6xxx alloy band and manufacturing process
A tailored aluminum alloy composition and manufacturing process enhance the stamping formability and mechanical properties of 6xxx series strips, addressing the limitations of existing alloys by improving LDH and yield strength, thus supporting efficient vehicle part production.
Patent Information
- Application Number
- FR2021012544
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-25
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-11-25
AI Technical Summary
Existing 6xxx series aluminum alloy strips used for automobile door skins lack sufficient stamping formability, particularly in terms of Limiting Dome Height (LDH), which hinders their widespread application in vehicle manufacturing.
A specific aluminum alloy composition with controlled amounts of Si, Mg, Cu, Fe, Mn, Ti, Cr, and Zn, combined with a manufacturing process involving semi-continuous casting, homogenization, hot rolling, cold rolling, solution quenching, and pre-tempering, to enhance formability and mechanical properties.
The alloy achieves improved stamping formability, as measured by LDH, while maintaining suitable yield strength and corrosion resistance, facilitating the production of vehicle parts with reduced weight and improved recyclability.
Smart Images

Figure 00000023_0000 
Figure 00000023_0001 
Figure 00000023_0002
Abstract
Description
Title of the invention: 6xxx alloy strip and manufacturing method Field of invention
[0001] The invention relates to the field of aluminum alloy strips intended for the manufacture by stamping of bodywork parts of the body in white of motor vehicles. State of the art
[0002] Aluminum alloys are increasingly used in automobile construction to reduce the weight of vehicles and thus reduce fuel consumption and greenhouse gas emissions.
[0003] Aluminum alloy strips are used in particular for the manufacture of numerous "body-in-white" parts, among which we distinguish on the one hand body skin parts (or exterior body panels) such as front wings, roofs or pavilions, hood, trunk or door skins. The manufacture of these parts requires an ability to stamp with high surface appearance requirements. On the other hand, linings (or interior body panels) have reduced surface appearance requirements but much higher requirements for stamping compared to body skin parts.
[0004] Michael Langille's thesis, defended at the University of Grenoble in 2019, studies the effects of Mg, Si and Cu additions on formability. Through the use of calorimetry and hardness testing, the state of the microstructure was revealed. The use of tensile tests and strain rate sensitivity tests made it possible to determine the mechanical properties in relation to the microstructure. The mechanical property parameters were then included in finite element simulations to understand their effects on the alloy formability. This thesis established a link between the composition, the microstructures for two different processing routes, the resulting mechanical properties and their influence on the final formability of these Al-Mg-Si-Cu alloys.
[0005] Application US20020005232 discloses an Al-Mg-Si-Cu aluminum alloy strip excellent in strength and formability and exhibiting improved filiform corrosion resistance, which is suitably used for automobile body panels. The aluminum alloy strip contains 0.25-0.6% Mg (mass %, hereinafter the same), 0.9-1.1% Si, 0.6-1.0% Cu, and at least one of 0.20% or less Mn and 0.10% or less Cr, with the remainder being Al and impurities, wherein the number of Q phases (Cu-Mg-Si-Al phases) with a size of 2 μm or more in diameter present in a matrix is 150 per mm2 or more. The aluminum alloy strip is manufactured by homogenizing an ingot of an aluminum alloy having the above composition at 530°C or more, cooling the ingot to 450°C or less at a cooling rate of 30°C / hour or less, hot rolling the ingot, cold rolling the hot-rolled product, and subjecting the cold-rolled product to a solution heat treatment.
[0006] Application US20020012605 discloses an aluminum alloy strip for an automobile with a chemical composition containing 0.8 to 1.5 mass% of Si, 0.4 to 0.7 mass% of Mg and 0.5 to 0.8 mass% of Cu. The crystal grain size is 10 to 40 pm. The Cu content obtained by analyzing the outermost surface of the aluminum alloy with an oxide film according to X-ray photoelectron spectroscopy (XPS) is 1 / 10 to / 2 of the Cu content of the core of the aluminum alloy plate.
[0007] Door linings, or interior panels, are often made with AA5182 alloy strips in the O state because this material has excellent stamping properties and these parts have few requirements in terms of surface finish. The skin of the doors, if it is made of aluminum, is always made of AA6xxx series alloys thanks to their excellent surface appearance property. Given the difference in composition of these aluminum alloys, recycling the doors of end-of-life vehicles is difficult. There is therefore a need to produce door linings made of AA6xxx alloy having a stamping ability comparable to that of FAA5182 in the O state. The 6xxx series alloys generally have a higher yield strength than that of 5182 O. Replacing 5182 O with an alloy of the 6xxxx series can reduce the mass of the vehicle and therefore the vehicle's consumption. Problem posed
[0008] The problem to be solved is to develop a 6xxx series alloy strip with improved stamping formability compared to traditional alloys used for door skins such as AA6016, AA6005, AA6022 alloys. The Limiting Dome Height (LDH) characterizes the ability to deform during stamping. The LDH of alloy 6005 in the T4 temper is typically 25mm.
[0009] The invention aims to obtain an excellent compromise between all of the desired properties:
[0010] • The formability of the strip which is assessed in state T4 after maturation, the maturation corresponding to the duration of transport and storage between the quenching of the strip and its stamping in the form of a part. The formability is characterized with the LDH test and the elastic limit. The objective is to obtain an LDH for a strip of 1.2 mm comparable to that of a strip of 1.2mm in 5182 state O, or 28.0mm. It is also necessary to control the elastic limit to ensure that the shape is obtained during stamping with reasonable force. • The properties necessary for the use of the part on a motor vehicle which are assessed on the finished part, therefore after stamping the strip, painting and baking the paints. Baking the paints is also known to those skilled in the art as “bake hardening” because it allows at the same time the hardening, by tempering, of the stamped strip to obtain the properties necessary for the use of the part on a motor vehicle. The suitability for use on a motor vehicle is characterized here by the elastic limit of the strip after a deformation of 2% and a heat treatment of 185°C for 20 minutes, representative of the baking heat treatment of the paints. Industrially, baking the paints can last from 10 to 30 minutes at a temperature between 170 and 195°C. • Corrosion which is assessed on the sheet after maturation. Corrosion is characterized by an intergranular corrosion test of the strip and a heat treatment of 185°C for 20 minutes. Subject of the invention
[0011] An object of the invention is an aluminum alloy strip of composition, in % by weight:
[0012] If: 1.00- 1.50, Fe: <= 0.30, Mn <= 0.30, Mg: 0.20 - 0.44, Cu: 0.80-1.50, Ti: 0.03 - 0.15, Cr: <= 0.10, Zn: <=0.10, other elements: each <=0.05, together <=0.15, remainder: Al.
[0013] Another object of the invention is a method of manufacturing a rolled strip of aluminum alloy according to the invention comprising the steps of:
[0014] a. Casting of a plate, preferably by semi-continuous vertical casting, in alloy according to the invention, b. Homogenization of the plate at a homogenization temperature preferably between 500°C and 600°C, c. Transfer of the homogenized plate directly to the hot rolling mill, optionally after forced cooling, d. Hot rolling of the plate with a hot rolling start temperature of at least 350°C and a maximum of 550°C and a hot rolling end temperature of at least 250°C and a maximum of 450°C, to obtain a strip with a final hot rolling thickness of between 2.4 mm and 10 mm, e. Optionally cold rolling, f. Solution treatment and quenching g. Pre-income, h. Maturation.
[0015] Another object of the invention is a method of manufacturing a motor vehicle part comprising the successive steps:
[0016] a. Manufacture of the strip according to the invention, b. Shaping the strip, c. Assembly in one piece of a motor vehicle, preferably a motor vehicle door, with at least one other component, preferably in alloy 6xxx, preferably an alloy AA6016 or AA6005 or AA6022, this other component being preferably manufactured from a sheet metal, preferably by stamping, d. Heat treatment, preferably by baking the paints.
[0017] Another subject of the invention is a motor vehicle part, in particular a motor vehicle door, obtained by the method according to the invention. Description of figures
[0018] [Fig.l]: This figure shows a motor vehicle door lining. It shows in particular the depth of the stamping carried out.
[0019] [Fig.2]: This figure represents the tool for measuring the LDH of a strip.
[0020] [Fig.3]: This figure shows the results of an intergranular corrosion test.
[0021] [Fig.4]: This graph shows the LDH value as a function of Cu content
[0022] [Fig.5]: This graph shows the value of LDH as a function of the elastic limit at the T4 state of the tape.
[0023] [Fig.6]: This graph shows the yield strength with 2% elongation then annealing paints depending on the elastic limit in the T4 state of the strip.
[0024] [Fig.7]: This graph shows the maturation of the band.
[0025] [Fig.8]: This graph shows the bands with an LDH higher or lower than 28mm in a graph of Cu content versus Fe, Mn and Cr content. Description of the invention
[0026] All aluminum alloys referred to below are designated, unless otherwise stated, according to the rules and designations defined by the “Aluminum As society" in the "Registration Record Series" that it publishes regularly. Unless otherwise stated, the compositions are expressed in % by weight. The expression 1.4 Cu means that the copper content expressed in % by weight is 1.4%.
[0027] The metallurgical states in question are designated according to the European standard EN-515.
[0028] The static mechanical characteristics in tension, in other words the breaking strength Rm, the conventional elastic limit at 0.2% elongation Rp0.2, the elongation at necking Ag% and the elongation at break A%, are determined by a tensile test according to standard NF EN ISO 6892-1, the sampling and the direction of the test being defined by standard EN 485-1.
[0029] The work hardening coefficient n is evaluated according to the standard EN ISO 10275.
[0030] The modulus of elasticity is measured according to ASTM 1876.
[0031] The Lankford anisotropy coefficient is measured according to the EN ISO 10113 standard.
[0032] The bending angles, called alpha norm, are determined by bending test 3-points according to standard NF EN ISO 7438 and procedures VDA 238-100 and VDA 239-200 version 2017.
[0033] Unless otherwise stated, the definitions of standard EN 12258 apply
[0034] The LDH parameter is widely used for evaluating the drawability of strips. It has been the subject of numerous publications, including that of R. Thompson, “The LDH test to evaluate sheet metal formability - Final Report of the LDH Committee of the North American Deep Drawing Research Group”, SAE conference, Detroit, 1993, SAE Paper No. 930815. This is a drawing test of a blank blocked at the periphery by a rod. The blank-holding pressure is adjusted to prevent slippage in the rod. The blank, measuring 120 mm x 160 mm, is stressed in a mode close to plane deformation. The punch used is hemispherical. [Fig. 2] specifies the dimensions of the tools used to carry out this test. Lubrication between the punch and the strip is provided by graphite grease. The punch descending speed is 50 mm / min.The so-called LDH value is the value of the punch displacement at break, i.e. the limit depth of drawing. It actually corresponds to the average of three tests, giving a 95% confidence interval on the measurement of 0.2 mm.
[0035] The standard for measuring intergranular corrosion is ASTM-G110.
[0036] Ambient temperature is any temperature compatible with human work from 5 to 35°C.
[0037] The strip according to the invention is made of aluminum alloy consisting of the following elements:
[0038] If: Silicon is, with magnesium, the first alloying element of the aluminum-magnesium-silicon systems (AA6xxx family) to form the intermediate compounds Mg2Si or Mg5Si6 metal precipitates that contribute to the structural hardening of these alloys. Si is in excess of Mg, with the Si content being at least 0.50% higher than that of Mg. The purpose of this excess is to obtain good ductility necessary for forming the strip. The hardening obtained by Mg2Si or Mg5Si6 precipitates is not sufficient to obtain the mechanical properties and the addition of Cu is necessary as explained in the corresponding paragraph. The Si content is a minimum of 1.00% and a maximum of 1.50%, or 1.40% or 1.35% or 1.30% or 1.25% or 1.20% or 1.10%. In one embodiment, the Si content is at least 1.10% and at most 1.50%, or 1.40% or 1.35% or 1.30% or 1.25% or 1.20%. In another embodiment, the Si content is at least 1.20% and at most 1.50%, or 1.40% or 1.35% or 1.30% or 1.25%; this embodiment and in particular the range Si: 1.20 - 1.30% is a preferred embodiment.In yet another embodiment, the Si content is at least 1.25% and at most and at most 1.50%, or 1.40% or 1.35% or 1.30%. In yet another embodiment, the Si content is at least 1.30% and at most and at most 1.50%, or 1.40% or 1.35%. In yet another embodiment, the Si content is at least 1.35% and at most and at most 1.50%, or 1.40%. In yet another embodiment, the Si content is at least 1.40% and at most and at most 1.50%.
[0039] Fe: Iron is generally considered an undesirable impurity, so the maximum iron content is 0.30%. The presence of intermetallic compounds containing iron is generally associated with a decrease in local formability. Reducing the Fe content improves the formability measured with the LDH. However, very pure Fe alloys are expensive. An advantageous compromise is an Fe content less than or equal to 0.30% and greater than or equal to 0.05%. In one embodiment, the Fe content is less than 0.25% and the minimum Fe content is 0.05% or 0.10% or 0.15% or 0.20%, the range 0.10 - 0.25 being particularly advantageous. In another embodiment, the Fe content is less than 0.20% and the minimum Fe content is 0.05% or 0.10% or 0.15%. In yet another embodiment the Fe content is less than 0.15% and the minimum Fe content is 0.05% or 0.10%.
[0040] Mn: Manganese has a similar effect to iron through its contribution to common intermetallic precipitates. Decreasing the Mn content improves formability as measured with LDH. The Mn content is a maximum of 0.30% and a minimum of 0%, or 0.05%, or 0.10%, or 0.15%, or 0.20%, or 0.25%. In one embodiment, the Mn content is a maximum of 0.25% and a minimum of 0%, 0.05%, 0.10%, 0.15%, or 0.20%. In another embodiment, the Mn content is a maximum of 0.20% and a minimum of 0%, 0.05%, 0.10%, or 0.15%. In another embodiment, the Mn content is a maximum of 0.20% and a minimum of 0%, 0.05%, 0.10%, or 0.15%. lization, the Mn content is at most 0.15% and at least 0%, 0.05%, or 0.10%. In another embodiment, the Mn content is at most 0.10% and at least 0%, 0.05%.
[0041] Mg: Generally, the level of mechanical characteristics of alloys in the AA6xxx family increases with the magnesium content. Combined with silicon to form the intermetallic compounds Mg2Si or Mg5Si6, magnesium contributes to the increase in mechanical properties. However, the Mg content must be limited because it increases the yield strength too much in the T4 state, which increases the stamping force and makes this operation more difficult. The Mg content can be combined with that of Cu to obtain the right compromise of properties both in the T4 state, such as the yield strength or LDH, and in the state of use such as the yield strength after 2% elongation and then paint treatment. The Mg content is at least 0.20% and at most 0.44% or 0.42% or 0.40% or 0.38% or 0.36% or 0.34% or 0.32% or 0.30% or 0.25%. In one embodiment, the Mg content is at least 0.25% and at most 0.44% or 0.42% or 0.40% or 0.38% or 0.36% or 0.35% or 0.34% or 0.32% or 0.30%, the range 0.25 - 0.35% being particularly advantageous. In yet another embodiment, the Mg content is at least 0.30% and at most 0.44% or 0.42% or 0.40% or 0.38% or 0.36% or 0.34% or 0.32%. In yet another embodiment, the Mg content is at least 0.32% and at most 0.44% or 0.42% or 0.40% or 0.38% or 0.36% or 0.34%. In yet another embodiment, the Mg content is at least 0.34% and at most 0.44% or 0.42% or 0.40% or 0.38% or 0.36%. In yet another embodiment, the Mg content is at least 0.36% and at most 0.44% or 0.42% or 0.40% or 0.38%. In yet another embodiment, the Mg content is at least 0.36% and at most 0.44% or 0.42% or 0.40% or 0.38%. In yet another embodiment, the Mg content is at least 0.38% and at most 0.44% or 0.42% or 0.40%.In yet another embodiment, the Mg content is at least 0.40% and at most 0.44% or 0.42%. In another embodiment, the Mg content is at least 0.42% and at most 0.44%.
[0042] Cu: In alloys of the AA6000 family, copper is an element participating in hardening precipitation but it is known to degrade the corrosion resistance. As explained previously, it is necessary to add Cu to harden the strip. Surprisingly, the addition of Copper makes it possible to increase the formability of the strip characterized in LDH. Indeed, the person skilled in the art usually expects that hardening causes a reduction in elongation and drawability. The copper content is a maximum of 1.50% and a minimum of 0.80% or 0.85% or 0.90% or 0.95% or 1.00% or 1.10% or 1.20% or 1.30% or 1.40%. In one embodiment, the copper content is a maximum of 1.40% and a minimum of 0.80% or 0.85% or 0.90% or 0.95% or 1.00% or 1.10% or 1.20% or 1.30%. In another embodiment, the copper content is a maximum of 1.30% and a minimum of 0.80% or 0.85% or 0.90% or 0.95% or 1.00% or 1.10% or 1.20%. In another embodiment, the copper content is a maximum of 1.20% and a minimum of 0.80% or 0.85% or 0.90% or 0.95% or 1.00% or 1.10%. In another embodiment, the copper content is a maximum of 1.10% and a minimum of 0.80% or 0.85% or 0.90% or 0.95% or 1.00%. In another embodiment, the copper content is a maximum of 1.00% and a minimum of 0.80% or 0.85% or 0.90% or 0.95%. In another embodiment, the copper content is a maximum of 0.95% and a minimum of 0.80% or 0.85% or 0.90%. In another embodiment, the copper content is a maximum of 0.90% and a minimum of 0.80% or 0.85%, the range 0.80 - 0.90% is particularly preferred. In another embodiment, the copper content is a maximum of 0.85% and a minimum of 0.80%.
[0043] Ti: This element can promote solid solution hardening leading to the required level of mechanical characteristics and this element also has a favorable effect on ductility in service and corrosion resistance. In order to compensate for the presence of Cu in the strip alloy, a minimum Ti content of 0.03% is necessary to ensure corrosion resistance by limiting the depth of pitting in intergranular corrosion to 150 pm for the strip according to the invention after 20 minutes at 185°C. On the other hand, a maximum content of 0.15% for Ti is required to avoid the conditions of formation of primary phases during vertical casting, which have a detrimental effect on all of the claimed properties. In one embodiment, the minimum Ti content is 0.04% and the maximum content is 0.15%, or 0.14% or 0.13% or 0.12% or 0.11% or 0.10% or 0.09% or 0.08% or 0.07% or 0.06% or 0.05%.In another embodiment, the minimum Ti content is 0.05% and the maximum content is 0.15%, or 0.14% or 0.13% or 0.12% or 0.11% or 0.10% or 0.09% or 0.08% or 0.07% or 0.06%, the range Ti 0.05 - 0.15 is particularly advantageous. In another embodiment, the minimum Ti content is 0.06% and the maximum content is 0.15%, or 0.14% or 0.13% or 0.12% or 0.11% or 0.10% or 0.09% or 0.08% or 0.07%. In another embodiment, the minimum Ti content is 0.07% and the maximum content is 0.15%, or 0.14% or 0.13% or 0.12% or 0.11% or 0.10% or 0.09% or 0.08%. In another embodiment, the minimum Ti content is 0.08% and the maximum content is 0.15%, or 0.14% or 0.13% or 0.12% or 0.11% or 0.10% or 0.09%. In another embodiment, the minimum Ti content is 0.09% and the maximum content is 0.15%, or 0.14% or 0.13% or 0.12% or 0.11% or 0.10%. In another embodiment, the minimum content . in Ti is 0.10% and the maximum content is 0.15%, or 0.14% or 0.13% or 0.12% or 0.11%. In another embodiment, the minimum Ti content is 0.11% and the maximum content is 0.15%, or 0.14% or 0.13% or 0.12%. In another embodiment, the minimum Ti content is 0.12% and the maximum content is 0.15%, or 0.14% or 0.13%. In another embodiment, the minimum Ti content is 0.13% and the maximum content is 0.15%, or 0.14.
[0044] Cr: It can be added to refine the grains and stabilize the structure. Reducing the Cr content improves the formability measured with LDH. The Cr content is a maximum of 0.10%, preferably less than 0.05%.
[0045] Zn: The content is a maximum of 0.10% so as not to degrade the corrosion resistance. Since Zn is an additional element in aluminum alloys, it is advantageous to accept it for the purpose of recycling aluminum scrap and waste, particularly from end-of-life vehicles. Indeed, Zn is used in certain alloys of certain components such as brazed heat exchangers. In one embodiment, the Zn content is less than 0.05%. In another embodiment, Zn is one of the other elements. In another embodiment, the Zn content is a maximum of 0.03%.
[0046] The other elements are typically impurities whose content is kept below 0.05%, the whole being less than 0.15%, the remainder being aluminum.
[0047] The method of manufacturing the strips according to the invention comprises the casting of a plate, preferably by vertical semi-continuous casting, followed by its homogenization.
[0048] The plate is cast with an alloy according to the composition previously described. The preferred dimensions of the plates according to the invention are 200mm to 600mm thick, 1000 to 3000mm wide and 2000 to 8000mm long.
[0049] The homogenization of the plate is carried out at a homogenization temperature preferably between 500°C and 600°C. In one embodiment, the homogenization temperature is a maximum of 580°C and a minimum of 500°C, or 520°C, or 540°C, or 560°C. In another embodiment, the homogenization temperature is a maximum of 560°C and a minimum of 500°C, or 520°C, or 540°C, in particular the range between 540°C and 560°C is particularly advantageous. In one embodiment, the homogenization temperature is a maximum of 540°C and a minimum of 500°C, or 520°C. In one embodiment, the homogenization temperature is a maximum of 520°C and a minimum of 500°C.
[0050] The homogenization time is preferably at least 1 hour.
[0051] The homogenized plate is transferred directly to the hot rolling mill, i.e. without cooling to room temperature. In one embodiment, the hot rolling start temperature is the homogenization temperature, op- tionally a cooling of 5°C to 10°C can take place during the transfer between homogenization and the start of hot rolling. In another embodiment, the plate is cooled from the homogenization temperature to the start of hot rolling temperature by forced cooling. This forced cooling is preferably carried out with a direct cooling rate of at least 150°C per hour. Advantageously the direct cooling rate is at most 500°C / h. The cooling can typically be carried out by a machine such as that described by application WO2016012691. Preferably this cooling is done in two stages, one of spraying and the other of uniformization. Optionally, this cooling can be carried out in two passes in the machine such as that described by application WO2016012691.
[0052] The plate is then hot rolled.
[0053] The hot rolling start temperature is at least 350°C and at most 550°C or 530°C or 510°C or 490°C or 470°C or 450°C or 430°C or 410°C or 390°C or 370°C. In one embodiment, the hot rolling start temperature is at least 370°C and at most 550°C or 530°C or 510°C or 490°C or 470°C or 450°C or 430°C or 410°C or 390°C. In another embodiment, the hot rolling start temperature is at least 390°C and at most 550°C or 530°C or 510°C or 490°C or 470°C or 450°C or 430°C or 410°C. In another embodiment, the hot rolling start temperature is at least 410°C and at most 550°C or 530°C or 510°C or 490°C or 470°C or 450°C or 430°C. In another embodiment, the hot rolling start temperature is at least 430°C and at most 550°C or 530°C or 510°C or 490°C or 470°C or 450°C.In another embodiment, the hot rolling start temperature is at least 450°C and at most 550°C or 530°C or 510°C or 490°C or 470°C. In another embodiment, the hot rolling start temperature is at least 470°C and at most 550°C or 530°C or 510°C or 490°C. In another embodiment, the hot rolling start temperature is at least 490°C and at most 550°C or 530°C or 510°C. In another embodiment, the hot rolling start temperature is at least 510°C and at most 550°C or 530°C. In another embodiment, the hot rolling start temperature is at least 530°C and at most 550°C. In a preferred embodiment, the hot rolling start temperature is the homogenization temperature, optionally cooling of 5°C to 10°C may take place during the transfer between homogenization and the start of hot rolling.In another preferred embodiment, the hot rolling start temperature is obtained by cooling, described above, to 140, or 150°C or 160°C from the homogenization temperature.
[0054] At the end of hot rolling, the plate has been rolled into a strip with a final hot rolling thickness of 2.4 to 10 mm, preferably 3 to 7 mm. The end of hot rolling temperature is at least 250°C and at most 450°C or 430°C or 410°C or 390°C or 370°C or 350°C or 330°C or 310°C or 290°C or 270°C, the range of 250 C to 330°C is particularly preferred, especially when there has been forced cooling between homogenization and the start of hot rolling. In one embodiment, the hot rolling end temperature is at least 270°C and at most 450°C or 430°C or 410°C or 390°C or 370°C or 350°C or 330°C or 310°C or 290°C.In another embodiment, the hot rolling end temperature is at least 290°C and at most 450°C or 430°C or 410°C or 390°C or 370°C or 350°C or 330°C or 310°C, the range of 290°C to 390°C is particularly preferred especially when there is no forced cooling between homogenization and the start of hot rolling. In another embodiment, the hot rolling end temperature is at least 310°C and at most 450°C or 430°C or 410°C or 390°C or 370°C or 350°C or 330°C. In another embodiment, the hot rolling end temperature is at least 330°C and at most 450°C or 430°C or 410°C or 390°C or 370°C or 350°C. In another embodiment, the hot rolling end temperature is at least 350°C and at most 450°C or 430°C or 410°C or 390°C or 370°C.In another embodiment, the hot rolling end temperature is at least 370°C and at most 450°C or 430°C or 410°C or 390°C. In another embodiment, the hot rolling end temperature is at least 390°C and at most 450°C or 430°C or 410°C. In another embodiment, the hot rolling end temperature is at least 410°C and at most 450°C or 430°C. In another embodiment, the hot rolling end temperature is at least 430°C and at most 450°C.
[0055] Cooling between the start and the end of hot rolling results from the usual heat exchange of the plate with the air at ambient temperature in the factory, with the equipment of the hot rolling mill such as, for example, but not limited to, the conveyor cylinders or rollers as well as with the usual lubricating or cooling fluids.
[0056] The strip is then optionally cold rolled. Annealing can take place before or after cold rolling. Intermediate annealing can also take place between two cold rolling stages. Annealing can be done in a static furnace or in a continuous furnace.
[0057] The preferred thickness of the strip obtained after hot rolling, optionally after cold rolling, is between 0.2 mm and 6 mm, preferably between 0.7 to 3.2mm.
[0058] The strip is then solution-treated, preferably in a continuous furnace and then quenched. The solution-treating temperature is advantageously a maximum of 580°C and a minimum of 540°C or 550°C or 560°C or 570°C. In one embodiment, the solution-treating temperature is a maximum of 570°C and a minimum of 540°C or 550°C or 560°C. In one embodiment, the solution-treating temperature is a maximum of 570°C and a minimum of 540°C or 550°C or 560°C. In one embodiment, the solution-treating temperature is a maximum of 560°C and a minimum of 540°C or 550°C, the range from 540°C to 560°C is particularly preferred. In one embodiment, the solution temperature is a maximum of 550°C and a minimum of 540°C. The solution temperature duration is between 15 and 60s, preferably between 15 and 30°C. The quenching can be carried out with water or with air. The strip is then cooled to room temperature.Preferably, the strip is cooled only to the temperature of a surface treatment when a surface treatment, known to those skilled in the art, is applied directly after quenching and before pre-tempering. This surface treatment temperature is between 50 and 70°C.
[0059] Then the strip is pre-tempered preferably at a pre-tempering temperature between 50 and 100°C. In one embodiment, the pre-tempering temperature is between 80 and 90°C. In another embodiment, the pre-tempering temperature is greater than 65°C, preferably greater than 70°C, and preferably less than 90°C and more preferably less than 85°C. This embodiment makes it possible to increase the response to paint baking, which is the difference between the yield strength after 2% elongation then 20 minutes at 185°C and that in the T4 state. Preferably, this embodiment is combined with an Mg content of less than or equal to 0.34%. This Mg content allows a lower yield strength in the T4 state to facilitate the stamping of the strip while having a good response to paint baking.In one embodiment, the strip is maintained for 8 hours at the pre-tempering temperature and then cooled to room temperature. In a preferred embodiment, the pre-tempering is obtained by winding the strip at the pre-tempering temperature, the strip is not maintained at the pre-tempering temperature and then the coiled strip cools naturally to room temperature for a period of between 8 hours and 24 hours.
[0060] The strip in the T4 state then matures at room temperature for between 72 hours and 6 months.
[0061] The elastic limit of the strip in the T4 state must not be too high to avoid too much stress during stamping. The elastic limit of the strip in the T4 state must not be too low because otherwise the elastic limit after 2% of elongation then 20 minutes at 185°C would be insufficient for use on a vehicle. The strip advantageously has a yield strength of at least 110 MPa and at most 170 MPa or 150 MPa or 140 MPa. In one embodiment, the strip has a yield strength of at least 140 MPa and at most 170 MPa or 150 MPa. In one embodiment, the strip has a yield strength of at least 150 MPa and at most 170 MPa.
[0062] The invention is also a method of manufacturing a motor vehicle part comprising the successive steps:
[0063] a. Manufacturing of the strip according to the invention, b. Shaping of the strip, preferably by stamping, preferably into a motor vehicle door lining, c. Assembly in one piece of a motor vehicle, preferably a motor vehicle door, with at least one other component, preferably in alloy 6xxx, preferably an alloy AA6016 or AA6005 or AA6022, this other component being preferably manufactured from a sheet metal, preferably by stamping, d. Heat treatment, preferably by baking the paints.
[0064] The motor vehicle part undergoes the treatments known to those skilled in the art, in particular painting, then heat treatment, preferably by baking the paints, known to those skilled in the art as “bake hardening”.
[0065] The invention is also a motor vehicle part, in particular a motor vehicle door, obtained by the method according to the invention.
[0066] In one embodiment, the strip according to the invention and the automotive part, preferably the door, according to the invention has an elastic limit after 2% elongation then 20 minutes at 185°C, of at least 200 MPa, preferably 210 MPa, more preferably 220 MPa, and / or at most 270 MPa or 290 MPa or 310 MPa.
[0067] In one embodiment, the strip in the T4 state has an LDH preferably greater than 28.0 mm, measured at a thickness of 1.2 mm, to obtain the deformation necessary for stamping. Preferably, to obtain an LDH greater than 28.0 mm, the impurity content, consisting of Fe, Mn and Cr, (Fe + Mn + Cr) £ C + 0.454*Cw, where C is a constant equal to 0.10%, preferably 0.05%, more preferably 0.00%. This inequality shows that the invention makes it possible to adjust the Cu content as a function of the sum of the Fe, Mn and Cr contents, which can be assimilated to the purity of the metal used, while maintaining the LDH level. This ability to adjust the composition makes it possible to optimize other properties of the strip according to the intended use as described below in two embodiments.
[0068] In a particular embodiment of this embodiment, a low Cu content and a high purity (a low content of Mn, Fe and Cr) is advantageous for obtaining a strip with a low yield strength, easier to stamp. A low Cu content corresponds to a composition whose maximum value, among the aforementioned maximum values, is less than or equal to 1.00%, preferably 0.90%. A high purity of Fe, Mn and Cr corresponds to the aforementioned compositions of these elements which respect the inequality described above. The yield strength in the T4 state can be low, thus the aforementioned maximum is preferably less than or equal to 150 MPa, preferably 140 MPa after at most 10 days of maturation.This low yield strength in the T4 state can be compensated as explained previously by the Mg content and the pre-tempering temperature to obtain a higher yield strength after 2% elongation then 20 minutes at 185°C which is greater than 200 MPa, preferably greater than 220 MPa.
[0069] In another embodiment of this embodiment, a high Cu content is advantageous for recycling alloys with a high Fe, Mn and Cr impurity content and for obtaining high elastic limits after 2% elongation then 20 minutes at 185°C. A high Cu content corresponds to a composition whose minimum value, among the aforementioned minimum values, is greater than or equal to 1.00%. A high Fe, Mn and Cr impurity content corresponds to the aforementioned compositions of these elements whose sum of the maximum of these elements respects the inequality (Fe+Mn+Cr}^C + 0.454*Cu,. Examples
[0070] Foundry plates were cast by vertical semi-continuous casting according to the compositions in Table 1. Plates 1, 2, 3 and 4 are examples of the invention.
[0071] Plates 1 to 4 are industrial plates, 660mm thick for plates 1 and 2, and 525mm thick for plates 3 and 4.
[0072] Plates 5 to 9 are 50mm thick laboratory plates. Plate Si Fe Cu Mn Mg Cr Zn Ti 1 1.25 0.20 0.84 0.15 0.33 0.01 0.01 0.090 2 1.27 0.19 0.81 0.15 0.40 0.01 0.01 0.090 3 1.18 0.17 0.86 0.08 0.39 0.008 0.006 0.100 4 1.23 0.16 0.84 0.09 0.28 0.008 0.006 0.100 5 1.32 0.25 1.36 0.21 0.29 0.03 0.020 6 1.31 0.24 0.83 0.20 0.27 0.03 0.020 7 1.26 0.12 0.72 0.06 0.27 0.01 0.020 8 1.28 0.25 0.77 0.21 0.28 0.03 0.020 9 1.27 0.24 0 0.21 0.27 0.03 0.020
[0074] These foundry plates were then homogenized, hot rolled, cold rolled into strips which were solution treated and then quenched according to the parameters in Table 2 and Table 3. Plates 3 and 4 underwent cooling between leaving the homogenization and the start of hot rolling with a speed of 250°C / h.
[0075] [Tables2] Plate Homogenization Hot rolling time (h) Temperature (°C) T-input (°C) Exit thickness (mm) Exit temperature (°C) 1 44 550 545 6.4 342 2 68 550 544 3.6 342 3 3 560 412 4.0 279 4 3 560 408 4.0 271 5 8 550 550 3.9 300 6 8 550 550 3.9 300 7 8 550 550 3.9 300 8 8 550 550 3.9 300 9 8 550 550 3.9 300
[0076] The cold rolling parameters are given in Table 3. LAF Plate Exit thickness (mm) Reduction (%) 1 2.2 65% 2 1.0 72% 3 1.2 70% 4 1.2 70% 5 1.2 69% 6 1.2 69% 7 1.2 69% 8 1.2 69% 9 1.2 69%
[0078] Solution treatment and quenching were carried out according to the parameters in Table 4.
[0079] The quenching speed of the strips quenched in air was 30°C / s.
[0080] The strips were then solution-treated, quenched and pre-tempered according to Table 4. Strips 3 and 4 were cut into several pieces which underwent different treatments. Strips 1 and 2 were quenched to a temperature of 70°C, strips 3 and 4 were quenched to a temperature of 50°C. Strips 31, 41, 5, 6 7, 8, and 9 were quenched to a temperature of 25°C. Pre-tempering is carried out either by exposing the strip to a temperature for the duration of Table 4, or by winding the strip, the resulting coil cooling to room temperature of approximately 21°C in 24 hours. Solution treatment and pre-tempering quenching plate strip Temperature (°C) Time (s) quenching pre-tempering (°C) pre-tempering 1 1 547 27 Water 71 coil 2 2 550 25 Air 65 coil 3 30 548 19 Air 62 coil 3 31 550 60 water 80 8h 4 40 552 22 air 62 coil 4 41 550 60 water 80 8h 5 5 550 60 water 85 8h 6 6 550 60 water 85 8h 7 7 550 60 water 85 8h 8 8 550 60 water 85 8h 9 9 550 60 water 85 8h
[0082] Strips 6, 7, 30 and 40 were exposed to an intergranular corrosion test after 20 minutes at 185°C. The presence of Ti in strips 30 and 40 makes it possible to limit intergranular corrosion to a depth of less than 150pm compared to strips 6 and 7 as shown in [Fig.3]. State T4 BH band Maturatio n (day) R0.2 (MPA ) Rm (MPa) Ag (%) A50 (%) n4-6 (%) nl0-15 (%) rlO (%)% LDH (mm) R.02 1 3 130 263 24.3 30.7 0.30 0.28 0.5 32.6 244 2 6 140 291 25.2 29.0 0.30 0.29 1.2 264 30 8 132 277 27.5 29.9 0.30 0.30 1.5 28.3 235 31 10 139 290 27.0 32.1 0.30 0.30 1.4 28.0 255 40 8 122 264 26.0 28.0 0.30 0.29 1.6 28.5 202 41 10 117 265 25.1 32.1 0.32 0.31 1.5 28.3 224 5 10 153 304 25.7 29.6 0.31 0.30 0.6 28.6 226 8 10 138 279 24.4 28.1 0.32 0.29 0.6 27.4 225 9 10 115 236 21.8 26.3 0.30 0.26 0.5 26.1 209
[0084] Strips 1, 2, 30, 40, 5, 8 and 9 in the T4 state were characterized in formability with the LDH test as well as their mechanical property in Table 5. The last column is the R0.2 measured after 2% elongation then 20 minutes at 185°C. The LDH values are the average value of the measurement in the rolling direction and the measurement in the cross rolling direction. The other mechanical properties were measured in the cross rolling direction.
[0085] Figures 4 and 5 show these results in particular for strips 30, 40, 5, 8 and 9. The LDH of coils 5, 8 and 9 increases with the copper content which also causes the increase in the yield strength content of said strips. Strips 30 and 40 show that it is possible to almost reach the LDH of strip 5 despite a lower copper content. This improvement in the LDH is obtained by reducing the amount of Fe+ Mn + Cr from 0.49% to 0.26%. This also makes it possible to reduce the yield strength in the T4 state, which reduces the stamping forces and therefore facilitates the stamping operation.
[0086] Strip 1 has a thickness of 2.2mm. The LDH value of a strip of 5182 state O at 2.2mm being 30.5mm and that of 5182 state 0 at 1.2mm being 28.0mm, it can therefore be estimated that strip 2 has an LDH greater than 28.0mm if it had been measured at 1.2mm.
[0087] Graph 6 shows the impact on the compromise between the yield strength in the T4 state and the yield strength after 2% elongation and then baking the paints at 185°C for 20 minutes ("Bake Hardening"). A slightly lower Mg content decreases these yield strengths (band 30 compared to band 40). Increasing the pre-tempering temperature to 80°C increases the yield strength after 2% elongation and then baking the paints for 20 minutes at 185°C. This increase obtained on band 41 compared to band 40 makes it possible to almost obtain the yield strength after 2% elongation and then baking the paints at 185°C for 20 minutes of band 30 which has a higher Mg content of 0.11%.
[0088] Strips 30, 31, 40 and 41 have a low maturation as shown in Table 6 and [Fig.7], which allows to ensure the subsequent drawing of the strip despite the storage duration. This graph also shows that a lower Mg content allows to limit the yield strength in the T4 state during maturation, which is advantageous to ensure drawing.
[0089] [Tableauxô] Maturation (day) 3 8 10 30 40 60 90 180 R0.2 band (Mpa) at T4 state 1 130 139 2 140 142 151 158 30 132 142 31 139 140 144 40 122 129 41 117 122 135
[0090] Figure 8 shows in a graph of Copper as a function of purity (sums of Fe, Mn and Cr contents) the LDH results of bands 1, 30, 31, 40, 41, 5, 8 and 9. The straight line (Fe+Mn + Cr) < 0.454 *Cll, separates the bands whose LDH measured or estimated at a thickness of 1.2mm is greater than 28.0mm from those whose LDH is less than 28.0mm.
Claims
Claims
1. Aluminum alloy strip of composition, in wt%: Si: 1.00-1.50, Fe: <= 0.30, Mn: <= 0.30, Mg: 0.20-0.35, Cu: 0.80-1.50, Ti: 0.03%-0.15, Cr: <= 0.10, Zn: <=0.10, other elements: each <=0.05, together <= 0.15, remainder: Al.
2.
3. Strip according to claim 1 characterized in that Si: 1.20 - 1.
30. Strip according to claim 1 or 2 characterized in that Mg: 0.25 -0.
35.
4. Strip according to one of claims 1 to 3 characterized in that Cu 0.80-0.
90.
5. Strip according to one of claims 1 to 4 characterized in that Fe: 0.10-0.
25.
6. Strip according to one of claims 1 to 5 characterized in that Ti >= 0.
05.
7. Strip according to one of claims 1 to 6 characterized in that the elastic limit R 0.2 in state T4 is greater than 110 MPa and / or less than 170 MPa and / or the LDH is greater than or equal to 28.0 mm, measured at a thickness of 1.2 mm.
8. Strip according to one of claims 1 to 7 characterized in that the strip has an elastic limit after elongation of 2% then a heat treatment of 20 minutes at 185°C greater than or equal to 200 MPa and / or less than or equal to 310 MPa and / or the strip has a maximum depth of pitting in intergranular corrosion after a heat treatment of 20 minutes at 185°C less than 150 pm.
9. Method of manufacturing the strip according to claims 1 to 8 comprising the successive steps: a. Casting of a plate, preferably by semi-continuous vertical casting b. Homogenization of the plate at a homogenization temperature, between 500°C and 600°C for at least
10.
11.
12.
13. less 1 hour, c. Transfer of the homogenized plate directly to the hot rolling mill, optionally after forced cooling, d. Hot rolling of the plate with a hot rolling start temperature of at least 350°C and a maximum of 550°C and a hot rolling end temperature of at least 250°C and a maximum of 450°C, to obtain a strip with a final hot rolling thickness of between 2.4 and 10 mm, e. Optionally cold rolling, f. Solution treatment at a temperature of 540 to 580°C for a period of 15 to 60s and quenching, g. Pre-tempered between 50 and 100°C for 8 hours, h. Maturation. Manufacturing method according to claim 9 characterized in that the pre-tempering temperature is between 50 and 100°C, preferably between 65°C and 90°C if the Mg content is less than 0.34%. Method of manufacturing a motor vehicle part comprising the successive steps: a. Manufacture of the strip according to claim 9 or 10, b. Shaping the strip, c. Assembly in one piece of a motor vehicle, preferably a motor vehicle door, with at least one other component, preferably in alloy 6xxx, preferably an alloy AA6016 or AA6005 or AA6022, this other component being preferably manufactured from a sheet metal, preferably by stamping, d. Heat treatment, preferably by baking the paints. Motor vehicle part, in particular a motor vehicle door, obtained by the method according to claim 11. Motor vehicle part according to claim 12 characterized in that the elastic limit of the strip has an elastic limit R0.2 after an elongation of 2% and a heat treatment of 20 minutes at 185°C at a minimum of 200 MPa and / or a maximum of 310 MPa.