Secondary battery and electronic apparatus

JP2022070247A5Inactive Publication Date: 2024-10-24SEMICON ENERGY LAB CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021174836
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-03-22
Filing Date
2021-10-26
Publication Date
2024-10-24
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries face challenges in maintaining charging and discharge capacity, cycle characteristics, reliability, and safety, particularly due to the collapse of the crystal structure of the positive electrode active material during repeated charging and discharging.

Method used

A positive electrode active material with a specific crystal structure, such as a layered rock-shaped structure, is developed using a composite oxide with additives like magnesium and fluorine, which stabilizes the crystal structure even at high charging depths, ensuring minimal volume change and maintaining capacity.

Benefits of technology

The solution provides a secondary battery with enhanced charging and discharge capacity, improved cycle characteristics, and increased safety by preventing the collapse of the crystal structure, even under high charging voltages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a secondary battery and an electronic apparatus, and a secondary battery with high safety or reliability.SOLUTION: A secondary battery includes a positive electrode active material with a broad peak at or around 4.55 V in a dQ / dVvsV curve when charging depth is increased. Alternatively, the secondary battery includes a positive electrode active material that can maintain a crystal structure in which the deviation of a CoO2 is suppressed and the H1-3 crystal structure is not formed even if the charging voltage is 4.6 V or more and 4.8 V or less and the charging depth is 0.8 or more and less than 0.9. When the peak at or around 4.55 V is broad in the dQ / dVvsV curve, it means that the change of energy required in the lithium extraction at or around this value is small and the change in crystal structure is small. Therefore, the positive electrode active material that is not much influenced by the volume change or the deviation of the CoO2 layer and that is relatively stable even when the charging depth is high can be obtained.SELECTED DRAWING: Figure 57
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] One aspect of the present invention relates to a product, a method, or a method of manufacture. Alternatively, the present invention relates to a process, a machine, a manufacture, or a composition of matter. Another aspect of the present invention relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, or a method of manufacturing the same.

[0002] In this specification, "electronic equipment" refers to all devices that have an energy storage device, and all electro-optical devices with an energy storage device, information terminal devices with an energy storage device, etc., are considered electronic equipment. [Background technology]

[0003] In recent years, there has been a great deal of development on various energy storage devices, including lithium-ion secondary batteries, lithium-ion capacitors, air batteries, and all-solid-state batteries. In particular, the demand for lithium-ion secondary batteries, which offer high output and high capacity, has expanded rapidly in line with the development of the semiconductor industry, and they have become indispensable as a source of rechargeable energy in today's information society.

[0004] In particular, there is a high demand for secondary batteries for mobile electronic devices that have a large discharge capacity per unit weight and excellent cycle characteristics. To meet these demands, there is a great deal of research being done on improving the positive electrode active material of secondary batteries (for example, Patent Documents 1 to 3). Research is also being conducted on the crystal structure of positive electrode active materials (Non-Patent Documents 1 to 3).

[0005] X-ray diffraction (XRD) is also one of the techniques used to analyze the crystal structure of positive electrode active materials. By using ICSD (Inorganic Crystal Structure Database), which is introduced in Non-Patent Document 4, XRD data can be analyzed. [Prior art documents] [Patent Documents]

[0006]

Patent Document 1

Patent document 2

Patent document 3

Non-licensed literature

[0007]

Non-licensed literature 1

Non-licensed Document 2

Non-licensed Document 4

[0008] Lithium-ion secondary batteries and the cathode active materials used in them still have room for improvement in various aspects, such as charge / discharge capacity, cycle characteristics, reliability, safety, and cost.

[0009] One aspect of the present invention aims to provide a positive electrode active material or composite oxide that can be used in lithium-ion secondary batteries and in which the decrease in charge / discharge capacity during charge / discharge cycles is suppressed. Alternatively, one aspect of the present invention aims to provide a positive electrode active material or composite oxide that does not easily collapse in crystal structure even after repeated charge / discharge cycles. Alternatively, one aspect of the present invention aims to provide a positive electrode active material or composite oxide with a large charge / discharge capacity. Alternatively, one aspect of the present invention aims to provide a secondary battery that is safe or highly reliable.

[0010] Furthermore, one aspect of the present invention aims to provide a positive electrode active material, a composite oxide, an energy storage device, or a method for producing the same.

[0011] Furthermore, the description of these problems does not preclude the existence of other problems. Moreover, one aspect of the present invention does not need to solve all of these problems. It is possible to extract other problems from the description, drawings, and claims. [Means for solving the problem]

[0012] To solve the above problems, one aspect of the present invention provides a positive electrode active material having a broad peak around 4.55V in the dQ / dVvsV curve as the depth of charge increases. The broadness of this peak indicates that the change in energy required for lithium extraction in this region is small and the change in crystal structure is small. Therefore, the effects of shift and volume change of the CoO2 layer are small, and a relatively stable positive electrode active material can be obtained even at high depths of charge.

[0013] Alternatively, in one aspect of the present invention, a positive electrode active material is provided that does not form an H1-3 type crystal structure and maintains a crystal structure in which the displacement of the CoO2 layer is suppressed, even when the charging voltage is 4.6V or more and 4.8V or less and the charging depth is 0.8 or more and less than 0.9.

[0014] More specifically, one aspect of the present invention is a secondary battery having a positive electrode, wherein the positive electrode is used as the positive electrode, lithium metal is used as the negative electrode, and when the battery is manufactured using 1 mol / L lithium hexafluoride phosphate and a mixture containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7 and 2 wt% vinylene carbonate as the electrolyte, the dQ / dVvsV curve obtained by differentiating the capacity (Q) with respect to voltage (V) (dQ / dV), measured when the battery is charged to 4.9V at 10mA / g in a 25°C environment, has a peak in the range of 4.5V to 4.6V, and the full width at half maximum of the peak is 0.10 or more.

[0015] Furthermore, one aspect of the present invention is a secondary battery having a positive electrode, wherein the positive electrode is used as the positive electrode, lithium metal is used as the negative electrode, and when the battery is manufactured using 1 mol / L lithium hexafluoride phosphate and a mixture containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7 and 2 wt% vinylene carbonate as the electrolyte, the dQ / dVvsV curve obtained by differentiating the capacity (Q) with respect to voltage (V) (dQ / dV) measured when the battery is charged to 4.9V at 10mA / g in a 25°C environment has a first peak in the range of 4.5V to 4.6V, a second peak in the range of 4.15V to 4.25V, and the ratio P1 / P2 of the intensity of the first peak to the intensity of the second peak is 0.8 or less.

[0016] Furthermore, in one aspect of the present invention, a secondary battery having a positive electrode, wherein the positive electrode is used as the positive electrode, lithium metal is used as the negative electrode, and when the battery is manufactured using 1 mol / L lithium hexafluoride phosphate and a mixture containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7 and 2 wt% vinylene carbonate as the electrolyte, the battery is charged to 4.75 V at a constant current of 10 mA / g in a 45°C environment, and then the positive electrode of the battery is analyzed by powder X-ray diffraction using CuKα1 rays in an argon atmosphere, the XRD pattern has diffraction peaks at least at 2θ=19.47±0.10° and 2θ=45.62±0.05°.

[0017] Furthermore, in one aspect of the present invention, a secondary battery having a positive electrode, wherein the positive electrode is used as the positive electrode, lithium metal is used as the negative electrode, and when the electrolyte is made using 1 mol / L lithium hexafluoride phosphate, a mixture containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7, and 2 wt% vinylene carbonate, the battery is charged at a constant current of 100 mA / g to 4.8V in a 25°C environment. After repeating the following cycles four times: constant voltage charging until the voltage reaches 10 mA / g, and constant current discharge at 100 mA / g to 2.5 V, the battery was then charged at a constant current of 10 mA / g to 4.8 V. When the positive electrode of the battery was analyzed by powder X-ray diffraction using CuKα1 rays in an argon atmosphere, the XRD pattern showed diffraction peaks at least at 2θ = 19.47 ± 0.10° and 2θ = 45.62 ± 0.05°, indicating that it is a secondary battery.

[0018] Furthermore, in one aspect of the present invention, in the initial stages of a charge-discharge cycle, the fast-responding resistance component R(0.1s), measured by the current pause method, is lower in the (n+1)th discharge than in the (n)th discharge (where n is a natural number greater than 1), and the discharge capacity in the (n+1)th discharge is higher than that in the (n)th discharge.

[0019] Furthermore, in one aspect of the present invention, in a charge-discharge cycle, a first step is to perform a constant current discharge of 100 mA / g for 5 minutes, and a second step is to perform a pause of 2 minutes without charging or discharging. When the difference between the voltage 0.1 seconds after the start of the second step and the voltage at the end of the first step is divided by the current value, the fast-responding resistance component R(0.1s) has its lowest value before the 10th discharge from the second to the tenth discharge, and has its highest discharge capacity before the 10th discharge from the second to the tenth discharge.

[0020] Furthermore, in the above, it is preferable that the positive electrode active material of the positive electrode has a layered rock salt type crystalline structure.

[0021] Furthermore, in the above, it is preferable that the transition metal M in the positive electrode active material of the positive electrode is cobalt, with a concentration of 90 atomic percent or more.

[0022] Another aspect of the present invention is an electronic device having the secondary battery described above, a display unit, and a sensor. [Effects of the Invention]

[0023] According to one aspect of the present invention, it is possible to provide a positive electrode active material or composite oxide that can be used in lithium-ion secondary batteries and in which the decrease in charge / discharge capacity during charge / discharge cycles is suppressed. Alternatively, it is possible to provide a positive electrode active material or composite oxide that is resistant to crystal structure collapse even after repeated charge / discharge cycles. Alternatively, it is possible to provide a positive electrode active material or composite oxide with a large charge / discharge capacity. Alternatively, it is possible to provide a secondary battery with high safety or reliability.

[0024] Furthermore, according to one aspect of the present invention, a positive electrode active material, an energy storage device, or a method for producing the same can be provided.

[0025] Furthermore, the description of these effects does not preclude the existence of other effects. Moreover, one aspect of the present invention does not necessarily have to possess all of these effects. Other effects will naturally become apparent from the description in the specification, drawings, and claims, and it is possible to extract other effects from the description in the specification, drawings, and claims. [Brief explanation of the drawing]

[0026] [Figure 1] Figure 1 is a diagram illustrating the method for preparing the positive electrode active material. [Figure 2] Figure 2 illustrates the method for preparing the positive electrode active material. [Figure 3] Figures 3(A) to 3(C) illustrate the method for preparing the positive electrode active material. [Figure 4] Figure 4(A) is a cross-sectional view of the positive electrode active material, and Figures 4(B1) to (C2) are partial cross-sectional views of the positive electrode active material. [Figure 5] Figures 5(A1) to 5(B) show the results of calculations regarding the distribution of magnesium and its crystal planes. [Figure 6] Figures 6(A) and 6(B) are cross-sectional views of the positive electrode active material, and Figures 6(C1) and 6(C2) are partial cross-sectional views of the positive electrode active material. [Figure 7] Figure 7 is a cross-sectional view of the positive electrode active material. [Figure 8] Figure 8 is a cross-sectional view of the positive electrode active material. [Figure 9] Figure 9 illustrates the charging depth and crystal structure of the positive electrode active material. [Figure 10] Figure 10 shows the XRD pattern calculated from the crystal structure. [Figure 11] Figure 11 illustrates the charging depth and crystal structure of the positive electrode active material in the comparative example. [Figure 12] Figure 12 shows the XRD pattern calculated from the crystal structure. [Figure 13] Figures 13(A) and 13(B) show the XRD patterns calculated from the crystal structure. [Figure 14]Figures 14(A) to 14(C) show the lattice constants calculated from XRD. [Figure 15] Figures 15(A) through 15(C) show the lattice constants calculated from XRD. [Figure 16] Figure 16 shows an example of a TEM image where the crystal orientation is roughly consistent. [Figure 17] Figure 17(A) is an example of a STEM image where the crystal orientation is roughly consistent. Figure 17(B) is the FFT pattern of the region of the rock salt crystal RS, and Figure 17(C) is the FFT pattern of the region of the layered rock salt crystal LRS. [Figure 18] Figures 18(A) and 18(B) are cross-sectional views of the active material layer when a graphene compound is used as the conductive material. [Figure 19] Figures 19(A) and 19(B) illustrate examples of secondary batteries. [Figure 20] Figures 20(A) through 20(C) illustrate examples of secondary batteries. [Figure 21] Figures 21(A) and 21(B) illustrate examples of secondary batteries. [Figure 22] Figures 22(A) through 22(C) illustrate coin-type rechargeable batteries. [Figure 23] Figures 23(A) through 23(D) illustrate a cylindrical secondary battery. [Figure 24] Figures 24(A) and 24(B) illustrate examples of secondary batteries. [Figure 25] Figures 25(A) through 25(D) illustrate examples of secondary batteries. [Figure 26] Figures 26(A) and 26(B) illustrate examples of secondary batteries. [Figure 27] Figure 27 illustrates an example of a secondary battery. [Figure 28] Figures 28(A) through 28(C) illustrate laminate-type secondary batteries. [Figure 29] Figures 29(A) and 29(B) illustrate laminate-type secondary batteries. [Figure 30]Figure 30 shows the external appearance of a secondary battery. [Figure 31] Figure 31 shows the external appearance of a secondary battery. [Figure 32] Figures 32(A) to 32(C) illustrate the method for manufacturing a secondary battery. [Figure 33] Figures 33(A) through 33(H) illustrate an example of an electronic device. [Figure 34] Figures 34(A) to 34(C) illustrate an example of an electronic device. [Figure 35] Figure 35 illustrates an example of an electronic device. [Figure 36] Figures 36(A) to 36(D) illustrate an example of an electronic device. [Figure 37] Figures 37(A) to 37(C) show examples of electronic devices. [Figure 38] Figures 38(A) to 38(C) illustrate an example of a vehicle. [Figure 39] Figures 39(A) to 39(F) are SEM images of the surface of the positive electrode active material. [Figure 40] Figures 40(A) to 40(H) are SEM images of the surface of the positive electrode active material. [Figure 41] Figures 41(A), 41(B), and 41(D) are cross-sectional STEM images of the positive electrode active material, and Figures 41(C) and 41(E) are FFT patterns. [Figure 42] Figure 42(A) is a cross-sectional STEM image of the positive electrode active material, and Figures 42(B1) to 42(D2) are EDX mapping images. [Figure 43] Figures 43(A1) to 43(A3), 43(B1) to 43(B3), 43(C1), 43(C2-1), 43(C3-1), 43(C2-2), and 43(C3-2) are cross-sectional STEM images of the positive electrode active material. Figures 43(A4) to 43(A6), 43(B4) to 43(B6), 43(C4-1) to 43(C6-1), and 43(C4-2) to 43(C6-2) are EDX mapping images. [Figure 44]Figures 44(A1) to 44(A3), 44(B1) to 44(B3), 44(C1), 44(C2-1), 44(C3-1), 44(C2-2), and 44(C3-2) are cross-sectional STEM images of the positive electrode active material. Figures 44(A4) to 44(A6), 44(B4) to 44(B6), 44(C4-1) to 44(C6-1), and 44(C4-2) to 44(C6-2) are EDX mapping images. [Figure 45] Figures 45(A) and 45(B) show the measured particle size distribution of the positive electrode active material. [Figure 46] Figures 46(A) to 46(C) are SEM images of the surface of the positive electrode active material. [Figure 47] Figures 47(A) to 47(C) are graphs showing the distribution of grayscale values ​​for the positive electrode active material. [Figure 48] Figures 48(A) to 48(C) are luminance histograms of the positive electrode active material. [Figure 49] Figures 49(A) to 49(D) are graphs showing the cycle characteristics of a secondary battery. [Figure 50] Figures 50(A) to 50(D) are graphs showing the cycle characteristics of a secondary battery. [Figure 51] Figures 51(A) to 51(D) are graphs showing the cycle characteristics of a secondary battery. [Figure 52] Figures 52(A) to 52(D) are graphs showing the cycle characteristics of a secondary battery. [Figure 53] Figures 53(A) and 53(B) are graphs showing the cycle characteristics of a secondary battery. [Figure 54] Figure 54(A) is a photograph of an LCO pellet. Figures 54(B) and 54(C) are SEM images of the surface of the cathode active material. [Figure 55] Figure 55(A) is a surface STEM image of the positive electrode active material, and Figure 55(B) is a cross-sectional STEM image of the positive electrode active material. [Figure 56]Figures 56(A1) and 56(B1) are cross-sectional HAADF-STEM images of the positive electrode active material. Figures 56(A2) to 56(A4) and 56(B2) to 56(B4) are EDX mapping images. [Figure 57] Figure 57 shows the dQ / dV vs V curve for a secondary battery. [Figure 58] Figure 58 shows the dQ / dV vs sV curve for a secondary battery. [Figure 59] Figure 59 shows the dQ / dV vs V curve for a secondary battery. [Figure 60] Figure 60 shows the XRD pattern of the positive electrode. [Figure 61] Figures 61(A) and 61(B) are enlarged XRD patterns of a portion of Figure 60. [Figure 62] Figure 62 shows the XRD pattern of the positive electrode. [Figure 63] Figures 63(A) and 63(B) are enlarged XRD patterns of a portion of Figure 62. [Figure 64] Figure 64 shows the XRD pattern of the positive electrode. [Figure 65] Figures 65(A) and 65(B) are enlarged XRD patterns of a portion of Figure 64. [Figure 66] Figure 66 shows the XRD pattern of the positive electrode. [Figure 67] Figures 67(A) and 67(B) are enlarged XRD patterns of a portion of Figure 66. [Figure 68] Figure 68 shows the XRD pattern of the positive electrode. [Figure 69] Figures 69(A) and 69(B) are enlarged XRD patterns of a portion of Figure 68. [Figure 70] Figure 70 shows the XRD pattern of the positive electrode. [Figure 71] Figures 71(A) and 71(B) are enlarged XRD patterns of a portion of Figure 70. [Figure 72] Figure 72 shows the XRD pattern of the positive electrode. [Figure 73] Figures 73(A) and 73(B) are enlarged XRD patterns of a portion of Figure 72. [Figure 74] Figure 74 shows the XRD pattern of the positive electrode. [Figure 75] Figures 75(A) and 75(B) are enlarged XRD patterns of a portion of Figure 74. [Figure 76] Figure 76 shows the XRD pattern of the positive electrode. [Figure 77] Figures 77(A) and 77(B) are enlarged XRD patterns of a portion of Figure 76. [Figure 78] Figure 78 is a diagram relating to powder resistance measurement. [Figure 79] Figure 79 is a graph showing the discharge curve obtained by the current pause method measurement. [Figure 80] Figure 80 shows the analysis method for current pause measurement. [Figure 81] Figures 81(A) and 81(B) show the analysis results of the current pause method measurement. [Figure 82] Figure 82 shows the analysis results of the current pause method measurement. [Modes for carrying out the invention]

[0027] The following describes embodiments for carrying out the present invention with reference to drawings and other illustrations. However, the present invention is not limited to the following embodiments. It is possible to modify the embodiments for carrying out the invention without departing from the spirit of the present invention.

[0028] In this specification, crystal planes and crystal directions are indicated using Miller indices. Individual crystal planes are indicated using parentheses ( ). In crystallography, crystal planes, crystal directions, and space groups are indicated by superscripts above the numbers; however, due to formatting constraints in this specification, a minus sign (-) may be placed before the number instead of a superscript above it.

[0029] In this specification, the theoretical capacity of the positive electrode active material refers to the amount of electricity when all of the insertable and detachable lithium present in the positive electrode active material has been detached. For example, the theoretical capacity of LiCoO2 is 274 mAh / g, the theoretical capacity of LiNiO2 is 274 mAh / g, and the theoretical capacity of LiMn2O4 is 148 mAh / g.

[0030] In this specification, the depth of charge is a value that indicates how much capacity has been charged to the positive electrode active material, relative to its theoretical capacity; in other words, how much lithium has been released from the positive electrode active material. For example, lithium cobalt oxide (LiCoO2) and lithium nickel-cobalt-manganate (LiNi x Co y Mn z In the case of a positive electrode active material with a layered rock salt structure such as O2(x+y+z=1), using the theoretical capacity of 274 mAh / g as a reference, a charge depth of 0 means that no lithium has been detached from the positive electrode, a charge depth of 0.5 means that lithium equivalent to 137 mAh / g has been detached from the positive electrode active material, and a charge depth of 0.8 means that lithium equivalent to 219.2 mAh / g has been detached from the positive electrode active material. a When expressed as CoO2(0≦a≦1), if the charging depth is 0, it is written as LiCoO2 with a=1, and if the charging depth is 0.5, it is written as Li with a=0.5. 0.5 It is labeled as CoO2, and when the charging depth is 0.8, the 'a' value is 0.2 Li. 0.2 It is written as CoO2.

[0031] Furthermore, in this specification, a value in the vicinity of a given numerical value A refers to a value between 0.9 × A and 1.1 × A.

[0032] Furthermore, while this specification and other documents may show an example of a secondary battery using a positive electrode and positive electrode active material according to one aspect of the present invention in which lithium metal is used as the counter electrode, the secondary battery according to one aspect of the present invention is not limited to this. Other materials, such as graphite or lithium titanate, may be used for the negative electrode. The properties of the positive electrode and positive electrode active material according to one aspect of the present invention, such as resistance to crystal structure collapse even after repeated charging and discharging and obtaining good cycle characteristics, are not affected by the material of the negative electrode. Furthermore, while an example of a secondary battery according to one aspect of the present invention may be shown in which charging and discharging is performed at a voltage higher than the typical charging voltage of about 4.7V with a lithium counter electrode, charging and discharging may be performed at a lower voltage. When charging and discharging at a lower voltage, it is expected that the cycle characteristics will be even better than those shown in this specification and other documents.

[0033] Furthermore, unless otherwise specified in this specification, the charging and discharging voltages refer to the voltages when the counter electrode is lithium. However, even with the same positive electrode, the charging and discharging voltages of a secondary battery change depending on the material used for the negative electrode. For example, the potential of graphite is approximately 0.1V (vs Li / Li + Therefore, in the case of a graphite negative electrode, the charge and discharge voltage will be approximately 0.1V lower than in the case of a lithium counter electrode. Furthermore, even if the charging voltage of a secondary battery is, for example, 4.7V or higher in this specification, the plateau region of the discharge voltage does not need to be 4.7V or higher.

[0034] (Embodiment 1) This embodiment describes a method for producing a positive electrode active material, which is one embodiment of the present invention.

[0035] Method for preparing positive electrode active material 1 <Step S11> In step S11 shown in Figure 1(A), lithium sources (Li sources) and transition metal sources (M sources) are prepared as the starting materials, lithium and transition metals, respectively.

[0036] As a lithium source, it is preferable to use a lithium-containing compound, such as lithium carbonate, lithium hydroxide, lithium nitrate, or lithium fluoride. The lithium source should preferably have high purity; for example, a material with a purity of 99.99% or higher is preferable.

[0037] The transition metal M can be selected from elements listed in groups 4 to 13 of the periodic table, for example, at least one of manganese, cobalt, and nickel can be used. The transition metal M may be cobalt only, nickel only, cobalt and manganese, cobalt and nickel, or cobalt, manganese, and nickel. When cobalt only is used, the resulting positive electrode active material contains lithium cobalt oxide (LCO), and when cobalt, manganese, and nickel are used, the resulting positive electrode active material contains nickel-cobalt-lithium manganese oxide (NCM).

[0038] As the transition metal M source, it is preferable to use a compound having the above-mentioned transition metal M. For example, oxides of the metals exemplified above, or hydroxides of the exemplified metals, etc., can be used as the transition metal M. If it is a cobalt source, cobalt oxide, cobalt hydroxide, etc., can be used. If it is a manganese source, manganese oxide, manganese hydroxide, etc., can be used. If it is a nickel source, nickel oxide, nickel hydroxide, etc., can be used. If it is an aluminum source, aluminum oxide, aluminum hydroxide, etc., can be used.

[0039] The transition metal M source should preferably have high purity; for example, a material with a purity of 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 4N5 (99.995%) or higher, and even more preferably 5N (99.999%) or higher should be used. By using a high-purity material, impurities in the positive electrode active material can be controlled. As a result, the capacity of the secondary battery is increased and / or the reliability of the secondary battery is improved.

[0040] In addition, it is preferable that the transition metal source has high crystallinity, for example, that it has single crystal grains. The crystallinity of the transition metal source can be evaluated by TEM (transmission electron microscope), STEM (scanning transmission electron microscope), HAADF-STEM (high-angle scattering annular dark-field scanning transmission electron microscope), ABF-STEM (annular bright-field scanning transmission electron microscope), etc., or by X-ray diffraction (XRD), electron diffraction, neutron diffraction, etc. The above methods for evaluating crystallinity can be applied not only to transition metal sources but also to the evaluation of other materials with similar crystallinity.

[0041] Furthermore, when using two or more transition metal sources, it is preferable to prepare them in a proportion (mixing ratio) that allows them to take on a layered rock salt-type crystalline structure.

[0042] <Step S12> Next, as step S12 shown in Figure 1(A), the lithium source and the transition metal source are crushed and mixed to prepare a mixed material. Crushing and mixing can be done dry or wet. Wet crushing is preferred because it allows for finer crushing. If wet crushing is used, a solvent is prepared. Suitable solvents include ketones such as acetone, alcohols such as ethanol and isopropanol, ethers, dioxane, acetonitrile, N-methyl-2-pyrrolidone (NMP), etc. It is more preferable to use an aprotic solvent that does not react easily with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or higher is used. It is preferable to mix the lithium source and the transition metal source with dehydrated acetone with a purity of 99.5% or higher, with a water content reduced to 10 ppm or less, and then crush and mix them. By using dehydrated acetone of such purity as described above, the amount of impurities that may be introduced can be reduced.

[0043] For grinding and mixing, a ball mill or a bead mill can be used. When using a ball mill, it is preferable to use aluminum oxide balls or zirconium oxide balls as the grinding media. Zirconium oxide balls are preferable because they produce less impurity. Also, when using a ball mill or a bead mill, the peripheral speed should be set to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media. In this embodiment, the peripheral speed is set to 838 mm / s (rotation speed 400 rpm, ball mill diameter 40 mm).

[0044] <Step S13> Next, in step S13 shown in Figure 1(A), the mixed material is heated. The heating is preferably carried out at 800°C to 1100°C, more preferably at 900°C to 1000°C, and even more preferably at around 950°C. If the temperature is too low, the decomposition and melting of the lithium source and the transition metal source may be insufficient. On the other hand, if the temperature is too high, defects may occur due to the evaporation of lithium from the lithium source and / or the excessive reduction of the metal used as the transition metal source. For example, when cobalt is used as the transition metal, excessive reduction can cause the cobalt to change from trivalent to divalent, which can induce oxygen defects.

[0045] The heating time should ideally be between 1 hour and 100 hours, and more preferably between 2 hours and 20 hours.

[0046] The heating rate depends on the target temperature, but a rate between 80°C / h and 250°C / h is generally recommended. For example, when heating to 1000°C for 10 hours, a heating rate of 200°C / h is appropriate.

[0047] Heating is preferably carried out in an atmosphere with little water, such as dry air, for example, an atmosphere with a dew point of -50°C or lower, more preferably an atmosphere with a dew point of -80°C or lower. In this embodiment, heating is carried out in an atmosphere with a dew point of -93°C. In order to suppress impurities that may be mixed into the material, the concentrations of impurities such as CH4, CO, CO2, and H2 in the heating atmosphere should be kept below 5 ppb (parts per billion) each.

[0048] An atmosphere containing oxygen is preferred as the heating atmosphere. For example, one method is to continuously introduce dry air into the reaction chamber. In this case, the flow rate of the dry air is preferably 10 L / min. The method of continuously introducing oxygen into the reaction chamber and having oxygen flowing through the chamber is called flow.

[0049] When the heating atmosphere is an oxygen-containing atmosphere, a method that does not involve flowing is also acceptable. For example, the reaction chamber can be depressurized and then filled with oxygen (which can also be called purging), and then the atmosphere can be prevented from leaving the reaction chamber or from entering from the outside. For example, the reaction chamber can be depressurized to -970 hPa and then filled with oxygen up to 50 hPa.

[0050] After heating, natural cooling is acceptable, but it is preferable that the cooling time from the specified temperature to room temperature is between 10 and 50 hours. However, cooling to room temperature is not always necessary; it is sufficient if it cools to a temperature acceptable for the next step.

[0051] Heating in this process may be carried out using a rotary kiln or a roller hearth kiln. When using a rotary kiln, heating can be performed while stirring, whether in a continuous or batch system.

[0052] The sheath (which may also be called a container or crucible) used during heating is preferably made of aluminum oxide. An aluminum oxide sheath is a material that does not contain impurities. In this embodiment, an aluminum oxide sheath with a purity of 99.9% is used. It is preferable to place a lid on the sheath before heating. This prevents the volatilization of the material.

[0053] After heating is complete, the material may be crushed and sieved as needed. When collecting the heated material, it may be transferred from the crucible to a mortar before collection. It is preferable to use an aluminum oxide mortar. An aluminum oxide mortar is made of a material that does not contain impurities. Specifically, an aluminum oxide mortar with a purity of 90% or higher, preferably 99% or higher, should be used. In addition, the same heating conditions as in step S13 can be applied to the heating processes described later, other than step S13.

[0054] <Step S14> Through the above process, a composite oxide containing a transition metal (LiMO2) can be obtained in step S14 shown in Figure 1(A). The composite oxide only needs to have the crystal structure of a lithium composite oxide represented as LiMO2, and its composition is not strictly limited to Li:M:O=1:1:2. When cobalt is used as the transition metal, it is called a composite oxide containing cobalt and is represented as LiCoO2. The composition is not strictly limited to Li:Co:O=1:1:2.

[0055] Although examples of producing composite oxides by solid-phase methods have been shown as in steps S11 to S14, composite oxides may also be produced by coprecipitation or by hydrothermal methods.

[0056] <Step S15> Next, as step S15 shown in Figure 1(A), the composite oxide is heated. Because this is the first heating of the composite oxide, the heating in step S15 is sometimes called initial heating. After initial heating, the surface of the composite oxide becomes smooth. A smooth surface means that there are few irregularities, the composite oxide is generally rounded, and the corners are also rounded. Furthermore, a smooth surface is defined as a state in which there are few foreign substances adhering to the surface. Foreign substances are thought to be a cause of irregularities, so it is preferable that they do not adhere to the surface.

[0057] Initial heating involves heating the composite oxide after it has been completed. The inventors have found that performing initial heating to smooth the surface can reduce degradation after charging and discharging. In initial heating to smooth the surface, it is not necessary to prepare a lithium compound source.

[0058] Alternatively, in the initial heating process to smooth the surface, it is not necessary to prepare an additive element source.

[0059] Alternatively, a flux agent does not need to be prepared during the initial heating to smooth the surface.

[0060] Initial heating is performed before step S20 shown below, and is sometimes referred to as preheating or pretreatment.

[0061] The lithium source and / or transition metal source prepared in step S11, etc., may contain impurities. It is possible to reduce impurities from the composite oxide completed in step S14 by initial heating.

[0062] The heating conditions for this step should be such that the surface of the composite oxide becomes smooth. For example, the heating conditions can be selected from those described in step S13. To elaborate on these heating conditions, the heating temperature in this step should be lower than the temperature in step S13 in order to maintain the crystal structure of the composite oxide. Also, the heating time in this step should be shorter than the time in step S13 in order to maintain the crystal structure of the composite oxide. For example, heating at a temperature of 700°C to 1000°C for 2 hours or more is recommended.

[0063] The above-mentioned composite oxide may develop a temperature difference between its surface and interior due to heating in step S13. This temperature difference can induce a difference in shrinkage. It is thought that the difference in shrinkage occurs because the fluidity of the surface and interior differs due to the temperature difference. The energy associated with the difference in shrinkage gives the composite oxide a difference in internal stress. This difference in internal stress is also called strain, and the energy associated with it is sometimes called strain energy. The internal stress is removed by the initial heating in step S15, or in other words, the strain energy is considered to be homogenized by the initial heating in step S15. When the strain energy is homogenized, the strain of the composite oxide is relieved. Therefore, after step S15, the surface of the composite oxide may become smoother. This is also referred to as the surface being improved. In other words, it is thought that after step S15, the difference in shrinkage that occurred in the composite oxide is relieved, and the surface of the composite oxide becomes smoother.

[0064] Furthermore, differences in shrinkage can cause microscopic displacements in the composite oxide, such as crystal displacements. This process is also recommended to reduce such displacements. This process makes it possible to homogenize the displacements in the composite oxide. When the displacements are homogenized, the surface of the composite oxide may become smoother. This can also be described as the crystal grains being aligned. In other words, it is believed that step S15 alleviates the crystal displacements and other issues that have occurred in the composite oxide, resulting in a smoother surface.

[0065] Using a composite oxide with a smooth surface as the positive electrode active material reduces degradation during charging and discharging in a secondary battery and prevents cracking of the positive electrode active material.

[0066] A smooth surface of a composite oxide can be described as having a surface roughness of 10 nm or less, when the surface irregularities information is quantified from measurement data in a cross-section of the composite oxide. A cross-section is, for example, the cross-section obtained when observing with a scanning transmission electron microscope (STEM).

[0067] Furthermore, a pre-synthesized composite oxide containing lithium, a transition metal, and oxygen may be used as step S14. In this case, steps S11 to S13 can be omitted. By performing step S15 on the pre-synthesized composite oxide, a composite oxide with a smooth surface can be obtained.

[0068] It is possible that the lithium in the composite oxide decreases due to initial heating. The reduced lithium, due to the decrease in the added elements (explained in the next step, S20, etc.), may make it easier for the lithium to enter the composite oxide.

[0069] <Step S20> Additive element X may be added to a composite oxide with a smooth surface, as long as it can adopt a layered rock salt-type crystalline structure. Adding additive element X to a composite oxide with a smooth surface allows for uniform addition of the additive element. Therefore, it is preferable to add the additive element after initial heating. The step of adding the additive element will be explained using Figures 1(B) and 1(C).

[0070] <Step S21> In step S21 shown in Figure 1(B), a source of additive elements to be added to the composite oxide is prepared. A lithium source may also be prepared along with the additive element source.

[0071] As additive elements, one or more can be selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. Alternatively, one or more can be selected from bromine and beryllium. However, since bromine and beryllium are toxic to living organisms, it is preferable to use the additive elements mentioned above.

[0072] When magnesium is selected as the additive element, the additive element source can be called a magnesium source. Suitable magnesium sources include magnesium fluoride, magnesium oxide, magnesium hydroxide, or magnesium carbonate. Multiple magnesium sources may also be used.

[0073] When fluorine is selected as the additive element, the additive element source can be called a fluorine source. Examples of such fluorine sources include lithium fluoride (LiF), magnesium fluoride (MgF2), aluminum fluoride (AlF3), titanium fluoride (TiF4), cobalt fluoride (CoF2, CoF3), nickel fluoride (NiF2), zirconium fluoride (ZrF4), vanadium fluoride (VF5), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF2), calcium fluoride (CaF2), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF2), cerium fluoride (CeF3, CeF4), lanthanum fluoride (LaF3), or sodium aluminum hexafluoride (Na3AlF6). Among these, lithium fluoride is preferred because it has a relatively low melting point of 848°C and is easily melted in the heating process described later.

[0074] Magnesium fluoride can be used as both a fluorine source and a magnesium source. Lithium fluoride can also be used as a lithium source. Another lithium source used in step S21 is lithium carbonate.

[0075] The fluorine source may also be a gas, such as fluorine (F2), carbon fluoride, sulfur fluoride, or oxygen fluoride (OF2, O2F2, O3F2, O4F2, O5F2, O6F2, O2F), which may be mixed into the atmosphere during the heating process described later. Multiple fluorine sources may also be used.

[0076] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF2) is prepared as both the fluorine source and the magnesium source. The effect of lowering the melting point is greatest when lithium fluoride and magnesium fluoride are mixed in a molar ratio of approximately LiF:MgF2 = 65:35. On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be in excess and the cycle characteristics will deteriorate. Therefore, the molar ratio of lithium fluoride to magnesium fluoride is preferably LiF:MgF2 = x:1 (0≦x≦1.9), more preferably LiF:MgF2 = x:1 (0.1≦x≦0.5), and even more preferably LiF:MgF2 = x:1 (x=approximately 0.33). In this specification, "approximately" means a value greater than 0.9 times and less than 1.1 times the value.

[0077] At the same time, the amount of magnesium added is preferably more than 0.1 atomic% and 3 atomic% or less based on LiCoO2, more preferably 0.5 atomic% to 2 atomic% or less, and even more preferably 0.5 atomic% to 1 atomic% or less. If the amount of magnesium added is 0.1 atomic% or less, the initial discharge capacity is high, but the discharge capacity decreases rapidly when repeated charge-discharge cycles with high charge depths are performed. If the amount of magnesium added is more than 0.1 atomic% and 3 atomic% or less, both the initial discharge characteristics and charge-discharge cycle characteristics are good even when repeated charge-discharge cycles with high charge depths are performed. On the other hand, if the amount of magnesium added exceeds 3 atomic%, both the initial discharge capacity and charge-discharge cycle characteristics tend to gradually deteriorate.

[0078] <Step S22> Next, in step S22 shown in Figure 1(B), the magnesium source and fluorine source are crushed and mixed. This step can be performed by selecting from the crushing and mixing conditions described in step S12.

[0079] A heating step may be performed after step S22 if necessary. The heating step can be performed by selecting from the heating conditions described in step S13. The heating time is preferably 2 hours or more, and the heating temperature is preferably 800°C to 1100°C.

[0080] <Step S23> Next, in step S23 shown in Figure 1(B), the material that has been crushed and mixed above is recovered to obtain an additive element source (X source). The additive element source shown in step S23 has multiple starting materials and can be called a mixture.

[0081] The particle size of the above mixture is preferably such that the D50 (median diameter) is 600 nm or more and 20 μm or less, and more preferably 1 μm or more and 10 μm or less. Even when one material is used as the source of added elements, the D50 (median diameter) is preferably such that it is 600 nm or more and 20 μm or less, and more preferably 1 μm or more and 10 μm or less.

[0082] Such finely powdered mixtures (including those with only one additive element) are more likely to uniformly adhere to the surface of the composite oxide particles when mixed with the composite oxide in a later step. Uniform adhesion of the mixture to the surface of the composite oxide particles is preferable because it facilitates the uniform distribution or diffusion of fluorine and magnesium to the surface layer of the composite oxide after heating. The region where fluorine and magnesium are distributed can also be called the surface layer. If there are regions in the surface layer that do not contain fluorine and magnesium, it may be difficult to achieve the O3' and O3'' crystal structures described later in the charged state. Although fluorine was used in this explanation, chlorine may also be used, and the term "halogen" can be used interchangeably if it includes these.

[0083] <Step S21> A process different from that shown in Figure 1(B) will be explained using Figure 1(C). In step S21 shown in Figure 1(C), four types of additive element sources are prepared to be added to the composite oxide. In other words, Figure 1(C) has different types of additive element sources than Figure 1(B). A lithium source may also be prepared along with the additive element sources.

[0084] Four types of additive element sources are prepared: a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source). The magnesium and fluorine sources can be selected from the compounds described in Figure 1(B). Nickel sources such as nickel oxide and nickel hydroxide can be used. Aluminum sources such as aluminum oxide and aluminum hydroxide can be used.

[0085] <Steps S22 and S23> Steps S22 and S23 shown in Figure 1(C) are the same as the steps described in Figure 1(B).

[0086] <Step S31> Next, in step S31 shown in Figure 1(A), the composite oxide and the additive element source (X source) are mixed. The ratio of the number of transition metal atoms M in the composite oxide containing lithium, a transition metal, and oxygen to the number of magnesium atoms Mg in the X source is preferably M:Mg=100:y (0.1≦y≦6), and more preferably M:Mg=100:y (0.3≦y≦3).

[0087] The mixing in step S31 is preferably carried out under milder conditions than the mixing in step S12 in order to avoid destroying the particles of the composite oxide. For example, it is preferable to use conditions with a lower rotation speed or a shorter time than the mixing in step S12. Also, dry mixing is generally milder than wet mixing. For mixing, for example, a ball mill or a bead mill can be used. When using a ball mill, it is preferable to use zirconium oxide balls as the media.

[0088] In this embodiment, the mixing is performed dry using a ball mill with zirconium oxide balls with a diameter of 1 mm at 150 rpm for 1 hour. The mixing is carried out in a dry room with a dew point of -100°C or higher and -10°C or lower.

[0089] <Step S32> Next, in step S32 of Figure 1(A), the mixed materials are recovered to obtain mixture 903. During recovery, if necessary, the materials may be crushed and then sieved.

[0090] In this embodiment, a method is described in which lithium fluoride is added as a fluorine source and magnesium fluoride as a magnesium source to the composite oxide after initial heating. However, the present invention is not limited to the above method. At step S11, that is, at the stage of the starting materials of the composite oxide, the magnesium source and fluorine source can be added to the lithium source and transition metal source. Then, in step S13, heating is performed to obtain LiMO2 with added magnesium and fluorine. In this case, it is not necessary to separate the processes of steps S11 to S14 from the processes of steps S21 to S23. This can be said to be a simple and highly productive method.

[0091] Alternatively, lithium cobalt oxide with magnesium and fluorine added beforehand may be used. Using lithium cobalt oxide with added magnesium and fluorine allows for the omission of steps S11 to S32 and step S20. This method is simple and highly productive.

[0092] Alternatively, magnesium and fluorine sources, or magnesium, fluorine, nickel, and aluminum sources, may be added to lithium cobalt oxide that has already been treated with magnesium and fluorine, in accordance with step S20.

[0093] <Step S33> Next, in step S33 shown in Figure 1(A), the mixture 903 is heated. This can be performed by selecting from the heating conditions described in step S13. A heating time of 2 hours or more is preferable.

[0094] Here, a supplementary note about the heating temperature is provided. The lower limit of the heating temperature in step S33 needs to be at least the temperature at which the reaction between the composite oxide (LiMO2) and the additive element source proceeds. The temperature at which the reaction proceeds may be the temperature at which the mutual diffusion of the elements possessed by LiMO2 and the additive element source occurs, and it may be lower than the melting temperature of these materials. Taking oxides as an example, it is known that solid-phase diffusion occurs from 0.757 times the melting temperature T m (Tammann temperature T d ). Therefore, the heating temperature in step S33 may be 500°C or higher.

[0095] Of course, if the temperature is at least the temperature at which at least a part of the mixture 903 melts, the reaction will proceed more easily. For example, when the additive element source has LiF and MgF2, since the eutectic point of LiF and MgF2 is around 742°C, it is preferable that the lower limit of the heating temperature in step S33 is 742°C or higher.

[0096] Also, for the mixture 903 obtained by mixing so that LiCoO2:LiF:MgF2 = 100:0.33:1 (molar ratio), an endothermic peak is observed around 830°C in differential scanning calorimetry (DSC measurement). Therefore, it is more preferable that the lower limit of the heating temperature is 830°C or higher.

[0097] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time can be shortened, and the productivity is high.

[0098] The upper limit of the heating temperature should be less than the decomposition temperature of LiMO2 (the decomposition temperature of LiCoO2 is 1130°C). Near the decomposition temperature, although the amount is small, there is concern about the decomposition of LiMO2. Therefore, it is more preferably 1000°C or lower, even more preferably 950°C or lower, and even more preferably 900°C or lower.

[0099] Based on these considerations, the heating temperature in step S33 is preferably 500°C to 1130°C, more preferably 500°C to 1000°C, even more preferably 500°C to 950°C, and even more preferably 500°C to 900°C. Furthermore, 742°C to 1130°C is preferred, more preferably 742°C to 1000°C, even more preferably 742°C to 950°C, and even more preferably 742°C to 900°C. Also, 800°C to 1100°C, 830°C to 1130°C are preferred, more preferably 830°C to 1000°C, even more preferably 830°C to 950°C, and even more preferably 830°C to 900°C. The heating temperature in step S33 should be higher than that in step S13.

[0100] Furthermore, when heating the mixture 903, it is preferable to control the partial pressure of fluorine or fluoride, which may be caused by the fluorine source, to an appropriate range.

[0101] In the manufacturing method described in this embodiment, some materials, such as LiF, a fluorine source, may function as a flux. This function allows the heating temperature to be lowered to below the decomposition temperature of the composite oxide (LiMO2), for example, between 742°C and 950°C, enabling the distribution of additive elements, including magnesium, to the surface layer and the production of a positive electrode active material with good properties.

[0102] However, since LiF is less dense than oxygen in its gaseous state, it may volatilize when heated, and if it volatilizes, the amount of LiF in mixture 903 will decrease. This weakens its function as a flux. Therefore, it is necessary to heat the mixture while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, Li on the surface of LiMO2 may react with F from the fluorine source to produce LiF, which may then volatilize. Therefore, even if a fluoride with a higher melting point than LiF is used, the same need to suppress volatilization is required.

[0103] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 while the partial pressure of LiF in the heating furnace is high. Such heating can suppress the volatilization of LiF in the mixture 903.

[0104] In this process, it is preferable to heat the mixture 903 in a way that prevents the particles from sticking together. If the particles of the mixture 903 stick together during heating, the contact area with oxygen in the atmosphere decreases, and the diffusion pathway of the added elements (e.g., fluorine) is obstructed, which may worsen the distribution of added elements (e.g., magnesium and fluorine) to the surface layer.

[0105] Furthermore, it is believed that if the additive elements (e.g., fluorine) are uniformly distributed on the surface, a smooth positive electrode active material with fewer irregularities can be obtained. Therefore, in order to maintain or further improve the smooth surface after heating in step S15 of this process, it is preferable that the particles do not adhere to each other.

[0106] Furthermore, when heating with a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere inside the kiln during heating. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to purge the atmosphere initially and then not allow the atmosphere to flow after introducing the oxygen atmosphere into the kiln. If oxygen flows, the fluorine source may evaporate, which is undesirable for maintaining surface smoothness.

[0107] When heating by roller hearth kiln, for example, the mixture 903 can be heated in an atmosphere containing LiF by placing a lid on the container containing the mixture 903.

[0108] A note regarding heating time: The heating time varies depending on conditions such as the heating temperature, the size of the LiMO2 particles in step S14, and their composition. When the particles are small, a lower temperature or shorter time may be preferable than when the particles are large.

[0109] When the median diameter (D50) of the composite oxide (LiMO2) in step S14 of Figure 1(A) is approximately 12 μm, the heating temperature is preferably, for example, 600°C to 950°C. The heating time is preferably, for example, 3 hours or more, more preferably 10 hours or more, and even more preferably 60 hours or more. The cooling time after heating is preferably, for example, 10 hours to 50 hours.

[0110] On the other hand, if the median diameter (D50) of the composite oxide (LiMO2) in step S14 is about 5 μm, the heating temperature is preferably, for example, 600°C to 950°C. The heating time is preferably, for example, 1 hour to 10 hours, and more preferably about 2 hours. The cooling time after heating is preferably, for example, 10 hours to 50 hours.

[0111] <Step S34> Next, in step S34 shown in Figure 1(A), the heated material is recovered and crushed as necessary to obtain the positive electrode active material 100. At this time, it is preferable to further sift the recovered particles. Through the above steps, one embodiment of the positive electrode active material 100 of the present invention can be produced. The positive electrode active material of one embodiment of the present invention has a smooth surface.

[0112] Method for preparing positive electrode active material (2) Next, we will describe one embodiment of the present invention that differs from method 1 for producing the positive electrode active material.

[0113] In Figure 2, steps S11 to S15 are performed in the same manner as in Figure 1(A) to prepare a composite oxide (LiMO2) with a smooth surface.

[0114] <Step S20a> As mentioned above, it is possible to add element X to the composite oxide as long as it can take on a layered rock salt-type crystalline structure. However, in this preparation method 2, the step of adding the element in two or more separate steps will be explained with reference to Figure 3.

[0115] <Step S21> In step S21 shown in Figure 3(A), a first additive element source is prepared. The first additive element source can be selected from the additive elements X described in step S21 shown in Figure 1(B). For example, as the additive element X1, one or more selected from magnesium, fluorine, and calcium can be suitably used. Figure 3(A) illustrates the case where a magnesium source (Mg source) and a fluorine source (F source) are used as the additive element X1.

[0116] Steps S21 to S23 shown in Figure 3(A) can be carried out under the same conditions as steps S21 to S23 shown in Figure 1(B). As a result, an additive element source (X1 source) can be obtained in step S23.

[0117] Furthermore, steps S31 to S33 shown in Figure 2 can be carried out in the same manner as steps S31 to S33 shown in Figure 1(A).

[0118] <Step S34a> Next, the material heated in step S33 is recovered to produce a composite oxide containing the additive element X1. This is also called the second composite oxide to distinguish it from the composite oxide of step S14.

[0119] <Step S40> In step S40, shown in Figure 2, a second source of added elements is added. This will be explained with reference to Figures 3(B) and 3(C).

[0120] <Step S41> In step S41 shown in Figure 3(B), a second additive element source is prepared. The second additive element source can be selected from the additive elements X described in step S21 shown in Figure 1(B). For example, as the additive element X2, one or more selected from nickel, titanium, boron, zirconium, and aluminum can be suitably used. Figure 3(B) illustrates the case where nickel and aluminum are used as the additive elements X2.

[0121] Steps S41 to S43 shown in Figure 3(B) can be carried out under the same conditions as steps S21 to S23 shown in Figure 1(B). As a result, an additive element source (X2 source) can be obtained in step S43.

[0122] Furthermore, Figure 3(C) shows a modified version of the steps described using Figure 3(B). In step S41 shown in Figure 3(C), a nickel source (Ni source) and an aluminum source (Al source) are prepared, and in step S42a, they are each pulverized independently. As a result, in step S43, multiple second additive element sources (X2 sources) are prepared. The steps in Figure 3(C) differ from those in Figure 3(B) in that the additive elements are pulverized independently in step S42a.

[0123] <Steps S51 to S53> Next, steps S51 to S53 shown in Figure 2 can be carried out under the same conditions as steps S31 to S34 shown in Figure 1(A). The conditions for step S53, which relates to the heating process, can be at a lower temperature and for a shorter time than in step S33. Through these steps, a positive electrode active material 100 according to one embodiment of the present invention can be produced in step S54. The positive electrode active material according to one embodiment of the present invention has a smooth surface.

[0124] As shown in Figures 2 and 3, in fabrication method 2, the additive elements to the composite oxide are introduced separately as additive element X1 and additive element X2. By introducing them separately, the depth profile of each additive element can be changed. For example, it is possible to profile additive element X1 so that its concentration is higher in the surface layer than in the interior, and additive element X2 so that its concentration is higher in the interior than in the surface layer.

[0125] As demonstrated in this embodiment, a positive electrode active material with a smooth surface can be obtained through the initial heating process.

[0126] The initial heating described in this embodiment is performed on a composite oxide. Therefore, it is preferable that the initial heating is performed under conditions that are lower than the heating temperature required to obtain the composite oxide and shorter than the heating time required to obtain the composite oxide. When adding additive elements to the composite oxide, it is preferable to perform the addition step after the initial heating. This addition step can be divided into two or more steps. Following this order of steps is preferable because it maintains the surface smoothness obtained in the initial heating. When the composite oxide contains cobalt as a transition metal, it can be interpreted as a composite oxide containing cobalt.

[0127] This embodiment can be used in combination with other embodiments.

[0128] (Embodiment 2) In this embodiment, a positive electrode active material according to one aspect of the present invention will be described with reference to Figures 4 to 15.

[0129] Figure 4(A) is a cross-sectional view of a positive electrode active material 100 according to one embodiment of the present invention. Figures 4(B1) and 4(B2) show enlarged views of the area around AB in Figure 4(A). Figures 4(C1) and 4(C2) show enlarged views of the area around CD in Figure 4(A).

[0130] As shown in Figures 4(A) to 4(C2), the positive electrode active material 100 has a surface layer 100a and an interior layer 100b. In these figures, the boundary between the surface layer 100a and the interior layer 100b is indicated by a dashed line. Also, in Figure 4(A), a dashed line shows a part of the grain boundary 101.

[0131] In this specification, the region extending from the surface of the positive electrode active material inward to 10 nm is referred to as the surface layer 100a. Surfaces formed by cracks may also be considered the surface. The surface layer 100a may also be referred to as the near-surface region, near-surface region, or shell. Furthermore, the region of the positive electrode active material deeper than the surface layer 100a is referred to as the interior 100b. The interior 100b may also be referred to as the interior region or core.

[0132] It is preferable that the surface layer 100a has a higher concentration of the additive elements described later than the interior layer 100b. It is also preferable that the additive elements have a concentration gradient. Furthermore, if there are multiple additive elements, it is preferable that the depth of the concentration peak from the surface differs for each additive element.

[0133] For example, it is preferable that a certain additive element X has a concentration gradient that increases from the interior 100b towards the surface, as shown by the gradient in Figure 4(B1). Examples of additive elements X that are preferable to have such a concentration gradient include magnesium, fluorine, titanium, silicon, phosphorus, boron, and calcium.

[0134] Preferably, the other additive element Y has a concentration gradient, as shown in the gradient in Figure 4(B2), and has a concentration peak in a region deeper than that of additive element X. The concentration peak may be located in the surface layer 100a or deeper than the surface layer 100a. It is preferable that the concentration peak be in a region other than the outermost layer. For example, it is preferable that the peak be in a region of 5 nm to 30 nm from the surface inward. Examples of additive elements Y that preferably have such a concentration gradient include aluminum and manganese.

[0135] Furthermore, due to the aforementioned concentration gradient of the added elements, it is preferable that the crystal structure changes continuously from the interior 100b toward the surface.

[0136] <Contained elements> The positive electrode active material 100 comprises lithium, a transition metal M, oxygen, and an additive element. The positive electrode active material 100 can also be described as a composite oxide represented by LiMO2 with the additive element added. However, the positive electrode active material in one embodiment of the present invention only needs to have the crystal structure of a lithium composite oxide represented by LiMO2, and its composition is not strictly limited to Li:M:O=1:1:2. Furthermore, a positive electrode active material with the additive element added may also be referred to as a composite oxide.

[0137] As the transition metal M in the positive electrode active material 100, it is preferable to use a metal that can form a layered rock salt type composite oxide that belongs to space group R-3m together with lithium. For example, at least one of manganese, cobalt, and nickel can be used. In other words, as the transition metal M in the positive electrode active material 100, only cobalt may be used, only nickel may be used, two types of cobalt and manganese may be used, two types of cobalt and nickel may be used, or three types of cobalt, manganese, and nickel may be used. In other words, the positive electrode active material 100 can have composite oxides containing lithium and a transition metal M, such as lithium cobalt oxide, lithium nickel oxide, lithium cobalt oxide in which part of the cobalt is substituted with manganese, lithium cobalt oxide in which part of the cobalt is substituted with nickel, and nickel-manganese-lithium cobalt oxide. Layered rock salt type composite oxides have a two-dimensional lithium ion diffusion pathway and are suitable for lithium ion insertion / desorption reactions.

[0138] In particular, using cobalt as the transition metal M in the positive electrode active material 100 in an amount of 75 atomic% or more, preferably 90 atomic% or more, and more preferably 95 atomic% or more, offers many advantages, such as being relatively easy to synthesize, easy to handle, and having excellent cycle characteristics. Furthermore, if nickel is included in addition to cobalt within the above range as the transition metal M, the displacement of the layered structure consisting of octahedra of cobalt and oxygen may be suppressed. Therefore, the crystal structure may become more stable, especially in the charged state at high temperatures, which is preferable.

[0139] Furthermore, the transition metal M does not necessarily have to contain manganese. By using a cathode active material 100 that is substantially free of manganese, the above advantages such as being relatively easy to synthesize, easy to handle, and having excellent cycle characteristics may be even greater. The weight of manganese contained in the cathode active material 100 is preferably, for example, 600 ppm or less, more preferably 100 ppm or less.

[0140] On the other hand, if nickel is used as the transition metal M in the positive electrode active material 100 in an amount of 33 atomic percent or more, preferably 60 atomic percent or more, and more preferably 80 atomic percent or more, the raw materials may be cheaper compared to the case where cobalt is abundant, and the charge / discharge capacity per unit weight may increase, which is preferable.

[0141] Note that the transition metal M does not necessarily have to include nickel.

[0142] It is preferable to use at least one of the following as additive elements for the positive electrode active material 100: magnesium, fluorine, aluminum, titanium, zirconium, vanadium, iron, chromium, niobium, cobalt, arsenic, zinc, silicon, sulfur, phosphorus, and boron. These additive elements may further stabilize the crystal structure of the positive electrode active material 100, as will be described later. In other words, the positive electrode active material 100 can include lithium cobalt oxide with magnesium and fluorine, lithium cobalt oxide with magnesium, fluorine, and titanium, lithium nickel-cobalt oxide with magnesium and fluorine, lithium cobalt-aluminate with magnesium and fluorine, lithium nickel-cobalt-aluminate with magnesium and fluorine, lithium nickel-manganese-cobalt oxide with magnesium and fluorine, etc. In this specification, additive elements may also be referred to as mixtures, part of raw materials, or impurity elements.

[0143] Furthermore, the additive elements do not necessarily have to include magnesium, fluorine, aluminum, titanium, zirconium, vanadium, iron, chromium, niobium, cobalt, arsenic, zinc, silicon, sulfur, phosphorus, or boron.

[0144] In one embodiment of the present invention, the positive electrode active material 100 is reinforced in a surface layer 100a, i.e., the outer periphery of the particles, where the concentration of the added element is high, so that the layered structure consisting of octahedra of transition metal M and oxygen does not break down even if lithium is removed from the positive electrode active material 100 due to charging.

[0145] Furthermore, it is preferable that the concentration gradient of the added elements be similar throughout the entire surface layer 100a of the positive electrode active material 100. It can also be said that it is preferable that the reinforcement resulting from the high concentration of added elements is uniformly present in the surface layer 100a. Even if there is reinforcement in a part of the surface layer 100a, if there are parts without reinforcement, stress may concentrate in those parts. If stress concentrates in a part of the particles, defects such as cracks may occur from there, which may lead to cracking of the positive electrode active material and a decrease in charge / discharge capacity.

[0146] In this specification, homogeneity refers to the phenomenon in which, in a solid composed of multiple elements (e.g., A, B, C), a certain element (e.g., A) is distributed in a specific region with similar characteristics. It is sufficient that the elemental concentrations in the specific regions are substantially the same. For example, the difference in elemental concentrations between specific regions should be within 10%. Examples of specific regions include the surface, surface layer, convex areas, concave areas, and interior.

[0147] However, the added elements do not necessarily have to have the same concentration gradient across the entire surface layer 100a of the positive electrode active material 100. For example, an example of the distribution of added element X near CD in Figure 4(A) is shown in Figure 4(C1), and an example of the distribution of added element Y near CD is shown in Figure 4(C2).

[0148] Here, the region near CD has a layered rock salt crystal structure of R-3m, and the surface is (001) oriented. The distribution of additive elements on the (001) oriented surface may differ from that of other surfaces. For example, on the (001) oriented surface and its surface layer 100a, the distribution of at least one of additive elements X and Y may remain in a shallower portion of the surface compared to surfaces other than the (001) oriented surface. Alternatively, the concentration of at least one of additive elements X and Y may be lower on the (001) oriented surface and its surface layer 100a compared to surfaces other than the (001) oriented surface. Alternatively, the concentration of at least one of additive elements X and Y may be below the detection limit on the (001) oriented surface and its surface layer 100a.

[0149] In the layered rock salt crystal structure of R-3m, cations are arranged parallel to the (001) plane. This indicates a structure in which MO2 layers, consisting of octahedrons of transition metal M and oxygen, and lithium layers are alternately stacked parallel to the (001) plane. Therefore, the diffusion pathways for lithium ions also exist parallel to the (001) plane.

[0150] Since the MO2 layer, which consists of an octahedron of transition metal M and oxygen, is relatively stable, the surface of the positive electrode active material 100 is more stable when it is oriented in the (001) direction. The (001) plane does not expose the diffusion pathway of lithium ions.

[0151] On the other hand, the lithium ion diffusion pathways are exposed on surfaces other than those oriented in the (001) direction. Therefore, the surfaces and surface layer 100a other than those oriented in the (001) direction are important regions for maintaining the lithium ion diffusion pathways, but at the same time, they are prone to instability because they are the regions where lithium ions first desorb. For this reason, reinforcing the surfaces and surface layer 100a other than those oriented in the (001) direction is extremely important for maintaining the overall crystal structure of the positive electrode active material 100.

[0152] Therefore, in another embodiment of the positive electrode active material 100 of the present invention, it is important that the distribution of the added elements on the surfaces other than the (001) oriented surface and its surface layer 100a is as shown in Figure 4(B1) or Figure 4(B2). On the other hand, in the (001) oriented surface and its surface layer 100a, the concentration of the added elements may be low or there may be no added elements at all, as described above.

[0153] In the manufacturing method described in the previous embodiment, in which high-purity LiMO2 is produced and then additive elements are mixed in and heated afterward, the additive elements spread mainly through the diffusion pathway of lithium ions, making it easier to bring the distribution of additive elements on surfaces other than the (001) orientation and its surface layer 100a to a desirable range.

[0154] Using Figures 5(A1) to 5(B), we will explain the results of calculations regarding the distribution of additive elements when high-purity LiMO2 is prepared, mixed with additive elements, and then heated.

[0155] Figure 5(A1) shows the calculation results for a (104) oriented surface and its surface layer 100a. The calculation was performed using classical molecular dynamics. LiCoO2 (LCO) was placed at the bottom of the system, and LiF and MgF2 were placed at the top of the system. The ensemble was NVT, and the density of the initial structure was 1.8 g / cm³. 3 The system temperature was 2000K, the elapsed time was 100 psec, the potential was optimized for the LCO crystal structure, and the other atoms were mixed with UFF (Universal Force Field). The system had 10,000 atoms and a neutral charge. To simplify the diagram, only Co and Mg atoms are shown.

[0156] Figure 5(A2) shows the results calculated up to 200 psec, and Figure 5(A3) shows the results calculated up to 1200 psec.

[0157] Mg diffuses through the following process. (1) Due to heat (not shown in the diagram), Li atoms are removed from LCO. (2) Mg atoms enter the Li layer of LCO and diffuse into the interior. (3) Li atoms from LiF enter the Li layer of LCO, and the Li atoms that were removed in (1) are replaced.

[0158] Figure 5(A1), taken after 100 psec, clearly shows the diffusion of Mg atoms into the LCO. The Mg atoms diffuse along the cobalt arrangement, and in Figure 5(A3), taken after 1200 psec, almost all of the Mg atoms prepared at the top of the system are incorporated into the LCO.

[0159] Figure 5(B) shows the same calculation results as Figure 5(A1), except that the orientation is (001). In Figure 5(B), it can be seen that the Mg atoms remain on the surface of the LCO.

[0160] As described above, the manufacturing method, which involves producing high-purity LiMO2 and then mixing in additive elements and heating, allows for a more favorable distribution of additive elements on surfaces other than the (001) oriented surface and its surface layer 100a compared to the (001) oriented surface. Furthermore, in a manufacturing method that includes initial heating, it is expected that lithium atoms in the surface layer will be detached from the LiMO2 by the initial heating, making it easier to distribute additive elements, including magnesium atoms, at a higher concentration in the surface layer.

[0161] Furthermore, while it is preferable that the surface of the positive electrode active material 100 be smooth and have few irregularities, it is not necessarily required that the entire surface of the positive electrode active material 100 be so. In composite oxides having a layered rock salt-type crystalline structure of R-3m, slip is likely to occur on planes parallel to the (001) plane, for example, on planes where lithium is arranged. As shown in Figure 6(A), if the (001) plane is horizontal, horizontal slip may occur and deformation may occur as shown by the arrow in Figure 6(B) after going through processes such as pressing.

[0162] In this case, the newly formed surface and its surface layer 100a resulting from the slip may either not contain the added element or its concentration may be below the detection limit. EF in Figure 6(B) is an example of the newly formed surface and its surface layer 100a resulting from the slip. Enlarged views of the area around EF are shown in Figures 6(C1) and 6(C2). Unlike Figures 4(B1) to 4(C2), there is no gradient of added element X and added element Y in Figures 6(C1) and 6(C2).

[0163] However, since slip tends to occur parallel to the (001) plane, the newly formed surface and its surface layer 100a will be (001) oriented. The (001) plane is relatively stable as the diffusion pathway of lithium ions is not exposed, so there is little problem even if the additive element is absent or its concentration is below the detection limit.

[0164] As mentioned above, in a composite oxide with a composition of LiMO2 and a layered rock salt crystal structure of R-3m, the atoms of the transition metal M are arranged parallel to the (001) plane. Furthermore, in HAADF-STEM images, the brightness of the transition metal M, which has the largest atomic number among the LiMO2 atoms, is the highest. Therefore, in HAADF-STEM images, the arrangement of atoms with high brightness can be considered to be the arrangement of transition metal M atoms. The repetition of this high-brightness arrangement can be called crystal fringes or lattice fringes. Moreover, if the crystal structure is a layered rock salt type with a crystal structure of R-3m, the crystal fringes or lattice fringes can be considered to be parallel to the (001) plane.

[0165] The positive electrode active material 100 may have depressions, cracks, pits, or V-shaped cross-sections. These are defects, and repeated charging and discharging may lead to the leaching of transition metal M, collapse of the crystal structure, cracking of the positive electrode active material 100, and desorption of oxygen. However, if there are embedded portions 102 (Figure 8) that fill these defects, the leaching of transition metal M and other defects can be suppressed. Therefore, a positive electrode active material 100 with excellent reliability and cycle characteristics can be obtained.

[0166] Furthermore, the positive electrode active material 100 may have protrusions 103 (Figure 8) as regions where the added elements are unevenly distributed.

[0167] As mentioned above, if the amount of additive elements in the positive electrode active material 100 is excessive, it may adversely affect the insertion and removal of lithium. Furthermore, when the positive electrode active material 100 is used in a secondary battery, it may lead to an increase in internal resistance and a decrease in charge / discharge capacity. On the other hand, if the amount of additive elements is insufficient, they may not be distributed throughout the entire surface layer 100a, and the effect of suppressing the deterioration of the crystal structure may be insufficient. Thus, the additive elements in the positive electrode active material 100 need to be at an appropriate concentration, but adjusting this is not easy.

[0168] Therefore, if the positive electrode active material 100 has regions where the additive elements are unevenly distributed, some of the excess atoms of the additive elements are removed from the interior 100b of the positive electrode active material 100, allowing for an appropriate concentration of the additive elements in the interior 100b. This suppresses the increase in internal resistance and the decrease in charge / discharge capacity when used as a secondary battery. The ability to suppress the increase in the internal resistance of a secondary battery is an extremely desirable characteristic, especially at high charge / discharge rates, such as 2C or higher.

[0169] Furthermore, in positive electrode active material 100 having regions where the added elements are unevenly distributed, it is permissible to mix in a certain degree of excess impurities during the manufacturing process. This is preferable because it widens the margin in production.

[0170] In this specification, "non-uniformity" refers to a situation where the concentration of an element in one region differs from that in other regions. It may also be described as segregation, precipitation, heterogeneity, bias, or a mixture of areas with high and low concentrations.

[0171] Magnesium, one of the additive elements X, is divalent and is more stable in lithium sites than transition metal sites in the layered rock salt crystal structure, thus easily occupying lithium sites. The presence of magnesium at an appropriate concentration in the lithium sites of the surface layer 100a makes it easier to maintain the layered rock salt crystal structure. Furthermore, the presence of magnesium can suppress the desorption of oxygen around the magnesium when the depth of charge is high. In addition, the presence of magnesium can be expected to increase the density of the positive electrode active material. Magnesium is preferable as it does not adversely affect the insertion and removal of lithium during charging and discharging when present at an appropriate concentration. However, if magnesium is present in excess, it may adversely affect the insertion and removal of lithium. Therefore, as will be described later, it is preferable that the surface layer 100a has a higher concentration of transition metal M than magnesium, for example.

[0172] Aluminum, one of the additive elements Y, is trivalent and can exist at transition metal sites in the layered rock salt crystal structure. Aluminum can suppress the dissolution of surrounding cobalt. Furthermore, because aluminum has a strong bonding force with oxygen, it can suppress the desorption of oxygen around the aluminum. Therefore, by including aluminum as an additive element, it is possible to create a positive electrode active material 100 whose crystal structure is less likely to collapse even after repeated charging and discharging.

[0173] Fluorine is a monovalent anion, and if some of the oxygen in the surface layer 100a is replaced by fluorine, the lithium desorption energy decreases. This is because the oxidation-reduction potential of cobalt ions during lithium desorption differs depending on the presence or absence of fluorine. In other words, if fluorine is absent, the cobalt ions change from trivalent to tetravalent during lithium desorption. On the other hand, if fluorine is present, the cobalt ions change from divalent to trivalent during lithium desorption. The oxidation-reduction potential of cobalt ions differs in these two cases. Therefore, if some of the oxygen in the surface layer 100a of the positive electrode active material 100 is replaced by fluorine, the desorption and insertion of lithium ions near the fluorine can occur more smoothly. This is preferable because it improves charge-discharge characteristics, rate characteristics, etc., when used in a secondary battery.

[0174] Titanium oxide is known to be superhydrophilic. Therefore, by using a positive electrode active material 100 having titanium oxide in its surface layer 100a, it is possible that wettability with highly polar solvents will be improved. When used in a secondary battery, good contact at the interface between the positive electrode active material 100 and the highly polar electrolyte may be achieved, potentially suppressing an increase in internal resistance.

[0175] As the charging voltage of a secondary battery increases, the voltage at the positive electrode generally rises. The positive electrode active material according to one aspect of the present invention has a stable crystal structure even at high voltages. The stability of the crystal structure of the positive electrode active material in the charged state suppresses the decrease in charge / discharge capacity that occurs with repeated charging and discharging.

[0176] In addition, a short circuit in a secondary battery not only causes problems in the charging operation and / or discharging operation of the secondary battery, but also may lead to heat generation and ignition. In order to realize a safe secondary battery, it is preferable that the short-circuit current is suppressed even at a high charging voltage. The positive electrode active material 100 according to one aspect of the present invention suppresses the short-circuit current even at a high charging voltage. Therefore, a secondary battery having both a high charge-discharge capacity and safety can be achieved.

[0177] The concentration gradient of the additive element can be evaluated, for example, using energy dispersive X-ray spectroscopy (EDX), electron probe microanalysis (EPMA), or the like. Among EDX measurements, the measurement while scanning within a region and the two-dimensional evaluation within the region is called EDX surface analysis. Also, the measurement while linearly scanning and the evaluation of the distribution of atomic concentration within the positive electrode active material particles is called line analysis. Further, in some cases, the data of a linear region extracted from the surface analysis of EDX is also called line analysis. Also, the measurement without scanning a certain region is called point analysis.

[0178] By EDX surface analysis (for example, element mapping), the concentration of the additive element in the surface layer portion 100a, the interior 100b, and the vicinity of the crystal grain boundary 101 of the positive electrode active material 100 can be quantitatively analyzed. Also, by EDX line analysis, the concentration distribution and the maximum value of the additive element can be analyzed. Also, an analysis that thins the sample like STEM-EDX can analyze the concentration distribution in the depth direction from the surface to the center of the particles in a specific region without being affected by the distribution in the depth direction, and is more preferable.

[0179] When EDX line analysis is performed on the positive electrode active material 100 having magnesium as an additive element, the peak of the magnesium concentration in the surface layer portion 100a preferably exists up to a depth of 3 nm from the surface of the positive electrode active material 100 toward the center, more preferably up to a depth of 1 nm, and even more preferably up to a depth of 0.5 nm.

[0180] In the case of the positive electrode active material 100 having magnesium and fluorine as additive elements, the distribution of fluorine preferably overlaps with the distribution of magnesium. Therefore, when EDX line analysis is performed, the peak of the fluorine concentration in the surface layer portion 100a preferably exists up to a depth of 3 nm from the surface of the positive electrode active material 100 toward the center, more preferably up to a depth of 1 nm, and even more preferably up to a depth of 0.5 nm.

[0181] Note that not all additive elements need to have the same concentration distribution. For example, when the positive electrode active material 100 has aluminum as an additive element, it preferably has a distribution slightly different from that of magnesium and fluorine as described above. For example, when EDX line analysis is performed, the peak of the magnesium concentration is preferably closer to the surface than the peak of the aluminum concentration in the surface layer portion 100a. For example, the peak of the aluminum concentration preferably exists at a depth of 0.5 nm or more and 50 nm or less from the surface of the positive electrode active material 100 toward the center, more preferably at a depth of 5 nm or more and 30 nm or less. Or it preferably exists at a depth of 0.5 nm or more and 30 nm or less. Or it preferably exists at a depth of 5 nm or more and 50 nm or less.

[0182] When line analysis or surface analysis is performed on the positive electrode active material 100, the ratio (I / M) of the number of atoms of the additive element I to the transition metal M in the surface layer portion 100a is preferably 0.05 or more and 1.00 or less. Further, when the additive element is titanium, the ratio (Ti / M) of the number of atoms of titanium to the transition metal M is preferably 0.05 or more and 0.4 or less, and more preferably 0.1 or more and 0.3 or less. When the additive element is magnesium, the ratio (Mg / M) of the number of atoms of magnesium to the transition metal M is preferably 0.4 or more and 1.5 or less, and more preferably 0.45 or more and 1.00 or less. When the additive element is fluorine, the ratio (F / M) of the number of atoms of fluorine to the transition metal M is preferably 0.05 or more and 1.5 or less, and more preferably 0.3 or more and 1.00 or less.

[0183] Furthermore, the surface of the positive electrode active material 100 in the EDX radiation analysis results can be estimated as follows: For elements uniformly present in the interior 100b of the positive electrode active material 100, such as oxygen or transition metals M such as cobalt, the point where the detected amount in the interior 100b becomes half is defined as the surface.

[0184] Since the positive electrode active material 100 is a composite oxide, it is preferable to estimate the surface using the detected amount of oxygen. Specifically, first, the average value of the oxygen concentration is obtained from the region where the detected amount of oxygen in the interior 100b is stable. ave We determine the amount of oxygen O in the region that is clearly outside the surface, which is thought to be due to chemiadsorption or background. background If detected, O background Subtracting this gives the average oxygen concentration O ave This can be done. This average value O ave Half of that value, that is, 1 / 2O ave The measurement point that shows the closest measurement value can be estimated to be the surface of the positive electrode active material.

[0185] The surface can also be estimated using the transition metal M present in the positive electrode active material 100. For example, if more than 95% of the multiple transition metals M are cobalt, the surface can be estimated in the same way as above using the detected amount of cobalt. Alternatively, it can be estimated in the same way using the sum of the detected amounts of the multiple transition metals M. The detected amount of transition metal M is suitable for surface estimation because it is less affected by chemiadsorption.

[0186] Furthermore, when line analysis or surface analysis is performed on the positive electrode active material 100, the ratio of the number of atoms of the added element I to the transition metal M near the grain boundary 101 (I / M) is preferably 0.020 or more and 0.50 or less. More preferably 0.025 or more and 0.30 or less. More preferably 0.030 or more and 0.20 or less. Or preferably 0.020 or more and 0.30 or less. Or preferably 0.020 or more and 0.20 or less. Or preferably 0.025 or more and 0.50 or less. Or preferably 0.025 or more and 0.20 or less. Or preferably 0.030 or more and 0.50 or less. Or preferably 0.030 or more and 0.30 or less.

[0187] For example, when the additive element is magnesium and the transition metal M is cobalt, the ratio of the number of atoms of magnesium to cobalt (Mg / Co) is preferably 0.020 or more and 0.50 or less. Furthermore, 0.025 or more and 0.30 or less is preferred. Furthermore, 0.030 or more and 0.20 or less is preferred. Or 0.020 or more and 0.30 or less is preferred. Or 0.020 or more and 0.20 or less is preferred. Or 0.025 or more and 0.50 or less is preferred. Or 0.030 or more and 0.50 or less is preferred. Or 0.030 or more and 0.30 or less is preferred.

[0188] Furthermore, progressive defects (also called pits) may occur in the positive electrode active material 100 when charged under conditions of high charging depth, such as charging at 4.5V or higher, or under high temperatures (45°C or higher). In addition, defects such as cracks may occur due to the expansion and contraction of the positive electrode active material due to charging and discharging. Figure 7 shows a schematic cross-sectional view of the positive electrode active material 51. In the positive electrode active material 51, the pits are shown as holes in 54 and 58, but the opening shape is not circular but has depth and a groove-like shape. The source of the pits may be point defects. It is also thought that the crystal structure of LCO collapses in the vicinity where the pits form, resulting in a crystal structure different from that of the layered rock salt type. When the crystal structure collapses, it may hinder the diffusion and release of lithium ions, which are carrier ions, and pits are considered to be a factor in the deterioration of cycle characteristics. In addition, cracks in the positive electrode active material 51 are shown in 57. 55 is a crystal plane parallel to the arrangement of cations, 52 is a recess, and 53 and 56 are regions where doped elements are present.

[0189] The positive electrode active materials of lithium-ion secondary batteries are typically LCO (lithium cobalt oxide) and NMC (nickel-manganese-lithium cobalt oxide), which can be described as alloys containing multiple metallic elements (cobalt, nickel, etc.). At least one of the positive electrode active materials has a defect, and this defect may change before and after charging and discharging. When used in secondary batteries, the positive electrode active material may be chemically or electrochemically eroded by the surrounding environmental substances (electrolyte, etc.), or the positive electrode active material may deteriorate. This deterioration does not occur uniformly on the surface of the positive electrode active material, but rather concentrates locally, and repeated charging and discharging of the secondary battery can cause defects to develop deeply from the surface into the interior.

[0190] The phenomenon in which defects in a positive electrode active material progress to form holes can also be called pitting corrosion, and the holes generated by this phenomenon are referred to as pits in this specification.

[0191] In this specification, cracks and pits are distinct. Cracks may exist immediately after the fabrication of the positive electrode active material, but pits do not. A pit can be described as a hole where several layers of cobalt and oxygen have been removed due to charging and discharging under conditions of high charging depth, such as high voltage conditions of 4.5V or higher or high temperature (45°C or higher), or as a location where cobalt has dissolved. A crack refers to a new surface created by the application of physical pressure, or a fissure caused by a grain boundary 101. Cracks may also occur due to the expansion and contraction of the positive electrode active material due to charging and discharging. In addition, pits may occur from cracks and / or cavities inside the positive electrode active material.

[0192] Furthermore, the positive electrode active material 100 may have a coating on at least a portion of its surface. Figure 8 shows an example of a positive electrode active material 100 having a coating 104.

[0193] Preferably, the coating 104 is formed by the accumulation of decomposition products of the electrolyte during charging and discharging. In particular, when charging to a high depth of charge is repeated, it is expected that the charge-discharge cycle characteristics will be improved by having a coating derived from the electrolyte on the surface of the positive electrode active material 100. This is due to reasons such as suppressing the increase in impedance on the surface of the positive electrode active material or suppressing the dissolution of the transition metal M. Preferably, the coating 104 contains carbon, oxygen, and fluorine. Furthermore, when LiBOB and / or SUN (suberonitrile) is used as the electrolyte, it is easier to obtain a good quality coating. Therefore, a coating 104 containing at least one of boron, nitrogen, sulfur, and fluorine may be a good quality coating and is therefore preferable. Also, the coating 104 does not have to cover the entire positive electrode active material 100.

[0194] <Crystal structure> Materials with a layered rock salt crystal structure, such as lithium cobalt oxide (LiCoO2), are known to have high discharge capacity and are excellent as positive electrode active materials for secondary batteries. Examples of materials with a layered rock salt crystal structure include composite oxides represented by LiMO2.

[0195] It is known that the Jahn-Teller effect in transition metal compounds differs in strength depending on the number of electrons in the d orbitals of the transition metal.

[0196] In nickel-containing compounds, strain can easily occur due to the Jahn-Teller effect. Therefore, when LiNiO2 is subjected to charging and discharging with high depths of charge, there is a concern that the crystal structure may collapse due to strain. In LiCoO2, the effect of the Jahn-Teller effect is suggested to be smaller, and it may have better resistance at high depths of charge, making it preferable.

[0197] The crystal structure of the positive electrode active material will be explained using Figures 9 to 13. Figures 9 to 13 describe the case where cobalt is used as the transition metal M in the positive electrode active material.

[0198] <Conventional positive electrode active material> The positive electrode active material shown in Fig. 11 is lithium cobalt oxide (LiCoO2) to which fluorine and magnesium are not added by the production method described later. As described in Non-Patent Document 1, Non-Patent Document 2, etc., the crystal structure of the lithium cobalt oxide shown in Fig. 11 changes depending on the depth of charge.

[0199] As shown in Fig. 11, lithium cobalt oxide with a charge depth of 0 (discharged state, which may also be referred to as SOC (State of Charge) 100%) has a region with a crystal structure of space group R-3m, where lithium occupies octahedral sites and there are three CoO2 layers in the unit cell. Therefore, this crystal structure is sometimes referred to as the O3-type crystal structure. Note that the CoO2 layer refers to a structure in which octahedral structures with six oxygen atoms coordinated to cobalt are continuously arranged in a plane in a state of sharing edges.

[0200] When the charge depth is 1, it has a crystal structure of space group P-3m1 and there is one CoO2 layer in the unit cell. Therefore, this crystal structure is sometimes referred to as the O1-type crystal structure.

[0201] Lithium cobalt oxide when the charge depth is about 0.8 has a crystal structure of space group R-3m. This structure can also be said to be a structure in which the CoO2 structure such as P-3m1 (O1) and the LiCoO2 structure such as R-3m (O3) are alternately stacked. Therefore, this crystal structure is sometimes referred to as the H1-3 type crystal structure. In reality, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is twice that of other structures. However, in this specification including Fig. 11, for easy comparison with other crystal structures, it will be shown in a figure where the c-axis of the H1-3 type crystal structure is halved of the unit cell.

[0202] As an example, in the H1-3 type crystal structure, as described in Non-Patent Literature 3, the coordinates of cobalt and oxygen in the unit cell can be expressed as Co(0,0,0.42150±0.00016), O1(0,0,0.27671±0.00045), and O2(0,0,0.11535±0.00045). O1 and O2 are oxygen atoms, respectively. Thus, the H1-3 type crystal structure is represented by a unit cell using one cobalt atom and two oxygen atoms. On the other hand, as will be described later, the O3' and O3'' type crystal structures of one embodiment of the present invention are preferably represented by a unit cell using one cobalt atom and one oxygen atom. This indicates that the symmetry between cobalt and oxygen differs between the O3' structure and the H1-3 type structure, and that the O3' structure shows less variation from the O3 structure compared to the H1-3 type structure. The choice of which unit cell is more preferable to represent the crystal structure of the positive electrode active material can be made, for example, by selecting the one that results in a smaller GOF (goodness of fit) value in the Rietveld analysis of the XRD pattern.

[0203] When high-voltage charging occurs, such as when the charging voltage is 4.6V or higher relative to the oxidation-reduction potential of lithium metal, or when deep charging occurs, such as when the charging depth is 0.8 or higher, and when this charging and discharging cycle is repeated, lithium cobalt oxide undergoes repeated changes in its crystal structure (i.e., non-equilibrium phase changes) between the H1-3 type crystal structure and the R-3m(O3) structure in the discharged state.

[0204] However, these two crystal structures exhibit a large displacement of the CoO2 layer. As shown by the dotted line and arrow in Figure 11, in the H1-3 type crystal structure, the CoO2 layer is significantly shifted from R-3m(O3). Such dynamic structural changes can negatively affect the stability of the crystal structure.

[0205] Furthermore, the volume difference is also significant. When comparing the same number of cobalt atoms, the volume difference between the H1-3 type crystal structure and the O3 type crystal structure in the discharged state is more than 3.0%.

[0206] In addition, the H1-3 type crystal structure, which consists of continuous CoO2 layers such as P-3m1(O1), is likely to be unstable.

[0207] Therefore, repeated charging and discharging that results in a high depth of charge causes the crystal structure of lithium cobalt oxide to break down. This breakdown of the crystal structure leads to a deterioration of cycle characteristics. This is thought to be because the breakdown of the crystal structure reduces the number of sites where lithium can exist stably, and also makes it more difficult for lithium to be inserted and removed.

[0208] <Positive electrode active material according to one aspect of the present invention> ≪Crystal structure≫ The positive electrode active material 100 according to one aspect of the present invention can reduce the displacement of the CoO2 layer during repeated charge-discharge cycles with high charge depths. Furthermore, it can reduce volume changes. Therefore, the positive electrode active material according to one aspect of the present invention can achieve excellent cycle characteristics. In addition, the positive electrode active material according to one aspect of the present invention can adopt a stable crystal structure at high charge depths. Therefore, the positive electrode active material according to one aspect of the present invention may be less prone to short circuits when maintaining a high charge depth. In such cases, safety is further improved, which is preferable.

[0209] In one embodiment of the present invention, the positive electrode active material exhibits a small change in crystal structure and a small difference in volume per unit of the same number of transition metal M atoms between a fully discharged state and a state with a high depth of charge.

[0210] Figure 9 shows the crystal structure of the interior 100b of the positive electrode active material 100 when the charging depth is 0 and when the charging depth is high, around 0.8. The interior 100b occupies most of the volume of the positive electrode active material 100 and is a part that contributes greatly to charging and discharging, so it can be said that this is the part where shifting and volume changes of the CoO2 layer are most problematic.

[0211] The positive electrode active material 100 is a composite oxide having lithium, cobalt as a transition metal M, and oxygen. In addition to the above, the interior 100b preferably has magnesium as an additive element, and more preferably has nickel in addition to cobalt as the transition metal M. The surface layer 100a preferably has fluorine as an additive element, and more preferably has aluminum and / or nickel. Details of the surface layer 100a will be described later.

[0212] The crystal structure at charge depth 0 (discharge state) in Figure 9 is R-3m(O3), the same as in Figure 11. On the other hand, the interior 100b of the positive electrode active material 100 has a crystal structure different from the H1-3 type crystal structure when it is fully charged. This structure belongs to the space group R-3m, and ions such as cobalt and magnesium occupy the oxygen 6 coordination positions. Furthermore, the symmetry of the CoO2 layer in this structure is the same as that of the O3 type. Therefore, this structure is referred to as the O3' type crystal structure in this specification. In both the O3 type crystal structure and the O3' type crystal structure, it is preferable to have dilute magnesium between the CoO2 layers, i.e., at the lithium sites. It is also preferable to have random and dilute fluorine at the oxygen sites.

[0213] In the O3' type crystal structure, light elements such as lithium may occupy the oxygen 4-coordinate position.

[0214] Furthermore, although Figure 9 shows that lithium is present at all lithium sites with a probability of 1 / 5 in O3', the positive electrode active material 100 in one embodiment of the present invention is not limited to this. It may be present preferentially at some lithium sites. For example, Li belonging to space group P2 / m 0.5 Similar to CoO2, lithium may be present at some aligned lithium sites. The distribution of lithium can be analyzed, for example, by neutron diffraction.

[0215] Furthermore, the O3' type crystal structure can be said to be similar to the CdCl2 type crystal structure, although it has lithium randomly placed between the layers. This crystal structure similar to the CdCl2 type is observed when lithium nickelate is charged to a depth of charge of 0.94 (Li 0.06 Although its crystal structure is similar to that of NiO2, it is known that pure lithium cobaltate or layered rock salt-type cathode active materials containing a large amount of cobalt do not usually adopt this crystal structure.

[0216] In one embodiment of the present invention, the change in crystal structure at high charge depths, i.e., when a large amount of lithium has been desorbed, is suppressed compared to conventional positive electrode active materials. For example, as shown by the dotted line in Figure 9, there is almost no displacement of the CoO2 layer in these crystal structures.

[0217] More specifically, the positive electrode active material 100 according to one embodiment of the present invention exhibits high crystal structure stability even at high charging depths. For example, in conventional positive electrode active materials, there is a charging voltage range in which the R-3m(O3) crystal structure can be maintained even at charging voltages that result in an H1-3 type crystal structure, such as a voltage of about 4.6V relative to the potential of lithium metal. Furthermore, there is a range in which an O3' type crystal structure can be adopted even at higher charging voltages, such as voltages between 4.65V and 4.7V relative to the potential of lithium metal. Only when the charging voltage is increased even further may an H1-3 type crystal structure be observed. Moreover, even at lower charging voltages (for example, charging voltages between 4.5V and 4.6V relative to the potential of lithium metal), the positive electrode active material 100 according to one embodiment of the present invention may be able to adopt an O3' type crystal structure.

[0218] Therefore, in the positive electrode active material 100 of one aspect of the present invention, the crystal structure is less likely to collapse even when repeated charging and discharging occurs with a high depth of charge.

[0219] Furthermore, the space group of a crystal structure is identified by methods such as XRD, electron diffraction, and neutron diffraction. Therefore, in this specification, "belonging to a certain space group" or "being a certain space group" can be rephrased as "being identified to a certain space group."

[0220] Furthermore, in the case of a secondary battery, if graphite is used as the negative electrode active material, the voltage of the secondary battery will decrease by the amount of the graphite's potential compared to the above. The potential of graphite is approximately 0.05V to 0.2V relative to the potential of lithium metal. Therefore, for example, even when the voltage of a secondary battery using graphite as the negative electrode active material is between 4.3V and 4.5V, the positive electrode active material 100 of one embodiment of the present invention can maintain the R-3m(O3) crystal structure, and can also adopt the O3' type crystal structure in regions with higher charging voltages, for example, when the secondary battery voltage is above 4.5V and below 4.6V. Moreover, even at lower charging voltages, for example, when the secondary battery voltage is between 4.2V and 4.3V, the positive electrode active material 100 of one embodiment of the present invention may adopt the O3' type crystal structure.

[0221] The O3' type crystal structure can be represented by the coordinates of cobalt and oxygen in the unit cell as follows: Co(0,0,0.5), O(0,0,x), within the range of 0.20≦x≦0.25. The lattice constants of the unit cell are typically a=2.817(Å) and c=13.781(Å). Note that 1Å = 10⁻¹⁰ -10 It is m.

[0222] Additive elements, such as magnesium, that are randomly and dilutely present between CoO2 layers, i.e., at lithium sites, have the effect of suppressing CoO2 layer displacement when the depth of charge is high. Therefore, when magnesium is present between CoO2 layers, an O3' type crystal structure is more likely to be formed. For this reason, it is preferable that magnesium is distributed throughout the particles of the positive electrode active material 100 according to one embodiment of the present invention. Furthermore, in order to distribute magnesium throughout the particles, it is preferable to perform a heat treatment in the manufacturing process of the positive electrode active material 100 according to one embodiment of the present invention.

[0223] However, if the heat treatment temperature is too high, cation mixing occurs, increasing the likelihood that added elements, such as magnesium, will enter the cobalt site. Magnesium present in the cobalt site does not help maintain the R-3m structure at high charge depths. Furthermore, if the heat treatment temperature is too high, there are concerns about adverse effects such as the reduction of cobalt to its divalent state and the evaporation of lithium.

[0224] Therefore, it is preferable to add a fluorine compound to lithium cobalt oxide before the heat treatment to distribute magnesium throughout the particles. Adding a fluorine compound lowers the melting point of lithium cobalt oxide. By lowering the melting point, it becomes easier to distribute magnesium throughout the particles at a temperature where cation mixing is less likely to occur. Furthermore, the presence of a fluorine compound is expected to improve corrosion resistance to hydrofluoric acid produced by the decomposition of the electrolyte.

[0225] Furthermore, by performing the initial heating described above, the distribution of additive elements, including magnesium and aluminum, can be improved. As a result, even when the charging voltage is higher, for example, when the charging voltage is 4.6V to 4.8V and the charging depth is 0.8 to less than 0.9, it may be possible to maintain a crystal structure in which the displacement of the CoO2 layer is suppressed, without forming an H1-3 type crystal structure. This crystal structure has the same symmetry as the O3' type crystal structure, but its lattice constant is different from that of the O3' type crystal structure. For this reason, this structure is referred to as the O3'' type crystal structure in this specification. The O3'' type crystal structure has a layered structure. The O3'' type can also be said to be a crystal structure similar to the CdCl2 type crystal structure.

[0226] Furthermore, if the magnesium concentration is increased beyond the desired value, the effect on stabilizing the crystal structure may decrease. This is thought to be because magnesium will occupy not only lithium sites but also cobalt sites. In addition, unwanted magnesium compounds (e.g., oxides, fluorides, etc.) that do not substitute for lithium sites or cobalt sites may be unevenly distributed on the surface of the positive electrode active material and may become a resistive component. The number of magnesium atoms in the positive electrode active material of one embodiment of the present invention is preferably 0.001 times or more and 0.1 times or less than the number of atoms of the transition metal M, more preferably greater than 0.01 times and less than 0.04 times, and even more preferably about 0.02 times. Alternatively, 0.001 times or more and less than 0.04 times is preferred. Alternatively, 0.01 times or more and 0.1 times or less is preferred. The magnesium concentration shown here may be, for example, a value obtained by elemental analysis of the entire particle of the positive electrode active material using GD-MS (glow discharge mass spectrometer), ICP-MS (inductively coupled plasma mass spectrometer), etc., or it may be based on the value of the raw material composition during the process of manufacturing the positive electrode active material.

[0227] Nickel and other transition metals M, as well as aluminum, are preferably present at the cobalt site, but some may be present at the lithium site. Magnesium is also preferably present at the lithium site. Oxygen may be partially substituted with fluorine.

[0228] In one embodiment of the present invention, the charge-discharge capacity of the positive electrode active material may decrease as the magnesium concentration increases. One reason for this is that the amount of lithium contributing to charge-discharge decreases due to the presence of magnesium at the lithium sites. In addition, excess magnesium may generate magnesium compounds that do not contribute to charge-discharge. In one embodiment of the present invention, the charge-discharge capacity per unit weight and per unit volume may be increased by including nickel as metal Z in addition to magnesium. In another embodiment of the present invention, the charge-discharge capacity per unit weight and per unit volume may be increased by including aluminum as metal Z in addition to magnesium. In yet another embodiment of the present invention, the charge-discharge capacity per unit weight and per unit volume may be increased by including nickel and aluminum in addition to magnesium.

[0229] The concentrations of elements such as magnesium and metal Z in the positive electrode active material according to one embodiment of the present invention are expressed below in terms of the number of atoms.

[0230] The number of nickel atoms in the positive electrode active material 100 according to one aspect of the present invention is preferably more than 0% and 7.5% or less of the number of cobalt atoms, preferably 0.05% to 4%, preferably 0.1% to 2%, and more preferably 0.2% to 1%. Alternatively, it is preferably more than 0% and 4% or less. Alternatively, it is preferably more than 0% and 2% or less. Alternatively, it is preferably 0.05% to 7.5% or less. Alternatively, it is preferably 0.05% to 2% or less. Alternatively, it is preferably 0.1% to 7.5% or less. Alternatively, it is preferably 0.1% to 4% or less. The nickel concentration shown herein may be, for example, a value obtained by elemental analysis of the entire particle of the positive electrode active material using GD-MS, ICP-MS, etc., or it may be based on the value of the raw material composition during the manufacturing process of the positive electrode active material.

[0231] Nickel present at the above concentrations readily dissolves uniformly throughout the positive electrode active material 100, thus contributing particularly to the stabilization of the crystal structure of the interior 100b. Furthermore, the presence of divalent nickel in the interior 100b allows divalent additive elements, such as magnesium, which are randomly and dilutely present at lithium sites nearby, to exist more stably. As a result, magnesium leaching can be suppressed even after charging and discharging to high depths of charge. This can improve charge-discharge cycle characteristics. Thus, combining the effects of nickel in the interior 100b with the effects of magnesium, aluminum, titanium, fluorine, etc., in the surface layer 100a is extremely effective in stabilizing the crystal structure at high depths of charge.

[0232] The number of aluminum atoms in the positive electrode active material according to one embodiment of the present invention is preferably 0.05% to 4% of the number of cobalt atoms, preferably 0.1% to 2%, and more preferably 0.3% to 1.5%. Alternatively, 0.05% to 2% is preferred, or 0.1% to 4% is preferred. The aluminum concentration shown here may be, for example, a value obtained by elemental analysis of the entire particle of the positive electrode active material using GD-MS, ICP-MS, etc., or it may be based on the value of the raw material composition during the manufacturing process of the positive electrode active material.

[0233] In one embodiment of the present invention, it is preferable to further use phosphorus as an additive element in the positive electrode active material. Furthermore, it is more preferable that the positive electrode active material in one embodiment of the present invention has a compound containing phosphorus and oxygen.

[0234] In one embodiment of the present invention, the positive electrode active material contains a phosphorus-containing compound, which may suppress short circuits when a high charge depth state is maintained.

[0235] In one embodiment of the present invention, if the positive electrode active material contains phosphorus, the hydrogen fluoride generated by the decomposition of the electrolyte may react with the phosphorus, potentially reducing the concentration of hydrogen fluoride in the electrolyte.

[0236] If the electrolyte contains LiPF6, hydrolysis may generate hydrogen fluoride. Hydrogen fluoride may also be generated by the reaction between PVDF, used as a component of the positive electrode, and alkali. Reducing the hydrogen fluoride concentration in the electrolyte may suppress corrosion of the current collector and / or peeling of the coating 104. Furthermore, it may suppress the decrease in adhesion due to gelation and / or insolubilization of the PVDF.

[0237] In one embodiment of the present invention, when the positive electrode active material contains phosphorus in addition to magnesium, the stability at high charge depths is extremely high. When phosphorus is present, the number of phosphorus atoms is preferably 1% to 20% of the number of cobalt atoms, more preferably 2% to 10%, and even more preferably 3% to 8%. Alternatively, 1% to 10% is preferred. Alternatively, 1% to 8% is preferred. Alternatively, 2% to 20% is preferred. Alternatively, 2% to 8% is preferred. Alternatively, 3% to 20% is preferred. Alternatively, 3% to 10% is preferred. In addition, the number of magnesium atoms is preferably 0.1% to 10% of the number of cobalt atoms, more preferably 0.5% to 5%, and even more preferably 0.7% to 4%. Alternatively, 0.1% to 5% is preferred. Alternatively, 0.1% to 4% is preferred. Alternatively, 0.5% to 10% is preferred. Alternatively, 0.5% to 4% is preferred. Alternatively, 0.7% to 10% is preferred. Alternatively, a concentration of 0.7% to 5% is preferred. The concentrations of phosphorus and magnesium shown herein may be, for example, values ​​obtained by elemental analysis of the entire particle of the positive electrode active material using ICP-MS, or they may be based on the values ​​of the raw material formulation during the manufacturing process of the positive electrode active material.

[0238] The positive electrode active material may have cracks. The presence of phosphorus, or more specifically, a compound containing phosphorus and oxygen, in the region in contact with the crack, for example, the embedded portion 102, may suppress the propagation of the crack.

[0239] ≪Surface layer≫ It is preferable that magnesium is distributed throughout the particles of the positive electrode active material 100 according to one embodiment of the present invention, but in addition, it is preferable that the magnesium concentration in the surface layer 100a is higher than the average of the entire particle. Alternatively, it is preferable that the magnesium concentration in the surface layer 100a is higher than the concentration in the interior 100b. For example, it is preferable that the magnesium concentration in the surface layer 100a measured by XPS, etc., is higher than the average magnesium concentration of the entire particle measured by ICP-MS, etc. Alternatively, it is preferable that the magnesium concentration in the surface layer 100a measured by EDX surface analysis, etc., is higher than the magnesium concentration in the interior 100b.

[0240] Furthermore, in a case where the positive electrode active material 100 of one embodiment of the present invention has one or more metals selected from additive elements, such as aluminum, manganese, iron, and chromium, it is preferable that the concentration of the additive element in the surface layer 100a is higher than the average concentration of the entire particle. Alternatively, it is preferable that the concentration of the metal in the surface layer 100a is higher than the concentration in the interior 100b. For example, it is preferable that the concentration of additive elements other than cobalt in the surface layer 100a, as measured by XPS, is higher than the average concentration of the element in the entire particle, as measured by ICP-MS. Alternatively, it is preferable that the concentration of additive elements other than cobalt in the surface layer 100a, as measured by EDX surface analysis, is higher than the concentration of additive elements other than cobalt in the interior 100b.

[0241] Unlike the interior 100b, where the crystalline structure is maintained, the surface layer 100a has broken bonds, and during charging, lithium escapes from the surface, making it a region where the lithium concentration tends to be lower than in the interior. Therefore, it is a region that is prone to instability and where the crystalline structure is easily disrupted. A higher magnesium concentration in the surface layer 100a can more effectively suppress changes in the crystalline structure. Furthermore, a higher magnesium concentration in the surface layer 100a can also be expected to improve corrosion resistance to hydrofluoric acid produced by the decomposition of the electrolyte.

[0242] Furthermore, it is preferable that the concentration of fluorine in the surface layer 100a of the positive electrode active material 100 in one embodiment of the present invention is higher than the average concentration of fluorine throughout the entire particle. Alternatively, it is preferable that the fluorine concentration in the surface layer 100a is higher than the concentration in the interior 100b. The presence of fluorine in the surface layer 100a, which is the region in contact with the electrolyte, can effectively improve corrosion resistance to hydrofluoric acid.

[0243] Thus, it is preferable that the surface layer 100a of the positive electrode active material 100 in one aspect of the present invention has a different composition from the interior 100b, with higher concentrations of additive elements, such as magnesium and fluorine. Furthermore, it is preferable that the composition adopts a crystalline structure that is stable at room temperature (25°C). For this reason, the surface layer 100a may have a different crystalline structure from the interior 100b. For example, at least a part of the surface layer 100a of the positive electrode active material 100 in one aspect of the present invention may have a rock salt type crystalline structure. Also, if the surface layer 100a and the interior 100b have different crystalline structures, it is preferable that the orientation of the crystals in the surface layer 100a and the interior 100b is approximately the same.

[0244] Layered rock salt crystals, and the anions in rock salt crystals, adopt a cubic close-packed structure (face-centered cubic lattice structure). It is also presumed that the anions in O3'-type crystals adopt a cubic close-packed structure.

[0245] In this specification, a structure in which anions are stacked in three layers with offsets from each other, such as ABCABC, will be referred to as a cubic close-packed structure. Therefore, the anions do not need to be strictly cubic in shape. At the same time, since real crystals always have defects, the analytical results do not necessarily conform to theory. For example, in FFT (Fast Fourier Transform) patterns such as electron diffraction patterns or TEM images, spots may appear at positions slightly different from the theoretical positions. For example, if the orientation from the theoretical position is 5 degrees or less, or 2.5 degrees or less, it can be said that it adopts a cubic close-packed structure.

[0246] When layered rock salt crystals are in contact with other rock salt crystals, there exists a crystal plane in which the orientation of the cubic close-packed structure composed of anions is aligned.

[0247] Alternatively, it can be explained as follows: The anions in the (111) plane of the cubic crystal structure have a triangular lattice. The layered rock salt type has a space group R-3m and a rhombohedral structure, but to facilitate understanding of the structure, it is generally represented by a composite hexagonal lattice, and the (0001) plane of the layered rock salt type has a hexagonal lattice. The triangular lattice of the cubic (111) plane has a similar atomic arrangement to the hexagonal lattice of the (0001) plane of the layered rock salt type. The consistency between the two lattices can be described as the orientation of the cubic close-packed structure being aligned.

[0248] However, the space group of layered rock salt crystals and O3'-type crystals is R-3m, which is different from the space group Fm-3m of rock salt crystals (the space group of typical rock salt crystals). Therefore, the Miller indices of crystal planes that satisfy the above conditions differ between layered rock salt crystals and O3'-type crystals and rock salt crystals. In this specification, it is sometimes said that the crystal orientations are approximately the same when the orientations of the cubic close-packed structure composed of anions are aligned in layered rock salt crystals, O3'-type and O3''-type crystals, and rock salt crystals.

[0249] The approximate agreement of crystal orientation in two regions can be determined from TEM (Transmission Electron Microscope) images, STEM (Scanning Transmission Electron Microscope) images, HAADF-STEM (High-angle Annular Dark Field Scanning TEM) images, ABF-STEM (Annular Bright-Field Scanning Transmission Electron Microscope) images, electron diffraction patterns, FFT patterns of TEM images, etc. XRD (X-ray Diffraction) and neutron diffraction can also be used as indicators.

[0250] Figure 16 shows an example of a TEM image in which the orientations of layered rock salt crystals (LRS) and rock salt crystals (RS) are roughly consistent. TEM, STEM, HAADF-STEM, ABF-STEM, etc., yield images that reflect the crystal structure.

[0251] For example, in high-resolution TEM images, contrast originating from crystal planes can be obtained. Due to the diffraction and interference of electron beams, for example, when an electron beam is incident perpendicular to the c-axis of a layered rock salt composite hexagonal lattice, contrast originating from the (0003) plane is obtained as a repetition of bright bands (bright strips) and dark bands (dark strips). Therefore, in TEM images, a repetition of bright and dark lines is observed, and the bright lines interact with each other (for example, L as shown in Figure 16). RS and L LRS If the angle between the dark lines is 5 degrees or less, or 2.5 degrees or less, it can be determined that the crystal planes roughly coincide, i.e., the crystal orientations roughly coincide. Similarly, if the angle between the dark lines is 5 degrees or less, or 2.5 degrees or less, it can be determined that the crystal orientations roughly coincide.

[0252] Furthermore, HAADF-STEM images provide contrast corresponding to atomic number, with elements with higher atomic numbers appearing brighter. For example, in the case of layered rock salt lithium cobalt oxide belonging to space group R-3m, cobalt (atomic number 27) has the highest atomic number, so electron beams are strongly scattered at the positions of cobalt atoms, and the arrangement of cobalt atoms is observed as bright lines or a sequence of bright points. Therefore, when lithium cobalt oxide with a layered rock salt crystal structure is observed perpendicular to the c-axis, the arrangement of cobalt atoms perpendicular to the c-axis is observed as bright lines or a sequence of bright points, while the arrangement of lithium atoms and oxygen atoms is observed as dark lines or low-brightness regions. The same applies when lithium cobalt oxide contains fluorine (atomic number 9) and magnesium (atomic number 12) as additive elements.

[0253] Therefore, in HAADF-STEM images, if the repetition of bright and dark lines is observed in two regions with different crystal structures, and the angle between the bright lines is 5 degrees or less, or 2.5 degrees or less, it can be determined that the atomic arrangement is roughly consistent, i.e., the crystal orientation is roughly consistent. Similarly, if the angle between the dark lines is 5 degrees or less, or 2.5 degrees or less, it can also be determined that the crystal orientation is roughly consistent.

[0254] In ABF-STEM, elements with smaller atomic numbers appear brighter, but since contrast corresponding to atomic number is obtained, similar to HAADF-STEM, the orientation of the crystal can be determined in the same way as with HAADF-STEM images.

[0255] Figure 17(A) shows an example of a STEM image where the orientations of layered rock salt crystals (LRS) and rock salt crystals (RS) are roughly consistent. The FFT pattern of the rock salt crystal region is shown in Figure 17(B), and the FFT pattern of the layered rock salt crystal region (LRS) is shown in Figure 17(C). The left side of Figures 17(B) and 17(C) shows the composition, JCPDS card number, and the d-value and angle calculated from these. The right side shows the measured values. Spots marked with O represent zero-order diffraction.

[0256] The spot labeled A in Figure 17(B) originates from the 11-1 reflection of the cubic crystal. The spot labeled A in Figure 17(C) originates from the 0003 reflection of the layered rock salt type. From Figures 17(B) and 17(C), it can be seen that the orientation of the 11-1 reflection of the cubic crystal and the orientation of the 0003 reflection of the layered rock salt type are roughly coincide. That is, the line passing through AO in Figure 17(B) and the line passing through AO in Figure 17(C) are roughly parallel. Here, roughly coincidental and roughly parallel means that the angle is 5 degrees or less, or 2.5 degrees or less.

[0257] Thus, in FFT patterns and electron diffraction, if the orientations of the layered rock salt crystal and the rock salt crystal are roughly the same, the <0003> orientation of the layered rock salt crystal and the <11-1> orientation of the rock salt crystal may roughly coincide. In this case, it is preferable that these reciprocal lattice points are spot-like, that is, not continuous with other reciprocal lattice points. The fact that the reciprocal lattice points are spot-like and not continuous with other reciprocal lattice points indicates high crystallinity.

[0258] Furthermore, as mentioned above, if the orientation of the 11-1 reflection of the cubic crystal and the orientation of the 0003 reflection of the layered rock salt type roughly coincide, depending on the incident orientation of the electron beam, spots not originating from the 0003 reflection of the layered rock salt type may be observed in a reciprocal space different from the orientation of the 0003 reflection of the layered rock salt type. For example, the spot labeled B in Figure 17(C) originates from the 1014 reflection of the layered rock salt type. This spot may be observed at an angle of 52° to 56° from the orientation of the reciprocal point originating from the 0003 reflection of the layered rock salt type (A in Figure 17(C)) (i.e., ∠AOB is between 52° and 56°), and where d is between 0.19 nm and 0.21 nm. Note that this index is just an example and does not necessarily have to match. For example, a reciprocal point equivalent to 0003 and 1014 would also be acceptable.

[0259] Similarly, spots not originating from the cubic 11-1 reflection may be observed in reciprocal space at a different orientation than the orientation where the cubic 11-1 reflection was observed. For example, the spot labeled B in Figure 17(B) originates from the cubic 200 reflection. This is because diffraction spots may be observed at an angle between 54° and 56° from the orientation of the cubic 11-1 reflection (A in Figure 17(B)) (i.e., ∠AOB is between 54° and 56°). Note that this index is just an example and does not necessarily have to match. For example, it could be a reciprocal lattice point equivalent to 11-1 and 200.

[0260] It is known that layered rock salt type cathode active materials, including lithium cobalt oxide, tend to exhibit (0003) planes and equivalent planes, as well as (10-14) planes and equivalent planes, as crystal planes. Therefore, when observing the shape of the cathode active material with SEM or the like, it is possible to thin the observation sample using FIB or the like so that the electron beam is incident at [12-10] in a TEM or the like, in order to make the (0003) plane easier to observe. When it is necessary to determine the consistency of the crystal orientation, it is preferable to thin the sample so that the (0003) plane of the layered rock salt type is easily observable.

[0261] However, if the surface layer 100a consists only of MgO, or only of a solid solution of MgO and CoO(II), lithium insertion and removal becomes difficult. Therefore, the surface layer 100a must contain at least cobalt, and in the discharge state, it must also contain lithium and have pathways for lithium insertion and removal. Furthermore, it is preferable that the concentration of cobalt is higher than that of magnesium.

[0262] Furthermore, it is preferable that the additive element X is located on the surface layer 100a of the positive electrode active material 100 according to one aspect of the present invention. For example, the positive electrode active material 100 according to one aspect of the present invention may be covered with a coating 104 having the additive element X.

[0263] ≪Grain boundary≫ In one embodiment of the present invention, the additive elements in the positive electrode active material 100 are, in addition to the distribution described above, more preferably partially concentrated at the grain boundaries 101 and their vicinity, as shown in Figure 4(A).

[0264] More specifically, it is preferable that the magnesium concentration at and near the grain boundary 101 of the positive electrode active material 100 is higher than that in other regions of the interior 100b. It is also preferable that the fluorine concentration at and near the grain boundary 101 is higher than that in other regions of the interior 100b.

[0265] The grain boundary 101 is a type of surface defect. Therefore, like the grain surface, it is prone to instability, and changes in the crystal structure are likely to begin. For this reason, if the magnesium concentration at and near the grain boundary 101 is high, changes in the crystal structure can be suppressed more effectively.

[0266] Furthermore, if the magnesium and fluorine concentrations are high at and near the grain boundary 101, even if a crack occurs along the grain boundary 101 of the positive electrode active material 100 according to one embodiment of the present invention, the magnesium and fluorine concentrations will be high near the surface created by the crack. Therefore, the corrosion resistance to hydrofluoric acid can be improved even in the positive electrode active material after the crack has occurred.

[0267] In this specification, the vicinity of grain boundary 101 refers to the region extending approximately 10 nm from the grain boundary. Furthermore, grain boundary 101 refers to a plane where the arrangement of atoms changes and can be observed with an electron microscope. Specifically, it refers to areas where the angle between repeating bright and dark lines exceeds 5 degrees in the electron microscope image, or areas where the crystal structure can no longer be observed.

[0268] ≪Particle size≫ In one embodiment of the present invention, if the particle size of the positive electrode active material 100 is too large, problems arise such as difficulty in lithium diffusion and excessive roughness of the surface of the active material layer when coated onto the current collector. On the other hand, if it is too small, problems arise such as difficulty in supporting the active material layer when coating onto the current collector and excessive reaction with the electrolyte. Therefore, the median diameter (D50) is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 40 μm or less, and even more preferably 5 μm or more and 30 μm or less. Or preferably 1 μm or more and 40 μm or less. Or preferably 1 μm or more and 30 μm or less. Or preferably 2 μm or more and 100 μm or less. Or preferably 2 μm or more and 30 μm or less. Or preferably 5 μm or more and 100 μm or less. Or preferably 5 μm or more and 40 μm or less.

[0269] <Analysis method> Whether a positive electrode active material is a positive electrode active material 100 according to one embodiment of the present invention, which exhibits an O3' or O3'' type crystal structure at high charge depths, can be determined by analyzing a positive electrode having a positive electrode active material with high charge depths using XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), etc. XRD is particularly preferable because it can analyze the symmetry of transition metals such as cobalt in the positive electrode active material with high resolution, compare the crystallinity and crystal orientation, analyze the periodic distortion of the lattice and crystallite size, and obtain sufficient accuracy even when measuring a positive electrode obtained by disassembling a secondary battery.

[0270] One aspect of the present invention, the positive electrode active material 100, is characterized by minimal change in its crystal structure between a high depth of charge state and a discharge state, as described above. Materials in which a crystal structure with a large change from the discharge state accounts for 50 wt% or more in the high depth of charge state are undesirable because they cannot withstand charging and discharging to high depths of charge. It is important to note that simply adding additive elements may not result in the desired crystal structure. For example, even if both materials are lithium cobalt oxide containing magnesium and fluorine, there are cases where the O3' and O3'' type crystal structures account for 60 wt% or more in the high depth of charge state, and cases where the H1-3 type crystal structure accounts for 50 wt% or more. Furthermore, at a predetermined voltage, the O3' and O3'' type crystal structures account for almost 100 wt%, and if the predetermined voltage is further increased, the H1-3 type crystal structure may be generated. Therefore, to determine whether or not a material is the positive electrode active material 100 of one aspect of the present invention, analysis of the crystal structure, including XRD, is necessary.

[0271] However, positive electrode active materials in high-depth charge or discharge states may undergo changes in their crystal structure when exposed to air. For example, they may change from O3' and O3'' type crystal structures to H1-3 type crystal structures. Therefore, it is preferable to handle all samples in an inert atmosphere such as an argon atmosphere.

[0272] ≪Charging method≫ High-voltage charging to determine whether a certain composite oxide is the positive electrode active material 100 according to one aspect of the present invention can be performed, for example, by fabricating a coin cell (CR2032 type, 20 mm in diameter and 3.2 mm in height) with lithium as the counter electrode and then charging it.

[0273] More specifically, the positive electrode can be made by coating an aluminum foil positive electrode current collector with a slurry of a mixture of positive electrode active material, conductive material, and binder.

[0274] Lithium metal can be used for the counter electrode. However, if a material other than lithium metal is used for the counter electrode, the potential of the secondary battery and the potential of the positive electrode will differ. Unless otherwise specified, the voltage and potential in this specification refer to the potential of the positive electrode.

[0275] The electrolyte in the electrolyte solution may be 1 mol / L lithium hexafluoride phosphate (LiPF6), and the electrolyte solution may be a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7, and vinylene carbonate (VC) at 2 wt%.

[0276] A 25 μm thick porous polypropylene film can be used as the separator.

[0277] The positive electrode and negative electrode cans can be made of stainless steel (SUS).

[0278] The coin cell prepared under the above conditions is charged with a constant current of 10 mA / g (0.05 C when 1 C is 200 mA / g) to an arbitrary voltage (e.g., 4.5V, 4.6V, 4.65V, 4.7V, 4.75V, or 4.8V). It is desirable to charge with such a small current to observe the phase change of the positive electrode active material. The temperature is 25°C or 45°C. After charging in this manner, the coin cell is disassembled in a glove box under an argon atmosphere, and the positive electrode is removed to obtain a positive electrode active material with a high depth of charge. When performing various analyses afterward, it is preferable to seal the cell under an argon atmosphere to suppress reactions with external components. For example, XRD can be performed by sealing the cell in a sealed container under an argon atmosphere. Furthermore, it is preferable to remove the positive electrode and subject it to analysis as soon as possible after charging is complete. Specifically, it is preferable to do so within 1 hour, and more preferably within 30 minutes.

[0279] Furthermore, when analyzing the crystal structure of the charged state after multiple charge-discharge cycles, the conditions for these multiple charge-discharge cycles may differ from the charging conditions described above. For example, charging can be performed by constant current charging at a current of 100 mA / g (0.5 C when 1 C is 200 mA / g) up to an arbitrary voltage (e.g., 4.6 V, 4.65 V, 4.7 V, 4.75 V, or 4.8 V), then constant voltage charging until the current reaches 10 mA / g (0.05 C when 1 C is 200 mA / g), and then constant current discharge at 2.5 V and 0.5 C.

[0280] Furthermore, when analyzing the crystal structure of the discharged state after multiple charge-discharge cycles, a constant current discharge can be performed, for example, at 2.5V and a current value of 100mA / g (0.5C when 1C is 200mA / g).

[0281] ≪XRD≫ The equipment and conditions for XRD measurement are not particularly limited. For example, measurements can be taken using the following equipment and conditions. XRD system: Bruker AXS D8 ADVANCE X-ray source:CuKα1 ray Output: 40kV, 40mA Slit type: Div.Slit, 0.5° Detector: LynxEye Scanning method: 2θ / θ continuous scan Measurement range (2θ): 15° to 90° Step width (2θ): 0.01° setting Counting time: 1 second / step Sample stage rotation: 15 rpm

[0282] If the sample to be measured is a powder, it can be set up by placing it in a glass sample holder or by sprinkling the sample onto a grease-coated silicone anti-reflective plate. If the sample to be measured is a positive electrode, the positive electrode can be attached to a substrate with double-sided tape, and the positive electrode active material layer can be set up to match the measurement surface required by the device.

[0283] Figures 10, 12, 13(A), and 13(B) show the ideal powder XRD patterns calculated using CuKα1 radiation from the O3'-type crystal structure and the H1-3-type crystal structure models. For comparison, the ideal XRD patterns calculated from the crystal structures of LiCoO2 (O3) with a charging depth of 0 and CoO2 (O1) with a charging depth of 1 are also shown. Figures 13(A) and 13(B) show the XRD patterns of the O3'-type crystal structure and the H1-3-type crystal structure side by side. Figure 13(A) is an enlarged view of the region where the 2θ range is between 18° and 21°, and Figure 13(B) is an enlarged view of the region where the 2θ range is between 42° and 46°. The patterns for LiCoO2(O3) and CoO2(O1) were created using the Reflex Powder Diffraction module in Materials Studio (BIOVIA) from crystal structure information obtained from ICSD (Inorganic Crystal Structure Database) (see Non-Patent Document 4). The 2θ range was set to 15° to 75°, with a step size of 0.01 and a wavelength λ1 = 1.540562 × 10⁻¹⁰. -10m and λ2 were not set, and the Monochromator was set to single. The H1-3 type crystal structure pattern was similarly created from the crystal structure information described in Non-Patent Literature 3. For the O3' type crystal structure pattern, the crystal structure was estimated from the XRD pattern of the positive electrode active material of one embodiment of the present invention, fitted using TOPAS ver.3 (crystal structure analysis software manufactured by Bruker), and the XRD pattern was created in the same manner as the others.

[0284] As shown in Figures 10 and 13, in the O3' type crystal structure, diffraction peaks appear at 2θ = 19.30 ± 0.20° (19.10° to 19.50°) and 2θ = 45.55 ± 0.10° (45.45° to 45.65°). More specifically, sharp diffraction peaks appear at 2θ = 19.30 ± 0.10° (19.20° to 19.40°) and 2θ = 45.55 ± 0.05° (45.50° to 45.60°). However, as shown in Figures 12 and 13, these peaks do not appear in the H1-3 type crystal structure and CoO2 (P-3m1, O1). Therefore, the appearance of peaks at 2θ = 19.30 ± 0.20° and 2θ = 45.55 ± 0.10° at a high depth of charge is a characteristic feature of the positive electrode active material 100 in one embodiment of the present invention.

[0285] This can also be described as the position where the XRD diffraction peaks appear being close between the crystal structure at a charging depth of 0 and the crystal structure at a high charging depth. More specifically, it can be said that for two or more, more preferably three or more, of the main diffraction peaks of the two structures, the difference in the position where the peaks appear is 2θ = 0.7 or less, and more preferably 2θ = 0.5 or less.

[0286] Although not shown in the diagram, in the O3" type crystal structure, diffraction peaks appear at 2θ = 19.47 ± 0.10° (19.37° to 19.57°) and 2θ = 45.62 ± 0.05° (45.57° to 45.67°). In the H1-3 type crystal structure and CoO2 (P-3m1, O1), peaks do not appear at these positions. Therefore, the appearance of peaks at 2θ = 19.47 ± 0.10° and 2θ = 45.62 ± 0.05° in a higher depth of charge state can be said to be a characteristic of the positive electrode active material 100 of one embodiment of the present invention, which is prepared after initial heating. A higher depth of charge state refers to, for example, a charging state in which the charging voltage is 4.8V or higher, and / or a depth of charge greater than 0.8 and 0.88 or less, more specifically, a state in which the depth of charge is 0.83 or more and 0.85 or less.

[0287] In one embodiment of the present invention, the positive electrode active material 100 has an O3' type or O3'' type crystal structure when the depth of charge is high, but not all particles have to have an O3' type or O3'' type crystal structure. Other crystal structures may be included, or part of it may be amorphous. However, when Rietveld analysis is performed on the XRD pattern, it is preferable that the O3' type and O3'' type crystal structures make up 50% or more, more preferably 60% or more, and even more preferably 66% or more. If the O3' type and O3'' type crystal structures make up 50% or more, more preferably 60% or more, and even more preferably 66% or more, a positive electrode active material with sufficiently excellent cycle characteristics can be obtained.

[0288] Furthermore, even after more than 100 charge-discharge cycles from the start of measurement, it is preferable that the O3' and O3'' crystal structures make up 35% or more, more preferably 40% or more, and even more preferably 43% or more when Rietveld analysis is performed.

[0289] Furthermore, the sharpness of diffraction peaks in the XRD pattern indicates high crystallinity. Therefore, it is preferable for each diffraction peak after charging to be sharp, i.e., have a narrow full width at half maximum (FMAX). The FMAX can vary depending on the XRD measurement conditions and / or the value of 2θ, even for peaks originating from the same crystalline phase. Under the measurement conditions described above, for peaks observed between 2θ = 43° and 46°, the FMAX is preferably 0.2° or less, more preferably 0.15° or less, and even more preferably 0.12° or less. It is not necessary for all peaks to satisfy this requirement. If some peaks satisfy this requirement, it can be said that the crystal phase has high crystallinity. Such high crystallinity contributes to the stabilization of the crystal structure after charging.

[0290] Furthermore, the crystallite size of the O3'-type crystal structure possessed by the particles of the positive electrode active material decreases to only about 1 / 10th of that of LiCoO2(O3) in the discharged state. Therefore, even under the same XRD measurement conditions as the positive electrode before charging and discharging, a clear peak of the O3'-type crystal structure can be observed when the depth of charge is high. On the other hand, in simple LiCoO2, even if some parts can adopt a structure similar to the O3'-type crystal structure, the crystallite size becomes small, and the peak becomes broad and small. The crystallite size can be determined from the full width at half maximum of the XRD peak.

[0291] In one embodiment of the present invention, the positive electrode active material preferably has a small effect of the Jahn-Teller effect, as described above. The positive electrode active material in one embodiment of the present invention preferably has a layered rock salt type crystal structure and mainly contains cobalt as a transition metal. In addition, in one embodiment of the present invention, the positive electrode active material may contain metal Z as described above, in addition to cobalt, as long as the effect of the Jahn-Teller effect is small.

[0292] In the cathode active material, we will use XRD analysis to investigate the range of lattice constants in which the Jahn-Teller effect is presumed to be small.

[0293] Figure 14 shows the results of calculating the lattice constants of the a-axis and c-axis using XRD when the positive electrode active material of one embodiment of the present invention has a layered rock salt type crystal structure and contains cobalt and nickel. Figure 14(A) shows the results for the a-axis, and Figure 14(B) shows the results for the c-axis. The XRD patterns used for these calculations are from the powder after synthesis of the positive electrode active material, before it is incorporated into the positive electrode. The nickel concentration on the horizontal axis represents the nickel concentration when the sum of the number of cobalt and nickel atoms is taken as 100%. The positive electrode active material was prepared according to the method shown in Figure 2, except that an aluminum source was not used.

[0294] Figure 15 shows the results of estimating the lattice constants on the a-axis and c-axis using XRD when the positive electrode active material according to one embodiment of the present invention has a layered rock salt type crystal structure and contains cobalt and manganese. Figure 15(A) shows the results for the a-axis, and Figure 15(B) shows the results for the c-axis. Note that the lattice constants shown in Figure 15 are for the powder after synthesis of the positive electrode active material, and were measured by XRD before being incorporated into the positive electrode. The manganese concentration on the horizontal axis represents the manganese concentration when the sum of the number of cobalt and manganese atoms is taken as 100%. The positive electrode active material was prepared according to the manufacturing method in Figure 2, except that a manganese source was used instead of a nickel source, and an aluminum source was not used.

[0295] Figure 14(C) shows the a-axis lattice constant divided by the c-axis lattice constant (a-axis / c-axis) for the positive electrode active material whose lattice constant results are shown in Figures 14(A) and 14(B). Figure 15(C) shows the a-axis lattice constant divided by the c-axis lattice constant (a-axis / c-axis) for the positive electrode active material whose lattice constant results are shown in Figures 15(A) and 15(B).

[0296] Figure 14(C) shows a significant change in the a-axis / c-axis at nickel concentrations of 5% and 7.5%, with the a-axis distortion being larger at a nickel concentration of 7.5%. This distortion may be Jahn-Teller distortion. This suggests that a superior cathode active material with low Jahn-Teller distortion can be obtained at nickel concentrations below 7.5%.

[0297] Next, Figure 15(A) suggests that when the manganese concentration is 5% or higher, the behavior of the lattice constant changes is different and does not follow Vegard's law. Therefore, it is suggested that the crystal structure is different when the manganese concentration is 5% or higher. Thus, a manganese concentration of, for example, 4% or less is preferable.

[0298] It should be noted that the above-mentioned ranges for nickel and manganese concentrations do not necessarily apply to the surface layer 100a. In other words, higher concentrations may be acceptable in the surface layer 100a.

[0299] Based on the above considerations regarding the preferred range of lattice constants, in a positive electrode active material according to one embodiment of the present invention, the layered rock salt type crystal structure of the particles of the positive electrode active material in a non-charged or discharged state, as estimated from the XRD pattern, has a lattice constant of 2.814 × 10⁻¹⁴ in the a-axis. -10 Larger than m, 2.817 × 10 -10 It is smaller than m, and the lattice constant of the c axis is 14.05 × 10⁻¹⁰. -10 Larger than m, 14.07 × 10 -10 It was found that a value smaller than m is preferable. The state without charging and discharging may, for example, be the powder state before the positive electrode of the secondary battery is manufactured.

[0300] Alternatively, in the layered rock salt type crystal structure of the positive electrode active material in a non-charging / discharging state or in a discharged state, it is preferable that the value obtained by dividing the lattice constant of the a-axis by the lattice constant of the c-axis (a-axis / c-axis) is greater than 0.20000 and less than 0.20049.

[0301] Alternatively, when XRD analysis is performed on the layered rock salt-type crystal structure of the positive electrode active material in a non-charging or discharged state, a first peak may be observed when 2θ is between 18.50° and 19.30°, and a second peak may be observed when 2θ is between 38.00° and 38.80°.

[0302] The peaks appearing in the powder XRD pattern reflect the crystal structure of the interior 100b of the positive electrode active material 100, which occupies most of the volume of the positive electrode active material 100. The crystal structure of the surface layer 100a, grain boundaries 101, etc., can be analyzed by electron diffraction of the cross-section of the positive electrode active material 100.

[0303] ≪Charging curve and dQ / dV vs sV curve≫ In one embodiment of the present invention, the positive electrode active material 100 may exhibit a characteristic voltage change as the depth of charge increases. The voltage change can be read from the dQ / dVvsV curve obtained by differentiating the capacitance (Q) of the charging curve with respect to voltage (V) (dQ / dV). For example, it is thought that a non-equilibrium phase change occurs before and after the peak in the dQ / dVvsV curve, and that the crystal structure changes significantly. In this specification, a non-equilibrium phase change refers to a phenomenon that causes a nonlinear change in a physical quantity.

[0304] In one embodiment of the present invention, the positive electrode active material 100 may have a broad peak around 4.55V in the dQ / dVvsV curve. The peak around 4.55V reflects the voltage change during the phase transition from the O3 type crystal structure to the O3' type crystal structure. Therefore, a broad peak means that the change in energy required to extract lithium is smaller than when the peak is sharp, i.e., the change in crystal structure is smaller. Smaller changes are preferable because they reduce the influence of shift and volume changes in the CoO2 layer.

[0305] More specifically, in the dQ / dV vs V curve of the charging curve, when the maximum value appearing between 4.5V and 4.6V is defined as the first peak, a full width at half maximum (FMAX) of the first peak of 0.10V or more is considered sufficiently broad and preferable. In this specification, the full width at half maximum (FMAX) of the first peak is defined as the difference between HWHM1, which is the average value of the first peak and the first minimum value when the minimum value of the dQ / dV value appearing between 4.3V and 4.5V is defined as the first minimum value, and HWHM2, which is the average value of the first peak and the second minimum value when the minimum value of the dQ / dV value appearing between 4.6V and 4.8V is defined as the second minimum value.

[0306] When acquiring the dQ / dV vs V curve, charging can be performed using constant current charging at 10mA / g (0.05C when 1C is set to 200mA / g) up to, for example, 4.9V. Furthermore, when acquiring the dQ / dV value for the initial charge, it is preferable to discharge the battery to 2.5V at 0.5C before starting the above charging process.

[0307] The data acquisition interval during charging can be set to, for example, every second or to acquire voltage and current when there is a voltage fluctuation of 1 mV. The integrated value of the current and time is used as the charging capacity.

[0308] The difference between the nth and (n+1)th data points of the above charging capacity data is taken as the nth value of the capacity change dQ. Similarly, the difference between the nth and (n+1)th data points of the above voltage data is taken as the nth value of the voltage change dV.

[0309] However, since the above data is susceptible to the effects of minute noise, the dQ / dV value may be calculated from a moving average of a certain number of intervals for the difference between voltage and charging capacity. The number of intervals can be, for example, 500.

[0310] Specifically, the average value of dQ from the nth to the n+500th value is calculated, and similarly, the average value of dV from the nth to the n+500th value is calculated. The dQ / dV value can be obtained by dividing dQ(average of 500 values) by dV(average of 500 values). Similarly, the voltage on the horizontal axis of the dQ / dV vs V graph can also use the value of a moving average with 500 intervals.

[0311] Furthermore, when analyzing the dQ / dV vs. V curve after multiple charge-discharge cycles, the conditions for these multiple cycles may differ from the charging conditions described above. For example, charging can be performed at an arbitrary voltage (e.g., 4.6V, 4.65V, 4.7V, 4.75V, or 4.8V) with a constant current of 0.5C (1C = 200mA / g), followed by constant voltage charging until the current reaches 0.05C, and then discharging can be performed at 2.5V with a constant current of 0.5C.

[0312] Furthermore, a phase change occurs from the O3-type crystal structure to the O3'-type crystal structure around 4.55V, where the O3-type crystal structure has a charging depth of approximately 0.7. This has the same symmetry as the O3-type crystal structure with a charging depth of 0, as explained in Figure 11, but the distance between the CoO2 layers is slightly different. In this specification, when distinguishing between O3-type crystal structures with different charging depths, the O3-type crystal structure with a charging depth of 0 is referred to as O3(2θ=18.85), and the O3-type crystal structure with a charging depth of approximately 0.7 is referred to as O3(2θ=18.57). This is because the position of the peak that appears around 2θ = 19° in XRD measurements corresponds to the distance between the CoO2 layers.

[0313] ≪Discharge curves and dQ / dV vs. sV curves≫ Furthermore, in one embodiment of the present invention, when the positive electrode active material 100 is charged at a high voltage and then discharged at a low rate of, for example, 0.2C or less, a characteristic voltage change may appear near the end of discharge. This change can be clearly confirmed by the presence of at least one peak in the dQ / dVvsV curve obtained from the discharge curve, at a voltage lower than the peak that appears around 3.9V and in the range up to 3.5V.

[0314] ≪Current pause method≫ The magnesium and other additive elements present in the surface layer of the positive electrode active material 100 according to one aspect of the present invention may undergo slight changes in their distribution during repeated charging and discharging cycles. For example, the distribution of the additive elements may improve, leading to a decrease in the electron conduction resistance. As a result, the electrical resistance, i.e., the fast-responding resistance component R(0.1s) measured by the current pause method, may decrease in the initial stages of the charge-discharge cycle.

[0315] For example, when comparing the nth charge (where n is a natural number greater than 1) with the (n+1)th charge, the fast-responding resistance component R(0.1s), measured by the current pause method, may be lower in the (n+1)th charge than in the nth charge. Consequently, the discharge capacity in the (n+1)th charge may be higher than that in the nth charge. When n is 1, that is, when comparing the first charge with the second charge, the second charge capacity may be larger, which can occur even with positive electrode active materials that do not contain additive elements. Therefore, it is preferable that n is, for example, between 2 and 10. However, this is not limited to the initial stages of the charge-discharge cycle. A charge-discharge capacity that is approximately equal to the rated capacity, for example, 97% or more of the rated capacity, can be considered the initial stage of the charge-discharge cycle.

[0316] ≪XPS≫ X-ray photoelectron spectroscopy (XPS) allows for analysis of regions from the surface to a depth of approximately 2 to 8 nm (usually less than 5 nm), enabling quantitative analysis of elemental concentrations in a region roughly half the depth of the surface layer (100a). Furthermore, narrow-scan analysis allows for the analysis of elemental bonding states. The quantitative accuracy of XPS is typically around ±1 atomic percent, and the detection limit is approximately 1 atomic percent, although this varies depending on the element.

[0317] When XPS analysis is performed on the positive electrode active material 100 according to one embodiment of the present invention, the number of atoms of the additive element is preferably 1.6 to 6.0 times the number of atoms of the transition metal M, and more preferably 1.8 to less than 4.0 times. When the additive element is magnesium and the transition metal M is cobalt, the number of magnesium atoms is preferably 1.6 to 6.0 times the number of cobalt atoms, and more preferably 1.8 to less than 4.0 times. Furthermore, the number of halogen atoms such as fluorine is preferably 0.2 to 6.0 times the number of atoms of the transition metal M, and more preferably 1.2 to 4.0 times.

[0318] For XPS analysis, for example, monochromatic aluminum Kα radiation can be used as the X-ray source. The extraction angle can be set to, for example, 45°. Measurements can be performed using, for example, the following equipment and conditions. Measurement device: PHI QuanteraII X-ray source: Monochromatic Al Kα (1486.6eV) Detection area: 100 μmφ Detection depth: Approximately 4-5 nm (extraction angle 45°) Measurement spectrum: Wide scan, narrow scan of each detected element

[0319] Furthermore, when the positive electrode active material 100 according to one embodiment of the present invention is subjected to XPS analysis, the peak indicating the bond energy between fluorine and other elements is preferably 682 eV or more and less than 685 eV, and more preferably around 684.3 eV. This value is different from both the bond energy of lithium fluoride, which is 685 eV, and the bond energy of magnesium fluoride, which is 686 eV. In other words, when the positive electrode active material 100 according to one embodiment of the present invention contains fluorine, it is preferable that the bond is with something other than lithium fluoride and magnesium fluoride.

[0320] Furthermore, when the positive electrode active material 100 according to one embodiment of the present invention is subjected to XPS analysis, the peak indicating the bond energy between magnesium and other elements is preferably 1302 eV or more and less than 1304 eV, and more preferably around 1303 eV. This value is different from the bond energy of magnesium fluoride, which is 1305 eV, and is close to the bond energy of magnesium oxide. In other words, when the positive electrode active material 100 according to one embodiment of the present invention contains magnesium, it is preferable that the bond is with an element other than magnesium fluoride.

[0321] For additive elements that are preferably present in large quantities in the surface layer 100a, such as magnesium and aluminum, it is preferable that the concentration measured by XPS or the like is higher than the concentration measured by ICP-MS (inductively coupled plasma mass spectrometry) or GD-MS (glow discharge mass spectrometry).

[0322] When magnesium and aluminum are processed to expose their cross-sections and analyzed using TEM-EDX, it is preferable that the concentration in the surface layer 100a is higher than the concentration in the interior 100b. For example, in TEM-EDX analysis, it is preferable that the magnesium concentration is attenuated to 60% or less of the peak at a depth of 1 nm from the peak top. It is also preferable that it is attenuated to 30% or less of the peak at a depth of 2 nm from the peak top. Processing can be performed, for example, by FIB (Focused Ion Beam).

[0323] In XPS (X-ray photoelectron spectroscopy) analysis, the number of magnesium atoms is preferably 0.4 to 1.5 times the number of cobalt atoms. On the other hand, the ratio of magnesium atoms (Mg / Co) determined by ICP-MS analysis is preferably 0.001 to 0.06.

[0324] On the other hand, it is preferable that the nickel contained in the transition metal M is not concentrated in the surface layer 100a, but is distributed throughout the particles of the positive electrode active material 100. However, this does not apply if there are regions in which the aforementioned additive elements are concentrated.

[0325] ≪ESR≫ As described above, in one embodiment of the present invention, the positive electrode active material preferably has cobalt and nickel as the transition metal M and magnesium as the additive element. As a result, some Co 3+ Ni 3+ It is replaced by, and also some Li + is Mg 2+ It is preferable that it be replaced with Li. + is Mg 2+ As a result of being replaced by, the Ni 3+ It is reduced to Ni 2+ This can happen. Also, some Li + is Mg 2+ It is replaced by Mg 2+ Nearby Co 3+ It is reduced to Co 2+ This can happen. Also, some Co 3+ is Mg 2+ It is replaced by Mg2+ Nearby Co 3+ It is oxidized to Co 4+ This can happen.

[0326] Therefore, in one aspect of the present invention, the positive electrode active material is Ni 2+ Ni 3+ Co 2+ and Co 4+ It is preferable to have one or more of the following. Also, the Ni per unit weight of the positive electrode active material 2+ Ni 3+ Co 2+ and Co 4+ The spin density resulting from one or more of the following is 2.0 × 10 17 spins / g or more 1.0×10 21 It is preferable that the spin density is less than or equal to spins / g. Using a positive electrode active material having the aforementioned spin density is preferable because it stabilizes the crystal structure, especially in the charged state. However, if the magnesium concentration is too high, Ni 2+ Ni 3+ Co 2+ and Co 4+ A decrease in spin density may occur due to one or more of the following factors.

[0327] The spin density in the positive electrode active material can be analyzed using methods such as electron spin resonance (ESR).

[0328] ≪EPMA≫ EPMA (Electron Probe Microanalysis) allows for quantitative analysis of elements. Area analysis allows for the analysis of the distribution of each element.

[0329] EPMA analyzes the region from the surface to a depth of approximately 1 μm. Therefore, the concentrations of each element may differ from those measured using other analytical methods. For example, when surface analysis is performed on cathode active material 100, the concentration of additive elements present in the surface layer may be lower than that obtained with XPS. Conversely, the concentration of additive elements present in the surface layer may be higher than that obtained with ICP-MS or the values ​​of the raw material formulation used in the production of the cathode active material.

[0330] When an EPMA surface analysis is performed on a cross-section of the positive electrode active material 100 according to one embodiment of the present invention, it is preferable that the concentration of the added elements has a concentration gradient that increases from the interior to the surface. More specifically, as shown in Figure 4(B1), it is preferable that magnesium, fluorine, titanium, and silicon have a concentration gradient that increases from the interior to the surface. Also, as shown in Figure 4(B2), it is preferable that aluminum has a concentration peak in a region deeper than the concentration peaks of the above elements. The aluminum concentration peak may be located at the surface or deeper than the surface.

[0331] Furthermore, the surface and surface layer of the positive electrode active material in one embodiment of the present invention do not contain carbonates, hydroxyl groups, etc., that have been chemically adsorbed after the positive electrode active material has been manufactured. It also does not contain electrolyte, binder, conductive material, or compounds derived therefrom that have adhered to the surface of the positive electrode active material. Therefore, when quantitatively analyzing the elements present in the positive electrode active material, corrections may be made to exclude carbon, hydrogen, excess oxygen, excess fluorine, etc., which can be detected by surface analysis such as XPS and EPMA. For example, XPS allows for the separation of bond types through analysis, and corrections may be made to exclude CF bonds derived from the binder.

[0332] Furthermore, before subjecting the sample to various analyses, the positive electrode active material and positive electrode active material layer may be washed to remove electrolyte, binder, conductive material, or compounds derived therefrom that adhere to the surface of the positive electrode active material. In this case, lithium may dissolve into the solvent used for washing, but even if this occurs, the added elements are unlikely to dissolve, so it will not affect the atomic ratio of the added elements.

[0333] ≪Surface roughness and specific surface area≫ In one embodiment of the present invention, the positive electrode active material 100 preferably has a smooth surface with few irregularities. A smooth surface with few irregularities is one factor indicating that the distribution of additive elements in the surface layer 100a is good.

[0334] The smoothness and minimal irregularities of the surface can be determined, for example, from a cross-sectional SEM image or TEM image of the positive electrode active material 100, or from the specific surface area of ​​the positive electrode active material 100.

[0335] For example, the surface smoothness of the positive electrode active material 100 can be quantified from a cross-sectional SEM image, as shown below.

[0336] First, the positive electrode active material 100 is processed using FIB or the like to expose its cross-section. At this time, it is preferable to cover the positive electrode active material 100 with a protective film, protective agent, etc. Next, an SEM image of the interface between the protective film, etc. and the positive electrode active material 100 is taken. Noise processing is performed on the SEM image using image processing software. For example, Gaussian blurring (σ=2) is performed, followed by binarization. Furthermore, interface extraction is performed using image processing software. Then, the interface line between the protective film, etc. and the positive electrode active material 100 is selected using an automatic selection tool, etc., and the data is extracted into spreadsheet software, etc. Using the functions of the spreadsheet software, correction is performed from the regression curve (quadratic regression), parameters for roughness calculation are obtained from the slope-corrected data, and the root mean square (RMS) surface roughness is calculated by calculating the standard deviation. Furthermore, this surface roughness is the surface roughness of the positive electrode active material at least at 400 nm from the outer circumference of the particle.

[0337] In this embodiment, the particle surface of the positive electrode active material 100 preferably has a root mean square (RMS) surface roughness of less than 3 nm, preferably less than 1 nm, and more preferably less than 0.5 nm.

[0338] The image processing software used for noise reduction, interface extraction, etc., is not particularly limited, but for example, "ImageJ" described in Non-Patent Documents 5 to 7 can be used.

[0339] For example, the actual specific surface area A measured by the gas adsorption method using the constant-volume method. R And the ideal specific surface area A i The surface smoothness of the positive electrode active material 100 can also be quantified from this ratio.

[0340] Ideal specific surface area A i This is calculated by assuming that all particles have the same diameter as D50, the same weight, and are ideal spheres.

[0341] The median diameter D50 can be measured using a particle size analyzer that employs laser diffraction and scattering methods. The specific surface area can be measured using a specific surface area measuring device that employs a gas adsorption method based on constant volume, for example.

[0342] In one embodiment of the present invention, the positive electrode active material 100 has an ideal specific surface area A determined from the median diameter D50. i And the actual specific surface area A R Ratio A R / A i It is preferable that the value is 2.1 or less.

[0343] Alternatively, the surface smoothness of the cathode active material 100 can be quantified from a cross-sectional SEM image using the following method.

[0344] First, a surface SEM image of the positive electrode active material 100 is obtained. A conductive coating may be applied as a pretreatment before observation. It is preferable that the observation surface is perpendicular to the electron beam. When comparing multiple samples, the measurement conditions and observation area should be the same.

[0345] Next, using image processing software (for example, "ImageJ"), the above SEM image is converted to, for example, an 8-bit image (this is called a grayscale image). A grayscale image contains luminance (brightness information). For example, in an 8-bit grayscale image, luminance can be represented by 2 to the power of 8 = 256 gradations. Darker areas have a lower number of gradations, and brighter areas have a higher number of gradations. The change in luminance can be quantified in relation to the number of gradations. This numerical value is called the grayscale value. By obtaining the grayscale value, it becomes possible to numerically evaluate the unevenness of the positive electrode active material.

[0346] Furthermore, it becomes possible to represent the brightness changes of the target area using a histogram. A histogram is a three-dimensional representation of the grayscale distribution in a target area, and is also called a brightness histogram. By obtaining a brightness histogram, it becomes possible to visually evaluate the unevenness of the positive electrode active material in an easy-to-understand manner.

[0347] In one embodiment of the present invention, the positive electrode active material 100 preferably has a difference of 120 or less between the maximum and minimum values ​​of the grayscale values, more preferably 115 or less, and even more preferably 70 or more and 115 or less. Furthermore, the standard deviation of the grayscale values ​​is preferably 11 or less, more preferably 8 or less, and even more preferably 4 or more and 8 or less.

[0348] This embodiment can be used in combination with other embodiments.

[0349] (Embodiment 3) In this embodiment, an example of a secondary battery according to one aspect of the present invention will be described using Figures 18 to 21.

[0350] <Example of a secondary battery configuration 1> The following explanation uses a secondary battery, in which the positive electrode, negative electrode, and electrolyte are enclosed in an outer casing, as an example.

[0351] [Positive electrode] The positive electrode comprises a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer contains a positive electrode active material and may also contain a conductive material (which may also be called a conductive additive) and a binder. The positive electrode active material used is a positive electrode active material manufactured using the manufacturing method described in the previous embodiment.

[0352] Alternatively, the positive electrode active material described in the previous embodiment may be used in combination with other positive electrode active materials.

[0353] Examples of other cathode active materials include composite oxides having an olivine-type crystal structure, a layered rock salt-type crystal structure, or a spinel-type crystal structure. Examples of such compounds include LiFePO4, LiFeO2, LiNiO2, LiMn2O4, V2O5, Cr2O5, MnO2, and the like.

[0354] In addition, as another cathode active material, a lithium-containing material having a spinel-type crystal structure containing manganese such as LiMn2O4 is preferably mixed with lithium nickelate (LiNiO2 or LiNi 1-x M x O2 (0 < x < 1) (M = Co, Al, etc.)). By adopting such a configuration, the characteristics of the secondary battery can be improved.

[0355] In addition, as another cathode active material, a lithium manganese composite oxide represented by the composition formula Li a Mn b M c O d can be used. Here, the element M is preferably a metal element selected from elements other than lithium and manganese, or silicon or phosphorus, and more preferably nickel. When measuring the entire particle of the lithium manganese composite oxide, it is preferable to satisfy 0 < a / (b + c) < 2, c > 0, and 0.26 ≤ (b + c) / d < 0.5 during discharge. The composition of metals, silicon, phosphorus, etc. in the entire particle of the lithium manganese composite oxide can be measured using, for example, ICP-MS (Inductively Coupled Plasma Mass Spectrometer). Also, the oxygen composition of the entire particle of the lithium manganese composite oxide can be measured using, for example, EDX (Energy Dispersive X-ray Analysis). Moreover, it can be determined by using valence evaluation of melting gas analysis and XAFS (X-ray Absorption Fine Structure) analysis in combination with ICP-MS analysis. The lithium manganese composite oxide refers to an oxide containing at least lithium and manganese, and may contain at least one element selected from the group consisting of chromium, cobalt, aluminum, nickel, iron, magnesium, molybdenum, zinc, indium, gallium, copper, titanium, niobium, silicon, and phosphorus.

[0356] The following describes an example of a cross-sectional configuration when graphene or a graphene compound is used as the conductive material in the active material layer 200.

[0357] Figure 18(A) shows a longitudinal cross-sectional view of the active material layer 200. The active material layer 200 includes granular positive electrode active material 100, graphene or graphene compound 201 as a conductive material, and a binder (not shown).

[0358] In this specification, graphene compound 201 includes multilayer graphene, multigraphene, graphene oxide, multilayer graphene oxide, multigraphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multigraphene oxide, graphene quantum dots, etc. A graphene compound is a material having carbon, having a plate-like or sheet-like shape, and having a two-dimensional structure formed by a six-membered carbon ring. The two-dimensional structure formed by the six-membered carbon ring may also be called a carbon sheet. Graphene compounds may have functional groups. Furthermore, graphene compounds preferably have a bent shape. Furthermore, graphene compounds may be rolled up to resemble carbon nanofibers.

[0359] In this specification, graphene oxide refers to a material having carbon and oxygen, having a sheet-like structure, and possessing functional groups, particularly epoxy groups, carboxyl groups, or hydroxyl groups.

[0360] In this specification, reduced graphene oxide refers to a material having carbon and oxygen, having a sheet-like shape, and possessing a two-dimensional structure formed by a six-membered carbon ring. It may also be called a carbon sheet. Reduced graphene oxide can function as a single sheet, but multiple sheets may be laminated together. It is preferable that reduced graphene oxide has a portion where the carbon concentration is greater than 80 atomic%, and the oxygen concentration is between 2 atomic% and 15 atomic%. By having such carbon and oxygen concentrations, it can function as a highly conductive material even in small quantities. Furthermore, it is preferable that the intensity ratio of the G band to the D band in the Raman spectrum of reduced graphene oxide is 1 or greater. Reduced graphene oxide with such an intensity ratio can function as a highly conductive material even in small quantities.

[0361] Graphene compounds may possess excellent electrical properties, such as high conductivity, and excellent physical properties, such as high flexibility and high mechanical strength. Furthermore, graphene compounds may have a sheet-like shape. Graphene compounds may have curved surfaces, enabling surface contact with low contact resistance. They may also exhibit very high conductivity even when thin, allowing for the efficient formation of conductive paths within the active material layer with a small amount. Therefore, using graphene compounds as a conductive material can increase the contact area between the active material and the conductive material. It is preferable that the graphene compound covers 80% or more of the active material's surface area. It is also preferable that the graphene compound adheres to at least a portion of the active material particles. Furthermore, it is preferable that the graphene compound overlaps at least a portion of the active material particles. It is also preferable that the shape of the graphene compound matches at least a portion of the shape of the active material particles. The shape of the active material particles refers, for example, to the irregularities of a single active material particle or the irregularities formed by multiple active material particles. It is also preferable that the graphene compound surrounds at least a portion of the active material particles. Furthermore, the graphene compound may have holes.

[0362] When using active material particles with small particle sizes, such as 1 μm or less, the specific surface area of ​​the active material particles is large, and more conductive paths are required to connect the active material particles. In such cases, it is preferable to use a graphene compound that can efficiently form conductive paths even in small amounts.

[0363] Due to the properties described above, graphene compounds are particularly effective as conductive materials in secondary batteries that require rapid charging and rapid discharging. For example, secondary batteries for two-wheeled or four-wheeled vehicles, and secondary batteries for drones, may require rapid charging and rapid discharging characteristics. Mobile electronic devices may also require rapid charging characteristics. Rapid charging and rapid discharging can also be described as high-rate charging and high-rate discharging. For example, this refers to charging and discharging at 1C, 2C, or 5C or higher.

[0364] In the longitudinal section of the active material layer 200, as shown in Figure 18(B), sheet-like graphene or graphene compound 201 is dispersed approximately uniformly within the active material layer 200. In Figure 18(B), graphene or graphene compound 201 is schematically represented by thick lines, but in reality, it is a thin film having a single or multilayer thickness of carbon molecules. Multiple layers of graphene or graphene compound 201 are formed to partially cover multiple granular positive electrode active materials 100, or to adhere to the surface of multiple granular positive electrode active materials 100, and are therefore in surface contact with each other.

[0365] Here, multiple graphenes or graphene compounds can bond together to form a mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or graphene net). When the active material is coated with the graphene net, the graphene net can also function as a binder that binds the active materials together. Therefore, the amount of binder can be reduced or eliminated, thereby improving the ratio of active material to electrode volume and electrode weight. In other words, the charge and discharge capacity of the secondary battery can be increased.

[0366] Here, it is preferable to use graphene oxide as graphene or graphene compound 201, mix it with the active material to form a layer that becomes the active material layer 200, and then reduce it. In other words, it is preferable that the completed active material layer has reduced graphene oxide. By using graphene oxide, which has extremely high dispersibility in polar solvents, for the formation of graphene or graphene compound 201, the graphene or graphene compound 201 can be dispersed approximately uniformly within the active material layer 200. By volatilizing and removing the solvent from the dispersion medium containing the uniformly dispersed graphene oxide and reducing the graphene oxide, the graphene or graphene compound 201 remaining in the active material layer 200 partially overlaps and is dispersed to the extent that it is in surface contact with each other, thereby forming a three-dimensional conductive path. The reduction of graphene oxide may be carried out, for example, by heat treatment or by using a reducing agent.

[0367] Therefore, unlike granular conductive materials such as acetylene black, which make point contact with the active material, graphene or graphene compound 201 enables surface contact with low contact resistance. As a result, the electrical conductivity between the granular positive electrode active material 100 and graphene or graphene compound 201 can be improved with a smaller amount than with conventional conductive materials. Consequently, the ratio of positive electrode active material 100 in the active material layer 200 can be increased. This allows for an increase in the discharge capacity of the secondary battery.

[0368] Furthermore, by using a spray-drying device beforehand, it is possible to cover the entire surface of the active material with a graphene compound, which is a conductive material, as a coating, and to further form conductive paths between the active materials using the graphene compound.

[0369] Alternatively, the active material layer 200 may be made by mixing the graphene compound with the material used to form the graphene compound. For example, particles used as a catalyst when forming the graphene compound may be mixed together with the graphene compound. Examples of catalysts used when forming the graphene compound include silicon dioxide (SiO2, SiO2). xExamples of particles include those having (x<2), aluminum oxide, iron, nickel, ruthenium, iridium, platinum, copper, germanium, etc. The median diameter (D50) of the particles is preferably 1 μm or less, and more preferably 100 nm or less.

[0370] [Binder] As a binder, it is preferable to use rubber materials such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, or ethylene-propylene-diene copolymer. Fluororubber can also be used as a binder.

[0371] Furthermore, it is preferable to use a water-soluble polymer as the binder. Examples of water-soluble polymers include polysaccharides. One or more of the following polysaccharides can be used: carboxymethylcellulose (CMC), methylcellulose, ethylcellulose, hydroxypropylcellulose, diacetylcellulose, cellulose derivatives such as regenerated cellulose, and starch. It is even more preferable to use these water-soluble polymers in combination with the aforementioned rubber material.

[0372] Alternatively, it is preferable to use materials such as polystyrene, methyl polyacrylate, polymethyl methacrylate (PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, or nitrocellulose as the binder.

[0373] You may use a combination of several of the binders mentioned above.

[0374] For example, a material with particularly excellent viscosity-modifying properties may be used in combination with other materials. For instance, rubber materials have excellent adhesive and / or elastic properties, but their viscosity can be difficult to adjust when mixed with a solvent. In such cases, it is preferable to mix them with a material with particularly excellent viscosity-modifying properties. As a material with particularly excellent viscosity-modifying properties, a water-soluble polymer may be used. As a water-soluble polymer with particularly excellent viscosity-modifying properties, the aforementioned polysaccharides, such as carboxymethylcellulose (CMC), methylcellulose, ethylcellulose, hydroxypropylcellulose, and diacetylcellulose, cellulose derivatives such as regenerated cellulose, and starch can be used.

[0375] Furthermore, cellulose derivatives such as carboxymethylcellulose can be made more effective as viscosity modifiers by increasing their solubility, for example, by using salts such as sodium salts and ammonium salts of carboxymethylcellulose. Increased solubility also improves the dispersibility of the active material and other components when preparing electrode slurries. In this specification, cellulose and cellulose derivatives used as electrode binders include their salts.

[0376] Water-soluble polymers stabilize viscosity by dissolving in water and can stably disperse active materials and other materials used as binders, such as styrene-butadiene rubber, in aqueous solutions. Furthermore, because they possess functional groups, they are expected to be easily and stably adsorbed onto the surface of the active material. Additionally, cellulose derivatives such as carboxymethylcellulose often contain functional groups such as hydroxyl and carboxyl groups, and because of these functional groups, the polymers interact with each other, allowing them to broadly cover the surface of the active material.

[0377] When a binder covers or is in contact with the surface of the active material, it is expected to act as a passivation film, suppressing the decomposition of the electrolyte. Here, a passivation film is a film that does not conduct electricity, or has extremely low electrical conductivity. For example, when a passivation film is formed on the surface of the active material, the decomposition of the electrolyte can be suppressed at the battery reaction potential. Furthermore, it is even more desirable for the passivation film to suppress electrical conductivity while still allowing lithium ions to conduct.

[0378] [Positive electrode current collector] As the positive electrode current collector, highly conductive materials such as stainless steel, gold, platinum, aluminum, titanium, and alloys thereof can be used. Furthermore, it is preferable that the material used for the positive electrode current collector does not dissolve at the positive electrode potential. Aluminum alloys with added elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, and molybdenum, can also be used. Alternatively, it may be formed from a metallic element that reacts with silicon to form a silicide. Examples of metallic elements that react with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The positive electrode current collector can be in various shapes, such as foil, plate, sheet, mesh, perforated metal, or expanded metal. The positive electrode current collector should preferably have a thickness of 5 μm to 30 μm.

[0379] [Negative electrode] The negative electrode comprises a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer may also contain a conductive material and a binder.

[0380] [Negative electrode active material] For example, alloy-based materials and / or carbon-based materials can be used as the negative electrode active material.

[0381] As the negative electrode active material, elements capable of undergoing charge-discharge reactions through alloying and dealloying reactions with lithium can be used. For example, materials containing at least one of silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc., can be used. Such elements have a larger charge-discharge capacity compared to carbon, and silicon in particular has a high theoretical capacity of 4200 mAh / g. For this reason, it is preferable to use silicon as the negative electrode active material. Compounds containing these elements may also be used. Examples include SiO, Mg2Si, Mg2Ge, SnO, SnO2, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb3, InSb, SbSn, etc. In this context, elements capable of undergoing charge-discharge reactions through alloying and de-alloying reactions with lithium, and compounds containing such elements, are sometimes referred to as alloying materials.

[0382] In this specification, SiO refers to silicon monoxide, for example. Alternatively, SiO refers to SiO x It can also be expressed as follows: Here, it is preferable that x has one neighboring value. For example, x is preferably between 0.2 and 1.5, and more preferably between 0.3 and 1.2. Or preferably between 0.2 and 1.2. Or preferably between 0.3 and 1.5.

[0383] Suitable carbon-based materials include graphite, easily graphitizable carbon (soft carbon), difficult-to-graphitize carbon (hard carbon), carbon nanotubes, graphene, and carbon black.

[0384] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, spheroidal graphite having a spherical shape can be used as artificial graphite. For example, MCMB may have a spherical shape and is therefore preferable. Also, it is relatively easy to reduce the surface area of ​​MCMB, which may be preferable. Examples of natural graphite include flake graphite and spheroidized natural graphite.

[0385] When lithium ions are inserted into graphite (during the formation of lithium-graphite intercalation compounds), graphite exhibits a potential as low as that of lithium metal (0.05V to 0.3V vs. Li / Li). + This allows the lithium-ion secondary battery to exhibit a high operating voltage. Furthermore, graphite is preferred because it has advantages such as a relatively high charge / discharge capacity per unit volume, relatively small volume expansion, low cost, and higher safety compared to lithium metal.

[0386] Furthermore, titanium dioxide (TiO2) and lithium titanium oxide (Li4Ti5O2) are used as negative electrode active materials. 12 ), lithium-graphite intercalation compound (Li x Oxides such as C6, niobium pentoxide (Nb2O5), tungsten oxide (WO2), and molybdenum oxide (MoO2) can be used.

[0387] Furthermore, as the negative electrode active material, a Li3N type structure is used, which is a lithium and transition metal binitride. 3-x M x N (M = Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 The N3 has a large charge / discharge capacity (900mAh / g, 1890mAh / cm²). 3 ) indicates a preference.

[0388] Using a lithium-transition metal complex nitride is preferable because it contains lithium ions in the negative electrode active material, allowing it to be combined with lithium-ion-free materials such as V2O5 and Cr3O8 as the positive electrode active material. Even when using a lithium-ion-containing material as the positive electrode active material, the lithium-transition metal complex nitride can be used as the negative electrode active material by pre-desorbing the lithium ions contained in the positive electrode active material.

[0389] Furthermore, materials that undergo a conversion reaction can also be used as the negative electrode active material. For example, transition metal oxides that do not form alloys with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), and iron oxide (FeO), may be used as the negative electrode active material. Other materials that undergo a conversion reaction include oxides such as Fe2O3, CuO, Cu2O, RuO2, Cr2O3, and CoS 0.89 This can also occur with sulfides such as NiS and CuS, nitrides such as Zn3N2, Cu3N, and Ge3N4, phosphides such as NiP2, FeP2, and CoP3, and fluorides such as FeF3 and BiF3.

[0390] The conductive material and binder that the negative electrode active material layer can have can be the same materials as the conductive material and binder that the positive electrode active material layer can have.

[0391] [Negative electrode current collector] The negative electrode current collector can be made of the same material as the positive electrode current collector. However, it is preferable to use a material for the negative electrode current collector that does not alloy with carrier ions such as lithium.

[0392] [Electrolyte] The electrolyte contains a solvent and an electrolyte. The solvent for the electrolyte is preferably an aprotic organic solvent, such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, sultone, etc., or two or more of these can be used in any combination and ratio.

[0393] Furthermore, by using one or more flame-retardant and non-volatile ionic liquids (room-temperature molten salts) as the solvent for the electrolyte, it is possible to prevent the secondary battery from rupturing and / or igniting even if the internal temperature rises due to an internal short circuit or overcharging. Ionic liquids consist of cations and anions, and include organic cations and anions. Examples of organic cations used in the electrolyte include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, as well as aromatic cations such as imidazolium cations and pyridinium cations. Examples of anions used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonic acid anions, perfluoroalkyl sulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, or perfluoroalkyl phosphate anions.

[0394] Furthermore, examples of electrolytes to be dissolved in the above solvent include LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4, and Li2B. 10 Cl 10 Li2B12 Cl 12 Lithium salts such as LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO2), and LiN(C2F5SO2)2 can be used individually or in any combination and ratio of two or more of these salts.

[0395] For secondary batteries, it is preferable to use a highly purified electrolyte with a low content of particulate matter or elements other than the constituent elements of the electrolyte (hereinafter also simply referred to as "impurities"). Specifically, it is preferable that the weight ratio of impurities to the electrolyte be 1% or less, preferably 0.1% or less, and more preferably 0.01% or less.

[0396] Furthermore, additives such as vinylene carbonate, propanesultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), and dinitrile compounds such as succinonitrile and adiponitrile may be added to the electrolyte. The concentration of the added material should be, for example, 0.1 wt% to 5 wt% relative to the total solvent. VC or LiBOB are particularly preferred because they readily form a good coating.

[0397] Alternatively, a polymer gel electrolyte, obtained by swelling a polymer with an electrolyte solution, may be used.

[0398] Using polymer gel electrolytes enhances safety against leakage and other issues. Furthermore, it enables the secondary battery to be made thinner and lighter.

[0399] As the polymer to be gelled, silicone gels, acrylic gels, acrylonitrile gels, polyethylene oxide-based gels, polypropylene oxide-based gels, fluorine-based polymer gels, and the like can be used.

[0400] Examples of polymers that can be used include polymers having a polyalkylene oxide structure such as polyethylene oxide (PEO), PVDF, polyacrylonitrile, and copolymers containing these. For example, PVDF-HFP, a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The resulting polymer may also have a porous structure.

[0401] Furthermore, instead of an electrolyte, a solid electrolyte containing inorganic materials such as sulfides or oxides, or a solid electrolyte containing polymeric materials such as PEO (polyethylene oxide), can be used. When a solid electrolyte is used, the installation of separators and / or spacers becomes unnecessary. In addition, since the entire battery can be solidified, the risk of leakage is eliminated, dramatically improving safety.

[0402] [Separator] Furthermore, secondary batteries preferably have a separator. As the separator, for example, paper, nonwoven fabric, glass fiber, ceramics, or synthetic fibers made of nylon (polyamide), vinylon (polyvinyl alcohol-based fiber), polyester, acrylic, polyolefin, or polyurethane can be used. It is preferable that the separator is processed into an envelope shape and arranged to enclose either the positive or negative electrode.

[0403] The separator may have a multilayer structure. For example, an organic material film such as polypropylene or polyethylene can be coated with a ceramic material, a fluorine material, a polyamide material, or a mixture thereof. Examples of ceramic materials include aluminum oxide particles and silicon oxide particles. Examples of fluorine materials include PVDF and polytetrafluoroethylene. Examples of polyamide materials include nylon and aramid (meta-aramid, para-aramid).

[0404] Coating with ceramic materials improves oxidation resistance, suppressing separator degradation during high-voltage charging and discharging, and thus improving the reliability of secondary batteries. Coating with fluorine-based materials improves adhesion between the separator and electrodes, thereby improving output characteristics. Coating with polyamide materials, particularly aramid, improves heat resistance, thus enhancing the safety of secondary batteries.

[0405] For example, a polypropylene film may be coated on both sides with a mixture of aluminum oxide and aramid. Alternatively, the side of the polypropylene film in contact with the positive electrode may be coated with a mixture of aluminum oxide and aramid, and the side in contact with the negative electrode may be coated with a fluorine-based material.

[0406] By using a multilayer separator, the safety of the secondary battery can be maintained even if the overall thickness of the separator is thin, thus increasing the charge / discharge capacity per unit volume of the secondary battery.

[0407] [Exterior] For the outer casing of a secondary battery, metal materials such as aluminum and / or resin materials can be used. Alternatively, a film-like outer casing can be used. As a film, for example, a three-layer film can be used, in which a highly flexible metal thin film such as aluminum, stainless steel, copper, or nickel is provided on a film made of materials such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and an insulating synthetic resin film such as a polyamide resin or polyester resin is provided on the metal thin film as the outer surface of the outer casing.

[0408] <Example of a secondary battery configuration 2> The following describes the configuration of a secondary battery using a solid electrolyte layer as an example of a secondary battery configuration.

[0409] As shown in Figure 19(A), a secondary battery 400 according to one embodiment of the present invention has a positive electrode 410, a solid electrolyte layer 420, and a negative electrode 430.

[0410] The positive electrode 410 has a positive electrode current collector 413 and a positive electrode active material layer 414. The positive electrode active material layer 414 has a positive electrode active material 411 and a solid electrolyte 421. The positive electrode active material 411 uses the positive electrode active material produced using the production method described in the previous embodiment. Also, the positive electrode active material layer 414 may have a conductive material and a binder.

[0411] The solid electrolyte layer 420 has a solid electrolyte 421. The solid electrolyte layer 420 is located between the positive electrode 410 and the negative electrode 430 and is an area that has neither the positive electrode active material 411 nor the negative electrode active material 431.

[0412] The negative electrode 430 has a negative electrode current collector 433 and a negative electrode active material layer 434. The negative electrode active material layer 434 has a negative electrode active material 431 and a solid electrolyte 421. Also, the negative electrode active material layer 434 may have a conductive material and a binder. When using lithium metal for the negative electrode 430, as shown in Fig. 19(B), the negative electrode 430 that does not have the solid electrolyte 421 can be used. When using lithium metal for the negative electrode 430, it is preferable because the energy density of the secondary battery 400 can be improved.

[0413] As the solid electrolyte 421 included in the solid electrolyte layer 420, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a halide-based solid electrolyte, etc. can be used.

[0414] Among the sulfide-based solid electrolytes, there are thiolischicon-based (Li 10 GeP2S 12 、Li 3.25 Ge 0.25 P 0.75 S4, etc.), sulfide glasses (70Li2S·30P2S5, 30Li2S·26B2S3·44LiI, 63Li2S·36SiS2·1Li3PO4, 57Li2S·38SiS2·5Li4SiO4, 50Li2S·50GeS2, etc.), sulfide crystallized glasses (Li7P3S 11 、Li 3.25 P 0.95It includes sulfide-based solid electrolytes (such as S4, etc.). Sulfide-based solid electrolytes have advantages such as having materials with high conductivity, being able to be synthesized at low temperatures, and being relatively soft, so the conductive path is likely to be maintained even after charge and discharge.

[0415] Oxide-based solid electrolytes include materials having a perovskite crystal structure (such as La 2 / 3-x Li 3x TiO3, etc.), materials having a NASICON crystal structure (such as Li 1-x Al x Ti 2-x (PO4)3, etc.), materials having a garnet crystal structure (such as Li7La3Zr2O 12 etc.), materials having a LISICON crystal structure (such as Li 14 ZnGe4O 16 etc.), LLZO (Li7La3Zr2O 12 ), oxide glasses (such as Li3PO4-Li4SiO4, 50Li4SiO4·50Li3BO3, etc.), oxide crystallized glasses (such as Li 1.07 Al 0.69 Ti 1.46 (PO4)3, Li 1.5 Al 0.5 Ge 1.5 (PO4)3, etc.). Oxide-based solid electrolytes have advantages such as being stable in the atmosphere.

[0416] Halide-based solid electrolytes include LiAlCl4, Li3InBr6, LiF, LiCl, LiBr, LiI, etc. Also, composite materials in which these halide-based solid electrolytes are filled in the pores of porous aluminum oxide and / or porous silica can be used as solid electrolytes.

[0417] Also, different solid electrolytes may be mixed and used.

[0418] Among them, Li having a NASICON crystal structure 1+x Al x Ti 2-x(PO4)3(0 < x < 1) (hereinafter referred to as LATP) contains elements such as aluminum and titanium, which may be included in the positive electrode active material used in the secondary battery 400 of one aspect of the present invention. Therefore, a synergistic effect can be expected for improving the cycle characteristics, which is preferable. In addition, an improvement in productivity due to reduction of processes can also be expected. In this specification and the like, the NASICON-type crystal structure is a compound represented by M2(XO4)3 (M: transition metal, X: S, P, As, Mo, W, etc.), and has a structure in which MO6 octahedrons and XO4 tetrahedrons share vertices and are three-dimensionally arranged.

[0419] 〔Shape of the exterior body and the secondary battery〕 For the exterior body of the secondary battery 400 of one aspect of the present invention, various materials and shapes can be used, but it is preferable that it has a function of pressing the positive electrode, the solid electrolyte layer, and the negative electrode.

[0420] For example, FIG. 20 shows an example of a cell for evaluating the materials of a all-solid-state battery.

[0421] FIG. 20(A) is a schematic cross-sectional view of the evaluation cell. The evaluation cell has a lower member 761, an upper member 762, and fixing screws or wing nuts 764 for fixing them. By rotating the pressing screw 763, the electrode plate 753 is pressed to fix the evaluation material. An insulator 766 is provided between the lower member 761 and the upper member 762 made of a stainless steel material. Also, an O-ring 765 for sealing is provided between the upper member 762 and the pressing screw 763.

[0422] The evaluation material is placed on the electrode plate 751, surrounded by an insulating tube 752 around it, and is in a state of being pressed by the electrode plate 753 from above. A perspective view of the periphery of this evaluation material enlarged is shown in FIG. 20(B).

[0423] As an example of the evaluation material, a laminate of a positive electrode 750a, a solid electrolyte layer 750b, and a negative electrode 750c is shown, and a cross-sectional view is shown in FIG. 20(C). The same reference numerals are used for the same parts in FIGS. 20(A) to 20(C).

[0424] The electrode plate 751 and lower member 761, which are electrically connected to the positive electrode 750a, can be considered to correspond to the positive electrode terminal. The electrode plate 753 and upper member 762, which are electrically connected to the negative electrode 750c, can be considered to correspond to the negative electrode terminal. Electrical resistance and other parameters can be measured while applying pressure to the evaluation material via the electrode plates 751 and 753.

[0425] Furthermore, it is preferable to use a package with excellent airtightness for the outer casing of a secondary battery according to one embodiment of the present invention. For example, a ceramic package and / or a resin package can be used. Also, when sealing the outer casing, it is preferable to block out the outside air and perform the sealing in a sealed atmosphere, for example, inside a glove box.

[0426] Figure 21(A) shows a perspective view of a secondary battery according to one embodiment of the present invention, having a different exterior and shape from that of Figure 20. The secondary battery in Figure 21(A) has external electrodes 771 and 772 and is sealed with an exterior having a plurality of package members.

[0427] Figure 21(B) shows an example of a cross-section cut by the dashed line in Figure 21(A). The laminate having a positive electrode 750a, a solid electrolyte layer 750b, and a negative electrode 750c is enclosed and sealed by a package member 770a having an electrode layer 773a on a flat plate, a frame-shaped package member 770b, and a package member 770c having an electrode layer 773b on a flat plate. Insulating materials, such as resin materials and / or ceramics, can be used for the package members 770a, 770b, and 770c.

[0428] The external electrode 771 is electrically connected to the positive electrode 750a via the electrode layer 773a and functions as a positive electrode terminal. The external electrode 772 is electrically connected to the negative electrode 750c via the electrode layer 773b and functions as a negative electrode terminal.

[0429] This embodiment can be used in appropriate combination with other embodiments.

[0430] (Embodiment 4) This embodiment describes an example of the shape of a secondary battery having a positive electrode, as described in the previous embodiment. The materials used in the secondary battery described in this embodiment can be referenced to those described in the previous embodiment.

[0431] <Coin-type rechargeable battery> First, let's describe an example of a coin-type rechargeable battery. Figure 22(A) is an external view of a coin-type (single-layer flat type) rechargeable battery, and Figure 22(B) is a cross-sectional view thereof.

[0432] The coin-type secondary battery 300 has a positive electrode casing 301, which also serves as the positive electrode terminal, and a negative electrode casing 302, which also serves as the negative electrode terminal, both insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed by a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with it. The negative electrode 307 is formed by a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with it.

[0433] Furthermore, for the positive electrode 304 and negative electrode 307 used in the coin-type secondary battery 300, the active material layer only needs to be formed on one side.

[0434] The positive electrode can 301 and the negative electrode can 302 can be made of metals such as nickel, aluminum, or titanium, which are corrosion-resistant to the electrolyte, or alloys thereof and / or alloys of these with other metals (e.g., stainless steel). Furthermore, it is preferable to coat them with nickel and / or aluminum, etc., to prevent corrosion by the electrolyte. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.

[0435] The negative electrode 307, positive electrode 304, and separator 310 are impregnated with an electrolyte, and as shown in Figure 22(B), the positive electrode 304, separator 310, negative electrode 307, and negative electrode 302 are stacked in this order with the positive electrode 301 at the bottom, and the positive electrode 301 and negative electrode 302 are pressed together via a gasket 303 to manufacture a coin-type secondary battery 300.

[0436] By using the positive electrode active material described in the previous embodiment for the positive electrode 304, a coin-type secondary battery 300 with high charge / discharge capacity and excellent cycle characteristics can be obtained.

[0437] Here, Figure 22(C) is used to explain the current flow during charging of a secondary battery. When a lithium-ion secondary battery is considered as a closed circuit, the movement of lithium ions and the flow of current are in the same direction. In a lithium-ion secondary battery, the anode and cathode are reversed during charging and discharging, and the oxidation and reduction reactions are reversed. Therefore, the electrode with the higher reaction potential is called the positive electrode, and the electrode with the lower reaction potential is called the negative electrode. Accordingly, in this specification, whether charging or discharging, whether a reverse pulse current is flowing or a charging current is flowing, the positive electrode will be called the "positive electrode" or "+ electrode (positive electrode)," and the negative electrode will be called the "negative electrode" or "- electrode (negative electrode)." Using the terms anode (positive electrode) and cathode (negative electrode) in relation to oxidation and reduction reactions could lead to confusion as they are reversed during charging and discharging. Therefore, the terms anode (positive electrode) and cathode (negative electrode) will not be used in this specification. If the terms anode and cathode are used, it should be specified whether they refer to the charging or discharging phase, and whether they correspond to the positive or negative electrode.

[0438] A charger is connected to the two terminals shown in Figure 22(C), and the secondary battery 300 is charged. As the secondary battery 300 charges, the potential difference between the electrodes increases.

[0439] <Cylindrical rechargeable battery> Next, an example of a cylindrical secondary battery will be described with reference to Figure 23. Figure 23(A) shows an external view of a cylindrical secondary battery 600. Figure 23(B) is a schematic cross-section of the cylindrical secondary battery 600. As shown in Figure 23(B), the cylindrical secondary battery 600 has a positive electrode cap (battery cover) 601 on the top surface and a battery casing (outer casing) 602 on the sides and bottom. The positive electrode cap 601 and the battery casing (outer casing) 602 are insulated from each other by a gasket (insulating packing) 610.

[0440] Inside the hollow cylindrical battery casing 602, a battery element is provided, in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with a separator 605 in between. Although not shown, the battery element is wound around a center pin. The battery casing 602 is closed at one end and open at the other. The battery casing 602 can be made of a metal such as nickel, aluminum, or titanium, or an alloy of these and / or an alloy of these with other metals (e.g., stainless steel), which is corrosion-resistant to the electrolyte. Furthermore, it is preferable to coat the battery casing 602 with nickel and / or aluminum to prevent corrosion by the electrolyte. Inside the battery casing 602, the battery element, in which the positive electrode, negative electrode, and separator are wound, is sandwiched between a pair of opposing insulating plates 608 and 609. In addition, a non-aqueous electrolyte (not shown) is injected into the inside of the battery casing 602 in which the battery element is provided. The non-aqueous electrolyte can be the same as that used in coin-type secondary batteries.

[0441] Since the positive and negative electrodes used in cylindrical storage batteries are wound, it is preferable to form active material on both sides of the current collector. A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. Both the positive electrode terminal 603 and the negative electrode terminal 607 can be made of metal materials such as aluminum. The positive electrode terminal 603 is resistance-welded to the safety valve mechanism 612, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 612 is electrically connected to the positive electrode cap 601 via a PTC element (Positive Temperature Coefficient) 611. The safety valve mechanism 612 disconnects the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the rise in the internal pressure of the battery exceeds a predetermined threshold. Furthermore, the PTC element 611 is a thermal resistance element whose resistance increases when the temperature rises, and it prevents abnormal heat generation by limiting the current amount through the increase in resistance. Barium titanate (BaTiO3) based semiconductor ceramics can be used for the PTC element.

[0442] Alternatively, as shown in Figure 23(C), a module 615 may be constructed by sandwiching multiple secondary batteries 600 between conductive plates 613 and 614. The multiple secondary batteries 600 may be connected in parallel, in series, or connected in parallel and then in series. By constructing a module 615 with multiple secondary batteries 600, a large amount of power can be extracted.

[0443] Figure 23(D) is a top view of module 615. The conductive plate 613 is shown with a dotted line for clarity. As shown in Figure 23(D), module 615 may have conductors 616 that electrically connect a plurality of secondary batteries 600. A conductive plate can be superimposed on the conductors 616. A temperature control device 617 may also be provided between the plurality of secondary batteries 600. When a secondary battery 600 is overheated, it can be cooled by the temperature control device 617, and when a secondary battery 600 is too cold, it can be heated by the temperature control device 617. This makes the performance of module 615 less susceptible to the influence of ambient temperature. The heat transfer medium in the temperature control device 617 is preferably insulating and non-flammable.

[0444] By using the positive electrode active material described in the previous embodiment for the positive electrode 604, a cylindrical secondary battery 600 with high charge / discharge capacity and excellent cycle characteristics can be obtained.

[0445] <Example of a secondary battery structure> Another example of a secondary battery structure will be explained using Figures 24 to 28.

[0446] Figures 24(A) and 24(B) show the external view of the battery pack. The battery pack includes a secondary battery 913 and a circuit board 900. The secondary battery 913 is connected to the antenna 914 via the circuit board 900. A label 910 is attached to the secondary battery 913. Furthermore, as shown in Figure 24(B), the secondary battery 913 is connected to terminals 951 and 952. The circuit board 900 is secured with a seal 915.

[0447] The circuit board 900 has terminal 911 and circuit 912. Terminal 911 is connected to terminal 951, terminal 952, antenna 914, and circuit 912. Multiple terminals 911 may be provided, and each of the multiple terminals 911 may be used as a control signal input terminal, a power supply terminal, etc.

[0448] The circuit 912 may be provided on the back surface of the circuit board 900. The antenna 914 is not limited to a coil shape, but may be, for example, linear or plate-shaped. Alternatively, antennas such as a planar antenna, aperture antenna, traveling wave antenna, EH antenna, magnetic field antenna, or dielectric antenna may be used. Or, the antenna 914 may be a flat conductor. This flat conductor can function as one of the conductors for electric field coupling. In other words, the antenna 914 may function as one of the two conductors of the capacitor. This makes it possible to exchange power not only through electromagnetic and magnetic fields, but also through electric fields.

[0449] The battery pack has a layer 916 between the antenna 914 and the secondary battery 913. The layer 916 has the function of shielding, for example, the electromagnetic field from the secondary battery 913. For the layer 916, a magnetic material can be used, for example.

[0450] Note that the structure of the battery pack is not limited to that shown in Figure 24.

[0451] For example, as shown in Figures 25(A) and 25(B), antennas may be provided on each of the opposing pairs of faces of the secondary battery 913 shown in Figures 24(A) and 24(B). Figure 25(A) is an external view showing one of the pair of faces, and Figure 25(B) is an external view showing the other of the pair of faces. For parts that are the same as those of the secondary battery shown in Figures 24(A) and 24(B), the explanation of the secondary battery shown in Figures 24(A) and 24(B) can be appropriately referred to.

[0452] As shown in Figure 25(A), an antenna 914 is provided on one of the pair of surfaces of the secondary battery 913 with a layer 916 in between, and as shown in Figure 25(B), an antenna 918 is provided on the other of the pair of surfaces of the secondary battery 913 with a layer 917 in between. The layer 917 has the function of shielding the electromagnetic field from, for example, the secondary battery 913. For the layer 917, a magnetic material can be used, for example.

[0453] By adopting the above structure, the size of both antenna 914 and antenna 918 can be increased. Antenna 918 has a function that allows for data communication with external devices, for example. Antenna 918 can be fitted with an antenna of a shape that is applicable to antenna 914, for example. As a communication method between the secondary battery and other devices via antenna 918, response methods that can be used between the secondary battery and other devices, such as NFC (Near Field Communication), can be applied.

[0454] Alternatively, as shown in Figure 25(C), a display device 920 may be provided on the secondary battery 913 shown in Figures 24(A) and 24(B). The display device 920 is electrically connected to terminal 911. Note that a label 910 does not need to be provided on the part where the display device 920 is provided. Note that for the same parts as the secondary battery shown in Figures 24(A) and 24(B), the explanation of the secondary battery shown in Figures 24(A) and 24(B) can be appropriately applied.

[0455] The display device 920 may display, for example, an image indicating whether or not it is charging, or an image indicating the amount of stored power. The display device 920 can be, for example, electronic paper, liquid crystal display, or electroluminescent (EL) display. For example, using electronic paper can reduce the power consumption of the display device 920.

[0456] Alternatively, as shown in Figure 25(D), a sensor 921 may be provided on the secondary battery 913 shown in Figures 24(A) and 24(B). The sensor 921 is electrically connected to terminal 911 via terminal 922. For parts that are the same as those of the secondary battery shown in Figures 24(A) and 24(B), the explanation of the secondary battery shown in Figures 24(A) and 24(B) can be appropriately applied.

[0457] The sensor 921 may have the function of measuring, for example, displacement, position, velocity, acceleration, angular velocity, rotational speed, distance, light, liquid, magnetism, temperature, chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, or infrared radiation. By providing the sensor 921, for example, data indicating the environment in which the secondary battery is placed (such as temperature) can be detected and stored in the memory of the circuit 912.

[0458] Furthermore, an example of the structure of the secondary battery 913 will be explained using Figures 26 and 27.

[0459] The secondary battery 913 shown in Figure 26(A) has a wound body 950 with terminals 951 and 952 inside a housing 930. The wound body 950 is impregnated with an electrolyte inside the housing 930. Terminal 952 is in contact with the housing 930, while terminal 951 is not in contact with the housing 930 due to the use of an insulating material or the like. In Figure 26(A), the housing 930 is shown separated for convenience, but in reality, the wound body 950 is covered by the housing 930, and terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (e.g., aluminum) or a resin material.

[0460] Furthermore, as shown in Figure 26(B), the housing 930 shown in Figure 26(A) may be formed from multiple materials. For example, in the secondary battery 913 shown in Figure 26(B), housing 930a and housing 930b are bonded together, and the winding body 950 is provided in the area surrounded by housing 930a and housing 930b.

[0461] For the housing 930a, an insulating material such as organic resin can be used. In particular, by using a material such as organic resin on the surface where the antenna is formed, shielding of the electric field by the secondary battery 913 can be suppressed. If the shielding of the electric field by the housing 930a is small, an antenna such as antenna 914 may be provided inside the housing 930a. For the housing 930b, for example, a metal material can be used.

[0462] Furthermore, the structure of the wound body 950 is shown in Figure 27. The wound body 950 has a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the separator 933 in between, and the stacked sheets are wound up. Note that multiple stacks of the negative electrode 931, positive electrode 932, and separator 933 may be stacked.

[0463] The negative terminal 931 is connected to terminal 911 shown in Figure 24 via one of terminals 951 and 952. The positive terminal 932 is connected to terminal 911 shown in Figure 24 via the other of terminals 951 and 952.

[0464] By using the positive electrode active material described in the previous embodiment for the positive electrode 932, a secondary battery 913 with high charge / discharge capacity and excellent cycle characteristics can be obtained.

[0465] <Laminated rechargeable battery> Next, an example of a laminated secondary battery will be described with reference to Figures 28 to 32(A). If a laminated secondary battery has a flexible structure, it can be bent in accordance with the deformation of the electronic device if it is mounted on an electronic device that has at least a part of a flexible component.

[0466] A laminated secondary battery 980 will be described using Figure 28. The laminated secondary battery 980 has a wound body 993 as shown in Figure 28(A). The wound body 993 has a negative electrode 994, a positive electrode 995, and a separator 996. Similar to the wound body 950 described in Figure 27, the wound body 993 is formed by stacking the negative electrode 994 and the positive electrode 995 with the separator 996 in between, and then winding the stacked sheet.

[0467] The number of layers in the stack consisting of the negative electrode 994, positive electrode 995, and separator 996 can be appropriately designed according to the required charge / discharge capacity and element volume. The negative electrode 994 is connected to a negative electrode current collector (not shown) via one of the lead electrodes 997 and 998, and the positive electrode 995 is connected to a positive electrode current collector (not shown) via the other of the lead electrodes 997 and 998.

[0468] As shown in Figure 28(B), a secondary battery 980 can be manufactured as shown in Figure 28(C) by housing the aforementioned wound body 993 in a space formed by bonding a film 981, which serves as the outer casing, and a film 982, which has a recess, by thermocompression or the like. The wound body 993 has lead electrodes 997 and 998 and is impregnated with an electrolyte solution inside the film 981 and the film 982, which has a recess.

[0469] The film 981 and the film 982 having recesses can be made of metal materials such as aluminum and / or resin materials. If resin materials are used for the film 981 and the film 982 having recesses, the film 981 and the film 982 having recesses can be deformed when an external force is applied, making it possible to create a flexible storage battery.

[0470] Furthermore, although Figures 28(B) and 28(C) show examples using two films, a space may be formed by folding a single film, and the aforementioned wound body 993 may be housed in that space.

[0471] By using the positive electrode active material described in the previous embodiment for the positive electrode 995, a secondary battery 980 with high charge / discharge capacity and excellent cycle characteristics can be obtained.

[0472] Furthermore, while Figure 28 illustrates an example of a secondary battery 980 having a wound body in a space formed by a film that serves as the outer casing, a secondary battery having multiple strip-shaped positive electrodes, separators, and negative electrodes in a space formed by a film that serves as the outer casing may also be used, for example, as shown in Figure 29.

[0473] The laminate-type secondary battery 500 shown in Figure 29(A) comprises a positive electrode 503 having a positive electrode current collector 501 and a positive electrode active material layer 502, a negative electrode 506 having a negative electrode current collector 504 and a negative electrode active material layer 505, a separator 507, an electrolyte 508, and an outer casing 509. The separator 507 is installed between the positive electrode 503 and the negative electrode 506, which are located inside the outer casing 509. The outer casing 509 is filled with the electrolyte 508. The electrolyte 508 can be the electrolyte shown in Embodiment 3.

[0474] In the laminate-type secondary battery 500 shown in Figure 29(A), the positive electrode current collector 501 and the negative electrode current collector 504 also serve as terminals for obtaining electrical contact with the outside. Therefore, parts of the positive electrode current collector 501 and the negative electrode current collector 504 may be arranged to be exposed to the outside from the outer casing 509. Alternatively, the positive electrode current collector 501 and the negative electrode current collector 504 may not be exposed to the outside from the outer casing 509, and instead, lead electrodes may be used to ultrasonically bond the lead electrodes to the positive electrode current collector 501 or the negative electrode current collector 504, thereby exposing the lead electrodes to the outside.

[0475] In a laminate-type secondary battery 500, the outer casing 509 can be made of a laminate film with a three-layer structure, in which a highly flexible metal thin film such as aluminum, stainless steel, copper, or nickel is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and an insulating synthetic resin film such as a polyamide resin or polyester resin is provided on the metal thin film as the outer surface of the outer casing.

[0476] Furthermore, an example of the cross-sectional structure of the laminate-type secondary battery 500 is shown in Figure 29(B). For simplicity, Figure 29(A) shows an example consisting of two current collectors, but in reality, it is composed of multiple electrode layers as shown in Figure 29(B).

[0477] Figure 29(B) shows an example where the number of electrode layers is 16. Even with 16 electrode layers, the secondary battery 500 retains its flexibility. Figure 29(B) shows a structure with a total of 16 layers: 8 layers of negative electrode current collectors 504 and 8 layers of positive electrode current collectors 501. Figure 29(B) also shows a cross-section of the negative electrode extraction section, where the 8 layers of negative electrode current collectors 504 are ultrasonically bonded. Of course, the number of electrode layers is not limited to 16; it can be more or fewer. A larger number of electrode layers allows for a secondary battery with greater charge and discharge capacity. Conversely, a smaller number of electrode layers allows for a thinner design and a secondary battery with superior flexibility.

[0478] Here, an example of the external view of a laminate-type secondary battery 500 is shown in Figures 30 and 31. Figures 30 and 31 show a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511.

[0479] Figure 32(A) shows the external view of the positive electrode 503 and the negative electrode 506. The positive electrode 503 has a positive electrode current collector 501, and the positive electrode active material layer 502 is formed on the surface of the positive electrode current collector 501. The positive electrode 503 also has a region where the positive electrode current collector 501 is partially exposed (hereinafter referred to as the tab region). The negative electrode 506 has a negative electrode current collector 504, and the negative electrode active material layer 505 is formed on the surface of the negative electrode current collector 504. The negative electrode 506 also has a region where the negative electrode current collector 504 is partially exposed, i.e., the tab region. The area and shape of the tab regions of the positive and negative electrodes are not limited to the example shown in Figure 32(A).

[0480] <Method for manufacturing laminated rechargeable batteries> Here, an example of a method for manufacturing a laminate-type secondary battery, whose external view is shown in Figure 30, will be explained using Figures 32(B) and (C).

[0481] First, the negative electrode 506, separator 507, and positive electrode 503 are stacked. Figure 32(B) shows the stacked negative electrode 506, separator 507, and positive electrode 503. Here, an example using 5 sets of negative electrodes and 4 sets of positive electrodes is shown. Next, the tab regions of the positive electrode 503 are joined together, and the positive electrode lead electrode 510 is joined to the tab region of the outermost positive electrode. For joining, ultrasonic welding, for example, can be used. Similarly, the tab regions of the negative electrode 506 are joined together, and the negative electrode lead electrode 511 is joined to the tab region of the outermost negative electrode.

[0482] Next, the negative electrode 506, separator 507, and positive electrode 503 are placed on the outer casing 509.

[0483] Next, as shown in Figure 32(C), the outer casing 509 is bent at the portion indicated by the dashed line. Then, the outer periphery of the outer casing 509 is joined. For joining, for example, heat sealing may be used. At this time, a region that is not joined (hereinafter referred to as the inlet) is provided on a part (or one side) of the outer casing 509 so that the electrolyte 508 can be added later.

[0484] Next, the electrolyte 508 (not shown) is introduced into the inside of the outer casing 509 through an inlet provided in the outer casing 509. It is preferable to introduce the electrolyte 508 under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is sealed. In this way, a laminate-type secondary battery 500 can be manufactured.

[0485] By using the positive electrode active material described in the previous embodiment for the positive electrode 503, a secondary battery 500 with high charge / discharge capacity and excellent cycle characteristics can be obtained.

[0486] In all-solid-state batteries, applying a predetermined pressure in the stacking direction of the stacked positive and negative electrodes can maintain good contact conditions at the internal interfaces. Applying a predetermined pressure in the stacking direction of the positive and negative electrodes can suppress expansion in the stacking direction due to charging and discharging of the all-solid-state battery, thereby improving the reliability of the all-solid-state battery.

[0487] This embodiment can be used in appropriate combination with other embodiments.

[0488] (Embodiment 5) This embodiment describes an example of mounting a secondary battery, which is one aspect of the present invention, into an electronic device.

[0489] First, Figures 33(A) to 33(G) show examples of mounting the bendable secondary battery described in the previous embodiment into an electronic device. Examples of electronic devices to which the bendable secondary battery is applied include television equipment (also called televisions or television receivers), monitors for computers, digital cameras, digital video cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices), portable game consoles, personal information terminals, sound playback devices, and large game machines such as pachinko machines.

[0490] Furthermore, the rechargeable battery, with its flexible shape, can be incorporated along the curved surfaces of interior or exterior walls of houses and buildings, or the interior or exterior of automobiles.

[0491] Figure 33(A) shows an example of a mobile phone. The mobile phone 7400 includes a display unit 7402 built into the housing 7401, as well as operation buttons 7403, an external connection port 7404, a speaker 7405, a microphone 7406, and the like. The mobile phone 7400 also has a secondary battery 7407. By using a secondary battery according to one embodiment of the present invention for the above secondary battery 7407, a lightweight and long-lasting mobile phone can be provided.

[0492] Figure 33(B) shows the mobile phone 7400 in a bent state. When the mobile phone 7400 is deformed by an external force and the entire device is bent, the secondary battery 7407 located inside is also bent. Figure 33(C) shows the state of the bent secondary battery 7407 at that time. The secondary battery 7407 is a thin storage battery. The secondary battery 7407 is fixed in the bent state. The secondary battery 7407 has lead electrodes that are electrically connected to a current collector. For example, the current collector is made of copper foil, and a portion of it is alloyed with gallium to improve the adhesion with the active material layer that is in contact with the current collector, resulting in a configuration that ensures high reliability of the secondary battery 7407 when it is bent.

[0493] Figure 33(D) shows an example of a bangle-type display device. The portable display device 7100 comprises a housing 7101, a display unit 7102, operation buttons 7103, and a secondary battery 7104. Figure 33(E) shows the state of the bent secondary battery 7104. When the secondary battery 7104 is worn on the user's arm in a bent state, the housing deforms, and the curvature of part or all of the secondary battery 7104 changes. The degree of curvature at any point in the curve is expressed as the radius of the corresponding circle, and the reciprocal of the radius of curvature is called the curvature. Specifically, part or all of the main surface of the housing or secondary battery 7104 changes within the range of a radius of curvature of 40 mm to 150 mm. High reliability can be maintained as long as the radius of curvature on the main surface of the secondary battery 7104 is within the range of 40 mm to 150 mm. By using a secondary battery according to one embodiment of the present invention for the above secondary battery 7104, a lightweight and long-life portable display device can be provided.

[0494] Figure 33(F) shows an example of a wristwatch-type personal information terminal. The personal information terminal 7200 includes a housing 7201, a display unit 7202, a band 7203, a buckle 7204, operation buttons 7205, input / output terminals 7206, and the like.

[0495] The 7200 personal digital assistant (PDCA) can run various applications such as mobile phone calls, email, document viewing and creation, music playback, internet communication, and computer games.

[0496] The display unit 7202 has a curved display surface, allowing it to display information along the curved surface. The display unit 7202 also features a touch sensor, allowing it to be operated by touching the screen with a finger or stylus. For example, touching the icon 7207 displayed on the display unit 7202 can launch an application.

[0497] The operation button 7205 can be assigned various functions, including time setting, power on / off, wireless communication on / off, silent mode activation / deactivation, and power saving mode activation / deactivation. For example, the functions of the operation button 7205 can be freely configured by the operating system built into the personal digital assistant 7200.

[0498] Furthermore, the 7200 portable information terminal is capable of performing standardized short-range wireless communication. For example, it can communicate with a wireless-enabled headset to enable hands-free calling.

[0499] Furthermore, the portable information terminal 7200 is equipped with an input / output terminal 7206, allowing it to directly exchange data with other information terminals via a connector. It can also be charged via the input / output terminal 7206. Note that charging may also be performed wirelessly without using the input / output terminal 7206.

[0500] The display unit 7202 of the portable information terminal 7200 has a secondary battery according to one aspect of the present invention. By using a secondary battery according to one aspect of the present invention, a lightweight and long-lasting portable information terminal can be provided. For example, the secondary battery 7104 shown in Figure 33(E) can be incorporated inside the housing 7201 in a curved state, or inside the band 7203 in a bendable state.

[0501] The portable information terminal 7200 preferably has sensors. Preferably, the sensors include, for example, human body sensors such as fingerprint sensors, pulse sensors, and body temperature sensors, as well as touch sensors, pressure sensors, acceleration sensors, and the like.

[0502] Figure 33(G) shows an example of an armband-type display device. The display device 7300 has a display unit 7304 and a secondary battery according to one embodiment of the present invention. The display device 7300 may also be equipped with a touch sensor on the display unit 7304 and can also function as a portable information terminal.

[0503] The display unit 7304 has a curved display surface, allowing it to display information along the curved surface. Furthermore, the display device 7300 can change its display status via standardized short-range wireless communication or other means.

[0504] Furthermore, the display device 7300 is equipped with input / output terminals, allowing it to directly exchange data with other information terminals via connectors. It can also be charged via the input / output terminals. Note that charging may also be performed wirelessly without using the input / output terminals.

[0505] By using a secondary battery according to one aspect of the present invention as the secondary battery of the display device 7300, a lightweight and long-life display device can be provided.

[0506] Furthermore, an example of mounting the secondary battery with good cycle characteristics shown in the previous embodiment into an electronic device will be explained using Figures 33(H), 34, and 35.

[0507] By using a secondary battery according to one embodiment of the present invention as a secondary battery in everyday electronic devices, it is possible to provide lightweight and long-lasting products. Examples of everyday electronic devices include electric toothbrushes, electric shavers, and electric beauty devices. For the secondary batteries in these products, there is a need for a stick-shaped battery that is easy for the user to hold, is small, lightweight, and has a large charge / discharge capacity.

[0508] Figure 33(H) is a perspective view of a device also known as a tobacco-containing smoking device (electronic cigarette). In Figure 33(H), the electronic cigarette 7500 consists of an atomizer 7501 including a heating element, a secondary battery 7504 that supplies power to the atomizer, and a cartridge 7502 including a liquid supply bottle and a sensor. To enhance safety, a protection circuit to prevent overcharging and / or over-discharging of the secondary battery 7504 may be electrically connected to the secondary battery 7504. The secondary battery 7504 shown in Figure 33(H) has external terminals so that it can be connected to a charging device. Since the secondary battery 7504 is the tip when held, it is desirable that its total length is short and its weight is light. A secondary battery according to one aspect of the present invention has a high charge / discharge capacity and good cycle characteristics, so it is possible to provide a small and lightweight electronic cigarette 7500 that can be used for a long time over a long period of time.

[0509] Next, Figures 34(A) and 34(B) show an example of a foldable tablet terminal. The tablet terminal 9600 shown in Figures 34(A) and 34(B) includes a housing 9630a, a housing 9630b, a movable part 9640 connecting housings 9630a and 9630b, a display unit 9631 having display units 9631a and 9631b, switches 9625 to 9627, a fastener 9629, and an operation switch 9628. By using a flexible panel for the display unit 9631, a tablet terminal with a larger display area can be created. Figure 34(A) shows the tablet terminal 9600 in an open state, and Figure 34(B) shows the tablet terminal 9600 in a closed state.

[0510] Furthermore, the tablet terminal 9600 has a power storage unit 9635 inside the housing 9630a and housing 9630b. The power storage unit 9635 is provided across housing 9630a and housing 9630b, passing through the movable part 9640.

[0511] The display unit 9631 can have all or part of its area designated as a touch panel area, and data can be entered by touching images, characters, input forms, etc., including icons, displayed in that area. For example, keyboard buttons may be displayed on the entire surface of the display unit 9631a on the housing 9630a side, and information such as characters and images may be displayed on the display unit 9631b on the housing 9630b side.

[0512] Alternatively, the display unit 9631b on the housing 9630b may be used to display a keyboard, while the display unit 9631a on the housing 9630a may be used to display information such as characters and images. Alternatively, the display unit 9631 may be used to display a touch panel keyboard display switching button, so that the keyboard is displayed on the display unit 9631 when the button is touched with a finger or stylus.

[0513] Furthermore, it is possible to simultaneously input touch input to the touch panel area of ​​the display unit 9631a on the housing 9630a and the touch panel area of ​​the display unit 9631b on the housing 9630b.

[0514] Furthermore, switches 9625 to 9627 may not only serve as an interface for operating the tablet terminal 9600, but also as an interface for switching various functions. For example, at least one of switches 9625 to 9627 may function as a switch to turn the tablet terminal 9600 on and off. Also, for example, at least one of switches 9625 to 9627 may have a function to switch the display orientation, such as portrait or landscape, or a function to switch between monochrome and color display. Also, for example, at least one of switches 9625 to 9627 may have a function to adjust the brightness of the display unit 9631. The brightness of the display unit 9631 can be optimized according to the amount of ambient light during use, as detected by the light sensor built into the tablet terminal 9600. Note that the tablet terminal may incorporate other detection devices in addition to the light sensor, such as a gyroscope, an accelerometer, or other sensors that detect tilt.

[0515] Furthermore, while Figure 34(A) shows an example where the display area of ​​the display unit 9631a on the housing 9630a side and the display unit 9631b on the housing 9630b side are approximately the same, the display areas of the display units 9631a and 9631b are not particularly limited, and the size of one may differ from the other, as may the display quality. For example, one display panel may be capable of displaying a higher resolution than the other.

[0516] Figure 34(B) shows the tablet terminal 9600 in a folded state. The tablet terminal 9600 includes a housing 9630, a solar cell 9633, and a charge / discharge control circuit 9634 including a DC-DC converter 9636. Furthermore, a secondary battery according to one embodiment of the present invention is used as the energy storage body 9635.

[0517] As mentioned above, the tablet terminal 9600 is foldable, so when not in use, the casings 9630a and 9630b can be folded together. Folding protects the display unit 9631, thereby increasing the durability of the tablet terminal 9600. Furthermore, the energy storage unit 9635 using a secondary battery according to one aspect of the present invention has a high charge / discharge capacity and good cycle characteristics, thus providing a tablet terminal 9600 that can be used for long periods of time over a long period of time.

[0518] In addition, the tablet terminal 9600 shown in Figures 34(A) and 34(B) may have functions such as displaying various information (still images, videos, text images, etc.), displaying a calendar, date, or time on the display unit, a touch input function for touch input operation or editing of the information displayed on the display unit, and a function for controlling processing by various software (programs).

[0519] The solar cell 9633 mounted on the surface of the tablet terminal 9600 can supply power to the touch panel, display unit, or video signal processing unit, etc. The solar cell 9633 can be installed on one or both sides of the housing 9630, allowing for an efficient configuration of charging the energy storage unit 9635. Using a lithium-ion battery as the energy storage unit 9635 offers advantages such as miniaturization.

[0520] Furthermore, the configuration and operation of the charge / discharge control circuit 9634 shown in Figure 34(B) will be explained with a block diagram in Figure 34(C). Figure 34(C) shows the solar cell 9633, energy storage unit 9635, DC-DC converter 9636, converter 9637, switches SW1 to SW3, and display unit 9631, with the energy storage unit 9635, DC-DC converter 9636, converter 9637, and switches SW1 to SW3 corresponding to the charge / discharge control circuit 9634 shown in Figure 34(B).

[0521] First, let's explain an example of operation when electricity is generated by the solar cell 9633 using ambient light. The power generated by the solar cell is boosted or stepped down by the DC-DC converter 9636 to obtain a voltage suitable for charging the energy storage unit 9635. When power from the solar cell 9633 is used to operate the display unit 9631, switch SW1 is turned on, and the converter 9637 boosts or steps down the voltage to the voltage required by the display unit 9631. When the display unit 9631 is not being used, SW1 is turned off and SW2 is turned on to charge the energy storage unit 9635.

[0522] The solar cell 9633 is shown as an example of a power generation method, but it is not particularly limited, and the storage unit 9635 may be charged by other power generation methods such as piezoelectric elements and thermoelectric elements (Peltier elements). For example, a contactless power transmission module that transmits and receives power wirelessly (non-contact) to charge the storage unit may be used, and a combination of other charging methods may also be used.

[0523] Figure 35 shows an example of another electronic device. In Figure 35, the display device 8000 is an example of an electronic device using a secondary battery 8004 according to one aspect of the present invention. Specifically, the display device 8000 corresponds to a display device for receiving TV broadcasts and has a housing 8001, a display unit 8002, a speaker unit 8003, a secondary battery 8004, etc. The secondary battery 8004 according to one aspect of the present invention is provided inside the housing 8001. The display device 8000 can receive power from a commercial power source or it can use power stored in the secondary battery 8004. Therefore, even when power cannot be supplied from a commercial power source due to a power outage or the like, the display device 8000 can be used by using the secondary battery 8004 according to one aspect of the present invention as an uninterruptible power source.

[0524] The display unit 8002 can use semiconductor display devices such as liquid crystal displays, light-emitting devices equipped with light-emitting elements such as organic EL elements in each pixel, electrophoretic displays, DMDs (Digital Micromirror Devices), PDPs (Plasma Display Panels), and FEDs (Field Emission Displays).

[0525] Furthermore, the term "display device" includes all information display devices, such as those for receiving TV broadcasts, personal computers, and advertising displays.

[0526] In Figure 35, the fixed-type lighting device 8100 is an example of an electronic device using a secondary battery 8103 according to one aspect of the present invention. Specifically, the lighting device 8100 includes a housing 8101, a light source 8102, a secondary battery 8103, etc. In Figure 35, the case in which the secondary battery 8103 is installed inside the ceiling 8104 on which the housing 8101 and light source 8102 are installed is illustrated, but the secondary battery 8103 may also be installed inside the housing 8101. The lighting device 8100 can receive power from a commercial power source, or it can use power stored in the secondary battery 8103. Therefore, even when power cannot be supplied from a commercial power source due to a power outage or the like, the lighting device 8100 can be used by using the secondary battery 8103 according to one aspect of the present invention as an uninterruptible power source.

[0527] Although Figure 35 illustrates a fixed lighting device 8100 installed on the ceiling 8104, the secondary battery according to one aspect of the present invention can also be used in fixed lighting devices installed on surfaces other than the ceiling 8104, such as the side wall 8105, floor 8106, window 8107, etc., or in tabletop lighting devices, etc.

[0528] Furthermore, the light source 8102 can be an artificial light source that artificially generates light using electricity. Specifically, examples of the above artificial light sources include incandescent light bulbs, discharge lamps such as fluorescent lamps, and light-emitting elements such as LEDs and organic EL elements.

[0529] In Figure 35, an air conditioner having an indoor unit 8200 and an outdoor unit 8204 is an example of an electronic device using a secondary battery 8203 according to one aspect of the present invention. Specifically, the indoor unit 8200 has a housing 8201, an air outlet 8202, a secondary battery 8203, etc. In Figure 35, the case in which the secondary battery 8203 is provided in the indoor unit 8200 is illustrated, but the secondary battery 8203 may also be provided in the outdoor unit 8204. Alternatively, the secondary battery 8203 may be provided in both the indoor unit 8200 and the outdoor unit 8204. The air conditioner can receive power from a commercial power source, or it can use power stored in the secondary battery 8203. In particular, when both the indoor unit 8200 and the outdoor unit 8204 are equipped with secondary batteries 8203, even when power cannot be supplied from the commercial power source due to a power outage or the like, the air conditioner can be used by using the secondary battery 8203 according to one aspect of the present invention as an uninterruptible power supply.

[0530] Although Figure 35 illustrates a separate-type air conditioner consisting of an indoor unit and an outdoor unit, the secondary battery according to one aspect of the present invention can also be used in an integrated-type air conditioner that has the functions of both the indoor and outdoor units in a single housing.

[0531] In Figure 35, the electric refrigerator-freezer 8300 is an example of an electronic device using a secondary battery 8304 according to one aspect of the present invention. Specifically, the electric refrigerator-freezer 8300 includes a housing 8301, a refrigerator door 8302, a freezer door 8303, a secondary battery 8304, etc. In Figure 35, the secondary battery 8304 is installed inside the housing 8301. The electric refrigerator-freezer 8300 can receive power from a commercial power source, or it can use power stored in the secondary battery 8304. Therefore, even when power cannot be supplied from a commercial power source due to a power outage or the like, the electric refrigerator-freezer 8300 can be used by using the secondary battery 8304 according to one aspect of the present invention as an uninterruptible power source.

[0532] Furthermore, among the electronic devices mentioned above, high-frequency heating devices such as microwave ovens and electric rice cookers require high power in a short period of time. Therefore, by using a secondary battery according to one aspect of the present invention as an auxiliary power source to supplement the power that cannot be supplied by the commercial power supply, it is possible to prevent the commercial power supply circuit breaker from tripping when the electronic device is in use.

[0533] Furthermore, by storing power in the secondary battery during periods when electronic devices are not in use, particularly during periods when the proportion of the total amount of power supplied by the commercial power source that is actually used (referred to as the power usage rate) is low, it is possible to suppress the increase in the power usage rate outside of these periods. For example, in the case of the electric refrigerator-freezer 8300, power is stored in the secondary battery 8304 at night when the temperature is low and the refrigerator door 8302 and freezer door 8303 are not opened or closed. Then, during the daytime when the temperature is high and the refrigerator door 8302 and freezer door 8303 are opened and closed, the secondary battery 8304 can be used as an auxiliary power source, thereby keeping the daytime power usage rate low.

[0534] According to one aspect of the present invention, the cycle characteristics of a secondary battery can be improved, thereby enhancing its reliability. Furthermore, according to one aspect of the present invention, a secondary battery with a high charge / discharge capacity can be created, thereby improving the characteristics of the secondary battery and thus making the secondary battery itself smaller and lighter. Therefore, by incorporating a secondary battery according to one aspect of the present invention into the electronic device described in this embodiment, it is possible to create an electronic device that has a longer lifespan and is lighter.

[0535] This embodiment can be implemented in appropriate combination with other embodiments.

[0536] (Embodiment 6) In this embodiment, an example of an electronic device using a secondary battery, as described in the previous embodiment, will be explained using Figures 36(A) to 37(C).

[0537] Figure 36(A) shows an example of a wearable device. Wearable devices use rechargeable batteries as a power source. Furthermore, in order to enhance splash resistance, water resistance, or dust resistance when used by users in daily life or outdoors, there is a demand for wearable devices that can be charged wirelessly in addition to wired charging with exposed connectors.

[0538] For example, a secondary battery according to one aspect of the present invention can be mounted in a spectacle-type device 4000 as shown in Figure 36(A). The spectacle-type device 4000 has a frame 4000a and a display unit 4000b. By mounting the secondary battery in the temple portion of the curved frame 4000a, a lightweight spectacle-type device 4000 with good weight balance and a long continuous usage time can be achieved. By incorporating a secondary battery according to one aspect of the present invention, a configuration that can accommodate space saving due to the miniaturization of the housing can be realized.

[0539] Furthermore, a secondary battery according to one aspect of the present invention can be mounted in the headset-type device 4001. The headset-type device 4001 has at least a microphone section 4001a, a flexible pipe 4001b, and an earphone section 4001c. A secondary battery can be provided in the flexible pipe 4001b and / or in the earphone section 4001c. By incorporating a secondary battery according to one aspect of the present invention, a configuration that can accommodate space saving due to the miniaturization of the housing can be realized.

[0540] Furthermore, a secondary battery according to one aspect of the present invention can be mounted in a device 4002 that can be directly attached to the body. The secondary battery 4002b can be provided within the thin housing 4002a of the device 4002. By incorporating a secondary battery according to one aspect of the present invention, a configuration that can accommodate space saving due to the miniaturization of the housing can be realized.

[0541] Furthermore, a secondary battery according to one aspect of the present invention can be mounted on the device 4003, which can be attached to clothing. The secondary battery 4003b can be provided within the thin housing 4003a of the device 4003. By incorporating the secondary battery according to one aspect of the present invention, a configuration that can accommodate space saving due to the miniaturization of the housing can be realized.

[0542] Furthermore, a secondary battery according to one aspect of the present invention can be mounted on the belt-type device 4006. The belt-type device 4006 has a belt portion 4006a and a wireless power supply and receiving portion 4006b, and a secondary battery can be mounted inside the belt portion 4006a. By incorporating a secondary battery according to one aspect of the present invention, a configuration that can accommodate space saving due to the miniaturization of the housing can be realized.

[0543] Furthermore, a secondary battery according to one aspect of the present invention can be mounted in the wristwatch-type device 4005. The wristwatch-type device 4005 has a display unit 4005a and a strap unit 4005b, and a secondary battery can be provided in either the display unit 4005a or the strap unit 4005b. By providing a secondary battery according to one aspect of the present invention, a configuration that can accommodate space saving due to the miniaturization of the housing can be realized.

[0544] The display unit 4005a can display not only the time, but also various other information such as incoming emails and phone calls.

[0545] Furthermore, since the wristwatch-type device 4005 is a wearable device that is worn directly on the wrist, it may be equipped with sensors to measure the user's pulse, blood pressure, etc. It can accumulate data on the user's exercise level and health, allowing for health management.

[0546] Figure 36(B) shows a perspective view of the wristwatch-type device 4005 after it has been removed from the arm.

[0547] A side view is also shown in Figure 36(C). Figure 36(C) shows the internal structure with the secondary battery 913 built in. The secondary battery 913 is the secondary battery shown in Embodiment 4. The secondary battery 913 is located in a position that overlaps with the display unit 4005a, and is small and lightweight.

[0548] Figure 36(D) shows an example of wireless earphones. Here, wireless earphones having a pair of main units 4100a and 4100b are illustrated, but they do not necessarily have to be a pair.

[0549] The main units 4100a and 4100b include a driver unit 4101, an antenna 4102, and a secondary battery 4103. They may also have a display unit 4104. Preferably, they also have a circuit board with a wireless IC or the like, charging terminals, etc. They may also have a microphone.

[0550] The case 4110 contains a secondary battery 4111. Preferably, it also has a circuit board on which wireless ICs, charge control ICs, and other circuits are mounted, as well as charging terminals. It may also have a display unit, buttons, etc.

[0551] The main units 4100a and 4100b can communicate wirelessly with other electronic devices such as smartphones. This allows them to play audio data sent from other electronic devices. Furthermore, if the main units 4100a and 4100b have microphones, they can send sound acquired by the microphones to other electronic devices, process the audio data, and then send it back to the main units 4100a and 4100b for playback. This allows them to be used, for example, as a translation device.

[0552] Furthermore, the secondary battery 4103 in the main unit 4100a can be charged from the secondary battery 4111 in the case 4100. The coin-type secondary battery, cylindrical secondary battery, etc., from the previous embodiment can be used as the secondary battery 4111 and secondary battery 4103. The secondary battery using the positive electrode active material 100 obtained in Embodiment 1 as the positive electrode has a high energy density, and by using it in the secondary battery 4103 and secondary battery 4111, a configuration that can accommodate space saving associated with the miniaturization of wireless earphones can be realized.

[0553] Figure 37(A) shows an example of a cleaning robot. The cleaning robot 6300 has a display unit 6302 located on the top surface of the housing 6301, multiple cameras 6303 located on the sides, a brush 6304, operation buttons 6305, a secondary battery 6306, and various sensors. Although not shown, the cleaning robot 6300 is equipped with wheels, a suction port, etc. The cleaning robot 6300 is self-propelled, can detect dirt 6310, and can suck up the dirt from a suction port located on the bottom surface.

[0554] For example, the cleaning robot 6300 can analyze images captured by the camera 6303 to determine the presence or absence of obstacles such as walls, furniture, or steps. Furthermore, if the image analysis detects an object that could become entangled in the brush 6304, such as wiring, the rotation of the brush 6304 can be stopped. The cleaning robot 6300 is equipped with a secondary battery 6306 according to one aspect of the present invention and a semiconductor device or electronic component. By using the secondary battery 6306 according to one aspect of the present invention in the cleaning robot 6300, the cleaning robot 6300 can be made into a highly reliable electronic device with a long operating time.

[0555] Figure 37(B) shows an example of a robot. The robot 6400 shown in Figure 37(B) is equipped with a secondary battery 6409, an illuminance sensor 6401, a microphone 6402, an upper camera 6403, a speaker 6404, a display unit 6405, a lower camera 6406 and an obstacle sensor 6407, a movement mechanism 6408, a computing device, and the like.

[0556] Microphone 6402 has the function of detecting the user's voice and ambient sounds. Speaker 6404 has the function of emitting sound. Robot 6400 can communicate with the user using microphone 6402 and speaker 6404.

[0557] The display unit 6405 has the function of displaying various types of information. The robot 6400 can display the information desired by the user on the display unit 6405. The display unit 6405 may be equipped with a touch panel. The display unit 6405 may also be a detachable information terminal, and by installing it in a fixed position on the robot 6400, charging and data transfer can be made possible.

[0558] The upper camera 6403 and lower camera 6406 have the function of imaging the area around the robot 6400. In addition, the obstacle sensor 6407 can detect the presence or absence of obstacles in the direction of travel when the robot 6400 moves forward using the movement mechanism 6408. The robot 6400 can recognize its surrounding environment and move safely using the upper camera 6403, lower camera 6406 and obstacle sensor 6407.

[0559] The robot 6400 is equipped with a secondary battery 6409 according to one aspect of the present invention and a semiconductor device or electronic components inside. By using the secondary battery according to one aspect of the present invention in the robot 6400, the robot 6400 can be made into an electronic device with a long operating time and high reliability.

[0560] Figure 37(C) shows an example of an aircraft. The aircraft 6500 shown in Figure 37(C) has a propeller 6501, a camera 6502, and a secondary battery 6503, and has the capability to fly autonomously.

[0561] For example, image data captured by camera 6502 is stored in electronic component 6504. Electronic component 6504 can analyze the image data and detect the presence or absence of obstacles during movement. Furthermore, electronic component 6504 can estimate the remaining battery level from the change in the storage capacity of secondary battery 6503. The aircraft 6500 is equipped with a secondary battery 6503 according to one aspect of the present invention. By using a secondary battery according to one aspect of the present invention in the aircraft 6500, the aircraft 6500 can be made into an electronic device with a long operating time and high reliability.

[0562] This embodiment can be implemented in appropriate combination with other embodiments.

[0563] (Embodiment 7) This embodiment shows an example in which a secondary battery according to one aspect of the present invention is mounted on a vehicle.

[0564] By installing secondary batteries in vehicles, next-generation clean energy vehicles such as hybrid vehicles (HV), electric vehicles (EV), or plug-in hybrid vehicles (PHV) can be realized.

[0565] Figure 38 illustrates a vehicle using a secondary battery, which is one embodiment of the present invention. The automobile 8400 shown in Figure 38(A) is an electric vehicle that uses an electric motor as a power source for driving. Alternatively, it is a hybrid vehicle that can appropriately select and use an electric motor and an engine as power sources for driving. By using one embodiment of the present invention, a vehicle with a long driving range can be realized. The automobile 8400 also has a secondary battery. The secondary battery can be used by arranging the secondary battery modules shown in Figures 23(C) and 23(D) on the floor of the vehicle. Alternatively, a battery pack combining multiple secondary batteries as shown in Figure 26 may be installed on the floor of the vehicle. The secondary battery can not only drive the electric motor 8406 but also supply power to light-emitting devices such as headlights 8401 and room lights (not shown).

[0566] Furthermore, the secondary battery can supply power to display devices such as the speedometer and tachometer of the 8400 automobile. The secondary battery can also supply power to semiconductor devices such as the navigation system of the 8400 automobile.

[0567] The automobile 8500 shown in Figure 38(B) can be charged by receiving power from an external charging facility via a plug-in method and / or a contactless power supply method to the secondary battery of the automobile 8500. Figure 38(B) shows the state in which the secondary battery 8024 mounted on the automobile 8500 is being charged from a ground-mounted charging device 8021 via a cable 8022. When charging, the charging method and connector specifications may be carried out as appropriate using a prescribed method such as CHAdeMO® or Combo. The charging device 8021 may be a charging station installed in a commercial facility or a household power supply. For example, the secondary battery 8024 mounted on the automobile 8500 can be charged by an external power supply using plug-in technology. Charging can be performed by converting AC power to DC power via a conversion device such as an AC / DC converter.

[0568] Although not shown in the diagram, the vehicle can also be charged by mounting a power receiving device on the vehicle and receiving power wirelessly from a ground-based power transmission device. In this wireless power supply method, charging can be performed not only when the vehicle is stopped but also while it is in motion by incorporating the power transmission device into the road and / or exterior wall. Furthermore, this wireless power supply method can be used to transmit and receive power between vehicles. In addition, solar cells can be installed on the exterior of the vehicle to charge the secondary battery when the vehicle is stopped and / or in motion. For such wireless power supply, electromagnetic induction and / or magnetic resonance methods can be used.

[0569] Furthermore, Figure 38(C) shows an example of a two-wheeled vehicle using a secondary battery according to one embodiment of the present invention. The scooter 8600 shown in Figure 38(C) is equipped with a secondary battery 8602, a side mirror 8601, and a turn signal light 8603. The secondary battery 8602 can supply electricity to the turn signal light 8603.

[0570] Furthermore, the scooter 8600 shown in Figure 38(C) can accommodate the secondary battery 8602 in the under-seat storage compartment 8604. The secondary battery 8602 can be stored in the under-seat storage compartment 8604 even if the compartment is small. The secondary battery 8602 is removable, so when charging, it can be carried indoors, charged, and then stored back in before riding.

[0571] According to one aspect of the present invention, the cycle characteristics of the secondary battery are improved, and the charge and discharge capacity of the secondary battery can be increased. Therefore, the secondary battery itself can be made smaller and lighter. If the secondary battery itself can be made smaller and lighter, it will contribute to the weight reduction of the vehicle, and thus the driving range can be improved. In addition, the secondary battery installed in the vehicle can be used as a power supply source other than the vehicle. In this case, for example, it is possible to avoid using commercial power during peak power demand. By avoiding the use of commercial power during peak power demand, it is possible to contribute to energy saving and the reduction of carbon dioxide emissions. Furthermore, if the cycle characteristics are good, the secondary battery can be used for a long period of time, so the amount of rare metals such as cobalt can be reduced.

[0572] This embodiment can be implemented in appropriate combination with other embodiments. [Examples]

[0573] In this example, a positive electrode active material 100 according to one embodiment of the present invention was prepared, and its characteristics were analyzed.

[0574] <Fabrication of positive electrode active material> The sample prepared in this embodiment will be described with reference to the preparation method shown in Figures 2 and 3.

[0575] In step S14 of Figure 2, commercially available lithium cobalt oxide (Cellseed C-10N, manufactured by Nippon Chemical Industrial Co., Ltd.) was prepared as LiMO2, containing cobalt as the transition metal M and no other additive elements. In the initial heating step S15, this lithium cobalt oxide was placed in a crucible, covered, and heated in a muffle furnace at 850°C for 2 hours. The muffle furnace was then subjected to an oxygen atmosphere and no flow occurred (O2 purging). Upon checking the recovered amount after the initial heating, it was found that the weight had decreased slightly. This decrease in weight may be due to the removal of impurities from LCO.

[0576] According to steps S21 and S41 shown in Figures 3(A) and 3(B), Mg, F, Ni, and Al were added separately as additive elements. According to step S21 shown in Figure 3(A), LiF was prepared as the F source and MgF2 was prepared as the Mg source. LiF and MgF2 were weighed in a molar ratio of 1:3. Next, LiF and MgF2 were mixed in dehydrated acetone and stirred at a rotational speed of 400 rpm for 12 hours to obtain the additive element source X A A mixture was prepared. A ball mill was used for mixing, and zirconium oxide balls were used as the grinding media. In a 45 mL ball mill, 20 mL of dehydrated acetone and 22 g of zirconium oxide balls (1 mmφ), along with a total of approximately 10 g of F source and Mg source, were added and mixed. The mixture was then sieved through a sieve with a 300 μm mesh to obtain a mixture of additive element X with uniform particle size. A I obtained it.

[0577] Next, the additive element source X A The amount was weighed to be 1 atomic percent of the transition metal M, and it was mixed dry with LCO after initial heating. The mixture was stirred at a rotational speed of 150 rpm for 1 hour. This was the added element source X. A The stirring conditions were gentler than those used to obtain the final result. Finally, the mixture was sieved through a sieve with a 300 μm mesh to obtain a mixture A with uniform particle size.

[0578] Next, mixture A was heated. The heating conditions were 900°C for 20 hours. During heating, a lid was placed over the crucible containing mixture A. The crucible was kept in an oxygen-containing atmosphere, and the entry and exit of oxygen was blocked. Heating yielded LCO (composite oxide A) containing Mg and F.

[0579] Next, the composite oxide A is combined with the added element source X. B Add the following. Following step S41 shown in Figure 3(B), nickel hydroxide was prepared as the Ni source and aluminum hydroxide as the Al source. Nickel hydroxide was weighed to be 0.5 atomic percent of the transition metal M, and aluminum hydroxide was weighed to be 0.5 atomic percent of the transition metal M, and mixed dry with composite oxide A. At this time, it was stirred at a rotation speed of 150 rpm for 1 hour. A ball mill was used for mixing, and zirconium oxide balls were used as the grinding media. Approximately 7.5 g of Ni source and Al source were added to a 45 mL capacity ball mill along with 22 g of zirconium oxide balls (1 mmφ) and mixed. This is the added element source X A The stirring conditions were gentler than those used to obtain the first result. Finally, the mixture was sieved using a sieve with a 300 μm mesh to obtain mixture B with uniform particle size.

[0580] Next, mixture B was heated. The heating conditions were 850°C for 10 hours. During heating, a lid was placed over the crucible containing mixture B. The crucible was kept in an oxygen-containing atmosphere, and the entry and exit of this oxygen was blocked. Heating yielded LCO containing Mg, F, Ni, and Al. The cathode active material (composite oxide) obtained in this way was designated as Sample 1-1.

[0581] Furthermore, Sample 1-2 was prepared in the same manner as Sample 1-1, except that the heating time in step S15 was set to 10 hours.

[0582] Furthermore, Sample 1-3 was prepared in the same manner as Sample 1-1, except that the heating temperature in step S15 was set to 750°C.

[0583] Furthermore, Sample 1-4 was prepared in the same manner as Sample 1-1, except that the heating temperature in step S15 was set to 900°C.

[0584] Furthermore, Sample 1-5 was prepared in the same manner as Sample 1-1, except that the heating temperature in step S15 was set to 950°C.

[0585] Furthermore, a sample in which step S15 heating was omitted was designated as Sample 2. In Sample 2, the heating in step S53 was performed with an oxygen flow rate of 10 L / min.

[0586] As a comparative example, untreated lithium cobalt oxide (Cellseed C-10N, manufactured by Nippon Chemical Industrial Co., Ltd.) was designated as Sample 10.

[0587] Sample 11 was obtained by simply heating lithium cobalt oxide as described in step S15.

[0588] Table 1 shows the preparation conditions for samples 1-1, 1-2, 1-3, 1-4, 1-5, 2, 10, and 11. As is clear from Table 1, samples 1-1 through 1-5 all share the common characteristic of being prepared by initially heating LiCoO2 without any additive elements, followed by the addition of magnesium, fluorine, nickel, and aluminum sources and further heating. Therefore, to distinguish them from samples that do not share this characteristic, they can all be referred to as Sample 1.

[0589] [Table 1]

[0590] <sem> Figure 39 shows the results of the SEM (Scanning Electron Microscope) observation. In this example, the SEM observation was performed using a Hitachi High-Tech SU8030 scanning electron microscope, with measurement conditions of an acceleration voltage of 5kV and magnifications of 5000x and 20,000x.

[0591] Figures 39(A) and 39(B) are SEM images of sample 10 (Cellseed C-10N, manufactured by Nippon Chemical Industrial Co., Ltd.), which is pre-synthesized lithium cobalt oxide (LCO). Figure 39(A) shows the overall structure of the LCO. Figure 39(B) is a magnified view of the same particle as in Figure 39(A), showing a portion of the LCO. Both observations reveal that the surface of the LCO is rough and appears to have foreign matter adhering to it. It can be seen that the surface of pre-synthesized LCO has many irregularities.

[0592] Figures 39(C) and 39(D) are SEM images of sample 11 (LCO that has undergone heat treatment on the above-mentioned Cell Seed C-10N). Figure 39(C) shows the entire LCO. Figure 39(D) is a magnified view of Figure 39(C), showing a part of the LCO. Both observations show that the surface of the LCO has become smoother. It can be seen that the surface of the LCO that has undergone initial heating has fewer irregularities.

[0593] Figures 39(E) and 39(F) show SEM images of sample 1-1 (LCO containing Mg, F, Ni, and Al as additive elements, obtained by heat treatment of the above-mentioned Cell Seed C-10N). Figure 39(E) shows the entire LCO. Figure 39(F) is a magnified view of Figure 39(E), showing a part of the LCO. Both observations show that the surface of the LCO has become smoother. It is smoother than the LCO that underwent only initial heating. It can be seen that the surface of the LCO that underwent initial heating and then had additive elements added has fewer irregularities.

[0594] SEM observations revealed that the LCO surface becomes smoother with initial heating. It is believed that the surface becomes smoother because the initial heating improves the LCO surface and also mitigates crystal displacement. Furthermore, it was found that the surface smoothness is maintained, or even becomes smoother, even when additive elements are added to the LCO after initial heating.

[0595] Next, the powder, which was completed as LCO, was observed using SEM before pressing, after pressing, and after the cycle test. First, the appearance of the powder is described. Figure 40(A) shows the SEM image of sample 1-1, which underwent initial heating. This corresponds to Figure 39(F). Figure 40(B) shows sample 10, which did not undergo initial heating. From Figures 40(A) and 40(B), it can be seen that the surface of sample 1-1, which underwent initial heating, is smooth and has less foreign matter adhering to it.

[0596] Next, we will describe the state before pressing. Before pressing refers to the LCO obtained by volatilizing the solvent from a slurry made by mixing the active material and conductive material under predetermined conditions, and then coating the current collector with it. The conditions were that powdered LCO as the active material, acetylene black (AB) as the conductive material, and PVDF as the binder were mixed in a ratio of LCO:AB:PVDF = 95:3:2 (wt%) at 2000 rpm to prepare the slurry. NMP was used as the solvent for the slurry, and after coating the aluminum current collector with the slurry, the solvent was volatilized. Figure 40(C) shows the SEM image of sample 1-1 before pressing, which underwent initial heating. Figure 40(D) ​​shows the SEM image of sample 10 before pressing, which did not undergo initial heating. From Figures 40(C) and 40(D), it can be confirmed that cracks appeared on the surface of the LCO, etc., as a result of the mixing.

[0597] Next, we will describe the condition after pressing. "After pressing" refers to the state after the solvent has evaporated and the slurry on the current collector has been pressed. The pressing conditions were to first apply pressure at 210 kN / m, and then apply pressure at 1467 kN / m. Figure 40(E) shows the SEM image of sample 1-1 after pressing, which underwent initial heating. Figure 40(F) shows the SEM image of sample 10 after pressing, which did not undergo initial heating. From Figures 40(E) and 40(F), it can be confirmed that slip occurred on the LCO surface, etc., due to pressing.

[0598] <Slip> Slip, also known as a stacking fault, refers to the deformation of LCOs along the lattice pattern direction (ab-plane direction) due to pressing. This deformation includes the shifting of the lattice patterns back and forth. When the lattice patterns shift back and forth, a step is created on the particle surface perpendicular to the lattice pattern (c-axis direction). This surface step can be seen as a linear line crossing the left and right sides of the photograph in Figures 40(E) and 40(F).

[0599] Next, we will describe the results after the cycle test. The cycle test involved creating a half-cell with the LCO after the pressing described above and performing measurements.

[0600] For the half-cell electrolyte, a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC = 3:7 was prepared, with 2 wt% vinylene carbonate (VC) added as an additive. The electrolyte in the electrolyte solution was 1 mol / L lithium hexafluoride phosphate (LiPF6).

[0601] Polypropylene was used as the separator for the half-cell. Lithium metal was used as the counter electrode for the half-cell. Coin-shaped half-cells were formed in this way, and their cycle characteristics were measured.

[0602] The discharge rate and charge rate of the cycle conditions will b...

Claims

1. A secondary battery having a positive electrode, The positive electrode has a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer has a plurality of positive electrode active material particles, the positive electrode active material particles include lithium cobalt oxide, magnesium, fluorine, aluminum, and nickel, The plurality of positive electrode active material particles are The positive electrode is Lithium metal is used as the counter electrode. The electrolyte used was a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7, with 2 wt% vinylene carbonate added. The electrolyte solution is incorporated into a battery prepared by using 1 mol / L lithium hexafluorophosphate as an electrolyte, A secondary battery in which, in a graph of dQ / dV (mAh / g V) obtained by differentiating the charge capacity (Q) measured when the battery is charged to 4.9 V at 10 mA / g in a 25° C. environment with respect to the voltage (V) and the voltage (V), the graph has a maximum value in the range of 4.5 V or more and 4.6 V or less, and has a peak with a full width at half maximum of 0.10 V or more.

2. A secondary battery having a positive electrode, The positive electrode has a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer has a plurality of positive electrode active material particles, the positive electrode active material particles include lithium cobalt oxide, magnesium, fluorine, aluminum, and nickel, The plurality of positive electrode active material particles are The positive electrode is incorporated into a battery prepared using lithium metal as a counter electrode, A secondary battery in which, in a graph of dQ / dV (mAh / g V) obtained by differentiating the charge capacity (Q) measured when the battery is charged to 4.9 V at 10 mA / g in a 25° C. environment with respect to the voltage (V) and the voltage (V), the graph has a maximum value in the range of 4.5 V or more and 4.6 V or less, and has a peak with a full width at half maximum of 0.10 V or more.

3. A secondary battery having a positive electrode, The positive electrode has a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer has a plurality of positive electrode active material particles, the positive electrode active material particles include lithium cobalt oxide, magnesium, fluorine, aluminum, and nickel, The plurality of positive electrode active material particles are The positive electrode is Lithium metal is used as the counter electrode. The electrolyte used was a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7, with 2 wt% vinylene carbonate added. The electrolyte solution is incorporated into a battery prepared by using 1 mol / L lithium hexafluorophosphate as an electrolyte, A secondary battery, in which a graph of dQ / dV (mAh / g V) obtained by differentiating a charge capacity (Q) with respect to a voltage (V) measured when the battery was charged to 4.9 V at 10 mA / g in an environment of 25° C., versus the voltage (V), has a first maximum value in the range of 4.5 V or more and 4.6 V or less, and a second maximum value in the range of 4.15 V or more and 4.25 V or less, and a ratio of the second maximum value to the first maximum value (first maximum value / second maximum value) is 0.8 or less.

4. A secondary battery having a positive electrode, The positive electrode has a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer has a plurality of positive electrode active material particles, the positive electrode active material particles include lithium cobalt oxide, magnesium, fluorine, aluminum, and nickel, The plurality of positive electrode active material particles are The positive electrode is It is incorporated into a battery made with lithium metal as the counter electrode, A secondary battery, in which a graph of dQ / dV (mAh / g V) obtained by differentiating a charge capacity (Q) with respect to a voltage (V) measured when the battery was charged to 4.9 V at 10 mA / g in an environment of 25° C., versus the voltage (V), has a first maximum value in the range of 4.5 V or more and 4.6 V or less, and a second maximum value in the range of 4.15 V or more and 4.25 V or less, and a ratio of the second maximum value to the first maximum value (first maximum value / second maximum value) is 0.8 or less.

5. In any one of claims 1 to 4, The secondary battery is discharged at 0.5C (1C=200mA / g) to 2.5V before being charged at 10mA / g to 4.9V in a 25°C environment.

6. In any one of claims 1 to 5, The charge capacity (Q) data in the measurement is taken at intervals of 1 second or when there is a voltage fluctuation of 1 mV. The data of the charging capacity (Q) is a value obtained by integrating the current of the battery and time when the voltage fluctuation of 1 mV occurs at the 1 second interval.

7. In any one of claims 1 to 6, In the measurement, data on the nth charge capacity (Q) and data on the n+1th charge capacity (Q) are obtained, and then the change in charge capacity (dQ), which is the difference between the nth and the n+1th, is defined as the change in charge capacity (dQ) of the nth charge capacity.

8. In any one of claims 1 to 7, A secondary battery, in which, after obtaining the nth voltage data and the n+1th voltage data in the measurement, the voltage change (dV) which is the difference between the nth and the n+1th voltage data is defined as the nth voltage change (dV).

9. In any one of claims 1 to 8, A secondary battery, comprising: a first average value (dQ average value) of the nth to n+500th values ​​of the change in charging capacity (dQ); a second average value (dV average value) of the nth to n+500th values ​​of the change in voltage (dV); and the first average value (dQ average value) / the second average value (dV average value) being the dQ / dV.

10. In any one of claims 1 to 9, In an XPS analysis of the positive electrode active material particles, the number of magnesium atoms is 0.4 to 1.5 times the number of cobalt atoms.

11. In any one of claims 1 to 10, The positive electrode active material particles have a layered rock salt type crystal structure in a discharged state.

12. 12. An electronic device comprising: the secondary battery according to claim 1; a display unit; and a sensor.