Methods for extending the service life of depleted SCR catalyst beds in NOx stationary source exhaust systems.
Patent Information
- Application Number
- JP2019528667
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2016-12-01
- Filing Date
- 2017-11-29
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2037-11-29
AI Technical Summary
The degradation of selective catalytic reduction (SCR) catalyst beds in NOx exhaust systems of stationary sources leads to increased ammonia slip and operating costs, necessitating frequent replacement, which is economically inefficient and environmentally undesirable.
Retrofitting an ammonia slip catalyst (ASC) downstream of the degraded SCR catalyst bed to extend its service life, converting ammonia to nitrogen and water, thereby reducing ammonia slip and maintaining compliance with emission standards.
The service life of the SCR catalyst is extended up to two times, reducing replacement costs and ammonia emissions, promoting sustainable resource use and maintaining efficient power generation.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Disclosure of the Invention]
[0001] The present invention relates to a method for extending the service life of a degraded selective catalytic reduction bed in an exhaust system for a stationary NOx pollution source.
[0002] Modern power generators fueled by natural gas, light fractions, or synthesis gas (e.g., coal-derived) operate a combined-cycle gas turbine where the gas is burned in a gas turbine to generate electricity in the first cycle, and the heat generated from the combustion of the gas is recovered in a steam-operated heat engine in the second cycle. This combination of two cycles improves the net overall efficiency of the system. The second cycle is carried out in what is usually known as a heat recovery steam generator (HRSG) system, which also typically includes catalytic components to process components in the exhaust gas resulting from the combustion of the gas in the first cycle, including nitrogen oxides (NOx), carbon monoxide (CO), and unburned hydrocarbons (HC). The catalytic activity of these catalytic components is enhanced by the transfer of heat from the exhaust gas being processed to the catalytic components themselves. The position of the catalytic components in the HRSG system can be selected for temperature-optimized catalytic activity.
[0003] NOx emissions from stationary pollution sources, primarily power plants, industrial heaters, cogeneration plants, such as wood-burning boilers, stationary diesel and gas engines, marine propulsion systems, diesel locomotives, industrial and municipal waste incinerators, chemical plants, and glass, steel, and cement manufacturing plants, are a major environmental problem. NOx causes ozone formation in the troposphere, acid rain formation, and problems with the human respiratory system. NOx is thermally produced during combustion processes by the combination of N2 and O2 present in the air. At temperatures exceeding approximately 1500°C, this reaction proceeds at considerable speed through a well-characterized mechanism called the Zeldovich mechanism.
[0004] To meet NOx emission standards set by various regulatory authorities, exhaust (flue) gas aftertreatment methods are required. Among such aftertreatment methods, selective catalytic reduction (SCR) is the most well-developed and widely used method globally for controlling NOx emissions from stationary pollutants due to its efficiency, selectivity (to N2 products), and economics. The SCR reaction generally consists of the reduction of NOx by ammonia (NH3), forming water and nitrogen.
[0005] The main reactions involved in the reduction of NOx in SCR are shown in reactions (1), (2), and (3): 4NO+4NH3+O 2 → 4N2 + 6H2O (1) 6NO2 + 8NH3 → 7N2 + 12H2O (2) NO + NO2 + 2NH3 → 2N2 + 3H2O (3)
[0006] Three types of catalysts have been developed to promote reactions (1) to (3): noble metals, metal oxides, and metal-promoting zeolites. Noble metal SCR catalysts can unnecessarily accelerate SO2 oxidation at temperatures above approximately 200°C, and are therefore primarily considered for low-temperature and natural gas applications.
[0007] Among the various metal oxide SCR catalysts developed for 300-400°C applications, vanadia supported on anatase-type titania and promoted with tungsten or molybdenum was found to resist sulfation and exhibit low activity in the SO2 oxidation reaction.
[0008] Mordenite is a commercially available zeolite SCR catalyst for treating NOx emissions from stationary pollution sources (see RH Heck et al., “Catalytic Air Pollution Control - Commercial Technology”, 3rd edition (2009), John Wiley & Sons, Inc., Hoboken, New Jersey). See Chapter 12 in particular.
[0009] Fe-enhanced zeolite catalysts have been proposed primarily for use in SCRs for gas combustion cogeneration plants at high temperatures, i.e., up to 600°C, where metal oxide catalysts can be thermally unstable.
[0010] Commercially available SCR catalysts are arranged as a coating on an extruded honeycomb monolith, plate, or inert honeycomb monolith.
[0011] For a more complete explanation of the rationale for applying the SCR method to stationary sources of NOx emissions, see P. Forzatti, App. Cat A: General 222 (2001) 221-236.
[0012] Reaction (3) is preferred because it is known to be a relatively fast reaction compared to either reaction (1) or especially reaction (2). For this purpose, a suitable oxidation catalyst placed upstream of the SCR catalyst is also relevant to treating the CO and HC components in the exhaust gas. The injection of reducing agents upstream of the SCR catalyst is generally carried out downstream of the oxidation catalyst to avoid inefficient consumption of ammonia (by oxidation to NOx), which would result in a decrease in the overall conversion performance of the system. Ammonia injection can be carried out via a suitable device such as an ammonia injection grid (AIG).
[0013] While any of the above SCR catalysts can be used to treat NOx in an HRSG system, the gas combustion exhaust gas temperature generally requires that the above metal oxides or metal-enhanced zeolites be suitable.
[0014] Gas turbine emission control systems typically include a CO oxidation catalyst (CO-Ox), followed by an ammonia injection grid (AIG), and finally a SCR catalyst bed (SCR). As the catalyst system degrades, the CO conversion rate decreases, and SCR performance deteriorates. To maintain the overall NOx emissions of the system below a predetermined minimum, plant operators increase the ammonia:NOx ratio to keep reactions (1), (2), and (3) running. However, this increases ammonia emissions ("slip") and increases operating costs through the consumption of reducing agents. Ammonia slip refers to the emission of unreacted ammonia resulting from the incomplete reaction of NOx and reducing agents. Ammonia slip can lead to the formation of ammonium sulfate, which can clog or corrode downstream components and contribute undesirable particulate matter (PM2.5) emissions into the atmosphere. In the United States, permissible ammonia slip levels are typically between 2 and 10 ppm.
[0015] Ultimately, the SCR catalytic activity degrades to the point where it can no longer increase the ammonia:NOx ratio without exceeding a predetermined maximum value. At this point, the typical practice is to remove and dispose of the spent catalyst and replace it with a new one so that the system can continue to comply with emission standards.
[0016] The inventors have found, to their great surprise, that the ability of a late-life SCR catalyst bed in a gas turbine exhaust system to treat NOx to within the violation limit can be extended by 50% without exceeding the violation NH3 slip limit by retrofitting an ammonia slip treatment catalyst (referred to here as an ammonia slip catalyst or "ASC") downstream of the late-life SCR catalyst bed, which is more economical than replacing the late-life SCR catalyst itself. This discovery has considerable advantages, as it allows the benefits to be obtained using a relatively small catalyst volume compared to the SCR catalyst bed volume, resulting in negligible additional back pressure added to the system and thus having no significant impact on the overall power generation efficiency.
[0017] According to one aspect, the present invention is NO xIn an exhaust gas aftertreatment system for a stationary pollution source, the exhaust gas discharged from the system to the atmosphere continuously meets the violation limit for both NO x and ammonia emissions. In a method for extending the service life of a deteriorated selective catalytic reduction (SCR) catalyst bed that catalyzes the conversion of nitrogen oxides (NO x ) to dinitrogen (N2) in the presence of a nitrogen-containing reducing agent, downstream of the deteriorated SCR catalyst bed, a honeycomb substrate monolith or plate-type substrate containing a catalyst for converting ammonia in the exhaust gas containing oxygen into nitrogen and water is retrofitted. The kNO x of the honeycomb substrate monolith containing a catalyst for converting ammonia in the exhaust gas containing oxygen into nitrogen and water is about 80 m / hr or more between about 250 °C and about 400 °C, where the kNO x of the catalyst sample deteriorated at 450 °C for 48 hours in 10% H2O (as water vapor) in air is determined by an SCR activity test in a laboratory-scale reactor using a gas composition of 50 ppm CO, 30 ppm NO, 36 ppm NH3, 15% O2, 8% water, 3% CO2, and the balance N2.
[0018] The present invention provides a number of important advantages. The service life of the SCR catalyst can be extended up to twice as long. This promotes the sustainable use of resources in that it is not necessary to recycle or send a relatively large SCR catalyst capacity to a landfill for a significant period of time.
[0019] In practice, a relatively small-capacity retrofitted honeycomb substrate monolith or plate-type substrate containing a catalyst for converting ammonia in the exhaust gas containing oxygen into nitrogen and water is just one of the factors that enables the production of the retrofit catalyst at a cost lower than the cost of replacing the SCR catalyst. The cost of the retrofit catalyst can be 20% or more lower than the SCR catalyst replacement cost.
[0020] The ammonia slip catalyst is selectively designed to promote the following overall reaction: 4NH3 + 3O2 → 2N2 + 6H2O (4)
[0021] As described in further detail below, U.S. Patent Application Publication Nos. 2007 / 0110643 A1, 2016 / 0245139 A1, and 2016 / 0256823 A1 propose the use of an ammonia slip catalyst (also known as an ammonia oxidation (“AMOX”) catalyst) downstream of, or in combination with, an SCR catalyst in an exhaust system of a gas turbine engine.
[0022] However, as described above, an SCR catalyst bed can convert NOx with very little ammonia slip, and in any case, releasing relatively low levels of ammonia to the atmosphere is permitted, so power plant operators generally do not include an ammonia slip catalyst downstream of a newly installed SCR catalyst bed. Therefore, adding an ammonia slip catalyst to the systems proposed by these publications is unnecessary and unduly increases the economic cost and burden on the plant operator installing the system.
[0023] U.S. Patent Application Publication No. 2007 / 0110643 A1 discloses an exhaust gas treatment device for reducing the concentrations of NOx, HC, and CO in an exhaust gas stream such as generated by a gas turbine engine of a power plant. The treatment device includes a multifunctional catalyst component having an upstream reduction-only portion and a downstream reduction-oxidation portion disposed downstream of an ammonia injection device. By injecting ammonia in excess of the stoichiometric concentration, selective catalytic reduction (SCR) of NOx is promoted in the upstream portion of the catalyst component, and the resulting ammonia slip is oxidized in the downstream portion of the catalyst component. Any additional NOx generated by the oxidation of ammonia is further reduced in the downstream portion before being sent to the atmosphere.
[0024] U.S. Patent Application Publication 2016 / 0245139A1 discloses an exhaust system for a power generator having a heat source for generating electricity by burning fuel in air, the exhaust system being configured to receive flowing exhaust gases and comprising a catalytic system for processing the exhaust gases, the catalytic system comprising a primary oxidation catalyst and a secondary catalyst, the primary oxidation catalyst being positioned downstream of the heat source such that the flowing exhaust gases come into contact with the primary oxidation catalyst before the secondary catalyst.
[0025] U.S. Patent Application Publication 2016 / 0256823A1 discloses a system including a nitrogen oxide reduction catalyst fluidly connected to the exhaust conduit of an engine system. The nitrogen oxide reduction catalyst is configured to reduce nitrogen oxides in the engine exhaust. The system also includes an ammonia oxidation catalyst fluidly connected to the exhaust conduit downstream of the nitrogen oxide reduction catalyst and configured to reduce ammonia in the engine exhaust. Furthermore, the system includes a reducing agent injection control system configured to control the injection of a reducing agent into the exhaust conduit, determine the primary nitrogen oxide conversion rate of the nitrogen oxide reduction catalyst, determine the ammonia storage value of the nitrogen oxide reduction catalyst, and determine the primary temperature of the engine exhaust upstream of the ammonia oxidation catalyst. The reducing agent injection control system is also configured to increase or decrease the injection of the reducing agent based on the primary nitrogen oxide conversion rate, the ammonia storage value, and the primary temperature.
[0026] U.S. Patent No. 7,727,499 discloses a method for removing excess ammonia (NH3) gas ("ammonia slip") from flue gas and exhaust gas subjected to selective catalytic reduction (SCR) for the reduction of nitrogen oxides (NOx) by ammonia by oxidation. More specifically, the method uses an ammonia oxidation catalyst consisting of zeolite, one or more noble metals, and base metal compounds to catalyze the oxidation of both ammonia and carbon monoxide (CO) while minimizing the generation of nitrogen oxides (NOx).
[0027] The rate constant kNOx is defined as follows: Rate constant (kNO x (m / hr))=-area velocity (Av (m / hr) × ln(1 - NO x Conversion rate / 100)) Here, the area velocity A v (m / hr) = Q (volume flow rate (m 3 / hr)) / A cat (catalyst surface area (m 2 ))).
[0028] From these equations, it can be seen that the kNO of the catalyst x constant does not depend on the pitch (or cells per square inch) of the honeycomb substrate monolith or plate - type substrate, and thus also does not depend on the volume of the honeycomb substrate monolith or plate - type substrate.
[0029] In practice, a catalyst for converting ammonia in exhaust gas containing oxygen into nitrogen and water, i.e., an ammonia slip catalyst (ASC), desirably has as low a pressure loss as economically possible. This is because adding an ASC to a system results in an additional pressure loss compared to a system containing only an SCR catalyst, and an additional energy input is required to address this. This additional energy input can be important for gas - turbine power generation as the additional energy requirements within the system can potentially reduce the efficiency of the overall power generation cycle.
[0030] An important component of the pressure loss is the depth of the ASC bed. The depth of the ASC bed can be affected, for example, by the operating temperature, kNOx of the substrate monolith constituting the ASC, and the pitch (or honeycomb cell density). Therefore, for example, at a fixed ASC pitch, by reducing kNOx, a more geometric ASC surface area - and thus the substrate monolith volume and the resulting increased back pressure - is required for compensation.
[0031] Similarly, by reducing the pitch of the ASC substrate monolith, an increased catalyst volume will be required to compensate for and maintain a fixed kNOx.
[0032] Therefore, there should be a balance to be determined among at least the pitch of the substrate monolith, the volume of the substrate monolith, the geometric surface area of the substrate monolith, and the composition of the ASC, according to the position of the ASC within the system and the temperature of the catalyst in use. The selection of those parameters can be determined based on cost and operational considerations and is comprehensively encompassed by kNOx.
[0033] The kNO of a honeycomb substrate monolith or plate-type substrate containing a catalyst x can be 300 m / hr or less.
[0034] Preferably, the kNOx of a honeycomb substrate monolith or plate-type substrate containing a catalyst is about 90 < kNOx < about 300 m / h between about 300 and about 400 °C.
[0035] The catalyst for converting ammonia in the exhaust gas containing oxygen into nitrogen and water preferably converts about 70% of NH3 at 250 °C or higher, more preferably > about 80% of NH3 at about 300 °C or higher.
[0036] The catalyst for converting ammonia in the exhaust gas containing oxygen into nitrogen and water preferably has < about 20% sNOx = NOx out divided by (NH3in - NH3out) at less than about four hundred, more preferably < about 10% sNOx at less than about 350 °C, where sNOx is determined using the same conditions as those defined for determining the above kNOx.
[0037] The space velocity at which the exhaust gas contacts the post-attached catalyst for converting ammonia in the exhaust gas containing oxygen into nitrogen and water is 50,000 - 500,000 h -1 , for example, 100,000 - 400,000 h -1 or 150,000 h -1 ~350,000 h -1 can be.
[0038] A retrofit catalyst for converting ammonia in oxygen-containing exhaust gas to nitrogen and water preferably comprises a platinum group metal supported on a refractory oxide carrier and a selective catalytic reduction catalyst.
[0039] The platinum group metals in platinum group metals supported on a refractory oxide support are approximately 1 to 40 g / ft 3 Preferably about 1 to 25 g / ft 3 Or approximately 1 to 10 g / ft 3 The mixture is filled to this extent. A small amount of platinum group metal is preferable because such a small amount promotes selectivity for reaction (4).
[0040] The SCR catalyst in an add-on catalyst for converting ammonia in oxygen-containing exhaust gas to nitrogen and water may include (i) vanadium supported on anatase-type titania and promoted with tungsten or molybdena; (ii) a metal-promoted molecular sieve; or (iii) a mixture of vanadium supported on anatase-type titania and promoted with tungsten or molybdena and a metal-promoted molecular sieve.
[0041] When the SCR catalyst in an add-on catalyst for converting ammonia in oxygen-containing exhaust gas to nitrogen and water includes a metal-promoted molecular sieve, the molecular sieve is preferably an aluminosilicate zeolite.
[0042] Preferably, when the SCR catalyst in an add-on catalyst for converting ammonia in oxygen-containing exhaust gas to nitrogen and water includes a metal-promoted molecular sieve, the molecular sieve has a maximum ring size of eight tetrahedral atoms and is more preferably selected from the group consisting of framework type codes CHA, AEI, and AFX. Aluminosilicate zeolites that are particularly resistant to hydrothermal degradation and hydrocarbon "coking" have a maximum ring size of eight tetrahedral atoms and are referred to in the art as "small-pore" zeolites. Zeolites are classified by the International Zeolite Association according to the type of framework they have. However, in certain applications where long-term durability is not a primary requirement, for example in relatively low-temperature applications, "medium-pore" zeolites, such as those with framework type codes MFI or FER, or "large-pore" zeolites, such as BEA or MOR, may also be applicable.
[0043] The silica-to-alumina ratio (SAR) of the zeolite can be any suitable SAR to promote reactions (1), (2), and (3). Generally, this is a balance between the desirable thermal stability of a relatively high silica content and the desirable ion-exchange transition metal-facilitating effect of a relatively high alumina content. In practice, the selected SAR may depend on the framework type code of the zeolite, but is typically in the range of about 10 to about 256, with SARs of about 15 to about 40 being preferred for small-pore zeolites such as CHA, AEI, and AFX.
[0044] Preferably, the metal in the metal-enhanced molecular sieve is copper and / or iron.
[0045] In retrofit catalysts for converting ammonia in oxygen-containing exhaust gases to nitrogen and water, the refractory oxide support for platinum group metals in the SCR catalyst may be silica-doped alumina, titania, or optionally doped zirconia.
[0046] In an add-on catalyst for converting ammonia in oxygen-containing exhaust gas to nitrogen and water, the honeycomb-based monolith or plate-type substrate in the SCR catalyst has an axial length and may be coated with a first wash coat layer containing platinum group metals supported on a refractory oxide carrier and a second wash coat layer containing the SCR catalyst.
[0047] The first wash coat layer may be located in a first zone coated from the first end of the honeycomb substrate monolith, and the second wash coat layer may be located in a second zone coated from the second end of the honeycomb substrate monolith or plate-type substrate, with the second layer located upstream of the first layer.
[0048] Alternatively, the first zone may be smaller than the axial length of the honeycomb substrate monolith or plate-type substrate, and the second layer of the second zone may at least partially cover the first layer. In this case, preferably, the second layer may extend along the entire axial length of the honeycomb substrate monolith or plate-type substrate.
[0049] Alternatively, the first layer may extend along the entire axial length of the honeycomb monolith or plate-type substrate, and the second layer may cover the first layer and also extend along the entire axial length of the honeycomb monolith or plate-type substrate.
[0050] Preferably, the violation limit for NOx emissions in the method according to the present invention is 2 ppm or less, and / or the violation limit for ammonia emissions is 10 ppm or less, for example, less than 5 ppm or less than 2 ppm.
[0051] The temperature at which the exhaust gas comes into contact with the SCR catalyst bed can range from approximately 200°C to approximately 450°C.
[0052] The nitrogen-containing reducing agent is ammonia (NH3) itself, hydrazine, or any suitable ammonia precursor, such as urea ((NH2)2CO), ammonium carbonate, ammonium carbamate, ammonium bicarbonate, or ammonium formate. It is important that the mixing of ammonia with the exhaust gas is carried out as completely as possible before the exhaust gas / ammonia enters the SCR catalyst. This can be done using various baffles and static mixers, for example, with herringbone and skew channel shapes, as needed, provided that they do not significantly contribute to an increase in back pressure. Good mixing of ammonia with the exhaust gas can be facilitated by complete two-dimensional coverage of the reducing agent injection across the duct carrying the exhaust gas. Such arrangements are known in the art as ammonia injection grids (AIGs).
[0053] To facilitate reaction (3) (and further reactions (1) and (2)), the alpha ratio of ammonia molecules to NOx molecules used in the reaction is preferably about 0.90 to about 2.00, preferably < about 1.8, for example, about 0.95 to about 1.5 or 1.00 to about 1.20.
[0054] The SCR catalyst may be in the form of a wash coat coated onto a substrate such as an inert ceramic honeycomb monolith or a metal monolith formed from cordierite, or it may be prepared as an extruded honeycomb, where the catalyst is mixed with a paste of binder (or matrix) components and then extruded into a desired shape having channels extending through it. The zeolite-containing wash coat composition used in the present invention for coating onto a monolithic substrate or for the manufacture of an extruded substrate monolith may contain a binder selected from the group consisting of alumina, silica, (non-zeolite) silica-alumina, naturally occurring clay, TiO2, ZrO2, and SnO2.
[0055] In particular, an SCR catalyst may be any of those described for use as a catalyst for converting ammonia in exhaust gas, which also contains oxygen, into the nitrogen and water mentioned above, namely one of the following: (i) vanadium supported on anatase-type titania and enhanced with tungsten or molybdenum; (ii) Metal-enhanced molecular sieves; or (iii) A mixture of vanadium supported on anatase-type titania and tungsten or molybdenum-enhanced vanadium and a metal-enhanced molecular sieve.
[0056] The method according to the present invention can be used to treat exhaust gases from any stationary pollution source of NOx emissions. In particular, the exhaust gases may be products of power plants, industrial heaters, cogeneration power plants, combined cycle power plants, wood-burning boilers, stationary diesel engines, stationary natural gas combustion engines, marine propulsion engines, diesel locomotives, industrial waste incinerators, municipal solid waste incinerators, chemical plants, glass manufacturing plants, steel manufacturing plants, or cement manufacturing plants.
[0057] In preferred applications, the exhaust gas is a product of a cogeneration plant, preferably a stationary natural gas combustion engine.
[0058] Preferably, the exhaust gas aftertreatment system includes a heat recovery steam generator (HRSG).
[0059] The term “contains” as used herein can be replaced with the definitions “essentially from” or “consisting of.” The term “contains” is intended to mean that the specified elements are essential, but other elements may be added to still form the components within the claims. The term “essentially from” limits the claims to the specified materials or processes, and to those that do not substantially affect the basic and novel features of the claimed invention. The term “consisting of” closes the claim to the inclusion of materials other than those described, excluding impurities that normally accompany them.
[0060] To avoid misunderstanding, the entire content of all cited literature is incorporated herein with proper attribution. [Brief explanation of the drawing]
[0061] A conventional HRSG exhaust system for a gas turbine, including an SCR catalyst, is shown in Figure 1, and the system is adapted to the method according to the present invention by inserting an ammonia slip catalyst downstream of the SCR catalyst at the position illustrated in Figure 2. Figures 1 and 2 require no explanation.
[0062] To allow for a more thorough understanding of the present invention, the following embodiments are provided only as examples. [Examples]
[0063] [Example 1] A double-layer ammonia slip catalyst (ASC) was prepared on a 230-cell / square-inch (cpsi) ceramic honeycomb substrate monolith with a cell wall thickness of 7 mil (1 / 1000 inch). The first (lower) layer was directly coated onto the substrate, which had a continuous alumina wash coat layer along the entire axial length of the substrate. The resulting coated parts were dried and calcined. Next, 5 g / ft of Pt was added from a platinum nitrate solution. 3 The wash coat alumina layer was impregnated until the Pt content reached the required amount. The resulting parts were then dried and calcined. Finally, a second wash coat layer containing Cu-impregnated CHA zeolite mixed with a binder was applied in a continuous layer covering 100% of the Pt alumina layer along the entire axial length of the substrate, and the resulting parts were then dried and calcined. Cylindrical cores with a diameter of 2 inches and a length of 3.3 inches were cut from the finished honeycomb substrate monolith coated with double-layer ASC.
[0064] [Example 2 (SCR test)] The cylindrical ASC core from Example 1 was degreened at 450°C for 48 hours in 10% H2O (as water vapor) in air, and then its SCR activity was tested in a laboratory-scale reactor. The gas composition supplied to the catalyst for the activity test was 50 ppm CO, 30 ppm NO, 36 ppm NH3, 15% O2, 8% water, 3% CO2, and the remainder N2. The conversion rates of CO, NOx, and NH3 were measured while the reactor was maintained at a steady-state temperature in the range of 200–450°C. The gas space velocity per hour (GHSV) relative to the ASC volume was 180,000 hr. -1 That was the case.
[0065] Table 1 shows the conversion rates of CO, NOx, and NH3 for various temperatures. The kNOx, defined as kNOx = -(area velocity) × ln(1-NOx conversion rate / 100), is also shown.
[0066] [Example 3 (NH3 oxidation test)] The cylindrical ASC core from Example 1 was degreened in 10% H2O air at 450°C for 48 hours, and then its NH3 oxidation activity was tested in a laboratory-scale reactor. The gas composition supplied to the catalyst was 50 ppm CO, 30 ppm NH3, 10% O2, 4% water, 3% CO2, and the remainder N2. The conversion rates of CO, NOx, and NH3 were measured while the reactor was maintained at a steady-state temperature in the range of 200–450°C. The gas space velocity per hour (GHSV) relative to the ASC volume was 120,000 hr. -1 That was the case.
[0067] The results, including the CO conversion rate and NH3 conversion rate, are shown in Table 2. sNOx, defined as (NOxout divided by (NH3in - NH3out)), is also shown.
[0068] [Example 4 (SCR test with high ammonia-to-NOx ratio (ANR))] The cylindrical ASC core from Example 1 was degreened in 10% H2O air at 450°C for 48 hours, and then its SCR activity was tested in a laboratory-scale reactor. The gas composition supplied to the catalyst for the activity test was 50 ppm CO, 30 ppm NO, 54 ppm NH3, 15% O2, 8% water, 3% CO2, and the remainder N2. The conversion rates of CO, NOx, and NH3 were measured while the reactor was maintained at a steady-state temperature in the range of 200–450°C. The gas space velocity per hour (GHSV) relative to the ASC volume was 180,000 hr. -1 That was the case.
[0069] Table 1 shows the CO conversion rates, NOx conversion rates, and NH3 conversion rates for various temperatures. The kNOx, defined as kNOx = -(area velocity) × ln(1-NOx conversion rate / 100), is also shown.
Claims
1. NO x In an exhaust gas aftertreatment system for a fixed pollution source, the exhaust gas discharged from the system to the atmosphere is NO x In order to maintain emissions of both nitrogen oxides (NO2) and ammonia below regulated limits, the x ) to dinitrogen (N 2 1. A method for extending the useful life of a depleted selective catalytic reduction (SCR) catalyst bed which catalyzes the conversion of CO to CO, comprising: downstream of the depleted SCR catalyst bed, retrofitting a honeycomb substrate monolith or plate-type substrate containing a retrofit catalyst for converting ammonia in an oxygen-containing exhaust gas to nitrogen and water; the retrofit catalyst for converting ammonia in an oxygen-containing exhaust gas to nitrogen and water comprises a platinum group metal and a selective catalytic reduction catalyst supported on a refractory oxide support; The platinum group metal supported on the refractory oxide support is 35 to 1413 g / m 3 (1-40g / ft 3 ) is filled, The process wherein the SCR catalyst in said retrofit catalyst is either vanadia supported on anatase form of titania and promoted with tungsta or molybdena, or a metal promoted molecular sieve.
2. 2. The method of claim 1, wherein the molecular sieve has a framework type code that is CHA, AEI, AFX, BEA, MOR, MFI or FER.
3. 3. The method of claim 1 or 2, wherein a honeycomb substrate monolith or a plate-shaped substrate has an axial length and is coated with a first washcoat layer comprising a platinum group metal supported on a refractory oxide support and a second washcoat layer comprising an SCR catalyst.
4. 4. The method of claim 3, wherein a honeycomb substrate monolith is retrofitted, a first washcoat layer is disposed in a first zone coated from a first end of the honeycomb substrate monolith, a second washcoat layer is disposed in a second zone coated from a second end of the honeycomb substrate monolith, and the second layer is disposed upstream from the first layer.
5. 5. The method of claim 4, wherein the first zone is smaller than an axial length of the honeycomb substrate monolith and the second layer of the second zone at least partially covers the first layer.
6. The method of claim 4 , wherein the second layer extends the entire axial length of the honeycomb substrate monolith.
7. 4. The method of claim 3, wherein the first layer extends the entire axial length of the honeycomb substrate monolith and the second layer covers the first layer and extends the entire axial length of the honeycomb substrate monolith.
8. The method of claim 1 or 2, wherein the retrofit catalyst comprises an SCR catalyst, and the SCR catalyst in the retrofit catalyst is a washcoat coated on a substrate or is a component of an extruded honeycomb body.
9. The SCR catalyst in the retrofit catalyst, (i) Vanadia supported on titania in the anatase form and promoted with tungsta or molybdena; (ii) a metal promoted molecular sieve; or (iii) Mixtures of vanadia and metal promoted molecular sieves supported on titania in the anatase form and promoted with tungsta or molybdena. The method of claim 8, wherein the
10. The rate constant kNO of the honeycomb substrate monolith containing the retrofit catalyst for converting ammonia in an oxygen-containing exhaust gas to nitrogen and water. x is about 80 m / hr or more between about 250 and about 400° C., where 10% H 2 The kNO of the retrofit catalyst sample aged in air containing O (as water vapor) at 450° C. for 48 hours x 50 ppm CO, 30 ppm NO, 36 ppm NH 3 , 15% O 2 , 8% water, 3% CO 2 , remainder N 2 was determined by SCR activity testing in a laboratory-scale reactor using a gas composition of x teeth: Rate constant (kNO x )=-area velocity (A v (m / hr))×ln(1-NO x Conversion rate / 100) [wherein the areal velocity A v (m / hr) = Q (volume flow rate (m 3 / hr)) / A cat (Catalyst surface area (m 2 )) 10. The method of any one of claims 1 to 9, wherein the honeycomb substrate monolith is coated with a first washcoat layer extending the entire axial length of the honeycomb substrate monolith and a second washcoat layer overlying the first layer and extending the entire axial length of the honeycomb substrate monolith, the first washcoat layer comprising alumina and the second washcoat layer comprising copper impregnated CHA zeolite mixed with a binder.