Structure comprising an ultrathin ionic dielectric layer and its manufacturing process
The ionic dielectric layer with a dopant gradient in two parts enhances conductivity and supports electrode growth, addressing low conductivity and interaction issues in nano-ionic transistors, ensuring efficient performance in micro- and nano-electronic structures.
Patent Information
- Application Number
- FR2023004384
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-02
- Publication Date
- 2024-11-08
AI Technical Summary
Existing micro- and nano-electronic structures face challenges with low ionic conductivity in electrolytes, leading to weakened synaptic performance in nano-ionic transistors and potential electrode growth inhibition due to element interaction and migration, which impacts electronic insulation properties.
A structure with an ionic dielectric layer comprising two parts: a first part with a matrix-based ionic conductor and a second part rich in dopant, creating a dopant gradient to enhance ionic conductivity and facilitate electrode growth while maintaining insulation properties, using a deposition process that maintains vacuum to prevent undesirable oxide formation.
The structure achieves improved ionic conductivity up to 10^6 S/cm and supports homogeneous electrode growth without altering electrical operation, suitable for MIM microstructures and nanostructures.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Structure comprising an ultrathin ionic dielectric layer and its manufacturing method Technical field
[0001] The invention relates to the field of micro- and nano-structures for micro- and nano-electronic devices.
[0002] More specifically, the invention relates to a structure comprising a stack of an ultrathin ionic dielectric layer - used as an electrolyte - nested between two electrodes as well as to its manufacturing method.
[0003] The invention also relates to an ionic dielectric layer.
[0004] The invention finds particular application in the manufacture of high-density capacitances, for example of the MIM (for Metal-Insulator-Metal) type or the manufacture of synaptic transistors for energy storage devices. State of the prior art
[0005] The advent of connected and intelligent objects is currently the subject of research, particularly research into highly advanced and increasingly complex micro- and nano-electronic devices.
[0006] In addition to developments related to the architecture and design of micro- and nano-electronic components enabling them to meet very advanced technological and performance criteria, the development of new materials plays a key role in this research.
[0007] In this wake, the miniaturization of energy storage devices has been made possible by the development of three-dimensional architectures, making it possible to increase their energy volume density, in particular by increasing their specific surface area. Thus, the development of new dielectric layers with very advanced ionic properties opens a new horizon for the use of capacitances, such as MIM-type capacitances - i.e. a dielectric layer nested between two electrodes.
[0008] Furthermore, nano-ionic transistors using lithium-based electrolytes are considered as promising synaptic devices for the construction of artificial neural networks for neuromorphic computing. However, the synaptic performance of these transistors is weakened in particular due to the low ionic conductivity exhibited by the electrolytes used in these transistors.
[0009] The objective of optimizing the performance of micro- and nanoelectronic structures therefore results in the introduction, into these structures, of new ionic dielectric layers that are extremely thin, very conformable and have a improved ionic conductivity.
[0010] Generally, such layers are deposited by atomic layer deposition (or ALD for "Atomic Layer Deposition" in English), allowing successive depositions of extremely thin and conformable layers, i.e. perfectly matching the surface of the substrate which is intended to support a stack of these layers. For example, in application EP 3570307-A1, a MOIM type structure - i.e. a substrate covered by a stack comprising a first electrode, an oxide layer, an ionic dielectric layer and a second electrode - has been proposed, the ionic dielectric layer possibly being made of LiPON, LiAlF4, LiNbO3 and the electrodes possibly being made of a metal such as titanium, tantalum or cobalt or of a metal nitride such as titanium nitride. The layers are deposited by ALD.
[0011] US patent 10,032,569-B2, for its part, proposes the manufacture of a MIM type capacitance in so-called AAO (for "Anodic Aluminum Oxide") structures. In this patent, the nature of the ionic dielectric layer can be chosen from a wide list of materials, including for example LiPON, LiA102 and A12O3 while the electrodes can be made of a metal and / or metal nitride such as aluminum, copper, tungsten, tungsten nitride and titanium nitride.
[0012] However, during the growth of a metal electrode on an ionic dielectric layer, the ionic elements of this layer are likely to interact with elements of the electrode, thus delaying or even inhibiting the growth of this electrode.
[0013] Furthermore, electrodes made of a nitrided metal are generally obtained from reactive species comprising a halogen and more particularly chlorine or iodine. However, these halogens are highly likely to migrate into the underlying ionic dielectric layer, thus impacting the electronic insulation properties of the latter.
[0014] In view of the above, the inventors set themselves the goal of overcoming the drawbacks of the prior art, in particular by proposing a structure comprising an ionic dielectric layer nested between two electrodes, the ionic dielectric layer also having greater ionic conductivity and allowing the growth of an electrode on its surface, while retaining its electronic insulation properties. Statement of the invention
[0015] The invention aims precisely to provide such a structure.
[0016] The subject of the invention is therefore, firstly, a structure which comprises a substrate successively covered by a first electrode, an ionic dielectric layer and a second electrode, characterized in that the dielectric layer ionic includes: - a first part, in contact with the first electrode, comprising a matrix based on an ionic conductor in which a dopant is incorporated; - a second part, in contact with the second electrode, comprising an oxide of the dopant or comprising the matrix based on the ionic conductor in which the dopant is incorporated; the atomic dopant content of the second part of the ionic dielectric layer being greater than the atomic dopant content of the first part of the ionic dielectric layer.
[0017] The invention is fundamentally distinguished from the prior art by the use of an ionic dielectric layer having two parts.
[0018] The second part of the ionic dielectric layer not only makes it possible to improve the overall ionic conductivity but also to have a surface promoting the growth of the upper electrode layer (i.e. the second electrode) without altering the electrical functioning of such a structure.
[0019] Such an ionic dielectric layer is efficient and easily integrated into the construction and manufacturing of MIM microstructures and nanostructures.
[0020] It should be noted that the matrix of the ionic dielectric layer may comprise one or more dopants and that this ionic dielectric layer may comprise one or more first parts and one or more second parts, in the form of an alternation of first parts and second parts, a second part being in contact with the second electrode.
[0021] By dopant is meant any compound which can be incorporated into the matrix of the ionic dielectric layer allowing an increase in the ionic conductivity of this layer.
[0022] The dopant is advantageously present in the matrix of the ionic dielectric layer according to a gradient, that is to say that the second part of this ionic dielectric layer is rich in dopant compared to the first part of this same layer which, itself, is rich in ionic conductor. In other words, the atomic content of dopant is increasing in the ionic dielectric layer from the first electrode towards the second electrode, or even up to the second electrode.
[0023] This gradient makes it possible to modify the surface of the ionic dielectric layer intended to be in contact with the second electrode. This modification makes it possible to make this surface easily functionalizable and, consequently, makes it possible to promote the growth of the second electrode.
[0024] In the foregoing and the following, "growth" means that the second electrode can be deposited and grown on the surface of an underlying ionic dielectric layer, so as to have a desired homogeneous thickness over this entire surface. The second electrode is continuous.
[0025] Furthermore, the second part of the ionic dielectric layer, rich in dopant and in contact with the second electrode, also has a “barrier” role, that is to say that it prevents or, at the very least, minimizes the possible diffusion or migration of chemical elements from the second electrode to the ionic dielectric layer, these elements not being desirable in the ionic dielectric layer in particular because they are likely to impact the electronic insulation properties of this layer. Such elements can be chlorine or iodine for example.
[0026] As indicated previously, according to a first embodiment, the second part of the ionic dielectric layer is made of an oxide of the dopant. For example, if the dopant is silicon, the second part of the ionic dielectric layer is made of silicon oxide.
[0027] According to a second embodiment variant, the second part of the ionic dielectric layer comprises the matrix based on the ionic conductor in which the dopant is incorporated. According to this embodiment variant, it is preferred that the second part of the ionic dielectric layer has an atomic dopant content ranging from 50% to 97%, preferably ranging from 90% to 97%, while the first part advantageously has an atomic dopant content ranging from 3% to 50%, preferably ranging from 3% to 10%.
[0028] In the above and the following, it is specified that the atomic content of dopant corresponds, in percentage, to the ratio of the number of atoms of this dopant present in the matrix of the ionic dielectric layer to the total number of atoms of the dopant added to the number of atoms of the ionic conductor. For example, for a LiPON type ionic dielectric layer doped with silicon, the atomic content of dopant, in percentage, is defined by the following ratio R: R = 100 x (d / (Li +d)) with d the number of dopant atoms, here silicon, Li the number of atoms of the ionic conductor, here lithium.
[0029] Furthermore, in the above and the following, the expressions "from ... to ..." and "between ... and ..." are equivalent and are intended to mean that the limits are included.
[0030] In the context of the invention, the ionic dielectric layer is an ultra-thin layer and advantageously has a total thickness of between 3 nm and 100 nm, preferably between 5 nm and 20 nm and, better still, equal to 10 nm.
[0031] Furthermore, it is preferred that the second part of the ionic dielectric layer represents from 5% to 20% of the total thickness of the ionic dielectric layer and, even better, from 5% to 10%.
[0032] According to the invention, the dopant of the ionic dielectric layer can be chosen from silicon, aluminum, titanium, tantalum, zirconium and lanthanum, preference being given to silicon.
[0033] Furthermore, in the foregoing and the following, the term "ionic conductor" means any element capable of providing cations with a sufficient degree of ionic mobility to give the ionic dielectric layer, initially, an ionic conductivity at least equal to 10 7 S / cm, such cations may be cations of lithium, magnesium, sodium, potassium, copper, silver, aluminum or even zinc.
[0034] For example, when the ionic conductor is chosen so as to provide lithium cations, the ionic dielectric layer may be made of a solid electrolyte based on sulfur compounds (such as the so-called LGPS or LPS compounds), of an oxide with a garnet-type structure (such as a lithium-lanthanum-zirconium oxide or so-called LLZO), of an ionic conductor of the NaSiCON type or of an oxynitride comprising lithium (such as LiPO, LiPON, LiA102 or LATP).
[0035] Another example may be when the ionic conductor is chosen to provide magnesium cations. In this case the ionic dielectric layer may be made of a magnesium phosphate.
[0036] According to the invention, the ionic dielectric layer is advantageously made of a material chosen from lithium phosphorus oxynitride (more simply noted LiPON), lithium metasilicate and magnesium phosphate, preference being however given to lithium phosphorus oxynitride.
[0037] Thus, by combining the ionic conductor and the dopant, the ionic dielectric layer of the structure according to the invention advantageously has an ionic conductivity at least equal to 106 S.cm1 and, better still, at least equal to 105 S.cm '.
[0038] As previously mentioned, the structure according to the invention comprises a substrate successively covered by a first electrode, an ionic dielectric layer and a second electrode.
[0039] Typically, the first and second electrodes are made of a material having low electrical resistivity, for example less than 200 pQ cm. The first electrode and the second electrode, identical or different, are preferably made of a metal such as titanium, platinum, tungsten, ruthenium, or molybdenum or of a metal nitride such as titanium nitride, tantalum nitride, tungsten nitride or molybdenum nitride, preference being given, however, to titanium nitride (denoted TiN).
[0040] The first electrode and the second electrode generally have a thickness of less than 20 nm, for example equal to 10 nm.
[0041] Furthermore, the substrate of the structure according to the invention may have a flat surface - i.e. in two dimensions - or a micro-structured surface - i.e. in three dimensions.
[0042] In the foregoing and the following, the term “microstructured surface” means a surface comprising pores or vias, for example of elongated shape, which makes it possible in particular to increase the specific surface area of the substrate - that is to say the surface area of the substrate intended to be covered successively by the first electrode, the ionic dielectric layer and the second electrode - compared to a flat surface.
[0043] Thus, a microstructured surface may have a more or less significant aspect ratio, this aspect ratio corresponding to the ratio of the longitudinal dimension to the transverse dimension of the pores or vias. Also, the higher the aspect ratio, the greater the specific surface area of the substrate. For example, an aspect ratio greater than 20 may be considered.
[0044] The substrate may also comprise microelectronic components.
[0045] The substrate may be made of silicon, metal nitride or a material based of metal oxide such as alumina, or any other suitable material.
[0046] The structure as previously described can in particular be prepared by a process which comprises at least the following successive steps: a) deposition of the first electrode on the substrate; then b) deposition of the ionic dielectric layer; then c) deposition of the second electrode; the method being characterized in that step b) is carried out by ALD according to the following sub-steps: i) formation of the first part of the ionic dielectric layer by repeating several times, for example between 40 and 180 times, the first cycle of sub-steps ii) and i2) following: ii) introduction and alternating circulation of precursors of the ionic conductor on the first electrode; then i2) introduction and alternating circulation of dopant precursors on the first electrode; ii) formation of the second part of the ionic dielectric layer by repeating several times, for example between 5 and 30 times, a sub-step consisting of introducing and circulating, alternately, precursors of the dopant oxide on the first electrode, or formation of the second part of the ionic dielectric layer by repeating several times, for example between 5 and 30 times, the following second cycle of sub-steps iil) and ii2): (ii) introduction and alternating circulation of the precursors of the ionic conductor on the first electrode; then ii2) introduction and alternating circulation of dopant precursors on the first electrode.
[0047] Steps a), b) and c) are carried out using the vacuum ALD deposition technique (from a few mTorr to a few Torr; i.e. between approximately 0.1 Pa and a few hundred Pa, for example 300 Pa), which in particular makes it possible to obtain very conformable layers of very high purity and very low thickness.
[0048] The sequence of steps a), b) and c) is carried out without breaking the vacuum, which makes it possible to avoid any formation of oxide layers between the first electrode and the ionic dielectric layer and / or between the ionic dielectric layer and the second electrode, these oxide layers not being desirable in such a structure because they could impair its proper electrical operation.
[0049] The principle of ALD deposition lies in introducing at least two reactive species, called “precursors”, into an ALD chamber, then circulating them alternately on the surface of a material.
[0050] The ALD deposition of step b) can be carried out at a temperature between 200°C and 420°C, for example at 330°C. It makes it possible in particular to control the distribution of the dopant during its incorporation into the matrix of the ionic dielectric layer, so as to obtain a gradient.
[0051] To do this, sub-step ii) is preferably repeated at least 10 times before carrying out sub-step i2). If sub-steps ii11) and ii2) are carried out, then ii2) is preferably repeated at least 10 times when implementing the second cycle.
[0052] In fact, the number of repetitions of the first cycle and / or the second cycle is directly related to the desired thickness of the first part of the ionic dielectric layer and / or the second part of the ionic dielectric layer.
[0053] For example, to obtain the first part of the ionic dielectric layer with a thickness of 9 nm, the first cycle of sub-step i) is typically repeated between 80 and 90 times, for example 88 times, and to obtain a thickness of 1 nm for the second part of this same layer, the second cycle of sub-step ii) can be repeated between 10 and 15 times, for example 12 times.
[0054] As a variant, for example, it is possible to repeat sub-steps i) and ii) of step b) cyclically to form an alternation of first parts and second parts in the ionic dielectric layer, a second part being in contact with the second electrode. For example, it is possible to carry out step b) so as to obtain a first part of the ionic dielectric layer with a thickness of 2 nm and a second part of this same layer with a thickness of 0.5 nm, then repeat the steps until an ionic dielectric layer is obtained, preferably with a thickness of 10 nm and comprising an alternation of first and second parts, it being understood that one of the second parts must be in contact with the second electrode.
[0055] Furthermore, the introduction of each of these precursors is followed by a time, called a waiting time, before purging them.
[0056] The waiting time represents the residence time of the precursors on the surface of the substrate or, where appropriate, on the surface of the underlying layer or electrode. It is directly proportional to the value of the aspect ratio of the substrate. The waiting time allows the precursors to diffuse and react optimally, particularly in complex structures comprising, for example, a micro-structured surface with a high aspect ratio.
[0057] Typically, during sub-steps ii), i2), iil) and ii2), after the introduction and circulation of each precursor of the ionic conductor and / or after the introduction and circulation of each precursor of the dopant, a waiting time of between 15 seconds and 100 seconds, preferably between 20 seconds and 50 seconds and, better still, equal to 30 seconds, is observed before carrying out a purge. The purge can be carried out for a duration at least equal to 40 seconds, to eliminate excess precursors and any unwanted by-products obtained during a reaction between the precursors.
[0058] Furthermore, in accordance with the invention, the precursors of the ionic conductor are chosen from one of the following pairs of precursors: lithium hexamethyldisilazane (denoted LiHMDS) coupled with diethyl phosphoramidate (denoted DEPA), lithium tert-butoxide (denoted LiOtBu) coupled with diethyl phosphoramidate and lithium tert-butoxide coupled with trimethyl phosphite (denoted TMPO) and / or the precursors of the dopant or the precursors of the dopant oxide are chosen from one of the following pairs of precursors: tris(dimethylamino)silane (denoted 3DMAS) coupled with ozone (denoted O3) or water, bis(dimethylamino)dimethylsilane (denoted BDEAS) coupled with ozone or water.
[0059] In fact, the precursors of the ionic conductor and of the dopant or, where appropriate, of the dopant oxide, are chosen according to the desired nature of the ionic dielectric layer and of the dopant. The pairs of precursors mentioned above make it possible, for example, to obtain the first part of the ionic dielectric layer in silicon-doped lithium phosphorus oxynitride (more simply noted LiSiPON) and the second part of this same layer in silicon oxide (SiO2).
[0060] Alternatively, trimethylaluminium (denoted TMA) can be used as a precursor of the dopant coupled with deionized water making it possible to obtain the second part of the ionic dielectric layer in an aluminium oxide and, more particularly here in alumina.
[0061] Another alternative can be implemented by using LiOtBu coupled with tetraethyl orthosilicate (denoted TEOS) as precursors, in which case the ionic dielectric layer is made of lithium metasilicate.
[0062] Another alternative may still be when the ionic conductor is chosen so as to provide magnesium cations. In this case, by using as precursors bis(methylcyclopentadienyl)magnesium (denoted Mg(EtCp)2) coupled with tris(dimethylamino)phosphine (denoted TDMAP), water and oxygen, an ionic dielectric layer of the magnesium phosphate type can be obtained.
[0063] By thus implementing step b) of the method of the invention, the ionic dielectric layer is obtained, from a macroscopic point of view, in a single step and comprises, from a microscopic point of view, two distinct parts, the second part of which - in contact with the second electrode - is rich in dopant, unlike the first part which is rich in ionic conductor.
[0064] Preferably, the sub-steps of step b) are carried out at the same temperature.
[0065] On the other hand, steps a) and c) of the method are typically implemented by ALD deposition and, preferably, at a temperature between 200°C and 450°C, for example equal to 400°C, while respecting the same waiting and purging time as those set in step b).
[0066] In addition, steps a) and c) are preferably carried out by depositing by ALD a metal halide and / or an organometallic, the metal halide preferably comprising chlorine, iodine or bromine.
[0067] During steps a) and c) the metal halide and / or the organometallic compound are generally coupled with ammonia.
[0068] In the context of the invention, the halide is generally preferred to the organometallic compound, in particular because it has high thermal stability, high saturated vapor pressure and high reactivity.
[0069] More particularly, the metal halide may be chosen from titanium tetrachloride, titanium iodide and titanium tetrabromide, preference being given, however, to titanium tetrachloride (TiClj.
[0070] In fact, the halide and / or the organometallic are chosen according to the desired nature of the first and second electrodes. For example, by implementing steps a) and c) with titanium tetrachloride coupled with ammonia, then a titanium nitride electrode is obtained.
[0071] It should be noted that the second electrode may comprise a single layer or a multitude of layers, the nature and deposition technique of which may differ from the first electrode.
[0072] Alternatively to deposition by ALD, steps a), b) and c) can also be implemented by a plasma-assisted ALD process (also called PEALD for “Plasma Enhanced Atomic Load Deposition” by a spatial ALD process (also called SALD for “Spatial Atomic Load Deposition”) or by an atmospheric pressure ALD process.
[0073] Other alternatives can be implemented, in particular for steps a) and c), such as deposition techniques adapted to thin layers, such as physical vapor deposition (or PVD for “Physical Vapor Deposition”) or even chemical vapor deposition (or CVD for “Chemical Vapor Deposition”).
[0074] A person skilled in the art knows perfectly well how to choose the most suitable deposition process, in particular depending on the surface of the substrate used (flat or microstructured).
[0075] The invention also relates to an ionic dielectric layer comprising: - a first part comprising a matrix based on an ionic conductor in which a dopant is incorporated; - a second part comprising an oxide of the dopant or comprising the matrix based on the ionic conductor in which the dopant is incorporated; the atomic dopant content of the second part of the ionic dielectric layer being greater than the atomic dopant content of the first part of the ionic dielectric layer.
[0076] Other characteristics and advantages of the invention will emerge from the additional description which follows.
[0077] It goes without saying that this additional description is given only as an illustration of the subject of the invention and must in no case be interpreted as a limitation of this subject. Brief description of the figures
[0078] [Fig-1] represents a substrate 1 having a flat surface covered by a first electrode 2, a dielectric layer 3 comprising a first part 31 and a second part 32 and a second electrode 4 according to a first particular embodiment of the invention.
[0079] [Fig.2] represents a substrate 1 having a microstructured surface covered by a first electrode 2 according to another particular embodiment of the invention.
[0080] [Fig.3] represents the steps of a synthesis of deposition of an ionic dielectric layer comprising a first part and a second part, according to a particular embodiment of the invention.
[0081] [Fig.4] represents a structure comprising the substrate 1 whose surface is covered by a stack comprising the first electrode 2 and an ionic dielectric layer 3, according to another particular embodiment (for reasons of readability, the detail of the ionic dielectric layer is not shown in this figure).
[0082] [Fig.5] is an enlargement of a part of [Fig.4]; it represents a structure comprising the substrate 1 whose surface is covered by a stack comprising the first electrode 2, the ionic dielectric layer 3 comprising a first part 31 and a second part 32.
[0083] [Fig.6] represents a MIM type SI structure comprising the substrate 1 whose surface is covered by a stack comprising the first electrode 2, the ionic dielectric layer 3 and a second electrode 4, according to another particular embodiment (for reasons of readability, the detail of the ionic dielectric layer is not shown in this figure).
[0084] [Fig.7] represents the steps of a synthesis of deposition of an ionic dielectric layer comprising a first part and a second part, according to another particular embodiment of the invention.
[0085] It should be noted that the figures described above are schematic representations whose relative dimensions and proportions of the substrate 1, the first electrode 2, the ionic dielectric layer 3 and the second electrode 4 are not representative of those likely to be presented in a real situation, for reasons of readability.
[0086] Detailed description of particular embodiments
[0087] In the various examples which follow, the substrate is a micro-structured substrate. However, as shown in [Fig.l], the method for manufacturing the MIM structure could be applied to a substrate 1 having a flat surface. The various elements (first electrode 2, ionic dielectric layer 3 comprising a first part 31 and a second part 32, second electrode 4) are then deposited successively on the substrate 1.
[0088] Example 1: manufacturing of a first SI structure 1.1- Deposition of the first electrode:
[0089] A substrate 1 is placed in a vacuum ALD chamber dedicated to electrode deposition.
[0090] The substrate 1 is made of silicon with electrical insulation made of silicon oxide. It has a micro-structured surface so as to give it an aspect ratio greater than 20 ([Fig.2]).
[0091] ALD deposition is carried out at a temperature of 400°C by carrying out the following cycle of steps: - injection of TiCl4 for an injection time equal to 2 seconds; - circulation of TiCl4 on the surface of substrate 1, respecting a waiting time equal to 30 s; - purge for 40 seconds of excess TiCl4; then - injection of ammonia (NH3); - circulation of NH3 on the surface of substrate 1; - purge of excess NH3 as well as any by-products obtained during a reaction between TiCl4 and NH3.
[0092] The injection time, waiting time and purging time of NH3 are the same as those applied for TiCl4
[0093] The above cycle is repeated 200 times.
[0094] Thus, the first electrode 2 made of TiN, with a thickness of 10 nm, is deposited homogeneously over the entire specific surface of the substrate 1, as illustrated in [Fig.2], 1.2- Deposition of the ionic dielectric layer:
[0095] The assembly formed by the substrate 1 and the first electrode 2 in TiN, obtained at point 1.1 above, is moved to a second vacuum ALD chamber, this time dedicated to the deposition of ionic dielectric layers.
[0096] The movement is carried out without passage to air - that is to say that the assembly remains under vacuum - to avoid any formation of an additional oxide layer on the surface of the TiN electrode 2.
[0097] A deposit by ALD is carried out at 330°C according to the steps as illustrated in [Fig.3], and which correspond to: i) the formation of the first part 31 of the ionic dielectric layer 3 by repeating 88 times the cycle of the following sub-steps 11) and 12): ii) introduction and alternating circulation of LiHMDS and DEPA on the surface of the first TiN electrode 2; this sub-step is repeated 10 times; i2) introduction and alternating circulation of 3DMAS and O3 on the surface of the first TiN electrode 2; ii) the formation of the second part 32 of the ionic dielectric layer 3 by repeating 12 times an introduction and an alternating circulation of 3DMAS and O3 on the surface of the first TiN electrode 2.
[0098] After each introduction and circulation of the LiHMDS, DEPA, 3DMAS and O3 compounds, a purge of each of these compounds is implemented.
[0099] The injection time, the waiting time and the purge time are the same for each of these compounds and are respectively 2 s, 30 s and 40 s.
[0100] Thus, the ionic dielectric layer 3 in LiSiPON is deposited homogeneously on the surface of the first electrode 2 in TiN, as illustrated in [Fig.4],
[0101] The LiSiPON layer 3 thus obtained has an ionic conductivity of the order of 105 S / cm, a total thickness of 10 nm and comprises, as illustrated in [Fig.5] - a first part 31 made of LiSiPON having a thickness of 9 nm and comprising an atomic content of silicon equal to 10% relative to the total number of lithium atoms; and - a second part 32 in SiO2 having a thickness of 1 nm and characterized by a very high silicon content. 1.3- Deposition of the second electrode:
[0102] The assembly formed by the substrate 1, the first electrode 2 in TiN and the ionic dielectric layer 3 in LiSiPON obtained in point 1.2 above, is moved to a third vacuum ALD chamber, dedicated to electrode depositions.
[0103] The movement from the second to the third ALD chamber is also carried out without passage to air, to avoid any formation of oxide layers on the surface of the ionic dielectric layer 3 in LiSiPON.
[0104] A second TiN electrode 4 is deposited homogeneously on the surface of the ionic dielectric layer 3 in LiSiPON, obtained in point 1.2 above, by implementing the same cycle of steps as that described in point 1.1.
[0105] The second TiN electrode 4 thus deposited has a thickness of 10 nm.
[0106] A MIM type SI structure is then obtained and is represented in [Fig.6]. Example 2: manufacturing a second structure
[0107] In this example, the substrate used is made of silicon with silicon oxide electrical insulation and has a micro-structured surface similar to the surface of substrate 1 used in the previous example.
[0108] Furthermore, in this example the deposition of the first electrode 2 and the deposition of the second electrode 4 are carried out in the same way as in example 1.
[0109] Only the step of depositing the ionic dielectric layer is different.
[0110] Here too, a deposit by ALD, at a temperature of 330°C, is carried out but this time by carrying out the steps shown in [Fig.7], which correspond to: i) the formation of the first part of the ionic dielectric layer by repeating 88 times the cycle of sub-steps 11) and 12) as follows: ii) introduction and alternating circulation of LiHMDS and DEPA on the surface of the first TiN electrode 2; this sub-step is repeated 10 times; i2) introduction and alternating circulation of 3DMAS and O3 on the surface of the first TiN electrode 2; and ii) the formation of the second part of the ionic dielectric layer by repeating 12 times the cycle of sub-steps iil) and ii2) as follows: (iil) introduction and alternating circulation of LiHMDS and DEPA on the surface of the first TiN electrode 2; i2) introduction and alternating circulation of 3DMAS and O3 on the surface of the first TiN electrode 2; this sub-step is repeated 10 times.
[0111] Again, after each introduction and circulation of the LiHMDS, DEPA, 3DMAS and O3 compounds, a purge of each of these compounds is implemented.
[0112] The injection time, waiting time and purge time are the same for each of these compounds and are respectively 2 s, 30 s and 40 s.
[0113] The ionic dielectric layer of LiSiPON thus deposited on the surface of the first TiN electrode 2, has an ionic conductivity of the order of 106 S / cm, a total thickness of 10 nm and comprises: - a first part made of LiSiPON having a thickness of 9 nm and comprising an atomic content of silicon equal to 10% relative to the total number of lithium atoms; and - a second part also in LiSiPON having a thickness of 1 nm and comprising an atomic content of silicon equal to 90% compared to the total number of lithium atoms.
Claims
Claims
1. Structure comprising a substrate (1) successively covered by a first electrode (2), an ionic dielectric layer (3) and a second electrode (4), characterized in that the ionic dielectric layer comprises: - a first part (31), in contact with the first electrode (2), comprising a matrix based on an ionic conductor in which a dopant is incorporated; - a second part (32), in contact with the second electrode (4), comprising an oxide of the dopant or comprising the matrix based on the ionic conductor in which the dopant is incorporated; the atomic content of dopant in the second part (32) of the ionic dielectric layer (3) being greater than the atomic content of dopant in the first part (31) of the ionic dielectric layer (3).
2. Structure according to claim 1, wherein the second part (32) of the ionic dielectric layer (3) has an atomic dopant content ranging from 50% to 97%, preferably from 90% to 97% and wherein the first part (31) has an atomic dopant content ranging from 3% to 50%, preferably from 3% to 10%.
3. Structure according to claim 1 or claim 2, wherein the ionic dielectric layer (3) has a total thickness of between 3 nm and 100 nm, preferably between 5 nm and 20 nm and, more preferably, equal to 10 nm.
4. The structure of claim 3, wherein the second portion (32) of the ionic dielectric layer (3) represents from 5% to 20% of the total thickness of the ionic dielectric layer (3) and, more preferably, from 5% to 10%.
5. Structure according to any one of claims 1 to 4, in which the dopant of the ionic dielectric layer (3) is chosen from silicon, aluminum, titanium, tantalum, zirconium and lanthanum, preference being given to silicon.
6. Structure according to any one of claims 1 to 5, in which the matrix of the ionic dielectric layer (3) is made of a material chosen from lithium phosphorus oxynitride, lithium metasilicate and magnesium phosphate, preference being given to lithium phosphorus oxynitride.
7. A structure according to any one of claims 1 to 6, wherein the ionic dielectric layer (3) has an ionic conductivity at least equal to 106 S.cm, preferably at least equal to 105 Sxm1.
8. Structure according to any one of claims 1 to 7, in which the first electrode (2) and the second electrode (4), identical or different, are made of a metal such as titanium, platinum, tungsten, ruthenium, or molybdenum or of a metal nitride such as titanium nitride, tantalum nitride, tungsten nitride or molybdenum nitride, preference being given to titanium nitride.
9. Structure according to any one of claims 1 to 8, in which the substrate (1) has a flat or microstructured surface.
10. A method of manufacturing a structure as defined according to any one of claims 1 to 9, comprising at least the following successive steps: a) deposition of the first electrode (2) on the substrate (1); then b) deposition of the ionic dielectric layer (3); then c) deposition of the second electrode (4); the method being characterized in that step b) is carried out by ALD according to the following sub-steps: i) formation of the first part (31) of the ionic dielectric layer (3) by repeating several times, for example between 40 and 180 times, the following first cycle of sub-steps ii) and i2): ii) introduction and alternating circulation of precursors of the ionic conductor on the first electrode (2); then i2) introduction and alternating circulation of precursors of the dopant on the first electrode (2);ii) forming the second part (32) of the ionic dielectric layer (3) by repeating several times, for example between 5 and 30 times, a sub-step consisting of introducing and circulating in an alternating manner precursors of the dopant oxide on the first electrode (2), or forming the second part (32) of the ionic dielectric layer (3) by repeating several times, for example between 5 and 30 times, the following second cycle of sub-steps iil) and ii2): iil) introducing and alternating circulation of the precursors of the ionic conductor on the first electrode (2); then ii2) introducing and alternating circulation of the precursors of the dopant on the first electrode (2).;
11. A method according to claim 10, wherein substep i1) is repeated at least 10 times before performing substep i2) and in which, if sub-steps iil) and Ü2) are carried out, then ii2) is repeated at least 10 times when implementing the second cycle.
12. Method according to claim 10 or claim 11, wherein during sub-steps ii), i2), iil) and ii2), after the introduction and circulation of each precursor of the ionic conductor or after the introduction and circulation of each precursor of the dopant, a waiting time of a duration of between 15 seconds and 100 seconds, preferably between 20 seconds and 50 seconds and, better still, equal to 30 seconds, is observed before carrying out a purge.
13. A method according to any one of claims 10 to 12, wherein the precursors of the ionic conductor are chosen from one of the following pairs of precursors: lithium hexamethyldisilazane coupled with diethyl phosphoramidate, lithium tert-butoxide coupled with diethyl phosphoramidate and lithium tert-butoxide coupled with trimethyl phosphite and / or wherein the precursors of the dopant or the precursors of the dopant oxide are chosen from one of the following pairs of precursors: tris(dimethylamino)silane coupled with ozone or water, bis(dimethylamino)dimethylsilane coupled with ozone or water.
14. A method according to any one of claims 10 to 13, wherein steps a) and c) are carried out by depositing by ALD a metal halide and / or an organometallic, the metal halide preferably comprising chlorine, iodine or bromine.
15. A method according to claim 14, wherein the metal halide is selected from titanium tetrachloride, titanium iodide and titanium tetrabromide, with preference being given to titanium tetrachloride.
16. Ionic dielectric layer (3) comprising: - a first part (31) comprising a matrix based on an ionic conductor in which a dopant is incorporated; - a second part (32) comprising an oxide of the dopant or comprising the matrix based on the ionic conductor in which the dopant is incorporated; the atomic content of dopant in the second part (32) of the ionic dielectric layer (3) being greater than the atomic content of dopant in the first part (31) of the ionic dielectric layer (3).
Citation Information
Patent Citations
Nanodevice arrays for electrical energy storage, capture and management and method for their formation
US10032569B2
Solid state energy storage devices
EP2620962A1
Dielectric thin film, capacitor element, and electronic component
EP3358039A1
Integrated energy storage component
EP3570307A1
Acceptor doped barium titanate based thin film capacitors on metal foils and methods of making thereof
US20060284233A1