
[0079] Advantageously, the premix comprises: - from 8% to 99% by weight of biodegradable polymer, preferably PLA, - from 0.01% to 5% by weight of a polysaccharide, preferably a natural gum such as gum arabic - from 0.1% to 20% by weight of a support polymer, as defined above, in particular PCL, and - from 0.01% to 2% by weight of enzymes having biodegradable polymer degradation activity, more particularly having PLA degradation activity, and where appropriate - from 0 to 35% by weight of mineral filler.
[0080] The final articles may be films, flexible or solid parts of shapes and volumes adapted to their uses. Examples of biodegradable plastic articles covered by the invention are films, mulching films, routing, food or non-food films; packaging such as packaging blisters, trays; disposable tableware such as cups, plates or cutlery; caps and lids; beverage capsules; and horticultural items.
[0081] Advantageously, the composition of the plastic article is as follows: - 60% to 98% by weight of biodegradable polymer or polymer blend(s), - 0.01% to 5% by weight of a polysaccharide, preferably a gum natural such as gum arabic, - 0.01% to 20% by weight of a support polymer, as defined above, - 0.01% to 2% by weight of enzymes having a degradation activity of biodegradable polymer, - 0% to 35% by weight of mineral filler, - 0% to 5% by weight of additives.
[0082] The biodegradable plastic articles obtained with the enzymatic masterbatch can be flexible and / or rigid.
[0083] In the case of flexible articles, the polyester capable of being degraded by enzymes comprises PLA. In one embodiment; the biodegradable polyester is a PBAT / PLA mixture whose weight ratio preferably ranges from 10 / 90 to 20 / 80, more preferably from 13 / 87 to 15 / 85.
[0084] In another embodiment, the biodegradable polyester is a PB AT / PLA blend whose weight ratio ranges from 10 / 90 to 30 / 70, from 10 / 90 to 40 / 60, from 10 / 90 to 50 / 50, from 10 / 90 to 60 / 40, from 10 / 90 to 70 / 30, from 10 / 90 to 80 / 20, from 10 / 90 to 90 / 10.
[0085] In another embodiment, the biodegradable polyester is a PB AT / PLA blend whose weight ratio is less than 10 / 90, equal to or less than 9 / 91, equal to or less than 8 / 92, equal to or less than 7 / 93, equal to or less than 6 / 94, equal to or less than 5 / 95, equal to or less than 4 / 96, equal to or less than 3 / 97, equal to or less than 2 / 98, equal to or less than 1 / 99.
[0086] In another embodiment, the biodegradable polyester is PLA.
[0087] The flexible biodegradable plastic articles are characterized by a thickness of less than 250 μm, preferably by a thickness of less than 200 μm. In a preferred embodiment, the films have a thickness of less than 100 μm, more preferably less than 50 μm, 40 μm or 30 μm, preferably between 10 and 20 μm. More preferably, the thickness of the flexible article is 15 μm. Examples are films, such as food films, routing films, industrial films or mulching films and bags.
[0088] Advantageously, the composition of the flexible article comprises: - from 70% to 98% by weight of biodegradable polymer or polymer blend gradable(s), - from 0.01% to 5% by weight of a polysaccharide, preferably a natural gum such as gum arabic, - from 0.1% to 20% by weight of a support polymer, as defined above, and - from 0.01% to 2% by weight of enzymes having a degradation activity of biodegradable polymer, - from 0% to 5% by weight of mineral filler, in particular from 0.01% to 5% by weight, in particular from 0.05 to 5% by weight, - from 0% to 5% by weight of additives.
[0089] The composition according to the invention is particularly suitable for the production of plastic films. The films according to the invention can be produced according to the usual methods of the art, in particular by extrusion-blowing. The films can be prepared from granules of composition according to the invention which are melted according to the usual techniques, in particular by extrusion.
[0090] The films of composition as defined above with enzymes may be single-layer or multi-layer films. In the case of a multi-layer film, at least one of the layers is of composition as defined above. The single-layer and multi-layer films, of composition as defined above, have both a high PLA content and retain mechanical properties as sought for the preparation of biodegradable and bio-sourced films, in particular for the packaging of food and non-food products. For this purpose, the constituents of the composition according to the invention will preferably be chosen from products compatible with food use.
[0091] The multilayer film may be a film comprising at least 3 layers, of type AB A, ABCA or ACBCA, the layers A, B and C being of different compositions. In a preferred embodiment, the multilayer films are of type ABA or ACBCA.
[0092] Generally, layers A and B comprise PLA and / or a polyester, advantageously of a composition according to the invention. Layers C, if present, are there to provide particular properties to the articles according to the invention, more particularly to provide barrier properties to gases and in particular to oxygen. Such barrier materials are well known to those skilled in the art, and in particular PVOH (polyvinyl alcohol), PVCD (polyvinyl chloride), PGA (polyglycolic acid), cellulose and its derivatives, milk proteins, or polysaccharides and their mixtures in all proportions.
[0093] In the case of multilayer films as defined above, and in particular ABA, ABCA or ACBCA type films, the enzymes may be present in all the layers or in only one of the layers, for example in layers A and B or only in layer A or in layer B.
[0094] According to a particular embodiment of the invention, the two layers A are made up of a composition according to the invention comprising PLA, polyester and polypropylene glycol diglycidyl ether (PPGDGE), without enzymes. The enzymes are in layer B, either in a composition according to the invention with enzymes as defined above, or in a particular composition, in particular an enzyme composition in a low-melting point polymer defined above.
[0095] Depending on the embodiments, the composition of the enzymatic layer of the flexible articles (mono- or multi-layer) may comprise up to 95% by weight of biodegradable polymer, preferably PLA. Thus, the enzymatic layer may comprise from 8% to 50%, from 8% to 60%, from 8% to 70%, from 8% to 80% or from 8% to 90% by weight of biodegradable polymer.
[0096] Advantageously, the composition of the enzymatic layer of the flexible articles (mono- or multi-layer) comprises: - from 8% to 95% by weight of biodegradable polymer, preferably PLA, in particular from 8% to 70%, from 8% to 60%, from 8% to 50%, or from 8% to 40%, - from 0.02% to 4% by weight of a polysaccharide, preferably a natural gum such as gum arabic, - from 0.1% to 19% by weight of a support polymer, as defined above, and - from 0.05% to 2% by weight of enzymes having a degradation activity of biodegradable polymer, more particularly having PLA degradation activity, and where appropriate - from 0 to 5% by weight of mineral filler, in particular from 0.01% to 5% by weight, in particular from 0.05% to 5% by weight.
[0097] Concerning rigid articles, the biodegradable polyester is PLA, preferably a PLA / calcium carbonate mixture whose weight ratio ranges from 100 / 0 to 25 / 75, preferably from 95 / 5 to 45 / 55, more preferably from 90 / 10 to 50 / 50. In another embodiment, the biodegradable polyester is a PB AT / PLA mixture whose weight ratio ranges preferably from 10 / 90 to 80 / 20, more preferably from 20 / 80 to 60 / 40.
[0098] The rigid articles have a thickness of between 200 μm and 5 mm, between 150 μm and 5 mm, preferably between 200 μm and 3 mm, or between 150 μm and 3 mm. In one embodiment, the articles have a thickness of between 200 μm and 1 mm, between 150 μm and 1 mm, preferably between 200 μm and 750 μm or between 150 μm and 750 μm. In another embodiment, the thickness is 450 μm.
[0099] Examples of such biodegradable plastic articles are cups, plates, cutlery, trays, beverage capsules and packaging blisters, more generally food or cosmetic packaging, or horticultural products.
[0100] Advantageously, the composition of the rigid article includes: from 60% to 95% by weight of biodegradable polymer or polymer blend(s), from 0.01% to 5% by weight of a polysaccharide, preferably a natural gum such as gum arabic, from 0.1% to 20% by weight of a carrier polymer, as defined above, from 0.01% to 2% by weight of enzymes having biodegradable polymer degradation activity, from 0% to 35% by weight of mineral filler, in particular 0.01 to 35% by weight, from 0% to 5% by weight of additives.
[0101] In another embodiment, the composition of the rigid article comprises: from 60% to 80% by weight of biodegradable polymer or polymer blend(s), from 0.01% to 5% by weight of a polysaccharide, preferably a natural gum such as gum arabic, from 0.1% to 20% by weight of a carrier polymer, as defined above, and from 0.01% to 2% by weight of enzymes having biodegradable polymer degradation activity, from 8% to 35% by weight of mineral filler, from 0% to 5% by weight of additives.
[0102] The composition of the rigid article thus comprises more than 60% by weight of biodegradable polymer or mixture of polymer(s), or even more than 70%, or even more than 80%, or even more than 90%.
[0103] The content of the mineral filler in the rigid article is between 0.01% and 35% by weight depending on the nature of the mineral filler.
[0104] According to embodiments, the rigid article thus comprises more than 0.01%, more than 0.1%, more than 1%, or even more than 2%, or even more than 3% by weight of mineral filler.
[0105] In other embodiments, the amount by weight of mineral filler is greater than or equal to 4%, greater than or equal to 5%, greater than or equal to 6%, greater than or equal to 7%, or greater than or equal to 8%.
[0106] In still other embodiments, the mineral filler included in the rigid article is 10 to 35% by weight, 15% to 30%, or 20% to 28% by weight.
[0107] Whether flexible or rigid, the final articles may also include plasticizers, compatibilizers and other usual additives used in the composition of plastic materials, such as pigments or colorants, release agents, impact modifiers, antiblock agents, etc.
[0108] Examples of plasticizers are citrate esters and oligomers of lactic acid (OLA).
[0109] Citrate esters are plasticizers known to those skilled in the art, in particular as bio-sourced materials. Mention will be made in particular of triethyl citrate (TEC), triethyl acetyl citrate (TEAC), tributyl citrate (TBC), tributyl acetyl citrate (TBAC). Preferably, the citrate ester used as plasticizer in the composition according to the invention is TBAC.
[0110] OLAs are also plasticizers known to those skilled in the art, in particular as biosourced materials. They are lactic acid oligomers with a molecular weight of less than 1500 g / mol. They are preferably esters of lactic acid oligomers, their carboxylic acid end being blocked by esterification with an alcohol, in particular a linear or branched Cl-CIO alcohol, advantageously a C6-C10 alcohol, or a mixture thereof. We will mention in particular the OLAs described in patent application EP 2 256 149 with their method of preparation, and the OLAs marketed by the company Condensia Quimica under the brand name Glyplast®, in particular the references Glyplast® OLA 2, which has a molecular weight of 500 to 600 g / mol and Glyplast® OLA 8 which has a molecular weight of 1000 to 1100 g / mol.According to a preferred embodiment of the invention, the OLAs have a molecular weight of at least 900 g / mol, preferably from 1000 to 1400 g / mol, more preferably from 1000 to 1100 g / mol.
[0111] Poly(propylene glycol) diglycidyl ethers are also called glycidyl ethers, described in particular as “reactive plasticizers” in patent application WO 2013 / 104743, used for the preparation of block copolymers with PLA and PB AT. They are also identified as liquid epoxy resin, from the company DOW, marketed under the reference “DER™ 732P”, or as aliphatic epoxy resin, from the company HEXION, marketed under the reference “Epikote™ Resin 877”.
[0112] The composition according to the invention may optionally comprise other PLA / Polyester compatibilizers associated with PPGDGE. Such PLA / Polyester compatibilizers are well known to those skilled in the art, in particular chosen from polyacrylates, terpolymers of ethylene, acrylic ester and glycidyl methacrylate (for example sold under the brand Lotader® by the company Arkema), PLA-PBAT-PLA triblock copolymers, PLA grafted with maleic anhydride (PLA-g-AM) or PB AT grafted with maleic anhydride (PBAT-g-AM), in particular poly(ethylene-co-methyl acrylate-co-glycidyl methacrylate) described in particular by Dong & al. (International Journal of Molecular Sciences, 2013, 14, 20189-20203) and Ojijo & al. (Polymer 2015, 80, 1-17), more particularly marketed under the name JONCRYL® by the company BASF, preferably the ADR 4468 grade. EXAMPLES.
[0113] Example 1: Use of the masterbatch in flexible articles
[0114] I. Preparation of a mixture of support polymer and enzymes
[0115] 1. Preparation of a masterbatch under state-of-the-art conditions
[0116] The mixture Al of carrier polymer and enzymes is prepared from granules of polycaprolactone (PCL), a polysaccharide (gum arabic), a mineral filler (calcium carbonate, CaCO3) and enzymes in solution. The mixture of support polymer and enzymes was manufactured using a Clextral Evolum 25 HT co-rotating twin-screw comprising 11 zones for which the temperature is independently controlled and regulated. The enzymes in solution, gum arabic and calcium carbonate were introduced simultaneously at the start of the extruder in order to achieve the mixture according to an increasing temperature profile between 25 and 50°C. The enzymes in solution were introduced at 2.6 kg / h using a peristaltic pump. The gum arabic was introduced at 1.4 kg / h using a specific powder feeder and the calcium carbonate was introduced at 2 kg / h. The PCL, also called support polymer, is introduced at 14 kg / h in a partially or completely molten state between zone 5 and zone 6 of the extruder at a temperature of 75°C.
[0117] Mixture A2 is made under the same conditions as mixture Al, on a different day.
[0118] The A3 mixture of carrier polymer and enzymes is prepared from polycaprolactone (PCL) granules, a polysaccharide (gum arabic), a mineral filler (calcium carbonate, CaCO3) and enzymes in solution. The mixture of carrier polymer and enzymes was manufactured with a Clextral Evolum 25 HT co-rotating twin-screw comprising 11 zones for which the temperature is independently controlled and regulated. The enzymes in solution, gum arabic and calcium carbonate were introduced simultaneously at the start of the extruder in order to achieve the mixture according to an increasing temperature profile between 25 and 50°C. The enzymes in solution are introduced at 2.2 kg / h using a peristaltic pump. The gum arabic is introduced at 1.8 kg / h using a specific powder dispenser and the calcium carbonate is introduced at 2 kg / h.The PCL, also called support polymer, is introduced at 14 kg / h in a partially or even completely molten state between zone 5 and zone 6 of the extruder at a temperature of 75°C.
[0119] The granulation of each mixture is done with an underwater cutter. The granules are dried at 45°C to 0.3% humidity.
[0120] 2. Preparation of a masterbatch according to the process of the invention
[0121] The mixture B1 of support polymer and enzymes is prepared from granules of polycaprolactone (PCL), a polysaccharide (gum arabic) and enzymes in solution according to the process of the invention.
[0122] The mixture of carrier polymer and enzymes was manufactured with a bi- CLEXTRAL EV25HT screw comprising 11 zones for which the temperature is independently controlled and regulated according to an increasing temperature profile between 25 and 50°C. The PCL is introduced at the top of the twin screw at 16kg / h, the enzymes in solution are introduced at 2.2kg / h using a peristaltic pump. The gum arabic is introduced at 1.8kg / h using a specific powder doser.
[0123] Mixture B2 is made under the same conditions as mixture B1, on a different day.
[0124] The mixture B3 of support polymer and enzymes is prepared from polycaprolactone (PCL) granules, a polysaccharide (gum arabic), a mineral filler (calcium carbonate, CaCO3) and enzymes in solution according to the process of the invention.
[0125] The mixture of support polymer and enzymes was manufactured with a CLEXTRAL EV25HT twin-screw extruder comprising 11 zones for which the temperature is independently controlled and regulated according to an increasing temperature profile between 25 and 60°C. The PCL is introduced at the top of the twin-screw at 14 kg / h, the enzymes in solution are introduced at 2.2 kg / h using a peristaltic pump. The gum arabic is introduced at 1.8 kg / h using a specific powder doser and the calcium carbonate is introduced at 2 kg / h.
[0126] II. Commercial products
[0127] In these examples, PCL marketed under the reference Capa™ 6500 by the company Perstorp, calcium carbonate marketed under the reference OMYAFILM 707-OG by the company Omya, gum arabic marketed under the reference InstantGum AA by the company Nexira were used.
[0128] A PLA / PBAT mix marketed under the reference ECO VIO F2223 by the company BASF was used.
[0129] III. Film production
[0130] For the inflation extrusion, a Labtech LF-250 laboratory line, 20mm width, 30 L / D screw type LBE20-30 / C was used. The screw speed is between 50 and 60 rpm, the top and bottom draw speeds are between 4.3 and 5.7 m / min.
[0131] The inflation extrusion temperatures are detailed in tables [3a], [3b] and [3c],
[0132] [Tables 3a]
[0133] Extrusion inflation temperatures for films 1 and 2 with the Al and A2 blends respectively. Zone ZI Z2 Z3 Z4 Line #1 Line #2 Temperature (°C) 150 150 150 150 155 150
[0134] [Tables 3b]
[0135] Extrusion inflation temperatures for films 4 and 5 with respectively the B1 and B2 mixtures. Zone ZI Z2 Z3 Z4 Line #1 Line #2 Temperature (°C) 125 165 155 155 160 160
[0136] [Tables 3c]
[0137] Extrusion inflation temperatures for films 3 and 6 with respectively the A3 and B3 mixes Zone ZI Z2 Z3 Z4 Line #1 Line #2 Temperature (°C) 135 145- 150 155 155 160 160
[0138] The films have an average thickness of 15 pm. The thicknesses were measured with a Positector electronic micrometer.
[0139] These films are transparent, without roughness and no passing defects were identified. The bubble was stable for all inflation extrusions. The opening of the film after inflation extrusion was described as standard, without difficulties.
[0140] IV. Method of analysis
[0141] The tensile and tear mechanical properties can be measured using a Zwick or Llyod type machine, equipped with a 50 N or a 5 kN sensor. The properties are measured in two different directions: longitudinally and transversely. The tensile and tear mechanical properties are measured according to EN ISO 527-3 and ISO 6383-1 respectively.
[0142] As for the resistance to perforation, it is measured using a Dart-Test according to the NF EN ISO 7765-1 standard.
[0143] The evaluation of the biodegradability of the films was evaluated with a depolymerization test carried out according to the following protocol: 100 mg of each sample were introduced into a plastic vial containing 50 mL of buffer solution at pH 8. The depolymerization is initiated by incubating each sample at 45°C, in an incubator shaken at 150 RPM. An aliquot of 1 mL of buffer solution is taken regularly and filtered using a 0.2 pm filter syringe in order to be analyzed by high performance liquid chromatography (HPLC) with an Aminex HPX-87H column to measure the release of lactic acid (LA) and its dimer. The chromatography system used is a Nexan Series, SHIMADZU HPLC machine comprising a pump, an automatic sampler, a column thermostated at 50°C and a UV detector at 220nm. The eluent is a 5 mM H2SO4 solution. The injection is 20 pL of sample. Lactic acid is measured from standard curves prepared from commercial lactic acid.
[0144] The hydrolysis of plastic films is calculated from the lactic acid and the released lactic acid dimer. The percentage of depolymerization is calculated with respect to the percentage of PLA in the sample.
[0145] V. Analysis results
[0146] Density of granules by pycnometry
[0147] The masterbatch A1 resulting from the preparation method described in paragraph L1a has a density equivalent to that of the masterbatch B1 resulting from the preparation method of the invention described in paragraph 1.2, namely 1.03 g / cm3 on average.
[0148] The masterbatch A2 resulting from the preparation method described in paragraph L1a has a density equivalent to that of the masterbatch B2 resulting from the preparation method of the invention described in paragraph L1.2, namely 1.05 g / cm3 on average.
[0149] The masterbatch A3 resulting from the preparation method described in paragraph L1a has a density equivalent to that of the masterbatch B3 resulting from the preparation method of the invention described in paragraph L1.2, namely 1.1 g / cm3 on average.
[0150] The method of preparing the polymer support and enzyme mixture has no impact on the density of the final compound.
[0151] Fluidity index measurements fMFI)
[0152] The masterbatch A1 resulting from the preparation method described in paragraph 1.1 has a fluidity index equivalent to that of the masterbatch B1 resulting from the preparation method of the invention described in paragraph 1.2, namely 10-10.5 for an analysis carried out at 160°C and 2.16 kg.
[0153] The masterbatch A3 resulting from the preparation method described in paragraph 1.1 has a fluidity index equivalent to that of the masterbatch B3 resulting from the preparation method of the invention described in paragraph 1.2, namely 10-10.5 for an analysis carried out at 160°C and 2.16 kg.
[0154] The method of preparing the polymer support and enzyme mixture has no impact on the fluidity of the final compound.
[0155] Thermogravimetric analyses
[0156] The thermogravimetric analyses carried out on these two mixtures prepared in paragraph I show that all the components of the formulation are found at equivalent decomposition temperatures.
[0157] [Tables 4]
[0158] Results of thermogravimetric analyses De-temperature Mixture Al 1.1 Mixture B 1.2 composition - 305°C - 6.8% - 7.6% - 390°C - 74.2% - 86% - 450°C - 8.5% -4% Residues - 10.6% - 2.9% Decomposition temperature Mixture A2 1.1 Mixture B2 1.2 - 300°C - 7.4% - 7.5% - 390°C - 72.4% -90% - 420°C -9.1% -0% Residues - 11.1% - 2.4% Decomposition temperature Mixture A3 1.1 Mixture B 3 1.2 - 300°C - 7.9% - 8.2% - 390°C - 70.6% - 70.4% - 450°C - 7.5% -7% Residues - 14.1% - 14%
[0159] The masterbatch formulations described in paragraphs 1.1 and 1.2 show compositional differences between compounds Al and B1; A2 and B2 as well as for A3 and B3. These differences are observed in terms of mass losses during thermogravimetric analysis.
[0160] Only masterbatches A3 and B3 have the same compositions and the mass losses do not show any significant differences depending on the process used.
[0161] Composition of films
[0162] The films were prepared with the polymer support and enzyme mixtures A1-A2-A3-B1-B2-B3 prepared in 1.1 and 1.2 and a grade based on PLA and PB AT marketed under the reference ECOVIO F2223 by the company BASF and named “Compound 1” in the examples below.
[0163] The compositions of these different films are listed in table [5].
[0164] [Tables 5]
[0165] Summary of the monolayer films produced Film composition Overall enzyme content (%) Film 1 Compound 1 + Mixture Al II.l >0.15% and identical to film 2 Film 2 Compound 1 + Mixture A2 II.l >0.15% and identical to film 1 Film 3 Compound 1 + Mixture A3 II.l >0.1% Film 4 Compound 1 + Mixture B1 II.2 > to the % of enzyme of films 1 and 2 and equivalent to film 5 Film 5 Compound 1 + Mixture B2 II.2 > to the % of enzyme of films 1 and 2 and equivalent to film 4 Film 6 Compound 1 + Mixture B3 II.2 >0.1% and identical to film 3
[0166] Film 1 serves as a reference of the state of the art for film 4 of the invention.
[0167] Film 2 serves as a reference of the state of the art for film 5 of the invention.
[0168] Film 3 serves as a reference of the state of the art for film 6 of the invention.
[0169] The manufacturing process of the mixture has no impact on the extrusion process. inflation. The process parameters of the extrusion inflation remain identical between the film of the technique and the invention. Regardless of the manufacturing process used, the appearance of the films is identical.
[0170] Mechanical properties of films 1 and 2
[0171] The mechanical properties measured on the film resulting from the technique and that resulting from the invention are presented in table [6]. The values indicated represent the average of all the measurements carried out.
[0172] [Tables 6]
[0173] Characterization of the mechanical properties of films Film 3 6 film density (g / cm3) film 1.23 1.23 thickness (pm) 12 11 Properties Direction of measurement Stress at break (%) SL 100% +0% ST 100% -7% Elongation at break (%) SL 100% -21% ST 100% +47% Young's Modulus (%) SL 100% +24% ST 100% +11% Tear Strength (%) ST 100% +0% (with SL = Longitudinal direction of the film and ST = Transverse direction of the film)
[0174] The mechanical properties thus measured show that the film described in the invention has mechanical properties maintained or even superior to the film of the technique.
[0175] Only the mechanical properties of films 3 and 6 were measured since the masterbatches used are of identical compositions, which facilitates their comparison on the finished products.
[0176] Depolymerization of PL A from films
[0177] Films 1 and 2 containing a polymer support and enzyme mixture manufactured under conventional conditions, and with the same enzyme level, have depolymerization results of between 34 and 38% after 20 days at 28°C. Films 4 and 5, containing a polymer support and enzyme mixture manufactured according to the process described in the invention and with the same enzyme level but lower than films 1 and 2, have depolymerization results of between 28% and 31%.
[0178] Films 3 and 6 with identical enzyme content and with MBs manufactured by both processes have a depolymerization rate of between 65% and 77% after 5 days at 45°C.
[0179] The addition of calcium carbonate to the composition of the polymer support and enzyme mixture promotes the depolymerization of the PLA. The process, for its part, has no negative impact on the performance of the enzymes in the masterbatch. The method of preparing the mixture described in the invention makes it possible to achieve depolymerization rates close to the conventional process but with fewer enzymes.
Claims
Claims
1. A process for preparing a masterbatch comprising a polysaccharide, enzymes capable of degrading polyesters and a support polymer in a mixer, characterized in that said process comprises the following steps of: a. separate and simultaneous introduction of a liquid enzyme formulation, the polysaccharide and the support polymer, b. their mixing at a temperature at which the support polymer is partially or completely melted, and c. recovery of the masterbatch after mixing.
2. Method according to claim 1, characterized in that the polysaccharide is chosen from starch derivatives, natural gums, soluble soy polysaccharides, marine extracts and microbial or animal polysaccharides, or their mixture in all proportions.
3. Method according to one of claims 1 or 2, characterized in that the polysaccharide is gum arabic.
4. Method according to one of claims 1 to 3, characterized in that the enzymes are added in the form of an aqueous solution.
5. Method according to one of claims 1 to 4, characterized in that the enzymatic formulation comprises 0.01 to 70% by weight of enzymes.
6. Method according to one of claims 1 to 5, characterized in that the enzymes are chosen from enzymes capable of degrading polyesters chosen from depolymerases, esterases, lipases, cutinases, carboxylesterases, proteases and polyesterases.
7. Method according to one of claims 1 to 6, characterized in that the support polymer is chosen from polycaprolactone (PCL), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), polydioxanone (PDS), polyhydroxyalkanoate (PHA) and polylactic acid (PLA) and mixtures thereof, preferably polycaprolactone (PCL).
8. Method according to one of claims 1 to 7, characterized in that the mixing in step b) is carried out between 10 and 35 seconds, advantageously between 15 and 35 seconds, in particular for approximately 20 seconds, approximately 25 seconds or approximately 30 seconds.
9. Method according to one of claims 1 to 8, characterized in that it comprises the simultaneous addition of a mineral filler in step a), in particular calcium carbonate.
10. Method according to one of claims 1 to 9, characterized in that the mixer is an extruder.
11. Method according to claim 10, characterized in that the extruder comprises at least 3 zones, a head zone where the first components are introduced, a mixing zone and an outlet zone through which the masterbatch is recovered, with the following steps a) to c): a. the separate and simultaneous introduction of a liquid enzyme formulation, a polysaccharide, a support polymer and optionally a mineral filler in the head zone, and their mixing at a temperature lower than or equal to the melting temperature of the support polymer, b. the mixing of the components in the mixing zone at a temperature at which the support polymer is partially or completely melted, and c. the recovery of the masterbatch at the outlet of the extruder.
12. Method according to one of claims 1 to 11, characterized in that the masterbatch is obtained in step c) in the form of granules.
13. A method according to claim 12, characterized in that the masterbatch granules are dried.
14. Method according to one of claims 1 to 13, characterized in that the formulation of the masterbatch contains: - 60 to 90% of support polymer, - 10 to 20% of enzymatic solution, - 2 to 15% of polysaccharide, - 0 to 20% of mineral filler.
15. A method of preparing a plastic article or a premix comprising a polymer capable of being degraded by enzymes and enzymes capable of degrading said polymer, characterized in that it comprises a step of preparing a masterbatch according to one of claims 1 to 14, and a step of mixing the masterbatch previously prepared with the polymer, the enzymes of the masterbatch being capable of degrading said polymer of the plastic article or premix.
16. A method according to claim 15, characterized in that the polymer capable of being degraded by enzymes in the plastic article or premix is polylactic acid (PLA).