Rail soles made from a 100% recycled masterbatch

The metactivation process effectively devulcanizes rubber from rail soles, producing a recycled material with comparable performance to virgin rubber, addressing the limitations of current recycling methods by maintaining mechanical integrity and reducing environmental impact.

FR3147132A1Pending Publication Date: 2024-10-04VAPE RAIL INT
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
FR2023002904
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Current recycling methods for vulcanized rubber parts, such as rail soles, result in materials with reduced physical and mechanical properties, making them unsuitable for high-performance applications due to complex and aggressive chemical treatments that break the three-dimensional network, and the processes are costly and environmentally harmful.

Method used

A devulcanization process using metactivation, which involves controlled shearing and compression at low temperatures to break sulfur bridges without depolymerizing the rubber, combined with plasticizers to produce a devulcanized polymeric material that can be reused in rail soles, maintaining mechanical and elastic properties similar to virgin rubber.

Benefits of technology

The process allows for the production of recycled rubber parts with properties comparable or superior to virgin rubber, using up to 80% recycled material, while being environmentally friendly and cost-effective, without generating chemical pollution or waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000019_0000
    Figure 00000019_0000
Patent Text Reader

Abstract

The present invention relates to a devulcanized polymeric material, railway industry parts, in particular rail pads, comprising this polymeric material and their preparation processes.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Rail soles made from a 100% recycled masterbatch Technical field

[0001] The present invention relates to a devulcanized polymeric material, parts for the railway industry, in particular rail soles, comprising this polymeric material as well as methods for their preparation. Prior art

[0002] The invention relates to the recycling of used vulcanized rubber parts from the railway industry, in particular rail soles, in order to allow the reuse of the vulcanized rubber contained in these original parts, without appreciable loss of performance of the resulting rubber compound. More particularly, the invention relates to a devulcanized polymeric material, the physicochemical properties of which make it possible to be revulcanized and thus to constitute the raw material for parts of the railway industry, in particular rail soles, in which it is incorporated.

[0003] Nowadays, tires and industrial rubber are the two main sectors that consume and process rubber raw materials. An industrial rubber part is usually single-use. If defective or worn, it becomes waste.

[0004] Current issues regarding the depletion of fossil resources and the growing concern for environmental preservation are contributing to the search for solutions for recycling waste from the rubber industry.

[0005] Natural or synthetic rubber is the raw material for rail pads used by the railway industry. These are placed directly under the pad to ensure better load distribution while increasing the elasticity of the ballasted tracks, which improves the wear behavior of the superstructure components and passenger comfort. The lifespan of a pad is on average 15 years.

[0006] After this time, the used rail soles are thrown into nature or collected to be crushed and incinerated without further recovery.

[0007] The rubber contained in these soles is a mixture of natural rubber (NR) and vulcanized styrene-butadiene rubber (SBR), i.e. it results in a three-dimensional network of different polymer chains crosslinked together by sulfur-based bonds forming a thermoset, dimensionally stable composite. After its shaping and hardening, the latter cannot be reshaped. To date, Recycling and reusing vulcanized rubber parts remains complex because vulcanized rubber cannot be reshaped or simply reconstituted by dissolving it in a solvent to give the vulcanized rubber a new shape.

[0008] Existing material recovery processes are based on grinding and granulation techniques, which are predominant on an industrial scale. However, the ground rubber particles obtained by this method are inert and have a use limited to relatively small quantities, similar to that of fillers, because the processes used generally negatively affect the properties essential to the performance of rubber parts.

[0009] Alternative recovery processes are based on devulcanization of used vulcanized rubber to then be revulcanized alone or in a mixture with virgin rubber and reused in rubber parts.

[0010] These processes are complex and are based on very aggressive chemical and thermal treatments during which the three-dimensional network of the vulcanized rubber is dismantled and do not, to date, allow vulcanized rubber to be returned to its uncured state, such as “virgin rubber”. Indeed, the product obtained at the end of such treatment, called “reclaimed rubber”, exhibits less efficient physical and mechanical properties than the original vulcanized rubber. The material obtained can therefore only be incorporated to a limited extent in products which must demonstrate high physical performance.

[0011] Generally, the costs of reclaiming vulcanized rubber by conventional recycling methods developed on an industrial scale exceed the cost of the virgin material, and the incorporation of recycled rubber in a blend with fresh rubber generally results in a product with considerably reduced physical properties.

[0012] Thus, there remains a need to develop a devulcanization process making it possible to recover a rubber material with physical properties allowing it to be modulated subsequently and reused to produce rubber parts for the railway industry, in particular rail soles.

[0013] The polymeric material developed by the Applicant and its preparation process meet these needs.

[0014] The process for recycling rubber from used rubber parts from the railway industry allows for the use of a higher percentage, in the order of 30 to 80%, of recycled rubber in the rubber recycling process compared to prior art recycling methods, while providing a recycled rubber part with comparable or superior performance.

[0015] In addition, the process is considered a green process since it is environmentally friendly, i.e. it does not generate chemical pollution or waste. secondary, no toxic dust, no fumes, no waste water... unlike the conventional waste incineration process, it also does not generate carbon dioxide.

[0016] The polymeric material obtained is a “regenerated” material, completely devulcanized and not degraded.

[0017] This regeneration is carried out using a new process called "metactivation" which makes it possible to produce a devulcanized polymeric material having physical properties allowing its use as a raw material in quantities greater than those of the prior art for producing parts for the railway industry, in particular rail soles, which are not used at all to date. Statement of the invention

[0018] The Applicant has developed a process which makes it possible to produce a devulcanized or “regenerated” polymeric material from vulcanized rubber from used parts from the railway industry, in particular rail soles. The complete regeneration of the rubber from these used parts thus allows them to be recycled and to recover a “virgin” rubber gum. They can thus be reused as a raw material to manufacture new rubber-based parts from the railway industry, in particular rail soles.

[0019] The polymeric material is obtained by a process carried out under environmentally friendly, inexpensive conditions and which does not require the addition of chemical elements such as devulcanizing agents conventionally used in the processes of the prior art.

[0020] More specifically, the polymeric material developed by the Applicant is obtained by mixing a powder, obtained from used rubber parts from the railway industry, with one or more plasticizer(s) at a temperature ranging from 80 to 130°C, said powder being obtained by steps of compression and shearing of an granulate obtained from said used rubber parts from the railway industry.

[0021] In the present invention, the term "vulcanized rubber" designates said rubber having undergone a chemical process during which it has been formulated with additives including a vulcanizing agent (for example sulfur) allowing vulcanization and has undergone a heat treatment so as to create bridges between the polymers of said rubber to form a three-dimensional network.

[0022] By "devulcanized rubber" is meant a rubber in which the sulfur-based crosslinking bridges between the polymer chains have been broken.

[0023] In the present invention, the term "regenerated" means that the polymeric material can be reused like the original material.

[0024] In the present invention, the term "metactivation" designates a process for transforming a rubber granulate into powder by compression steps and controlled low temperature projection as described in documents FR 2946896 A1 and WO2011 / 004079 A2.

[0025] In the present invention, the term “metactivated powder” designates a powder which has undergone metactivation as described in documents FR 2946896 A1 and WO2011 / 004079 A2

[0026] In the present invention, the term "raw mix" means the mix before curing or vulcanization.

[0027] In the present invention, the term "masterbatch" denotes a mixture with defined mechanical properties.

[0028] Within the scope of the invention, the terms “rail pads” and “under-rail pads” may be used interchangeably.

[0029] Granulate from used rubber parts from the railway industry

[0030] The rubber granulate constitutes the raw material for the manufacture of rubber powder, by metactivation, necessary for obtaining the polymeric material according to the invention.

[0031] In the context of the invention, the aggregate has a particle size ranging from 1 to 4 mm, preferably from 2 to 4 mm and preferentially 3 mm, measured by ASTM D5644.

[0032] This aggregate is typically obtained by grinding.

[0033] Preferably, the grinding is carried out dry.

[0034] In certain embodiments, it may also be implemented wet or semi-wet.

[0035] Generally, the rubber granulate can be obtained by conventional grinding methods known from the prior art.

[0036] Typically, it is obtained by simple grinding of used vulcanized rubber parts from the railway industry. The grinding is carried out using conventional grinding machines well known to those skilled in the art, such as knife or hammer grinding machines or grinders and granulators sold by the company MTB Recycling®, for example.

[0037] Powder from used rubber parts from the railway industry

[0038] The powder is obtained by metactivation of the granulate from a rubber part.

[0039] This powder is “metactivated”, that is to say it is obtained by a “metactivation” process as described in documents FR 2946896 A1 and WO2011 / 004079 A2.

[0040] This “metactivation” process is a purely mechanical and physical process comprising shearing and compression steps.

[0041] In other words, the metactivation process is a temperature-controlled micro-cracking process.

[0042] In embodiments, the shearing and compression steps may be performed successively or simultaneously.

[0043] In embodiments, these steps are performed successively.

[0044] In embodiments, these steps are performed simultaneously.

[0045] The process is typically implemented in a reactor comprising one or more compartments installed in a chain one after the other. The compartments are separated by locks.

[0046] Examples of reactors include, but are not limited to, mixers, blenders, mills, ball mills, crackers, pulverizers, micronizers, single-screw or twin-screw extruders, disc mills, high-shear mills, high-energy mills, planetary mills.

[0047] Shearing is typically implemented by discs or screws.

[0048] The shear rate varies from 100 to 20,000 sec1.

[0049] The shear rate varies within the compartment from slow shear to fast shear. very rapid projection.

[0050] A person skilled in the art, based on this knowledge, will be able to adapt the shearing speed in order to optimize this step.

[0051] The application of a compression ratio varying from 2 to 20 times makes it possible to obtain the powder according to the invention.

[0052] Temperature control during the process is important. Indeed, too high a temperature leads to degradation of the rubber polymers and the possible breaking of the carbon bonds. The breaking of these bonds means the depolymerization of the rubber and the loss of its essential mechanical and elastic properties.

[0053] Shearing leads to significant internal heating of the treated vulcanized rubber. It is therefore essential to specifically regulate the temperature during the metactivation process, in order to prevent any problem of thermal degradation linked to excessive self-heating of the vulcanized rubber treated according to the invention. This is why it is important to control the temperature of the system. The latter must therefore remain below 80°C during the process, preferably below 60°C.

[0054] At this temperature, only bonds containing sulfur are broken.

[0055] Typically, the temperature may vary from 25 to 80°C, preferably from 40 to 80°C, preferably from 50 to 75°C, preferably from 40 to 60°C, preferably from 60 to 80°C and even more preferably from 50 to 70°C.

[0056] On the other hand, the compression of the rubber grains produces an expansion of these grains similar to an “explosion” of the grains into finer particles forming the powder according to the invention.

[0057] This expansion of the grains is critical to obtain a malleable powder and reusable and which has the mechanical properties of virgin rubber.

[0058] The powder thus obtained has an expansion rate varying from 0.5 to 1.20, preferably from 1.0 to 1.20 and even more preferably from 1.1 to 1.15.

[0059] Compared to rubber granules, the powder obtained has a reduced density.

[0060] The density of the powder according to the invention can thus range from 0.3 to 0.5, preferably from 0.40 to 0.47.

[0061] The powder, obtained by the metactivation process, comes from used rubber parts from the railway industry, in particular rail soles.

[0062] Used rubber parts are chosen from the group comprising rail soles, sleeper shoes, track switch mats and wagon mats.

[0063] Preferably, the used rubber parts are rail soles.

[0064] Since rubber is the majority component of these parts, its content in said parts is at least 30% by weight relative to the weight of the sole, preferably 40 to 90% by weight, preferably 40 to 80% by weight, preferably 40 to 70% by weight and even more preferably 40 to 60% by weight.

[0065] Typically, the rubber included in these parts is a vulcanized rubber selected from the group consisting of natural rubber, polyisoprene, styrene-butadiene rubber (SBR), polybutadiene (BR), hydrogenated nitrile rubber (HNBR), nitrile rubber (NBR), chlorobutadiene (CR), ethylene-propylene-diene monomer rubbers (EPDM), ethylene-propylene rubber (EPM), chlorosulfonated polyethylene (CSM), isobutylene-isoprene rubber (IIR), polyurethanes, acrylic rubber (ACM) and combinations thereof.

[0066] Examples of preferred vulcanized rubber within the scope of the invention are natural rubber (NR), butadiene rubber (BR) and styrene-butadiene rubber alone or in a mixture.

[0067] Preferably, the vulcanized rubber is a blend of NR / SBR.

[0068] Typically, the rubber content contained in the powder described above is at least 30% by weight, preferably at least 40% by weight, preferably at least 50% by weight and even more preferably at least 60%.

[0069] In certain embodiments, the rubber content contained in the powder ranges from 30 to 80% by weight, preferably from 35 to 80% by weight, preferably from 35 to 70% by weight, preferably from 40 to 75% by weight and even more preferably from 40 to 55% by weight.

[0070] The powder obtained by this process contains partially devulcanized rubber.

[0071] These mild physical conditions allow only the C- bonds to be “broken”. S and SS without breaking CC bonds and thus avoid depolymerization or degradation of the polymers contained in the starting rubber.

[0072] The rubber contained in this powder has mechanical and elastic properties similar to virgin rubber.

[0073] This rubber is malleable, reusable, revulcanizable, crosslinkable, recom-poundable.

[0074] The devulcanization rate of the rubber contained in the powder, measured by the Swelling technique of the gel fraction according to the Soxhlet method and the Flory-Rehner equation for example, varies from 5 to 99% relative to the vulcanized elastomer(s) contained in the used rubber, preferably from 10 to 90% and even more preferably from 20 to 70%.

[0075] Typically, the powder obtained has a particle size ranging from 1 to 1000 pm, preferably from 5 to 500 pm and even more preferably from 10 to 400 pm.

[0076] The metactivation process makes it possible to preserve the structure of the rubber polymers except for the sulfur bridges.

[0077] Thus, the degradation rate, measured in gel fraction by the Soxhlet method for example, is less than 30% and preferably ranges from 10 to 20%. Regenerated polymeric material

[0078] The polymeric material developed by the Applicant is obtained by mixing a powder, obtained from used rubber parts from the railway industry, with one or more plasticizers at a temperature ranging from 80 to 130°C, said powder being obtained by steps of compression and shearing of an granulate obtained from said used rubber parts from the railway industry.

[0079] The material may be in the form of a paste or a powder at room temperature.

[0080] In the context of the invention, the term “ambient temperature” means a temperature ranging from 10 to 30°C, preferably from 20 to 25°C.

[0081] The material is preferably in the form of a powder at room temperature.

[0082] When this material is heated, it transforms into a paste. Obtaining a paste, under the effect of temperature, is important and allows for a homogeneous structure compatible with other materials and, at the same time, the subsequent reaction of the polymeric material with the compounds necessary to produce a new part of the railway industry.

[0083] In other words, the resulting paste ensures that a homogeneous mixture is obtained during the subsequent reaction of the polymeric material with various additives, for example to prepare a raw mixture.

[0084] The paste obtained, under the effect of temperature, thus has a very good suitability for reformulation in rubber recycling processes, which is superior to that of the powder resulting directly from the metactivation process.

[0085] The rubber contained in the polymeric material is in fact malleable and has mechanical and elastic properties similar to virgin rubber, which facilitates its reaction with other materials such as virgin rubber during the preparation of a raw mixture, for example.

[0086] Generally, used rubber parts from the railway industry useful in the context of the invention include, but are not limited to, rail pads, sleeper shoes, track switch mats and wagon mats.

[0087] The resulting polymeric material comprises completely devulcanized rubber. In addition, the sulfur present in the rubber contained in the powder as described above is no longer present. Preferably, the material is in the form of a paste or powder.

[0088] The polymeric material thus obtained is regenerated and can be reused as a raw mix, a masterbatch or as virgin rubber.

[0089] The mixing of the powder from vulcanized rubber with one or more plasticizers is typically carried out at a temperature ranging from 80 to 130°C, preferably from 90 to 120°C, preferably from 80 to 120°C, preferably from 90 to 110°C.

[0090] A minimum temperature of 80°C, or even 90°C, is necessary to evaporate the sulfur present in the rubber.

[0091] These temperature ranges remain relatively mild compared to the temperatures disclosed in the prior art, often around 200-300°C.

[0092] These reduced temperatures also contribute to the preservation of carbon bonds and make it possible to maintain the integrity of the rubber and in particular its mechanical and elastic properties.

[0093] Advantageously, the mixing time is short and does not exceed 1 hour. Thus, the mixing time typically ranges from 3 to 20 minutes, preferably from 4 to 15 minutes and even more preferably from 5 to 10 minutes.

[0094] In some embodiments, the sulfur is completely evaporated after 5 min of mixing.

[0095] In some embodiments, the sulfur is completely evaporated after 8 min of mixing.

[0096] In some embodiments, the sulfur is completely evaporated after 10 min of mixing.

[0097] The mixing step can be carried out in an internal mixer, in particular a Banbury® type mixer, an external mixer, a blender mixer, a kneader, a twin-roll mill or an extruder-mixer.

[0098] The plasticizer(s) used in the mixture allow the material to be obtained in the form of a paste, in particular when the latter is heated. Examples of plasticizers include, but are not limited to, oils such as vegetable oils, mineral oils, non-petroleum oils, fatty acids such as stearic acid or a salt thereof and tall oil fatty acids (TOFA).

[0099] The plasticizer(s) are typically incorporated at a level of 5 to 10% by weight of the mixture.

[0100] In addition, traditional additives in the rubber industry can also be added to this mixture, such as polymerizers, antioxidants, reinforcing fillers, mineral residues, stabilizers, compatibilizers, accelerators, retarders, etc.

[0101] Antioxidants are for example 6PPD, 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ) and dioctyldiphenylamine.

[0102] Reinforcing fillers typically useful in the context of the invention include carbon black, silica, clay, organic fiber, inorganic metal powder, mineral powder, talc, calcium sulfate, calcium silicate, etc.

[0103] A preferred reinforcing filler is carbon black.

[0104] Polymerizers may be, for example, vinyl acetate, isocyanates, silanes, epoxy resins or phenolic resins.

[0105] Compatibilizers and stabilizers are additives known in the field of rubber and to those skilled in the art.

[0106] Compatibilizers include, for example, acrylates.

[0107] Non-limiting examples of accelerators include N-cyclohexylbenzothiazole-2-sulfenamide (CBS) and AUV'-dicy-clohexylbenzothiazole-2-sulfenamide (DCB S).

[0108] A preferred retarder within the scope of the invention is V-(cyclohexylthio)phthalimide (PVI).

[0109] A person skilled in the art, based on his knowledge, will be able to select the appropriate additives and their content according to the desired properties of the railway industry part. Preferably, this part is a rail sole.

[0110] The content of these additives in the mixture does not exceed 5% by weight, preferably 2% by weight and even more preferably 1% by weight.

[0111] The obtained polymeric material can be used as a raw mix or masterbatch or virgin rubber.

[0112] In embodiments, the polymeric material is used to form a green mixture

[0113] In embodiments, the polymeric material is used to form a masterbatch.

[0114] In embodiments, the polymeric material may also be blended with a raw mix or a masterbatch.

[0115] The raw mix is ​​typically prepared by compounding.

[0116] It is then shaped and vulcanized by compression, injection, or extrusion to produce a new rubber part for the railway industry, in particular rail soles. Rubber parts for the railway industry

[0117] The final part is manufactured after successive stages of compounding, shaping and firing.

[0118] Compounding makes it possible to prepare, for example, a raw mixture, prepared in a mixer.

[0119] The mixing temperature can vary from 60 to 140°C, preferably from 80 to 140°C, preferably from 80 to 110°C, preferably it is 90°C.

[0120] This raw mixture typically comprises a polymeric material according to the invention alone or in a mixture with virgin rubber.

[0121] In this raw mixture, the polymeric material is present at a content of at least 30% by weight, preferably at least 40% and even more preferably at least 50% by weight.

[0122] The total rubber content in the raw mixture may range from 30 to 90% by weight, preferably from 35 to 80% by weight and even more preferably from 40 to 70% by weight.

[0123] The invention also relates to a rubber part for the railway industry comprising a polymeric material according to the invention.

[0124] The polymeric material is present at a content of at least 30% by weight.

[0125] In embodiments, the part comprises the polymeric material in admixture with a raw mix or masterbatch or virgin rubber. Preferably, the part comprises the material according to the invention in admixture with virgin rubber.

[0126] It is essential that at least 30% of the rubber raw material of the rubber part comes from waste from used rubber parts of the railway industry in order for the finished part to be qualified as a "green part".

[0127] The rubber part of the railway industry is chosen from the group comprising rail pads, sleeper shoes, switch mats and wagon mats.

[0128] Preferably, the rubber part is a rail sole.

[0129] In preferred embodiments, the rubber part is prepared from a green mixture comprising the polymeric material described above alone or in admixture with virgin rubber.

[0130] In embodiments, the polymeric material is present at a content of at least 30% by weight, preferably at least 40% and even more preferably of at least 50% by weight. Preferably, the rubber part is a rail sole.

[0131] Preferably, the virgin rubber may be NR or SBR or a blend of NR / SBR.

[0132] In these embodiments, the proportion of polymeric material / virgin rubber varies from 5 to 80%, preferably from 10 to 80%, preferably from 30 to 80%, preferably from 40 to 60% by weight.

[0133] Examples of rubber contained in the part according to the invention include natural rubber, polyisoprene, styrene-butadiene rubber (SBR), poly-butadiene (BR), hydrogenated nitrile rubber (HNBR), nitrile rubber (NBR), chlorobutadiene (CR), ethylene-propylene-diene monomer rubbers (EPDM), ethylene-propylene rubber (EPM), chlorosulfonated polyethylene (CSM), isobutylene-isoprene rubber (IIR), polyurethanes, acrylic rubber (ACM) and combinations thereof.

[0134] The rubber contained in the part according to the invention is a vulcanized rubber.

[0135] Advantageously, the rubber part comprises a rubber content ranging from 30 to 90% by weight, preferably from 35 to 70% by weight and even more preferably from 40 to 60% by weight.

[0136] In embodiments, the rubber part comprises: 40 to 50% by weight of rubber, from 4 to 10% by weight of plasticizers, from 15 to 30% in carbon black and from 15 to 30% by weight of mineral residues

[0137] The nature of the plasticizers, rubber and mineral residues is as described above.

[0138] In embodiments, the rubber contained in the part according to the invention is derived solely from the polymeric material described above.

[0139] In embodiments, the rubber contained in the part according to the invention comes from a mixture of the polymeric material described above and virgin rubber.

[0140] In embodiments, the part is prepared from a masterbatch comprising the polymeric material according to the invention.

[0141] In embodiments, the ratio of polymeric material to virgin rubber may typically vary from 10 / 90 to 90 / 10, preferably 30 / 70 to 70 / 30 and even more preferably 50 / 50.

[0142] The part according to the invention further comprises additives chosen from the group comprising polymerizers, compatibilizers, reinforcing fillers, accelerators, antioxidants, retarders, vulcanization activators, agents vulcanizers and other additives traditionally used by the rubber industry and known to those skilled in the art.

[0143] The selection of these additives and the quantities to be used depend on the rubbers used and the final application of the railway industry part and are readily selectable by a person of ordinary skill in the art.

[0144] A preferred reinforcing filler is carbon black.

[0145] In the present invention, the railway industry part is shaped by conventional rubber processing techniques known to those skilled in the art.

[0146] The part is thus typically shaped by injection, extrusion or compression of the raw mixture or masterbatch comprising the polymeric material according to the invention.

[0147] Advantageously, the polymeric material according to the invention makes it possible to produce a recycled rubber part for the railway industry having mechanical and physical properties comparable or superior to those of a part produced by a conventional process.

[0148] Its elongation at break typically varies from 200 to 700%, preferably from 300 to 600%, measured by ASTM D412

[0149] The rubber part for the railway industry obtained according to the invention has a hardness ranging from 30 to 90 Shore A, preferably from 40 to 80 Shore A measured according to the ASTM D2240 standard.

[0150] The rubber part for the railway industry obtained according to the invention also has a density ranging from 0.9 to 1.5 measured according to the stacking method.

[0151] The invention also relates to a rail base comprising a polymeric material as described above.

[0152] The invention also relates to a process for preparing the polymeric material described above comprising the following successive steps: a. Grinding and granulation of vulcanized rubber from used rubber parts from the railway industry b. Compression and shearing of the rubber granulate formed in step a) c. Mixing the powders obtained in step b) with one or more plasticizers a temperature ranging from 80 to 130°C

[0153] The temperature of step b) is advantageously less than 80°C, preferably less than 60°C.

[0154] The temperature in step c) preferably ranges from 80 to 120°C and preferably from 90 to 120°C.

[0155] The invention also relates to a method for preparing a ca- rail industry outlet including the following steps: a. Devulcanization of rubber from a used part from the railway industry to produce a polymeric material as described above, b. Compounding of the polymeric material obtained in step a), and c. Shaping and vulcanization

[0156] Preferably, the prepared rubber part is a rail sole.

[0157] Compounding of the polymeric material allows the formation of a raw or masterbatch.

[0158] Vulcanization is carried out by conventional methods well known to those skilled in the art, including the addition of vulcanizing agents.

[0159] Examples of vulcanizing agents known from the prior art include sulfur-based compounds, sulfur donors and vulcanization accelerators, vulcanizing resins (e.g. resorcinol-formaldehyde based) or peroxides.

[0160] The shaping of the final part is typically obtained by injection, extrusion or compression, advantageously by extrusion.

[0161] The process makes it possible to provide a new, recycled part for the railway industry, with performance comparable to the parts obtained containing only “new” rubber.

[0162] The following examples are given for illustrative purposes, but should in no way be considered as limiting the present invention.

[0163] [Fig.l] shows a curve of the rheological monitoring during the cooking stage of a rail sole in preparation.

[0164] EXAMPLES

[0165] Example 1: composition and physicochemical characteristics of a rail base

[0166] The chemical composition of a used traditional rail sole is described in Table 1a and its physicochemical characteristics are presented in Table 1b. Components Content in parts (phr), by weight, per 100 parts of rubber Natural rubber SMR CV 60 100 Zinc oxide 5.0 Carbon black SRF N-774 80.0 TMQ 1.0 IPPD 1.5 Struktol Zeh-DL 3.0 Protector G35 5.0 MBS 1.44 Struktol TBTD 65 0.65 Struktol SU 135 0.8 Table 1a: Chemical composition of a rail base Physicochemical characteristics Value Curing 15 minutes / 150 °C Modulus 100 5.0 MPa Modulus 300 17.9 MPa Tensile strength 18.9 MPa Effective absorption band 320% Rebound 37 % Hardness 66 Shore A Relative density 1.19 g.cm3 DRC (22 h / 70 °C) 18 % Oscillating disc rheometer (150 °C) T2: 5.2 / T90: 9.0 Mooney viscosity (ML(l+4) 100 °C) 80 Table 1b: Physicochemical characteristics of a rail base

[0167] Example 2: Preparation of polymeric materials according to the invention

[0168] The rail base described in Example 1 is crushed and an aggregate with a particle size of 3 mm is obtained.

[0169] This granulate is then subjected to the metactivation process in a metactivation machine as described in documents FR 2946896 A1 and WO2011 / 004079 A2.

[0170] The powder obtained has a density of 0.45 and a particle size of less than 0.4 mm measured by ASTM D5644.

[0171] Its composition is as follows: - NR / SBR / BR rubber (57%) - carbon black (28%). - Acetone extract (6%) - Ashes (9%)

[0172] This powder is used to manufacture the following polymeric materials 2A, 2B and 2C. 2A polymeric material

[0173] The powder is introduced into a mixer with TOFA (5 phr). The mixture is heated at 90 °C for 10 min. The powder turns into a paste. The polymeric material 2A is allowed to cool and then collected. 2B polymeric material

[0174] The powder is introduced into a mixer with vegetable oil (5 phr). The mixture is heated at 90 °C for 10 min. The powder turns into a paste. The polymeric material 2B is allowed to cool and then collected. 2C polymeric material

[0175] The powder is introduced into a mixer with TOFA (5 phr), 6PPD (1.5 phr) and 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ) (1.5 phr). The mixture is heated at 90 °C for 10 min. The powder turns into a paste. The 2C polymeric material is allowed to cool and then collected.

[0176] Example 3: Preparation of rail soles according to the invention

[0177] 3A sole prepared from 30% of 2A polymeric material

[0178] Into an internal Banbury type mixer are introduced the polymeric material 2A (67 phr), natural rubber, carbon black HAF774 (55 phr), paraffin oil (5 phr), 6PPD (1.5 phr), TMQ (1.5 phr), paraffin wax (2 phr), zinc oxide (5 phr) and stearic acid (1 phr).

[0179] The mixture is heated to 90°C in a Banbury mixer.

[0180] The following additives are then added during the reaction, as known from those skilled in the art, tetramethylthiuram disulfide (TMTD) (0.75 phr), 2,2-dithiobis(benzothiazole) (MBTS) (1.75 phr), dipropylene glycol (DPG) (0.75 phr) and sulfur (0.75 phr).

[0181] The part is cooked at 150°C for 15 min.

[0182] This 3A sole has a modulus of 15 MPa, an elongation at break of 460% and a hardness of 72 Shore A.

[0183] Example 4: Studies of the rheological behavior, according to ASTM 2084, of a rail sole according to the invention during the baking step

[0184] The vulcanization of the rubber contained in a rail sole made from the polymeric material according to the invention is studied.

[0185] The rheological profile of the rubber of a rail sole in preparation comprising 40% of polymeric material, during its curing, is monitored by rheometry on an oscillating disk rheometer.

[0186] The cooking temperature is 160°C and the duration is 10 min.

[0187] The curve obtained is presented in [Fig. 1].

[0188] The change in curve indicates a chemical modification of the rubber and thus attests to the vulcanization of the rubber contained in the sole being prepared. Crosslinking is very rapid and confirms that the polymeric material obtained according to the invention behaves like virgin rubber.

Claims

Claims

1. Polymeric material obtained by mixing a powder, obtained from used rubber parts from the railway industry, with one or more plasticizers at a temperature ranging from 80 to 130°C, said powder being obtained by steps of compression and shearing of an granulate obtained from said used rubber parts from the railway industry.

2. Polymeric material according to claim 1 characterized in that the powder has a particle size ranging from 1 to 1000 pm, preferably from 5 to 500 pm and even more preferably from 10 to 400 pm.

3. Polymeric material according to one of the preceding claims characterized in that the rubber parts of the railway industry comprise vulcanized rubber chosen from the group comprising natural rubber, polyisoprene, styrene-butadiene rubber (SBR), polybutadiene (BR), hydrogenated nitrile rubber (HNBR), nitrile rubber (NBR), chlorobutadiene (CR), ethylene-propylene-diene monomer rubbers (EPDM), ethylene-propylene rubber (EPM), chlorosulfonated polyethylene (CSM), isobutylene-isoprene rubber (IIR), polyurethanes, acrylic rubber (ACM) and their combination.

4. Polymeric material according to one of the preceding claims, characterized in that the plasticizer(s) are chosen from the group comprising oils such as vegetable oils, mineral oils, non-petroleum oils, fatty acids such as stearic acid or one of its salts and tall oil fatty acids (TOFA).

5. Polymeric material according to one of the preceding claims, characterized in that the aggregate has a particle size ranging from 1 to 4 mm, preferably from 2 to 4 mm and preferentially from 3 mm.

6. Polymeric material according to one of the preceding claims, characterized in that the used rubber parts from the railway industry are chosen from the group comprising rail soles, sleeper shoes, track device mats and wagon mats.

7. Rubber part for the railway industry characterized in that it comprises a polymeric material which is the subject of one of claims 1 QA

8. d U. Rubber part for the railway industry according to claim 7, characterized in that the polymeric material is mixed with a raw mixture or a masterbatch or virgin rubber, of preferably with virgin rubber.

9. Rubber part for the railway industry according to one of claims 7 or 8, characterized in that the polymeric material is present at a content of at least 30% by weight.

10. Rubber part for the railway industry according to one of claims 7 to 9, characterized in that it comprises: - between 40 and 50% by weight of rubber, - between 4 and 10% by weight of plasticizers, - between 15 and 30% by weight of carbon black - between 15 and 30% by weight of mineral residues.

11. Rubber part for the railway industry according to claim 10, characterized in that the rubber is selected from the group comprising natural rubber, polyisoprene, styrene-butadiene rubber (SBR), polybutadiene (BR), hydrogenated nitrile rubber (HNBR), nitrile rubber (NBR), chlorobutadiene (CR), ethylene-propylene-diene monomer rubbers (EPDM), ethylene-propylene rubber (EPM), chlorosulfonated polyethylene (CSM), isobutylene-isoprene rubber (IIR), polyurethanes, acrylic rubber (ACM) and their combination.

12. Rubber part for the railway industry according to claim 11 characterized in that the rubber is a mixture of NR / SBR.

13. Rubber part for the railway industry according to one of claims 7 to 12, characterized in that the part is chosen from the group comprising rail soles, sleeper shoes, track device mats and wagon mats, preferably rail soles.

14. Rubber part for the railway industry according to claim 13 characterized in that the part is a rail sole.

15. Rail base comprising a polymeric material according to one of claims 1 to 6.

Citation Information

Patent Citations

  • REACTEUR MULTIPHASE A MICRO AUTO-EXPLOSION

    FR2946896A1

  • Automatic rubber powder plasticizing method and equipment for automatic rubber powder plasticizing method

    EP2371886B1

  • Elastomer-based shock-absorber pad for railway

    FR2630466A1

  • Rubber mixture for an elastic intermediate layer for a rail support

    US5735457A

  • Rail arrangement

    US6471139B1