Aluminum alloy for recycling and manufacturing process

The aluminum alloy composition addresses the need for recyclable materials by providing enhanced mechanical properties and formability, leveraging specific element ratios and manufacturing processes to create high-quality automotive components from post-consumer waste.

FR3148443A1Pending Publication Date: 2024-11-08CONSTELLIUM NEUF BRISACH SAS +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
FR2023004472
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

There is a need for aluminum alloys that provide an excellent compromise between mechanical strength, formability, corrosion resistance, and the ability to be manufactured using maximum post-consumer waste, particularly from end-of-life vehicles, to meet the increasing demand for recycled materials in automobile manufacturing.

Method used

An aluminum alloy composition comprising specific weight percentages of Si, Fe, Cu, Mn, Mg, Zn, Ti, Cr, and other elements, with controlled ranges to enhance recyclability and mechanical properties, manufactured through processes like semi-continuous vertical casting, homogenization, hot deformation, and quenching, resulting in products suitable for rolling or extrusion.

Benefits of technology

The alloy achieves improved formability, mechanical strength, and corrosion resistance while utilizing high percentages of post-consumer waste, optimizing the recycling process and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The invention relates to an aluminum alloy with the following composition, in % by weight: Si: approximately 1.7% – approximately 7.0%, Fe: approximately 0.3% – approximately 0.5%, Cu: approximately 0.3% – approximately 1.0%, Mn: approximately 0.2% – approximately 0.6%, Mg: approximately 0.2% – approximately 0.6%, Zn: approximately 0.2% – approximately 0.6%, Ti, Cr, Sn, Pb, Zr, V, Sr, Ni: ≤ approximately 0.1%, other elements: each ≤0.05%, together ≤ 0.15%, remainder: Al. The invention also relates to a rolled or extruded alloy product according to the invention. The alloy according to the invention is particularly suitable for recycling and preferably comprises at least 20% post-consumer waste, preferably from end-of-life vehicles, more preferably from aluminum fragmented by automotive shredders, the twitch. Abbreviated figure: Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Aluminum alloy for recycling and manufacturing process Field of invention

[0001] The invention relates to the field of aluminum alloys intended for the manufacture of parts for motor vehicles produced from recycled products. State of the art

[0002] Aluminum alloys are increasingly used in automobile construction to reduce the weight of vehicles and thus reduce fuel consumption and greenhouse gas emissions.

[0003] Usually, aluminum alloys used in automobile construction are recycled in castings and in particular engine parts. However, the evolution of automobile propulsion from thermal engines to electric motors will eliminate this recycling channel.

[0004] There is therefore a demand for aluminium alloys made from recycled products, which is all the more important as manufacturers must increase the use of recycled products to reduce the quantity of CO2 equivalent emitted by vehicle production.

[0005] Application US20210108293 discloses an aluminum alloy sheet having a chemical composition containing Si: 2.3-3.8 mass%, Mn: 0.35-1.05 mass%, Mg: 0.35-0.65 mass%, Fe: 0.01-0.45 mass%, and at least one element selected from the group consisting of Cu: 0.0010-1.0 mass%, Cr: 0.0010-0.10 mass%, Zn: 0.0010-0.50 mass%, and Ti: 0.0050-0.20 mass%. The ratio of the Si content to the Mn content is 2.5 or more and 9.0 or less. Aluminum alloy sheet has an elongation of 23% or more and a work hardening exponent of 0.28 or more at a nominal strain of 3%. Such aluminum alloy sheet is well suited for press forming (stamping) applications, such as automotive body panel forming.

[0006] Application WO2018 / 175876 discloses techniques for casting metal products having high strength and formability from recycled scrap metal, without adding a substantial amount or even any amount of primary aluminum. Additional alloying elements, such as magnesium, can be added to scrap metal, which can be cast and processed to produce a metal coil of a desired final thickness and having desirable metallurgical and mechanical properties, such as high strength and formability. Inexpensive and recycled scrap metal can thus be reused efficiently for new applications, in the automotive industry or as raw material for beverage cans.

[0007] Application JP2005298922 addresses the problem of inexpensively providing an aluminum alloy sheet for forming, which has adequate bending formability, low bending anisotropy and superior bake hardening ability after coating, which has low room temperature aging and adequate resistance to line marks.Its solution is an aluminum alloy sheet made of an Al-Mg-Si base alloy or an Al-Mg-Si-Cu base alloy; satisfying each condition of (C1 / 10+ Ci / 4) / 2 > Ci / 2 and 30 < (C 1 / 10+C1 / 4) < 500, when C1 / 10, Ci / 4 and Ci / 2 are defined as the cube orientation density at positions of 1 / 10, 1 / 4 and 1 / 2 depth from the sheet surface in the sheet thickness direction, respectively; has an orientation density {001} <210> in a range of 2 to 50, in a region of 1 / 10 to 1 / 4 depth in the direction of the sheet thickness; and has horn rates at 0 degrees and 90 degrees of 5% or more. The manufacturing method includes strictly prescribed casting and hot rolling conditions. The conditions of metallographic structures in a cast plate and a sheet after being hot rolled, which are intermediate products, are prescribed.

[0008] Application WO2022 / 026825 discloses novel 6xxx aluminum alloys. In one approach, a novel 6xxx aluminum alloy may comprise 0.25-0.60 wt.% Fe, 0.8-1.2 wt.% Si, 0.35-1.1 wt.% Mg, 0.05-0.8 wt.% Mn, up to 0.30 wt.% Cu, up to 0.35 wt.% Zn, up to 0.15 wt.% Ti, up to 0.15 wt.% each of Cr, Zr, and V, with the remainder being aluminum, accessory elements, and impurities. The novel 6xxx aluminum alloys may be made from recycled aluminum alloys.

[0009] WO9960181 discloses an automotive aluminum alloy which has an aluminum alloy composition comprising 3.5-5 wt% Si, 0.3-1.5 wt% Mg, 0.4-1.5 wt% Zn, 0.4-1.5 wt% Cu, 0.4-1.5 wt% Fe and 0.6-1 wt% Mn, and further one or more of 0.01-0.2 wt% Cr, 0.01-0.2 wt% Ti, 0.01-0.2 wt% Zr and 0.01-0.2 wt% V, the residue of the composition being aluminum and obligatory impurities.

[0010] There is therefore a need to recycle scraps and waste to produce bodywork sheets for the automotive industry. Problem posed

[0011] The problem to be solved is to develop an aluminum alloy which aims for an excellent compromise between mechanical strength, its formability, its corrosion resistance, its manufacturing ability while being produced with a maximum post-consumer waste. Subject of the invention

[0012] A first object of the invention is an aluminum alloy of composition, in % by weight: Si: about 1.7% - about 7.0%, Fe: about 0.2% - about 0.8%„ Cu: about 0.3% - about 1.0%, Mn: about 0.2% - about 0.6%, Mg: about 0.2% - about 0.6%, Zn: about 0.2% - about 0.6%, Ti, Cr, Sn, Pb, Zr, V, Sr, Ni: < about 0.1%, other elements: each <0.05%, together <0.15%, remainder: Al.

[0013] A second subject of the invention is a rolled or extruded alloy product according to the invention.

[0014] A third object of the invention is a method of manufacturing a product according to the invention comprising the successive steps: (a) Supply of aluminium alloys and additive metals, with at least 20% of aluminium alloys in the form of post-consumer waste, b) Optional sorting of post-consumer waste, c) Production of an alloy according to the invention, from aluminium alloys comprising optionally sorted post-consumer waste and supplied addition metals d) Casting of the alloy in a raw form, preferably by semi-continuous vertical casting, e) Homogenization and / or reheating of the raw form, f) Hot and optionally cold deformation by rolling or extrusion of the raw form, g) Solution treatment then quenching of the raw form thus deformed, h) Optionally pre-tempered typically at a pre-tempering temperature of 60 to 120°C for a period of 1 to 24 hours, i) Maturation preferably from 24 hours to 6 months.

[0015] A fourth object of the invention is the use of a product according to the invention for the manufacture of parts for motor vehicles. Description of figures

[0016] [Fig.l]: This figure shows the LDH as a function of the recycling ability. [Fig.2]: This figure shows the Ag% elongation in the T4 state as a function of the tendency to crack during cold rolling (crackability). [Fig.3]: This figure shows the trade-off between LDH and yield strength at T4. [Fig.4]: This figure shows describes the LDH measuring tool. Description of the invention

[0017] All aluminium alloys referred to below are designated, unless otherwise stated, according to the rules and designations defined by the "Aluminum Association" in the "Registration Record Series" which it publishes regularly. Unless otherwise stated, the compositions are expressed in % by weight. The expression 1.4 Cu means that the copper content expressed in % by weight is 1.4%. The alloy groups, also called series, are defined in EN 573-1 (2005).

[0018] The metallurgical states in question are designated according to European standard EN-515.

[0019] The static mechanical characteristics in tension, in other words the breaking strength Rm, the conventional elastic limit at 0.2% elongation Rp0.2, the elongation at necking Ag% and the elongation at break A%, are determined by a tensile test according to standard NF EN ISO 6892-1, the sampling and the direction of the test being defined by standard EN 485-1.

[0020] The bending angles, called alpha, are determined by 3-point bending test according to standard NF EN ISO 7438 and procedures VDA 238-100 and VDA 239-200 version 2017.

[0021] Unless otherwise stated, the definitions of standard EN 12258 apply.

[0022] The LDH parameter is widely used for evaluating the stamping ability of sheet metal. It has been the subject of numerous publications, including that of R. Thompson, "The LDH test to evaluate sheet metal formability - Final Report of the LDH Committee of the North American Deep Drawing Research Group", SAE conference, Detroit, 1993, SAE Paper No. 930815. This is a stamping test of a blank blocked at the periphery by a retaining ring. The blank-holding pressure is adjusted to prevent slippage in the retaining ring. The blank, measuring 120 mm x 160 mm, is stressed in a mode close to plane deformation. The punch used is hemispherical. [Fig. 4] specifies the dimensions of the tools used to carry out this test. Lubrication between the punch and the sheet is provided by graphite grease. The punch descent speed is 50 mm / min. The so-called LDH value is the value of the punch displacement at break, i.e. the limit depth of the drawing.It actually corresponds to the average of three tests, giving a 95% confidence interval on the measurement of 0.2 mm.

[0023] Unless otherwise stated, the definitions of EN 12258-1 (1998) apply.

[0024] Unless otherwise stated, the definitions of EN 12258-3 (2003) apply.

[0025] Pure or alloyed aluminum in the form of a primary metal ingot generally has the disadvantage of generating significant CO2 emissions during its manufacture and we therefore try to limit its use. As regards other sources of metal, we distinguish between pre-consumer manufacturing scrap, which is generated before the metal is delivered to the end customer: the window buyer, the vacuum chamber user, the car buyer, the airline, etc. and post-consumer waste which is recovered after use of the product, typically from the car at the scrapyard, in a sorting center. The manufacturing stages of aluminum products generate numerous pre-consumer manufacturing scraps during all the stages.Examples of post-consumer waste include the ends of cast plates or billets that have been dropped before hot working, the ends of rolled or extruded products that have been dropped during the sheet or profile manufacturing process, the skeletons of blanks used for stamping, machining chips, etc. Examples of post-consumer waste include used window frames, scrapped car parts, crushed cars, dismantled aircraft, etc. Post-consumer waste can be supplied raw, in compacted form, or optionally after being melted separately and possibly solidified. Additional elements are also supplied in suitable forms. These can be elements in their metallic form or in an alloyed form.

[0026] Unless otherwise stated, the definitions of the ISRI (Institute of Scrap Recycling Industries) “Scrap Specification Circular 2022” apply. In particular, twitch is defined as aluminum waste or scrap fragmented by automotive shredders.

[0027] The twitch is derived from the wet or dry media separation device, the material is dry and contains not more than 1% maximum of free zinc, 1% maximum of free magnesium and 1% maximum of analytical iron. It contains not more than 2% total of non-metallic materials, including not more than 1% rubber and plastic. It is free from excessively oxidized materials, airbag cartridges or any sealed or pressurized articles.

[0028] Ambient temperature is any temperature compatible with human work from 5 to 35°C. Ambient temperature can be a temperature of 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C.

[0029] The term "approximately," when used in connection with a measurable numerical variable, refers to the stated value of the variable and all values ​​of the variable that are within the experimental error of the stated value or within ±10 percent of the stated value, whichever is greater. restraint. Detailed description

[0030] The invention is based on the observation made by the applicant that it is entirely possible, thanks to a suitable composition and manufacturing process, to produce sheets from the recycling of post-consumer aluminium waste having an acceptable suitability for stamping, good resistance to corrosion and mechanical properties particularly suited to the production of automobile bodywork.

[0031] The concentration ranges imposed on the constituent elements of this type of alloy are therefore explained by the following reasons:

[0032] Si: The Si content is from about 1.7% to about 7.0%. A Si content of at least about 1.7% facilitates the use of recycled products and in particular twitch. The Mg2Si or Mg5Si6 precipitates contribute to the hardening of the alloy during tempering, for example during the baking of paints. However, a Si content greater than about 7.0% degrades the suitability for hot and cold rolling by causing edge cracks which reduce the usable width of a rolled sheet or even cause it to break during manufacture. The excess of Si relative to Mg contributes to the formability in the T4 temper.

[0033] Advantageously Si > 2.0%, preferably Si > 2.2%, more preferably Si > 2.5%, more preferably Si >2.8% and / or Si < 6%, preferably Si < 5%, more preferably Si < 4.3%, more preferably Si <4.1%.

[0034] In one embodiment, the Si content is at least about 1.9%, or is at least about 2.1%, or is at least about 2.3%, or is at least about 2.5%, or is at least about 2.7%, or is at least about 2.9%, or is at least about 3.1%, or is at least about 3.3%, or is at least about 3.5%, or is at least about 3.7%, or is at least about 3.9%, or is at least about 4.1%, or is at least about 4.3%, or is at least about 4.5%, or is at least about 4.7%, or is at least about 4.9%, or is at least about 5.1%, or is at least about 5.3%, or is at least about 5.5%, or is at least about 5.7%, or is at least about 5.9%, or is at least about 6.1%, or is at least about 6.3%, or is at least about 6.5%, or is at least about 6.7%, and / or is at most about 6.8%, or is at most about 6.6%, or is at most about 6.4%, or is at most about 6.2%, or is at most about 6.0%, or is at most about 5.8%, or is at most about 5.6%, or is at most about 5.4%, or is at most about 5.2%, or is at most about 5.0%, or is at most about 4.8%, or is at most about 4.6%, or is at most about 4.4%, or is at most about 4.2%, or is at most about 4.0%, or is at most about 3.8%, or is at most about 3.6%, or is at most about 3.4%, or is at most about 3.2%, or is at most about 3.0%, or is at most about 2.8%, or is at most about 2.6%, or is at most about 2.4%, or is at most about 2.2%, or is at most about 2.0%.

[0035] Fe: The Fe content is from about 0.2% to about 0.8%. An Fe content of at least about 0.2% facilitates the use of recycled products. An Fe content above about 0.8% degrades the hot and cold rolling ability by causing edge cracks that reduce the usable width of a rolled sheet or even cause it to break during manufacture. An Fe content above about 0.8% may also make the product unsuitable for forming, in particular because the bending ability may be degraded.

[0036] Advantageously Fe > 0.25%, preferably Fe >0.30%, more preferably Fe > 0.33%, more preferably Fe >0.35%, more preferably Fe >0.37% and / or Fe < 0.75%, preferably Fe <0.65%, more preferably Fe < 0.55%, more preferably Fe <0.50%, more preferably Fe <0.45%.

[0037] In one embodiment, the Fe content is at least about 0.22%, or is at least about 0.24%, or is at least about 0.26%, or is at least about 0.28%, or is at least about 0.30%, or is at least about 0.32%, or is at least about 0.34%, or is at least about 0.36%, or is at least about 0.38%, or is at least about 0.40%, or is at least about 0.42%, or is at least about 0.44%, or is at least about 0.46%, or is at least about 0.48%, or is at least about 0.50%, or is at least about 0.52%, or is at least about 0.54%, or is at least about 0.56%, or is at least about 0.58%, or is at least about 0.60%, or is at least about 0.62%, or is at least about 0.64%, or is at least about 0.66%, or is at least about 0.68%, or is at least about 0.70%, or is at least about 0.72%, or is at least about 0.74%, or is at least about 0.76%, and / or is at most about 0.78%, or is at most about 0.76%,or is at most about 0.74%, or is at most about 0.72%, or is at most about 0.70%, or is at most about 0.68%, or is at most about 0.66%, or is at most about 0.64%, or is at most about 0.62%, or is at most about 0.60%, or is at most about 0.58%, or is at most about 0.56%, or is at most about 0.54%, or is at most about 0.52%, or is at most about 0.50%, or is at most about 0.48%, or is at most about 0.46%, or is at most about 0.44%, or is at most about 0.42%, or is at most about 0.40%, or is at most about 0.38%, or is at most about 0.36%, or is at plus about 0.34%, or is at most about 0.32%, or is at most about 0.30%, or is at most about 0.28%, or is at most about 0.26%, or is at most about 0.24%. ,

[0038] Cu: The Cu content is about 0.3% about 1.0%. Copper is an element participating in hardening precipitation, which is favorable for increasing the yield strength in the T4 state and after baking of paints. A Cu content greater than 0.3% also facilitates the use of recycled products. A Cu content greater than about 1% degrades the ability to roll hot and cold by causing edge cracks which reduce the usable width of a rolled sheet or even cause it to break during manufacturing. In addition, a Cu content above about 1% hardens too much and then degrades the formability, in particular the bending ability.

[0039] Advantageously Cu > 0.43%, preferably Cu > 0.45%, more preferably Cu > 0.48%, more preferably Cu > 0.50%, more preferably Cu > 0.35% and / or Cu < 0.98%, preferably Cu < 0.97%, more preferably Cu < 0.95%, more preferably Cu < 0.92%, more preferably Cu < 0.90%.

[0040] In one embodiment, the Cu content is at least about 0.35%, or is at least about 0.40%, or is at least about 0.45%, or is at least about 0.50%, or is at least about 0.55%, or is at least about 0.60%, or is at least about 0.65%, or is at least about 0.70%, or is at least about 0.75%, or is at least about 0.80%, or is at least about 0.85%, or is at least about 0.90%, and / or is at most about 0.95%, or is at most about 0.90%, or is at most about 0.85%, or is at most about 0.80%, or is at most about 0.75%, or is at most about 0.70%, or is at most about 0.65%, or is at most about 0.60%, or is at most about 0.55%, or is at most about 0.50%, or is at most about 0.45%, or is at most about 0.40%.

[0041] Mn: The Mn content is about 0.2% to about 0.6%. Manganese can contribute to common intermetallic precipitates and dispersoids. A minimum Mn content of about 0.2% facilitates the use of recycled products. A Mn content above about 0.6% can degrade formability in the T4 state due in particular to the increase in the intermetallic fraction and the decrease in work hardening capacity at high deformations.

[0042] Advantageously Mn > 0.21%, preferably Mn >0.22%, more preferably Mn > 0.23%, more preferably Mn >0.24%, more preferably Mn >0.25% and / or Mn < 0.55%, preferably Mn <0.52%, more preferably Mn < 0.50%, more preferably Mn <0.47%, more preferably Mn <0.45%.

[0043] In one embodiment Mn > 0.2% and < 0.35% and preferably, Mn > 0.22% and < 0.33%.

[0044] In one embodiment, the Mn content is at least about 0.22%, or is at least about 0.24%, or is at least about 0.26%, or is at least about 0.28%, or is at least about 0.30%, or is at least about 0.32%, or is at least about 0.34%, or is at least about 0.36%, or is at least about 0.38%, or is at least about 0.40%, or is at least about 0.42%, or is at least about 0.44%, or is at least about 0.46%, or is at least about 0.48%, or is at least about 0.50%, or is at least about 0.52%, or is at least about 0.54%, or is at least about 0.56%, and / or is at most about 0.58%, or is at most approximately 0.56%, or is at most about 0.54%, or is at most about 0.52%, or is at most about 0.50%, or is at most about 0.48%, or is at most about 0.46%, or is at most about 0.44%, or is at most about 0.42%, or is at most about 0.40%, or is at most about 0.38%, or is at most about 0.36%, or is at most about 0.34%, or is at most about 0.32%, or is at most about 0.30%, or is at most about 0.28%, or is at most about 0.26%, or is at most about 0.24%.

[0045] Mg: The Mg content is from about 0.2% to about 0.6%. A Mg content of at least about 0.2% facilitates the use of recycled products. Mg2Si precipitates contribute to the hardening of the alloy during tempering, for example during paint baking. The excess of Si over Mg is favorable for formability in the T4 temper.

[0046] Advantageously Mg > 0.22%, preferably Mg >0.25%, more preferably Mg > 0.27%, more preferably Mg >0.32%, more preferably Mg >0.35% and / or Mg < 0.55%, preferably Mg <0.52%, more preferably Mg < 0.50%, more preferably Mg <0.47%, more preferably Mg <<0.45%.

[0047] In one embodiment, the Mg content is at least about 0.22%, or is at least about 0.24%, or is at least about 0.26%, or is at least about 0.28%, or is at least about 0.30%, or is at least about 0.32%, or is at least about 0.34%, or is at least about 0.36%, or is at least about 0.38%, or is at least about 0.40%, or is at least about 0.42%, or is at least about 0.44%, or is at least about 0.46%, or is at least about 0.48%, or is at least about 0.50%, or is at least about 0.52%, or is at least about 0.54%, or is at least about 0.56%, and / or is at most about 0.58%, or is at most about 0.56%, or is at most about 0.54%, or is at most about 0.52%, or is at most about 0.50%, or is at most about 0.48%, or is at most about 0.46%, or is at most about 0.44%, or is at most about 0.42%, or is at most about 0.40%, or is at most about 0.38%, or is at most about 0.36%, or is at most about 0.34%,or is at most about 0.32%, or is at most about 0.30%, or is at most about 0.28%, or is at most about 0.26%, or is at most about 0.24%. ,

[0048] Zn: The content is from about 0.2% to about 0.6%. Since Zn is an addition element in aluminum alloys, it is advantageous to accept it for the purpose of recycling aluminum scrap and waste, particularly from end-of-life vehicles. Thus, a Zn content of at least about 0.2% facilitates the use of recycled products. A Zn content greater than about 0.6% hardens the alloy to the T4 state but degrades its formability.

[0049] In one embodiment, the Zn content is at least about 0.22%, or is at least about 0.24%, or is at least about 0.26%, or is at least about 0.28%, or is at least about 0.30%, or is at least about 0.32%, or is at least about 0.34%, or is at least about 0.36%, or is at least about 0.38%, or is at least about 0.40%, or is at least about 0.42%, or is at least about 0.44%, or is at least about 0.46%, or is at least about 0.48%, or is at least about 0.50%, or is at least about 0.52%, or is at least about 0.54%, or is at least about 0.56%, and / or is at most about 0.58%, or is at most about 0.56%, or is at most about 0.54%, or is at most about 0.52%, or is at most about 0.50%, or is at most about 0.48%, or is at most about 0.46%, or is at most about 0.44%, or is at most about 0.42%, or is at most about 0.40%, or is at most about 0.38%, or is at most about 0.36%, or is at most about 0.34%, or is at most about 0.32%, or is at most about 0.30%, or is at most about 0.28%, or is at most about 0.26%, or is at most about 0.24%.

[0050] Cr: The Cr content is at most about 0.1% by weight. In some cases it can be added to refine the grains and stabilize the structure. Reducing the Cr content generally improves the formability measured with LDH. In some cases the present inventors have surprisingly found that a maximum Cr content of 0.08%, advantageously 0.05% and preferably 0.02% does not prevent the recycling of significant quantities of scrap from the automotive industry, in particular twitch.

[0051] In one embodiment, the Cr content is at least about 0.01%, or is at least about 0.02%, or is at least about 0.03%, or is at least about 0.04%, or is at least about 0.05%, or is at least about 0.06%, or is at least about 0.07%, or is at least about 0.08%, and / or is at most about 0.09%, or is at most about 0.08%, or is at most about 0.07%, or is at most about 0.06%, or is at most about 0.05%, or is at most about 0.04%, or is at most about 0.03%, or is at most about 0.02%.

[0052] In an advantageous embodiment the Cr content is at most 0.08%.

[0053] Ti: A maximum content of approximately 0.1%, preferably 0.10%, is required to avoid the conditions for the formation of primary phases during vertical casting, which have a detrimental effect on all of the claimed properties. This element can promote solid solution hardening leading to the required level of mechanical characteristics and this element also has a favorable effect on ductility in service and corrosion resistance. In one embodiment, the Ti content is at least approximately 0.01%.

[0054] In one embodiment, the Ti content is at least about 0.01%, or is at least about 0.02%, or is at least about 0.03%, or is at least about 0.04%, or is at least about 0.05%, or is at least about 0.06%, or is at least about 0.07%, or is at least about 0.08%, and / or is at most about 0.09%, or is at most about 0.08%, or is at most about 0.07%, or is at most about 0.06%, or is at most about 0.05%, or is at most about 0.04%, or is at most about 0.03%, or is at most about 0.02%.

[0055] Sn, Pb, Zr, V, Sr, Ni: The maximum content of these elements is approximately 0.1%, preferably 0.10%. In one embodiment, the content of these elements is at least approximately 0.01%. In one embodiment, the content of these elements is at least about 0.01%, or is at least about 0.02%, or is at least about 0.03%, or is at least about 0.04%, or is at least about 0.05%, or is at least about 0.06%, or is at least about 0.07%, or is at least about 0.08%, and / or is at most about 0.09%, or is at most about 0.08%, or is at most about 0.07%, or is at most about 0.06%, or is at most about 0.05%, or is at most about 0.04%, or is at most about 0.03%, or is at most about 0.02%.

[0056] In certain cases, the present inventors have surprisingly found that a maximum Ni content of 0.08% and advantageously 0.05% and preferably 0.03% does not prevent the recycling of significant quantities of scrap from the automobile industry, in particular twitch.

[0057] The other elements are typically impurities whose content is kept less than or equal to 0.05%, preferably strictly less than 0.05%, the whole being less than 0.15%, the remainder being aluminum.

[0058] In one embodiment the alloy according to the invention comprises at least 20% or at least 30% or at least 40% or at least 50% or at least 60% or at least 70% or at least 80% or at least 90% of post-consumer waste or at least, preferably from end-of-life motor vehicles, more preferably from aluminum fragmented by automotive shredders.

[0059] In an advantageous embodiment, the composition of the alloy according to the invention is: If: 1.7%-7.0%, Fe: 0.2% - 0.8% Cu: 0.3% - 1.0%, Mn: 0.2% -0.35%, Mg: 0.2% -0.6%, Zn: 0.2% -0.6%, Ti, Sn, Pb, Zr, V, Sr,: < 0.1%, Cr < 0.08%, Ni < 0.08% other elements: each <0.05%, together <0.15%, remainder: Al.

[0060] In another advantageous embodiment, the composition of the alloy according to the invention is: Si: 1.7%-7.0%, Fe: 0.2% - 0.8%, Cu: 0.40% - 1.0%, Mn: 0.2% -0.6%, Mg: 0.2% -0.6%, Zn: 0.2% -0.6%, Ti, Sn, Pb, Zr, V, Sr: < 0.1%, Cr < 0.08%, Ni < 0.08%, other elements: each <0.05%, together < 0.15%, remainder: Al.

[0061] The invention also relates to rolled or extruded alloy products according to the invention.

[0062] In an advantageous embodiment, the rolled products according to the invention are in the solution-treated, quenched and pre-tempered or solution-treated, quenched and tempered state.

[0063] The products according to the invention have an advantageous ability to be deformed by rolling. The rolling ability is considered satisfactory in particular when few cracks or cracks of short length form during rolling, that is to say in particular when the tendency to crack during cold rolling is low. By carrying out cold rolling tests as described in the example, a crackability in mm is measured corresponding to the maximum length of the cracks formed after cold rolling up to a thickness of 1 mm. The rolled products according to the invention advantageously have a crackability of less than or equal to 5 mm, preferably less than or equal to 4 mm, more preferably less than or equal to 3 mm.

[0064] In one embodiment, the rolled product according to the invention has an LDH greater than or equal to 27.5 mm, preferably greater than or equal to 28.0 mm, more preferably greater than or equal to 28.5 mm, more preferably greater than or equal to 28.7 mm. Increasing the LDH value makes it possible to improve the formability during stamping.

[0065] In one embodiment, the rolled product according to the invention has a minimum yield strength Rp0.2 in the T4 state of 70 MPa, preferably 80 MPa, more preferably 90 MPa and / or has a maximum yield strength Rp0.2 in the T4 state of 140 MPa, preferably 130 MPa, more preferably 120 MPa. Too low a yield strength in the T4 state will limit the yield strength after baking the paints. Too high a yield strength in the T4 state increases the drawing force. Limiting the maximum of the yield strength in the T4 state is a compromise which makes it possible to improve the formability measured with the LDH. In one embodiment, the yield strength Rp0.2 in the T4 state is at least 80 MPa and at most 100 MPa. This embodiment is a compromise which makes it possible to increase the formability and the ability to deform hot and cold without cracking. In another embodiment, the yield strength Rp0.2 in the T4 state is at least 105 MPa and at most 125 MPa. This embodiment is a compromise which makes it possible to increase the recyclability.

[0066] In one embodiment, the rolled product according to the invention has a minimum yield strength Rp0.2 after baking the paints of 200 MPa, preferably 210 MPa and / or has a maximum yield strength Rp0.2 after baking the paints of 260 MPa, preferably 250 MPa. Increasing the yield strength after baking the paints is advantageous for reducing the thickness of the parts. In one embodiment, the yield strength after baking the paints is at least 225 MPa, preferably 235 MPa. This embodiment is a compromise which also makes it possible to increase the suitability for recycling.

[0067] The manufacturing process for rolled or extruded products comprises the successive stages: supply, optionally sorting, alloying, casting, homogenization and / or reheating, hot and optionally cold deformation, solution treatment and quenching, optionally pre-tempering, and maturation.

[0068] The supply of aluminum alloys and addition metals is carried out, the aluminum alloys being at least 20%, preferably at least 30%, preferably at least 40%, preferably at least 50%, preferably at least 60%, preferably at least 70% in the form of post-consumer waste.

[0069] The post-consumer waste is preferably at least 20%, preferably at least 30%, preferably at least 40%, preferably at least 50%, preferably at least 60%, preferably at least 70% in the form of aluminum fragmented by automotive or twitch shredders.

[0070] Optionally, the post-consumer waste is sorted. In an advantageous embodiment, the post-consumer waste is crushed, separated by sieving, and waste larger than 1 cm is sorted between alloy families, the analysis being advantageously carried out by LIBS (Laser Induced Breakdown Spectroscopy) or by XRT (X-Ray Transmission).

[0071] An alloy according to the invention is produced from aluminum alloys comprising optionally sorted post-consumer waste and supplied addition metals.

[0072] A raw form is cast with an alloy according to the invention. Preferably the casting is carried out by semi-continuous vertical casting, with direct cooling (DC Casting). For hot deformation by extrusion the raw form is advantageously a billet, typically at least 70 mm in diameter. For hot deformation by rolling, the raw form is advantageously a rolling plate, typically at least 250 mm thick.

[0073] The raw form is homogenized and / or reheated typically to a temperature above the solvus temperature of the alloy, while avoiding local melting or burning for a period of at least 2 hours, preferably 3 hours, more preferably 4 hours and at most 7 hours, preferably 6 hours, more preferably 5 hours. The homogenization and / or reheating temperature is preferably at most 560°C, preferably 550°C, more preferably 540°C, more preferably 530°C, and at least 490°C, preferably 500°C. Too high or too low a temperature degrades the mechanical properties of the product.

[0074] The raw form is deformed hot and optionally cold by rolling or extrusion.

[0075] In one embodiment the raw form, in the form of a rolling plate, is hot rolled typically to a thickness of 3 to 8 mm. The hot rolling start temperature is typically 450°C to 550°C. Optionally the rolled product obtained after hot rolling is cold rolled to a thickness typically of 0.5 to 4 mm. In one embodiment the thickness is 0.7 to 3 mm. In one embodiment the thickness is 0.9 to 2 mm.

[0076] In one embodiment the raw form, in billet form, is hot extruded. The hot extrusion start temperature is typically 450°C to 550°C.

[0077] The raw form thus deformed is put into solution then quenched.

[0078] Solution treatment is typically carried out at a solution temperature above the solvus temperature of the alloy, while avoiding local melting or burning, and then quenched, preferably in a continuous furnace. Too cold a solution treatment and / or too short a solution treatment degrades the mechanical properties of the sheet by insufficient solution treatment. Too hot a solution treatment causes burns degrading the mechanical properties. Too long a solution treatment degrades productivity. Preferably, the solution treatment lasts from 15 seconds to 300 seconds. The solution treatment temperature is preferably a maximum of 560°C, preferably 550°C, more preferably 540°C, more preferably 530°C, and a minimum of 490°C, preferably 500°C.

[0079] Then the product thus put into solution is quenched typically at a speed of more than 30°C / s and better of at least 100°C / s with water or with air or with a successive combination of water or air. Preferably the product is quenched to a temperature of 60 to 100°C. An insufficient cooling speed degrades the mechanical properties of the sheet because the solution is then in- complete.

[0080] Optionally the product is then reheated to carry out pre-tempering typically at a pre-tempering temperature of 60°C to 120°C for a period of 1 to 24 hours, preferably 60°C to 100°C for 2 to 16 hours. In the case of rolled products the pre-tempering can be obtained by coiling then cooling to room temperature, preferably for at least 40 hours. Pre-tempering makes it possible to improve the response to baking of the paints which is the difference between the yield strength in the T4 state and the yield strength after baking of the paints.

[0081] The product obtained then matures at room temperature, preferably between 24 hours and 6 months, preferably between 72 hours and 5 months.

[0082] In one embodiment, the product thus obtained then undergoes tempering.

[0083] In another embodiment, the product thus obtained is painted and can undergo a heat treatment of baking the paint.

[0084] The product according to the invention is advantageously used for the manufacture of parts for motor vehicles. In one embodiment, the product according to the invention is used as a sheet metal for lining, such as for example door or hood linings. For certain automotive parts, in particular linings, the thicknesses are between 0.7 and 2.0 mm. A thickness of less than 0.7 mm is too thin to ensure the rigidity of the component containing the lining. A thickness greater than 2.0 mm makes the component containing the lining too heavy for the user and the vehicle. In one embodiment, the product according to the invention is used as a structural part, such as for example top hat stiffeners. In one embodiment, the product according to the invention is used as a battery tray element, in particular as a battery tray bottom.For battery tray bottoms, thicknesses are typically between 1.5 and 4.0 mm and preferably between 2 and 3 mm. Examples

[0085] The disclosure is further illustrated by the following examples. These examples are intended only to illustrate the invention and not to limit it.

[0086] Different alloys were tested in the laboratory according to the compositions in Table 1. They were cast by vertical semi-continuous casting (direct chill casting) in ingots 50 mm thick after scalping. Alloys J, K and L are examples of alloys of the 6XXX series used for sheets for applications in the automotive industry. The examples according to the invention, C and D, are identified "E" and the counter-examples by "CE" in Table 1. The compositions in Table 1 are in % by weight, the other elements are each <0.05%, together <0.15% the remainder is aluminum.

[0087] [Tables 1] Si Fe Cu Mn Mg Cr Ni ZN Ti Sn Pb A CE 4.99 0.49 1.43 0.22 1.01 0.02 0.05 0.7 0.05 0.02 0.04 B CE 5.04 0.50 1.40 0.23 0.36 0.02 0.05 0.69 0.05 0.02 0.04 EC 2.83 0.38 0.58 0.22 0.4 0.02 0.02 0.33 0.04 0.01 0.02 DE 4.09 0.43 0.97 0.22 0.38 0.02 0.03 0.52 0.04 0.02 0.04 E CE 4.96 0.77 1.44 0.23 0.38 0.02 0.05 0.69 0.05 0.02 0.04 F CE 4.93 0.51 2.02 0.23 0.38 0.02 0.05 0.69 0.05 0.02 0.04 G CE 5 0.51 0.62 0.23 0.35 0.02 0.05 0.69 0.05 0.02 0.04 H EC 5.05 0.51 1.39 0.22 0.38 0.02 0.05 0.97 0.05 0.02 0.04 I EC 2.59 0.5 0.8 0.59 1.37 0.04 0.05 0.4 0.08 0.01 0.02 J CE 0.71 0.15 0.13 0.13 0.66 0.03 0.03 0.1 0.03 0.01 0.01 K CE 4.49 0.22 0.09 0.17 0.33 0.11 0.03 0.11 0.15 0.01 0.01 L EC 0.61 0.16 0.51 0.12 0.58 0.01 0.01 0.06 0.01 0.01

[0088] The recyclability of these alloys was evaluated using a representative composition of the twitch according to Table 2.

[0089] [Tables2] Si Fe Cu Mn Mg Zn Ti 4.7 0.5 1.1 0.2 0.5 0.4 0.04

[0090] The recyclability of the different alloys A to L is evaluated by calculating the maximum quantity of the average composition calculated in Table 2 below for each element. A value greater than 100% means that the twitch does not provide the quantity of the element considered, therefore nothing limits the introduction of twitch to produce the alloy for the element considered. A value less than 100% implies that the twitch provides too much of the element considered and that the introduction of twitch must be limited to produce the alloy. It is therefore necessary to take into account only the minimum on all the elements for each alloy evaluated to define its recyclability. Alloys J, K and L are alloys with a lower recyclability of the twitch Si Fe Cu Mn Mg Zn Ti suitability for recycling A >100% 98% >100% >100% >100% >100% >100% 98% B >100% 100% >100% >100% 72% >100% >100% 72% C 60% 76% 53% >100% 80% 83% 100% 53% D 87% 86% 88% >100% 76% >100% 100% 76% E >100% >100% >100% >100% 76% >100% >100% 76% F >100% >100% >100% >100% 76% >100% >100% 76% G >100% >100% 56% >100% 70% >100% >100% 56% H >100% >100% >100% >100% 76% >100% >100% 76% I 55% 100% 73% >100% >100% 100% >100% 55% J 15% 30% 12% 65% >100% 25% 75% 12% K 96% 44% 8% 85% 66% 28% >100% 8% L 13% 32% 46% 60% >100% 3% >100% 3%

[0092] The ingots were reheated to 520°C except for references J and L, which were reheated to 560°C, then hot rolled while maintaining a temperature above 300°C.

[0093] The ingots were then cold rolled in 6 passes from the hot rolled thickness of 5 mm to the thickness of 1 mm except for references J and L which were cold rolled from the hot rolled thickness of 7 mm.

[0094] The cracking tendency during cold rolling was evaluated by measuring the crack length in the edges in the transverse direction, which will be called "crackability". The crack length was measured on the edges after cold rolling to 1 mm and the results are given in Table 4. crackability (mm) A 8 B 8 C 3 D 5 E 9 F 6 G 6 H 8 I 6 K 3

[0096] Samples were taken at a thickness of 3 mm. These samples were dissolved for 10 s at a temperature of 510°C (560°C for references J and L), then quenched in water and then pre-tempered for 8 hours at 80°C. These samples were then characterized at state 4 or after simulation of the baking of the paints for 20 minutes at 180°C (BH). The results are in Table 5.

[0097] The static mechanical characteristics in tension were measured in the cross direction of rolling.

[0098] The LDH was measured in the cross rolling direction.

[0099] The folding, alpha, was characterized with the folding axis parallel to the rolling direction.

[0100] Intergranular corrosion in an acidic environment was measured according to ISO 11846.

[0101] The results are presented in Table 5. Rp0.2 T4 (MPa) RmT4 (MPa) Ag% T4 Rp0.2 BH (MPa) Rm BH (MPa) Ag% BH (MPa) Folding T4 [°] LDH T4 [mm] Corrosion BH [pm] A 134 298 18.5 264 343 12 60 26.5 151 B 135 306 22.7 253 343 14.3 72 27.9 112 C 92 232 22.4 219 295 12.1 101 29.1 142 D 115 274 20.6 241 326 15 90 28.8 118 E 137 311 18.6 262 349 13.1 66 27.9 82 F 163 341 19.2 249 354 15.8 64 27.9 66 G 98 242 17.5 227 302 12.7 86 28 153 H 141 311 18.5 253 345 14.9 70 28.4 127 I 117 265 16.5 244 324 12.2 71 26.3 123 J 99 215 17.7 234 298 14.1 126 32.3 121 K 100 223 17.9 161 239 14.6 118 30.1 147 L 90 213 22.9 210 280 12.1 132 32 74

[0103] Figures 1 to 3 show that examples of the invention C and D in particular present the best compromise between the suitability for recycling, the suitability for transformation evaluated by cracks and the suitability for shaping (LDH) and the mechanical properties of elastic limit and elongation in the T4 state.

Claims

Claims

1. Aluminum alloy of composition, in wt%: Si: about 1.7% - about 7.0%, Fe: about 0.2% - about 0.8%,, Cu: about 0.3% - about 1.0%, Mn: about 0.2% - about 0.6%, Mg: about 0.2% - about 0.6%, Zn: about 0.2% - about 0.6%, Ti, Cr, Sn, Pb, Zr, V, Sr, Ni: < about 0.1%, other elements: each <0.05%, together <0.15%, remainder: Al.

2. An alloy according to claim 1 comprising at least 20% post-consumer waste, preferably from end-of-life vehicles, more preferably from aluminum fragmented by automotive shredders.

3. Alloy according to one of the preceding claims of composition, in % by weight: Si: 1.7%-7.0%, Fe: 0.2% - 0.8%, Cu: 0.3% - 1.0%, Mn: 0.2% -0.35%, Mg: 0.2% -0.6%, Zn: 0.2% -0.6%, Ti, Sn, Pb, Zr, V, Sr, : < 0.1%, Cr < 0.08%, Ni < 0.08% other elements: each <0.05%, together < 0.15%, remainder: Al.

4. Alloy according to claim 1 or claim 2 of composition, in % by weight: Si: 1.7%-7.0%, Fe: 0.2% - 0.8%, Cu: 0.40% - 1.0%, Mn: 0.2% -0.6%, Mg: 0.2% -0.6%, Zn: 0.2% -0.6%, Ti, Sn, Pb, Zr, V, Sr: <0.1%, Cr < 0.08%, Ni < 0.08%, other elements: each <0.05%, together < 0.15%, remainder: Al.

5. Alloy according to one of the preceding claims characterized in that Si > 2.0%, preferably Si > 2.2%, more preferably Si > 2.5%, more preferably Si >2.8% and / or Si < 6%, preferably Si < 5%, more preferably Si < 4.3%, more preferably Si <4.1%.

6. Alloy according to one of the preceding claims characterized in that Fe > 0.25%, preferably Fe > 0.30%, more preferably Fe > 0.33%, more preferably Fe > 0.35%, more preferably Fe > 0.37% and / or Fe < 0.75%, preferably Fe < 0.65%, more preferably Fe < 0.55%, more preferably Fe < 0.50%, more preferably Fe < 0.45%

7. / V. Alloy according to one of the preceding claims characterized in that Cu > 0.43%, preferably Cu >0.45%, more preferably Cu > 0.48%, more preferably Cu >0.50%, more preferably Cu >0.35% and / or Cu < 0.98%, preferably Cu <0.97%, more preferably Cu < 0.95%, more preferably Cu <0.92%, more preferably Cu <0.90%.

8. Alloy according to one of the preceding claims characterized in that Mg > 0.22%, preferably Mg > 0.25%, more preferably Mg > 0.27%, more preferably Mg > 0.32%, more preferably Mg > 0.35% and / or Mg < 0.55%, preferably Mg < 0.52%, more preferably Mg < 0.50%, more preferably Mg < 0.47%, more preferably Mg < 0.45%.

9. Rolled or extruded alloy product according to one of claims 1 to 0

10. O. Rolled product according to claim 9 in the solution treated, quenched and pre-tempered state or in the solution treated, quenched and tempered state.

11. Rolled product according to claim 9 or claim 10 characterized in that the crackability is less than or equal to 5mm, preferably less than or equal to 4mm, more preferably less than or equal to 3mm.

12. A method of manufacturing a product according to claim 9 comprising the successive steps: a) Supply of aluminum alloys and addition metals, the aluminum alloys being at least 20% in the form of waste post-consumer, b) Optional sorting of post-consumer waste, c) Production of an alloy according to any one of claims 1 to 8, from aluminum alloys comprising optionally sorted post-consumer waste and supplied addition metals d) Casting of the alloy in a raw form, preferably by semi-continuous vertical casting, e) Homogenization and / or reheating of the raw form, f) Hot and optionally cold deformation by rolling or extrusion of the raw form, g) Solution treatment then quenching of the raw form thus deformed, h) Optionally pre-tempered typically at a pre-tempering temperature of 60 to 120°C for a period of 1 to 24 hours, i) Maturation preferably from 24 hours to 6 months.

13. Use of a product according to any one of claims 9 to 11 for the manufacture of parts for motor vehicles.

Citation Information

Patent Citations

  • Aluminum alloy plate to be formed, and manufacturing method therefor

    JP2005298922A

  • Aluminum-alloy sheet

    US20210108293A1

  • Aluminum plate for automobile and method for producing the same

    WO1999060181A1

  • Casting recycled aluminum scrap