Two-component composition based on epoxy resin
A two-component epoxy resin composition with aromatic epoxy resin, phenolic Mannich bases, and lamellar fillers addresses the slow curing and adhesion issues of existing compositions, enabling single-day floor preparation with low water vapor permeability and reduced toxicity, enhancing flooring efficiency and safety.
Patent Information
- Application Number
- FR2022009897
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2042-09-29
AI Technical Summary
Existing two-component epoxy resin compositions used as moisture barriers in flooring applications require a lengthy curing time, necessitating at least two days to prepare a floor, and do not meet requirements for quick hardening, low water vapor permeability, good adhesion on wet concrete, and low toxicity, while also needing to be easily applied and mixed efficiently.
A two-component composition comprising aromatic epoxy resin, phenolic Mannich bases as a hardener, and lamellar fillers like micaceous iron oxide, which accelerates hardening, provides low water vapor permeability, and ensures adhesion on wet concrete, with a formulation that is less toxic and easier to apply.
The composition allows for a single-day preparation of floors, achieves low water vapor permeability, exhibits excellent adhesion on wet concrete, and reduces toxicity, while maintaining a suitable mixing and application time, thus improving efficiency and safety in flooring processes.
Abstract
Description
Title of the invention: Two-component epoxy resin-based composition Field of invention
[0001] The present invention relates to a two-component composition and its use, a moisture barrier, a method for sealing a surface and a method for preparing soil. Technical background
[0002] Various two-component epoxy resin compositions are available on the market, and these can be used in many fields, particularly in the building sector. In particular, some two-component epoxy resin compositions can be used as a moisture barrier and are then applied to a surface (especially a floor surface) to protect the coatings applied as a finish to said surface from moisture (especially moisture from the ground).
[0003] In general, preparing a floor for the installation of finishing floor covering(s) (for example linoleum, PVC tile, parquet, etc.), especially in concrete, requires the following three steps: first the application of a moisture barrier, then the preparation of the surface for example by sandblasting or application of a bonding layer (most often water-based), and finally the application of a self-leveling composition (most often cement-based).
[0004] Epoxy resin-based moisture barriers currently on the market need to be left overnight to harden before the bonding coat can be applied. Therefore, preparing a floor (including the three steps mentioned above) takes at least two days.
[0005] There is therefore a need to provide a two-component epoxy resin-based composition that hardens more quickly. In particular, it would be advantageous for said composition to harden sufficiently quickly so that the preparation of a floor (comprising the three aforementioned steps) could be completed in a single day.
[0006] In addition, said composition must have a low water vapor permeance, in particular less than or equal to 10 mg / h / m2 / mmHg, in order to be able to be used as a moisture barrier.
[0007] Furthermore, when the floor to be waterproofed is concrete, said composition must have good adhesion to wet concrete.
[0008] Another object of the invention is to provide a two-component epoxy resin-based composition that has a sufficiently low viscosity to be able to be applied fa- cilement.
[0009] Another object of the invention is to provide a two-component epoxy resin-based composition that has a mixing life sufficient for the user to have time to apply the entire composition to the surface to be sealed before it hardens.
[0010] Another object of the invention is to provide a two-component epoxy resin-based composition that can be applied at a high grammage on a surface.
[0011] Another object of the invention is to provide a two-component epoxy resin-based composition that is less toxic, in particular with low emissions of volatile organic compounds (VOCs), and / or is essentially free of ingredients classified as CMR (carcinogenic, mutagenic and / or reprotoxic) and SVHC (substances of very high concern). Summary of the invention
[0012] The present invention relates to a two-component composition comprising: - a component (A) comprising: • at least one aromatic epoxy resin, and - a component (B) comprising: • a hardener (H) selected from phenolic Mannich bases having at least one primary and / or secondary amine group, preferably selected from phenalkamines, and • the reaction products (P) chosen from: - the reaction products (IP) of at least: a fatty acid, a polyamine (Dl) and a compound (E) comprising at least one epoxide group, and / or - the reaction products (P2) of at least: a dimerized fatty acid and a polyamine (D2),
[0013] component (A) and / or component (B) further comprising at least 20% by weight, relative to the total weight of said component, of a lamellar filler (C) selected from micaceous iron oxide, vermiculite, mica and mixtures thereof, preferably micaceous iron oxide.
[0014] The present invention also relates to the use of the two-component composition according to the invention as a moisture barrier, particularly in the field of buildings.
[0015] The present invention also relates to a moisture barrier obtained after hardening of the two-component composition according to the invention.
[0016] The present invention also relates to a method for sealing a surface comprising applying the two-component composition according to the invention to said surface then hardening of said composition to form a moisture barrier, especially at room temperature (particularly between 18°C and 28°C).
[0017] Finally, the present invention relates to a soil preparation process comprising: - applying the two-component composition according to the invention to the soil surface, then - the hardening of said composition to form a moisture barrier, and - preparing a surface suitable for the application of a self-leveling compound, then - the application of a self-smoothing composition.
[0018] Surprisingly, it was found that the two-component composition according to the invention can be used as a moisture barrier and cures much faster than the epoxy resin-based compositions usually used as moisture barriers. It also has good adhesion to damp concrete.
[0019] In particular, the two-component composition according to the invention makes it possible to carry out the preparation of a soil (comprising the three aforementioned steps) in a single day. Description of the invention
[0020] The present invention relates to a two-component composition comprising: - a component (A) comprising: • at least one aromatic epoxy resin, and - a component (B) comprising: • a hardener (H) selected from phenolic Mannich bases having at least one primary and / or secondary amine group, preferably selected from phenalkamines, and • the reaction products (P) chosen from: - the reaction products (IP) of at least: a fatty acid, a polyamine (Dl) and a compound (E) comprising at least one epoxide group, and / or - the reaction products (P2) of at least: a dimerized fatty acid and a polyamine (D2),
[0021] component (A) and / or component (B) further comprising at least 20% by weight, relative to the total weight of said component, of a lamellar filler (C) selected from micaceous iron oxide, vermiculite, mica and mixtures thereof, preferably micaceous iron oxide. Two-component composition Epoxy resin
[0022] By "aromatic epoxy resin" is meant a compound comprising at least two, preferably exactly 2, epoxide groups and comprising one or more aromatic rings.
[0023] Preferably, the aromatic epoxy resin has a molar mass of less than 500 g / mol, more preferably less than or equal to 400 g / mol.
[0024] According to a preferred embodiment, the aromatic epoxy resin is a di-glycidyl ether derivative.
[0025] Advantageously, the aromatic epoxy resin is selected from the diglycidic ethers of bis-(4-hydroxy-3,5-difluorophenyl)methane, 1,1-bis-(4-hydroxyphenyl)ethane (bisphenol E), 2,2-bis-(4-hydroxy-3-methylphenyl)propane (CAS: 79-97-0), 2,2-bis-(4-hydroxy-3,5-dichlorophenyl)propane (CAS: 79-95-8), 2,2-bis(4-hydroxyphenyl)butane (bisphenol B), 2,2-bis-(4-hydroxyphenyl)propane (bisphenol A), 4,4'-methylenediphenol (4,4'-bisphenol F isomer), 2,4'-methylenediphenol (2,4'-bisphenol F isomer), 2,2'-methylenediphenol (isomer 2,2'-bisphenol F) and their mixtures.
[0026] Preferably, the aromatic epoxy resin is chosen from diglycidic ethers of 1,1-bis-(4-hydroxyphenyl)ethane, 2,2-bis-(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis-(4-hydroxyphenyl)propane, 4,4'-methylenediphenol, 2,4'-methylenediphenol, 2,2'-methylenediphenol and mixtures thereof.
[0027] More preferably, the aromatic epoxy resin is chosen from diglycidic ethers of 1,1-bis-(4-hydroxyphenyl)ethane, 2,2-bis-(4-hydroxyphenyl)propane, 4,4'-methylenediphenol, 2,4'-methylenediphenol, 2,2'-methylenediphenol and mixtures thereof.
[0028] Even more preferably, the aromatic epoxy resin is chosen from among the diglycidic ethers of 2,2-bis-(4-hydroxyphenyl)propane, 4,4'-methylenediphenol, 2,4'-methylenediphenol, 2,2'-methylenediphenol and their mixtures.
[0029] In particular, the aromatic epoxy resin is a mixture of diglycidic ethers of 2,2-bis-(4-hydroxyphenyl)propane, 4,4'-methylenediphenol, 2,4'-methylenediphenol and 2,2'-methylenediphenol.
[0030] Examples of commercial 2,2-bis-(4-hydroxyphenyl)propane diglycidic ether (CAS: 1675-54-3) are DER™ 331 marketed by OLIN, EPIKOTE 828 from Westlake, EPOKUKDO YD 128 from Kukdo Chemical and EPILOX® A 19-00 from Leuna Harze.
[0031] An example of a commercial mixture of 4,4'-methylenediphenol, 2,4'-methylenediphenol and 2,2'-methylenediphenol diglycidic ethers (CAS: 9003-36-5) is HEXION's EPIKOTE Resin 862.
[0032] Examples of commercial 2,2-bis-(4-hydroxyphenyl)propane diglycidic ether mixtures (CAS: 1675-54-3) and 4,4'-methylenediphenol, 2,4'-methylenediphenol and 2,2'-methylenediphenol diglycidic ethers (CAS: 9003-36-5) are DER™ 351 marketed by OLIN, EPILOX® AF 18-50 from Leuna-Harze and EPOKUKDO YDF 161 from Kukdo.
[0033] According to a particular embodiment, the aromatic epoxy resin is a mixture of diglycidic ethers of 2,2-bis-(4-hydroxyphenyl)propane, 4,4'-methylenediphenol, 2,4'-methylenediphenol and 2,2'-methylenediphenol, the weight ratio of diglycidic ether of 2,2-bis-(4-hydroxyphenyl)propane to diglycidic ethers of 4,4'-, 2,4'- and 2,2'-methylenediphenol being between 0.01 and 15, preferably between 0.02 and 11, more preferably between 0.04 and 7.
[0034] The total aromatic epoxy resin content in component (A) is advantageously at least 50% by weight relative to the total weight of component (A), preferably at least 60% by weight, and more preferably at least 70% by weight. For example, the aromatic epoxy resin content in component (A) may range from 50% to 99% by weight relative to the total weight of component (A), preferably from 60% to 97% by weight, and more preferably from 70% to 95% by weight.
[0035] In the context of the invention, the ranges of values are understood to include the limits. For example, the range "between 0% and 25%" includes, in particular, the values 0% and 25%.
[0036] Furthermore, by "approximately X", we mean plus or minus 10% of the value of X. Reactive diluent
[0037] Advantageously, component (A) further comprises a reactive diluent.
[0038] By "reactive diluent" is meant a compound having exactly one epoxide group and which may include an aromatic ring, or an aliphatic compound having exactly two epoxide groups, preferably a compound having exactly one epoxide group.
[0039] Reactive diluents are well known to those skilled in the art and are generally used to reduce the viscosity of epoxy resin-based components.
[0040] Advantageously, the reactive diluent is selected from 4-tert-butylphenyl glycidyl ether (CAS: 3101-60-8), the reaction products of cashew nut shell liquid and epichlorohydrin (CAS: 68413-24-1), C12-C14 alkyl glycidyl ethers (CAS: 68609-97-2), C13-C15 alkyl glycidyl ethers (CAS: 68081-84-5), 1,4-butanediol diglycidyl ether (CAS: 2425-79-8), 1,6-hexanediol diglycidyl ether (CAS: 16096-31-4), ether diglycidic polypropylene glycol (CAS: 26142-30-3) and their mixtures.
[0041] Preferably, the reactive diluent is chosen from glycidyl ether of 4-tert-butylphenyl, the reaction products of cashew nut shell liquid and epichlorohydrin, C12-C14 alkyl glycidyl ethers, C13-C15 alkyl glycidyl ethers and mixtures thereof, in particular C12-C14 alkyl glycidyl ethers.
[0042] The content of reactive diluent in component (A) can range from 1% to 30% by weight relative to the total weight of component (A), preferably from 2% to 25% by weight, more preferably from 4% to 17% by weight. Component additives (A)
[0043] The component (A) may further comprise one or more additives selected from plasticizers, mineral fillers, thickeners, pigments, debubbling agents and mixtures thereof, in particular from debubbling agents.
[0044] The total content of the aforementioned additives, excluding mineral fillers, can range from 0.01% to 10% by weight relative to the total weight of component (A), preferably from 0.02% to 5% by weight, more preferably from 0.03% to 3% by weight.
[0045] The component (A) may comprise up to 5% by weight of plasticizer relative to the total weight of the component (A), preferably up to 2% by weight.
[0046] The plasticizer can, for example, be chosen from mineral oils of petroleum origin, paraffinic oils, polyolefins, esters of benzoic, phthalic, trimellitic, pyromellitic, adipic, sebacic, fumaric, maleic, itaconic and citric acids, and mixtures thereof.
[0047] The mineral filler is different from the lamellar filler (C), and can be chosen from carbonate fillers (such as calcium carbonate or dolomite), quartz, barium sulfate, nepheline syenite, glass beads, hollow mineral microspheres (for example in sodium and calcium borosilicate or aluminosilicate) and mixtures thereof.
[0048] Component (A) may comprise up to 20% by weight of mineral filler relative to the total weight of component (A). When component (A) already comprises a lamellar filler (C), the mineral filler content (other than the lamellar filler (C)) is preferably chosen so that the total filler content (mineral and lamellar (C)) does not exceed 65% by weight relative to the total weight of component (A).
[0049] The thickener may be silica, which may be pyrogenated or precipitated, optionally hydrophobic, preferably pyrogenated silica. Advantageously, the thickener is pyrogenated (hydrophilic) silica.
[0050] The thickener content may vary from 0.01% to 5% by weight relative to the total weight of component (A), preferably from 0.1% to 2% by weight, more preferably from 0.4% to 1.0% by weight.
[0051] Component (A) may comprise up to 3% by weight of pigment relative to the total weight of component (A), preferably up to 2% by weight.
[0052] The pigment can be an organic or inorganic pigment, for example based on TiO2 (such as TRONOX's TIONA® 595) or based on manganese ferrite (such as LANXESS's BAYFERROX® 303 T).
[0053] Advantageously, component (A) further comprises a debubbling agent.
[0054] Defoaming agents are usually used by those skilled in the art to allow the rapid elimination of bubbles formed during the preparation and application of epoxy resins.
[0055] The debubbling agent can be any debubbling agent commonly used in epoxy resin-based compositions.
[0056] By way of example, silicone oil in a hydrotreated light distillate (petroleum) solvent (CAS: 64742-47-8) and a polyolefin in a light aromatic naphtha (petroleum) solvent (CAS: 64742-95-6) are examples. Commercial examples include Münzig's AGIT AN® DF 311 M and BYK Chemie's BYK 057.
[0057] The content of debubbling agent in component (A) can range from 0.01% to 1% by weight relative to the total weight of component (A), preferably from 0.02% to 0.5% by weight. Component embodiment methods (A)
[0058] According to one embodiment, component (A) comprises: - at least 50% by weight of aromatic epoxy resin relative to the total weight of component (A), - from 1% to 30% by weight of reactive diluent relative to the total weight of component (A), - optionally from 0.01% to 10% by weight of one or more additives selected from plasticizers, thickeners, pigments, debubbling agents and mixtures thereof, relative to the total weight of component (A), and - optionally up to 20% by weight of mineral filler other than the filler lamellar (C) relative to the total weight of the component (A).
[0059] Preferably, component (A) consists essentially of the ingredients mentioned above. By "consists essentially of", it is meant that component (A) comprises less than 5% by weight of ingredients other than the aforementioned ingredients, relative to the total weight of component (A), preferably less than 2% by weight, and even more preferably less than 1% by weight.
[0060] The ingredients of this embodiment and their particular contents are as described above, including preferred characteristics and embodiments.
[0061] According to a particular embodiment, component (A) comprises: - 70% to 95% by weight of aromatic epoxy resin relative to the total weight of component (A), the aromatic epoxy resin being preferably chosen from the diglycidic ethers of 2,2-bis-(4-hydroxyphenyl)propane, of 4,4'-methylenediphenol, of 2,4'-methylenediphenol, of 2,2'-methylenediphenol and mixtures thereof, - 4% to 17% by weight of reactive diluent relative to the total weight of component (A), the reactive diluent preferably being selected from 4-tert-butylphenyl glycidyl ether, the reaction products of cashew nut shell liquid and epichlorohydrin, C12-C14 alkyl glycidyl ethers, C13-C15 alkyl glycidyl ethers and mixtures thereof, and - optionally from 0.03% to 3% by weight, relative to the total weight of component (A), of one or more additives chosen from plasticizers, pigments, de-bubbling agents and their mixtures, in particular from de-bubbling agents.
[0062] Preferably, component (A) consists essentially of the ingredients mentioned above.
[0063] The ingredients of this embodiment and their specific contents are as described above, including preferred characteristics and embodiments. Hardener (H)
[0064] The hardener (H) is selected from phenolic Mannich bases having at least one primary and / or secondary amine group. These can be obtained by a Mannich reaction between a phenol derivative, an aldehyde, and an amine having at least one primary amine group (-NH2) or at least two secondary amine groups, preferably having at least one primary amine group.
[0065] Advantageously, the hardener (H) is a phenolic Mannich base of formula (I): OH (I), . Jx , rS R3
[0066] in which: - R2 and R4 independently represent a hydrogen atom or a saturated or unsaturated hydrocarbon radical, preferably with a linear or branched open chain, comprising 1 to 20 carbon atoms, and - R1, R3 and R5 represent independently: • a hydrogen atom, or • a saturated or unsaturated hydrocarbon radical, preferably with a linear or branched open chain, comprising 1 to 20 carbon atoms and optionally one or more heteroatoms selected from nitrogen and oxygen, or • a monovalent radical of formula (II):
[0067] in which: • R6 represents a hydrogen atom or a hydrocarbon radical comprising 1 to 15 carbon atoms, saturated or unsaturated, with a linear or branched open chain, or comprising one or more possibly aromatic rings, and • R7 represents a hydrocarbon radical comprising at least two carbon atoms, saturated or unsaturated, with a linear or branched open chain, or comprising one or more rings, possibly aromatic, and possibly comprising one or more nitrogen atoms,
[0068] at least one, preferably exactly one, of the substituents R1, R3 and R5 being of formula (II).
[0069] The various groups, radicals and letters which are included in the formulas described in this application, retain throughout this text, and, in the absence of any indication to the contrary, the same definition.
[0070] By "unsaturated" we mean one or more unsaturations. The unsaturations may be bonding (for example double or triple bond) and / or ring unsaturations.
[0071] The following characteristics of the phenolic Mannich base of formula (I) are particularly preferred, taken individually or in combination with each other.
[0072] Advantageously, in the phenolic Mannich base of formula (I), R6 represents a hydrogen atom, a phenyl group, a cyclohexyl group, a cyclopentyl group or a saturated linear alkyl group having from 1 to 10 carbon atoms, in particular a hydrogen atom.
[0073] Advantageously, in the phenolic Mannich base of formula (I), the radical R7 is such that the amine of formula R7NH2 is selected from isophorone diamine, 1,2-diaminocyclohexane, m-xylylene diamine, 2-methyl-1,5-pentanediamine, hexamethylene diamine, trimethylhexamethylene diamine, and the (poly)ethylamines of formula H2N-(CH2-CH2-NH)X-CH2-CH2-NH2, x being an integer from 0 to 5, preferably from 0 to 3. Preferably, the radical R7 is such that the amine of formula R7NH2 is selected from m-xylylene diamine and the (poly)ethylamines of formula H2N-(CH2-CH2-NH)X-CH2-CH2-NH2, x being an integer from 0 to 5, preferably between 0 and 3.
[0074] According to one embodiment, the hardener (H) is a phenolic Mannich base of formula (I), in which: - R2 and R4 represent a hydrogen atom, and the substituents R1, R3 and R5, not being of formula (II), are hydrogen atoms, or - R2 represents a linear aliphatic group, possibly including one or more double bonds, and having 15 carbon atoms, R4 represents a hydrogen atom, and the substituents R1, R3 and R5, not being of formula (II), are hydrogen atoms, or - R4 represents a hydrogen atom, R2 or one of the substituents R1, R3 or R5 (not being of formula (II)) is a phenyl group, and the other substituents (R1, R2, R3 and R5 not being of formula (II), nor a phenyl group) are hydrogen atoms, or - R4 represents a hydrogen atom, R2 or one of the substituents R1, R3 or R5 (not being of formula (II)) is a saturated hydrocarbon radical with a linear or branched open chain comprising 1 to 12 carbon atoms, and the other substituents (R1, R2, R3 and R5 not being of formula (II), nor a saturated hydrocarbon radical with a linear or branched open chain comprising 1 to 12 carbon atoms) are hydrogen atoms, or - R4 represents a hydrogen atom, R2 or one of the substituents R1, R3 or R5 (not being of formula (II)) is a tert-butyl group, and the other substituents (R1, R2, R3 and R5 not being of formula (II), nor a tert-butyl group) are hydrogen atoms.
[0075] Preferably, the hardener (H) is a phenolic Mannich base of formula (I), in which: - R2 and R4 represent a hydrogen atom, and the substituents R1, R3 and R5, not being of formula (II), are hydrogen atoms, or - R2 represents a linear aliphatic group, possibly including one or more double bonds, and having 15 carbon atoms, R4 represents a hydrogen atom, and the substituents R1, R3 and R5 not being of formula (II) are hydrogen atoms.
[0076] According to a preferred embodiment, the hardener (H) is a phenalkamine. Phenalkamines are Mannich bases obtained from cardanol as a phenol derivative. Cardanol comprises four compounds extracted from cashew nut shell liquid of formula (III): OH (III),
[0077] in which R2 represents a linear aliphatic group having 15 carbon atoms chosen from the groups whose formulas below show the free valence (the free valence is directly linked to the carbon atom in the meta position relative to the hydroxyl group, as indicated in formula (III)): - saturated group of formula (Ilia): - monounsaturated group of formula (Illb): - bi-unsaturated group of formula (IIIc): - tri-unsaturated group of formula (Illd):
[0078] Thus, according to this preferred embodiment, the hardener (H) is a phenolic Mannich base of formula (I), in which: - R2 represents a group of formula (Ilia), (Illb), (IIIc) or (Illd), R4 represents a hydrogen atom, and the substituents R1, R3 and R5 not being of formula (II) are hydrogen atoms.
[0079] Preferably, the hardener (H) is a phenolic Mannich base of formula (I), in which: - R2 represents a group of formula (Ilia), (Illb), (IIIc) or (Illd), R4 represents a hydrogen atom, and the substituents R1, R3 and R5, not being of formula (II), are hydrogen atoms, and - R6 represents a hydrogen atom, a phenyl group, a cyclohexyl group, a cyclopentyl group, or a saturated linear alkyl group having from 1 to 10 carbon atoms, in particular a hydrogen atom, and - R7 represents a hydrocarbon radical comprising at least two carbon atoms, saturated or unsaturated, with a linear or branched open chain, or comprising one or more possibly aromatic rings, and possibly comprising one or more nitrogen atoms.
[0080] Preferably, according to this embodiment, the radical R7 is such that the amine of formula R7NH2 is chosen from isophorone diamine, 1,2-diaminocyclohexane, m-xylylene diamine, 2-methyl-1,5-pentanediamine, hexamethylene diamine, tri-methylhexamethylene diamine and the (poly)ethylamines of formula H2N-(CH2-CH2-NH)X-CH2-CH2-NH2, x being an integer between 0 and 5, preferably between 0 and 3. More preferably, the radical R7 is such that the amine of formula R7NH2 is chosen from m-xylylene diamine and the (poly)ethylamines of formula H2N-(CH2-CH2-NH)X-CH2-CH2-NH2, x being an integer between 0 and 5, preferably between 0 and 3.
[0081] The hardener (H) content in component (B) is advantageously between 3% and 30% by weight relative to the total weight of component (B), preferably between 4% and 23% by weight, more preferably between 5% and 18% by weight. Co-hardener
[0082] Component (B) may further comprise a co-hardener; this co-hardener is different from the phenolic Mannich base described above, in particular this co-hardener is not a Mannich base.
[0083] Advantageously, the co-hardener comprises at least one primary amine group, preferably at least two primary amine groups.
[0084] The co-hardener can be selected from diethylenetriamine, triethylenetetramine, pentaethylenehexamine, hexamethylenediamine, trimethylhexamethylenediamine, 1-piperazineethanamine, 3-(dimethylamino)-1-propylamine, 1,3-pentanediamine, 2-methyl-1,5-pentanediamine, N-(2-aminoethyl)-1,3-propanediamine, N,N'-1,2-ethanediylbis(1,3-propanediamine), dipropylenetriamine, m-xylylenediamine, p-xylylenediamine, 1,2-diaminocyclohexane, 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, 4,4'-methylenebis(cyclohexanamine), m-phenylenediamine, the 4,4'-diaminodiphenylmethane, l-(2-aminoethyl)piperazine and mixtures thereof.
[0085] Advantageously, the co-hardener is selected from diethylenetriamine, triethylenetetramine, pentaethylenehexamine, hexamethylenediamine, trimethylhexamethylenediamine, 1,3-pentanediamine, 2-methyl-1,5-pentanediamine, m-xylylenediamine, p-xylylenediamine, 1,2-diaminocyclohexane, l,3-bis(aminomethyl)cyclohexane, isophorone diamine, 4,4'-methylenebis(cyclohexanamine), m-phenylenediamine, 4,4'-diaminodiphenylmethane and mixtures thereof.
[0086] Preferably, the co-hardener is chosen from diethylenetriamine, triethylenetetramine, trimethylhexamethylenediamine, m-xylylenediamine, l,3-bis(aminomethyl)cyclohexane, isophorone diamine and mixtures thereof.
[0087] More preferably, the co-hardener is chosen from m-xylylenediamine, isophorone diamine, and mixtures thereof. In particular, the co-hardener is a mixture of m-xylylenediamine and isophorone diamine.
[0088] The co-hardener content in component (B) may range from 1% to 15% by weight relative to the total weight of component (B), preferably from 3% to 11% by weight. Reaction products (P)
[0089] The reaction products (P) correspond to the mixture of products obtained after reaction of on the one hand at least: a fatty acid, a polyamine (D1) and a compound (E) comprising at least one epoxide group (reaction products (PI)), and / or on the other hand at least: a dimerized fatty acid and a polyamine (D2) (reaction products (P2)).
[0090] By "fatty acid" is meant a molecule having a linear (unbranched) aliphatic chain, which may include one or more double bonds, and comprising a carboxylic acid group (-C(O)OH).
[0091] Advantageously, the fatty acid used to obtain the reaction products (RP) comprises between 4 and 28 carbon atoms, preferably between 10 and 22 carbon atoms, more preferably between 16 and 18 carbon atoms. In particular, the fatty acid is a mixture of tall oil fatty acids (also referred to as "TOFA" for "tall oil fatty acid" in English).
[0092] The term "polyamine" means a compound comprising at least two primary amine groups (-NH2), preferably exactly two primary amine groups. In addition to the primary amine groups, the polyamine (D1) and / or (D2) may comprise one or more secondary and / or tertiary amine groups.
[0093] The polyamines (D1) and (D2) used to obtain the reaction products (P) may be identical or different.
[0094] Advantageously, the polyamine (Dl) comprises one or more secondary amine groups and between 4 and 20 carbon atoms. In particular, the polyamine (Dl) is a polyethylenepolyamine of formula: H2N-(CH2-CH2-NH)y-CH2-CH2-NH2, in which y is an integer between 1 and 5, preferably equal to 1 or 2, especially equal to 2. Thus, when y is equal to 1 the polyamine (Dl) is diethylenetriamine (DETA), and when y is equal to 2 the polyamine (Dl) is triethylenetetramine (TETA).
[0095] The compound (E) comprises at least one epoxide group and can be selected from glycidyl ether derivatives.
[0096] Advantageously, compound (E) is selected from p-tolyl glycidyl ether (CAS: 2186-24-5), p-phenyl glycidyl ether (CAS: 122-60-1), 4-tert-butylphenyl glycidyl ether, cashew nut shell liquid reaction products and epichlorohydrin, C12-C14 alkyl glycidyl ethers, C13-C15 alkyl glycidyl ethers, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, polypropylene glycol diglycidyl ether, bisphenol A diglycidyl ether, ether diglycidic bisphenol E, diglycidic ether of 2,2-bis-(4-hydroxy-3-methylphenyl)propane, diglycidic ether of bisphenol B, diglycidic ether of 4,4'-, 2,4'- and / or 2,2'-bisphenol F, and mixtures thereof.
[0097] Preferably, compound (E) is selected from p-tolyl glycidyl ether, p-phenyl glycidyl ether, 4-tert-butylphenyl glycidyl ether, bisphenol A diglycidyl ether, 4,4'-, 2,4'- and / or 2,2'-bisphenol F diglycidyl ether, and mixtures thereof.
[0098] More preferably, compound (E) is chosen from p-tolyl glycidyl ether and / or bisphenol A diglycidyl ether, in particular a mixture of p-tolyl glycidyl ether and bisphenol A diglycidyl ether.
[0099] The compound (E) can be formed in situ, that is, the precursors of the compound (E) can be used to obtain the reaction products (P). For example, when the compound (E) comprises or is bisphenol A diglycidyl ether, the latter can be introduced in the form of a mixture of bisphenol A and
[0100]
[0101]
[0102]
[0103]
[0104] of epichlorohydrin. In particular, compound (E) is a mixture of p-tolyl glycidyl ether, bisphenol A and epichlorohydrin. According to one embodiment, the reaction products (IPs) are obtained by reacting at least: - a fatty acid comprising between 10 and 22 carbon atoms, - a polyamine (Dl) comprising, in addition to the at least two amine groups primary (-NH2), one or more secondary amine groups and between 4 and 20 carbon atoms, and - a compound (E) selected from p-tolyl glycidyl ether (CAS: 2186-24-5), p-phenyl glycidyl ether (CAS: 122-60-1), 4-tert-butylphenyl glycidyl ether, the reaction products of cashew nut shell liquid and epichlorohydrin, C12-C14 alkyl glycidyl ethers, C13-C15 alkyl glycidyl ethers, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, polypropylene glycol diglycidyl ether, bisphenol A diglycidyl ether, bisphenol E diglycidyl ether, ether 2,2-bis-(4-hydroxy-3-methylphenyl)propane diglycidic ether, bisphenol B diglycidic ether, 4,4'-, 2,4'- and / or 2,2'-bisphenol F diglycidic ether, and mixtures thereof. Preferably, the reaction products (RPs) are obtained by reacting at least: - a fatty acid comprising between 4 and 28 carbon atoms, - a polyamine (Dl) being a polyethylenepolyamine of formula: H2N-(CH2 - CH2-NH)y-CH2- CH2-NH2, where y is an integer between 1 and 5, and - a compound (E) selected from p-tolyl glycidyl ether, p-phenyl glycidyl ether, 4-tert-butylphenyl glycidyl ether, bisphenol A diglycidyl ether, 4,4'-, 2,4'- and / or 2,2'-bisphenol F diglycidyl ether, and mixtures thereof. More preferably, the reaction products (RPs) are obtained by reacting at least: - a fatty acid comprising between 16 and 18 carbon atoms, - a polyamine (Dl) being a polyethylenepolyamine of formula: H2N-(CH2 - CH2-NH)y-CH2- CH2-NH2, where y is an integer equal to 1 or 2, and - a compound (E) selected from p-tolyl glycidyl ether and / or bisphenol A diglycidyl ether. In particular, reaction products (RPs) are obtained by reaction: - a mixture of fatty acids from tall oil, - of triethylenetetramine as a polyamine (Dl), and - of a mixture of p-tolyl glycidyl ether, bisphenol A and epichlorohydrin as compound (E).
[0105] These particular reaction products (RPs) are identified by CAS number 186321-96-0.
[0106] The term "dimerized fatty acid" means a compound obtained by dimerization of fatty acids comprising one or more double bonds. Unlike fatty acids, dimerized fatty acids are not linear.
[0107] Advantageously, the dimerized fatty acid comprises between 8 and 48 carbon atoms, preferably between 32 and 40 carbon atoms, more preferably 36 carbon atoms.
[0108] Advantageously, the polyamine (D2) comprises one or more secondary amine groups and between 4 and 20 carbon atoms. In particular, the polyamine (D2) is a polyethylenepolyamine of formula: H2N-(CH2-CH2-NH)y-CH2-CH2-NH2, in which y is an integer between 1 and 5, preferably equal to 1 or 2, in particular equal to 2.
[0109] Advantageously, a fatty acid is further used to obtain the reaction products (P2). Preferably, the fatty acid used to obtain the reaction products (P2) comprises between 4 and 28 carbon atoms, preferably between 10 and 22 carbon atoms, and more preferably between 16 and 18 carbon atoms. In particular, the fatty acid is a mixture of tall oil fatty acids.
[0110] According to one embodiment, the reaction products (P2) are obtained by reacting at least: - a dimerized fatty acid comprising between 8 and 48 carbon atoms, - a polyamine (D2) comprising, in addition to at least two primary amine groups (-NH2), one or more secondary amine groups and between 4 and 20 carbon atoms, and - optionally a fatty acid comprising between 4 and 28 carbon atoms.
[0111] Preferably, the reaction products (P2) are obtained by reacting at least: - a dimerized fatty acid comprising between 32 and 40 carbon atoms, - a polyamine (D2) being a polyethylenepolyamine of formula: H2N-(CH2 - CH2-NH)y-CH2- CH2-NH2, in which y is an integer between 1 and 5, and - optionally a fatty acid comprising between 10 and 22 carbon atoms.
[0112] More preferably, the reaction products (P2) are obtained by reacting at least: a dimerized fatty acid comprising 36 carbon atoms, a polyamine (D2) being a polyethylenepolyamine of formula: H2N-(CH2 - CH2-NH)y-CH2- CH2-NH2, in which y is an integer equal to 1 or 2, and - a fatty acid comprising between 16 and 18 carbon atoms.
[0113] In particular, the reaction products (P2) are obtained by reaction of: - dimerized fatty acid(s) comprising 36 carbon atoms, - triethylenetetramine as polyamine (D2), and - a mixture of tall oil fatty acids.
[0114] These latter particular reaction products (P2) bear the CAS number 68082-29-1.
[0115] Advantageously, the reaction products (P) are the reaction products (IP), the reaction products (IP) being as described above, including preferred features and embodiments. Thus, the reaction products (P) are in particular identified by CAS number 186321-96-0.
[0116] The content of reaction products (P) in component (B) is advantageously between 5% and 37% by weight relative to the total weight of component (B), preferably between 7% and 32% by weight, more preferably between 10% and 27% by weight. Lamellar charge (C)
[0117] Component (A) and / or component (B) further comprises at least 20% by weight, relative to the total weight of said component, of a lamellar filler (C). Preferably, the lamellar filler (C) is present only in component (B).
[0118] The charge (C) is said to be lamellar because it is in the form of a set of sheets, adjacent to each other.
[0119] Mica iron oxide is a type of hematite and can be synthetic or natural. The micaceous iron oxide used in the present invention is preferably natural.
[0120] Vermiculite belongs to the group of clays.
[0121] Mica refers to a group of phyllosilicates based on potassium, sodium, aluminum, magnesium and / or iron.
[0122] Preferably, the lamellar filler (C) is micaceous iron oxide, for example MIOX® SG marketed by Kärntner Montanindustrie or IRONOR® P marketed by CMMP.
[0123] Advantageously, at least 65% of the particles constituting the lamellar charge (C) are lamellar particles (relative to the total number of particles constituting said charge), preferably at least 75%, more preferably at least 80%.
[0124] The content of lamellar particles can be determined by microscopic examination, for example in accordance with ISO 10601.
[0125] The lamellar load (C) can be of type 2 according to ISO 10601.
[0126] The lamellar filler content (C) can range from 20% to 65% by weight relative to the total weight of the component in which it is present (preferably (B)), preferably 30% to 60% by weight, more preferably 40% to 55% by weight. Accelerator
[0127] Advantageously, component (B) further comprises an accelerator.
[0128] The accelerator can be any accelerator known to a person skilled in the art to accelerate the crosslinking of epoxy resin.
[0129] The accelerator can be chosen from alcohols comprising an aromatic ring and tertiary amines.
[0130] Advantageously, the accelerator is an isomer of nonylphenol, benzyl alcohol, resorcinol, 2-phenoxyethanol, styrene phenol (CAS: 61788-44-1), bisphenol A, cardanol, salicylic acid, triethanolamine, benzyldimethylamine and / or 2,4,6-tris(dimethylaminomethyl)phenol, preferably benzyl alcohol, styrene phenol and / or 2,4,6-tris(dimethylaminomethyl)phenol, more preferably benzyl alcohol, styrene phenol and 2,4,6-tris(dimethylaminomethyl)phenol.
[0131] By "nonylphenol isomer" is meant a phenol having an aliphatic substituent with 9 carbon atoms. The nonylphenol isomer may, for example, be 4-(2,4-dimethylheptan-3-yl)phenol or 4-(3,6-dimethylheptan-3-yl)phenol.
[0132] The accelerator content may vary from 1% to 30% by weight relative to the total weight of component (B), preferably from 7% to 27% by weight, more preferably from 10% to 24% by weight. Component additives (B)
[0133] Component (B) may further comprise one or more additives selected from plasticizers, mineral fillers, pigments, debubbling agents, thickeners and mixtures thereof, in particular from thickeners.
[0134] The total content of the aforementioned additives, excluding mineral fillers, may range from 0.01% to 10% by weight relative to the total weight of component (B), preferably from 0.1% to 5% by weight, more preferably from 0.2% to 3% by weight.
[0135] Component (B) may comprise up to 5% by weight of plasticizer relative to the total weight of component (B), preferably up to 2% by weight.
[0136] The plasticizer can for example be chosen from mineral oils of petroleum origin, paraffinic oils, polyolefins, esters of benzoic, phthalic, trimellitic, pyromellitic, adipic, sebacic, fumaric, maleic, itaconic and citric acid, and mixtures thereof.
[0137] The mineral filler is different from the lamellar filler (C), and can be selected from carbonate fillers (such as calcium carbonate or dolomite), quartz, barium sulfate, nepheline syenite, glass beads, hollow mineral microspheres (for example, of sodium and calcium borosilicate or in aluminosilicate), and their mixtures.
[0138] Component (B) may comprise up to 20% by weight of mineral filler per relative to the total weight of component (B). When component (B) already includes a lamellar filler (C), the mineral filler content (other than the lamellar filler (C)) is preferably chosen so that the total filler content (mineral and lamellar (C)) does not exceed 65% by weight relative to the total weight of component (B).
[0139] Component (B) may comprise up to 3% by weight of pigment relative to the total weight of component (B), preferably up to 2% by weight.
[0140] The pigment can be an organic or inorganic pigment, for example based on TiO2 (such as TRONOX's TIONA® 595) or based on manganese ferrite (such as LANXESS's BAYFERROX® 303 T).
[0141] Component (B) may include a debubbling agent.
[0142] The debubbling agent can be any debubbling agent commonly used in epoxy resin-based compositions.
[0143] By way of example, silicone oil in a hydrotreated light distillate (petroleum) solvent (CAS: 64742-47-8) and a polyolefin in a light aromatic naphtha (petroleum) solvent (CAS: 64742-95-6) are examples. Commercial examples include Münzig's AGIT AN® DF 311 M and BYK Chemie's BYK 057.
[0144] The content of debubbling agent in component (B) may be up to 1% by weight relative to the total weight of component (B), preferably up to 0.5% by weight.
[0145] Advantageously, component (B) further comprises a thickener.
[0146] The thickener may be silica, which may be pyrogenated or precipitated, optionally hydrophobic, preferably pyrogenated silica. Advantageously, the thickener is pyrogenated (hydrophilic) silica.
[0147] The thickener content may vary from 0.01% to 5% by weight relative to the total weight of component (B), preferably from 0.1% to 2% by weight, more preferably from 0.4% to 1.0% by weight. Other characteristics of component (B)
[0148] The weight ratio of reaction products (P) / hardener (H) may be greater than or equal to 0.6, preferably between 0.6 and 5, more preferably between 0.8 and 4, for example between 1 and 3.
[0149] According to one embodiment, component (B) comprises: - between 3% and 30% by weight of hardener (H) relative to the total weight of the component (B), - 15% by weight of co-hardener relative to the total weight of component (B), - from 20% to 65% by weight of lamellar load (C) relative to the total weight of the component (B), - between 5% and 37% by weight of reaction products (P) relative to the total weight of the component (B), - from 1% to 30% by weight of accelerator relative to the total weight of component (B), - from 0.01% to 10% by weight of one or more additives selected from plasticizers, pigments, debubbling agents, thickeners and mixtures thereof, relative to the total weight of component (B), and - optionally up to 20% by weight of mineral filler other than lamellar filler (C) relative to the total weight of the component (B).
[0150] Preferably, component (B) consists essentially of the ingredients mentioned above. By "consists essentially" means that component (B) comprises less than 5% by weight of ingredients other than the aforementioned ingredients, relative to the total weight of component (B), preferably less than 2% by weight, and even more preferably less than 1% by weight.
[0151] The ingredients of this embodiment and their particular contents are as described above, including preferred characteristics and embodiments.
[0152] According to a particular embodiment, component (B) comprises: - between 5% and 18% by weight of hardener (H) relative to the total weight of component (B), the hardener (H) preferably being a phenalkamine represented by formula (I) in which R2 represents a group of formula (Ilia), (Illb), (IIIc) or (Illd), R4 represents a hydrogen atom, and the substituents R1, R3 and R5 not being of formula (II) are hydrogen atoms, - 3% to 10% by weight of co-hardener relative to the total weight of component (B), the co-hardener preferably being chosen from m-xylylenediamine, isophorone diamine and their mixture, - 40% to 55% by weight of lamellar filler (C) relative to the total weight of the component (B), the lamellar filler (C) preferably being micaceous iron oxide, - between 10% and 27% by weight of reaction products (P) relative to the total weight of component (B), the reaction products (P) preferably being the reaction products (PI), in particular the reaction products (PI) obtained by reaction of at least: • a fatty acid comprising between 16 and 18 carbon atoms, • a polyamine (Dl) being a polyethylenepolyamine with the formula: H 2N-(CH2-CH2-NH)y-CH2-CH2-NH2, where y is an integer equal to 1 or 2, and • a compound (E) selected from p-tolyl glycidyl ether and / or bisphenol A diglycidyl ether, - 10% to 24% by weight of accelerator relative to the total weight of component (B), the accelerator preferably being an isomer of nonylphenol, benzyl alcohol, resorcinol, 2-phenoxyethanol, styrene phenol, bisphenol A, cardanol, salicylic acid, triethanolamine, benzyldimethylamine and / or 2,4,6-tris(dimethylaminomethyl)phenol, and - from 0.2% to 3% by weight of one or more additives chosen from plasticizers, pigments, debubbling agents, thickeners and their mixtures, relative to the total weight of component (B), in particular from thickeners.
[0153] Preferably, component (B) consists essentially of the ingredients mentioned above.
[0154] The ingredients of this embodiment and their particular contents are as described above, including preferred characteristics and embodiments.
[0155] Other features of the two-component composition according to the invention
[0156] The ratio of components (A) and (B) in the two-component composition according to the invention can be determined with respect to the epoxy equivalent weight (or EEW for "epoxy equivalent weight" in English) of component (A) and the active hydrogen equivalent weight (or AHEW for "active hydrogen equivalent weight" in English) of component (B).
[0157] The epoxy equivalent weight of an ingredient (in g / eq) corresponds to the weight in grams of said ingredient required to have 1 mole of epoxide groups.
[0158] It can be measured in accordance with ASTM D 1652.
[0159] Unless otherwise indicated, the standards referred to throughout the application are those in force at the date of filing of the application.
[0160] The epoxy equivalent weight of component (A) is calculated on the basis of each of the ingredients e of component (A) comprising at least one epoxide group: EEWA = mA / (S(me / EEWe)), where EEWA is the epoxy equivalent weight of component (A) in grams of (A) for 1 mole of epoxide groups, mA is the total mass in grams of component (A), mL is the mass in grams in (A) of an ingredient e comprising at least one epoxide group, and EEWe is the average epoxy equivalent weight of ingredient e in grams of i for 1 mole of epoxide groups.
[0161] The equivalent weight in active hydrogen of an ingredient (in g / eq) corresponds to the weight in grams of said ingredient required to have 1 mole of active hydrogen, i.e. of hydrogen atoms bonded to a nitrogen atom.
[0162] It can be calculated from the molar mass of the ingredient and is given by the supplier of the ingredient.
[0163] The equivalent weight of active hydrogen of component (B) is calculated on the basis of each of the ingredients h of component (B) comprising at least one primary or secondary amine group: AHEWB = mB / (S(mh / AHEWh)), where AHEWB is the equivalent weight in active hydrogen of component (B) in grams of (B) for 1 mole of active hydrogen, mB is the total mass in grams of component (B), mh is the mass in grams in (B) of an ingredient h comprising at least one primary or secondary amine group, and AHEWh is the average equivalent weight in active hydrogen of ingredient h in grams of h for 1 mole of active hydrogen.
[0164] The ratio of components (A) and (B) in the two-component composition according to the invention is advantageously chosen so that the ratio AHEWb / EEWa is greater than or equal to 1, preferably greater than or equal to 1.0, more preferably between 1.0 and 2.0, even more preferably between 1.0 and 1.5, AHEWb being the equivalent weight in active hydrogen of component (B) in grams of (B) for 1 mole of active hydrogen and EEWA being the equivalent epoxy weight of component (A) in grams of (A) for 1 mole of epoxy groups.
[0165] The two-component composition according to the invention advantageously has a solvent content of less than 3% by weight relative to the total weight of the two-component composition, preferably less than 1% by weight, more preferably less than 0.5% by weight.
[0166] This allows for a two-component composition that can be applied to a high basis weight on a surface. In particular, the two-component composition according to the invention can be applied to a basis weight of at least 300 g / m², preferably at least 450 g / m², notably between 450 g / m² and 700 g / m².
[0167] Solvents are well known to those skilled in the art and are used in particular to dilute, dissolve or suspend other compounds without chemically altering them and without themselves being altered.
[0168] Advantageously, the two-component composition according to the invention has low emissions of volatile organic compounds (VOCs). In particular, the total VOC concentration expressed in toluene equivalents 3 days after application of said composition is advantageously less than or equal to 3000 pg / m3, preferably less than or equal to 1000 pg / m3, and after 28 days is advantageously less than or equal to 300 pg / m3, preferably less than or equal to 200 pg / m3.
[0169] The total VOC concentration expressed in toluene equivalents can be determined in accordance with EN 16516, by implementing a two-component composition layer applied at a basis weight of 300 g / m2 and at an AHEWB / EEWA ratio of 1.1.
[0170] Advantageously, the two-component composition according to the invention is essentially free of ingredients classified as CMR (carcinogenic, mutagenic and / or reprotoxic) and SVHC (substances of very high concern).
[0171] By "essentially free", we mean in particular a content of ingredients classified as CMR or SVHC of less than 5% by weight, preferably less than 3% by weight, in relation to the total weight of the two-component composition; more preferably, the two-component composition according to the invention is totally free of ingredients classified as CMR and SVHC.
[0172] According to one embodiment, the two-component composition according to the invention comprises: - a component (A) comprising: • at least 50% by weight of aromatic epoxy resin relative to the total weight of component (A), • 1% to 30% by weight of reactive diluent relative to the total weight of component (A), • optionally from 0.01% to 10% by weight of one or more additives selected from plasticizers, thickeners, pigments, debubbling agents and mixtures thereof, relative to the total weight of component (A), and • optionally up to 20% by weight of mineral filler other than lamellar filler (C) relative to the total weight of the component (A), and - a component (B) comprising: • between 3% and 30% by weight of hardener (H) relative to the total weight of the component (B), • 15% by weight of co-hardener relative to the total weight of component (B), • 20% to 65% by weight of lamellar load (C) relative to the total weight of the component (B), • between 5% and 37% by weight of reaction products (P) relative to the total weight of the component (B), • 1% to 25% by weight of accelerator relative to the total weight of component (B), • from 0.01% to 10% by weight of one or more additives selected from plasticizers, pigments, debubbling agents, thickeners and mixtures thereof, relative to the total weight of component (B), and • optionally up to 20% by weight of mineral filler other than lamellar filler (C) relative to the total weight of the component (B).
[0173] Preferably, the two-component composition according to the invention consists essentially of the ingredients mentioned above. By "consists essentially of" means that the two-component composition comprises less than 5% by weight of ingredients other than the aforementioned ingredients, relative to the total weight of the two-component composition, preferably less than 2% by weight, even more preferably less than 1% by weight.
[0174] The ingredients of this embodiment and their particular contents are as described above, including preferred characteristics and embodiments.
[0175] According to a particular embodiment, the two-component composition according to the invention comprises: - a component (A) comprising: • 70% to 95% by weight of aromatic epoxy resin relative to the total weight of component (A), the aromatic epoxy resin preferably being selected from the diglycidic ethers of 2,2-bis-(4-hydroxyphenyl)propane (bisphenol A), 4,4'-methylenediphenol (4,4'-bisphenol F isomer), 2,4'-methylenediphenol (2,4'-bisphenol F isomer), 2,2'-methylenediphenol (2,2'-bisphenol F isomer) and mixtures thereof, • 4% to 17% by weight of reactive diluent relative to the total weight of component (A), the reactive diluent preferably being selected from the glycidic ether of 4-tert-butylphenyl, the reaction products of cashew nut shell liquid and epichlorohydrin, C12-C14 alkyl glycidic ethers, ethers glycidyl compounds of C13-C15 alkyls and their mixtures, and • optionally from 0.03% to 3% by weight, relative to the total weight of component (A), of one or more additives selected from plasticizers, pigments, debubbling agents and mixtures thereof, in particular from debubbling agents, and - a component (B) comprising: • between 5% and 18% by weight of hardener (H) relative to the total weight of component (B), the hardener (H) preferably being a phenalkamine represented by formula (I) in which R2 represents a group of formula (Ilia), (Illb), (IIIc) or (Illd), R4 represents a hydrogen atom, and the substituents R1, R3 and R5 not being of formula (II) are hydrogen atoms, • 3% to 10% by weight of co-hardener relative to the total weight of component (B), the co-hardener preferably being chosen from m-xylylenediamine, isophorone diamine and their mixture, • 40% to 55% by weight of lamellar filler (C) relative to the total weight of the component (B), the lamellar filler (C) preferably being micaceous iron oxide, • between 10% and 27% by weight of reaction products (P) relative to the total weight of component (B), the reaction products (P) preferably being the reaction products (PI), in particular the reaction products (PI) obtained by reaction of at least: - a fatty acid comprising between 16 and 18 carbon atoms, - a polyamine (Dl) being a polyethylenepolyamine of formula: H2N-(CH2-CH2-NH)y-CH2-CH2-NH2, where y is an integer equal to 1 or 2, and - a compound (E) selected from p-tolyl glycidyl ether and / or bisphenol A diglycidyl ether, • 10% to 24% by weight of accelerator relative to the total weight of component (B), the accelerator preferably being an isomer of non-nylphenol, benzyl alcohol, resorcinol, 2-phenoxyethanol, styrene phenol, bisphenol A, cardanol, salicylic acid, triethanolamine, benzyldimethylamine and / or 2,4,6-tris(dimethylaminomethyl)phenol, and • 0.2% to 3% by weight of one or more additives chosen from plasticizers, pigments, debubbling agents, thickeners and mixtures thereof, relative to the total weight of component (B), in particular from thickeners.
[0176] Preferably, the two-component composition according to the invention consists essentially of the ingredients mentioned above.
[0177] The ingredients of this embodiment and their particular contents are as described above, including preferred characteristics and embodiments.
[0178] The two-component composition according to the invention advantageously has a viscosity at 23°C of less than 2,800 mPa.s.
[0179] The viscosity of the two-component composition according to the invention can be determined using a Brookfield LVT viscometer, for example as described in Example 1 below.
[0180] The two-component composition according to the invention advantageously has a Persoz hardness greater than or equal to 10 s, preferably greater than or equal to 12 s, less than 6 h, preferably less than 5 h after its application at a temperature of about 21°C and at ambient humidity (in particular at between 30% and 80% relative humidity, for example at 30% relative humidity). Preferably, the two-component composition according to the invention has a Persoz hardness greater than or equal to 10 s, preferably greater than or equal to 12 s, 4 h or less after its application under the temperature and humidity conditions mentioned above.
[0181] The Persoz hardness can be determined using a Persoz pendulum, for example such as as described in Example 1.
[0182] Advantageously, the two-component composition according to the invention exhibits adhesion to wet concrete greater than 3 MPa, in particular greater than or equal to 4 MPa. Preferably, the two-component composition according to the invention exhibits sufficiently high adhesion to wet concrete to achieve cohesive failure of the concrete at more than 90% during the adhesion test (and not delamination of the layer formed by the two-component composition).
[0183] Adhesion on wet concrete can be measured in accordance with EN 13578:2003, for example as described in Example 1.
[0184] The two-component composition according to the invention advantageously has a water vapor permeance of less than or equal to 10 mg / h / m² / mmHg, which allows its use as a moisture barrier. Preferably, the two-component composition according to the invention has a water vapor permeance of less than or equal to 8 mg / h / m² / mmHg.
[0185] Water vapor permeance can be determined by measuring water vapor permeability according to standard NF EN ISO 7783:2011 (wet cup method), for example as described in Example 1.
[0186] Advantageously, the mixing life at 21 °C of the two-component composition according to the invention is between 20 min and 60 min, preferably between 20 min and 50 min.
[0187] The mixture life can be determined as described in Example 1 below.
[0188] Preparation of the two-component composition according to the invention
[0189] Each of the components (A) and (B) of the two-component composition according to the invention is prepared separately, by simple mixing of its ingredients, preferably under vacuum for component (B).
[0190] By "under vacuum" is meant a pressure lower than atmospheric pressure, advantageously between 0.1 kPa and 10 kPa, preferably between 0.5 kPa and 5 kPa.
[0191] The two-component composition according to the invention can be prepared just before its use by mixing the components (A) and (B), for example using a rotary mixer equipped with a whisk, at room temperature, in particular between 18°C and 28°C, and at atmospheric pressure.
[0192] An example of the preparation of components (A) and (B) and of the two-component composition according to the invention is described in Example 2. Other objects of the present invention
[0193] The present invention also relates to the use of the two-component composition according to the invention as a moisture barrier, particularly in the field of buildings.
[0194] The present invention also relates to a moisture barrier obtained after hardening of the two-component composition according to the invention.
[0195] In particular, the hardening time corresponds to the time required for the two-component composition according to the invention to have a Persoz hardness as described above (advantageously a Persoz hardness greater than or equal to 10 s, preferably greater than or equal to 12 s).
[0196] The moisture barrier according to the invention advantageously has a water vapor permeance less than or equal to 10 mg / h / m2 / mmHg, preferably less than or equal to 8 mg / h / m2 / mmHg.
[0197] Water vapor permeance can be determined by measuring water vapor permeability according to standard NF EN ISO 7783:2011 (wet cup method), for example as described in Example 1.
[0198] The present invention also relates to a method of sealing a surface comprising applying the two-component composition according to the invention to said surface and then hardening said composition to form a moisture barrier, particularly at room temperature (in particular between 18°C and 28°C).
[0199] The surface may in particular be concrete.
[0200] In particular, the hardening time corresponds to the time required for the two-component composition according to the invention to have a Persoz hardness as described above.
[0201] Preferably, no primary layer is present between the moisture barrier according to the invention and the surface to be sealed.
[0202] The two-component composition according to the invention can be applied to a basis weight of at least 300 g of said composition per m2 of said surface, preferably of at least 400 g / m2, in particular between 450 g / m2 and 550 g / m2.
[0203] The two-component composition according to the invention can be applied using a notched spatula.
[0204] Preferably, the method for sealing a surface according to the invention comprises a single step of applying the two-component composition according to the invention. Thus, the moisture barrier according to the invention is preferably "single-layer".
[0205] Advantageously, the surface sealing process according to the invention is implemented in less than 6 hours, preferably in less than 5 hours. Thus, the moisture barrier is advantageously fully formed in less than 6 hours, preferably in less than 5 hours.
[0206] Finally, the present invention relates to a soil preparation process comprising: - applying the two-component composition according to the invention to the soil surface, then - the hardening of said composition to form a moisture barrier, And - preparing a surface suitable for the application of a self-leveling compound, then - the application of a self-smoothing composition.
[0207] In particular, the hardening time corresponds to the time required for the two-component composition according to the invention to have a Persoz hardness as described above.
[0208] The soil preparation process can be carried out at ambient temperature (in particular between 18°C and 28°C) and at ambient humidity (in particular between 30% and 80% relative humidity, especially at 30%).
[0209] The ground surface may be the surface described above, in particular concrete.
[0210] Preferably, no primary layer is present between the moisture barrier and the surface of the ground.
[0211] The application of the two-component composition according to the invention is as described above, in particular with regard to the basis weight.
[0212] Preferably, the soil preparation process according to the invention comprises a single step of applying the two-component composition according to the invention. Thus, the moisture barrier according to the invention is preferably "single-layer".
[0213] Preparing a surface suitable for the application of a self-leveling compound improves the adhesion of the self-leveling compound to the ground. This step can be a sandblasting step of the two-component compound according to the invention or a step of applying a bonding coat to the cured moisture barrier.
[0214] The sandblasting step is carried out before the hardening of the two-component composition according to the invention. During this step, mineral particles (for example, sand, corundum, or vitrified slag) are projected onto said composition in order to create a rough surface.
[0215] The tack coat can be any tack coat known to a person skilled in the art to improve adhesion between a self-leveling composition and a composition comprising an epoxy resin.
[0216] Advantageously, the tack coat is an aqueous phase emulsion formulation loaded with sand.
[0217] The self-leveling compound allows the floor to be smoothed to obtain a perfectly horizontal surface. It can be any self-leveling compound known to those skilled in the art.
[0218] Advantageously, the self-leveling composition is cement-based, for example MANGSOL 3 marketed by BOSTIK.
[0219] Advantageously, the soil preparation process according to the invention is carried out in less than 10 hours, preferably in less than 8 hours. Thus, the preparation process The floor according to the invention can be implemented in one day, and a floor covering such as parquet or linoleum can be laid on the sealed floor after 24 to 72 hours depending on the covering.
[0220] All the embodiments described above can be combined with each other. In particular, the various aforementioned ingredients of the two-component composition according to the invention, and especially the preferred embodiments, can be combined with each other.
[0221] The following examples are given purely for illustrative purposes of the invention and should not be interpreted as limiting its scope. Examples Example 1: Ingredients and measurement methods Ingredients used
[0222] The following ingredients were used: - RE1 epoxy resin: bisphenol A diglycidic ether (CAS: 1675-54-3) having an average EEW of approximately 187 g / eq; - RE2 epoxy resin: mixture having an average EEW of about 175 g / eq and comprising about 50% by weight of bisphenol A diglycidyl ether and about 50% by weight of bisphenol F isomers diglycidyl ethers (reaction products of bisphenol F 4,4'-, 2,2'- and 2,4'- isomers and epichlorohydrin, CAS 9003-36-5), the weight percentages being relative to the total weight of the mixture; - Grilonit® Epoxide 8 marketed by EMS-GRILTECH: C12-C14 alkyl glycine ethers (CAS: 68609-97-2) having an average EEW of approximately 285 g / eq, reactive diluent; - AGIT AN® DF 311 M marketed by Münzing: silicone oil in a hydrotreated light distillate (petroleum) solvent (CAS: 64742-47-8), debubbling agent; - ARADUR® 450-1 S marketed by HUNTSMAN: mixture having an AHEW of about 115 g / eq and comprising between 30% and 60% by weight of the reaction products (P) of tall oil fatty acids with bisphenol A, epichlorohydrin, glycidyltolyl ether and triethylenetetramine (CAS: 186321-96-0), between 13% and 30% by weight of benzyl alcohol, between 7% and 13% by weight of isophorone diamine, between 7% and 13% by weight of styrene phenol, between 5% and 10% by weight of m-xylylenediamine and between 3% and 7% by weight of 2,4,6-tris(dimethylaminomethyl)phenol, the percentages by weight being relative to the total weight of the mixture; - Phenalkamine H1: AHEW of approximately 95 g / eq, obtained notably from cardanol, formaldehyde and polyethyleneamine, hardener; - ANCAMINE K54 marketed by EVONIK: 2,4,6-tris(dimethylaminomethyl)phenol (CAS: 90-72-2), accelerator; - MIOX® SG marketed by Kârntner Montanindustrie: micaceous iron oxide, lamellar filler; - HD K® N20 marketed by Wacker: hydrophilic fumed silica, thickener; - EPIKOTE™ Resin 240 marketed by HEXION: mixture having an average EEW of about 190 g / eq and comprising between 50% and 75% by weight of bisphenol A diglycidic ether, between 25% and 35% by weight of bisphenol F isomers diglycidic ethers (CAS: 9003-36-5) and between 10% and 20% by weight of C12-C14 alkyl glycidic ethers (CAS: 68609-97-2), the percentages by weight being relative to the total weight of the mixture, epoxy resin; - BYK-A 530 marketed by BYK: silicone oil in a solvent based on hydrotreated light distillates (petroleum) (CAS: 64742-47-8), debubbling agent. Measurement methods
[0223] The viscosity is determined immediately after obtaining the two-component composition at 30 rpm (revolutions per minute) and at 23°C using a Brookfield LVT viscometer and a No. 3 needle.
[0224] The pot life of the mixture is determined at 21°C for 1 kg of the two-component composition and corresponds to the time available to use the product once the mixture has been prepared. It is determined from the temperature-time curve of the mixture. Tangent lines are then drawn at the beginning of the curve on one side and at the exothermic peak on the other. The intersection of these two lines gives the pot life value of the mixture.
[0225] The hardness of the films obtained is evaluated using a Persoz pendulum. For this purpose, the composition to be evaluated is applied immediately after its preparation to a glass plate approximately 300 µm thick using a filmograph. The plate is then placed in a climatic chamber set at 21°C and 30% relative humidity. After the desired delay, here 4 hours, the plate is placed on the device and the measurement is taken.
[0226] Adhesion to wet concrete is measured in accordance with EN 13578:2003. The two-component composition is applied at 10°C to a concrete slab conforming to NF EN 12004-2, with 500 g of said composition per m² of surface area. The concrete slab is then kept in a water bath for the duration of the test, with the water level 1 cm below the surface of the concrete coated with said composition. Adhesion is then evaluated after 28 days. exposure to a water bath at 10°C by a tensile test with a SATTEC manual adhesion device in accordance with standard NF EN 1542.
[0227] Water vapor permeability is evaluated on a loose film according to standard NF EN ISO 7783:2011 (wet cup method). To produce the films, the composition to be evaluated is applied immediately after preparation to a suitable substrate, for example, a PET (polyethylene terephthalate) film with a basis weight of approximately 700 g / m². After the product has hardened, the film is cut to the diameter of the cup, and the substrate is removed. The resulting discs are then conditioned for at least 14 days at 23°C and 50% relative humidity.
[0228] In the wet cup method, the film to be evaluated separates a high-humidity atmosphere (93% relative humidity obtained with a saturated solution of ammonium dihydrogen phosphate) from a moderate-humidity atmosphere (50% relative humidity) obtained in a climatic chamber. The test is carried out at 23°C. The water vapor flux through the film is controlled by regularly weighing the cup. The water vapor permeance corresponds to the water vapor permeability of the film (in mg / h / m / mmHg) divided by its thickness (in m).
[0229] Example 2: Two-component composition 1 according to the invention
[0230] In a reactor maintained under stirring, the various ingredients of component IA are mixed in the proportions indicated in Table 1 below, in several stages according to the process described below. The mixer is at ambient temperature (approximately 23°C) before the ingredients are added.
[0231] In a mixer, the different ingredients of component IA are mixed in the proportions indicated in Table 1 below, until a homogeneous mixture is obtained.
[0232] [Tables 1] Ingredient % by weight relative to the total weight of component IA epoxy resin RE1 61.9 epoxy resin RE2 23.7 Grilonit® Epoxide 8 14.3 AGIT AN® DF 311 M 0.1
[0233] In a mixer equipped for vacuum, the various ingredients of component IB are mixed in the proportions indicated in Table 2 below, in several stages according to the process described below. The mixer is at ambient temperature (approximately 23°C) before the ingredients are added.
[0234] The ingredients of step 1 are mixed under vacuum (approximately between 1 and 2 kPa) for about 10 minutes and at a sufficient stirring speed to homogenize.
[0235] Next, the ingredient from step 2 is added to the mixer used for step 1, and mixed for about 10 minutes to form a paste.
[0236] Finally, the ingredient from step 3 is added to the mixer, mixed for about 10 minutes to form a paste, then the whole thing is mixed under vacuum for 30 minutes.
[0237] [Tables2] Step Ingredient % by weight relative to the total weight of component IB 1 ARADUR® 450-1 S 41.45 Phenalkamine H1 7.8 ANCAMINE K54 2.6 2 HDK® N20 1.0 3 MIOX® SG 47.15
[0238] Composition 1 according to the invention is then obtained by mixing components IA and IB at room temperature (23°C) so that the ratio AHEWiB / EEWia is equal to 1.0 (i.e. a weight ratio 1B / 1A equal to 0.86), for example using a rotary mixer equipped with a whisk.
[0239] Example 3: comparative two-component composition 2
[0240] Comparative two-component composition 2 corresponds to a standard moisture barrier composition. It consists of a component 2A made up of EPIKOTE™ Resin 240, and a component 2B whose composition is indicated in Table 3 below.
[0241] Component 2B is prepared in several steps according to the process described in Example 2 for component IB.
[0242] [Tables3] Step Ingredient % by weight relative to the total weight of component 2B 1 ARADUR® 450-1 S 41.7 BYK-A 530 0.8 2 HDK® N20 1.2 3 MIOX® SG 56.3
[0243] The comparative composition 2 is then obtained by mixing components 2A and 2B at room temperature (23°C) so that the ratio AHEW2b / EEW2a is equal to 1.0, for example using a rotary mixer equipped with a whisk.
[0244] Example 4: Mechanical properties of compositions 1 and 2
[0245] The mechanical properties of composition 1 according to the invention and of composition 2 comparative (measured in accordance with Example 1) are summarized in Table 4 below.
[0246] [Tables4] Composition 1 (invention) 2 (comparative) Viscosity at 23°C (mPa.s) 1450 2000 Pot life (min) 42 60 Persoz hardness at 4 h (s) 13 not measurable Adhesion to wet concrete (MPa) >3 (RB) 3.9 (RB) Permeance (mg / h / m2 / mmHg) 8 ND
[0247] ND: not determined; RB: concrete failure
[0248] The viscosity of composition 1 according to the invention allows for easy application and its mixing life is sufficient for the duration of the application.
[0249] Composition 1 according to the invention has good adhesion to wet concrete. Indeed, during the measurement of this adhesion, the concrete broke before the film of composition 1 detached.
[0250] Furthermore, composition 1 according to the invention has good moisture-resistant properties. Indeed, in France and in this field of application, a product is considered a moisture barrier when the permeance measured according to Example 1 is less than or equal to 10 mg / h / m2 / mmHg.
[0251] Furthermore, composition 1 according to the invention has the advantage of hardening much more quickly than the comparative composition 2 (standard moisture barrier composition). Indeed, after only 4 hours, composition 1 according to the invention has sufficient hardness to allow the application of a different layer, in particular a bonding coat, while the comparative composition 2 is still liquid. Composition 1 according to the invention therefore makes it possible to carry out, in a single day, instead of two days for composition 2, the preparation of a floor including the application of a moisture barrier (composition 1), the application of a bonding coat (or alternatively sanding) followed by the application of a self-leveling compound.
[0252] Finally, composition 1 according to the invention has the advantage of not containing a significant amount of solvent, has low emissions of volatile organic compounds (VOCs) and does not include any CMR or SVHC ingredients, which limits its toxicity.
Claims
Claims
1. Two-component composition comprising: - a component (A) comprising: • at least one aromatic epoxy resin, and - a component (B) comprising: • a hardener (H) chosen from phenolic Mannich bases having at least one primary and / or secondary amine group, preferably chosen from phenalkamines, and • the reaction products (P) chosen from: - the reaction products (PI) of at least: one fatty acid, one polyamine (D1) and one compound (E) comprising at least one epoxide group, and / or - the reaction products (P2) of at least: one dimerized fatty acid and one polyamine (D2), the component (A) and / or the component (B) further comprising at least 20% by weight, relative to the total weight of said component, of a lamellar filler (C) chosen from micaceous iron oxide, vermiculite, mica and mixtures thereof, preferably iron oxide micaceous.
2. A two-component composition according to claim 1, wherein the aromatic epoxy resin is selected from diglycidyl ethers of bis-(4-hydroxy-3,5-difluorophenyl)methane, 1,1-bis-(4-hydroxyphenyl)ethane, 2,2-bis-(4-hydroxy-3-methylphenyl)propane, 2,2-bis-(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis-(4-hydroxyphenyl)propane, 4,4'-methylenediphenol, 2,4'-methylenediphenol, 2,2'-methylenediphenol and mixtures thereof.
3. A two-component composition according to claim 1 or 2, wherein component (A) further comprises a reactive diluent.
4. A two-component composition according to any one of claims 1 to 3, wherein the hardener (H) is a phenolic Mannich base of formula (I):
5. OH (I), r- in which: - R2 and R4 independently represent a hydrogen atom or a saturated or unsaturated hydrocarbon radical, preferably with a linear or branched open chain, comprising 1 to 20 carbon atoms, and - R1, R3 and R5 independently represent: • a hydrogen atom, or • a saturated or unsaturated hydrocarbon radical, preferably with a linear or branched open chain, comprising 1 to 20 carbon atoms and optionally one or more heteroatoms chosen from nitrogen and oxygen, or • a monovalent radical of formula (II): NHR7 (II), R-' in which: • R6 represents a hydrogen atom or a hydrocarbon radical comprising 1 to 15 carbon atoms, saturated or unsaturated, with a linear or branched open chain, or comprising one or more optionally aromatic cycles, and • R7 represents a hydrocarbon radical comprising at least two carbon atoms, saturated or unsaturated, with a linear or branched open chain, or comprising one or more optionally aromatic cycles, and optionally comprising one or more nitrogen atoms, at least one, preferably exactly one, of the substituents R1, R3 and R5 being of formula (II). Two-component composition according to claim 4, in which the hardener (H) is a phenolic Mannich base of formula (I), in which: - R2 represents a group of formula (Ilia), (Illb), (IIIc) or (Illd), the formulas below of which show the free valence: (Ilia): R4 represents a hydrogen atom, and the substituents R1, R3 and R5 not being of formula (II) are hydrogen atoms.
6. Two-component composition according to any one of claims 1 to 5, in which the reaction products (PI) are obtained by reaction of at least: - a fatty acid comprising between 10 and 22 carbon atoms, - a polyamine (Dl) comprising, in addition to the at least two primary amine groups (-NH2), one or more secondary amine groups and between 4 and 20 carbon atoms, and - a compound (E) chosen from p-tolyl glycidyl ether, p-phenyl glycidyl ether, 4-tert-butylphenyl glycidyl ether, the reaction products of the liquid of cashew nut shell and epichlorohydrin, C12-C14 alkyl glycidyl ethers, C13-C15 alkyl glycidyl ethers, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, polypropylene glycol diglycidyl ether, bisphenol A diglycidyl ether, bisphenol E diglycidyl ether, 2,2-bis-(4-hydroxy-3-methylphenyl)propane diglycidyl ether, bisphenol B diglycidyl ether, 4,4'-, 2,4'- and / or 2,2'-bisphenol F diglycidyl ether, and mixtures thereof.
7. Two-component composition according to any one of claims 1 to 6, in which the reaction products (P2) are obtained by reaction of at least: - a dimerized fatty acid comprising between 8 and 48 carbon atoms, - a polyamine (D2) comprising, in addition to the at least two primary amine groups (-NH2), one or more secondary amine groups and between 4 and 20 carbon atoms, and - optionally a fatty acid comprising between 4 and 28 carbon atoms.
8. Two-component composition according to any one of claims 1 to 7, in which at least 65% of the particles constituting the lamellar filler (C) are lamellar particles, preferably at least 75%, more preferably at least 80%.
9. A two-component composition according to any one of claims 1 to 8, wherein component (B) further comprises an accelerator.
10. Use of the two-component composition according to any one of claims 1 to 9, as a moisture barrier.
11. Moisture barrier obtained after curing the two-component composition according to any one of claims 1 to 9.
12. A method of sealing a surface comprising applying the two-component composition according to any one of claims 1 to 9 to said surface and then curing said composition to form a moisture barrier, in particular at room temperature.
13. A method of preparing a floor comprising: - applying the two-component composition according to any one of claims 1 to 9 to the surface of the floor, then - curing said composition to form a moisture barrier, and - preparing a surface suitable for the application of a self-cleaning health composition, then - applying a self-cleaning health composition.