PREPARATION OF A PRIMARY CATHODE LAYER
A dual polyacrylic binding agent approach with varying molecular masses improves cathode layer adhesion and compatibility, addressing inefficiencies in existing cathode preparation methods for secondary batteries.
Patent Information
- Application Number
- FR2023004465
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-04
- Publication Date
- 2024-11-08
AI Technical Summary
Existing cathode preparation compositions for secondary batteries are inadequate in terms of adhesion, thermal stability, chemical and electrochemical stability, tensile strength, flexibility, and compatibility with battery electrolytes, leading to inefficiencies and defects in the cathode layer.
A method involving the use of two polyacrylic binding agents of different molecular masses, combined with carbon particles, to form a primary cathode layer, where one agent has a molecular mass ranging from 100,000 to 1,000,000 g/mol and the other from 2,000 to 100,000 g/mol, applied with a specific drying process, enhancing adhesion and compatibility.
The method improves adhesion to the metal substrate, enhances compatibility with electroactive compounds, and ensures a stable, homogeneous cathode layer, suitable for secondary batteries.
Abstract
Description
Title of the invention: PREPARATION OF A PRIMARY CATHODE LAYER
[0001] The invention relates to a method for preparing a primary cathode layer combining two polyacrylic binding agents of different molecular weights and carbon particles. The invention also relates to a composition suitable for this method and to a cathode usable for the manufacture of secondary battery cells.
[0002] Cathode preparation compositions are known which generally comprise carbon and a metal in the form of particles associated with a binding agent. The binding agents allow the particles to be fixed to a metallic substrate. The binding strength is therefore crucial when manufacturing a cathode using these compositions.
[0003] The manufacturing time and yield of the cathodes are also important factors. Therefore, improving the efficiency of the various reactions involved should be sought.
[0004] As electrochemically inactive components during cathode operation, the binding compounds do not directly contribute to the capacity of the battery cell including the cathode, but their influence remains considerable on the overall electrochemical performance. These binding compounds must contribute to the formation of stable networks of the active or conductive solid components present in the cathodes.
[0005] The binding compounds used in the preparation of a cathode should also improve thermal stability, chemical and electrochemical stability, tensile strength, in particular through good adhesion and cohesion, as well as a certain degree of flexibility.
[0006] Furthermore, the compatibility of the various ingredients in the cathode and battery preparation compositions is also an important factor to consider when preparing these compositions, as well as when preparing the cathodes using these compositions. In particular, compatibility, and especially the absence of solubility or low solubility, with the battery electrolyte is a crucial property.
[0007] Easy and homogeneous application of cathode preparation compositions is sought in order to obtain a homogeneous layer and to limit or avoid defects on the electrode surface, resulting in a homogeneous and particularly efficient conductive layer. Surface leveling, restructuring, and behavior The flow of cathode preparation compositions must be well controlled.
[0008] Cathode preparation compositions must also be stable and homogeneous during their preparation, storage, or application. Sedimentation, formation of agglomerates or aggregates, and separation of ingredients must therefore be limited or avoided.
[0009] Generally, improving the adhesion of the active elements should always be a priority during cathode preparation. Therefore, the adhesion of the various layers of ingredients deposited on the metallic substrate must be enhanced. In particular, when a primary layer containing carbon is deposited on the metallic substrate, improving its adhesion is essential. Because they are in direct contact with the metallic substrate of the cathode and with the binding composition of the electroactive compound, the properties of the primary layer compositions are especially important.
[0010] The known compositions used in the preparation of the primary cathode layer in the prior art are not always satisfactory. Therefore, there is a need for compositions used in the preparation of the primary cathode layer that provide solutions to all or some of the problems with prior art compositions.
[0011] Thus, the invention provides a method for preparing a primary cathode layer comprising: * the application: - of at least one Q binding agent comprising at least one water-soluble PI polymer, of molecular mass Mw, measured by CES, ranging from more than 100,000 g / mol to 1,000,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiating compound, of at least one compound (al) selected from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt and their combinations, - of at least one binding agent R comprising at least one water-soluble polymer P2, of molecular mass Mw, measured by CES, ranging from 2,000 g / mol to strictly less than 100,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiating compound, of at least one compound (a2) selected from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt, and combinations thereof, and - of at least one material E comprising carbon particles; * the drying of the primary layer.
[0012] Preferably for the method according to the invention, the compound (al) is chosen among acrylic acid, methacrylic acid, a salt of acrylic acid, a salt of methacrylic acid and their combinations, preferably the compound (al) is acrylic acid or methacrylic acid.
[0013] The PI polymer implemented according to the invention is a water-soluble polymer. Preferably according to the invention, the PI polymer is water-soluble at a pH greater than 4.
[0014] Preferably according to the invention, the PI polymer can be a homopolymer of compound (al). Also preferably according to the invention, the PI polymer can be a copolymer of compounds (al) or be a copolymer of at least one compound (al) and at least one other compound (b).
[0015] Preferably, compound (b) is chosen from: - a compound (bl) selected from the Ci-Ci2 esters of methacrylic acid, the C1-C12 esters of acrylic acid and their combinations, preferably the CrC8 esters of methacrylic acid, the Ci-C8 esters of acrylic acid and their combinations, preferably methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, more preferably methyl acrylate, ethyl acrylate, butyl acrylate; - a compound (b2) selected from acrylonitrile, acrylamide, N-methylolacrylamide, vinyl-lactam, N-vinylpyrrolidone, ureidomethacrylate and their combinations, preferably acrylonitrile; - a compound (b3) chosen from maleic acid, maleic anhydride, itaconic acid, crotonic acid and their combinations; - a compound (b4) selected from hydroxyethylacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, caprolactone methacrylate, caprolactone acrylate, polycaprolactone methacrylate, polycaprolactone acrylate, lactam methacrylate, lactam acrylate, polycaprolactame methacrylate, polycaprolactame acrylate, styrene, more preferably styrene; - a compound (b5) selected from 2-acrylamido-2-methylpropane sulfonic acid, a salt of 2-acrylamido-2-methylpropane sulfonic acid, ethoxymethacrylate sulfonic acid, sodium methallyl sulfonate, styrene sulfonate, phosphated hydroxyethyl acrylate, phosphated hydroxyethyl methacrylate, phosphated hydroxypropyl acrylate, phosphated hydroxypropyl methacrylate, phosphated hydroxybutyl methacrylate; - a crosslinking compound (b6).
[0016] Preferably according to the invention, the PI polymer is not crosslinked. Also preferably, the compound (b) is not acrylonitrile or acrylamide, or it does not contain fluorine; the PI polymer is then not a fluorinated polymer. Also preferably according to the invention, the PI polymer is a free polymer, It is not grafted, in particular it is not grafted to a fluorinated polymer.
[0017] The quantities of monomers present in the PI polymer can vary relatively significantly. Preferably according to the invention, the PI polymer can be prepared by a polymerization reaction from 55% by weight to 100% by weight of compound (a1) and from 0% by weight to 45% by weight of compound (b).
[0018] Also preferably, the PI polymer can be prepared by a polymerization reaction of 55 wt% to 90 wt% of compound (al) and 10 wt% to 45 wt% of compound (b) or of 55 wt% to 80 wt% of compound (al) and 20 wt% to 45 wt% of compound (b).
[0019] According to the invention, the PI polymer can also be prepared by a polymerization reaction of 55 wt% to 70 wt% of compound (al) and of 30 wt% to 45 wt% of compound (b).
[0020] Essentially, according to the invention, the PI polymer has a molecular mass Mw, measured by CES, greater than 100,000 g / mol. Preferably, according to the invention, the PI polymer has a molecular mass Mw, measured by CES, ranging from 120,000 g / mol to 800,000 g / mol or from 150,000 g / mol to 800,000 g / mol.
[0021] Also preferably according to the invention, the PI polymer has a molecular mass Mw, measured by CES, ranging from 200,000 g / mol to 800,000 g / mol or from 250,000 g / mol to 800,000 g / mol.
[0022] More preferably according to the invention, the PI polymer has a molecular mass Mw, measured by CES, ranging from 120,000 g / mol to 500,000 g / mol or from 150,000 g / mol to 500,000 g / mol or from 200,000 g / mol to 500,000 g / mol or from 250,000 g / mol to 500,000 g / mol.
[0023] According to the invention, the molecular weight or mass of the PI and P2 polymers is determined by Size Exclusion Chromatography (SEC). A test portion of the polymer solution, corresponding to 90 mg of dry matter, is introduced into a 10 mL bottle. Mobile phase, supplemented with 0.04% dimethylformamide (DMF), is added up to a total mass of 10 g. The composition of this mobile phase is as follows: NaHCO3: 0.05 mol / L, NaNO3: 0.1 mol / L, triethanolamine: 0.02 mol / L, NaN3 0.03 wt%. The CES chain consists of a Waters 510 type isocratic pump, with a flow rate set at 0.8 mL / min, a Waters 717+ sample changer, a furnace containing a 6 cm long and 40 mm internal diameter Waters Guard Column Ultrahydrogel pre-column, followed by a 30 cm long and 7.8 mm internal diameter Waters Ultrahydrogel linear column.Detection is ensured by means of a Waters RI 410 type differential refractometer. The furnace is heated to 60°C and the refractometer to 45°C. The CES device is calibrated with a series of poly- standards. Sodium acrylates supplied by Polymer Standards Service, with peak molecular weights between 1000 g / mol and 1106 g / mol and polymolecularity indices between 1.4 and 1.7, were used. The calibration curve is linear and incorporates the correction obtained using the flow marker dimethylformamide (DMF). Chromatogram acquisition and processing were performed using PSS WinGPC Scientific v4.02 software. The resulting chromatogram is integrated into the region corresponding to molecular weights greater than 250 g / mol.
[0024] Also preferably according to the invention, the PI polymer has a glass transition temperature Tg, calculated according to the Flory-Fox equation, ranging from -10°C to 230°C or from 20°C to 230°C. More preferably according to the invention, the PI polymer is a homopolymer whose Tg is greater than 0°C, preferably greater than 10°C.
[0025] Also more preferably according to the invention, the PI polymer is a copolymer whose Tg is greater than 50°C, preferably greater than 100°C.
[0026] The Flory-Fox equation allows the glass transition temperature of a copolymer to be calculated from the parameters of the monomers used for its preparation.
[0027] The PI polymer implemented according to the invention can be used in its acidic form or in a form in which all or part of its carboxylic groups can be neutralized. Preferably according to the invention, the PI polymer is therefore totally or partially acidic or totally or partially non-neutralized. More preferably, the PI polymer is partially neutralized. According to the invention, the neutralization of the PI polymer is preferably carried out using at least one compound selected from LiOH, NaOH, KOH, Zn(OH)2, Mg(OH)2, Ca(OH)2, ZnO, MgO, CaO, ammonium derivatives, ammonia, amino bases, for example triethanolamine, aminomethylpropanol or 2-amino-2-methylpropanol (AMP) and their combinations, more preferably LiOH or Zn(OH)2 or ZnO.
[0028] Essentially, the method for preparing a primary cathode layer according to the invention comprises the application of binders Q and R and material E, as well as drying the primary layer. Preferably for the method according to the invention, the binding agent Q comprises at least one polymer PI and at least one liquid support, preferably water, alone or combined with at least one polar solvent, for example, a solvent selected from ethanol, isopropanol, and combinations thereof.
[0029] Also preferably according to the invention, the binding agent Q comprises: - from 5% by weight to 60% by weight of PI polymer and from 40% by weight to 95% by weight of liquid support, more preferably: - from 10% by weight to 40% by weight of PI polymer and from 60% by weight to 90% by weight of liquid support.
[0030] Preferably for the method according to the invention, compound (a2) is chosen among acrylic acid, methacrylic acid, a salt of acrylic acid, a salt of methacrylic acid and their combinations, preferably compound (a2) is acrylic acid or methacrylic acid.
[0031] The P2 polymer implemented according to the invention is a water-soluble polymer. Preferably according to the invention, the P2 polymer is water-soluble at a pH greater than 4.
[0032] The polymer P2 may be a homopolymer of compound (a2). Preferably according to the invention, the polymer P2 may be a copolymer of compounds (a2) or a copolymer of at least one compound (a2) and at least one other compound (c). More preferably according to the invention, the polymer P2 may be a copolymer of at least one compound (a2) and at least one other compound (c).
[0033] Preferably, compound (c) is chosen from: - a compound (cl) selected from CrCi2 esters of methacrylic acid, C1-C12 esters of acrylic acid and their combinations, preferably CrC8 esters of methacrylic acid, CrC8 esters of acrylic acid and their combinations, preferably methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, more preferably methyl acrylate, ethyl acrylate, butyl acrylate; - a compound (c2) selected from acrylonitrile, acrylamide, N-methylolacrylamide, vinyl-lactam, N-vinylpyrrolidone, ureidomethacrylate and their combinations, preferably acrylonitrile; - a compound (c3) selected from maleic acid, maleic anhydride, itaconic acid, crotonic acid and their combinations; - a compound (c4) selected from hydroxyethylacrylate, hydroxyethylmethacrylate, hydroxypropylacrylate, hydroxypropylmethacrylate, hydroxybutylmethacrylate, caprolactone methacrylate, caprolactone acrylate, polycaprolactone methacrylate, polycaprolactone acrylate, lactam methacrylate, lactam acrylate, polycaprolactame methacrylate, polycaprolactame acrylate, styrene, more preferably styrene; - a compound (c5) selected from 2-acrylamido-2-methylpropane sulfonic acid, a salt of 2-acrylamido-2-methylpropane sulfonic acid, ethoxymethacrylate sulfonic acid, sodium methallyl sulfonate, styrene sulfonate, phosphated hydroxyethyl acrylate, phosphated hydroxyethyl methacrylate, phosphated hydroxypropyl acrylate, phosphated hydroxypropyl methacrylate, phosphated hydroxybutyl methacrylate; - a crosslinking (c6) compound.
[0034] The quantities of monomers present in the P2 polymer can vary relatively significantly. Preferably according to the invention, the P2 polymer can be prepared by a polymerization reaction from 55% by weight to 100% by weight of compound (a2) and from 0% by weight to 45% by weight of compound (c).
[0035] Also preferably, the polymer P2 can be prepared by a polymerization reaction of 55 wt% to 90 wt% of compound (a2) and 10 wt% to 45 wt% of compound (c) or of 55 wt% to 80 wt% of compound (a2) and 20 wt% to 45 wt% of compound (c).
[0036] According to the invention, the P2 polymer can also be prepared by a polymerization reaction of 55 wt% to 70 wt% of compound (a2) and of 30 wt% to 45 wt% of compound (c).
[0037] Essentially according to the invention, the P2 polymer has a molecular mass Mw, measured by CES, strictly less than 100,000 g / mol. Preferably according to the invention, the P2 polymer has a molecular mass Mw, measured by CES, ranging from 2,000 g / mol to 80,000 g / mol or from 2,000 g / mol to 50,000 g / mol;
[0038] Also preferably according to the invention, the P2 polymer has a molecular mass Mw, measured by CES, ranging from 2,000 g / mol to 40,000 g / mol or from 2,000 g / mol to 30,000 g / mol. More preferably according to the invention, the P2 polymer has a molecular mass Mw, measured by CES, ranging from 2,000 g / mol to 25,000 g / mol or from 2,000 g / mol to 20,000 g / mol or from 5,000 g / mol to 25,000 g / mol or from 5,000 g / mol to 20,000 g / mol
[0039] Also preferably according to the invention, the P2 polymer has a glass transition temperature Tg, calculated according to the Flory-Fox equation, ranging from -10°C to 230°C or from 20°C to 230°C. More preferably according to the invention, the P2 polymer is a homopolymer whose Tg is greater than 0°C, preferably greater than 10°C.
[0040] Also, more preferably according to the invention, the P2 polymer is a copolymer whose Tg is greater than 50°C, preferably greater than 100°C.
[0041] The polymer P2 implemented according to the invention can be used in its acidic form or in a form in which all or part of its carboxylic groups can be neutralized. Preferably according to the invention, the polymer P2 is therefore totally or partially acidic or totally or partially non-neutralized. More preferably, the polymer P2 is partially neutralized. According to the invention, the neutralization of the polymer P2 is preferably carried out using at least one compound selected from LiOH, NaOH, KOH, Zn(OH)2, Mg(OH)2, Ca(OH)2, ZnO, MgO, CaO, ammonium derivatives, ammonia, amino bases, for example triethanolamine, aminomethylpropanol or 2-amino-2-methylpropanol (AMP) and their combinations, more preferably LiOH or Zn(OH)2 or ZnO.
[0042] Preferably for the method according to the invention, the binding agent R comprises at least one polymer P2 and at least one liquid support, preferably water, alone or combined with at least one polar solvent, for example a solvent selected from ethanol, isopropanol and their combinations.
[0043] Also preferably according to the invention, the binding agent R comprises: - from 5% by weight to 60% by weight of P2 polymer and from 40% by weight to 95% by weight of liquid support, more preferably: - from 10% by weight to 40% by weight of P2 polymer and from 60% by weight to 90% by weight of liquid support.
[0044] Preferably according to the invention, the metallic substrate is a purely metallic substrate or a composite substrate comprising at least one metal and at least one insulating support.
[0045] Also preferably according to the invention, the electro-active compound comprises at least one metal selected from lithium, iron, nickel, manganese, cobalt and their combinations.
[0046] Also preferably according to the invention, the electro-active compound is in the form of a metallic salt, preferably a polymetallic salt, more preferably the electro-active compound is chosen from LiFePO4 (LFP), Li(Ni,Mn,Co)O2 (NMC) and their combinations.
[0047] Preferably according to the invention, the binding compound for the electroactive compound is selected from polyvinylidene fluoride (PVDF). Preferably according to the invention, the binding compound for the electroactive compound is not a (meth)acrylic polymer.
[0048] Preferably according to the invention, the organic solvent is a polar aprotic solvent, preferably selected from pyrrolidone, N-methylpyrrolidone (NMP), alkyl carbonates and their combinations.
[0049] Essentially, according to the invention, the material E comprises carbon particles. Preferably, according to the invention, the material E is selected from carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanotubes, carbon nanofibers, hardened carbon, and combinations thereof. Also preferably, according to the invention, the electroactive composition comprises carbon, preferably selected from carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanotubes, carbon nanofibers, hardened carbon, and combinations thereof.
[0050] The method according to the invention allows for the preparation of a primary cathode layer. It comprises the application of the binding agents Q and R and of the material E, as well as the drying of the primary layer. Preferably, for the method according to the invention, the application of the binding agents Q and R and of the material E is carried out on a metallic substrate comprising at least one metal selected from aluminum, nickel, and combinations thereof. Aluminum is particularly preferred.
[0051] According to the invention, the preparation method may include calendering the metallic substrate bearing the primary layer.
[0052] Preferably, for the method according to the invention, the binding agent Q and the material E are applied simultaneously, and the agent R is applied separately. Also preferably, the binding agent Q and the material E are applied simultaneously, and then the agent R is subsequently applied separately. Also preferably, according to the invention, the binding agent Q, the agent R, and the material E are applied simultaneously.
[0053] More preferably, the method according to the invention comprises the application of a composition QE comprising the binding agent Q and the material E and of a composition RE comprising the binding agent R and the material E. More preferably, it comprises the application of a composition QE comprising the binding agent Q and the material E and then of a composition RE comprising the binding agent R and the material E.
[0054] Also, more preferably, the method according to the invention comprises the application of a composition QE comprising the binding agent Q and the material E and of the binding agent R. More preferably, it comprises the application of a composition QE comprising the binding agent Q and the material E and then of the binding agent R.
[0055] Also, more preferably, the method according to the invention includes the application of a QRE composition comprising the binding agent Q, the binding agent R and the material E.
[0056] The method for preparing a primary cathode layer according to the invention comprises the application of the binding agents Q and R and of the material E. The application can be carried out using a particular composition. Thus, the invention also provides a QRE composition, preferably an aqueous QRE composition, for preparing a primary cathode layer, comprising: - at least one binding agent Q comprising at least one water-soluble polymer PI, of molecular mass Mw, measured by CES, ranging from more than 100,000 g / mol to 1,000,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiating compound, of at least one compound (al) selected from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt and their combinations, - at least one binding agent R comprising at least one water-soluble polymer P2, of molecular mass Mw, measured by CES, ranging from 2,000 g / mol to strictly less than 100,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiating compound, at least one compound (a2) selected from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt, and combinations thereof, and - at least one material E comprising carbon particles.
[0057] Preferably according to the invention, the QRE composition comprises, by dry weight: - from 0.5% to 40% of Q binding agent, - from 0.5% to 30% of binding agent R, - from 30% to 99% E-material, relative to the total quantity by dry weight of binding agents Q and R and material E.
[0058] Preferably according to the invention, it comprises, by dry weight: - from 0.5% to 50% of binding agent Q, - from 0.5% to 20% of binding agent R, - from 30% to 99% E-material, compared to the total dry weight quantity of binding agents Q and R and material E.
[0059] Advantageously, the method for preparing a primary cathode layer can be implemented during cathode preparation. Thus, the invention also provides a method for preparing a cathode comprising: * the application, on a metallic substrate comprising at least one metal chosen from aluminium, nickel and their combinations, of a primary layer obtained by the application: - of at least one binding agent Q comprising at least one water-soluble polymer PI, of molecular mass Mw, measured by CES, ranging from more than 100,000 g / mol to 1,000,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiating compound, of at least one compound (al) selected from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt and their combinations, - of at least one binding agent R comprising at least one water-soluble polymer P2, of molecular mass Mw, measured by CES, ranging from 2,000 g / mol to strictly less than 100,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiating compound, of at least one compound (a2) selected from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt, and combinations thereof, and - of at least one material E comprising carbon particles; * the drying of the primary layer, then the possible calendering of the metallic substrate carrying the primary layer, then * the application, on the primary layer, of an electro-active composition comprising at least one electro-active compound, at least one binding compound for the electro-active compound, and at least one organic solvent, * the drying and then calendering of the metallic substrate carrying the primary layer and the electro-active coating.
[0060] The method for preparing a cathode according to the invention therefore comprises the pre- preparation of a primary cathode layer defined according to the invention.
[0061] This preparation method according to the invention makes it possible to obtain a cathode that possesses particularly advantageous properties. Thus, the invention also provides a cathode comprising at least one metallic substrate coated with at least one primary layer comprising a binding agent Q, a binding agent R, and at least one material E according to the invention. Preferably, the cathode according to the invention is obtained according to the method for preparing a primary layer according to the invention or by a method for preparing a cathode according to the invention. Also preferably, the cathode according to the invention is prepared using a QRE composition according to the invention. Particularly preferred according to the invention, the QRE composition according to the invention comprises a mass quantity of polymer PI greater than the mass quantity of polymer P2.
[0062] The combination of PI and P2 polymers present in the Q and R binding agents implemented according to the invention possesses particularly advantageous properties for the preparation of a primary cathode layer and thus for obtaining a cathode. This polymer combination used according to the invention notably improves the adhesion of the cathode to the metallic substrate. In particular, it improves adhesion to the metallic substrate when used in combination with the binding agent of the electroactive compound. The compatibility of the PI and P2 polymers, in particular the compatibility of the P2 polymer, and the binding agent of the electroactive compound is particularly advantageous during the preparation of a cathode.
[0063] Thus, the invention also provides a method for improving adhesion on a metallic cathode substrate comprising at least one metal selected from aluminium, nickel and their combinations, of an electroactive composition comprising at least one electroactive compound, at least one binding compound for the electroactive compound and at least one organic solvent, comprising: - the preliminary application directly onto the metallic substrate, followed by possible drying and calendering, of at least one aqueous primer preparation composition defined according to the invention, then - the application of the electro-active composition, - the drying and then the calendering of the metallic substrate carrying the primary layer and the electro-active coating.
[0064] The combination of PI and P2 polymers, and in particular polymer P2, implemented according to the invention, improves subsequent adhesion to the binding compound of the electroactive compound. This combination, and in particular polymer P2, acts as adhesion promoters between the metallic substrate and this binding compound of the electroactive compound. They also contribute to the adhesion of the particles of carbon of material E on the metallic substrate.
[0065] The advantageous, particular or preferred characteristics of the method of preparing a primary cathode layer according to the invention define methods of preparing a cathode according to the invention, primary layer preparation compositions, methods of improving adhesion to a metallic cathode substrate, as well as cathodes, which are also advantageous, particular or preferred.
[0066] The various aspects of the invention can be illustrated by examples. EXAMPLES
[0067] Preparation and characterization of PI and P2 polymers and O and R agents according to the invention Polymer Pl.l and agent Q1:
[0068] In a 1 L glass reactor equipped with mechanical stirring and oil bath heating, 498 g of deionized water is introduced. The assembly is then heated to approximately 95°C and, over 120 minutes, the following are added using peristaltic pumps: - in a first test tube, 270 g of acrylic acid, - in a second test tube 2.55 g of ammonium persulfate dissolved in 50 g of deionized water.
[0069] Then, heating is continued for 60 minutes. The mixture is then cooled and diluted to obtain agent Q1 according to the invention, which has a dry matter content of 25% by weight, a pH of 2.3 and comprises the PLI polymer, whose molecular mass Mw, measured by CES, is 220,000 g / mol. Polymer P1.2 and agent Q2:
[0070] In a 1 L glass reactor equipped with mechanical stirring and oil bath heating, 498 g of deionized water is introduced. The assembly is then heated to approximately 95°C and, over 120 minutes, the following are added using peristaltic pumps: - in a first test tube, 270 g of acrylic acid, - in a second test tube 1.8 g of ammonium persulfate dissolved in 50 g of deionized water.
[0071] Then, heating is continued for 60 minutes. The mixture is then cooled and diluted to obtain agent Q2 according to the invention, which has a dry matter content of 25% by weight, a pH of 2.3 and comprises polymer P 1.2, whose molecular mass Mw, measured by CES, is 125,000 g / mol. Polymer P1.3 and agent Q3:
[0072] In a 1 L glass reactor equipped with mechanical stirring and oil bath heating, 498 g of deionized water is introduced. The assembly is then heated to approximately 95°C and, over 120 minutes, the following are added using peristaltic pumps: - in a first test tube 270 g of acrylic acid, - in a second test tube 5.2 g of ammonium persulfate dissolved in 50 g of deionized water.
[0073] Then, heating is continued for 60 minutes. The mixture is then cooled and diluted to obtain agent Q3 according to the invention, which has a dry matter content of 25% by weight, a pH of 2.3 and comprises polymer P 1.3, whose molecular mass Mw, measured by CES, is 305,000 g / mol. Polymer P1.4 and agent Q4:
[0074] In a 1 L glass reactor equipped with mechanical stirring and oil bath heating, 90 g of acrylic acid (monomer a), 10 g of ethyl acrylate (monomer b), and 875 g of deionized water are introduced. The mixture is heated to 70°C. Then, a solution comprising 0.35 g of ammonium persulfate in 10 g of deionized water is added all at once.
[0075] Then, heating is continued for 60 minutes at 85°C. Again, a solution comprising 0.35 g of ammonium persulfate in 20 g of deionized water is poured in one go.
[0076] Then, heating is continued for 60 minutes. The mixture is then cooled and diluted to obtain agent Q4 according to the invention, which has a dry matter content of 10.4% by weight, a pH of 2.5 and comprises polymer P1.4, whose molecular mass Mw, measured by CES, is 256,000 g / mol. Polymer P1.5 and agent Q5:
[0077] In a 1 L glass reactor equipped with mechanical stirring and oil bath heating, 100 g of acrylic acid (monomer a) and 875 g of deionized water are introduced.
[0078] It is heated to 70°C. Then, a solution comprising 0.45 g of ammonium persulfate in 10 g of deionized water is poured in one go.
[0079] Then, heating is continued for 60 minutes at 85°C. The mixture is then cooled and diluted to obtain agent Q5 according to the invention, which has a dry matter content of 10.4% by weight, a pH of 2.5 and comprises polymer P1.5, whose molecular mass Mw, measured by CES, is 370,000 g / mol. P2.1 polymer and RI agent:
[0080] In a 1 L reactor equipped with mechanical stirring, an oil bath heater, and peristaltic pumps, 200 g of isopropanol and 1.7 g of AZDN are weighed out. The mixture is then heated under reflux at approximately 80°C, and over 120 minutes, using the peristaltic pumps, 200 g of acrylic acid and 81 g of butyl acrylate are added. Heating under reflux is then continued for 60 minutes.
[0081] The isopropanol is then distilled and gradually replaced with water during distillation. The mixture is then cooled and diluted to obtain the RI agent according to the invention, which has a dry matter content of 40% by weight, a pH of 2.3 and comprises the polymer P2.1, whose molecular mass Mw, measured by CES, is 9,000 g / mol. Polymer P2.2 and agent R2:
[0082] In a 1 L reactor equipped with mechanical stirring, an oil bath heater, and peristaltic pumps, 200 g of isopropanol and 1.7 g of AZDN are weighed out. The mixture is then heated under reflux at approximately 80°C, and over 120 minutes, using the peristaltic pumps, 200 g of acrylic acid and 80 g of ethyl acrylate are added. Heating under reflux is then continued for 60 minutes. The isopropanol is then distilled, and it is gradually replaced by water during the distillation process.
[0083] The mixture is then cooled and diluted to obtain agent R2 according to the invention, which has a dry matter content of 40% by weight, a pH of 2.2, and comprises polymer P2.2, whose molecular weight Mw, measured by CES, is 9,500 g / mol. Polymer P2.3 and agent R3:
[0084] In a 1 L reactor equipped with mechanical stirring, an oil bath heater, and peristaltic pumps, 200 g of isopropanol and 1.9 g of AZDN are weighed out. The mixture is then heated under reflux at approximately 80°C, and over 120 minutes, using the peristaltic pumps, 200 g of acrylic acid and 83 g of methyl methacrylate are added. Heating under reflux is then continued for 60 minutes. The isopropanol is then distilled, and it is gradually replaced by water during the distillation process.
[0085] The mixture is then cooled and diluted to obtain agent R3 according to the invention, which has a dry matter content of 40% by weight, a pH of 2.5, and comprises polymer P2.3, whose molecular weight Mw, measured by CES, is 8,000 g / mol. Polymer P2.4 and agent R4:
[0086] In a 1 L reactor equipped with mechanical stirring, an oil bath heater, and peristaltic pumps, the following are weighed out: 209.7 g of water, 0.08 g of iron(II) sulfate heptahydrate, and 0.011 g of copper(II) sulfate pentahydrate. The mixture is then heated to 95°C, and over 120 minutes, using the peristaltic pumps, the following are added: 302.5 g of acrylic acid and 13 g of water, 25.6 g of sodium hypophosphite monohydrate dissolved in 29 g of water, and 20.46 g of 130V hydrogen peroxide diluted with 25 g of water. Heating is then continued for 60 minutes.
[0087] The assembly is then cooled and diluted to obtain the agent R4 according to the invention, the dry matter content of which is 40% by weight, the pH is 2.1 and which comprises the polymer P2.4, the molecular mass of which Mw, measured by CES, is 4,400 g / mol. Polymer P2.5 and agent R5:
[0088] In a 1 L reactor equipped with mechanical stirring, an oil bath heater, and peristaltic pumps, the following are weighed out: 121 g of water, 121 g of isopropanol, 0.06 g of iron(II) sulfate heptahydrate, and 11 g of hydrazine hydrate at a concentration of 35% in water. The mixture is then heated under reflux to approximately 81°C, and over 120 minutes, the following are added using the peristaltic pumps: - in a first test tube, 174 g of acrylic acid, 35 g of methyl methacrylate, 110 g of ethylene glycol phosphate and 80 g of water, - in a second test tube 20 g of hydrogen peroxide at 130V and 100 g of water.
[0089] After the additions are complete, heating is continued under reflux for 60 minutes at 80°C, and then the isopropanol is distilled with the addition of water during the distillation. The mixture is then cooled and diluted to obtain agent R5 according to the invention, which has a dry matter content of 40% by weight, a pH of 2.0, and comprises polymer P2.5, whose molecular weight Mw, measured by CES, is 15,000 g / mol. Polymer P2.6 and agent R6:
[0090] In a 1 L reactor equipped with mechanical stirring, an oil bath heater, and peristaltic pumps, 200 g of isopropanol and 2 g of AZDN are weighed out. The mixture is then heated under reflux at approximately 80°C, and over 120 minutes, using the peristaltic pumps, 200 g of acrylic acid and 80 g of a calcium prolactone acrylate marketed by the "Arkema" group under the reference SR 495B are added. Heating under reflux is then continued for 60 minutes. The isopropanol is then distilled, and it is gradually replaced by water during the distillation process. The mixture is then cooled and diluted to obtain agent R6 according to the invention, which has a dry matter content of 40% by weight, a pH of 2.3 and comprises polymer P2.6, whose molecular mass Mw, measured by CES, is 7,500 g / mol.
[0091] Preparation of aqueous ORE compositions for primary layer preparation of cathode according to the invention
[0092] 150 g of deionized water is weighed with 28 g of agent Q1 and 7.5 g of agent RI according to the invention and then mixed under stirring using a dispersing apparatus (VMI) equipped with a toothed paddle 6.5 cm in diameter. Then, 10 g of carbon black (C-Nergy Super C65 "Imerys") is added, with stirring maintained for 1.25 h at 1500 rpm to obtain a composition whose homogeneity and absence of aggregates are checked using a North gauge. The QRE1 composition is obtained from agents Q1 and RI.
[0093] Similarly, primary cathode layer compositions QRE2 to QRE14 are prepared from agents Q1 to Q5 and RI to R6 according to the respective dry matter amounts of polymers PI and P2 and a total quantity of 10 g in dry matter of PI and P2 polymers present in agents Q and R and described in Table 1.
[0094] Preparation and characterization of cathodes according to the invention
[0095] On a sheet of aluminum degreased with acetone, 12 µm of the QRE1 cathode primer preparation composition according to the invention is applied using a coater equipped with a threaded rod (RK Control Coater), at an application speed of 10 mm / s. It is then dried at 150°C in an oven for 5 minutes. The primer layer obtained using the QRE1 composition, once applied and dried, has a mass, measured using a precision balance, of 0.2 mg for an aluminum disc 12 mm in diameter and 10 µm + / -1 µm thick.
[0096] In a similar manner, primary cathode layers are prepared using compositions QRE2 to QRE14.
[0097] The adhesion of the primary layer obtained using compositions QRE1 to QRE14 according to the invention to the aluminum cathode substrate is evaluated by a peel test. A standardized adhesive strip (“Intertape” 51596 CIC8091013) is manually applied to the primary cathode layer. The adhesive strip is then peeled off, and the adhesion of the primary layer to the aluminum is visually assessed.
[0098] The compatibility of the primary layer prepared according to the invention with a secondary layer of binding agent is evaluated for a polyvinylidene fluoride (PVDF, “Kynar” HSV900 “Arkema”) binding agent applied in N-methylpyrrolidone (NMP) solvent medium.
[0099] On a primary cathode layer obtained according to the method described above, a layer of PVDF bonding agent is applied using a solution with a 5% concentration of PVDF in NMP, then applied in a 9 pm layer and then dried at 150°C in an oven for 5 minutes.
[0100] A standard adhesive strip (“Intertape” 51596 CIC8091013) is manually applied to the secondary cathode layer. Then, the adhesive strip is peeled off and the adhesion is visually assessed.
[0101] The results obtained for the adhesion of the primary layer and for its compatibility with the secondary PVDF layer are presented in Table 1 according to the scale: - 1: aluminum foil visible on the majority of the surface of the adhesive strip, - 2: aluminum foil visible on part of the surface of the adhesive strip, - 3: aluminum foil not visible on the surface of the adhesive strip, - 4: primary layer mostly intact, - 5: primary layer totally intact.
[0102] Ratings 1 and 2 are not acceptable for the use of the cathode in a secondary battery. Ratings 3 to 5 are acceptable for the use of the cathode in a secondary battery. The results are presented in Table 1.
[0103] [tab.1] Composition QRE Mass content of PI in Q Mass content of P2 in R Adhesion Compatibility 1 P14 70% P24 30% 4 5 7 PLI 80% P2-2 20% .5 3 Pl-1 90% P2-3 10% 5 4 '4 PI4. 70% P2-4 30% 4 4 5 PI-2 80% P2-1 20% 4 5 6 P1-2 90% P2-4 10% 5 4 P1-3 80% P2-5 20% 5 5 8 P1-3 80% CS O •-.G 4 5 9 P14 70% P2--5 30% 5 10 P1-3 70% P24 30% 4 5 11 P1-4 70% NJ j O -.0 4 5 12 PI-4 80% P2-2 20% 4 5 13 P1-5 80% P2-2 20% 5 5 14 PI-5 75% P2~5 25% 5 5
[0104] The Q and R bonding agents, comprising the polymers according to the invention, make it possible, on the one hand, to create high-quality primary adhesion layers that very effectively retain the conductive carbon on the surface of the aluminum foil. They also act as bonding agents compatible with the PVDF secondary bonding agent, which is the polymeric constituent of the LFP layer, thereby increasing the adhesion of the LFP layer to the primary adhesion layer of the cathode.
Claims
Claims
1. A method of preparing a cathode primer layer comprising: * applying: - at least one binding agent Q comprising at least one water-soluble polymer PI, of molecular mass Mw, measured by CES ranging from more than 100,000 g / mol to 1,000,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiator compound, of at least one compound (al) chosen from acrylic acid, methacrylic acid, an oligomer of acrylic acid, an oligomer of methacrylic acid, an acrylic acid salt, a methacrylic acid salt, an oligomer salt of acrylic acid, a methacrylic acid oligomer salt and combinations thereof, - at least one binding agent R comprising at least one water-soluble polymer P2, with a molecular mass Mw, measured by CES, ranging from 2,000 g / mol to strictly less than 100,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiator compound, of at least one compound (a2) chosen from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt, and combinations thereof, and - at least one material E comprising carbon particles; * drying of the primer coat.
2. Method according to claim 1 wherein: * compound (al) is selected from acrylic acid, methacrylic acid, a salt of acrylic acid, a salt of methacrylic acid and combinations thereof, preferably compound (al) is acrylic acid or methacrylic acid; or * the PI polymer is water-soluble at a pH greater than 4 or in which: * polymer PI is a homopolymer of compound (al); or * the polymer PI is a copolymer of compounds (al); or * the polymer PI is a copolymer of at least one compound (al) and at least one other compound (b), preferably a compound (b) chosen from: - a compound (bl) chosen from CrCi2 esters of methacrylic acid, Ci-Ci2 esters of acrylic acid and combinations thereof,
3. preferably CrC8 esters of methacrylic acid, CrC8 esters of acrylic acid and combinations thereof, preferably methylmethacrylate, ethylmethacrylate, propylmethacrylate, butylmethacrylate, methylacrylate, ethylacrylate, propylacrylate, butylacrylate, more preferably, methylacrylate, ethylacrylate, butylacrylate; - a compound (b2) chosen from acrylonitrile, acrylamide, N-methylolacrylamide, vinyl-lactam, N-vinylpyrrolidone, ureidomethacrylate and their combinations, preferably acrylonitrile; - a compound (b3) chosen from maleic acid, maleic anhydride, itaconic acid, crotonic acid and combinations thereof; - a compound (b4) chosen from hydroxyethylacrylate, hydroxyethylmethacrylate, hydroxypropylacrylate, hydroxypropylmethacrylate, hydroxybutylmethacrylate, caprolactone methacrylate, caprolactone acrylate, polycaprolactone methacrylate, polycaprolactone acrylate, lactam methacrylate, lactam acrylate, polycaprolactam methacrylate, polycaprolactam acrylate, styrene, more preferably styrene; - a compound (b5) chosen from 2-acrylamido-2-methylpropane sulfonic acid, a salt of 2-acrylamido-2-methylpropane sulfonic acid, ethoxymethacrylate sulfonic acid, sodium methallyl sulfonate, styrene sulfonate hydroxyethylacrylate phosphate, hydroxyethylmethacrylate phosphate, hydroxypropylacrylate phosphate, hydroxypropylmethacrylate phosphate, hydroxybutylmethacrylate phosphate; - a crosslinking compound (b6). Method according to claim 2 wherein: * the PI polymer is prepared by a polymerization reaction: - from 55% by weight to 100% by weight of compound (al) and from 0% by weight to 45% by weight of compound (b); or - from 55% by weight to 90% by weight of compound (al) and from 10% by weight to 45% by weight of compound (b); or - from 55% by weight to 80% by weight of compound (al) and from 20% by weight to 45% by weight of compound (b); or - from 55% by weight to 70% by weight of compound (al) and from 30% by weight to 45% by weight of compound (b); or for which: * the PI polymer has a molecular mass Mw, measured by CES, ranging from 120,000 g / mol to 800,000 g / mol or from 150,000 g / mol to 800,000 g / mol, preferably from 200,000 g / mol to 800,000 g / mol or from 250,000 g / mol to 800,000 g / mol, more preferably from 120,000 g / mol to 500,000 g / mol or from 150,000 g / mol to 500,000 g / mol or from 200,000 g / mol to 500,000 g / mol or from 250,000 g / mol to 500,000 g / mol; Or * the polymer PI has a glass transition temperature Tg, calculated according to the Flory-Fox equation, ranging from -10°C to 230°C or from 20°C to 230°C; or for which the polymer PI is a homopolymer whose Tg is greater than 0°C, preferably greater than 10°C or for which the polymer PI is a copolymer whose Tg is greater than 50°C, preferably greater than 100°C; or * the polymer PI is totally or partially acidic or totally or partially non-neutralized, preferably the polymer PI is partially neutralized, preferably by means of at least one compound chosen from LiOH, NaOH, KOH, Zn(OH)2, Mg(OH)2, Ca(OH)2, ZnO, MgO, CaO, ammonium derivatives, ammonia, aqueous ammonia, amine bases, for example triethanolamine, aminomethylpropanol or 2-amino-2-methyl-propanol (AMP) and combinations thereof, more preferably LiOH or Zn(OH)2 or ZnO.
4. Method according to one of claims 1 to 3 for which: * the binding agent Q comprises at least one polymer PI and at least one liquid support, preferably water, alone or combined with at least one polar solvent, for example a solvent chosen from ethanol, isopropanol and their combinations; or for which: * the binding agent Q includes: - from 5% by weight to 60% by weight of PI polymer and from 40% by weight to 95% by weight of liquid support, more preferably: - from 10% by weight to 40% by weight of PI polymer and from 60% by weight to 90% by weight of liquid support.
5. Method according to one of claims 1 to 4 for which: * compound (a2) is selected from acrylic acid, methacrylic acid, a salt of acrylic acid, a salt of methacrylic acid and combinations thereof, preferably compound (a2) is acrylic acid or methacrylic acid; or * polymer P2 is water-soluble at a pH greater than 4 or in which: * polymer P2 is a homopolymer of compound (a2); or * polymer P2 is a copolymer of compounds (a2); or * polymer P2 is a copolymer of at least one compound (a2) and at least one other compound (c), preferably a compound (c)
6. chosen from: - a compound (cl) chosen from C1-C12 esters of methacrylic acid, C1-C12 esters of acrylic acid and combinations thereof, preferably Cr-C8 esters of methacrylic acid, Cr-C8 esters of acrylic acid and combinations thereof, preferably methylmethacrylate, ethylmethacrylate, propylmethacrylate, butylmethacrylate, methylacrylate, ethylacrylate, propylacrylate, butylacrylate, more preferably, methylacrylate, ethylacrylate, butylacrylate; - a compound (c2) chosen from acrylonitrile, acrylamide, N-methylolacrylamide, vinyl-lactam, N-vinylpyrrolidone, ureidomethacrylate and their combinations, preferably acrylonitrile; - a compound (c3) chosen from maleic acid, maleic anhydride, itaconic acid, crotonic acid and their combinations; - a compound (c4) chosen from hydroxy ethylacrylate, hydroxyethylmethacrylate, hydroxypropylacrylate, hydroxypropylmethacrylate, hydroxybutylmethacrylate, caprolactone methacrylate, caprolactone acrylate, polycaprolactone methacrylate, polycaprolactone acrylate, lactam methacrylate, lactam acrylate, polycaprolactam methacrylate, polycaprolactam acrylate, styrene, more preferably styrene; - a compound (c5) chosen from 2-acrylamido-2-methylpropane sulfonic acid, a salt of 2-acrylamido-2-methylpropane sulfonic acid, ethoxymethacrylate sulfonic acid, sodium methallyl sulfonate, styrene sulfonate, phosphated hydroxyethylacrylate, phosphated hydroxyethylmethacrylate, phosphated hydroxypropylacrylate, phosphated hydroxypropylmethacrylate, phosphated hydroxybutylmethacrylate; - a crosslinking compound (c6). Method according to claim 5 wherein: * polymer P2 is prepared by a polymerization reaction: - from 55% by weight to 100% by weight of compound (a2) and from 0% by weight to 45% by weight of compound (c); or - from 55% by weight to 90% by weight of compound (a2) and from 10% by weight to 45% by weight of compound (c); or - from 55% by weight to 80% by weight of compound (a2) and from 20% by weight to 45% by weight of compound (c); or - from 55% by weight to 70% by weight of compound (a2) and from 30% by weight to 45% by weight of compound (c); or for which: * polymer P2 has a molecular mass Mw, measured by CES, ranging from 2,000 g / mol to 80,000 g / mol or from 2,000 g / mol to 50,000 g / mol, preferably from 2,000 g / mol to 40,000 g / mol or from 2,000 g / mol to 30,000 g / mol, more preferably from 2,000 g / mol to 25,000 g / mol or from 2,000 g / mol to 20,000 g / mol or from 5,000 g / mol to 25,000 g / mol or from 5,000 g / mol to 20,000 g / mol; or * the polymer P2 has a glass transition temperature Tg, calculated according to the Flory-Fox equation, ranging from -10°C to 230°C or from 20°C to 230°C; or for which the polymer P2 is a homopolymer whose Tg is greater than 0°C, preferably greater than 10°C or for which the polymer P2 is a copolymer whose Tg is greater than 50°C, preferably greater than 100°C;or * the polymer P2 is totally or partially acidic or totally or partially non-neutralized, preferably the polymer P2 is partially neutralized, preferably by means of at least one compound chosen from LiOH, NaOH, KOH, Zn(OH)2, Mg(OH)2, Ca(OH)2, ZnO, MgO, CaO, ammonium derivatives, ammonia, aqueous ammonia, amine bases, for example triethanolamine, aminomethylpropanol or 2-amino-2-methyl-propanol (AMP) and combinations thereof, more preferably LiOH or Zn(OH)2 or ZnO.;
7. Method according to one of claims 1 to 6 for which: * the binding agent R comprises at least one polymer P2 and at least one liquid support, preferably water, alone or combined with at least one polar solvent, for example a solvent chosen from ethanol, isopropanol and their combinations; or for which: * the binding agent R comprises: - from 5% by weight to 60% by weight of polymer P2 and from 40% by weight to 95% by weight of liquid support, more preferably: - from 10% by weight to 40% by weight of polymer P2 and from 60% by weight to 90% by weight of liquid support.
8. Method according to one of claims 1 to 7 for which: the material E is chosen from carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanotubes, carbon nanofiber, hardened carbon and their combinations.
9. Method according to one of claims 1 to 8 for which: * the application of the binding agents Q and R and of the material E is carried out on a metal substrate comprising at least one metal chosen from aluminum, nickel and their combinations; or also comprising: * the calendering of the metal substrate carrying the primary layer; or for which: * the binding agent Q and the material E are applied simultaneously and the agent R is applied separately, preferably the binding agent Q and the material E are applied simultaneously and then the agent R is subsequently applied separately; or * the binding agent Q, the agent R and the material E are applied simultaneously; or * including the application: - of a composition QE comprising the binding agent Q and the material E and of a composition RE comprising the binding agent R and the material E, preferably: - a QE composition comprising the binding agent Q and the material E then a composition RE comprising the binding agent R and the material E; or - of a composition QE comprising the binding agent Q and the material E and the binding agent R, preferably: - a composition QE comprising the binding agent Q and the material E then the binding agent R; or - a QRE composition comprising the binding agent Q, the binding agent R and the material E.
10. QRE composition, preferably an aqueous QRE composition, for preparing a cathode primer layer, comprising: * at least one binding agent Q comprising at least one water-soluble polymer PI, with a molecular mass Mw, measured by CES, ranging from more than 100,000 g / mol to 1,000,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiator compound, of at least one compound (al) chosen from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt and combinations thereof, * at least one binding agent R comprising at least one water-soluble polymer P2, of molecular mass Mw, measured by CES, ranging from 2,000 g / mol to strictly less than 100,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiator compound, of at least one compound (a2) chosen from acrylic acid, methacrylic acid, an oligomer of acrylic acid, an oligomer of methacrylic acid, an acrylic acid salt, a salt of metha- acrylic acid, an oligomeric salt of acrylic acid, an oligomeric salt of methacrylic acid, and combinations thereof, and * at least one material E comprising carbon particles.
11. QRE composition according to claim 10 comprising, by dry weight: - from 0.5% to 40% of binding agent Q, - from 0.5% to 30% of binding agent R, - from 30% to 99% of material E; preferably: - from 0.5% to 50% of binding agent Q, - from 0.5% to 20% of binding agent R, - from 30% to 99% of material E; relative to the total quantity by dry weight of binding agents Q and R and material E.
12. A method of preparing a cathode comprising: * the application on a metal substrate comprising at least one metal chosen from aluminum, nickel and their combinations, of a primer layer obtained by the application: - at least one binding agent Q comprising at least one water-soluble polymer PI, with a molecular mass Mw, measured by CES, ranging from more than 100,000 g / mol to 1,000,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiator compound, of at least one compound (al) chosen from acrylic acid, methacrylic acid, an oligomer of acrylic acid, an oligomer of methacrylic acid, an acrylic acid salt, a methacrylic acid salt, an oligomer salt of acrylic acid, a methacrylic acid oligomer salt and combinations thereof, - at least one binding agent R comprising at least one water-soluble polymer P2, with a molecular mass Mw, measured by CES, ranging from 2,000 g / mol to strictly less than 100,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiator compound, of at least one compound (a2) chosen from acrylic acid, methacrylic acid, an acrylic acid oligomer, a methacrylic acid oligomer, an acrylic acid salt, a methacrylic acid salt, an acrylic acid oligomer salt, a methacrylic acid oligomer salt, and combinations thereof, and - at least one material E comprising carbon particles; * drying of the primer layer, then possible calendering of the metal substrate bearing the primer layer, then * the application, on the primary layer, of an electro-active composition comprising at least one electroactive compound, at least one binding compound of the electroactive compound and at least one organic solvent, * drying then calendering the metal substrate carrying the primer layer and the electroactive coating.
13. A method of preparing a cathode according to claim 12 comprising preparing a cathode primer layer defined according to one of claims 1 to 9.
14. A method for preparing a cathode according to claim 13, wherein: - the metal substrate is a purely metal substrate or a composite substrate comprising at least one metal and at least one insulating support; or - the electroactive compound comprises at least one metal selected from lithium, iron, nickel, manganese, cobalt and combinations thereof; or - the electroactive compound is in the form of a metal salt, preferably a polymetallic salt, preferably the electroactive compound is selected from LiFePO4 (LFP), Li(Ni,Mn,Co)O2 (NMC) and combinations thereof; or - the binder compound of the electroactive compound is selected from polyvinylidene fluoride (PVDF); or - the organic solvent is an aprotic polar solvent, preferably selected from pyrrolidone, N-methyl-pyrrolidone (NMP), alkyl carbonates and combinations thereof;or - the electroactive composition comprises carbon, preferably selected from carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanotubes, carbon nanofiber, hardened carbon and combinations thereof.;
15. Cathode comprising at least one metal substrate covered with at least one primary layer comprising a binding agent Q, a binding agent R and at least one material E, obtained according to the method of preparing a primary layer according to one of claims 1 to 9, or prepared using a QRE composition according to one of claims 10 or 11 or even prepared according to the preparation method according to one of claims 12 or 13.
16. Method for improving the adhesion to a metal cathode substrate comprising at least one metal selected from aluminum, nickel and combinations thereof, of an electroactive composition comprising at least one electroactive compound, at least one compound binding compound of the compound electroactive and at least one organic solvent, comprising: * the prior application directly onto the metal substrate, then the possible drying and the possible calendering, of at least one aqueous composition for preparing a primer layer comprising: - at least one binding agent Q comprising at least one water-soluble polymer PI, of molecular mass Mw, measured by CES ranging from more than 100,000 g / mol to 1,000,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiator compound, of at least one compound (al) chosen from acrylic acid, methacrylic acid, an oligomer of acrylic acid, an oligomer of methacrylic acid, an acrylic acid salt, a methacrylic acid salt, an oligomer salt of acrylic acid, a methacrylic acid oligomer salt and combinations thereof, - at least one binding agent R comprising at least one water-soluble polymer P2, of molecular mass Mw, measured by CES, ranging from 2,000 g / mol to strictly less than 100,000 g / mol, prepared by a polymerization reaction, in the presence of at least one initiator compound, of at least one compound (a2) chosen from acrylic acid, methacrylic acid, an oligomer of acrylic acid, an oligomer of methacrylic acid, an acrylic acid salt, a methacrylic acid salt, an oligomer salt of acrylic acid, a methacrylic acid oligomer salt, and combinations thereof, and - at least one material E comprising carbon particles, then * the application of the electro-active composition, * drying and then calendering of the metal substrate bearing the primer layer and the electro-active coating.
Citation Information
Patent Citations
Conductive binder and preparation method thereof, current collector, electrode and battery
CN115881966A
Method for manufacturing a positive electrode sheet for a lithium ion secondary battery and a positive electrode sheet for a lithium ion secondary battery
US20170018770A1
KR20190143256A