Positive plate and battery

By adjusting the particle size ratio of lithium nickelate to the positive active material and adding titanium, the conduction of lithium ions is optimized, which solves the problem of insufficient conduction in lithium-ion batteries by replenishing lithium in the positive electrode, and achieves high capacity retention and low impedance. Improved battery cycle life and charge and discharge efficiency.

CN118841520APending Publication Date: 2024-10-25ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 7 Cited by

Patent Information

Application Number
CN202410838673.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

The existing positive electrode lithium replenishment method has deficiencies in controlling lithium ion conduction, resulting in low capacity retention and high impedance of lithium-ion batteries, affecting their application in fields such as electric vehicles and smartphones.

Method used

By regulating the particle size ratio between lithium nickelate and the positive active material, the conduction of lithium ions is optimized, and titanium is added to the positive active material to stabilize the structure of lithium nickelate, reduce battery internal resistance and improve cycle life.

Benefits of technology

It achieves high capacity retention and low impedance of lithium-ion batteries, improves charge and discharge efficiency and cycle life, while reducing battery self-discharge and gas production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004913851340000171
    Figure BDA0004913851340000171
  • Figure BDA0004913851340000181
    Figure BDA0004913851340000181
Patent Text Reader

Abstract

The invention relates to the field of batteries, in particular to a positive plate and a battery comprising the positive plate. The positive plate comprises lithium nickelate and a positive active material; the ratio of the particle size of the lithium nickelate to the particle size of the positive electrode active material is (0.1-40): 1. The positive plate provided by the invention can improve the problem of poor conduction controllability of a positive lithium supplement mode on lithium ions. Comprising the positive plate disclosed by the invention can give consideration to high capacity and low impedance, and has better cycle life and charge-discharge efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a positive electrode sheet and a battery comprising the positive electrode sheet. Background Art

[0002] In recent years, lithium-ion batteries have become the main power source for modern electronic devices and electric vehicles, and people are extremely concerned about their high energy density and long service life. During the first charge and discharge process of lithium-ion batteries, the solid electrolyte interface (SEI) film formed on the surface of the negative electrode consumes a large amount of lithium from the positive electrode, sacrificing the capacity of the lithium-ion battery, which to a large extent restricts its widespread application in electric vehicles, smart phones and other fields.

[0003] In order to solve the problem of large lithium ion consumption in the SEI film formation process, the main technologies used are positive electrode lithium replenishment and negative electrode lithium replenishment. However, negative electrode lithium replenishment is difficult and requires a large investment, so positive electrode lithium replenishment is a common method. However, the positive electrode lithium replenishment method is still insufficient in controlling lithium ion conduction. Therefore, it is necessary to improve the positive electrode lithium replenishment method so that the battery has both high capacity retention and low impedance. Summary of the invention

[0004] The purpose of the present invention is to overcome the problem that the positive electrode lithium replenishment method in the prior art is insufficient in controlling the lithium ion conduction, and provide a positive electrode sheet and a battery including the positive electrode sheet. The positive electrode sheet of the present invention improves the problem of poor controllability of the lithium ion conduction of the positive electrode lithium replenishment method by regulating the particle size relationship between the lithium replenisher (i.e., lithium nickelate) and the positive electrode active material. The battery including the positive electrode sheet of the present invention can take into account both high capacity retention and low impedance, and has a better cycle life and charge and discharge efficiency.

[0005] A first aspect of the present invention provides a positive electrode sheet, which includes lithium nickelate and a positive electrode active material; the ratio of the particle size of the lithium nickelate to the particle size of the positive electrode active material is (0.1-40):1.

[0006] A second aspect of the present invention provides a battery, comprising the positive electrode sheet described in the first aspect of the present invention.

[0007] Through the above technical solution, the present invention has at least the following advantages compared with the prior art:

[0008] (1) The positive electrode sheet of the present invention can promote the conduction of lithium ions, reduce the internal resistance of the battery, and improve the charge and discharge efficiency of the battery by regulating the relationship between the particle size of the lithium supplement agent and the positive electrode active material;

[0009] (2) The battery including the positive electrode sheet of the present invention can achieve both high capacity retention and low impedance, and has a better cycle life and charge and discharge efficiency.

[0010] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. DETAILED DESCRIPTION

[0011] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0012] The positive electrode lithium replenishment method in the related art often has the problem of insufficient control over lithium ion conduction. After a lot of research, the inventors of the present invention found that the reasons for the above problems are: First, the conventional lithium replenisher (such as lithium nickelate) itself has a large impedance, resulting in a large resistance to lithium ion transmission. Second, when the lithium replenisher (such as lithium nickelate) is added to the positive electrode sheet, after the battery is charged and discharged, the lithium ions in the lithium replenisher are released, and their particle size does not match the particle size of the positive electrode active material in the positive electrode sheet, which also increases the transmission resistance of lithium ions. Based on the above findings, the inventors of the present invention proposed the following scheme:

[0013] A first aspect of the present invention provides a positive electrode sheet, which may include lithium nickelate and a positive electrode active material. The ratio of the particle size of the lithium nickelate to the particle size of the positive electrode active material may be (0.1-40):1, for example, 0.1:1, 0.5:1, 1:1, 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1 or 40:1.

[0014] In one example, the ratio of the particle size of the lithium nickelate to the particle size of the positive electrode active material is (0.6-25):1.

[0015] In one example, the ratio of the particle size of the lithium nickelate to the particle size of the positive electrode active material is (1-4):1.

[0016] The inventor of the present invention has found that by controlling the particle size ratio of lithium nickelate to the positive electrode active material, the lithium nickelate, the positive electrode active material and the positive electrode conductive agent can be connected more closely after the lithium ions are released, thereby improving the transmission efficiency of lithium ions during the battery charge and discharge cycle. When the ratio of the particle size of lithium nickelate to the positive electrode active material is too low (for example, less than 0.1:1), the particle size of lithium nickelate is too small relative to the particle size of the positive electrode active material, and the two do not match, resulting in too slow kinetics of the positive electrode active material, resulting in too low reversible capacity and too high impedance, affecting the cycle performance and low-temperature cold start capability; and when the ratio of the particle size of lithium nickelate to the positive electrode active material is too high (for example, greater than 40:1), the particle size of lithium nickelate is too large relative to the particle size of the positive electrode active material, and also does not match. The oversized lithium nickelate particles are easy to form a steric hindrance effect on the diffusion of lithium ions, making the lithium ion diffusion path longer, increasing concentration polarization, and weakening the cold start performance.

[0017] In the present invention, the particle size of the lithium nickelate can be 0.8μm-16μm, for example, 0.8μm, 0.9μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm or 16μm.

[0018] In one example, the particle size of the lithium nickelate is 1 μm-10 μm.

[0019] Under the premise that the particle size ratio of lithium nickel acid to positive electrode active material is within a specific range, the battery's charge and discharge efficiency can be further improved by adjusting the particle size of lithium nickel acid. When the particle size of lithium nickel acid is too small (for example, less than 0.8 μm), the specific capacity is smaller, which will reduce the energy density of the battery; when the particle size of lithium nickel acid is too large (for example, greater than 16 μm), the lithium ions released from the lithium nickel acid will have too long a transmission path, thereby reducing the cold start performance.

[0020] In the present invention, the particle size of the positive electrode active material can be 0.2μm-8μm, for example, 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm or 8μm.

[0021] In one example, the particle size of the positive electrode active material is 0.25 μm-6 μm.

[0022] Under the premise that the particle size ratio of lithium nickelate to positive electrode active material is within a specific range, the battery charge and discharge efficiency can be further improved by adjusting the particle size of the positive electrode active material. When the particle size of the positive electrode active material is too small (for example, less than 0.2 μm), the smaller particles are prone to agglomeration, affecting the transmission of lithium ions, increasing the internal resistance, and weakening the battery cycle capacity; when the particle size of the positive electrode active material is too large (for example, greater than 8 μm), the migration path of lithium ions will be increased, reducing the cold start performance.

[0023] In the present invention, the particle size of the lithium nickel oxide and the particle size of the positive electrode active material can be tested by conventional methods in the art, such as using a scanning electron microscope (SEM), disassembling the battery, taking out the positive electrode sheet, randomly selecting a field of view, measuring the particle sizes of at least 50 lithium nickel oxide particles and at least 50 positive electrode active material particles within the field of view, and taking the average value.

[0024] In the present invention, the positive electrode sheet may include a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector. The positive electrode active material layer may include the lithium nickelate and the positive electrode active material. The lithium nickelate includes elemental nickel, and the positive electrode active material includes elemental titanium. In the positive electrode active material layer, the ratio of the mass content of elemental nickel to the mass content of elemental titanium may be (0.05-70):1, for example, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 20:1, 30:1, 40:1, 50:1, 60:1 or 70:1.

[0025] In one example, in the positive electrode active material layer, the ratio of the mass content of the element nickel to the mass content of the element titanium is (0.07-20):1.

[0026] In one example, in the positive electrode active material layer, the ratio of the mass content of the element nickel to the mass content of the element titanium is (0.5-11):1.

[0027] The positive electrode lithium supplementation technology used in the related art will also cause the battery to produce serious gas during the cycle. The inventors of the present invention found that the reason for the serious gas production of the battery is: first, the structural stability of lithium nickel acid itself is poor, and it is easy to react with the electrolyte, resulting in gas production; in addition, after the lithium in lithium nickel acid is released, the structural stability is further deteriorated, and the oxygen in the lattice is oxidized and lost in the form of oxygen, thereby exacerbating the occurrence of gas production. Based on the above findings, the inventors of the present invention have conducted a large number of targeted studies and further found that by setting titanium elements in the positive electrode active material and controlling the content of nickel elements in lithium nickel acid in the positive electrode active material layer and the content of titanium elements in the positive electrode active material layer, the battery can take into account both high capacity retention and low impedance, while improving the gas production of the battery, and further improving the cycle life and capacity of the battery. This is because, during the battery charging process, the lithium in lithium nickel acid will be released. At this time, the divalent nickel ions in lithium nickel acid will be converted into smaller trivalent nickel ions and occupy the lithium site, thereby causing local structural collapse. If titanium is set in the positive electrode active material, the titanium in the positive electrode active material will preferentially move to the lithium position in the lithium nickel oxide to maintain the structure of the lithium nickel oxide and avoid the collapse of the lithium nickel oxide structure. When titanium occupies the lithium position, it can not only improve the structural stability of the lithium nickel oxide and reduce the risk of side reactions with the electrolyte; it can also stabilize the oxygen in the lattice and stabilize it inside the lattice, thereby effectively inhibiting the occurrence of gas production. And after the element titanium occupies the lithium position, it will maintain the patency of the lithium replenishment channel, ensure the continuous lithium replenishment ability of the lithium nickel oxide, and avoid the problem of poor lithium replenishment effect caused by the blockage of the lithium replenishment channel. When the ratio of the mass content of elemental nickel to the mass content of elemental titanium in the positive electrode active material layer is too small (for example, less than 0.05:1), the elemental titanium is excessive relative to the elemental nickel. At this time, in addition to occupying the lithium site, the inactive titanium ions will also compete with the nickel ions and further occupy the active nickel ion sites, thereby affecting the stability of the lithium nickelate structure; and when the ratio of the mass content of elemental nickel to the mass content of elemental titanium in the positive electrode active material layer is too large (for example, greater than 70:1), the elemental nickel is excessive relative to the elemental titanium, and the nickel ions migrate to the lithium site in large quantities, causing the transition metal to break away from the constraints of the oxygen atoms. The formed oxygen vacancies cause structural collapse, which seriously deteriorates the cycle performance of the battery.

[0028] In the present invention, the mass content of element nickel in the positive electrode active material layer can be 400ppm-60000ppm, for example, 400ppm, 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 2000ppm, 3000ppm, 4000ppm, 5000ppm, 6000ppm, 7000ppm, 8000ppm, 9000ppm, 10000ppm, 20000ppm, 30000ppm, 40000ppm, 50000ppm or 60000ppm.

[0029] In one example, the mass content of element nickel in the positive electrode active material layer is 4000ppm-30000ppm.

[0030] The inventors of the present invention have found that, under the premise that the ratio of the mass content of elemental nickel to the mass content of elemental titanium in the positive electrode active material layer is within a specific range, the self-discharge of the battery can be improved by controlling the mass content of elemental nickel in the positive electrode active material layer. When the mass content of elemental nickel in the positive electrode active material layer is too high (for example, greater than 60,000 ppm), nickel easily migrates and diffuses from the interlayer to the negative electrode, and accumulates at the negative electrode, causing serious self-discharge.

[0031] In the present invention, the mass content of element titanium in the positive electrode active material layer can be 500ppm-10000ppm, for example, 500ppm, 1000ppm, 2000ppm, 3000ppm, 4000ppm, 5000ppm, 6000ppm, 7000ppm, 8000ppm, 9000ppm or 10000ppm.

[0032] In one example, the mass content of element titanium in the positive electrode active material layer is 2500 ppm-7500 ppm.

[0033] In the present invention, the mass content of element nickel in the positive electrode active material layer and the mass content of element titanium in the positive electrode active material layer can be measured by conventional methods in the art, such as by inductively coupled plasma (ICP) or energy dispersive spectrometer (EDS).

[0034] In the present invention, the mass content of elemental nickel in the lithium nickelate may be 100000 ppm-600000 ppm, for example, 100000 ppm, 200000 ppm, 300000 ppm, 400000 ppm, 500000 ppm or 600000 ppm.

[0035] In one example, the mass content of element nickel in the lithium nickelate is 500,000 ppm-600,000 ppm.

[0036] In the present invention, the mass content of elemental titanium in the positive electrode active material may be 2000ppm-10000ppm, for example, 2000ppm, 3000ppm, 4000ppm, 5000ppm, 6000ppm, 7000ppm, 8000ppm, 9000ppm or 10000ppm.

[0037] In one example, the mass content of element titanium in the positive electrode active material is 3000ppm-8000ppm.

[0038] In the present invention, the mass content of the element nickel in the lithium nickelate and the mass content of the element titanium in the positive electrode active material can be measured by conventional methods in the art, such as ICP.

[0039] In the present invention, the mass ratio of the lithium nickelate to the positive electrode active material can be 1:(9-199), for example, 1:9, 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, 1:110, 1:120, 1:130, 1:140, 1:150, 1:160, 1:170, 1:180, 1:190 or 1:199.

[0040] In one example, the mass ratio of the lithium nickelate to the positive electrode active material is 1:(19-99).

[0041] In the present invention, the porosity of the positive electrode sheet may be 30%-60%, for example, 30%, 35%, 40%, 45%, 50%, 55% or 60%.

[0042] In one example, the porosity of the positive electrode sheet is 35%-50%.

[0043] The inventors of the present invention have found that by regulating the porosity range of the positive electrode sheet, it helps to maintain the stability of the positive electrode active material and reduce the precipitation of active oxygen, so as to further inhibit the gas production of the battery and improve safety and reliability. And the appropriate porosity also helps to increase the energy density of the battery. When the porosity of the positive electrode sheet is too low (for example, less than 30%), the electrolyte does not sufficiently infiltrate the positive electrode sheet, resulting in poor kinetic performance of the positive electrode sheet, affecting the cycle, and even causing lithium precipitation; and when the porosity of the positive electrode sheet is too high (for example, greater than 60%), the conductive network of the positive electrode sheet deteriorates, resulting in an increase in the internal resistance of the battery and weakening the cycle performance.

[0044] In the present invention, the porosity of the positive electrode sheet can be tested by conventional methods in the art, such as disassembling the battery in a dry environment, separating the positive electrode sheet, soaking the positive electrode sheet with dimethyl carbonate for at least 3 times, each soaking time is not less than 30 minutes, and then placing it in a blast oven for drying; measuring the length, width and thickness of the positive electrode sheet; weighing the mass of the positive electrode sheet with an analytical balance, winding it and placing it in a sample cup for true density testing, and calculating the porosity.

[0045] In the present invention, the positive electrode active material may include at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate and lithium-rich manganese-based materials.

[0046] In one example, the positive electrode active material includes lithium iron phosphate.

[0047] In the present invention, the positive electrode active material layer may further include at least one of a positive electrode conductive agent and a positive electrode binder. The positive electrode conductive agent may include a conductive agent conventionally used in the art, for example, including at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, carbon nanotubes (including at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes) and carbon fibers. The positive electrode binder may include at least one of polyvinylidene fluoride, sodium carboxymethyl cellulose, styrene-butadiene rubber, polytetrafluoroethylene and polyethylene oxide.

[0048] In the present invention, based on the total mass of the positive electrode active material layer, the content of the positive electrode active material can be 80%-99.8% (for example, 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, 98%, 99% or 99.8%), the content of the positive electrode conductor can be 0.1%-10% (for example, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5% or 0.1%), and the content of the positive electrode binder can be 0.1%-10% (for example, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5% or 0.1%).

[0049] A second aspect of the present invention provides a battery, comprising the positive electrode sheet described in the first aspect of the present invention.

[0050] <Negative electrode>

[0051] In the present invention, the battery may further include a negative electrode sheet. The negative electrode sheet may include a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector. After the battery has been charged and discharged for 200 times, the mass content of elemental nickel in the negative electrode active material layer is less than or equal to 8000ppm, for example, 8000ppm, 7000ppm, 6000ppm, 5000ppm, 4000ppm, 3000ppm, 2000ppm, 1000ppm, 900ppm, 800ppm, 700ppm, 600ppm, 500ppm, 400ppm, 300ppm, 200ppm or 100ppm.

[0052] In one example, after the battery has been charged and discharged for 200 times, the mass content of element nickel in the negative electrode active material layer is less than or equal to 3000 ppm.

[0053] In one example, after the battery has been charged and discharged for 200 times, the mass content of element nickel in the negative electrode active material layer is less than or equal to 550 ppm.

[0054] When the battery is charged, lithium nickel oxide delithium, and during the process of nickel ions migrating between layers, it is very easy to migrate to the negative electrode and deposit at the negative electrode to form lithium dendrites, which seriously affects the safety and stability of the battery. The less nickel content in the negative electrode active material layer, the more nickel ions migrate in the lithium nickel oxide layer, which can bind oxygen in the lattice, and in the discharge process, the bound oxygen is reduced, maintaining the layered structure of lithium nickel oxide and reducing the risk of gas production. When the battery has undergone 200 charge and discharge cycles, when the mass content of elemental nickel in the negative electrode active material layer is too high (for example, higher than 8000ppm), the dissolved nickel element leads to a decrease in the battery capacity, which seriously affects the battery energy density and cycle capacity. In addition, the reduction of nickel ions to nickel elemental substances will also cause the battery diaphragm to be punctured, causing serious self-discharge and short circuit risks.

[0055] In the present invention, the mass content of element nickel in the negative electrode active material layer can be measured by conventional methods in the art, such as ICP or EDS.

[0056] In the present invention, the negative electrode active material layer may include a negative electrode active material, a negative electrode conductive agent, and a negative electrode binder. The negative electrode active material may include at least one of a silicon-based material and a carbon-based material. The silicon-based material may include at least one of nano-silicon, a silicon alloy, silicon oxide (SiOx, 0 < x < 2), and silicon carbide. The silicon oxide refers to a material including elemental silicon and elemental oxygen. The silicon carbide refers to a material including elemental silicon and elemental carbon. The carbon-based material may include at least one of artificial graphite, natural graphite, mesocarbon microbeads, soft carbon, and hard carbon. The negative electrode conductive agent may include at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, carbon nanotubes (including at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes), and carbon fibers. The negative electrode binder may include at least one of polyvinylidene fluoride, sodium carboxymethyl cellulose, styrene-butadiene rubber, polytetrafluoroethylene, and polyethylene oxide.

[0057] In the present invention, based on the total mass of the negative electrode active material layer, the content of the negative electrode active material may be 80% - 99.8% (for example, 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, 98%, 99%, or 99.8%), the content of the negative electrode conductive agent may be 0.1% - 10% (for example, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, or 0.1%), and the content of the negative electrode binder may be 0.1% - 10% (for example, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, or 0.1%).

[0058] <Separator>

[0059] In the present invention, the battery may further include a separator. The porosity of the separator is k, and the particle size of the lithium nickelate is d. k and d may satisfy 0.01 ≤ k / d ≤ 0.6, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.2, 0.3, 0.4, 0.5, or 0.6.

[0060] In one example, 0.05 ≤ k / d ≤ 0.4.

[0061] By regulating the relationship between the porosity of the diaphragm and the particle size of lithium nickelate, the conduction of lithium ions can be promoted. When the ratio of the porosity k of the diaphragm to the particle size d of lithium nickelate is too small (for example, less than 0.01), the porosity of the diaphragm is smaller than the particle size of lithium nickelate, resulting in blockage of the ion transmission channel, which will increase the resistance of ion transmission, thereby causing the internal resistance of the battery and weakening the low-temperature cold start performance; and when the ratio of the porosity k of the diaphragm to the particle size d of lithium nickelate is too large (for example, greater than 0.6), the porosity of the diaphragm is larger than the particle size of lithium nickelate, which not only easily causes the lithium ions inside the battery to continuously migrate between the positive and negative electrodes, resulting in serious self-discharge; it also causes the accumulation of nickel in the negative electrode to increase, further worsening the self-discharge.

[0062] In the present invention, k may be 25%-70%, for example, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65% or 70%.

[0063] In one example, k is 35%-55%.

[0064] In the present invention, the porosity k of the diaphragm can be tested by conventional methods in the art, such as disassembling the battery in a dry environment, separating the diaphragm, soaking the diaphragm in dimethyl carbonate for at least 3 times, each soaking time is not less than 30 minutes, and then placing it in a blast oven for drying; measuring the length, width and thickness of the diaphragm; weighing the mass of the diaphragm with an analytical balance, winding it and placing it in a sample cup for true density testing, and calculating the porosity.

[0065] In the present invention, the separator may include a substrate layer. The substrate layer may include at least one of polyethylene, polypropylene, aramid and polyamide.

[0066] In one example, the substrate layer includes polyethylene and polypropylene.

[0067] The inventors of the present invention have found that a specific substrate layer is beneficial to the conduction effect of ions, thereby improving the charge and discharge efficiency of the battery.

[0068] In addition to the substrate layer, the diaphragm in the related art generally has a glue layer and / or a ceramic layer. The glue layer can easily block the transmission channel of lithium ions, which reduces the ion conductivity of the diaphragm and leads to a weakening of the battery cycle performance; and the ceramic layer also has the problem of self-discharge due to the shedding of ceramic particles. Furthermore, in order to ensure the conduction of lithium ions while reducing the accumulation of nickel at the negative electrode and reducing the occurrence of battery self-discharge, the diaphragm of the present invention may not be provided with a glue layer and / or a ceramic layer on the surface of the substrate layer.

[0069] In one example, the diaphragm does not include a glue layer and / or a ceramic layer.

[0070] In the present invention, the thickness of the diaphragm may be 7 μm-20 μm, for example, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm.

[0071] In one example, the thickness of the separator is 9 μm-16 μm.

[0072] By controlling the thickness of the diaphragm, the energy density and safety of the battery can be balanced. When the thickness of the diaphragm is too thick (for example, greater than 20 μm), it will affect the energy density of the battery; and when the thickness of the diaphragm is too thin (for example, less than 7 μm), it is easy to cause internal short circuits in the battery.

[0073] In the present invention, the battery may further include an electrolyte and / or an electrolyte, and the electrolyte may include an electrolyte conventionally used in the art. The electrolyte may include an electrolyte conventionally used in the art.

[0074] In the present invention, the battery may be a wound battery or a laminated battery.

[0075] In one example, the battery is a lithium-ion battery.

[0076] The present invention will be described in detail below by way of examples. The examples described in the present invention are only a part of the examples of the present invention, rather than all of the examples. Based on the examples in the present invention, all other examples obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0077] In the following examples, unless otherwise specified, all materials used were commercially available of analytical grade.

[0078] Example

[0079] The following examples are provided to illustrate the batteries of the present invention.

[0080] Example 1

[0081] Prepare the battery as follows:

[0082] (1) Preparation of positive electrode sheet

[0083] The positive electrode active material lithium iron phosphate (particle size of 4 μm, mass content of elemental titanium of 3000 ppm), lithium nickelate (particle size of 5 μm, mass content of elemental nickel of 600000 ppm), polyvinylidene fluoride and conductive carbon black are mixed in a mass ratio of 88.825:4.675:3.5:3 to form a uniform and stable mixture, and N-methylpyrrolidone (NMP) is added to prepare a positive electrode active material slurry (solid content of 60 wt%), and the above positive electrode active material slurry is evenly coated on both sides of aluminum foil, and after drying and roller pressing, a positive electrode sheet is obtained, wherein the particle size ratio of lithium nickelate to lithium iron phosphate is 1.25:1; in the positive electrode active material layer, the mass content of elemental nickel is 28049 ppm, the mass content of elemental titanium is 2661 ppm, and the mass content ratio of elemental nickel to elemental titanium is 10.5:1; the porosity of the positive electrode sheet is 45%.

[0084] (2) Preparation of negative electrode sheet

[0085] Artificial graphite, styrene-butadiene rubber and conductive carbon black are mixed in a mass ratio of 95:3:2 to form a uniform and stable mixture, deionized water is added to prepare a negative electrode active material slurry (solid content is 46wt%), the negative electrode active material slurry is evenly coated on both sides of a copper foil, and after drying and roller pressing, a negative electrode sheet is obtained.

[0086] (3) Preparation of electrolyte

[0087] In a glove box filled with argon (H2O < 0.1 ppm, O2 < 0.1 ppm), ethylene carbonate, dimethyl carbonate and 1,2-propylene carbonate were mixed in a volume ratio of 1:1:1, 1 M lithium hexafluorophosphate was added, stirred evenly, and the electrolyte was obtained after passing the moisture and free acid tests.

[0088] (4) Preparation of batteries

[0089] The positive electrode sheet prepared in step (1), the separator (thickness 12 μm, the substrate layer is a polyethylene and polypropylene composite film, without a glue layer and a ceramic layer, and the porosity k is 45%) and the negative electrode sheet prepared in step (2) are wound to form a bare battery cell, and the aluminum pole ear and the copper-plated nickel pole ear are welded after hot pressing; after liquid injection, the battery is formed, sealed, sorted, and OCV tested to obtain a battery, wherein k / d is 0.09.

[0090] Example 2

[0091] The method is carried out with reference to Example 1, except that step (1) and step (4) are specifically as follows:

[0092] (1) Preparation of positive electrode sheet

[0093] The positive electrode active material lithium iron phosphate (particle size of 0.25 μm, mass content of elemental titanium of 8000 ppm), lithium nickelate (particle size of 1 μm, mass content of elemental nickel of 500000 ppm), polyvinylidene fluoride and conductive carbon black are mixed in a mass ratio of 92.565:0.935:3.5:3 to form a uniform and stable mixture, and N-methylpyrrolidone (NMP) is added to prepare a positive electrode active material slurry (solid content of 60 wt%), and the above positive electrode active material slurry is evenly coated on both sides of aluminum foil, and after drying and roller pressing, a positive electrode sheet is obtained, wherein the particle size ratio of lithium nickelate to lithium iron phosphate is 4:1; in the positive electrode active material layer, the mass content of elemental nickel is 4672 ppm, the mass content of elemental titanium is 7401 ppm, and the mass content ratio of elemental nickel to elemental titanium is 0.63:1; the porosity of the positive electrode sheet is 45%.

[0094] (4) Preparation of batteries

[0095] The positive electrode sheet prepared in step (1), the separator (thickness 16 μm, the substrate layer is a polyethylene and polypropylene composite film, without a glue layer and a ceramic layer, and the porosity k is 35%) and the negative electrode sheet prepared in step (2) are wound to form a bare battery cell, and the aluminum pole ear and the copper-plated nickel pole ear are welded after hot pressing; after liquid injection, the battery is formed, sealed, sorted, and OCV tested to obtain a battery, wherein k / d is 0.35.

[0096] Example 3

[0097] The method is carried out with reference to Example 1, except that step (1) and step (4) are specifically as follows:

[0098] (1) Preparation of positive electrode sheet

[0099] The positive electrode active material lithium iron phosphate (particle size of 6 μm, mass content of elemental titanium of 5000 ppm), lithium nickelate (particle size of 10 μm, mass content of elemental nickel of 550000 ppm), polyvinylidene fluoride and conductive carbon black are mixed in a mass ratio of 91.667:1.833:3.5:3 to form a uniform and stable mixture, and N-methylpyrrolidone (NMP) is added to prepare a positive electrode active material slurry (solid content of 60 wt%), and the above positive electrode active material slurry is evenly coated on both sides of aluminum foil, and after drying and roller pressing, a positive electrode sheet is obtained, wherein the particle size ratio of lithium nickelate to lithium iron phosphate is 1.7:1; in the positive electrode active material layer, the mass content of elemental nickel is 10083 ppm, the mass content of elemental titanium is 4579 ppm, and the mass content ratio of elemental nickel to elemental titanium is 2.2:1; the porosity of the positive electrode sheet is 45%.

[0100] (4) Preparation of batteries

[0101] The positive electrode sheet prepared in step (1), the separator (thickness 9 μm, the substrate layer is a polyethylene and polypropylene composite film, without a glue layer and a ceramic layer, and the porosity k is 55%) and the negative electrode sheet prepared in step (2) are wound to form a bare battery cell, and the aluminum pole ear and the copper-plated nickel pole ear are welded after hot pressing; after liquid injection, the battery is formed, sealed, sorted, and OCV tested to obtain a battery, wherein k / d is 0.055.

[0102] Example 4 Group

[0103] This group of examples is used to verify the impact of changes in the "ratio of the particle size of lithium nickel oxide to the particle size of lithium iron phosphate".

[0104] This group of examples is carried out with reference to Example 1, except that the particle size of lithium iron phosphate and the particle size of lithium nickelate are changed, as follows:

[0105] Example 4a, the particle size of lithium iron phosphate is 6 μm, the particle size of lithium nickelate is 1 μm, the particle size ratio of lithium nickelate to lithium iron phosphate is 0.17:1, and k / d is 0.45;

[0106] In Example 4b, the particle size of lithium iron phosphate is 0.25 μm, the particle size of lithium nickelate is 10 μm, the particle size ratio of lithium nickelate to lithium iron phosphate is 40:1, and k / d is 0.045.

[0107] Example 5 Group

[0108] This group of examples is used to verify the impact of changes in the "particle size d of lithium nickelate".

[0109] This group of examples is carried out with reference to Example 1, except that the particle size d of lithium nickelate is changed, as follows:

[0110] Example 5a, the particle size of lithium nickelate is 0.8 μm, the particle size ratio of lithium nickelate to lithium iron phosphate is 0.2:1, and k / d is 0.56;

[0111] In Example 5b, the particle size of lithium nickelate is 16 μm, the particle size ratio of lithium nickelate to lithium iron phosphate is 4:1, and k / d is 0.03.

[0112] Example 6 Group

[0113] This group of examples is used to verify the influence of the change of "particle size of positive electrode active material".

[0114] This group of examples is carried out with reference to Example 1, except that the particle size of lithium iron phosphate is changed, as follows:

[0115] In Example 6a, the particle size of lithium iron phosphate is 0.2 μm, and the particle size ratio of lithium nickelate to lithium iron phosphate is 25:1;

[0116] In Example 6b, the particle size of lithium iron phosphate is 8 μm, and the particle size ratio of lithium nickelate to lithium iron phosphate is 0.625:1.

[0117] Example 7 Group

[0118] This group of examples is used to verify the influence of the change of "the ratio of the mass content of the element nickel to the mass content of the element titanium in the positive electrode active material layer".

[0119] This group of examples is carried out with reference to Example 1, except that the mass content of element titanium in lithium iron phosphate and / or the mass content of element nickel in lithium nickelate and / or the mass ratio of lithium iron phosphate and lithium nickelate in the positive electrode active material slurry are changed, specifically as follows:

[0120] In Example 7a, a positive electrode active material, lithium iron phosphate (particle size of 4 μm, mass content of elemental titanium of 1000 ppm), lithium nickelate (particle size of 5 μm, mass content of elemental nickel of 600000 ppm), polyvinylidene fluoride and conductive carbon black are mixed in a mass ratio of 92.565:0.935:3.5:3 to form a uniform and stable mixture, wherein in the positive electrode active material layer, the mass content of elemental nickel is 56105 ppm, the mass content of elemental titanium is 843 ppm, and the mass content ratio of elemental nickel to elemental titanium is 66.6:1;

[0121] In Example 7b, a positive electrode active material, lithium iron phosphate (with a particle size of 4 μm and a mass content of elemental titanium of 2000 ppm), lithium nickelate (with a particle size of 5 μm and a mass content of elemental nickel of 600000 ppm), polyvinylidene fluoride and conductive carbon black are mixed in a mass ratio of 87.657:5.843:3.5:3 to form a uniform and stable mixture, wherein in the positive electrode active material layer, the mass content of elemental nickel is 35062 ppm, the mass content of elemental titanium is 1751 ppm, and the mass content ratio of elemental nickel to elemental titanium is 20:1;

[0122] In Example 7c, the positive electrode active material lithium iron phosphate (particle size of 4 μm, mass content of elemental titanium of 9000 ppm), lithium nickelate (particle size of 5 μm, mass content of elemental nickel of 100000 ppm), polyvinylidene fluoride and conductive carbon black are mixed in a mass ratio of 92.786:0.714:3.5:3 to form a uniform and stable mixture, wherein the mass content of elemental nickel in the positive electrode active material layer is 713 ppm, the mass content of elemental titanium is 8350 ppm, and the mass content ratio of elemental nickel to elemental titanium is 0.085:1;

[0123] Example 7d, the positive electrode active material lithium iron phosphate (particle size is 4 μm, the mass content of elemental titanium is 10000 ppm), lithium nickelate (particle size is 5 μm, the mass content of elemental nickel is 100000 ppm), polyvinylidene fluoride and conductive carbon black are mixed in a mass ratio of 93.032:0.468:3.5:3 to form a uniform and stable mixture, wherein the mass content of elemental nickel in the positive electrode active material layer is 472 ppm, the mass content of elemental titanium is 9311 ppm, and the ratio of the mass content of elemental nickel to elemental titanium is 0.051:1.

[0124] Example 8 Group

[0125] This group of embodiments is used to verify the impact of changes in the "porosity of the positive electrode sheet".

[0126] This group of examples is carried out with reference to Example 1, except that the porosity of the positive electrode sheet is changed by adjusting the compaction density of the positive electrode sheet, as follows:

[0127] In Example 8a, the porosity of the positive electrode sheet is 30%;

[0128] In Example 8b, the porosity of the positive electrode sheet is 35%;

[0129] In Example 8c, the porosity of the positive electrode sheet is 50%;

[0130] In Example 8d, the porosity of the positive electrode sheet is 60%.

[0131] Example 9

[0132] This example is used to verify the influence of the change of the “positive electrode active material”.

[0133] The same method is carried out as in Example 1, except that the positive electrode active material is replaced with lithium manganese iron phosphate of the same mass.

[0134] Example 10 Group

[0135] This group of embodiments is used to verify the impact of the change of "k / d".

[0136] This group of examples is carried out with reference to Example 1, except that k / d is changed by adjusting the particle size d of lithium nickelate and the porosity k of the diaphragm, as follows:

[0137] Example 10a, d is 1, the unit is μm, k is 55%, k / d is 0.55, and the particle size ratio of lithium nickelate to lithium iron phosphate is 0.25:1;

[0138] In Example 10b, d is 10, the unit is μm, k is 35%, k / d is 0.035, and the particle size ratio of lithium nickelate to lithium iron phosphate is 2.5:1.

[0139] Example 11 Group

[0140] This group of embodiments is used to verify the influence of the change of the "porosity k of the diaphragm".

[0141] This group of examples is carried out with reference to Example 1, except that the porosity k of the diaphragm is changed, as follows:

[0142] Example 11a, k is 25%, k / d is 0.05;

[0143] In Example 11b, k is 70% and k / d is 0.14.

[0144] Example 12 Group

[0145] This group of examples is used to verify the impact of changes in the "diaphragm substrate layer".

[0146] This group of examples is carried out with reference to Example 1, except that the substrate layer of the diaphragm is changed, as follows:

[0147] In embodiment 12a, the substrate layer is polyethylene;

[0148] In Example 12b, the substrate layer is polypropylene.

[0149] Example 13 Group

[0150] This group of embodiments is used to verify the influence of the "glue layer and / or ceramic layer in the diaphragm".

[0151] This group of examples is carried out with reference to Example 1, except that the diaphragm is changed, as follows:

[0152] In Example 13a, the thickness of the separator is 12 μm, the substrate layer is a composite film of polyethylene and polypropylene, both sides of the substrate layer include adhesive layers, and the porosity k is 45%;

[0153] Example 13b, the thickness of the diaphragm is 12 μm, the substrate layer is a composite film of polyethylene and polypropylene, both sides of the substrate layer include ceramic layers, and the porosity k is 45%;

[0154] In Example 13c, the thickness of the diaphragm is 12 μm, the substrate layer is a composite film of polyethylene and polypropylene, one side of the substrate layer is a ceramic layer, the other side of the substrate layer and the outer surface of the ceramic layer are adhesive layers, and the porosity k is 45%.

[0155] Example 14 Group

[0156] This group of embodiments is used to verify the influence of the change of "thickness of the diaphragm".

[0157] This group of examples is carried out with reference to Example 1, except that the thickness of the diaphragm is changed, as follows:

[0158] Example 14a, the thickness of the separator is 7 μm;

[0159] In Example 14b, the thickness of the separator is 20 μm.

[0160] Comparative Example 1

[0161] The method is carried out with reference to Example 1, except that the particle sizes of lithium iron phosphate and lithium nickelate are changed, specifically as follows: the particle size of lithium iron phosphate is 6 μm, the particle size of lithium nickelate is 0.5 μm, and the particle size ratio of lithium nickelate to lithium iron phosphate is 0.08:1.

[0162] Comparative Example 2

[0163] The method is carried out with reference to Example 1, except that the particle sizes of lithium iron phosphate and lithium nickelate are changed, specifically as follows: the particle size of lithium iron phosphate is 0.2 μm, the particle size of lithium nickelate is 10 μm, and the particle size ratio of lithium nickelate to lithium iron phosphate is 50:1.

[0164] Comparative Example 3

[0165] The method is carried out in accordance with Example 1, except that the positive electrode sheet does not contain lithium nickelate, a lithium supplement. Specifically, the positive electrode active material lithium iron phosphate (particle size is 4 μm, the mass content of elemental titanium is 3000 ppm), polyvinylidene fluoride and conductive carbon black are mixed in a mass ratio of 93.5:3.5:3 to form a uniform and stable mixture, NMP is added to prepare a positive electrode active material slurry (solid content is 60 wt%), and the above positive electrode active material slurry is evenly coated on both sides of the aluminum foil, and after drying and roller pressing, a positive electrode sheet is obtained.

[0166] Test Case

[0167] (1) Energy density test

[0168] The batteries prepared in the embodiments and comparative examples were subjected to an energy density test. The specific test method is as follows: the mass of the battery after the second sealing process is recorded as the battery mass. In the sorting process, the battery is fully charged to 3.65V at a 1C standard constant current and constant voltage, with a cut-off current of 0.05C. After standing for 5 minutes, the energy discharged to 2.2V at a 1C standard constant current is recorded as the discharge energy. The ratio of the discharge energy to the mass of the battery cell is the energy density, in Wh / kg. The results are recorded in Table 1.

[0169] (2) Cold start test

[0170] The batteries prepared in the embodiments and comparative examples were subjected to a cold start test, and the specific test method is as follows: at (25±2)℃, discharge to 2.2V with 1C standard constant current and stand for 30min; then charge to 3.65V with 1C standard constant current and constant voltage, with a cutoff current of 0.05C, and stand for 30min; discharge to 2.2V with 1C standard constant current and constant voltage, and obtain the actual capacity C0 of the battery; stand for 30min; charge to 3.65V with 1C standard constant current and constant voltage, with a cutoff current of 0.05C, and discharge with 1C0 for 30min, which is 50% SOC; stand at (25±2)℃ for 2h; put the battery in a -30℃ constant temperature box and keep the constant temperature for 4h; the terminal voltage value of the 6C constant current discharge for 1s is the battery cold start terminal voltage, in V, and the results are recorded in Table 1.

[0171] (3) Cycle test

[0172] The batteries prepared in the embodiments and comparative examples were subjected to cycle tests, and the specific test method is as follows: at 55°C, discharged at a 1C standard constant current to a discharge termination voltage of 2.2V, and left for 30 minutes; then charged at a 1C standard constant current and constant voltage to a charge limit voltage of 3.65V, a cut-off current of 0.05C, and left for 30 minutes; discharged at a 1C standard constant current to a discharge termination voltage of 2.2V, left for 30 minutes, and the battery thickness PPG1 was recorded with a caliper; the above full charge and discharge steps were repeated until the capacity decayed to 80% and the battery thickness PPG2 was recorded with a caliper, and the number of repeated cycles was the number of cycle cycles, which was used to evaluate the cycle performance of the battery after aging, and the thickness expansion rate of the battery was (PPG2-PPG1) / PPG1×100%, and the results were recorded in Table 1.

[0173] (4) Self-discharge test

[0174] The batteries prepared in the embodiments and comparative examples were subjected to a self-discharge test, and the specific test method is as follows: at (25±2)°C, discharge at a 1C standard constant current to a discharge termination voltage of 2.2V, and leave for 30 minutes; then charge at a 1C standard constant current and constant voltage to a charge limit voltage of 3.65V, with a cut-off current of 0.05C, and leave for 30 minutes; discharge at a 1C standard constant current to a discharge termination voltage of 2.2V, record the actual capacity C0 of the battery, and leave for 30 minutes; charge at a 1C0 constant current to 36% SOC, then discharge 3% SOC at 1C0, which is 33% SOC, and leave for 30 minutes; record the initial voltage OCV1, and after storage at room temperature for 7 days, record the terminal voltage OCV2; Battery self-discharge rate = (OCV1-OCV2) / storage time, in mV / h, and the results are recorded in Table 1.

[0175] (5) Test of the mass content of element nickel in the negative electrode active material layer

[0176] The battery prepared in the embodiment was disassembled in a dry environment, and the negative electrode sheet was separated and soaked in dimethyl carbonate for at least 3 times, each soaking time was not less than 30 minutes, and then placed in a blast oven for drying; after scraping off the coating in the negative electrode sheet, the mass content of elemental nickel was obtained by ICP testing, and the results are recorded in Table 1.

[0177] Table 1

[0178]

[0179]

[0180] Note: “ / ” in Table 1 means no data.

[0181] It can be seen from Table 1 that the battery prepared by the positive electrode sheet of the present invention has both high capacity and low impedance, and has better cycle life and charge and discharge efficiency than the comparative example.

[0182] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A positive electrode sheet, characterized in that: The positive electrode sheet includes lithium nickelate and a positive electrode active material; the ratio of the particle size of the lithium nickelate to the particle size of the positive electrode active material is (0.1-40):

1.

2. The positive electrode sheet according to claim 1, wherein: The ratio of the particle size of the lithium nickelate to the particle size of the positive electrode active material is (0.6-25):1; preferably (1-4):1; And / or, the particle size of the lithium nickelate is 0.8 μm-16 μm; preferably 1 μm-10 μm; And / or, the particle size of the positive electrode active material is 0.2 μm-8 μm; preferably 0.25 μm-6 μm.

3. The positive electrode sheet according to claim 1 or 2, wherein: The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector; the positive electrode active material layer includes the lithium nickelate and the positive electrode active material; the lithium nickelate includes elemental nickel, and the positive electrode active material includes elemental titanium; in the positive electrode active material layer, the ratio of the mass content of elemental nickel to the mass content of elemental titanium is (0.05-70):1; preferably (0.5-11):

1.

4. The positive electrode sheet according to claim 3, wherein: The mass content of element nickel in the positive electrode active material layer is 400ppm-60000ppm; preferably 4000ppm-30000ppm; And / or, the mass content of element titanium in the positive electrode active material layer is 500 ppm-10000 ppm; preferably 2500 ppm-7500 ppm.

5. The positive electrode sheet according to claim 1 or 2, wherein: The porosity of the positive electrode sheet is 30%-60%, preferably 35%-50%.

6. A battery, characterized in that: The battery comprises the positive electrode sheet according to any one of claims 1 to 5.

7. The battery according to claim 6, wherein The battery further comprises a negative electrode sheet; the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector; after the battery has been charged and discharged for 200 times, the mass content of elemental nickel in the negative electrode active material layer is less than or equal to 8000 ppm; Preferably, after the battery has been charged and discharged for 200 times, the mass content of element nickel in the negative electrode active material layer is less than or equal to 550 ppm.

8. The battery according to claim 6 or 7, wherein: The battery further comprises a diaphragm; the porosity of the diaphragm is k, the particle size of the lithium nickelate is d, and k and d satisfy 0.01≤k / d≤0.6; preferably, 0.05≤k / d≤0.4; And / or, k is 25%-70%; preferably 35%-55%.

9. The battery according to claim 8, wherein The diaphragm includes a substrate layer; the substrate layer includes at least one of polyethylene, polypropylene, aramid and polyamide; Preferably, the substrate layer comprises polyethylene and polypropylene; Preferably, the diaphragm does not include a glue layer and / or a ceramic layer.

10. The battery according to claim 8, wherein The thickness of the separator is 7 μm-20 μm, preferably 9 μm-16 μm.

Citation Information

Cited By

  • High-energy-density lithium ion battery

    CN119481219A

  • A high energy density lithium ion battery

    CN119481219B

  • Lithium ion battery with high energy density

    CN119812434A

  • A high energy density lithium ion battery

    CN119812434B

  • Positive plate and lithium ion secondary battery

    CN119852326A