Rubber composition comprising a highly saturated diene elastomer
A rubber composition combining a highly saturated diene elastomer with a functionalized liquid butadiene polymer addresses the challenge of balancing tire rigidity and rolling resistance, enhancing handling and reducing hysteresis for improved tire performance.
Patent Information
- Application Number
- FR2022013473
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-15
AI Technical Summary
Tire manufacturers face a challenge in balancing the need for increased tire rigidity for improved handling with reduced rolling resistance, as conventional methods to enhance rigidity often lead to increased hysteresis losses and rolling resistance.
A rubber composition comprising a highly saturated diene elastomer, a reinforcing filler, a vulcanization system, and a liquid butadiene polymer functionalized with an alkoxysilyl group, which enhances rigidity while reducing hysteresis.
The composition achieves improved rigidity and reduced hysteresis, leading to better rolling resistance and road behavior, particularly under heavy loads.
Abstract
Description
Title of the invention: Rubber composition comprising a highly saturated diene elastomer technical field
[0001] The field of the present invention is that of highly saturated diene elastomer-based rubber compositions intended for use in a tire, particularly in its tread. Previous technique
[0002] The use of highly saturated diene elastomers is known in the manufacture of tires. For example, the Applicant described ethylene and 1,3-butadiene copolymers and their application in a tire tread in document WO2014114607A1. This document indicates that the use of these copolymers in the tread results in good wear resistance and rolling resistance properties for the tire.
[0003] Tire manufacturers are constantly seeking solutions to improve tire performance. This research involves the continuous improvement of the properties of the rubber compounds used in tire manufacturing. The compounds that make up a tire generally represent compromises between performance properties that are difficult to reconcile simultaneously (namely, rigidity, which must be high, and rolling resistance, which must be low in order to minimize fuel consumption). Therefore, it is an ongoing objective for tire manufacturers to find formulas that improve the balance between all these performance properties.
[0004] In the field of tires comprising a highly saturated diene elastomer in the tread discussed above, there is a need, particularly in certain conditions of transporting heavy loads, to have rubber compositions which give the tire increased rigidity to improve road behavior, as well as improved hysteretic properties to minimize rolling resistance.
[0005] It is known that the stiffness of a tire rubber compound can be improved by increasing the reinforcing charge ratio or by incorporating certain reinforcing resins. However, experience shows that such stiffening negatively impacts rolling resistance properties, often to a prohibitive degree, and is accompanied by a significant increase in the hysteresis losses of the rubber compound. Improving stiffness performance while maintaining low rolling resistance is therefore a constant concern for tire designers. Description of the invention
[0006] Continuing its efforts, the Applicant has found a rubber composition that meets this need in the field of application of highly saturated diene elastomers to rubber compositions for tires, and in particular for the tread. Specifically, the Applicant has found, unexpectedly, a rubber composition that combines the use of a highly saturated diene elastomer with the use of a functionalized liquid butadiene polymer. This combination increases rigidity while significantly reducing the hysteresis of the composition, whereas a composition using a non-functional liquid polybutadiene degrades both of these properties. These improved properties promise to give the tire good rolling resistance and improved road handling, particularly when transporting heavy loads.
[0007] Thus, a first object of the invention is a rubber composition based on at least - an elastomeric matrix comprising predominantly a highly saturated diene elastomer, - a reinforcing load, - a vulcanization system and - a liquid butadiene polymer functionalized at the end of the chain by an alkoxysilyl function, optionally partially or totally hydrolyzed.
[0008] Another object of the invention is a pneumatic or non-pneumatic tire comprising a rubber composition according to the invention, preferably in its tread. Summary of the invention
[0009] The invention, described in more detail below, relates to at least one of the embodiments listed in the following points:
[0010] 1. Rubber composition based on at least - an elastomeric matrix comprising predominantly a highly saturated diene elastomer, which highly saturated diene elastomer is a copolymer of ethylene and a 1,3-diene in which the ethylene units represent at least 50% by mole of the monomer units of the copolymer, - a reinforcing load, - a vulcanization system and - a liquid butadiene polymer functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed, having a number-average molar mass (Mn) greater than or equal to 1000 g / mol.
[0011] 2. Rubber composition according to embodiment 1, wherein the ethylene units represent 50% to 95% by mole of the monomer units of the highly saturated diene copolymer.
[0012] 3. Rubber composition according to any one of the preceding embodiments, wherein the ethylene units represent at least 60% by mole of the monomer units of the highly saturated diene copolymer, preferably from 65% to 90% by mole of the monomer units of the highly saturated diene copolymer.
[0013] 4. Rubber composition according to any one of the preceding embodiments, in which the 1,3-diene is 1,3-butadiene, isoprene, myrcene or [3-famesene, or a mixture of myrcene and [3-farnesene, preferably 1,3-butadiene.
[0014] 5. Rubber composition according to any one of the preceding embodiments, in which the copolymer of ethylene and a 1,3-diene is a copolymer of ethylene and 1,3-butadiene.
[0015] 6. Rubber composition according to any one of the preceding embodiments, in which the copolymer is statistical.
[0016] 7. Rubber composition according to any one of the preceding embodiments, in which the proportion of the highly saturated diene elastomer varies in a range of 60 to 100 pc, preferably 80 to 100 pc and most preferably 90 to 100 pc.
[0017] 8. Composition according to any one of the preceding embodiments in which the Liquid butadiene polymer is a liquid polybutadiene functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed.
[0018] 9. Composition according to any one of the preceding embodiments in which the Alkoxysilyl functions are functions corresponding to the formula -Si(OR)nR'3 n, in which each R, independently of the others, designates a hydrogen atom or a Ci-C4 alkyl, each R', independently of the others, designates a Ci-Cio alkyl, preferably Ci-C4, and n is an integer from 1 to 3, preferably 3.
[0019] 10. Composition according to any one of the preceding embodiments in which Alkoxysilyl functions are functions corresponding to the formula Si(OR)3, in which each R, independently of the others, designates a hydrogen atom or an alkyl in the form of Ci-Cio, preferably in CrC4, preferably an alkyl in CrC4.
[0020] 11. Composition according to any one of the preceding embodiments in which Alkoxysilyl functions are trimethoxysilyl or triethoxysilyl functions, optionally partially or totally hydrolyzed.
[0021] 12. Composition according to any one of the preceding embodiments in which the Functionalized liquid butadiene polymer is functionalized at each end of the main chain by an alkoxysilyl function, optionally partially or totally hydrolyzed.
[0022] 13. Composition according to any one of the preceding embodiments in which the Functionalized liquid butadiene polymer is a liquid polybutadiene functionalized at each end of the main chain by an alkoxysilyl function, optionally partially or totally hydrolyzed.
[0023] 14. Composition according to any one of the preceding embodiments in which the the proportion of liquid butadiene polymer functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed, is in the range of 0.5 to 25 pc, preferably 5 to 15 pc.
[0024] 15. Composition according to any one of the preceding embodiments in which the Liquid butadiene polymer has a Tg within a range of -60°C to -100°C, more preferably from -80°C to -100°C.
[0025] 16. Composition according to any one of the preceding embodiments in which the liquid butadiene polymer has a number-average molar mass greater than or equal to 1000 g / mol and less than or equal to 50000 g / mol, preferably less than or equal to 10000 g / mol, even more preferably less than or equal to 5000 g / mol.
[0026] 17. Composition according to any one of the preceding embodiments in which the reinforcing filler includes at least one silica, one carbon black or a mixture of silica and carbon black.
[0027] 18. Composition according to any one of the preceding embodiments in which the reinforcing filler includes silica as the major reinforcing filler.
[0028] 19. Composition according to any one of the preceding embodiments in which the Reinforcing load rate is within a range of 5 to 150 pc.
[0029] 20. Composition according to any one of the preceding embodiments in which the silica content is within a range of 20 to 60 parts per cent.
[0030] 21. Pneumatic or non-pneumatic bandage comprising a composition according to any one of the previous achievements.
[0031] 22. Pneumatic or non-pneumatic bandage according to the preceding embodiment comprising a composition according to any one of the realizations 1 to 20 in all or part of its tread. Definitions
[0032] The expression "composition based on" means a composition comprising the mixture and / or the in situ reaction product of the various constituents used, some of these constituents being able to react and / or intended to react with each other, at least partially, during the different phases of manufacturing the composition; the composition may thus be in a totally or partially crosslinked state. or in the non-crosslinked state.
[0033] By the expression "part by weight per hundred parts by weight of elastomer" (or pce), it is necessary to understand in the context of the present invention, the part, by mass per hundred parts by mass of elastomer.
[0034] On the other hand, any interval of values designated by the expression "between a and b" represents the domain of values from greater than a to less than b (i.e., excluding the bounds a and b), while any interval of values designated by the expression "from a to b" means the domain of values from a to b (i.e., including the strict bounds a and b). In the present case, when an interval of values is designated by the expression "from a to b", the interval represented by the expression "between a and b" is also designated.
[0035] In this application, "all the monomer units of the elastomer" or "all the monomer units of the elastomer" means all the repeating units constituting the elastomer that result from the insertion of the monomers into the elastomer chain by polymerization. Unless otherwise specified, the contents of a monomer unit or repeating unit in the highly saturated diene elastomer are given as a molar percentage calculated on the basis of all the monomer units of the elastomer.
[0036] When referring to a "major" compound, for the purposes of this invention, it is understood that this compound is the majority among the compounds of the same type in the composition; that is, it is the one that represents the largest quantity by mass among the compounds of the same type. Thus, for example, a major elastomer is the elastomer representing the greatest mass relative to the total mass of the elastomers in the composition. Similarly, a so-called major filler is the one representing the greatest mass among the fillers in the composition. By way of example, in a system comprising a single elastomer, this elastomer is the major component for the purposes of this invention; and in a system comprising two elastomers, the major elastomer represents more than half of the mass of the elastomers. Conversely, a "minor" compound is a compound that does not represent the largest mass fraction among the compounds of the same type.Preferably, "major" means a mass proportion of more than 50%; when the compound represents 100% by mass, it is also described as "major".
[0037] The compounds mentioned in the description may be of fossil origin or bio-based. In the latter case, they may be partially or totally derived from biomass or obtained from renewable raw materials derived from biomass. Similarly, the compounds mentioned may also come from the recycling of materials already used, that is to say, they may be partially or totally derived from a recycling process, or obtained from materials These are themselves derived from a recycling process. This includes, in particular, polymers, fillers, etc. Detailed description of the invention 1- Elastomer matrix
[0038] By "elastomeric matrix", we mean all the elastomers in the composition.
[0039] According to the invention, the elastomeric matrix mainly comprises at least one highly saturated diene elastomer, namely a copolymer containing ethylene units and 1,3-diene units (hereinafter referred to as "the copolymer").
[0040] The highly saturated diene elastomer useful for the purposes of the invention is a copolymer, preferably a statistical copolymer. A "statistical copolymer" is understood to be a copolymer in which the sequential distribution of the monomer units obeys a known statistical law.
[0041] The highly saturated diene elastomer useful for the purposes of the invention is a copolymer comprising ethylene units resulting from the polymerization of ethylene. The term "ethylene unit" refers, as is known, to the motif -(CH2-CH2)- resulting from the insertion of ethylene into the elastomer chain. The highly saturated diene elastomer is rich in ethylene units, since ethylene units represent at least 50% by mole of all the monomer units of the elastomer. The maximum proportion of ethylene units is determined by the elastomeric nature of the polymer; this proportion is preferably at most 95% by mole, more preferably at most 90% by mole, and even more preferably at most 85% by mole. Thus, preferably, the highly saturated diene elastomer comprises from 50% to 95% by mole of ethylene units, the mole percentage being calculated on the basis of all the monomer units of the highly saturated diene elastomer.
[0042] Preferably, the highly saturated diene elastomer comprises at least 60% by mole of ethylene units.In other words, ethylene units preferably represent at least 65% by mole of all monomer units in the highly saturated diene elastomer, and more preferably at least 70% by mole of all monomer units in the highly saturated diene elastomer. More preferably, the highly saturated diene elastomer comprises 65% to 90% by mole of ethylene units, the mole percentage being calculated on the basis of all monomer units in the highly saturated diene elastomer.
[0043] The highly saturated diene elastomer according to the invention being a copolymer of ethylene and a 1,3-diene, it also comprises 1,3-diene units resulting from the polymerization of a 1,3-diene. As is known, the expression "1,3-diene unit" refers to the units resulting from the insertion of 1,3-diene.
[0044] The 1,3-diene units are those, for example, of a 1,3-diene having 4 to 24 atoms of carbon.
[0045] Suitable 1,3-diene includes butadiene, isoprene, 2,3-di(alkyl in C1 to C5)-1,3-butadiene such as, for example, 2,3-dimethyl-1,3-butadiene, 2,3-diethyl-1,3-butadiene, 2-methyl-3-ethyl-1,3-butadiene or 2-methyl-3-isopropyl-1,3-butadiene, aryl-1,3-butadiene such as phenyl-1,3-butadiene, 1,3-pentadiene. A suitable 1,3-diene is also a 1,3-diene of the formula CH2=CR-CH=CH2, in which R represents a hydrocarbon chain having 3 to 20 carbon atoms, such as for example a linear monoterpene (Ci0H16), like myrcene, a linear sesquiterpene (Ci5H24), like [3-farnesene etc....
[0046] The highly saturated diene elastomer is preferably a copolymer of ethylene and a 1,3-diene among 1,3-butadiene, isoprene, myrcene, [3-farnesene and a mixture of myrcene and [3-farnesene.
[0047] Preferably, the 1,3-diene is 1,3-butadiene or isoprene, more preferably 1,3-butadiene, in which case the highly saturated diene elastomer is a copolymer of ethylene and 1,3-butadiene, statistically preferred.
[0048] According to the invention, particularly when the first 1,3-diene is 1,3-butadiene or a mixture of 1,3-butadiene and at least one other 1,3-diene, the highly saturated diene elastomer may further contain 1,2-cyclohexanediyl units. The presence of these cyclic structures in the copolymer results from a very specific insertion of ethylene and 1,3-butadiene during polymerization. The content of 1,2-cyclohexanediyl units in the copolymer varies according to the respective contents of ethylene and 1,3-butadiene in the copolymer. The copolymer preferably contains less than 15 mol% of 1,2-cyclohexanediyl unit units.
[0049] The highly saturated diene elastomer useful for the purposes of the invention can be obtained by various synthetic methods known to those skilled in the art, particularly depending on the desired microstructure of the highly saturated diene elastomer. Generally, it can be prepared by copolymerization of at least one 1,3-diene, preferably 1,3-butadiene, and ethylene, according to known synthetic methods, particularly in the presence of a catalytic system comprising a metallocene complex. Examples include catalytic systems based on metallocene complexes, which are described in documents EP 1 092 731, WO 2004035639, WO 2007054223 and WO 2007054224, as well as WO2020070442, WO2020070443 and WO2020074804 on behalf of the Applicant.The highly saturated diene elastomer, including when statistical, can also be prepared by a process using a preformed catalytic system such as those described in documents WO 2017093654 Al, WO 2018020122 Al and WO 2018020123 AL. The highly saturated diene elastomer is statistical according to an embodiment of the invention.
[0050] The highly saturated diene elastomer useful for the needs of the invention may consist of a mixture of highly saturated diene elastomers which differ from each other by their microstructures or by their macrostructures.
[0051] According to the invention, the content of the highly saturated diene elastomer in the rubber composition is preferably at least 50 parts by weight per hundred parts of elastomer in the rubber composition (wt). Even more preferably, the content of the highly saturated diene elastomer in the rubber composition varies in the range of 60 to 100 wt, preferably 80 to 100 wt. More preferably, it varies in the range of 90 to 100 wt.
[0052] In addition, the elastomer matrix of the composition of the invention may include at least one other elastomer, in a minor quantity. In particular, we note diene elastomers known to those skilled in the art for their use in the field of tires, such as polybutadiene (abbreviated "BR"), synthetic polyisoprene (IR), natural rubber (NR), butadiene copolymers such as butadiene-styrene copolymer (SBR), isoprene copolymers and mixtures of these elastomers. 2- Liquid butadiene polymer
[0053] The composition of the invention comprises a liquid butadiene polymer functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed, having a number-average molar mass (Mn) greater than or equal to 1000 g / mol.
[0054] The term "liquid butadiene polymer" according to the invention means a more or less viscous butadiene polymer which is liquid at room temperature (approximately 23°C below atmospheric temperature), that is to say, as a reminder, having the capacity to eventually take the shape of its container.
[0055] The term "butadiene polymer" means a homopolymer or copolymer of butadiene, in other words, a diene polymer selected from the group consisting of polybutadienes, various butadiene copolymers, and mixtures of these polymers. Among butadiene copolymers, particular examples include copolymers of butadiene and a vinylaromatic monomer, preferably styrene.
[0056] Preferably, the liquid butadiene polymer is a liquid polybutadiene.
[0057] According to the invention, the liquid butadiene polymer is functionalized at the end of chain by an alkoxysilyl group, optionally partially or totally hydrolyzed. By "chain-end functionalized polymer" is meant a polymer having an alkoxysilyl functional group at at least one chain end, i.e., at one end of the main chain of the polymer or at each of the two ends of the main chain of the polymer. Preferably, the liquid butadiene polymer is functionalized with an alkoxysilyl group at each end of the main chain of the polymer, that is to say at the two ends of the chain.
[0058] By "alkoxysilyl function, optionally partially or totally hydrolyzed", is meant a function corresponding to the formula -Si(OR)nR'3 n, each R, independently of the others, represents a hydrogen atom or an alkyl radical in the form of Ci-Cio, preferably in C1-C4, or aryl in the form of C6-C10, each R', independently of the others, designates an alkyl in the form of Ci-Cio, preferably in C1-C4, or aryl in the form of C6-C10, and n is an integer from 1 to 3, preferably 3. Preferably, the alkoxysilyl function is a function corresponding to the formula -Si(OR)3, R being as defined above, preferably an alkyl in the form of Ci-Cio, preferably also in CrC4. Even more preferably the alkoxysilyl function is a trimethoxysilyl or triethoxysilyl function, optionally partially or totally hydrolyzed.
[0059] According to the invention, the alkoxysilyl function, optionally partially or totally hydrolyzed, is linked to the butadiene polymer by a covalent bond or by a group that may comprise one or more heteroatoms selected from N and O.
[0060] All preferential and advantageous aspects concerning the functionalized liquid butadiene polymer are combinable according to the invention. Thus, advantageously, the liquid butadiene polymer functionalized at the chain end by an alkoxysilyl group is a functionalized liquid polybutadiene bearing at each end of the main chain a trialcoxysilyl group, preferably trimethoxysilyl or triethoxysilyl, the alkoxysilyl groups optionally being partially or totally hydrolyzed.
[0061] According to the invention, the liquid butadiene polymer functionalized at the end of the chain has a number-average molar mass (Mn) greater than or equal to 1000 g / mol and preferably less than or equal to 50,000 g / mol, more preferably less than or equal to 10,000 g / mol, and even more preferably less than or equal to 5,000 g / mol. Thus, according to a preferred embodiment, the liquid butadiene polymer functionalized at the end of the chain has a number-average molar mass (Mn) ranging from 1000 g / mol to 5,000 g / mol.
[0062] Preferably, the end-functionalized liquid butadiene polymer according to the invention also has a Tg in the range of -60°C to -100°C, more preferably from -80°C to -100°C.
[0063] According to the invention, the various preferred characteristics above of the liquid butadiene polymer functionalized at the chain end are combinable with each other.
[0064] The liquid butadiene polymer functionalized at the chain end by an alkoxysilyl group can be obtained in a simple and known manner by functionalizing a liquid telechelic butadiene polymer bearing -OH groups at the chain ends, obtained by radical polymerization, with an alkoxysilane-type functionalizing agent capable of reacting with the -OH groups of the polymer. Examples of such functionalizing agents include alkoxysilane compounds bearing an isocyanate group. Polymers of this type useful for the purposes of the invention and their synthesis are described, for example, in document WO2016180649Al.
[0065] The Tg of the liquid polymer is measured by DSC according to ASTM D3418 (1999). The macrostructure (Mw, Mn and IP) of the liquid polymer is determined by size exclusion chromatography (SEC): tetrahydrofuran solvent; temperature 35°C; concentration 1 g / L; flow rate 1 mL / min; solution filtered through a 0.45 µm porosity filter before injection; Moore calibration with polystyrene standards; set of 3 "WATERS" columns in series ("STYRAGEL" HR4E, HR1 and HR0.5); detection by differential refractometer ("WATERS 2410") and its associated operating software ("WATERS EMPOWER").
[0066] Liquid polymers of butadiene useful for the needs of the invention can be found commercially under the name for example "POLYVEST EP ST-E 60" and "POLYVEST EP ST-E 100" marketed by the company EVONIK.
[0067] According to any one of the embodiments of the invention, the proportion of liquid butadiene polymer functionalized at each end of the chain by an al-coxysilyl function is advantageously greater than or equal to 0.5 pc, preferably within a range of 0.5 pc to 25 pc, preferably from 1 to 20 pc, preferably still from 5 pc to 15 pc.
[0068] The liquid butadiene polymer functionalized at each chain end by an alkoxysilyl function can be a mixture of several liquid butadiene polymers functionalized at each chain end by an alkoxysilyl function as described above.
[0069] According to one embodiment of the invention, the liquid butadiene polymer functionalized at its chain end with alkoxysilyl groups, optionally partially or totally hydrolyzed, is the sole plasticizer in the rubber composition. In other words, the rubber composition does not comprise any plasticizer other than the liquid butadiene polymer functionalized at its chain end with alkoxysilyl groups, optionally partially or totally hydrolyzed. 3- Reinforcing load
[0070] The composition according to the invention comprises a reinforcing filler. Any type of reinforcing filler known for its ability to reinforce a rubber composition suitable for tire manufacturing can be used, for example, an organic filler such as carbon black, an inorganic reinforcing filler such as silica, alumina, or a mixture of these two types of filler. More specifically, the reinforcing filler comprises at least one silica, one carbon black, or a mixture of silica and carbon black.
[0071] All carbon blacks are suitable as carbon blacks, particularly those of pneumatic grade. Among the latter, reinforcing carbon blacks of the 100, 200, or 300 series (ASTM grades) are particularly suitable, such as NI 15, N134, N234, N326, N330, N339, N347, N375, or, depending on the intended application, blacks of higher series (e.g., N660, N683, N772). Carbon blacks could, for example, already be incorporated into an isoprene elastomer in the form of a masterbatch (see, for example, applications WO 97 / 36724 or WO 99 / 16600).
[0072] Examples of organic fillers other than carbon blacks include functionalized polyvinyl organic fillers as described in applications WO-A-2006 / 069792, WO-A-2006 / 069793, WO-A-2008 / 003434 and WO-A-2008 / 003435.
[0073] The composition may contain one type of silica or a blend of several silicas. The silica used may be any reinforcing silica known to those skilled in the art, in particular any precipitated or pyrogenated silica having a BET surface area and a CTAB specific surface area both less than 450 m2 / g, preferably from 30 to 400 m2 / g. Examples of highly dispersible precipitated silicas (HDS) include "Ultrasil 7000" and "Ultrasil 7005" silicas from Degussa, "Zeosil" 1165MP, 1135MP and 1115MP silicas from Solvay, "Hi-Sil EZ150G" silica from PPG, "Zeopol" 8715, 8745 and 8755 silicas from Huber, treated precipitated silicas such as, for example, aluminium-doped silicas described in application EP-A-0735088 or high specific surface area silicas as described in application WO 03 / 16837.
[0074] According to one embodiment of the invention, the reinforcing filler is predominantly an inorganic reinforcing filler (preferably silica), that is to say, it comprises more than 50% (>50%) by weight of an inorganic reinforcing filler such as silica relative to the total weight of the reinforcing filler. Optionally, according to this embodiment, the reinforcing filler also comprises carbon black. According to this option, the carbon black is used at a rate less than or equal to 20%, more preferably less than or equal to 10% (for example, the carbon black content may be in the range of 0.5 to 20%, in particular from 1 to 10%). Within the indicated ranges, the coloring (black pigmenting agent) and anti-UV properties of carbon black are benefited, without otherwise compromising the typical performance provided by the inorganic reinforcing filler.
[0075] In the present exposition, the specific surface area BET is determined by adsorption of gas using the Brunauer-Emmett-Teller method described in "The Journal of the American Chemical Society" (Vol. 60, page 309, February 1938), and more specifically according to a method adapted from the standard NF ISO 5794-1, Annex E of June 2010 [multipoint volumetric method (5 points) - gas: nitrogen - degassing under vacuum: one hour at 160°C - relative pressure range w / in: 0.05 to 0.2].
[0076] For inorganic fillers such as silica for example, the specific surface area values CT AB were determined according to standard NF ISO 5794-1, Annex G of June 2010. The process is based on the adsorption of CTAB (N-hexadecyl-N,N,N-trimethylammonium bromide) on the "external" surface of the reinforcing filler.
[0077] A person skilled in the art will understand that, as an equivalent filler to silica, a reinforcing filler of another nature, in particular organic, could be used, provided that this reinforcing filler is covered with a layer of silica, or has functional sites on its surface, in particular hydroxyl sites, requiring the use of a coupling agent to establish the bond between the filler and the elastomer.
[0078] The physical state in which the reinforcing charge is presented is indifferent, whether in the form of powder, microbeads, granules, balls or any other suitable densified form.
[0079] For the purposes of the invention, the total reinforcing filler content (carbon black and / or inorganic reinforcing filler such as silica) is from 5 to 150 parts per annum, more preferably from 20 to 65 parts per annum. Below 5 parts per annum, the composition may not be sufficiently reinforced, while above 150 parts per annum, the composition may have reduced rolling resistance.
[0080] Preferably, silica is used as the major filler. Silica preferably represents more than 50% by mass of the reinforcing filler. In other words, the proportion of silica in the reinforcing filler is greater than 50% by weight of the total weight of the reinforcing filler. More preferably, silica represents more than 85% by mass of the reinforcing filler. According to some preferred embodiments, the silica content varies from 20% to 60%.
[0081] Carbon black, when present, is then used in a minority, preferably at a rate in the range of 0.1 to 10 pc, more preferably from 0.5 to 10 pc, in particular from 1 to 5 pc.
[0082] To couple the reinforcing inorganic filler to the diene elastomer, a coupling agent (or bonding agent) that is at least bifunctional can be used in a well-known manner to ensure sufficient chemical and / or physical connection between the inorganic filler (surface of its particles) and the diene elastomer. Organosilanes or polyorganosiloxanes are particularly commonly used. less bifunctional. By "bifunctional," we mean a compound possessing a first functional group capable of interacting with the inorganic filler and a second functional group capable of interacting with the diene elastomer. For example, such a bifunctional compound may comprise a first functional group consisting of a silicon atom, said first functional group being capable of interacting with the hydroxyl groups of an inorganic filler, and a second functional group consisting of a sulfur atom, said second functional group being capable of interacting with the diene elastomer.
[0083] Preferably, the organosilanes are chosen from the group consisting of polysulfide organosilanes (symmetric or asymmetric) such as bis(3-triethoxysilylpropyl) tetrasulfide, abbreviated TESPT and marketed under the name "Si69" by Evonik, or bis-(3-triethoxysilylpropyl) disulfide, abbreviated TESPD and marketed under the name "Si75" by Evonik, polyorganosiloxanes, mercaptosilanes, and blocked mercaptosilanes, such as "NXT-Silane" or "NXT-Z45 Silane" marketed by Momentive. Of course, mixtures of these coupling agents could also be used.
[0084] Those skilled in the art will understand that the coupling agent content depends on the amount of reinforcing inorganic filler to be coupled to the elastomer. Typically, the coupling agent content represents 0.5% to 15% by weight relative to the amount of reinforcing inorganic filler, particularly silica.
[0085] The composition according to the invention may optionally also contain coupling activators, inorganic filler recovery agents or more generally processing aids capable, in a known manner, through an improvement in the dispersion of the filler in the rubber matrix and a reduction in the viscosity of the composition, of improving its processing ability in the raw state, these agents being known elsewhere. 4- Crosslinking system
[0086] The crosslinking system can be any type of system known to those skilled in the art in the field of tire rubber compositions. In particular, it can be sulfur-based, and / or peroxide-based, and / or bismaleimide-based.
[0087] Preferably, the crosslinking system is sulfur-based; this is referred to as a vulcanization system. The sulfur can be supplied in any form, including molecular sulfur or a sulfur-donating agent. At least one vulcanization accelerator is also preferably present, and optionally, various known vulcanization activators such as zinc oxide, stearic acid, or equivalent compounds such as stearic acid salts and transition metal salts, guanidine derivatives (in particular diphenylguanidine), or known vulcanization retardants may be used.
[0088] Sulfur is used at a preferential rate of between 0.2 and 10 parts per annum, more preferably between 0.3 and 5 parts per annum. The vulcanization accelerator or accelerator mixture is used at a preferential rate of between 0.5 and 10 parts per annum, more preferably between 0.5 and 5 parts per annum.
[0089] Any compound capable of acting as a vulcanization accelerator for diene elastomers in the presence of sulfur can be used as an accelerator, in particular accelerators of the thiazole type and their derivatives, accelerators of the sulfenamide, thiuram, dithiocarbamate, dithiophosphate, thiourea and xanthate types. Examples of such accelerators include the following compounds: 2-mercaptobenzothiazyl disulfide (abbreviated "MBTS"), N-cyclohexyl-2-benzothiazyl sulfenamide ("CBS"), N,N-dicyclohexyl-2-benzothiazyl sulfenamide ("DCBS"), N-ter-butyl-2-benzothiazyl sulfenamide ("TBBS"), N-ter-butyl-2-benzothiazyl sulfenimide ("TBSI"), tetrabenzylthiuram disulfide ("TBZTD"), zinc dibenzyldithiocarbamate ("ZBEC") and mixtures of these compounds. 5- Additives
[0090] The rubber composition according to the invention may optionally also include all or part of the usual additives commonly used in tire elastomer compositions, pigments, protective agents such as anti-ozone waxes, chemical anti-ozonants, antioxidants, plasticizers, anti-fatigue agents, reinforcing resins (as described for example in application WO 02 / 10269).
[0091] It goes without saying that the invention relates to the rubber compositions described above both in the so-called "raw" or non-crosslinked state (i.e., before cooking) and in the so-called "cooked" or crosslinked state, or even vulcanized (i.e., after crosslinking or vulcanization). 6- Preparation of the rubber compound
[0092] The composition according to the invention can be manufactured in suitable mixers, using two successive preparation phases well known to those skilled in the art: - a first thermomechanical working or mixing phase (the so-called "non-productive" phase), which can be carried out in a single thermomechanical step during which all the necessary constituents, including the elastomer matrix, the liquid polybutadiene polymer, the reinforcing filler, and any other miscellaneous additives, with the exception of the crosslinking system, are introduced into a suitable mixer such as a standard internal mixer (for example, a 'Banbury' type). The incorporation of any filler into the elastomer can be carried out in one or more stages by thermomechanical mixing. In the case where the filler is already in incorporated in whole or in part into the elastomer in the form of a master mix as described for example in applications WO 97 / 36724 or WO 99 / 16600, it is the master mix which is directly mixed and where appropriate other elastomers or fillers present in the composition which are not in the form of a master mix are incorporated, as well as any other miscellaneous additives other than the crosslinking system.
[0093] - a second phase of mechanical work (the so-called "productive" phase), which is carried out in an external mixer such as a roller mixer, after cooling the mixture obtained during the first non-productive phase to a lower temperature, typically below 120°C.
[0094] Such phases are well known to those skilled in the art.
[0095] The final composition thus obtained is then calendered, for example, into a sheet or plate, particularly for laboratory characterization, or extruded (or co-extruded with another rubber composition) into a semi-finished (or profile) rubber product usable in a tire, for example as a tread. These products can then be used for tire manufacturing, according to techniques known to those skilled in the art.
[0096] The composition can be either in the raw state (before crosslinking or vulcanization), or in the cooked state (after crosslinking or vulcanization), can be a semi-finished product that can be used in a tire.
[0097] Crosslinking (or curing), where applicable vulcanization, is carried out in a known manner at a temperature generally between 130°C and 200°C, for a sufficient time which can vary for example between 5 and 90 min depending in particular on the curing temperature, the crosslinking system adopted and the crosslinking kinetics of the composition considered. 7 Pneumatics
[0098] The present invention also relates to a pneumatic or non-pneumatic bandage comprising a rubber composition according to the invention.
[0099] The aforementioned features of the present invention, as well as others, will be better understood upon reading the following description of several examples of embodiments of the invention, given by way of illustration and not limitation. EXAMPLES OF THE INVENTION'S IMPLEMENTATION 1- Tests and measurements:
[0100] 1-L Determination of the microstructure of elastomers:
[0101] The microstructure of the elastomers is determined by ¹H NMR analysis, supplemented by ¹³C NMR analysis when the resolution of the ¹H NMR spectra does not allow for the identification and quantification of all species. The measurements are carried out at using a BRUKER 500MHz NMR spectrometer at frequencies of 500.43 MHz for proton observation and 125.83 MHz for carbon observation.
[0102] For insoluble elastomers that swell in a solvent, a 4mm z-grad HRMAS probe is used to observe the proton and carbon in proton-decoupled mode. Spectra are acquired at rotation speeds of 4000 Hz to 5000 Hz.
[0103] For measurements on soluble elastomers, a liquid NMR probe is used allowing observation of the proton and carbon in proton-decoupled mode.
[0104] The preparation of insoluble samples is carried out in rotors filled with the material being analyzed and a deuterated solvent that allows swelling, generally deuterated chloroform (CDC13). The solvent used must always be deuterated, and its chemical nature can be adapted by those skilled in the art. The quantities of material used are adjusted to obtain spectra with sufficient sensitivity and resolution.
[0105] The soluble samples are dissolved in a deuterated solvent (approximately 25 mg of elastomer in µL), generally deuterated chloroform (CDC13). The solvent or solvent cutting agent used must always be deuterated, and its chemical nature can be adapted by those skilled in the art.
[0106] In both cases (soluble sample or swollen sample):
[0107] For proton NMR, a single 30° pulse sequence is used. The spectral window is adjusted to observe all the resonance lines belonging to the analyzed molecules. The accumulation number is adjusted to obtain a signal-to-noise ratio sufficient for quantifying each motif. The recycling time between each pulse is adapted to obtain a quantitative measurement.
[0108] For carbon NMR, a simple 30° pulse sequence is used with proton decoupling only during acquisition to avoid Nuclear Overhauser (NOE) effects and maintain quantitative accuracy. The spectral window is adjusted to observe all resonance lines belonging to the analyzed molecules. The accumulation number is set to obtain a signal-to-noise ratio sufficient for quantifying each motif. The recycling time between each pulse is adjusted to obtain a quantitative measurement.
[0109] NMR measurements are carried out at 25°C. 1-2. Determination of the Tg of elastomers
[0110] Glass transition temperature (Tg) values are measured in a known manner by DSC (Differential Scanning Calorimetry) according to ASTM D3418 (1999). 1-3. Measurement of dynamic properties:
[0111] The dynamic properties G*(25%) and tanômax(25%) at 60°C are measured on a viscoelastic analyzer (Metravib VA4000), according to ASTM D 5992-96. The response of a cross-linked composite sample (cylindrical specimen 4 mm thick and 400 mm² cross-section) is recorded under sinusoidal alternating simple shear loading at a frequency of 10 Hz, under defined temperature conditions, for example, 60°C, according to ASTM D 1349-99. A strain amplitude sweep is performed from 0.1 to 100% (forward cycle), then from 100% to 0.1% (reverse cycle). The results used are the complex dynamic shear modulus G* and the loss factor tan(ô). For the return cycle, we indicate the value of tan(ô)max at 25% strain observed at 60°C, noted tanômax (25%), as well as the complex dynamic shear modulus G* at 25% strain, at 60°C.
[0112] The tanômax (25%) measurement is a descriptor of hysteresis and therefore an indication of the rolling resistance property of the tire. The value, based on 100, is calculated using the following formula: (tanômax (25%) value at 60°C of the control / tanômax (25%) value at 60°C of the sample) * 100. In this way, a value lower than the control represents a decrease in hysteresis performance (i.e., an increase in hysteresis), while a higher value represents better hysteresis performance (i.e., lower hysteresis).
[0113] The G* (25%) measurement is a stiffness descriptor and therefore an indication of the tire's wear resistance. The value, expressed as a base of 100, is calculated as follows: (G* (25%) value at 60°C of the sample / G* (25%) value at 60°C of the control) * 100. Thus, a value lower than the control represents a decrease in stiffness, while a higher value represents greater stiffness. 2- Preparation of rubber compositions:
[0114] The rubber compositions, the detailed formulation of which is shown in Table 1, were prepared in the following manner:
[0115] The elastomer is introduced into an internal mixer (final filling level: approximately 70% by volume), the initial tank temperature of which is approximately 90°C. When the temperature reaches 100°C, the liquid butadiene polymer, silica, carbon black, and coupling agent are introduced, along with the various other ingredients except for sulfur and vulcanization accelerators. A thermomechanical process (non-productive phase) is then carried out in one step, lasting approximately 3 to 4 minutes in total, until a maximum "drop" temperature of 160°C is reached. The resulting mixture is recovered, cooled, and then the sulfur and vulcanization accelerators are incorporated using a roller tool at 25°C, mixing the entire mixture (productive phase) for an appropriate time (e.g., 5 minutes).
[0116] The compositions thus obtained are then calendered either in the form of plates (thickness 2 to 3 mm) or thin sheets of rubber for measuring their physical or mechanical properties. Crosslinking was then carried out at a temperature of 150°C, under pressure. Preparation of the elastomer
[0117] El elastomer is a highly saturated diene elastomer, a copolymer of ethylene and 1,3-butadiene prepared according to the following procedure: In a 70 L reactor containing methylcyclohexane (64 L), ethylene (5600 g), and 1,3-butadiene (2948 g), butylmagnesium ethylcyclohexane (BOMAG) solution is added to the methylcyclohexane and the catalytic system. The Mg / Nd ratio is 6.2. The volume of the catalytic system solution introduced is 840 mL, with an Nd concentration of 0.0065 M. The reaction temperature is regulated at 80°C, and the polymerization reaction is initiated. The polymerization reaction proceeds at a constant pressure of 8.3 bar. The reactor is fed with ethylene and 1,3-butadiene in a molar ratio of 73 / 27 throughout the polymerization process. The polymerization reaction is stopped by cooling, degassing the reactor, and adding ethanol. An antioxidant is added to the polymer solution. The copolymer is recovered after steam stripping and drying to a constant mass.The polymerization time is 225 minutes. The weighed mass (6.206 kg) allows the average catalytic activity of the catalytic system to be determined, expressed in kilograms of polymer synthesized per mole of neodymium metal per hour (kg / mol.h). The copolymer has a ML value of 62. The catalytic system is a preformed catalytic system. It is prepared in methylcyclohexane from a metallocene, [Me₂Si(Flu)₂Nd(q-BH₄)₂Li(THF)] at 0.0065 mol / L, a cocatalyst, butylmagnesium (BOMAG) with a BOMAG / Nd molar ratio of 2.2, and a preforming monomer, 1,3-butadiene with a 1,3-butadiene / Nd molar ratio of 90. The medium is heated to 80°C for 5 hours. It is prepared according to a method conforming to paragraph II.1 of patent application WO 2017093654 AL
[0118] [Tables 1] Tl Cl C2 Elastomer El (1) 100 100 100 Silica (2) 38 38 38 Carbon Black (3) 2 2 2 Coupling Agent (4) 3.1 3.1 3.1 LBR-307 (5) 10 POLYVEST ST E 100 (6) 10 DPG (7) 1.2 1.2 1.2 Ozone Wax (8) 1 1 1 Antioxidant 6PPD (9) 2 2 2 Stearic Acid (10) 2 2 2 ZNO(ll) 2.5 2.5 2.5 Sulfur 1.3 1.3 1.3 CBS (12) 1 1 1 G*25% at 60°C (Base 100) 100 83 123 Tanômax 25% at 60°C (Base 100) 100 79 115 1. Ethylene-1,3-butadiene copolymer containing 74 mol% ethylene units, 19 mol% butadiene units in the form of 1,2 and 1,4 units, and 7 mol% 1,2-cyclohexanediyl units, with a Tg of -44°C 2. “Zeosil 1165 MP” from Solvay-Rhodia in the form of microbeads 3. Carbon black, grade N234 according to ASTM Dl 765, from Cabot Corporation 4. Silane Mercapto-Thiocarboxylate Oligomer (“NXT-Z45”) - CAS 922519-17-3 - Momentive Company 5. LBR-307, Kuraray company (non-functional liquid polybutadiene, Tg - 95°C and Mn 8000 g / mol) 6. POLYVEST ST E 100 from Evonik (functional liquid triethoxysilyl polybutadiene at each end of the chain, Tg -80°C and Mn 3300 g / mol) 7. Diphenylguanidine “Perkacit DPG” from Flexsys 8. Anti-ozone wax “VARAZON 4959” from the company Sasol Wax 9. N-(l,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine "Santaflex 6PPD" from the company Flexys 10. Stearic acid “Pristerene 4931” from the company Uniqema 11. Industrial grade zinc oxide from Umicore 12. N-cyclohexyl-2-benzothiaz.ol-sulfenamide “Santicure CBS” from Flexsys 3- Results:
[0119] Composition T1 is the control without liquid butadiene polymer to evaluate the effect of the nature of the liquid butadiene polymer used in compositions Cl and C2. Composition C2 is in accordance with the invention.
[0120] The results show that the composition according to the invention, with an elastomeric matrix based on an EBR and a liquid polybutadiene functionalized at each chain end by an alkoxysilyl group, significantly improves both hysteresis performance (reduction of hysteresis) and stiffness compared to a composition not comprising liquid polybutadiene. This effect is unexpected since the combined use of an EBR and a non-functionalized liquid polybutadiene degrades these two properties. The combined improvement in hysteresis performance and stiffness suggests that a tire comprising such a composition will have reduced rolling resistance and improved handling.
Claims
Claims
1. Rubber composition comprising at least - an elastomer matrix comprising predominantly a highly saturated diene elastomer, which highly saturated diene elastomer is a copolymer of ethylene and a 1,3-diene in which the ethylene units represent at least 50 mol% of the monomer units of the copolymer, - a reinforcing filler, - a vulcanization system and - a liquid butadiene polymer functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed, having a number-average molar mass (Mn) greater than or equal to 1,000 g / mol.
2. A rubber composition according to claim 1, wherein the ethylene units represent at least 50% and at most 95% by mole of the monomer units of the copolymer, preferably from 65% to 90%.
3. A rubber composition according to any preceding claim, wherein the copolymer of ethylene and a 1,3-diene is a copolymer of ethylene and 1,3-butadiene.
4. Rubber composition according to any one of the preceding claims, in which the level of the highly saturated diene elastomer varies in a range from 60 to 100 phr, preferably from 80 to 100 phr, very preferably from 90 to 100 phr.
5. Rubber composition according to any one of the preceding claims in which the functionalized liquid butadiene polymer is a liquid polybutadiene functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed.
6. Rubber composition according to any one of the preceding claims in which the functionalized liquid butadiene polymer is functionalized at each end of the main chain by an alkoxysilyl function, optionally partially or totally hydrolyzed.
7. Rubber composition according to any one of the preceding claims in which the alkoxysilyl function, optionally partially or totally hydrolyzed, corresponds to the formula Si(OR)3, in which each R, independently of the others, denotes an atom hydrogen or a CrCio, preferably Ci-C4 alkyl.
8. Rubber composition according to any one of the preceding claims in which the alkoxysilyl function is a tri-alkyloxysilyl function, preferably trimethoxysilyl or triethoxysilyl, optionally partially or totally hydrolyzed.
9. Rubber composition according to any one of the preceding claims in which the functionalized liquid butadiene polymer is a liquid polybutadiene functionalized at each end of the main chain by a trialkoxysilyl function, preferably trimethoxysilyl or triethoxysilyl, optionally partially or totally hydrolyzed.
10. Rubber composition according to any one of the preceding claims in which the level of liquid butadiene polymer functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed, is within a range from 0.5 to 25 phr, preferably from 1 to 20 phr, more preferably from 5 to 15 phr.
11. Rubber composition according to any one of the preceding claims in which the liquid butadiene polymer functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed, has a Tg comprised in a range from -60°C to -100°C.
12. Rubber composition according to any one of the preceding claims in which the liquid butadiene polymer functionalized at the chain end by an alkoxysilyl function, optionally partially or totally hydrolyzed, has a number-average molar mass in a range from 1000 g / mol to 5000 g / mol.
13. A rubber composition according to any preceding claim wherein the reinforcing filler comprises silica as the major reinforcing filler.
14. A rubber composition according to any one of the preceding claims in which the silica content is within a range of 20 to 60 phr.
15. A pneumatic or non-pneumatic tire comprising a rubber composition according to any one of the preceding claims.