Decontamination process of natural rubber by filtration of a wet coagulum of natural rubber.
The process filters natural rubber coagulum through a grooved and fingered extruder without a gear pump, enhancing flow rate and reducing energy consumption, addressing the complexity and cost of existing methods.
Patent Information
- Application Number
- FR2022003534
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-04-15
AI Technical Summary
Existing natural rubber decontamination processes require the use of a gear pump to increase the flow rate of decontaminated rubber, making the devices more complex and costly.
A process that filters a wet coagulum of natural rubber through an extruder with grooved and fingered sheath, applying specific pressure and temperature conditions without a gear pump, using an extruder with grooves on its interior surface and fingers extending radially towards the sheath, and a filter at the outlet.
Increases the flow rate of decontaminated natural rubber and reduces energy consumption while eliminating the need for a gear pump, achieving up to 50% water loss and maintaining a residual water content of greater than 7% in the decontaminated rubber.
Smart Images

Figure 00000017_0000 
Figure 00000017_0001 
Figure 00000018_0000
Abstract
Description
Title of the invention: Process for decontaminating natural rubber by filtration of a wet coagulum of natural rubber.
[0001] The invention relates to a method for decontaminating natural rubber by filtration of a wet coagulum of natural rubber, which method makes it possible to remove contaminants present in the natural rubber.
[0002] Natural rubber containing a high cis polyisoprene matrix is a very widely used elastomer in the field of tires due to its remarkable properties. For example, it is used in rubber compositions intended for the manufacture of semi-finished tires for vehicles carrying heavy loads, due to the performance compromise it can bring to the tire. Indeed, the introduction of natural rubber into a rubber composition reinforced with a reinforcing filler such as carbon black gives the rubber composition a very interesting compromise in terms of hysteresis and wear which translates for the tire into a good performance compromise between endurance and tire wear.
[0003] Natural rubber comes from the dry rubbery matter of natural rubber latex, very often extracted from the rubber tree after bleeding: the latex is generally collected in a cup called a cup. According to a first coagulation process called spontaneous, the latex coagulates directly in the cup to form a coagulum called cup lump, a name well known to those skilled in the art in the field of natural rubber manufacturing. According to a second coagulation process called induced, the latex still liquid in the cup is transferred, possibly stabilized, then coagulated for example using a chemical agent.
[0004] The product of spontaneous or induced coagulation of natural rubber latex, hereinafter referred to as the coagulation product, comprises the polyisoprene matrix soaked in a serum. Very often, it also contains leaves, twigs, sand and other debris that contaminate the coagulum during harvesting. In traditional natural rubber manufacturing processes, the coagulum is generally cut and washed to remove larger contaminants (primary decontamination). To remove finer contaminants (secondary decontamination), the coagulum is also shredded into crumbs, then washed with water in pools, and then fed into creping machines.
[0005] It is also known from patent application WO 2016162645 A2 to remove the finest contaminants from a natural rubber by passing a wet coagulum of natural rubber through a device comprising an extruder and a filter installed at the outlet of the extruder at temperatures below 100°C. Patent application WO 2018224773 A1 also describes a method for filtering a wet coagulum of natural rubber, but at higher pressures, in particular above 100 bars. The devices implementing the filtration methods described in these two patent applications preferably include a gear pump to be able to increase the flow rate of decontaminated natural rubber. However, the need to use a gear pump in the decontamination process has the effect of complicating the device by adding an additional device between the extruder and the filter. There is an interest in having a method which makes it possible to increase the flow rate of decontaminated natural rubber without having to use a gear pump.
[0006] The Applicant, continuing its efforts, has developed a method for filtering a wet coagulum of natural rubber by passing it through an extruder which is novel and which makes it possible to increase the flow rate of decontaminated natural rubber without having to resort to a gear pump. This objective is achieved by applying specific pressure and temperature conditions to a wet coagulum of natural rubber in an extruder which comprises a barrel having grooves on its inner surface and fingers which extend radially towards the inside of the barrel and which are present in at least a portion of the barrel which extends from the end of the barrel closest to the outlet of the extruder.
[0007] Thus, an object of the invention is a process for preparing a decontaminated natural rubber, which comprises a decontamination step by passing a coagulum of natural rubber having a humidity level greater than 12% by weight, in a device comprising an extruder comprising a barrel and an endless screw, and a filter installed at the outlet of the extruder, the barrel comprising on its inner surface grooves which extend from the end of the barrel closest to the feed zone of the extruder, the extruder having fingers in the barrel which extend radially inward of the barrel relative to the axis of rotation of the screw and which are present at least in a portion of the barrel which extends from the end of the barrel closest to the outlet of the extruder, the pressure applied to the coagulum at the filter inlet ranging from 70 bars to 120 bars, the temperature of the coagulum at the filter inlet being greater than 130°C and less than 190°C. Detailed description
[0008] [Fig. 1] very schematically represents a device useful for the purposes of the invention. The device comprises an extruder (11) and a filter holder (12) (filter not visible in the figure). The extruder (11) comprises a feed hopper (111), a barrel (112) which is grooved and carries fingers, not shown in the figure, and a single screw (113) having an axis of rotation (XI13) and comprising a hub and a thread which extends radially outwardly relative to the hub. The inner surface (1121) of the barrel is also shown in [Fig.l]. At the extruder outlet, the system comprises one or more filters installed on a filter holder (12). The system comprises measuring means, in particular for measuring the pressures and temperatures (P, T).
[0009] [Fig.2] shows a sectional view of a grooved sheath. In the right part of the semicircle (marked A in the figure), the grooves (211) are dovetail-shaped. In the left part of the semicircle (marked B in the figure), the grooves (212) are crenellated. The grooves (211, 212) define ribs (221, 222).
[0010] [Fig. 3] schematically represents in three dimensions two consecutive grooves separated by a rib. The groove comprises - a bottom face (34) delimited by two bottom edges (332, 333), - two lateral faces (322, 323) extending inwardly from the bottom face (34), each being delimited by a bottom edge (332, 333) and an intersection edge (312, 313) with the inner surface of the sheath. The grooves define ribs whose upper faces (31), delimited by two intersecting edges (311, 312), constitute the inner surface of the sheath. In [Fig.3], the distance between two consecutive ribs is the distance between the two intersecting edges (312) and (313), represented by the double arrow. The distance between two grooves is the distance between the two intersecting edges (311) and (312). In [Fig.3], the minimum distance separating the bottom face (34) and the plane passing through the intersection edges (312) and (313) is represented by the highlighted double arrow.
[0011] Any range of values designated by the expression "between a and b" represents the range of values from more than a to less than b (i.e., excluding limits a and b), while any range of values designated by the expression "from a to b" means the range of values from a to b (i.e., including the strict limits a and b). Unless expressly stated otherwise, all percentages (%) indicated are % by mass.
[0012] In the present application, natural rubber latex is understood to mean latex obtained from the tapping of the Hevea Brasiliensis.
[0013] The method according to the invention has the characteristic of passing a wet coagulum of natural rubber into a device which comprises an extruder and a filter installed at the outlet of the extruder. As the method can be implemented without the use of a gear pump at the outlet of the extruder upstream of the filter, the device useful for the needs of the invention is preferably without a gear pump between the screw and the filter.
[0014] The natural rubber coagulum intended to feed the extruder in the process according to the invention is hereinafter referred to as wet coagulum. It is described as wet because it contains a water content greater than 12%. It is soaked with a serum and most often with water which comes, for example, from the washing water resulting from the coagulum washing operations generally carried out in an underwater pool, in particular implemented in primary decontamination operations. It is recalled that primary decontamination operations aim to eliminate coarse objects. The coagulum has a water content preferably greater than or equal to 15%. The percentages are expressed by weight, relative to the total weight of the coagulum. Preferably, the water content in the wet coagulum is at most 40%. Advantageously, the extruder is fed with a natural rubber coagulum having a water content varying from 15% to 40%.
[0015] The wet coagulum can be in any form, its form being indifferent to the efficiency of the process. It can therefore be in the form of sheets or granules. The natural rubber coagulum is a product of the coagulation of natural rubber latex, indifferently obtained by spontaneous or induced coagulation. According to any of the embodiments of the invention, the natural rubber coagulum is preferably a cup bottom coagulum.
[0016] An extruder is a worm screw machine which comprises, in a well-known manner, a barrel and a worm screw arranged in the barrel. In a well-known manner, the barrel has an opening connected to a feed hopper which is conventionally fitted to an extruder and which allows the introduction of the wet coagulum. Also in a well-known manner, an extruder comprises a feed zone and a pressurization zone (compression zone). The feed zone is the zone of the barrel which is located under the opening of the hopper. The compression zone is a zone of the barrel dedicated to the increase in temperature and pressure of the material to be extruded, in this case the wet coagulum, and which is located downstream of the feed zone and which extends to the end closest to the outlet of the extruder.In the following, the terms upstream and downstream will be referred to when considering the direction and direction of extrusion of the coagulum from the feed zone of the extruder to the compression zone of the extruder. As is known, the end closest to the outlet of the extruder is opposite the end closest to the feed zone of the extruder.
[0017] The sheath also comprises in the feed zone one or more openings intended to evacuate from the sheath the water which can be expelled from the coagulum during the pressure build-up in the barrel. The openings for discharging water may be in the form of slots or circular holes. The worm screw has a hub, also called a core, and a thread that extends radially outward relative to the hub. Preferably, the diameter of the screw hub is constant and the pitch of the screw thread is regular. Preferably, the extruder is a single-screw extruder.
[0018] The extruder useful for the purposes of the invention has the essential characteristic of comprising a barrel which comprises on its inner surface grooves which extend from the end of the barrel closest to the feed zone of the extruder. The barrel being an axially symmetrical structure, preferably a cylindrical structure, therefore comprises in its thickness grooves which open onto the inner surface of the barrel.
[0019] The extruder useful for the purposes of the invention also has the essential characteristic of comprising fingers in the barrel. The fingers which extend radially towards the inside of the barrel relative to the axis of rotation of the screw are present at least in a portion of the barrel which extends from the end of the barrel closest to the outlet of the extruder. According to the invention, the fingers are present at least in a portion of the barrel which is downstream of the feed zone and which extends from the end of the barrel closest to the outlet of the extruder. In particular, the fingers are present in the compression zone.
[0020] According to one embodiment of the invention, the part of the sheath in which the fingers are present extends to the feed zone. According to this embodiment, the parts of the sheath other than that which extends from the end of the sheath closest to the outlet of the extruder to the feed zone are preferably without fingers.
[0021] According to another embodiment of the invention, the part of the sheath in which the fingers are present extends to the end of the sheath closest to the feed zone. In other words, the fingers are present in the sheath over its entire length.
[0022] The fingers may be present both in the feed zone of the extruder and in the compression zone of the extruder.
[0023] According to a first variant of the invention, the grooves of the sheath extend over the entire length of the sheath, that is to say from the end of the sheath closest to the feed zone to the end of the sheath closest to the outlet of the extruder. According to the first variant, the fingers may also be present along the entire length of the sheath or only in the part of the sheath which extends from the end of the sheath closest to the outlet of the extruder to the feed zone or downstream of the feed zone. In particular, they may be present only in the compression zone of the extruder.
[0024] According to a second variant of the invention, the grooves of the sheath extend only over a portion of the sheath. According to the second variant, they extend upstream of the compression zone, preferably up to the compression zone. According to the second variant, the fingers may be present in the sheath over its entire length or only in the portion of the sheath which extends from the end of the sheath closest to the outlet of the extruder to the feed zone or downstream of the feed zone. In particular, they may be present only in the compression zone of the extruder.
[0025] The sheath may consist of a single cylinder or several cylinders, preferably two, placed end to end, the cylinder in the feed zone being grooved. The other cylinders are or are not grooved, depending on the variant of the invention implemented.
[0026] Each groove is defined by a bottom face delimited by two bottom edges, two side faces extending inwardly from the bottom face, each of the two faces being delimited by a bottom edge and an edge of intersection with the inner surface of the grooved sleeve. Preferably, the grooved sleeve is such that, in any plane perpendicular to the axis of the sleeve, R, expressed in mm, being the distance between the center of the sleeve and the inner surface of the grooved sleeve: - the ratio (cumulative length of the groove openings, expressed in mm) / (2irR), called A, is at least equal to 0.25 and at most equal to 0.9; - the ratio (number of grooves / 2R), called B, is greater than or equal to 0.1; - the ratio (depth of grooves, expressed in mm) / (2R), called C, is greater than 0.02, and - the plane passing through the two bottom edges forming with each plane, passing through a bottom edge and an intersection edge, delimiting a lateral face, an angle δ at least equal to 60° and at most equal to 90°.
[0027] For the purposes of the present invention, the grooves define ribs whose upper faces, delimited by two intersecting edges, constitute the inner surface of the sheath. For the purposes of the present invention, the “intersection edge” or “intersection edge with the inner surface of the sheath” (311, 312, 313) is the edge between the side face and the inner surface of the sheath. For the purposes of the present invention, the "cumulative length of the groove openings" is the sum of the distances, expressed in mm, between the two intersection edges between two ribs. For the purposes of the present invention, the “depth of the groove” is defined by the minimum distance, expressed in mm, separating the bottom face and the plane passing through the > 0.02 I) intersection edges. For the purposes of the present invention, the “minimum distance” is the minimum radial distance from the axis of the sheath.
[0028] The grooved sheath is advantageously such that A is at least equal to 0.3 and at most equal to 0.7. More particularly, A is at least equal to 0.45 and at most equal to 0.55.
[0029] In any plane perpendicular to the axis of the sheath, the distance between the two intersection edges between two ribs is advantageously 8 to 15 mm, for an internal diameter of the grooved sheath, 2R, of 60 to 230 mm. In any plane perpendicular to the axis of the sheath, the depth of the grooves is advantageously 2 to 10 mm, for an internal diameter of the grooved sheath, 2R, of 60 to 230 mm.
[0030] The grooves may be in the form of a crenellation or a dovetail. Thus, each groove is advantageously trapezoidal in shape, the large base of the trapezoid forming the bottom of the groove, the sides of the trapezoid adjacent to the large base forming the lateral faces of the groove, the height of the trapezoid being the depth of the groove.
[0031] In particular, the bottom of the grooves is an arc of a circle CR, and the ratio C is calculated by the formula (I) SfîitF - DintF being the diameter of the inner surface of the grooved sleeve, i.e. 2R, DeXtF being the diameter of the circle CR which has the hub axis as its center.
[0032] The grooves may be parallel to the axis of the sheath or helical, preferably they are parallel to the axis of the sheath.
[0033] The fingers facilitate the movement of the wet coagulum in the barrel to the end of the barrel closest to the extruder outlet. Their presence helps to increase the extruder's flow rate of decontaminated natural rubber, even in the absence of a gear pump at the extruder outlet between the screw and the filter. The higher the number of fingers in the barrel, the greater the flow rate of decontaminated natural rubber. For example, a reduction by a factor of 2 in the number of fingers in the barrel results in a reduction in the flow rate of approximately 20% of decontaminated natural rubber for a filter inlet temperature of between 140°C and 150°C. The number of fingers in the barrel is adjusted by a person skilled in the art according to the length and diameter of the barrel. The fingers are generally distributed regularly in the area where they are present. The fingers are preferably carried by the barrel.When the sleeve carries fingers which extend radially inwardly of the sleeve relative to the axis of rotation of the screw, the thread of the screw which is helical and which extends radially from a central shaft of the screw is interrupted so as to form cylindrical annular spaces in . which the fingers are arranged. The distance between the surface of the screw hub and the end of the finger closest to the screw hub is advantageously in a range from 2 to 10 mm, more advantageously in a range from 3 to 5 mm. The dimensions of the fingers useful for the purposes of the invention are typically those of the kneading fingers otherwise known for equipping extruder barrels typically used in the extrusion of polymers.
[0034] The filter is installed at the outlet of the extruder. For the purposes of the present invention, "at the outlet of the extruder" means after the screw. The filter is advantageously carried by a filter holder (12). The filter is any suitable filtration means. It may in particular be one or more mesh filters, the size of which is chosen according to the filtration mesh, installed on a filter holder. Advantageously, the mesh size is chosen so as to retain on the filter any object having a size greater than 500 μm or having a size greater than 750 μm, which typically corresponds to a mesh size less than 35 US mesh ("US sieve size"), preferably less than 25 US mesh. These ranges defining the size of the filter mesh may apply to any of the embodiments of the invention. If necessary, several filters may be arranged one after the other.The filters can then be easily changed during the process using a suitable system, either continuously or discontinuously.
[0035] The pressure applied to the coagulum at the inlet of the filter ranges from 70 bars to 120 bars, preferably from 80 bars to 110 bars. The pressure is typically measured by means of pressure sensors installed upstream of the filter. It can be measured as close as possible to the filter, for example less than 3 cm from the surface formed by the meshes of the filter or the filter first crossed by the wet coagulum in the case where several filters are used.
[0036] The temperature of the coagulum at the inlet of the filter is greater than 130°C and less than 190°C. The temperature can be measured by means of sensors installed at the inlet of the filter, as close as possible to the filter, for example less than 3 cm from the surface formed by the meshes of the filter or of the filter first crossed by the wet coagulum in the case where several filters are used. It is typically the mechanical work under pressure which is exerted on the coagulum in the barrel which is at the origin of the temperature levels of the coagulum recorded in the barrel. Heat can also be provided by heating the screw or the barrel or even both, screw and barrel, by means of a double jacket or electrical resistors. If necessary, the extruder can also include cooling means, for example by means of the double jacket already mentioned.Preferably, the temperature of the coagulum at the inlet of the filter is less than 170°C. This embodiment is particularly preferential when decontaminated natural rubber is introduced. immediately after filtration in a second extruder to be dried according to a process comprising an adiabatic flash expansion step as described for example in patent applications WO 2017207912, WO 2019102107, WO 2019102108, WO 2021224568, WO 2021111082 and WO 2022064144.
[0037] The presence of both fingers and grooves in the sheath according to the invention and the pressure and temperature conditions according to the invention make it possible not only to eliminate the use of a gear pump while increasing the flow rate of decontaminated natural rubber, but also to reduce the energy consumption of the process.
[0038] During its passage through the sheath, the wet coagulum is subjected to mechanical stresses which have the effect of wringing it out. It can lose up to 50% by weight of its water content, or even more. The water loss under the effect of wringing depends on the initial water content of the wet coagulum which feeds the extruder and on the pressure and temperature conditions. Typically, the natural rubber decontaminated according to the process according to the invention and recovered at the outlet of the filter has a residual water content greater than 7%, preferably greater than 10%.
[0039] Once the natural rubber has been decontaminated according to the process according to the invention, it can be subjected after the filtration operation to a further treatment. As further treatment, mention may be made, for example, of drying in tunnels under air circulation traditionally used for the preparation of TSR20 grades of natural rubber, drying in a second extruder by adiabatic flash expansion as described above.
[0040] Any device may also be provided after the filter to obtain the desired shape of the decontaminated natural rubber, for example the shape of a strip, slice, sausage, granule, etc., in particular to carry out the subsequent treatments mentioned above.
[0041] In summary, the invention is advantageously implemented according to any one of the following embodiments 1 to 23:
[0042] Method 1: Process for preparing a decontaminated natural rubber, which comprises a decontamination step by passing a coagulum of natural rubber having a humidity level greater than 12% by weight, into a device comprising an extruder comprising a barrel and an endless screw, and a filter installed at the outlet of the extruder, the barrel comprising on its inner surface grooves which extend from the end of the barrel closest to the feed zone of the extruder, the extruder having fingers in the barrel which extend radially inward of the barrel relative to the axis of rotation of the screw and which are present at least in a portion of the barrel which extends ... close to the extruder outlet, the pressure applied to the coagulum at the filter inlet ranging from 70 bars to 120 bars, the temperature of the coagulum at the filter inlet being greater than 130°C and less than 190°C.
[0043] Mode 2: Method according to mode 1 in which the part of the sheath in which the fingers are present extends to the feed zone.
[0044] Mode 3: Method according to mode 1 in which the part of the sheath in which the fingers are present extends to the end of the sheath closest to the feed zone.
[0045] Mode 4: Method according to any one of modes 1 to 3 in which the fingers are carried by the sheath.
[0046] Mode 5: Method according to any one of modes 1 to 4 in which the distance between the surface of the screw hub and the end of the finger closest to the screw hub is within a range of 2 to 10 mm.
[0047] Mode 6: Method according to any one of modes 1 to 5 in which the distance between the surface of the hub of the screw and the end of the finger closest to the hub of the screw is within a range of 3 to 5 mm.
[0048] Mode 7: Method according to any one of modes 1 to 6 in which the grooves of the barrel extend to the end of the barrel closest to the outlet of the extruder.
[0049] Mode 8: Method according to any one of modes 1 to 7 in which the grooves of the barrel extend upstream of the compression zone, the compression zone being downstream of the feed zone and extending to the end closest to the outlet of the extruder.
[0050] Mode 9: Method according to any one of modes 1 to 8 in which the grooves of the barrel extend to the compression zone, the compression zone being downstream of the feed zone and extending to the end closest to the outlet of the extruder.
[0051] Mode 10: Method according to any one of modes 1 to 9 in which the pressure applied to the coagulum at the inlet of the filter ranges from 80 bars to 110 bars.
[0052] Mode 11: Method according to any one of modes 1 to 10 in which the temperature of the coagulum at the inlet of the filter is less than 170°C.
[0053] Mode 12: Method according to any one of modes 1 to 11 in which: each groove comprising: - a bottom face delimited by two bottom edges, - two lateral faces extending inwards from the bottom face, each being delimited by a bottom edge and an edge of intersection with the inner surface of the sheath, in any plane perpendicular to the axis of the sheath, R, expressed in mm, being the distance between the center of the sheath and the inner surface of the sheath, the ratio (cumulative length of the groove openings, expressed in mm) / (2jtR), called A, is at least equal to 0.25 and at most equal to 0.9; the ratio (number of grooves / 2R), called B, is greater than or equal to 0.1; the ratio (depth of grooves, expressed in mm) / (2R), called C, is greater than 0.02, and the plane passing through the two bottom edges forming with each plane, passing through a bottom edge and an intersection edge, delimiting a lateral face, an angle δ at least equal to 60° and at most equal to 90°.
[0054] Mode 13: Method according to mode 12 in which A is at least equal to 0.3 and at most equal to 0.7.
[0055] Mode 14: Method according to mode 12 or 13 in which A is at least equal to 0.45 and at most equal to 0.55.
[0056] Mode 15: Method according to any one of modes 12 to 14 in which each groove is trapezoidal in shape, the large base of the trapezoid forming the bottom of the groove, the sides of the trapezoid adjacent to the large base forming the lateral faces of the groove, the height of the trapezoid being the depth of the groove.
[0057] Mode 16: Method according to any one of modes 12 to 15 in which the bottom of the grooves is an arc of a circle CR, and the ratio C is calculated by the formula (I) > 0.02 DintF being the diameter of the inner surface of the sheath, or 2R DextF being the diameter of the circle CR which has the hub axis as its center.
[0058] Mode 17: Method according to any one of modes 12 to 16 in which the grooves of the sheath are parallel to the axis of the sheath.
[0059] Mode 18: Method according to any one of modes 1 to 17 in which the extruder is a single-screw extruder.
[0060] Mode 19: Method according to any one of modes 1 to 18 in which the mesh size is chosen so as to retain on the filter any object having a size greater than 500 pm.
[0061] Mode 20: Method according to any one of modes 1 to 18 in which the mesh size is chosen so as to retain on the filter any object having a size greater than 750 pm.
[0062] Mode 21: Process according to any one of modes 1 to 20 in which the extruder is fed with a natural rubber coagulum having a water content varying from 15% to 40%.
[0063] Mode 22: Method according to any one of modes 1 to 21 in which the coagulum natural rubber is a cup bottom coagulum.
[0064] Mode 23: Method according to any one of modes 1 to 22 in which the device is without a gear pump arranged at the outlet of the extruder between the screw and the filter.
[0065] The above-mentioned characteristics of the present invention, as well as others, will be better understood upon reading the following description of several exemplary embodiments of the invention, given for illustrative and non-limiting purposes. Examples
[0066] Single screw extruder: Screw diameter (D): 150 mm with constant hub diameter and constant screw pitch, Screw length: 12 D, Sheath consisting of two cylinders of the same length, only the cylinder in the feed zone is grooved, only the cylinder in the compression zone has fingers, 64 distributed regularly in the cylinder
[0067] Filter: Filter diameter: 200 mm 3 superimposed meshes: 1 mesh 6+1 mesh 20+1 mesh 10 (US mesh).
[0068] The extruder is fed with a wet coagulum of cup bottom treated with primary decontamination ("slab cutter", "wet prebreakers") with a humidity level given in Table 1. The pressure (P) and temperature (T) conditions at the inlet of the filter are shown in Table 1, as well as the water content of the decontaminated natural rubber and the flow rate of decontaminated natural rubber both measured at the outlet of the filter. The energy consumption to operate the process is also shown in Table 1.
[0069] Two tests are conducted. Test 1 is not in accordance with the invention, since the temperature at the inlet of the filter (T) is 100°C. Test 2 is in accordance with the invention.
[0070] The water content is determined with a Mettler Toledo HB43-S halogen desiccator. The desiccator is an automated device that incorporates a cup, a scale, and a lid for closing the cup. The cup is positioned on the scale. The lid includes a heating means using a halogen lamp, this heating means being triggered when the lid is closed over the cup. In the cup, a 10-gram sample of natural rubber is weighed exactly: the device records the corresponding weight "a". The lid is closed to close the cup, which triggers the temperature rise to reach a set point of 160°C. When the device detects a decrease in weight of less than 0.001 g per minute, the device records a weight "b". The water content in the sample is given in mass percentage by the following equation: Water content (%) = 100*((ab) / a)
[0071] The flow rate of decontaminated natural rubber is given on a base of 100 compared to test 1 taken as reference.
[0072] The energy consumption is given on a base of 100 compared to test 1 taken as a reference. The values are given for the same quantity of decontaminated natural rubber.
[0073] [Tables 1] Test P (bar) T (°C) Flow Energy consumption % water in the coagulum which feeds the extruder at the outlet of the extruder after the filter 1 85 100 100 100 24% 11% 2 75 150 170 58 24% 12%
[0074] Table 1 shows that the method according to the invention does indeed increase the flow rate and also reduces energy consumption. This result is obtained without having to resort to using a gear pump. It is observed that the flow rate of test 2 is reduced by approximately 20% if the number of fingers is reduced by a factor of 2.
[0075] Three other tests in accordance with the invention (3 to 5) are carried out on an extruder which comprises a grooved barrel along its entire length and fingers carried by the barrel along its entire length. The pressure (P) and temperature (T) conditions at the filter inlet, the water contents, the flow rates and the energy consumptions are shown in Table 2. The flow rate and energy consumption values are given on a base of 100 compared to test 3 taken as a reference. The values relating to energy consumption are given for the same quantity of decontaminated natural rubber.
[0076] [Tables2] Test P (bar) T (°C) Flow Energy consumption % water in the coagulum which feeds the extruder at the outlet of the extruder after the filter 3 90 155 100 100 24% 10% 4 100 160 107 99 23% 12% 5 90 145 92 (*) 23% 14%
[0077] (*) not measured
[0078] Tests 3 to 5 show reproducibility in the results regarding flow rate and energy consumption, even though a pressure variation of 10 bars (test 3 compared to test 4) or a temperature variation of 10 degrees (test 3 compared to test 5) is observed at the filter inlet.
Claims
Claims
1. A method for preparing a decontaminated natural rubber, which comprises a decontamination step by passing a coagulum of natural rubber having a moisture content greater than 12% by weight, through a device comprising an extruder comprising a barrel and a worm screw, and a filter installed at the outlet of the extruder, the barrel comprising on its inner surface grooves which extend from the end of the barrel closest to the feed zone of the extruder, the extruder having fingers in the barrel which extend radially towards the inside of the barrel relative to the axis of rotation of the screw and which are present at least in a portion of the barrel which extends from the end of the barrel closest to the outlet of the extruder, the pressure applied to the coagulum at the inlet of the filter ranging from 70 bars to 120 bars, the temperature of the coagulum at the filter inlet being greater than 130°C and less than 190°C.
2. A method according to claim 1 wherein the portion of the sheath in which the fingers are present extends to the feed zone.
3. A method according to claim 1 wherein the portion of the sheath in which the fingers are present extends to the end of the sheath closest to the feed zone.
4. A method according to any one of claims 1 to 3 wherein the grooves of the barrel extend to the end of the barrel closest to the outlet of the extruder.
5. A method according to any one of claims 1 to 3 wherein the grooves of the sleeve extend upstream of the compression zone, preferably as far as the compression zone, the compression zone being downstream of the feed zone and extending to the end closest to the outlet of the extruder.
6. A method according to any one of claims 1 to 5 wherein the pressure applied to the coagulum at the inlet of the filter ranges from 80 bars to 110 bars.
7. A method according to any one of claims 1 to 6 wherein the temperature of the coagulum at the inlet of the filter is less than 170°C.
8. A method according to any one of claims 1 to 7 wherein: each groove comprising: - a bottom face delimited by two bottom edges, - two lateral faces extending inwards from the bottom face, each being delimited by a bottom edge and an edge of intersection with the inner surface of the sheath, in any plane perpendicular to the axis of the sheath, R, expressed in mm, being the distance between the center of the sheath and the inner surface of the sheath, the ratio (cumulative length of the groove openings, expressed in mm) / (2irR), called A, is at least equal to 0.25 and at most equal to 0.9; the ratio (number of grooves / 2R), called B, is greater than or equal to 0.1; the ratio (depth of the grooves, expressed in mm) / (2R), called C, is greater than 0.02, and the plane passing through the two bottom edges forming with each plane, passing through a bottom edge and an intersection edge, delimiting a lateral face, an angle δ at least equal to 60° and at most equal to 90°.
9. Method according to claim 8 in which the bottom of the grooves is an arc of a circle CR, and the ratio C is calculated by the formula (I) > a02 ^>n! DintF being the diameter of the inner surface of the sheath, or 2R DextF being the diameter of the circle CR which has as its center the axis of the hub.
10. A method according to any one of claims 8 to 9 wherein the grooves of the sheath are parallel to the axis of the sheath.
11. A method according to any one of claims 1 to 10 wherein the extruder is a single screw extruder.
12. A method according to any one of claims 1 to 11 wherein the extruder is fed with a natural rubber coagulum having a water content ranging from 15% to 40%.
13. A method according to any one of claims 1 to 12 wherein the device is without a gear pump between the screw and the filter.