Composition, method, and article related to in situ crosslinking of polyamide during addition production

JP2022084025A5Active Publication Date: 2024-11-28XEROX CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021191212
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-25
Filing Date
2021-11-25
Publication Date
2024-11-28
Estimated Expiration
2041-11-25

AI Technical Summary

Technical Problem

Existing polyamide materials used in additive manufacturing often fail to meet the enhanced physical characteristics required for specific applications due to limitations in flow characteristics and crosslinking, leading to issues with density and melt flow speed during the manufacturing process.

Method used

The development of unsaturated polyamide compositions and methods that incorporate a starting agent to promote crosslinking, allowing for improved heat resistance and wear resistance, enabling better melt and flow characteristics during additive manufacturing processes.

Benefits of technology

The unsaturated polyamide compositions enhance the physical properties of manufactured objects by providing higher density and improved melt flow, resulting in objects with enhanced mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a composition and method that allow in-situ cross-linking of polyamide during a consolidation process of addition production.SOLUTION: A particle containing unsaturated polyamide and initiator can be produced. The particles are used in an addition production method that includes depositing the particles on a surface, optionally in combination with other thermoplastic polymer particles, and after deposition, heating at least a portion of the particles to promote their consolidation and cross-linking of the unsaturated polyamide, thereby forming a consolidation containing cross-linked polyamide.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure includes compositions, synthesis methods, and articles relating to polyamides that are crosslinked during additive manufacturing processes. [Background technology]

[0002] Thermoplastic polymers are often used to produce extruded objects such as films, bags, particles, and filaments. An example of a thermoplastic polymer is polyamide. Polyamides, such as nylon, are off-white polymers that can withstand high or low temperatures without compromising their physical properties. Therefore, objects formed from polyamide can be used in demanding applications such as power tools, automotive parts, gears, and electrical appliance components. Additive manufacturing is increasingly being used to produce such objects.

[0003] Generally, additive manufacturing broadly describes the technique of constructing three-dimensional objects by adding layers of material. The addition of layers can be achieved using filaments or powders. In the case of filaments, the filament material is melted, extruded, and deposited in layers to produce the desired object. Such a method may be called fused filament fabrication (FFF). Selective laser sintering (SLS) is another additive manufacturing method in which thin layers of powder (typically fine particles) are applied as layers. Selected areas within these layers are fused together by exposure to laser light (e.g., CO2 laser light) to construct a solid object supported by unused powder. [Overview of the Initiative] [Problems that the invention aims to solve]

[0004] Polyamides are one of the most common polymers used in addition manufacturing due to their flow properties, lower cost compared to other polymers, and desirable sintering window. However, the physical properties required for objects produced by addition manufacturing may exceed those of polyamides.

[0005] This disclosure includes compositions, synthesis methods, and articles relating to polyamides that are crosslinked during additive manufacturing processes. Specifically, the compositions and methods described herein enable in-situ crosslinking of polyamides during the densification process of additive manufacturing.

[0006] This specification discloses compositions comprising particles containing an unsaturated polyamide and an initiator.

[0007] This specification discloses a method comprising depositing the aforementioned composition onto a surface in an optional combination with other thermoplastic polymer particles, and after deposition, heating at least a portion of the particles to promote densification and crosslinking of the unsaturated polyamide, thereby forming a compacted body containing the crosslinked polyamide.

[0008] This specification discloses a method comprising: mixing a mixture containing an unsaturated polyamide, an immiscible dispersion medium for the unsaturated polyamide, and optionally an emulsifying stabilizer at a temperature above the melting or softening temperature of the unsaturated polyamide and at a shear rate high enough to disperse the unsaturated polyamide in the dispersion medium; and cooling the mixture to below the melting or softening temperature of the unsaturated polyamide to form unsaturated polyamide particles containing the unsaturated polyamide and, if present, an emulsifying stabilizer associated on the outer surface of the unsaturated polyamide particles. [Brief explanation of the drawing]

[0009] The following figures are included to illustrate specific aspects of the disclosure and should not be viewed as exclusive. The disclosed subject matter can be substantially modified, altered, combined, and equivalent in form and function as can be conceived by those skilled in the art who are interested in the disclosure.

[0010] [Figure 1] Figure 1 is a flowchart of a non-limiting, exemplary method of the present disclosure. **DETAILED DESCRIPTION**

[0011] The present disclosure includes compositions, synthesis methods, and articles related to polyamides that are crosslinked during an additive manufacturing process. More specifically, the polyamide synthesis described herein uses one or more polyamide monomers having at least one unsaturated aliphatic carbon-carbon bond. The resulting polyamide is referred to herein as an unsaturated polyamide and contains unsaturated aliphatic carbon-carbon bonds.

[0012] The present disclosure also relates to particles comprising unsaturated polyamides and related methods. The particles are referred to herein as unsaturated polyamide particles. The unsaturated polyamide particles may be doped with an initiator. Methods for preparing unsaturated polyamide particles doped with an initiator and methods for using unsaturated polyamide particles doped with an initiator in additive manufacturing are described herein. During additive manufacturing, more specifically during densification, the initiator can cause crosslinking between the unsaturated polyamides. Crosslinking of the polyamides can impart higher heat resistance, improved wear resistance, and other physical properties that can be improved compared to the polyamides when not crosslinked. Thus, the improved properties may be imparted to articles and objects produced by an additive manufacturing method.

[0013] Furthermore, in additive manufacturing methods, due to the low melt flow rate, it can be difficult to operate directly with highly crosslinked polyamides. Thus, particles containing highly crosslinked polyamides may not be effectively consolidated, or filaments containing highly crosslinked polyamides have suitable melting and flow characteristics. Advantageously, the compositions and methods of the present disclosure utilize in-situ crosslinking of unsaturated polyamides. Thus, during an additive manufacturing method, the desirable melting and flow characteristics of the unsaturated polyamide can be utilized to provide good consolidation of the particles, while the temperature and / or laser wavelength encountered in the additive manufacturing method can initiate crosslinking of the unsaturated polyamide by activation of an initiator. This can allow sufficient time for the unsaturated polyamide to melt and / or consolidate in the desired location and for crosslinks to form, such that the resulting article or object is actually formed from the crosslinked polyamide. Thus, the resulting article can have improved physical properties of the crosslinked polyamide. Definitions and Test Methods

[0014] As used herein, the term "immiscibility" refers to a mixture of two or more components that, when combined, form two or more phases having a solubility in each other of less than 5 wt% at ambient pressure at room temperature or, if solid at room temperature, at the melting point of the component. For example, polyethylene oxide having a molecular weight of 10,000 g / mol is solid at room temperature and has a melting point of 65 °C. Thus, if a material that is liquid at room temperature and the polyethylene oxide have a solubility of less than 5 wt% at 65 °C, the polyethylene oxide is immiscible with the material.

[0015] As used herein, the term "thermal initiator" refers to a molecule that produces reactive species (e.g., free radicals, cations, or anions) when exposed to heat. The temperature required to activate a thermal initiator depends on the molecule and can be readily achieved by reference and / or by simple experimentation by one of ordinary skill in the art.

[0016] As used herein, the term “photoinitiator” refers to a molecule that, when exposed to electromagnetic radiation (e.g., ultraviolet light, visible light, and any combination thereof), produces a reactive species (e.g., a free radical, a cation, or anion).

[0017] As used herein, the term “initiator” generally refers to one or more thermal initiators, one or more photoinitiators, or a combination of one or more thermal initiators and one or more photoinitiators.

[0018] As used herein, the term "polyamide monomer" refers to the monomer that forms a polyamide.

[0019] As used herein, the term "polyacid" refers to a compound having two or more carboxylic acid moieties. In this specification, the anhydride moiety is considered a carboxylic acid moiety because the anhydride undergoes ring-opening to a carboxylic acid during synthesis.

[0020] As used herein, the term "polyamine" refers to a compound having two or more amine moieties.

[0021] As used herein, the term "amino acid" refers to a compound having one or more carboxylic acid moieties and one or more amine moieties. Here again, the anhydride moiety is considered a carboxylic acid moiety because the anhydride undergoes ring-opening to the carboxylic acid during synthesis.

[0022] When a polymer is referred to using the term -mer unit (e.g., polyamide monomer), those skilled in the art will understand that the -mer unit is in a polymerized form within the polymer.

[0023] As used herein, the term "thermoplastic polymer" refers to a plastic polymer material that reversibly softens and hardens upon heating and cooling. Thermoplastic polymers include thermoplastic elastomers.

[0024] As used herein, the term “elastomer” refers to a copolymer comprising a crystalline “rigid” portion and an amorphous “soft” portion. In the case of polyurethane, the crystalline portion may include a portion of polyurethane containing urethane functionality and optionally selected chain-extending groups, and the soft portion may include, for example, a polyol.

[0025] As used herein, the term "polyurethane" refers to the polymer reaction product between a diisocyanate, a polyol, and any chain extender.

[0026] As used herein, the term “oxide” refers to both metallic oxides and non-metallic oxides. For the purposes of this disclosure, silicon is considered a metal.

[0027] In this specification, the terms “associated,” “association,” and their grammatical variations are used to refer to the chemical bonding and / or physical adhesion of the emulsifying stabilizer to the surface. While not limited to theory, the associations described herein between polymers and emulsifying stabilizers are primarily considered to be physical adhesions via hydrogen bonding and / or other mechanisms. However, some degree of chemical bonding may also occur.

[0028] As used herein, the terms “embedded” with respect to nanoparticles and the surface of polymer particles mean that the nanoparticles extend at least partially into the surface such that the polymer is in contact with the nanoparticles to a greater extent than would occur if the nanoparticles were simply deposited on the surface of the polymer particles.

[0029] As used herein, the term “dry blend” refers to a mixture of components in which each component comprises less than 10% by weight of the solvent and / or dispersant (e.g., water, methanol, acetone, etc., and any combination thereof) present by the weight of the component.

[0030] As used herein, the term “wet blend” means that at least one component is mixed with another component in the presence of 10% by weight or more of a solvent and / or dispersant (e.g., water, methanol, acetone, etc., and any combination thereof) by the weight of that component.

[0031] In this specification, D10, D50, D90, and diameter span are primarily used to describe particle size. As used herein, the term "D10" refers to a diameter in which 10% of the sample (on a volume basis, unless otherwise specified) consists of particles with a diameter less than the specified diameter value. As used herein, the term "D50" refers to a diameter in which 50% of the sample (on a volume basis, unless otherwise specified) consists of particles with a diameter less than the specified diameter value. As used herein, the term "D90" refers to a diameter in which 90% of the sample (on a volume basis, unless otherwise specified) consists of particles with a diameter less than the specified diameter value.

[0032] As used herein, the terms “diameter span,” “span,” and “span size” refer to diameter and provide an indicator of the extent of the particle size distribution, calculated as (D90-D10) / D50 (again, each D value is based on volume unless otherwise stated).

[0033] Particle size can be determined by light scattering techniques using a Malvern MASTERSIZER® 3000 or by analysis of optical digital microscope images. Unless otherwise stated, light scattering techniques are used to analyze particle size.

[0034] For light scattering techniques, the control samples were glass beads with diameters ranging from 15 μm to 150 μm, obtained from Malvern Analytical Ltd. under the trademarked Quality Audit Standards QAS4002™. Unless otherwise noted, samples were analyzed as dry powder. The analyzed particles were dispersed in air and analyzed using the AERO S dry powder dispersion module with MASTERSIZER™ 3000. Particle size was derived using instrument software from plots of volume density as a function of size.

[0035] Particle size and diameter span can also be determined by optical digital microscopy. Optical images are obtained using a Keyence VHX-2000 digital microscope with version 2.3.5.1 software (system version 1.93) for particle size analysis.

[0036] When referring to sieves in this specification, the pore / screen size is as specified in USA Standard Sieve (ASTM E11-17).

[0037] As used herein, the terms “circularity” and “sphericity” for particles refer to how close a particle is to being a perfect sphere. To determine the circularity, an optical microscope image of the particle is taken. The perimeter (P) and area (A) of the particle in the plane of the microscope image are calculated (for example, using a SYSMEX FPIA 3000 particle shape and particle size analyzer available from Malvern Instruments). The circularity of the particle is C EA / P and C EA This is the circumference of a circle having an area equivalent to the area (A) of the actual particle.

[0038] As used herein, the term “shear force” refers to agitation or similar processes that induce mechanical agitation in a fluid.

[0039] As used herein, the term "aspect ratio" refers to the ratio obtained by dividing length by width, where length is greater than width.

[0040] Unless otherwise specified, the melting point of a polymer is determined using a heating rate of 10°C / min and a cooling rate of 10°C / min according to ASTM E794-06 (2018).

[0041] Unless otherwise specified, the softening temperature or softening point of a polymer is determined by ASTM D6090-17. The softening temperature can be measured using a 0.50 g sample at a heating rate of 1 °C / min using a cup-and-ball apparatus available from Mettler-Toledo.

[0042] The angle of repose is a measure of the fluidity of a powder. The angle of repose was determined using the Hosokawa Micron Powder Characteristics Tester PT-R, following ASTM D6393-14 "Standard Test Method for Bulk Solids Characterized by Carr Indices".

[0043] Hausner ratio (H r ) is a measure of the fluidity of powders, H r =ρ tap / ρ bulk Calculated by ρ bulk This is the bulk density according to ASTM D6393-14, and ρ tap This is the tap density according to ASTM D6393-14.

[0044] When used herein, the viscosity of the dispersion medium is the kinetic viscosity at 25°C, measured according to ASTM D445-19, unless otherwise specified. For commercially obtained dispersion mediums (e.g., PDMS oil), the kinetic viscosity data referenced herein is provided by the manufacturer, whether measured according to the aforementioned ASTM or according to another standard measurement technique. Unsaturated polyamide

[0045] Unsaturated polyamides can be synthesized by various methods, each containing at least one monomer with at least one unsaturated aliphatic carbon-carbon bond. Examples of these methods include, but are not limited to, condensation polymerization (also known herein as polycondensation) and ring-opening polymerization. While not theoretically bound, the synthesis method may preferably be carried out at a temperature in which the unsaturated bond does not participate in polymerization. This temperature varies depending on the monomer used, but preferably, unsaturated polyamides are synthesized at temperatures below 100°C.

[0046] In this specification, these polymerizations are carried out in the presence of one or more polyamine monomers, one or more polyacid monomers, one or more amino acid monomers, or any combination thereof, wherein at least one of the monomers contains at least one unsaturated aliphatic carbon-carbon bond.

[0047] Several examples of polycondensation and ring-opening polymerization reactions are presented below, followed by non-limiting examples of polyamide monomers suitable for use in one or more of these reactions. The following examples are not limited to polyamide monomers.

[0048] Scheme 1 shows a polycondensation reaction of an amino acid polyamide monomer, where C-1 represents the portion of the amino acid polyamide monomer between the carboxylic acid and amine moieties involved in the polycondensation reaction. With respect to the compositions and methods of this disclosure, C-1 in this example comprises at least one unsaturated aliphatic carbon-carbon bond. Scheme 2 is a non-limiting example of Scheme 1. [ka]

[0049] Scheme 3 illustrates a polycondensation reaction between two amino acid polyamide monomers, where C-1 and C-2 represent the respective amino acid polyamide monomer portions between the carboxylic acid and amine moieties involved in the polycondensation reaction. With respect to the compositions and methods of this disclosure, C-1, C-2, or both C-1 and C-2 may comprise at least one unsaturated aliphatic carbon-carbon bond. [ka]

[0050] Scheme 4 is a non-restrictive example of Scheme 3, where C-1 does not contain an unsaturated aliphatic carbon-carbon bond and C-2 contains an unsaturated aliphatic carbon-carbon bond. In examples like Scheme 4, where one polyamide monomer contains at least one unsaturated aliphatic carbon-carbon bond and the other does not, the relative ratio of the two monomers can be used to control the amount of unsaturated aliphatic carbon-carbon bonds in the resulting polyamide. [ka]

[0051] Scheme 5 illustrates a polycondensation reaction between an amino acid polyamide monomer and a polyamine amide monomer, where C-1 and C-2 represent the respective polyamide monomer portions between the carboxylic acid and amine moiety or the two amine moieties involved in the polycondensation reaction. With respect to the compositions and methods of this disclosure, C-1, C-2, or both C-1 and C-2 may contain at least one unsaturated aliphatic carbon-carbon bond. [ka]

[0052] In the formula, C-1 in Scheme 5 contains at least one unsaturated aliphatic carbon-carbon bond, and the majority of the resulting polyamide contains an unsaturated aliphatic carbon-carbon bond. In the formula, C-2 in Scheme 5 contains at least one unsaturated aliphatic carbon-carbon bond, and C-1 in Scheme 5 does not contain an unsaturated aliphatic carbon-carbon bond, and only the unsaturated aliphatic carbon-carbon bond of C-2, in the case of a single bond per polymer chain, may be involved in future crosslinking (e.g., during densification in an addition method). In such examples, the resulting polyamide has a lower crosslinking potential than some other examples herein. Scheme 6 is a non-limiting example of Scheme 5, in which C-2 contains at least one unsaturated aliphatic carbon-carbon bond, and C-1 does not contain an unsaturated aliphatic carbon-carbon bond. [ka]

[0053] Scheme 7 illustrates a polycondensation reaction between an amino acid polyamide monomer and a polyacid polyamide monomer, where C-1 and C-2 represent the respective polyamide monomer portions between a carboxylic acid and an amine moiety or two carboxylic acid moieties involved in the polycondensation reaction. With respect to the compositions and methods of this disclosure, C-1, C-2, or both C-1 and C-2 may comprise at least one unsaturated aliphatic carbon-carbon bond. [ka]

[0054] In the formula, C-1 in Scheme 7 contains at least one unsaturated aliphatic carbon-carbon bond, and the majority of the resulting polyamide contains an unsaturated aliphatic carbon-carbon bond. In the formula, C-2 in Scheme 7 contains at least one unsaturated aliphatic carbon-carbon bond, and C-1 in Scheme 7 does not contain an unsaturated aliphatic carbon-carbon bond, and only the unsaturated aliphatic carbon-carbon bond of C-2, in the case of a single bond per polymer chain, may be involved in future crosslinking (e.g., during densification in an addition method). In such examples, the resulting polyamide has a lower crosslinking potential than some of the other examples herein. Scheme 8 is a non-limiting example of Scheme 7, in which C-2 contains at least one unsaturated aliphatic carbon-carbon bond, and C-1 does not contain an unsaturated aliphatic carbon-carbon bond. [ka]

[0055] Scheme 9 shows a polycondensation reaction between an amino acid polyamide monomer, a polyamine polyamide monomer, and a polyacid polyamide monomer, where C-1, C-2, and C-3 represent the respective polyamide monomer portions between the carboxylic acid involved in the polycondensation reaction, the amine moiety (C-1), the two amine moieties (C-2), and the two carboxylic acid moieties (C-3). With respect to the compositions and methods of this disclosure, one or more of C-1, C-2, and C-3 may contain at least one unsaturated aliphatic carbon-carbon bond. [ka]

[0056] Scheme 10 illustrates a polycondensation reaction between a polyamine polyamide monomer and a polyacid polyamide monomer, where C-1 and C-2 represent the respective polyamide monomer portions between two amine moieties or two carboxylic acid moieties involved in the polycondensation reaction. With respect to the compositions and methods of this disclosure, C-1, C-2, or both C-1 and C-2 may contain at least one unsaturated aliphatic carbon-carbon bond. [ka]

[0057] The polycondensation reaction examples in Schemes 1-10 are non-limiting examples. Additional polyamide monomers may be included in such schemes. For example, Scheme 10 may include a third polyamide monomer which is a polyacid polyamide monomer having a C-3 moiety between two amine moieties. Furthermore, Schemes 1-10 show diacid polyamide monomers, diamine polyamide monomers, and amino acid polyamide monomers having one amine moiety and one carboxylic acid moiety. Those skilled in the art will recognize how the schemes extend to polyacid polyamide monomers, polyamine polyamide monomers, and amino acid polyamide monomers having one or more amine moieties and one or more carboxylic acid moieties.

[0058] Scheme 11 illustrates a ring-opening reaction between a cyclic polyamide monomer and an amino acid polyamide monomer, where C-1 represents the portion of the amino acid polyamide monomer between the amine and carboxylic acid moiety involved in the reaction. With respect to the compositions and methods of this disclosure, C-1 comprises at least one unsaturated aliphatic carbon-carbon bond. [ka]

[0059] Scheme 12 illustrates a ring-opening reaction between a cyclic polyamide monomer and a polyacid polyamide monomer, where C-1 represents the portion of the polyacid polyamide monomer between the two carboxylic acid moieties involved in the reaction. With respect to the compositions and methods of this disclosure, C-1 comprises at least one unsaturated aliphatic carbon-carbon bond. [ka]

[0060] Scheme 13 shows a ring-opening reaction between a cyclic polyamide monomer and a polyamine polyamide monomer, where C-1 represents the portion of the polyamine polyamide monomer between the two amine moieties involved in the reaction. With respect to the compositions and methods of the present disclosure, C-1 contains at least one unsaturated aliphatic carbon-carbon bond.

Chemical formula

[0061] The ring-opening reaction examples of Schemes 11 - 13 are non-limiting examples. Additional polyamide monomers may be included in such schemes. For example, Scheme 13 may include a third polyamide monomer that is a polyacid polyamide monomer having a C-2 portion between two carboxylic acid moieties. Further, Schemes 11 - 13 show diacid polyamide monomers, diamine polyamide monomers, and amino acid polyamide monomers having one amine moiety and one carboxylic acid moiety. Those skilled in the art will recognize how the schemes extend to polyacid polyamide monomers, polyamine polyamide monomers, and amino acid polyamide monomers having one or more amine moieties and one or more carboxylic acid moieties.

[0062] Examples of amino acid polyamide monomers having no at least one unsaturated aliphatic carbon-carbon bond and suitable for use in polycondensation include, but are not limited to, HN-(CH2) where n is 1 - 20 n -COOH, branched aliphatic amino acids (e.g., C4 - C 20 ), cyclic aliphatic amino acids (e.g., C4 - C 20 ), aromatic amino acids (e.g., 3-aminobenzoic acid, 4-aminobenzoic acid), etc., and any combination thereof.

[0063] Examples of amino acid polyamide monomers having at least one unsaturated aliphatic carbon-carbon bond include, but are not limited to, maleamic acid, N-propylmaleamic acid, etc., and any combination thereof.

[0064] Examples of polyacid polyamide monomers suitable for use in polycondensation that do not have at least one unsaturated aliphatic carbon-carbon bond include, but are not limited to, HOOC-(CH2) with n = 1 to 20. n -COOH (e.g., adipic acid, terephthalic acid, isophthalic acid, pimelic acid, suberic acid, decandioic acid, dodecandioic acid), isophthalic acid, terephthalic acid, pento-2-endioic acid, dodeca-2-endioic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, adic acid, sebacic acid, undecandioic acid, dodecandioic acid, 1,3-cyclohexanedicarboxylic acid, and any combination thereof.

[0065] Examples of polyacid polyamide monomers having at least one unsaturated aliphatic carbon-carbon bond include, but are not limited to, fumaric acid, maleic acid, glutaconic acid, aconitic acid, itaconic acid, and any combination thereof.

[0066] Examples of polyamine polyamide monomers that do not have at least one unsaturated aliphatic carbon-carbon bond and are suitable for use in polycondensation include, but are not limited to, HN-(CH2) with n = 1 to 20. n-NH, 1,5-diamino-2-methylpentane, 1,2-diaminopropane, trimethylhexamethylenediamine, 2-methyloctane-1,8-diamine, n-methyl1,6-hexamethylenediamine with N = 2 or 3, n-methyl1,7-heptamethylenediamine with N = 2 to 4, n-methyl1,8-octamethylenediamine with N = 2 to 4, n-methyl1,12-dodecamethylenediamine with N = 2 to 6, 1,3-bis(aminomethyl)benzene, ortho-phenyl Examples include n-bis(methylamine), 1,4-bis(aminomethyl)benzene, 1,4-cyclohexanediamine, 4-methylcyclohexane-1,3-diamine, 4-methylcyclohexane-1,3-diamine, diphenylethylenediamine, diphenylethylenediamine, 1,3-bis(aminomethyl)cyclohexane, 4,4'-methylenebis(cyclohexylamine), 4,4'-biphenyldiamine, 1,8-diaminonaphthalene, and any combination thereof.

[0067] Examples of polyamine polyamide monomers having at least one unsaturated aliphatic carbon-carbon bond include, but are not limited to, 1,4-diamino-2-butene, 1,5-bis(3-aminophenyl)-1,4-pentadiene-3-one (DADBA), trans-4-cyclohexene-1,2-diamine, and any combination thereof.

[0068] Examples of cyclic polyamide monomers suitable for use in ring-opening polymerization include, but are not limited to, azelidinone, 2-azetidinone, 2-pyrrolidinone, 2-piperidinone, ε-caprolactam, 2-azacyclooctanone, 2-azacyclononanone, 2-azacyclodecanone, 2-azacycloundodecanone, 2-aza-cyclododecanone, laurolactam, butyrolactam, pivalolactam, ε-caprolactam, capryloractam, enantractam, undecanonelactam, laurolactam (dodecanolactam), and any combination thereof.

[0069] Polycondensation reactions (e.g., schemes 1-10 and their variations) can be carried out in the presence of activators and / or metal salts. Examples of activators include, but are not limited to, triphenylphosphine and any combination thereof. Examples of metal salts include, but are not limited to, calcium chloride, cesium fluoride and any combination thereof.

[0070] Polycondensation reactions (e.g., schemes 1-10 and their variations) can be carried out at approximately 50°C to approximately 200°C (or approximately 50°C to approximately 100°C, or approximately 75°C to approximately 150°C, or approximately 125°C to approximately 200°C).

[0071] Polycondensation reactions (e.g., schemes 1-10 and their variations) can take place over a period of approximately 5 minutes to 24 hours (or approximately 5 minutes to 6 hours, or approximately 2 hours to 12 hours, or approximately 6 hours to 24 hours).

[0072] Polycondensation reactions (e.g., schemes 1-10 and their variations) can be carried out in solvents including, but not limited to, N-methylpyrrolidone (NMP), pyridine, dichloromethane, dimethyl sulfoxide (DMSO), N,N-dimethylformamide, acetonitrile, tetrahydrofuran, and any combination thereof.

[0073] Polycondensation reactions (e.g., schemes 1-10 and their variations) involve a molar ratio of polyamide monomers having (cumulatively) at least one unsaturated aliphatic carbon-carbon bond to polyamide monomers not having (cumulatively) at least one unsaturated aliphatic carbon-carbon bond, where the molar ratio is approximately 500:1 to approximately 1:500 (or approximately 500:1 to approximately 100:1, or approximately 250:1 to approximately 50:1, or approximately 100:1 to approximately 10:1, or The reaction can be carried out in ratios of approximately 50:1 to 1:1, or approximately 25:1 to 1:25, or approximately 1:1 to 1:50, or approximately 1:10 to 1:100, or approximately 1:50 to 1:250, or approximately 1:100 to 1:500. The more polyamide monomers containing at least one unsaturated aliphatic carbon-carbon bond that are included in the polycondensation reaction, the more potential crosslinking sites there will be (for example, during densification in addition manufacturing methods).

[0074] Ring-opening polymerization reactions (e.g., schemes 11-13 and their variations) can be carried out in the presence of activators and / or metal salts. Examples of activators include, but are not limited to, triphenylphosphine and any combination thereof. Examples of metal salts include calcium chloride, cesium fluoride and any combination thereof.

[0075] Ring-opening polymerization reactions (e.g., schemes 11-13 and their variations) can be carried out at approximately 50°C to approximately 200°C (or approximately 50°C to approximately 100°C, or approximately 75°C to approximately 150°C, or approximately 125°C to approximately 200°C).

[0076] Ring-opening polymerization reactions (e.g., schemes 11-13 and their variations) can be carried out over a period of approximately 5 minutes to 24 hours (or approximately 5 minutes to 6 hours, or approximately 2 hours to 12 hours, or approximately 6 hours to 24 hours).

[0077] Ring-opening polymerization reactions (e.g., schemes 11-13 and their variations) can be carried out in solvents including, but not limited to, N-methylpyrrolidone (NMP), pyridine, dichloromethane, dimethyl sulfoxide (DMSO), N,N-dimethylformamide, acetonitrile, tetrahydrofuran, and any combination thereof.

[0078] Ring-opening polymerization reactions (e.g., schemes 11-13 and their variations) can be carried out with a molar ratio of polyamide monomers having (cumulatively) at least one unsaturated aliphatic carbon-carbon bond to polyamide monomers not having (cumulatively) at least one unsaturated aliphatic carbon-carbon bond of about 500:1 to about 1:500 (or about 500:1 to about 100:1, or about 250:1 to about 50:1, or about 100:1 to about 10:1, or about 50:1 to about 1:1, or about 25:1 to about 1:25, or about 1:1 to about 1:50, or about 1:10 to about 1:100, or about 1:50 to about 1:25, or about 1:10 to about 1:25, or about 1:10 to about 1:50, or about 1:10 to about 1:100, or about 1:50 to about 1:25, or about 1:10 to about 1:50). The more polyamide monomers having at least one unsaturated aliphatic carbon-carbon bond included in the polycondensation reaction, the more potential crosslinking sites there are.

[0079] Unsaturated polyamides obtained from any suitable synthetic route may have molar equivalents of at least one polyamide unit having an unsaturated aliphatic carbon-carbon bond and at least one polyamide unit not having an unsaturated aliphatic carbon-carbon bond in a ratio of about 500:1 to about 1:500 (or about 500:1 to about 100:1, or about 250:1 to about 50:1, or about 100:1 to about 10:1, or about 50:1 to about 1:1, or about 25:1 to about 1:25, or about 1:1 to about 1:50, or about 1:10 to about 1:100, or about 1:50 to about 1:250, or about 1:100 to about 1:50 to about 1:50). Initiator dope, unsaturated polyamide composition and method

[0080] The methods and compositions described herein include unsaturated polyamides doped with an initiator suitable for crosslinking the unsaturated polyamide (for example, during densification in an addition process). The initiator may be a thermal initiator, a photoinitiator, or a combination of a thermal initiator and a photoinitiator.

[0081] Examples of thermal initiators include ammonium persulfate, sodium persulfate; potassium persulfate; organic peroxides (e.g., benzoyl peroxide, t-amyl peracetate, 2,5-dimethyl-2,5-bis(t-butylperoxy)-3-hexine, 2,5-dimethyl-2,5-di-(t-butylperoxy)-hexane, t-butylalpha-cumyl peroxide, dibutyl peroxide, t-butyl hydroperoxide, dichlorobenzoyl peroxide, dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoic acid) )-3-hexine, 1,3-bis(t-butylperoxyisopropyl)benzene, lauroyl peroxide, di-t-amyl peroxide, 1,1-di-(t-butylperoxy)cyclohexane, 2,2-di-(t-butylperoxy)butane, and 2,2-di-(t-amylperoxy)propane), 2,2'-azobis(2-methylpropanenitrile, 2,2'-azobis(isobutyronitrile, AIBN), 1,1'-azobis(cyclohexanecarbonitride), 1,1'-azobis (Cyanocyclohexane), 2,2'-Azodi(2-methylbutyronitrile, 2-methyl2-2'-azobispropanenitrile, 2-2'-azobiisobutylamide dehydrated, 2,2'-azobis(2-methyl-N-phenylpropionamidine)dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-hydroxyphenyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[N-(4-aminophenyl)-2-methylpropionamidine]dihydrochloride 2,2'-Azobis[2-methyl-N(phenylmethyl)propionamidine]dihydrochloride, 2,2'-Azobis[2-methyl-N-2-propenylpropionamidine]dihydrochloride, 2,2'-Azobis[N-(2-hydroxy-ethyl)-2-methylpropionamidine]dihydrochloride, 2,2'-Azobis[2(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-Azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-Azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepine-2-yl)propane]dihydrochloride, 2,2'-Azobis[2-(3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-Azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidine-2-yl)propane]dihydrochloride, 2,2'-Azobis{2-[1-(2-hydroxyethyl)-2-imidazoline-2-yl]propane}dihydrochloride, 2,2'-Azobis(4-methoxy-2,4- Examples include, but are not limited to, dimethylvaleronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitride), dimethyl2,2'-azobis(2-methylpropionate), 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, and any combination thereof.

[0082] Examples of photoinitiators, though not limited to them, include (±)-canfaquinone, acetophenone, 3-acetophenol, 4-acetophenol, benzophenone, 2-methylbenzylphenone, 3-methylbenzophenone, 3-hydroxybenzophenone, 3,4-dimethylbenzphenone, 4-hydroxybenzophenone, 4-benzoylbenzoic acid, 2-benzoylbenzoic acid, methyl-2-benzoylbenzoate, 4,4'-dihydroxybenzophenone, 4-(dimethylammonium) (no)-benzophenone, 4,4'-bis(dimethylamino)-benzophenone, 4,4'-bis(diethylamino)-benzophenone, 4,4'-dichlorobenzophenone, 4-(p-tolylthio)benzophenone, 4-phenylbenzophenone, 1,4-dibenzoylbenzene, benzyl, 4,4'-dimethylbenzyl, p-anisyl, 2-benzoyl-2-propanol, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 1-benzoylcycline Rohexanol, benzoin, anisonin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, O-tosylbenzoin, 2,2-diethoxyacetophenone, benzyldimethylketal, 2-methyl-4'-(methylthio)-2-morpholinopropiophenone, 2-benzyl-2-(dimethylamino)-4'-morpholinobylophenone, 2-isonitrosopropiophenone, anthraquinone, 2-ethyl Anthraquinone, anthraquinone-2-sulfonate sodium hydrate, 9,10-phenanthrenequinone, 9,10-phenanthrenequinone, dibenzosverenone, 2-chlorothioxanthone, 2-isopropylthioxanthone, 2,4-diethylthiozanten-9-one, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,Examples include (trimethylbenzoyl)phosphine oxide (TPO), acylphosphine oxide (APO), bisacylphosphine oxide (BAPO), lithium phenyl (2,4,6-trimethylbenzoyl) phosphine, and any combination thereof.

[0083] Several methods can be used to dope unsaturated polyamides with initiators. Generally, doping can be achieved by melt blending, dry blending (as defined above), wet blending (as defined above), or a combination thereof.

[0084] In melt blending, one or more unsaturated polyamides are melted and mixed with one or more initiators. Such blends may optionally contain other additives (e.g., other thermoplastic polymers, fillers, etc.). However, the melting temperature should be below the temperature at which one or more initiators cause crosslinking. Generally, melt blending methods are limited because the initiators available at the temperature required to melt the unsaturated polyamides are restricted.

[0085] In dry blends, one or more unsaturated polyamides may be mixed with one or more initiators. Such blends may optionally contain other additives (e.g., other thermoplastic polymers, fillers, etc.). In dry blends, each component being blended should contain less than 10% by weight of the solvent and / or dispersant (e.g., water, methanol, acetone, etc., and any combination thereof) present by weight of the component. Dry blending may be performed in a blender or other mixer that generates a shear force that breaks down the fine particles of unsaturated polyamide and / or initiator. In some cases, the initiator may be liquid at room temperature. In such cases, the initiator may be coated and / or absorbed into the unsaturated polyamide particles.

[0086] In wet blends, one or more unsaturated polyamides may be mixed with one or more initiators in the presence of a solvent and / or dispersant (e.g., water, methanol, acetone, etc., and any combination thereof). Such blends may optionally contain other additives (e.g., other thermoplastic polymers, fillers, etc.). In the methods described herein, one or more unsaturated polyamides may generally be dispersed in a fluid, typically as solid particles, and one or more initiators (either dry or wet) may be added to the dispersion and / or added during the fluid addition of the unsaturated polyamides. Again, the dispersion may contain other additives. The dispersion may be mixed for a desired time (e.g., about 15 minutes to about 1 day, or about 30 minutes to about 3 hours), then filtered, washed, and dried to remove the fluid (preferably dried so that less than 10% by weight of fluid remains). In some cases, during mixing, the initiators may be absorbed by the unsaturated polyamide particles.

[0087] The goal of each blending method is to produce a mixture of one or more unsaturated polyamides and one or more initiators.

[0088] The weight ratio of unsaturated polyamide (cumulatively) to initiator (cumulatively) may be approximately 90:10 to approximately 99:1. Selective laser sintering using initiator-doped, unsaturated polyamide

[0089] As described herein, SLS uses polymer particles (or powders) to produce objects. The methods and compositions of this disclosure include particles comprising unsaturated polyamides and initiators as described herein.

[0090] The particles can be produced by precipitation, cold milling, or melt emulsification. Depending on these methods, the initiator may be present during and / or after particle formation.

[0091] An exemplary precipitation method for generating particles is direct emulsion polymerization, in which the polycondensation and / or ring-opening reactions described herein occur in the emulsion. The discontinuous phase of the emulsion is where the polycondensation reaction takes place. When the reaction stops, the discontinuous phase becomes unsaturated polyamide particles. In this embodiment, initiator doping is preferably carried out after the formation of the unsaturated polyamide particles. If the initiator is present during the polycondensation reaction, crosslinking may occur. Therefore, initiator-doped unsaturated polyamide particles are preferably formed by first forming unsaturated polyamide particles by direct emulsion polymerization and precipitation, and then wet and / or dry blending the resulting particles with the initiator. As a non-limiting example, the methods of the present disclosure may include emulsion polymerization via polycondensation and / or ring-opening reactions (e.g., via one or more of schemes 1 to 13) between a first polyamide monomer and a second polyamide monomer, wherein the second polyamide monomer comprises at least one unsaturated aliphatic carbon-carbon bond for producing an unsaturated polyamide; emulsion polymerization; precipitation of the unsaturated polyamide as particles; and blending the particles containing the unsaturated polyamide with an initiator (via wet and / or dry blending).

[0092] In another particle generation example, an unsaturated polyamide may be dissolved in a solvent (e.g., ethanol or propanol) under high pressure and high temperature (e.g., about 100°C to about 150°C). Upon cooling, the unsaturated polyamide precipitates in the particles. This method is referred to herein as thermally inductive precipitation. In this example, the initiator may be present with the unsaturated polyamide after precipitation. Alternatively, or in addition to such embodiments, the precipitated particles may be wet and / or dry blended with the initiator. In non-limiting examples, the methods of the present disclosure may include dissolving an unsaturated polyamide (e.g., one or more products from schemes 1 to 13) in a solvent, precipitating the unsaturated polyamide as particles, and blending the particles containing the unsaturated polyamide with the initiator (via wet and / or dry blending). In another non-limiting example, the method of the present disclosure may include dissolving an unsaturated polyamide (e.g., one or more products from schemes 1 to 13) and an initiator in a solvent, and precipitating the unsaturated polyamide to obtain particles containing the unsaturated polyamide and the initiator.

[0093] In yet another embodiment, the unsaturated polyamide may be chilled and milled to produce particles. In this embodiment, the initiator may be present with the unsaturated polyamide before chill milling. Alternatively, or in addition to such embodiments, the resulting particles may be wet and / or dry blended with the initiator. In a non-limiting example, the method of the present disclosure may include chilling an unsaturated polyamide (e.g., one or more products from schemes 1 to 13), milling the chilled unsaturated polyamide to obtain particles, and blending the particles containing the unsaturated polyamide with the initiator (via wet and / or dry blending). In another non-limiting example, the method of the present disclosure may include chilling an unsaturated polyamide (e.g., one or more products from schemes 1 to 13) in the presence of an initiator, and milling the chilled unsaturated polyamide to obtain particles containing the unsaturated polyamide and the initiator.

[0094] In another example, the unsaturated polyamide may be formed into particles by melt emulsification (described in more detail herein). In this example, the initiator may be present in the melt. However, as discussed herein, the temperature of the melt is preferably lower than the temperature at which the initiator crosslinks the unsaturated polyamide. Alternatively, or in addition to such embodiments, the resulting particles may be wet and / or dry blended with the initiator. In a non-limiting example, the method of the present disclosure may include melt emulsifying an unsaturated polyamide (e.g., one or more products from schemes 1 to 13), cooling the melt emulsification to obtain particles, and blending the particles containing the unsaturated polyamide with the initiator (via wet and / or dry blending). In another non-limiting example, the method of the present disclosure may include melt emulsifying an unsaturated polyamide (e.g., one or more products from schemes 1 to 13) in the presence of an initiator, and cooling the melt emulsification to obtain particles containing the unsaturated polyamide and the initiator.

[0095] In the case of thermal induction precipitation, low-temperature milling, and melt emulsification, the resulting particles include an unsaturated polyamide, optionally a thermoplastic polymer different from the unsaturated polyamide, and optionally a compatibilizer. That is, the starting materials for such methods may include an unsaturated polyamide, optionally a thermoplastic polymer different from the unsaturated polyamide, and optionally a compatibilizer. For example, the thermoplastic polymer and optionally the compatibilizer may be dissolved in the solvent before precipitation by thermal induction precipitation. In another example, an unsaturated polyamide may be melt-blended with a thermoplastic polymer different from the unsaturated polyamide and optionally the compatibilizer. The resulting blended polymer may be used in low-temperature milling. In yet another example, the components of melt emulsification may include an unsaturated polyamide, optionally a thermoplastic polymer different from the unsaturated polyamide, and optionally a compatibilizer.

[0096] Thermoplastic polymers may also have unsaturated sites that participate in crosslinking. Thermoplastic polymers may not participate in crosslinking but may provide other mechanical, thermal, or physical properties. Combinations of the two types of thermoplastic polymers described above may be included.

[0097] The weight ratio of unsaturated polyamide (cumulatively) to thermoplastic polymers other than unsaturated polyamide may be approximately 500:1 to approximately 1:10 (or approximately 500:1 to approximately 100:1, or approximately 250:1 to approximately 50:1, or approximately 100:1 to approximately 10:1, or approximately 50:1 to approximately 1:1, or approximately 25:1 to approximately 1:10). If a large amount of thermoplastic polymers other than unsaturated polyamides are included, the amount of crosslinking in the resulting object formed by the SLS method will be reduced, provided that these thermoplastic polymers are not involved in crosslinking.

[0098] Examples of thermoplastic polymers include saturated polyamides, polyurethanes, polyethylene, polypropylene, polyacetals, polycarbonates, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polytrimethylene terephthalate (PTT), polyhexamethylene terephthalate, polystyrene, polyvinyl chloride, polytetrafluoroethylene, polyester (e.g., polylactic acid), polyethers, polyethersulfones, polyetheretherketones, polyacrylates, polymethacrylates, polyimides, and acrylonitrile butadiene styrene. Styrene (ABS), polyphenylene sulfide, vinyl polymer, polyarylene ether, polyarylene sulfide, polysulfone, polyether ketone, polyamide-imide, polyether-imide, polyether ester, copolymers containing polyether blocks and polyamide blocks (PEBA or polyether block amide), grafted or ungrafted thermoplastic polyolefin, functionalized or unfunctionalized ethylene / vinyl monomer polymer, functionalized or unfunctionalized ethylene / alkyl (meth)acrylate, functionalized or unfunctionalized (meth)acrylic acid polymer, functionalized or non-functionalized Polyethylene / vinyl monomer / alkyl(meth)acrylate terpolymer, ethylene / vinyl monomer / carbonyl terpolymer, ethylene / alkyl(meth)acrylate / carbonyl terpolymer, methylmethacrylate-butadiene-styrene (MBS) type core-shell polymer, polystyrene-block-polybutadiene-block-poly(methyl methacrylate) (SBM) block terpolymer, chlorinated or chlorosulfonated polyethylene, polyvinylidene fluorideExamples include, but are not limited to, fluoride (PVDF), phenolic resins, poly(ethylene / vinyl acetate), polybutadiene, polyisoprene, styrene-based block copolymers, polyacrylonitrile, silicones, and any combination thereof. Furthermore, copolymers containing one or more of the above may be used in the methods and systems of this disclosure.

[0099] Other thermoplastic polymers in the compositions and methods of this disclosure may be elastomers or non-elastomers. Some of the aforementioned examples of other thermoplastic polymers may be elastomers or non-elastomers depending on the exact composition of the polymer. For example, polyethylene, which is a copolymer of ethylene and propylene, may be elastomer or non-elastomer depending on the amount of propylene in the polymer.

[0100] Thermoplastic elastomers generally fall within one of six classes: styrene-based block copolymers, thermoplastic polyolefin elastomers, thermoplastic vulcanized rubber (also called elastomer alloys), thermoplastic polyurethanes, thermoplastic copolyesters, and thermoplastic polyamides (typically block copolymers containing polyamides). Examples of thermoplastic polymers can be found in the Handbook of Thermoplastic Elastomers, 2nd edition, eds., BMWalker and CPRader, Van Nostrand Reinhold, New York, 1988. Examples of thermoplastic elastomers include elastomeric polyamides, polyurethanes, copolymers containing polyether blocks and polyamide blocks (PEBA or polyether block amides), methyl methacrylate-butadiene-styrene (MBS) type core-shell polymers, polystyrene-block-polybutadiene-block-poly(methyl methacrylate) (SBM) block copolymers, polybutadiene, polyisoprene, styrene-based block copolymers, and polyacrylonitrile, silicones, and others. Examples of elastic styrene-based block copolymers include at least one block selected from the group consisting of isoprene, isobutylene, butylene, ethylene / butylene, ethylene-propylene, and ethylene-ethylene / propylene. More specific examples of elastic styrene-based block copolymers include, but are not limited to, poly(styrene-ethylene / butylene), poly(styrene-ethylene / butylene-styrene), poly(styrene-ethylene / propylene), styrene-ethylene / propylene-styrene), poly(styrene-ethylene / propylene-styrene-ethylene-propylene), poly(styrene-butadiene-styrene), poly(styrene-butylene-butadiene-styrene), etc., and any combination thereof.

[0101] Examples of polyamides, though not limited to them, include polycaproamide, poly(hexamethylenesuccinate), polyhexamethyleneadipamide, polypentamethyleneadipamide, polyhexamethylenesebamide, polyundekaamide, polydodekaamide, polyhexamethyleneterephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semi-aromatic polyamides, aromatic polyamides, any copolymers thereof, and any combination thereof. Copolyamides may also be used. Examples of copolyamides include, but are not limited to, PA11 / 10.10, PA6 / 11, PA6.6 / 6, PA11 / 12, PA10.10 / 10.12, PA10.10 / 10.14, PA11 / 10.36, PA11 / 6.36, and PA10.10 / 10.36, as well as any combination thereof. Examples of polyamide elastomers include, but are not limited to, polyesteramides, polyether esteramides, polycarbonate esteramides, and polyether block amide elastomers.

[0102] Examples of polyurethanes include, but are not limited to, polyether polyurethanes, polyester polyurethanes, mixed polyethers and polyester polyurethanes, and any combination thereof. Examples of thermoplastic polyurethanes include, but are not limited to, poly[4,4'-methylenebis(phenylisocyanate)-alt-1,4-butanediol / di(propylene glycol) / polycaprolactone], ELASTOLLAN® 1190A (polyether polyurethane elastomer, available from BASF), ELASTOLLAN® 1190A10 (polyether polyurethane elastomer, available from BASF), and any combination thereof.

[0103] Compatibilizers can optionally be used to improve the blending efficiency and effect of unsaturated polyamides with one or more thermoplastic polymers. Examples of polymer compatibilizers, though not limited to them, include: PROPOLDER® MPP2020 20 (polypropylene, available from Polygroup Inc.), PROPOLDER® MPP2040 40 (polypropylene, available from Polygroup Inc.), NOVACOM® HFS2100 (maleic anhydride-functionalized high-density polyethylene polymer, available from Polygroup Inc.), KEN-REACT® CAPS® L® 12 / L (organometallic coupling agent, available from Kenrich Petrochemicals), KEN-REACT® CAPOW® L® 12 / H (organometallic coupling agent, available from Kenrich Petrochemicals), KEN-REACT® LICA® 12 (organometallic coupling agent, available from Kenrich Petrochemicals), and KEN-REACT® CAPS® KPR® 12 / LV (organometallic coupling agent, available from Kenrich Petrochemicals). Available from Petrochemicals), KEN-REACT(trademark) CAPOW(trademark) KPR(trademark) 12 / H (organometallic coupling agent, available from Kenrich Petrochemicals), KEN-REACT(trademark) titanate & zirconate (organometallic coupling agent, KenrichAvailable from Petrochemicals), VISTAMAXX (Trademark) (Ethylene-propylene copolymer, available from ExxonMobil), SANTOPRENE (Trademark) (Thermoplastic vulcanized ethylene-propylene-diene rubber and polypropylene, available from ExxonMobil), VISTALON (Trademark) (Ethylene-propylene-diene rubber, available from ExxonMobil), EXACT (Trademark) (Plastomer, available from ExxonMobil) EXXELO R(trademark) (polymer resin, available from ExxonMobil), FUSABOND(trademark) M603 (random ethylene copolymer, available from Dow), FUSABOND(trademark) E226 (anhydrous modified polyethylene, available from Dow), BYNEL(trademark) 41E710 (co-extrudeable adhesive resin, available from Dow), SURLYN(trademark) 1650 (ionomer resin, available from Dow), FUSABOND(trademark) P353 (chemically modified polypropylene copolymer, available from Dow) (Available from Dow), ELVALOY (Trademark) PTW (Ethylene terpolymer, available from Dow), ELVALOY (Trademark) 3427AC (Ethylene and butyl acrylate copolymer, available from Dow), LOTADER (Trademark) AX8840 (Ethylene acrylate terpolymer, available from Arkema), LOTADER (Trademark) 3210 (Ethylene acrylate terpolymer, available from Arkema), LOTADER (Trademark) 3410 (Ethylene acrylate terpolymer LIMAR (available from Arkema), LOTADER(trademark) 3430 (ethylene acrylate terpolymer, available from Arkema), LOTADER(trademark) 4700 (ethylene acrylate terpolymer, available from Arkema), LOTADER(trademark) AX8900 (ethylene acrylate terpolymer, available from Arkema), LOTADER(trademark) 4720 (ethylene acrylate terpolymer, available from Arkema), BAXXODUR(trademark) EC 301 (amine for epoxy, available from BASF), BAXXODUR(trademark) EC 311 (amine for epoxy, available from BASF), BAXXODUR(trademark) ECExamples include 303 (epoxy amine, available from BASF), BAXXODUR® EC 280 (epoxy amine, available from BASF), BAXXODUR® EC 201 (epoxy amine, available from BASF), BAXXODUR® EC 130 (epoxy amine, available from BASF), BAXXODUR® EC 110 (epoxy amine, available from BASF), styrene resins, polypropylene, polyamides, polycarbonates, EASTMAN® G-3003 (maleic anhydride grafted polypropylene, available from Eastman), RETAIN® (polymer modifier available from Dow), AMPLIFY TY® (maleic anhydride grafted polymer, available from Dow), INTUNE® (olefin block copolymer, available from Dow), and any combination thereof.

[0104] As described herein, the SLS method uses heat from a laser and other sources to compact particles (for example, the chamber may be heated to below the melting temperature of the polymer in the particles). To enhance the heating caused by the laser, the particles used in the SLS method may contain and / or be mixed with an infrared absorber. Generally, infrared absorbers absorb electromagnetic radiation (for example, at one or more wavelengths from about 100 nm to about 1 mm) and generate heat. Infrared absorbers can accelerate the initiation of initiators, resulting in crosslinking (for example, during compaction in an additive manufacturing method). Examples of infrared absorbers include, but are not limited to, carbon black, charcoal, carbon fibers, carbon nanotubes, graphite, copper hydroxide phosphate, chalk, bone, colorants and / or pigments (e.g., organic or inorganic, and synthetic or natural) such as interference pigments (e.g., IRIODIN® available from Merck), pearlescent pigments, and metal oxide-coated mica pigments, oxides and sulfides such as antimony oxide, tin oxide, indium oxide, zinc oxide, zinc sulfide, tin sulfide, or mixtures thereof, activators based on melamine cyanurate (MELAPUR® available from DSM), or flame retardants such as activators based on phosphorus, preferably phosphates, phosphite esters, phosphonits, or red phosphorus, carbon fibers, glass beads (hollow, porous, or solid kaolin, wollastonite, etc.), and any combination thereof. The infrared absorber may be dispersed as is or subsequently dispersed on a substrate such as mica. The infrared absorber may be present in the particles and incorporated with the particles, as described for the initiator.

[0105] The particles used in the SLS method described herein may include (a) initiator-doped unsaturated polyamide particles comprising an unsaturated polyamide, an initiator, optionally an infrared absorber, optionally a thermoplastic polymer different from the unsaturated polyamide, optionally a compatibilizer, and optionally other additives, and optionally (b) other thermoplastic particles comprising a thermoplastic polymer different from the unsaturated polyamide and optionally a compatibilizer.

[0106] The SLS method may involve depositing initiator-doped unsaturated polyamide particles (and optionally other thermoplastic particles) onto a surface, and then heating at least a portion of the deposited particles to promote compaction and crosslinking of the unsaturated polyamide to form a compacted body. While not theoretically bound, it is believed that heating the particles and / or exposure to a laser initiates the crosslinking of unsaturated bonds in the unsaturated polyamide by the initiator.

[0107] Examples of objects that can be produced by the SLS method using the unsaturated polyamides described herein include, but are not limited to, particles, films, packaging, toys, household goods, automotive parts, aerospace / aircraft parts, containers (e.g., containers for food, beverages, cosmetics, personal care compositions, pharmaceuticals, etc.), shoe soles, furniture parts, decorative household goods, plastic gears, screws, nuts, bolts, cable ties, jewelry, works of art, sculptures, medical items, prostheses, orthopedic implants, artifacts to aid learning in education, 3D anatomical models to assist surgery, robotics equipment, biomedical devices (orthotics), household appliances, dental supplies, electronic equipment, and sporting goods, and may be all or part of such articles. Furthermore, particles may be useful in applications such as paints, powder coatings, inkjet materials, electrophotographic toners, and 3D printing, but are not limited to these. Melt emulsification method and resulting particles

[0108] The figure is a flow chart of a non-limiting exemplary method 100 of the present disclosure. A thermoplastic polymer 102 (including one or more unsaturated polyamides described herein and optionally one or more other thermoplastic polymers described herein), a dispersion medium 104, and optionally an emulsifying stabilizer 106 are combined in 108 to produce a mixture 110. The components 102, 104, and 106 are added in any order and may include mixing and / or heating in process 108 to combine the components 102, 104, and 106.

[0109] Optionally, other additives such as initiators, infrared absorbers, and compatibilizers described herein may be included in the mixture and combined with components 102, 104, and 106 in any order.

[0110] Next, the mixture 110 is treated by applying a sufficiently high shear force to the mixture 110 at a temperature exceeding the melting or softening temperature of the thermoplastic polymer 102 (112) to form a molten emulsion 114. Since the temperature is higher than the melting or softening temperature of the thermoplastic polymer 102, the thermoplastic polymer 102 becomes a polymer melt. The shear rate should be sufficient to disperse the polymer melt in the dispersion medium 104 as droplets (i.e., polymer emulsion 114). Although not bound by theory, it is assumed that increasing the shear force should decrease the size of the polymer melt droplets in the dispersion medium 104, all other things being equal. However, at some point, there may be diminishing returns due to increasing the shear force and decreasing the droplet diameter, or there may be fragmentation into droplet contents that degrades the quality of the particles produced.

[0111] Next, the molten emulsion 114 inside and / or outside the mixing vessel is cooled (116) to solidify the polymer droplets into thermoplastic polymer particles (also called solidified thermoplastic polymer particles). The cooled mixture 118 is then processed (120) to isolate the thermoplastic polymer particles 122 from the other components 124 (e.g., dispersion medium 104, excess emulsion stabilizer 106, etc.), and the thermoplastic polymer particles 122 may be washed or otherwise purified. The thermoplastic polymer particles 122 include a thermoplastic polymer 102, and, if present, at least a portion of the emulsion stabilizer 106 coating the outer surface of the thermoplastic polymer particles 122. The emulsion stabilizer 106 or a portion thereof may be deposited on the thermoplastic polymer particles 122 as a uniform coating. In some cases, depending on non-limiting factors such as temperature (including cooling rate), the type of thermoplastic polymer 102, and the type and size of the emulsifying stabilizer 106, the nanoparticles of the emulsifying stabilizer 106 may become at least partially embedded within the outer surface of the thermoplastic polymer particles 122 during the process of association therewith. Even when embodiments are not performed, at least the nanoparticles in the emulsifying stabilizer 106 may remain firmly associated with the thermoplastic polymer particles 122, facilitating their further use. In contrast, dry blends of already formed (e.g., formed by a cryogenic grinding or precipitation process) thermoplastic polymer microparticles with a flow aid such as silica nanoparticles do not result in a robust and uniform coating of the flow aid on the thermoplastic polymer microparticles.

[0112] Advantageously, the dispersion medium and washing solvent of the systems and methods described herein (e.g., Method 100) can be regenerated and reused. Those skilled in the art will recognize any necessary washing of the used dispersion medium and solvent required for the regeneration process.

[0113] The thermoplastic polymer 102 and the dispersion medium 104 should be selected such that they are immiscible at various processing temperatures (e.g., from room temperature to the process temperature). An additional factor to consider is the difference (e.g., difference or ratio) in viscosity between the molten polyamide 102 and the dispersion medium 104 at the process temperature. The difference in viscosity can affect droplet breakdown and particle size distribution. While not theoretically bound, if the viscosities of the molten polyamide 102 and the dispersion medium 104 are too similar, the overall roundness of the product may be reduced, and particles may become more oval and elongated.

[0114] The thermoplastic polymer 102 may have a melting point or softening temperature of about 50°C to about 450°C (or about 50°C to about 125°C, or about 100°C to about 175°C, or about 150°C to about 280°C, or about 200°C to about 350°C, or about 300°C to about 450°C).

[0115] The thermoplastic polymer 102 may have a glass transition temperature of about -50°C to about 400°C (or about -50°C to about 0°C, or about -25°C to about 50°C, or about 0°C to about 150°C, or about 100°C to about 250°C, or about 150°C to about 300°C, or about 200°C to about 400°C) (using a heating and cooling rate of 10°C / min as specified in ASTM E1356-08 (2014)).

[0116] The thermoplastic polymer 102 may optionally contain additives. Typically, the additives are present before the thermoplastic polymer 102 is added to the mixture 110. Thus, in the thermoplastic polymer molten droplets and the resulting thermoplastic polymer particles, the additives are dispersed throughout the thermoplastic polymer. Accordingly, for clarity, these additives are referred to herein as “internal additives.” The internal additives may be blended with the thermoplastic polymer immediately before the mixture 110 or wells are prepared.

[0117] When describing the amounts of components in the compositions described herein (e.g., mixture 110 and thermoplastic polymer particles 122), the weight percentages are based on thermoplastic polymer 102 without internal additives. For example, a composition containing 1% by weight of emulsifying stabilizer per 100 g of thermoplastic polymer 102 containing 10% by weight of internal additives and 90% by weight of thermoplastic polymer is a composition containing 0.9 g of emulsifying stabilizer, 90 g of thermoplastic polymer, and 10 g of internal additives.

[0118] The internal additive may be present in the thermoplastic polymer 102 in an amount of about 0.1% to about 60% by weight (or about 0.1% to about 5% by weight, or about 1% to about 10% by weight, or about 5% to about 20% by weight, or about 10% to about 30% by weight, or about 25% to about 50% by weight, or about 40% to about 60% by weight) of the thermoplastic polymer 102. For example, the thermoplastic polymer 102 may consist of about 70% to about 85% by weight of the thermoplastic polymer and about 15% to about 30% by weight of the internal additive, such as glass fibers or carbon fibers.

[0119] Examples of internal additives include, but are not limited to, fillers, reinforcing agents, pigments, pH adjusters, and combinations thereof. Examples of fillers include, but are not limited to, glass fibers, glass particles, mineral fibers, carbon fibers, oxide particles (e.g., titanium dioxide and zirconium dioxide), metal particles (e.g., aluminum powder), and any combination thereof. Examples of pigments include, but are not limited to, organic pigments, inorganic pigments, carbon black, and any combination thereof.

[0120] The thermoplastic polymer 102 may be present in the mixture 110 in an amount of about 5% to about 60% by weight (or about 5% to about 25% by weight, or about 10% to about 30% by weight, or about 20% to about 45% by weight, or about 25% to about 50% by weight, or about 40% to about 60% by weight) of the combined thermoplastic polymer 102 and dispersion medium 104.

[0121] A suitable dispersion medium 104 has a viscosity of approximately 1,000 cSt to approximately 150,000 cSt (or approximately 1,000 cSt to approximately 60,000 cSt, or approximately 40,000 cSt to approximately 100,000 cSt, or approximately 75,000 cSt to approximately 150,000 cSt) at 25°C.

[0122] Examples of dispersion medium 104 include, but are not limited to, silicone oil, fluorinated silicone oil, perfluorinated silicone oil, polyethylene glycol, alkyl-terminated polyethylene glycol (e.g., C1-C4 terminal alkyl groups such as tetraethylene glycol dimethyl ether (TDG)), paraffin, liquid petrolatum, mink oil, turtle oil, soybean oil, perhydrosqualene, sweet almond oil, calophyllum oil, palm oil, pearl reem oil, grapeseed oil, sesame oil, corn oil, rapeseed oil, sunflower oil, cottonseed oil, apricot oil, castor oil, avocado oil, jojoba oil, olive oil, cereal germ oil, lanolinic acid esters, oleic acid esters, lauric acid esters, stearic acid esters, aliphatic esters, higher fatty acids, aliphatic alcohols, fatty acid-modified polysiloxanes, aliphatic alcohol-modified polysiloxanes, polyoxyalkylene-modified polysiloxanes, and any combination thereof. Examples of silicone oils, but not limited to, include polydimethylsiloxane, methylphenylpolysiloxane, alkyl-modified polydimethylsiloxane, alkyl-modified methylphenylpolysiloxane, amino-modified polydimethylsiloxane, amino-modified methylphenylpolysiloxane, fluorine-modified polydimethylsiloxane, fluorine-modified methylphenylpolysiloxane, polyether-modified polydimethylsiloxane, polyether-modified methylphenylpolysiloxane, and any combination thereof. If the dispersion medium 104 contains two or more of the above, the dispersion medium 104 may have one or more phases. For example, polysiloxanes modified with fatty acids and polysiloxanes modified with aliphatic alcohols (preferably having similar chain lengths to fatty acids and aliphatic alcohols) can form a single-phase dispersion medium 104. In another example, a dispersion medium 104 containing a silicone oil and alkyl-terminated polyethylene glycol can form a two-phase dispersion medium 104.

[0123] The dispersion medium 104 may be present in the mixture 110 in an amount of about 40% to about 95% by weight (or about 75% to about 95% by weight, or about 70% to about 90% by weight, or about 55% to about 80% by weight, or about 50% to about 75% by weight, or about 40% to about 60% by weight) of the combined thermoplastic polymer 102 and dispersion medium 104.

[0124] In some cases, the dispersion medium 104 is approximately 0.6 g / cm³. 3 ~Approx. 1.5g / cm 3 The density may be approximately 0.7 g / cm³ for the thermoplastic polymer 102. 3 ~Approx. 1.7g / cm 3 The thermoplastic polymer has a density similar to, lower than, or higher than that of the dispersion medium.

[0125] The emulsifying stabilizers used in the methods and compositions of this disclosure may include nanoparticles (e.g., oxide nanoparticles, carbon black, polymer nanoparticles, and combinations thereof), surfactants, and any combination thereof.

[0126] Oxide nanoparticles may be metal oxide nanoparticles, nonmetal oxide nanoparticles, or mixtures thereof. Examples of oxide nanoparticles include, but are not limited to, silica, titania, zirconia, alumina, iron oxide, copper oxide, tin oxide, boron oxide, cerium oxide, thallium oxide, and tungsten oxide, as well as any combination thereof. Mixed metal oxides and / or nonmetal oxides such as aluminosilicates, borosilicates, and aluminoborosilicates are also included in the term metal oxides. Oxide nanoparticles may be hydrophilic or hydrophobic, and may be natural particles or the result of surface treatment of particles. For example, silica nanoparticles having a hydrophobic surface treatment such as dimethylsilyl or trimethylsilyl may be used in the methods and compositions of this disclosure. In addition, silica with a functional surface treatment such as methacrylate functional groups may be used in the methods and compositions of this disclosure. Non-functionalized oxide nanoparticles may also be suitable for use.

[0127] Examples of commercially available silica nanoparticles include, but are not limited to, AEROSIL® (registered trademark) available from Evonik (e.g., AEROSIL® R812S (hydrophobic modified surface and 260±30m)). 2 Silica nanoparticles with an average diameter of approximately 7 nm and a BET surface area of ​​1 / g, AEROSIL® RX50 (hydrophobic modified surface and 35±10 m 2 Silica nanoparticles with an average diameter of approximately 40 nm and a BET surface area of ​​1 / g, AEROSIL® 380 (hydrophobic modified surface and 380±30m 2 Examples include silica nanoparticles having a surface area of ​​ / g, and any combination thereof.

[0128] Carbon black is another type of nanoparticle that may be present as an emulsifying stabilizer in the compositions and methods disclosed herein. Various grades of carbon black are familiar to those skilled in the art, and any of them may be used herein. Other nanoparticles capable of absorbing infrared radiation may be used similarly.

[0129] Polymer nanoparticles are another type of nanoparticle that may be present as emulsifying stabilizers in the disclosure herein. Suitable polymer nanoparticles may comprise one or more polymers that are thermosetting and / or crosslinked so as not to melt when treated by melt emulsification as disclosed herein. High molecular weight thermoplastic polymers having high melting or decomposition points may similarly comprise suitable polymer nanoparticle emulsifying stabilizers.

[0130] Nanoparticles may have an average diameter (D50 based on volume) of approximately 1 nm to approximately 500 nm (or approximately 10 nm to approximately 150 nm, or approximately 25 nm to approximately 100 nm, or approximately 100 nm to approximately 250 nm, or approximately 250 nm to approximately 500 nm).

[0131] The nanoparticles are approximately 10m 2 / g~about 500m 2 / g (or approximately 10m) 2 / g~about 150m 2 / g, or approximately 25m 2 / g~about 100m 2 / g, or approximately 100m 2 / g ~ approx. 250m 2 / g, or 250m 2 / g~about 500m 2 It may have a BET surface area of ​​( / g).

[0132] Nanoparticles may be present in the mixture 110 at concentrations of about 0.01% to about 10% by weight (or about 0.01% to about 1% by weight, or about 0.1% to about 3% by weight, or about 1% to about 5% by weight, or about 5% to about 10% by weight) based on the weight of the thermoplastic polymer 102.

[0133] Surfactants can be anionic, cationic, nonionic, or dipolar ionic. Examples of surfactants include, but are not limited to, sodium dodecyl sulfate, sorbitan oleate, poly[dimethylsiloxane-co-[[3-(2-(2-hydroxyethoxy)ethoxy)propylmethylsiloxane], sodium docusate (sodium 1,4-bis(2-ethylhexoxy)-1,4-dioxobutane-2-sulfonate), and any combination thereof. Examples of commercially available surfactants include, but are not limited to, CALFAX® DB-45 (sodium dodecyldiphenyl oxide disulfonate, available from Pilot Chemicals), SPAN® 80 (sorbitan maleate nonionic surfactant), MERPOL® surfactant (available from Stepan Company), TERGITOL® TMN-6 (water-soluble nonionic surfactant, available from DOW), TRITON® X-100 (octylphenol ethoxylate, available from Sigma-Aldrich), IGEPAL® CA-520 (polyoxyethylene(5) isooctylphenyl ether, available from Sigma-Aldrich), BRIJ® S10 (polyethylene glycol octadecyl ether, available from Sigma-Aldrich), and any combination thereof.

[0134] The surfactant may be present in mixture 110 at a concentration of about 0.01% to about 10% by weight (or about 0.01% to about 1% by weight, or about 0.5% to about 2% by weight, or about 1% to about 3% by weight, or about 2% to about 5% by weight, or about 5% to about 10% by weight) based on the weight of polyamide 102. Alternatively, mixture 110 may not contain (or may be absent from) the surfactant.

[0135] The weight ratio of nanoparticles to surfactant may be approximately 1:10 to approximately 10:1 (or approximately 1:10 to approximately 1:1, or approximately 1:5 to approximately 5:1, or approximately 1:1 to approximately 10:1).

[0136] As described above, components 102, 104, and 106 may be added in any order and may include mixing and / or heating in process 108 containing components 102, 104, and 106. For example, the emulsifying stabilizer 106 may first be dispersed in the dispersion medium 104 before the addition of the thermoplastic polymer 102, optionally accompanied by heating of the dispersion. In another non-limiting example, the thermoplastic polymer 102 may be heated to produce a polymer melt to which the dispersion medium 104 and the emulsifying stabilizer 106 are added together or in any order. In yet another non-limiting example, the thermoplastic polymer 102 and the carrier fluid 104 may be mixed at a temperature above the melting point or softening temperature of the thermoplastic polymer 102 and at a shear rate sufficient to disperse the thermoplastic polymer melt in the carrier fluid 104. The emulsifying stabilizer 106 is then added to form a mixture 110 and may be maintained under suitable process conditions for a set period of time.

[0137] The combination of components 102, 104, and 106 in any combination (108) may be performed in the mixing apparatus used in process 112 and / or in another suitable container. In non-limiting examples, the thermoplastic polymer 102 may be heated to a temperature above its melting point or softening temperature in the mixing apparatus used in process 112, and the emulsifying stabilizer 106 may be dispersed in the dispersion medium 104 in a separate container. The dispersion may then be added to the molten thermoplastic polymer 102 in the mixing apparatus used in process 112.

[0138] The mixing apparatus used in process 112 to produce the molten emulsion 114 should be able to maintain the molten emulsion 114 at a temperature above the melting point or softening temperature of the thermoplastic polymer 102 and apply a shear rate sufficient to disperse the polymer melt as droplets in the dispersion medium 104.

[0139] Examples of mixing equipment used in the process 112 for producing the molten emulsion 114 include, but are not limited to, extruders (e.g., continuous extruders, batch extruders, etc.), agitated reactors, blenders, reactors equipped with inline homogenizer systems, and equipment derived therefrom.

[0140] Processing 112 under suitable process conditions (e.g., temperature, shear rate, etc.) for a set period of time and formation of a molten emulsion 114.

[0141] The temperature at which the treatment 112 and the molten emulsion 114 are formed should be above the melting point or softening temperature of the thermoplastic polymer 102, and below the decomposition temperature of any of the components 102, 104, and 106 in the mixture 110. For example, if the temperature at which the treatment 112 and the molten emulsion 114 are formed is below the decomposition temperature of any of the components 102, 104, and 106 in the mixture 110, the temperature at which the treatment 112 and the molten emulsion 114 are formed may exceed the melting point or softening temperature of the thermoplastic polymer 102 by about 1°C to about 50°C (or about 1°C to about 25°C, or about 5°C to about 30°C, or about 20°C to about 50°C).

[0142] The shear rate of the process 112 and the formation of the molten emulsion 114 should be high enough to disperse the polymer melt as droplets in the dispersion medium 104. The droplets should include droplets with a diameter of about 1000 μm or less (or about 1 μm to about 1000 μm, or about 1 μm to about 50 μm, or about 10 μm to about 100 μm, or about 10 μm to about 250 μm, or about 50 μm to about 500 μm, or about 250 μm to about 750 μm, or about 500 μm to about 1000 μm).

[0143] The time for maintaining the temperature and shear rate for the process 112 and the formation of the molten emulsion 114 may be 10 seconds to 18 hours or more (or 10 seconds to 30 minutes, or 5 minutes to 1 hour, or 15 minutes to 2 hours, or 1 hour to 6 hours, or 3 hours to 18 hours). Although not bound by theory, it is thought that a steady state of droplet diameter is reached at a point when the process 112 can be stopped. This time may depend, in particular, on the temperature, shear rate, the composition of the thermoplastic polymer 102, the composition of the dispersion medium 104, and the composition of the emulsifying stabilizer 106.

[0144] The molten emulsion 114 may then be cooled in 116. Cooling in 116 can be slow (e.g., allowing the molten emulsion to be cooled under ambient conditions) or fast (e.g., rapid cooling). For example, the cooling rate may range from about 10°C / hour to about 100°C / second, or even nearly instantaneous by rapid cooling (e.g., dry ice) (or about 10°C / hour to about 60°C / hour, or about 0.5°C / min to about 20°C / min, or about 1°C / min to about 5°C / min, or about 10°C / min to about 60°C / min, or about 0.5°C / second to about 10°C / second, or about 10°C / second to about 100°C / second).

[0145] During cooling, shear force may be applied little to no to the molten emulsion 114. In some cases, the shear force applied during heating may be applied during cooling.

[0146] The cooled mixture 118 obtained from the cooling 116 of the molten emulsion 114 comprises solidified thermoplastic polymer particles 122 (or simply thermoplastic polymer particles) and other components 124 (e.g., dispersion medium 104, excess emulsion stabilizer 106, etc.). The thermoplastic polymer particles may be dispersed in the dispersion medium or settled in the dispersion medium.

[0147] The cooled mixture 118 may then be treated to separate thermoplastic polymer particles 122 (or simply thermoplastic polymer particles 122) from the other components 124 (120). Suitable treatments include, but are not limited to, washing, filtering, centrifugation, and decanting, as well as any combination thereof.

[0148] The solvent used to wash the thermoplastic polymer particles 122 should generally be (a) miscible with the dispersion medium 104 and (b) nonreactive with the thermoplastic polymer 102 (e.g., non-swelling and non-melting). The choice of solvent will depend, in particular, on the composition of the dispersion medium and the composition of the thermoplastic polymer 102.

[0149] Examples of solvents, but not limited to, include hydrocarbon solvents (e.g., pentane, hexane, heptane, octane, cyclohexane, cyclopentane, decane, dodecane, tridecane, and tetradecane), aromatic hydrocarbon solvents (e.g., benzene, toluene, xylene, 2-methylnaphthalene, and cresol), ether solvents (e.g., diethyl ether, tetrahydrofuran, diisopropyl ether, and dioxane), ketone solvents (e.g., acetone and methyl ethyl ketone), alcohol solvents (e.g., methanol, ethanol, isopropanol, and n-propanol), ester solvents (e.g., ethyl acetate, methyl acetate, butyl acetate, butyl propionate, and butyl butyrate), halogenated solvents (e.g., chloroform, bromoform, 1,2-dichloromethane, 1,2-dichloroethane, carbon tetrachloride, chlorobenzene, and hexafluoroisopropanol), water, and any combination thereof.

[0150] The solvent may be removed from the thermoplastic polymer particles 122 by drying using a suitable method such as air drying, heat drying, vacuum drying, freeze-drying, or a hybrid thereof. Heating may preferably be carried out at a temperature lower than the glass transition temperature of the thermoplastic polymer (e.g., about 50°C to about 150°C).

[0151] The thermoplastic polymer particles 122, after being separated from the other components 124, may optionally be further sorted to produce purified thermoplastic polymer particles 128. For example, to narrow the particle size distribution (or reduce the diameter span), the thermoplastic polymer particles 122 may be passed through a sieve having a pore size of about 10 μm to about 250 μm (or about 10 μm to about 100 μm, or about 50 μm to about 200 μm, or about 150 μm to about 250 μm).

[0152] In another example of the purification technique, the thermoplastic polymer particles 122 may be washed with water to remove the surfactant while retaining substantially all nanoparticles associated on the surface of the thermoplastic polymer particles 122. In yet another example of the purification technique, the thermoplastic polymer particles 122 may be blended with additives to obtain the desired final product. For clarity, such additives are blended with the thermoplastic polymer particles 122 or other particles obtained by the method described herein after the particles have solidified, and are therefore referred to herein as “external additives.” Examples of external additives include flow aids, other polymer particles, fillers, and any combination thereof.

[0153] In some cases, the surfactants used in the production of the thermoplastic polymer particles 122 may be unnecessary in downstream applications. Accordingly, yet another example of purification techniques may include removing the surfactants from the thermoplastic polymer particles 122 (e.g., by washing and / or thermal decomposition), at least substantially.

[0154] Thermoplastic polymer particles 122 and / or purified thermoplastic polymer particles 128 (referred to as particles 122 / 128) may be characterized by their composition, physical structure, etc.

[0155] As described above, the emulsifying stabilizer is located at the interface between the polymer molten material and the dispersion medium. As a result, when the mixture cools, the emulsifying stabilizer remains at or near this interface. Therefore, the structure of particles 122 / 128 generally includes (a) an emulsifying stabilizer dispersed on the outer surface of particles 122 / 128 and / or (b) an emulsifying stabilizer embedded in the outer portion of particles 122 / 128 (e.g., the outer 1 vol%).

[0156] Furthermore, if voids are formed inside the polymer molten droplets, the emulsifying stabilizer 106 should generally be present (and / or embedded) at the interface between the inside of the void and the thermoplastic polymer. The voids generally do not contain the thermoplastic polymer. Rather, the voids may contain, for example, the dispersion medium, air, or be empty. The particles 122 / 128 may contain the dispersion medium in an amount of about 5% by weight or less of the particles 122 / 128 (or about 0.001% by weight to about 5% by weight, or about 0.001% by weight to about 0.1% by weight, or about 0.01% by weight to about 0.5% by weight, or about 0.1% by weight to about 2% by weight, or about 1% by weight to about 5% by weight).

[0157] Thermoplastic polymer 102 may be present in particles 122 / 128 in an amount of about 90% to about 99.5% by weight (or about 90% to about 95% by weight, or about 92% to about 97% by weight, or about 95% to about 99.5% by weight) of particles 122 / 128.

[0158] If present, the emulsifying stabilizer 106 may be present in particles 122 / 128 in amounts of about 10% by weight or less (or about 0.01% to about 10% by weight, or about 0.01% to about 1% by weight, or about 0.5% to about 5% by weight, or about 3% to about 7% by weight, or about 5% to about 10% by weight). If purified to remove at least substantially any surfactant or other emulsifying stabilizer, the emulsifying stabilizer 106 may be present in particles 128 in amounts of less than 0.01% by weight (or 0% to about 0.01% by weight, or 0% to 0.001% by weight).

[0159] When forming thermoplastic microparticles according to the disclosure herein, at least a portion of the nanoparticles, such as silica nanoparticles, may be arranged as a coating on the outer surface of the thermoplastic microparticles. At least a portion of the surfactant, if used, may similarly associate on the outer surface. The coating may be distributed substantially uniformly on the outer surface. As used herein with respect to coatings, the term “substantially uniform” means a uniform coating thickness at surface locations covered by the coating composition (e.g., nanoparticles and / or surfactant), in particular the entire outer surface. The emulsifying stabilizer 106 may form a coating covering at least 5% (or about 5% to about 100%, or about 5% to about 25%, or about 20% to about 50%, or about 40% to about 70%, or about 50% to about 80%, or about 60% to about 90%, or about 70% to about 100%) of the surface area of ​​the particles 122 / 128. If purified to remove at least substantially any surfactant or other emulsifying stabilizer, the emulsifying stabilizer 106 may be present in particles 128 in an area of ​​less than 25% of the surface area of ​​particle 128 (or 0% to about 25%, or about 0.1% to about 5%, or about 0.1% to about 1%, or about 1% to about 5%, or about 1% to about 10%, or about 5% to about 15%, or about 10% to about 25%). The coverage of the emulsifying stabilizer 106 on the outer surface of particles 122 / 128 may be determined using image analysis of scanning electron microscope (SEM) images. The emulsifying stabilizer 106 may form a coating that covers at least 5% (or about 5% to about 100%, or about 5% to about 25%, or about 20% to about 50%, or about 40% to about 70%, or about 50% to about 80%, or about 60% to about 90%, or about 70% to about 100%) of the surface area of ​​particles 122 / 128. If purified to remove at least substantially any surfactant or other emulsifying stabilizer, the emulsifying stabilizer 106 may be present in particles 128 in amounts less than 25% (or 0% to about 25%, or about 0.1% to about 5%, or about 0.1% to about 1%, or about 1% to about 5%, or about 1% to about 10%, or about 5% to about 15%, or about 10% to about 25%) of the surface area of ​​particles 128. The coverage rate of the emulsifying stabilizer 106 on the outer surface of particles 122 / 128 can be determined using image analysis of SEM microscope photographs.

[0160] Particles 122 / 128 can have a D10 of about 0.1 μm to about 125 μm (or about 0.1 μm to about 5 μm, about 1 μm to about 10 μm, about 5 μm to about 30 μm, or about 1 μm to about 25 μm, or about 25 μm to about 75 μm, or about 50 μm to about 85 μm, or about 75 μm to about 125 μm), a D50 of about 0.5 μm to about 200 μm (or about 0.5 μm to about 10 μm, or about 5 μm to about 50 μm, or about 30 μm to about 100 μm, or about 30 μm to about 70 μm, or about 25 μm to about 50 μm, or about 50 μm to about 100 μm, or about 75 μm to about 150 μm, or about 100 μm to about 200 μm), and a D90 of about 3 μm to about 300 μm (or about 3 μm to about 15 μm, or about 10 μm to about 50 μm, or about 25 μm to about 75 μm, or about 70 μm to about 200 μm, or about 60 μm to about 150 μm, or about 150 μm to about 300 μm), with D10 < D50 < D90. Particles 122 / 128 can also have a diameter span of about 0.4 to about 3 (or about 0.6 to about 2, or about 0.4 to about 1.5, or about 1 to about 3). Without limitation, a diameter span value of 1.0 or greater is considered wide, and a diameter span value of 0.75 or less is considered narrow. For example, particles 122 / 128 can have a D10 of about 5 μm to about 30 μm, a D50 of about 30 μm to about 100 μm, and a D90 of about 70 μm to about 120 μm, with D10 < D50 < D90.

[0161] Particles 122 / 128 can also have a diameter span of about 0.4 to about 3 (or about 0.6 to about 2, or about 0.4 to about 1.5, or about 1 to about 3).

[0162] In a first non-limiting example, particles 122 / 128 can have a D10 of about 0.5 μm to about 5 μm, a D50 of about 0.5 μm to about 10 μm, and a D90 of about 3 μm to about 15 μm, with D10 < D50 < D90.

[0163] In a second non-limiting example, particles 122 / 128 can have a D10 of about 1 μm to about 50 μm, a D50 of about 25 μm to about 100 μm, and a D90 of about 60 μm to about 300 μm, with D10 < D50 < D90.

[0164] In a third non-limiting example, the particles 122 / 128 may have a D10 of about 5 μm to about 30 μm, a D50 of about 30 μm to about 70 μm, and a D90 of about 70 μm to about 120 μm, with D10 < D50 < D90. The particles 122 / 128 may have a diameter span of about 1.0 to about 2.5.

[0165] In a fourth non-limiting example, the particles 122 / 128 may have a D10 of about 25 μm to about 60 μm, a D50 of about 60 μm to about 110 μm, and a D90 of about 110 μm to about 175 μm, with D10 < D50 < D90. The particles 122 / 128 may have a diameter span of about 0.6 to about 1.5.

[0166] In a fifth non-limiting example, the particles 122 / 128 may have a D10 of about 75 μm to about 125 μm, a D50 of about 100 μm to about 200 μm, and a D90 of about 125 μm to about 300 μm, with D10 < D50 < D90. The particles 122 / 128 may have a diameter span of about 0.2 to about 1.2.

[0167] The particles 122 / 128 may have a circularity of about 0.7 or more (or about 0.90 to about 1.0, or about 0.93 to about 0.99, or about 0.95 to about 0.99, or about 0.97 to about 0.99, or about 0.98 to 1.0).

[0168] The particles 122 / 128 may have an angle of repose of about 25° to about 45° (or about 25° to about 35°, or about 30° to about 40°, or about 35° to about 45°).

[0169] The particles 122 / 128 may have a Hausner ratio of about 1.0 to about 1.5 (or about 1.0 to about 1.2, or about 1.1 to about 1.3, or about 1.2 to about 1.35, or about 1.3 to about 1.5).

[0170] The particles 122 / 128 may have a density of about 0.3 g / cm 3 ~ about 0.8 g / cm 3 (or about 0.3 g / cm 3 ~ about 0.6 g / cm 3 , or about 0.4 g / cm 3 ~ about 0.7 g / cm3 , or approximately 0.5 g / cm³ 3 ~about 0.6g / cm 3 , or approximately 0.5 g / cm³ 3 ~about 0.8g / cm 3 It may have a bulk density of ).

[0171] Depending on the temperature and shear rate of the process 112, and the composition and relative concentration of components 102, 104, and 106, different shapes of the structures constituting the particles 122 / 128 have been observed. Typically, particles 122 / 128 include substantially spherical particles (with a circularity of about 0.97 or greater). However, other structures, including disk structures and elongated structures, have been observed in particles 122 / 128. Thus, particles 122 / 128 may include one or more of the following: (a) substantially spherical particles with a circularity of 0.97 or greater, (b) disk structures with an aspect ratio of about 2 to about 10, and (c) elongated structures with an aspect ratio of 10 or greater. Each of the above structures (a), (b), and (c) has an emulsifying stabilizer dispersed on the outer surface of the (a), (b), and (c) structure, and / or an emulsifying stabilizer embedded in the outer portion of the (a), (b), and (c) structure. At least some of the structures (a), (b), and (c) can aggregate. For example, the elongated structure of (c) may be located on the surface of the substantially spherical particles of (a).

[0172] Particles 122 / 128 may have a sintering window of thermoplastic polymer 102 within 10°C, preferably within 5°C.

[0173] Non-restrictive examples

[0174] A first non-limiting exemplary embodiment of the present disclosure is a composition comprising particles comprising an unsaturated polyamide and an initiator. The first non-limiting exemplary embodiment includes Element 1: the particles have a circularity of about 0.9 to about 1.0, Element 2: the weight ratio of the unsaturated polyamide to the initiator is about 90:10 to about 99:1, Element 3: the particles further comprise an infrared absorber, Element 4: the composition further comprises an infrared absorber mixed with the particles, Element 5: the particles further comprise a thermoplastic polymer other than the unsaturated polyamide, Element 6: the particles further comprise an emulsifying stabilizer associated with the outer surface of the particles, Element 7: Element 6, wherein at least some of the particles have voids containing the emulsifying stabilizer at the void / polymer interface, Element 8: Element 6, wherein the emulsifying stabilizer comprises nanoparticles, and the nanoparticles are embedded in the outer surface of the particles, Element 9: the particles have a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, and a D90 of about 3 μm to about 300 μm, with D10 < D50 < D90, Element 10: the particles have a diameter span of about 0.2 to about 10, and Element 11: the solidified particles have a Hausner ratio of about 1.0 to about 1.5, and may further include one or more of the above. Examples of combinations include, but are not limited to, Element 1 combined with one or more of Elements 2 to 11, Element 2 combined with one or more of Elements 3 to 11, Element 3 combined with one or more of Elements 4 to 11, Element 4 combined with one or more of Elements 5 to 11, Element 6 (optionally combined with Element 7 and / or Element 8) combined with one or more of Elements 9 to 11, and combinations of two or more of Elements 9 to 11.

[0175] A second non-limiting exemplary embodiment includes depositing the composition of the first non-limiting exemplary embodiment (optionally having one or more of Elements 1 to 11) on a surface, optionally in combination with other thermoplastic polymer particles, and after deposition, heating at least a portion of the particles to promote their consolidation and crosslinking of the unsaturated polyamide, thereby forming a consolidated body comprising a crosslinked polyamide.

[0176] A third non-limiting exemplary embodiment is a method comprising: mixing a mixture comprising an unsaturated polyamide, a dispersion medium immiscible with the unsaturated polyamide, and optionally an emulsifying stabilizer at a temperature above the melting or softening temperature of the unsaturated polyamide and at a shear rate sufficiently high to disperse the unsaturated polyamide in the dispersion medium; and cooling the mixture to below the melting or softening temperature of the unsaturated polyamide to form unsaturated polyamide particles comprising the unsaturated polyamide and, if present, an emulsifying stabilizer associated on the outer surface of the unsaturated polyamide particles. A first non-limiting exemplary embodiment further comprises: Element 1, Element 9, Element 10, Element 11, Element 12: The method further comprises dry blending unsaturated polyamide particles with an initiator, wherein the weight ratio of unsaturated polyamide to initiator is about 90:10 to about 99:1; Element 13: The method further comprises wet blending unsaturated polyamide particles with an initiator, wherein the weight ratio of unsaturated polyamide to initiator is about 90:10 to about 99; Element 14: The initiator is a photoinitiator; Element 15: The initiator is a thermal initiator; Element 16: The mixture is Element 17: The mixture further comprises a thermoplastic polymer that is not an unsaturated polyamide; Element 18: The mixture contains an emulsifying stabilizer, the emulsifying stabilizer is associated with the outer surface of the unsaturated polyamide particles; Element 19: The mixture of Element 18, wherein the emulsifying stabilizer contains nanoparticles, the nanoparticles are embedded in the outer surface of the unsaturated polyamide particles; and Element 20: The mixture further comprises an initiator, the weight ratio of the initiator to the unsaturated polyamide being about 90:10 to about 99:1, and may further comprise one or more of these.Examples of combinations, though not limited to them, include combinations of two or more elements from 12, 13, and 20; element 1 combined with one or more elements from 9 to 20; element 9 combined with one or more elements from 10 to 20; element 10 combined with one or more elements from 11 to 20; element 11 combined with one or more elements from 12 to 20; element 12 combined with one or more elements from 13 to 20; element 13 combined with one or more elements from 14 to 20; element 14 combined with one or more elements from 15 to 20; element 15 combined with one or more elements from 16 to 20; element 16 combined with one or more elements from 17 to 20; and combinations of two or more elements from 18 to 20.

[0177] A fourth non-limiting exemplary embodiment is a method comprising emulsion polymerization via polycondensation and / or ring-opening reaction between a first polyamide monomer and a second polyamide monomer, wherein the second polyamide monomer comprises at least one unsaturated aliphatic carbon-carbon bond for producing an unsaturated polyamide; precipitation of the unsaturated polyamide as particles; and blending the particles containing the unsaturated polyamide with an initiator. The fourth non-limiting exemplary embodiment may further comprise one or more of the following: element 21: blend comprises a dry blend; element 22: blend comprises a wet blend; element 23: initiator is a photoinitiator; element 24: initiator is a thermal initiator; and element 25: method further comprises blending the particles containing the unsaturated polyamide with an infrared absorber.

[0178] A fifth non-limiting exemplary embodiment is a method comprising dissolving an unsaturated polyamide in a solvent, precipitating the unsaturated polyamide as particles, and blending the particles containing the unsaturated polyamide with an initiator. The fifth non-limiting exemplary embodiment may include one or more of the following: element 26: the blend comprises a dry blend; element 27: the blend comprises a wet blend; element 28: the initiator is a photoinitiator; element 29: the initiator is a thermal initiator; and element 30: the method further comprises blending the particles containing the unsaturated polyamide with an infrared absorber.

[0179] A sixth non-limiting exemplary embodiment is a method comprising dissolving an unsaturated polyamide in a solvent, precipitating the unsaturated polyamide as particles, and blending the particles containing the unsaturated polyamide with an initiator. The sixth non-limiting exemplary embodiment may include one or more of the following: element 31: the blend comprises a dry blend; element 32: the blend comprises a wet blend; element 33: the initiator is a photoinitiator; element 34: the initiator is a thermal initiator; and element 35: the method further comprises blending the particles containing the unsaturated polyamide with an infrared absorber.

[0180] A seventh non-limiting exemplary embodiment is a method comprising dissolving an unsaturated polyamide and an initiator in a solvent, and precipitating the unsaturated polyamide to obtain particles comprising the unsaturated polyamide and the initiator. The seventh non-limiting exemplary embodiment may include one or more of the following: element 36: further comprising dry blending particles comprising the unsaturated polyamide and the initiator with another initiator (same as or different from the initiator); element 37: further comprising wet blending particles comprising the unsaturated polyamide and the initiator with another initiator (same as or different from the initiator); element 38: the initiator is a photoinitiator; element 39: the initiator is a thermal initiator; and element 40: the method further comprising blending particles comprising the unsaturated polyamide and the initiator with an infrared absorber.

[0181] An eighth non-limiting exemplary embodiment is a method comprising: cooling an unsaturated polyamide to a low temperature; milling the low-temperature cooled unsaturated polyamide to obtain particles; and blending the particles containing the unsaturated polyamide with an initiator. A sixth non-limiting exemplary embodiment may include one or more of the following: element 41: the blend comprises a dry blend; element 42: the blend comprises a wet blend; element 43: the initiator is a photoinitiator; element 44: the initiator is a thermal initiator; and element 45: the method further comprises blending the particles containing the unsaturated polyamide with an infrared absorber.

[0182] A ninth non-limiting exemplary embodiment is a method comprising: chilling an unsaturated polyamide to a low temperature in the presence of an initiator; and milling the chilled unsaturated polyamide to obtain particles comprising the unsaturated polyamide and the initiator. The ninth non-limiting exemplary embodiment may further comprise one or more of the following: element 46: dry blending particles comprising the unsaturated polyamide and the initiator with another initiator (same as or different from the initiator); element 47: wet blending particles comprising the unsaturated polyamide and the initiator with another initiator (same as or different from the initiator); element 48: the initiator is a photoinitiator; element 49: the initiator is a thermal initiator; and element 50: the method further comprises blending particles comprising the unsaturated polyamide and the initiator with an infrared absorber.

[0183] A tenth non-limiting exemplary embodiment is a method comprising: melt emulsifying an unsaturated polyamide; cooling the melt emulsified mixture to obtain particles; and blending the particles containing the unsaturated polyamide with an initiator. The tenth non-limiting exemplary embodiment may further include one or more of the following: element 51: the blend comprises a dry blend; element 52: the blend comprises a wet blend; element 53: the initiator is a photoinitiator; element 54: the initiator is a thermal initiator; and element 55: the method further comprises blending the particles containing the unsaturated polyamide with an infrared absorber.

[0184] An eleventh non-limiting exemplary embodiment is a method comprising melt emulsifying an unsaturated polyamide in the presence of an initiator, and cooling the melt emulsified to obtain particles comprising the unsaturated polyamide and the initiator. The eleventh non-limiting exemplary embodiment may further comprise one or more of the following: element 56: dry blending particles comprising the unsaturated polyamide and the initiator with another initiator (same as or different from the initiator); element 57: wet blending particles comprising the unsaturated polyamide and the initiator with another initiator (same as or different from the initiator); element 58: the initiator is a photoinitiator; element 59: the initiator is a thermal initiator; and element 60: the method further comprises blending particles comprising the unsaturated polyamide and the initiator with an infrared absorber.

[0185] An additional non-limiting exemplary embodiment is a method comprising depositing a composition prepared according to one or more of the 4th to 11th non-limiting exemplary embodiments onto a surface in optional combination with other thermoplastic polymer particles, and after deposition, heating at least a portion of the particles to promote their compaction and crosslinking of the unsaturated polyamide, thereby forming a compacted body containing the crosslinked polyamide.

[0186] Clause

[0187] Clause 1. A composition comprising particles containing an unsaturated polyamide and an initiator.

[0188] Clause 2. The composition according to Clause 1, wherein the particles have a circularity of about 0.9 to about 1.0.

[0189] Clause 3. The composition according to Clause 1, wherein the weight ratio of the unsaturated polyamide to the initiator is about 90:10 to about 99:1.

[0190] Clause 4. The composition according to Clause 1, wherein the particles further comprise an infrared absorbent.

[0191] Clause 5. The composition according to Clause 1, further comprising an infrared absorbent mixed with particles.

[0192] Clause 6. The composition according to Clause 1, wherein the particles further comprise a thermoplastic polymer that is not an unsaturated polyamide.

[0193] Clause 7. The composition according to Clause 1, further comprising an emulsifying stabilizer associated with the outer surface of the particles.

[0194] Clause 8. The composition according to Clause 7, wherein at least some of the particles have voids containing an emulsifying stabilizer at the void / polymer interface.

[0195] Clause 9. The composition according to Clause 7, wherein the emulsifying stabilizer comprises nanoparticles, the nanoparticles being embedded on the outer surface of the particles.

[0196] Clause 10. A method comprising depositing the composition described in Clause 1 on a surface in an optional combination with other thermoplastic polymer particles, and after deposition, heating at least a portion of the particles to promote densification and crosslinking of the unsaturated polyamide, thereby forming a compacted body containing a crosslinked polyamide.

[0197] Clause 11. A method comprising: mixing a mixture containing an unsaturated polyamide, an unsaturated polyamide-immiscible dispersion medium, and optionally an emulsifying stabilizer at a temperature above the melting or softening temperature of the unsaturated polyamide and at a shear rate sufficiently high to disperse the unsaturated polyamide in the dispersion medium; and cooling the mixture to below the melting or softening temperature of the unsaturated polyamide to form unsaturated polyamide particles containing the unsaturated polyamide and, if present, an emulsifying stabilizer associated on the outer surface of the unsaturated polyamide particles.

[0198] Clause 12. The method according to Clause 11, further comprising dry blending unsaturated polyamide particles with an initiator, wherein the weight ratio of the unsaturated polyamide to the initiator is about 90:10 to about 99:1.

[0199] Clause 13. The method according to Clause 11, further comprising wet blending unsaturated polyamide particles with an initiator, wherein the weight ratio of the unsaturated polyamide to the initiator is about 90:10 to about 99:1.

[0200] Clause 14. The method according to Clause 11, wherein the initiator is a photoinitiator.

[0201] Clause 15. The method according to Clause 11, wherein the initiator is a thermal initiator.

[0202] Clause 16. The method according to Clause 11, wherein the mixture further comprises a thermoplastic polymer that is not an unsaturated polyamide.

[0203] Clause 17. The method according to Clause 11, wherein the mixture further comprises an infrared absorbent.

[0204] Clause 18. The method according to Clause 11, wherein the emulsifying stabilizer is contained in the mixture and the emulsifying stabilizer is associated with the outer surface of the unsaturated polyamide particles.

[0205] Clause 19. The method according to Clause 18, wherein the emulsifying stabilizer comprises nanoparticles, the nanoparticles being embedded on the outer surface of unsaturated polyamide particles.

[0206] Clause 20. The method according to Clause 11, wherein the mixture further comprises an initiator, and the weight ratio of the initiator to the unsaturated polyamide is about 90:10 to about 99:1.

[0207] Clause 21. A method comprising emulsion polymerization via polycondensation and / or ring-opening reaction between a first polyamide monomer and a second polyamide monomer, wherein the second polyamide monomer comprises at least one unsaturated aliphatic carbon-carbon bond for producing an unsaturated polyamide; precipitation of the unsaturated polyamide as particles; and blending the particles containing the unsaturated polyamide with an initiator.

[0208] Clause 22. The method according to Clause 21, wherein the blend includes a dry blend.

[0209] Clause 23. The method described in Clause 21, wherein the blend includes a wet blend.

[0210] Clause 24. The method according to Clause 21, wherein the initiator is a photoinitiator.

[0211] Clause 25. The method according to Clause 21, wherein the initiator is a thermal initiator.

[0212] Clause 26. The method according to Clause 21, further comprising blending particles containing an unsaturated polyamide with an infrared absorber.

[0213] Clause 27. A method comprising: dissolving an unsaturated polyamide in a solvent; precipitating the unsaturated polyamide as particles; and blending the particles containing the unsaturated polyamide with an initiator.

[0214] Clause 28. The method of Clause 27, wherein the blend includes a dry blend.

[0215] Clause 29. The method of Clause 27, wherein the blend includes a wet blend.

[0216] Clause 30. The method according to Clause 27, wherein the initiator is a photoinitiator.

[0217] Clause 31. The method according to Clause 27, wherein the initiator is a thermal initiator.

[0218] Clause 32. The method according to Clause 27, further comprising blending particles containing an unsaturated polyamide with an infrared absorber.

[0219] Article 33. Method,

[0220] Dissolving the unsaturated polyamide and initiator in a solvent,

[0221] A method comprising precipitating an unsaturated polyamide to obtain particles containing the unsaturated polyamide and an initiator.

[0222] Clause 34. The method according to Clause 33, further comprising dry blending particles containing an unsaturated polyamide and an initiator with a second initiator.

[0223] Clause 35. The method according to Clause 33, further comprising wet blending particles containing an unsaturated polyamide and an initiator with a second initiator.

[0224] Clause 36. The method according to Clause 33, wherein the initiator is a photoinitiator.

[0225] Clause 37. The method according to Clause 33, wherein the initiator is a thermal initiator.

[0226] Clause 38. The method according to Clause 33, further comprising blending particles containing an unsaturated polyamide and an initiator with an infrared absorber.

[0227] Clause 39. A method comprising: cooling an unsaturated polyamide to a low temperature; milling the cooled unsaturated polyamide to obtain particles; and blending the particles containing the unsaturated polyamide with an initiator.

[0228] Clause 40. The method described in Clause 39, wherein the blend includes a dry blend.

[0229] Clause 41. The method described in Clause 39, wherein the blend includes a wet blend.

[0230] Clause 42. The method according to Clause 39, wherein the initiator is a photoinitiator.

[0231] Clause 43. The method according to Clause 39, wherein the initiator is a thermal initiator.

[0232] Clause 44. The method according to Clause 39, further comprising blending particles containing an unsaturated polyamide with an infrared absorber.

[0233] Clause 45. A method comprising: cooling an unsaturated polyamide to a low temperature in the presence of an initiator; and milling the low-temperature cooled unsaturated polyamide to obtain particles containing the unsaturated polyamide and the initiator.

[0234] Clause 46. The method according to Clause 45, further comprising dry blending particles containing an unsaturated polyamide and an initiator with a second initiator.

[0235] Clause 47. The method according to Clause 45, further comprising wet blending particles containing an unsaturated polyamide and an initiator with a second initiator.

[0236] Clause 48. The method according to Clause 45, wherein the initiator is a photoinitiator.

[0237] Clause 49. The method according to Clause 45, wherein the initiator is a thermal initiator.

[0238] Clause 50. The method according to Clause 45, further comprising blending particles containing an unsaturated polyamide and an initiator with an infrared absorber.

[0239] Clause 51. A method comprising: melt emulsifying an unsaturated polyamide; cooling the melt emulsified mixture to obtain particles; and blending the particles containing the unsaturated polyamide with an initiator.

[0240] Clause 52. The method according to Clause 51, wherein the blend includes a dry blend.

[0241] Clause 53. The method according to Clause 51, wherein the blend includes a wet blend.

[0242] Clause 54. The method according to Clause 51, wherein the initiator is a photoinitiator.

[0243] Clause 55. The method according to Clause 51, wherein the initiator is a thermal initiator.

[0244] Clause 56. The method according to Clause 51, further comprising blending particles containing an unsaturated polyamide with an infrared absorber.

[0245] Clause 57. A method comprising: melt emulsifying an unsaturated polyamide in the presence of an initiator; and cooling the melt emulsified mixture to obtain particles containing the unsaturated polyamide and the initiator.

[0246] Clause 28. The method according to Clause 57, further comprising dry blending particles containing an unsaturated polyamide and an initiator with a second initiator.

[0247] Clause 59. The method according to Clause 57, further comprising wet blending particles containing an unsaturated polyamide and an initiator with a second initiator.

[0248] Clause 60. The method according to Clause 57, wherein the initiator is a photoinitiator.

[0249] Clause 61. The method according to Clause 57, wherein the initiator is a thermal initiator.

[0250] Clause 62. The method according to Clause 57, further comprising blending particles containing an unsaturated polyamide and an initiator with an infrared absorber.

[0251] Unless otherwise stated, all numbers used herein and in the related claims, representing quantities of components, properties such as molecular weight, and reaction conditions, should be understood in all cases as being modified by the term “approximately.” Therefore, unless otherwise indicated, the numerical parameters described in the following specification and the appended claims are approximations that may vary depending on the desired properties expected to be obtained by the embodiment of the present invention. At the very least, without any intention to limit the application of the doctrine of equivalents to the claims, each numerical parameter should be interpreted by applying the usual rounding method in light of the number of significant figures reported.

[0252] One or more exemplary embodiments incorporating one or more inventive elements are presented herein. For clarity, not all features of the physical implementations are described or indicated in this application. In developing physical embodiments incorporating one or more elements of the present invention, it is understood that numerous implementation-specific decisions must be made to achieve the developer's goals, such as implementation and compliance with system-related, business-related, government-related, and other constraints that change over time. While the developer's efforts may be time-consuming, such efforts are nevertheless routine for those skilled in the art and will benefit from this disclosure.

[0253] Although compositions and methods are described herein using the term "includes" various components or steps, compositions and methods may also "essentially consist of" or "consist of" various components and steps.

[0254] To facilitate a better understanding of the embodiments of the present invention, the following examples of preferred or representative embodiments are given. The following examples should not be read to limit or define the scope of the present invention. [Examples]

[0255] Comparative Example 1 describes the synthesis of an unsaturated polyamide by interfacial polycondensation. Interfacial polycondensation can be carried out at a constant speed of 2000 RPM in a 2 L glass vessel equipped with an overhead stirrer. A 500 mL solution of dichloride fumarate in toluene at a concentration of 0.2 mol (M) may be added to a stirring vessel containing a 500 mL aqueous suspension of 4,4'-methylenedianiline (MDA). The aqueous suspension of MDA may be mixed with KOH in the form of a 0.5 N (normality, N) solution, added to the aqueous phase at a rate of 1 mole of KOH per mole of MDA, to ensure the maximum molecular weight of the polyamide. After mixing the solutions at 20°C ± 2°C for 30 minutes, a concentrated solution should be formed. After distilling off the toluene by rotary evaporation under pressure or under vapor, the polymer should be in the form of a thin film. This film may be crushed and washed with a large amount of water until no chlorine is detected in the effluent. The polymer may be further washed to remove residual monomers using 30% methanol at high temperature, and then dried in a vacuum oven. The melting point of the resulting polymer (polymer A) should be approximately 230°C. [ka]

[0256] Synthesis of unsaturated polyamides from dicarboxylic acids will be described, where aliphatic and aromatic dicarboxylic acids can react directly with 1,5-bis(3-aminophenyl)-1,4-pentadien-3-one (DADBA). These monomers may be reacted in a polar solvent at low temperature (e.g., about 10 °C or below) in the presence of thionyl chloride. An exemplary synthetic procedure can be carried out by adding 21.9 g (150 mmol) of adipic acid in 300 mL of dimethylformamide (DMF) to a 2 L glass kettle equipped with an overhead stirrer, a thermocouple, and a nitrogen purge. The mixture may then be cooled to -5 °C in a NaNO3 / ice bath while 35.7 g (300 mmol) of thionyl chloride is added with stirring. After about 1 - 2 minutes, 39.6 g (150 mmol) of DADBA and 30.3 g (300 mmol) of triethylamine (TEA) are added to the mixture, and it may be stirred at 0 °C - 5 °C for 10 hours. After the reaction is complete, the polymer solution may be poured into an ice bath and immediately filtered. The polymer may then be washed several times with cold water and ethanol. If the DMF solution is to be removed for further purification, methanol may be used as a non-solvent. The melting point of the resulting polymer (Polymer B) should be about 220 °C. [Chemical formula]

[0257] Comparative Example 3 Unsaturated polyamides may also be produced by low-temperature polymerization by directly reacting aliphatic and aromatic dicarboxylic acid dioxides with DADBA. An exemplary synthesis procedure may be carried out by adding 27.3 g (150 mmol) of adipoyl chloride to 300 mL of N-methylpyrrolidone (NMP) in a glass kettle equipped with an overhead stirrer, thermocouple, and nitrogen purge. The mixture may then be cooled to -5°C in a NaNO3 / ice bath, while simultaneously adding 39.6 g (150 mmol) of DADBA and 30.3 g (300 mmol) of triethylamine (TEA) to the mixture and stirring at 0°C to 5°C for 10 hours. After the reaction is complete, the polymer solution may be poured into an ice bath and immediately filtered. The polymer may then be washed with ethanol and chloroform. The final purification step may include dissolving the polymer in DMF and then precipitation in methanol. The melting point of the resulting polymer (polymer B) should be approximately 220°C.

[0258] The comparative example 4 microparticles can be produced from the unsaturated polyamides synthesized in comparative examples 1 to 3 in a Haake small-scale twin-screw extruder having a high-shear rotor. The dispersion medium may be the dispersion media described herein (e.g., PDMS oil having a viscosity of about 10,000 cSt to about 30,000 cSt at room temperature). First, a dispersion medium in which 1 wt% of AEROSIL® R812S silica nanoparticles (relative to the polymer) is dispersed may be added and brought to a temperature near the melting point of the polymer. Then, room-temperature polymer pellets of the unsaturated polyamide and an initiator (preferably, when thermally triggered, an initiator having an activation energy higher than the melting emulsification temperature) may be added to the heated dispersion medium in the extruder. The weight ratio of the dispersion medium to the polyamide may be about 60:40 to about 80:20. The weight ratio of the polyamide to the initiator may be about 90:10 to about 99:1. In terms of temperature, the extruder may be operated at about 200 rpm for about 20 minutes to about 30 minutes. Then, the mixture can be discharged from the extruder onto a low-temperature surface for rapid cooling. The oil may be washed away from the unsaturated polyamide microparticles using ethyl acetate and filtered from the oil / ethyl acetate mixture. The washing procedure may include three washes with about 200 mL to about 500 mL of ethyl acetate at room temperature. The particles may be separated from the solvent by vacuum filtration onto Whatman #1, 90 mm filter paper. Then, the microparticles can be air-dried overnight in an aluminum pan in a fume hood to evaporate the residual ethyl acetate. The final unsaturated polyamide particles should have a D50 of about 30 microns to about 70 microns and a span of about 0.9 to about 1.3.

[0259] Comparative Example 5: Fine particles can be produced from the unsaturated polyamides synthesized in Comparative Examples 1-3 in a Haake small twin-screw extruder having a high-shear rotor. The dispersion medium may be a dispersion medium described herein (e.g., PDMS oil having a viscosity of about 10,000 cSt to about 30,000 cSt at room temperature). To mitigate premature crosslinking of the polymer during melt emulsification, a dispersion medium containing 1% by weight of AEROSIL® R812S silica nanoparticles (relative to the polymer) may be added first and heated to a temperature near the melting point of the polymer. Then, room-temperature polymer pellets of the unsaturated polyamide may be added to the heated dispersion medium in the extruder. The weight ratio of the dispersion medium to the polyamide may be about 60:40 to about 80:20. At this temperature, the extruder may be operated at about 200 rpm for about 20 to 30 minutes. The mixture can then be discharged from the extruder onto a low-temperature surface for rapid cooling. The oil may be washed away from the unsaturated polyamide particles using ethyl acetate, and the oil / ethyl acetate mixture may be filtered. The washing procedure may include three washes with about 200 mL to about 500 mL of ethyl acetate at room temperature. The particles may be separated from the solvent by vacuum filtration onto Whatman #1, 90 mm filter paper. The fine particles can then be air-dried overnight in an aluminum pan in a fume hood to evaporate any remaining ethyl acetate. The final unsaturated polyamide particles will have a D50 of about 30 microns to about 70 microns and a span of about 0.9 to about 1.3.

[0260] The resulting unsaturated polyamide particles may then be dry-blended with the initiator. The weight ratio of polyamide to initiator may be approximately 90:10 to approximately 99:1.

[0261] Comparative Example 6: Fine particles can be produced from the unsaturated polyamides synthesized in Comparative Examples 1-3 in a Haake small twin-screw extruder having a high-shear rotor. The dispersion medium may be any dispersion medium described herein (e.g., PDMS oil having a viscosity of about 10,000 cSt to about 30,000 cSt at room temperature). To mitigate premature crosslinking of the polymer during melt emulsification, a dispersion medium containing 1% by weight of AEROSIL® R812S silica nanoparticles (relative to the polymer) may be added first and heated to a temperature near the melting point of the polymer. Then, room-temperature polymer pellets of the unsaturated polyamide may be added to the heated dispersion medium in the extruder. The weight ratio of the dispersion medium to the polyamide may be about 60:40 to about 80:20. At this temperature, the extruder may be operated at about 200 rpm for about 20 to 30 minutes. The mixture can then be discharged from the extruder onto a low-temperature surface for rapid cooling. The oil may be washed away from the unsaturated polyamide particles using ethyl acetate, and the oil / ethyl acetate mixture may be filtered. The washing procedure may include three washes with about 200 mL to about 500 mL of ethyl acetate at room temperature. The particles may be separated from the solvent by vacuum filtration onto Whatman #1, 90 mm filter paper. The fine particles can then be air-dried overnight in an aluminum pan in a fume hood to evaporate any remaining ethyl acetate. The final unsaturated polyamide particles will have a D50 of about 30 microns to about 70 microns and a span of about 0.9 to about 1.3.

[0262] The resulting unsaturated polyamide particles can then be dispersed in methanol with a solid load of about 15% to about 30% by weight. The weight ratio of polyamide to initiator may be about 90:10 to about 99:1. After the particles have been wetted, a dispersion of about 1% to about 10% by weight of the initiator in methanol may be added to the particle slurry. Mixing may be continued at ambient temperature ± about 10°C. When heating, the temperature does not need to be high enough to initiate crosslinking. After mixing for about 30 minutes to about 3 hours, the particles may be filtered and dried overnight in a vacuum oven.

[0263] Comparative Example 7: Initiator-doped unsaturated polyamide particles from Comparative Examples 4-6 may be used in SLS to form a compacted structure. For example, as the CO2 laser passes through the powder bed during the sintering step of the printing process, it may slightly penetrate the top layer of particles, resulting in a crosslinking reaction of unsaturated bonds. These bonds may also crosslink with each other within previously printed layers, improving the degree of curing and the final properties of the finally printed portion. The laser speed may be reduced to ensure sufficient thermal penetration and to enhance crosslinking between printed layers. As the layers are scanned with the laser, the layers beneath the newly added layers may remain partially molten and may also be partially crosslinked until the next layer of powder spreads on top. The new layers may be heated, and the powder-enabled particles of the new layer may be further melted and chemically reacted with other particles in the vicinity.

[0264] Comparative Example 8: Preparation of unsaturated lactam monomers, 1-aza-4-cyclooctene, or 1-aza-2-ketocycloocta-5-ene can be obtained from SRWilson, RASAWicki, J.Org.Chem. 44 (1979) 287-291. The synthesis of the amine requires a series of reactions, first generating the oxime of 4-cycloheptene, followed by treatment with p-toluenesulfonyl chloride and pyridine to obtain the tosylate form. The tosyl oxime undergoes a Beckmann rearrangement to obtain the lactam form, a white crystalline material.

[0265] Ring-opening polymerization can be carried out by first adding 1-aza-4-cyclooctene (125.17 g, 1 mol) and a second-generation Grubbs catalyst such as [RuCl2(p-cymene)]2 / PCy3 (0.59 g, 10 mmol) in a flask under nitrogen, followed by the addition of dry chlorobenzene (1 L). The mixture is stirred at 60°C for 5 minutes, and then 300 mL of trimethylsilyldiazomethane (TMSD, 0.1 M in chlorobenzene, 3 × 10⁻⁶) is added. -2 mmol) may be added via a syringe pump. TMSD is used in situ for catalytic processes. RThis is required to generate a highly reactive, coordinating unsaturated ruthenium-carbene species that activates the carbene. The solution may be stirred at 60°C for 24 hours. The transformation may be monitored by gas chromatography (GC). The mixture may then be cooled to ambient temperature and poured into a large amount of n-heptane. The precipitated polymer may then be dried overnight under vacuum.

[0266] Accordingly, the present invention is well adapted to achieve the objectives and advantages described above, as well as the inherent advantages among them. The present invention may be modified and implemented in different but equivalent ways, which will be obvious to those skilled in the art who are interested in the teachings herein, so the specific examples and configurations disclosed above are merely illustrative. Furthermore, it is not intended to limit the present invention to any structural or design details other than those described in the following claims. Accordingly, the specific exemplary examples disclosed above may be changed, combined, or modified, and it is clear that all such variations are considered within the scope and spirit of the present invention. The present invention as exemplary disclosed herein may be implemented in the absence of any elements not specifically disclosed herein and / or any elements disclosed herein. Compositions and methods are described using the terms “comprising,” “containing,” or “including” various components or processes, but compositions and methods may also “essentially consist of” or “consist of” various components and processes. All the number and scope disclosed above may vary somewhat. Whenever a numerical range with lower and upper limits is disclosed, any number and any range included within that range are specifically disclosed. In particular, all ranges of values ​​disclosed herein (in the form of "about a to about b," or equivalently "approximately a to b," or equivalently "about a to b") should be understood to describe all numbers and ranges encompassed within a broad range of values. Furthermore, terms in the claims have plain, ordinary meanings unless explicitly and clearly defined by the patent holder. In addition, when used in claims, the indefinite article "a" or "an" is defined herein to mean one or more of the elements it introduces.

Claims

1. A process for depositing particles on a surface, the particles comprising: i) an unsaturated polyamide; ii) an initiator; and iii) an infrared absorber that absorbs electromagnetic radiation in the range of 100 nm to 1 nm, the process comprising the steps of: a nanoparticle emulsion stabilizer coating is disposed on the outer surface of the particle; and the particles have a circularity of about 0.9 to about 1.0, and the unsaturated polyamide is i) the polycondensation reaction product of at least one amino acid monomer having an unsaturated aliphatic carbon-carbon bond; ii) polycondensation reaction products of amino acid monomers having unsaturated aliphatic carbon-carbon bonds and amino acid monomers lacking unsaturated aliphatic carbon-carbon bonds; iii) a polycondensation reaction product of an amino acid monomer and a polyamine monomer, wherein at least one of the amino acid monomer and the polyamine monomer has an unsaturated aliphatic carbon-carbon bond; iv) a polycondensation reaction product of an amino acid monomer and a polyacid monomer, wherein at least one of the amino acid monomer and the polyacid monomer has an unsaturated aliphatic carbon-carbon bond; v) a polycondensation reaction product of an amino acid monomer, a polyamine monomer, and a polyacid monomer, at least one of the amino acid monomer, the polyamine monomer, and the polyacid monomer having an unsaturated aliphatic carbon-carbon bond; vi) ring-opening reaction products of cyclic amide monomers and amino acid monomers having unsaturated aliphatic carbon-carbon bonds; vii) ring-opening reaction products of cyclic amide monomers and polyacid monomers having unsaturated aliphatic carbon-carbon bonds; viii) ring-opening reaction products of cyclic amide monomers and polyamine monomers having unsaturated aliphatic carbon-carbon bonds; and ix) ring-opening reaction products of cyclic amide monomers, polyamine monomers, and polyacid monomers, wherein at least one of the polyamine monomers and the polyacid monomers has an unsaturated aliphatic carbon-carbon bond; depositing, the depositing step including at least one of and heating at least a portion of said particles after depositing to promote consolidation thereof and crosslinking of said unsaturated polyamide, thereby forming a consolidated body comprising crosslinked polyamide.

2. The method of claim 1, wherein the weight ratio of said unsaturated polyamide to said initiator is from about 90:10 to about 99:

1.

3. The method of claim 1 , wherein the particles further comprise a thermoplastic polymer that is not the unsaturated polyamide.

4. The method of claim 1 , wherein at least some of the particles have voids that contain the nanoparticles at the void / polymer interface.

5. The method of claim 1 , wherein the nanoparticles are embedded in the outer surface of the particle.

6. The method of claim 1, wherein the particles have a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, and a D90 of about 3 μm to about 300 μm, and D10<D50<D90.

7. The method of claim 1, wherein the unsaturated polyamide has a melting point or softening temperature of 200°C or greater.

8. A composition comprising particles comprising: i) an unsaturated polyamide; ii) an initiator; and iii) an infrared absorber that absorbs electromagnetic radiation from 100 nm to 1 nm, a nanoparticle emulsion stabilizer coating disposed on an outer surface of the particle; The unsaturated polyamide i) the polycondensation reaction product of at least one amino acid monomer having an unsaturated aliphatic carbon-carbon bond; ii) polycondensation reaction products of amino acid monomers having unsaturated aliphatic carbon-carbon bonds and amino acid monomers lacking unsaturated aliphatic carbon-carbon bonds; iii) a polycondensation reaction product of an amino acid monomer and a polyamine monomer, wherein at least one of the amino acid monomer and the polyamine monomer has an unsaturated aliphatic carbon-carbon bond; iv) a polycondensation reaction product of an amino acid monomer and a polyacid monomer, wherein at least one of the amino acid monomer and the polyacid monomer has an unsaturated aliphatic carbon-carbon bond; v) a polycondensation reaction product of an amino acid monomer, a polyamine monomer, and a polyacid monomer, at least one of the amino acid monomer, the polyamine monomer, and the polyacid monomer having an unsaturated aliphatic carbon-carbon bond; vi) ring-opening reaction products of cyclic amide monomers and amino acid monomers having unsaturated aliphatic carbon-carbon bonds; vii) ring-opening reaction products of cyclic amide monomers and polyacid monomers having unsaturated aliphatic carbon-carbon bonds; viii) ring-opening reaction products of cyclic amide monomers and polyamine monomers having unsaturated aliphatic carbon-carbon bonds; and ix) ring-opening reaction products of cyclic amide monomers, polyamine monomers, and polyacid monomers, wherein at least one of the polyamine monomers and the polyacid monomers has an unsaturated aliphatic carbon-carbon bond; A composition comprising at least one of the following:

9. The composition described in claim 8, wherein the particles have a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, and a D90 of about 3 μm to about 300 μm, and D10<D50<D90.

10. The composition of claim 8, wherein the particles have a circularity of about 0.9 to about 1.

0.

11. A process for shearing a mixture comprising: i) an unsaturated polyamide; ii) a dispersion medium immiscible with said unsaturated polyamide; iii) an infrared absorber absorbing electromagnetic radiation of 100 nm to 1 nm; and iv) an emulsion stabilizer consisting of nanoparticles dispersible in said dispersion medium, at a temperature above the melting point or softening temperature of said unsaturated polyamide, and at a shear rate high enough to disperse said unsaturated polyamide as droplets in said dispersion medium and to position nanoparticles at interfaces between the droplets and a carrier fluid, comprising: Optionally, at least a portion of said infrared absorbing agent comprises said nanoparticles; The unsaturated polyamide i) the polycondensation reaction product of at least one amino acid monomer having an unsaturated aliphatic carbon-carbon bond; ii) polycondensation reaction products of amino acid monomers having unsaturated aliphatic carbon-carbon bonds and amino acid monomers lacking unsaturated aliphatic carbon-carbon bonds; iii) a polycondensation reaction product of an amino acid monomer and a polyamine monomer, wherein at least one of the amino acid monomer and the polyamine monomer has an unsaturated aliphatic carbon-carbon bond; iv) a polycondensation reaction product of an amino acid monomer and a polyacid monomer, wherein at least one of the amino acid monomer and the polyacid monomer has an unsaturated aliphatic carbon-carbon bond; v) a polycondensation reaction product of an amino acid monomer, a polyamine monomer, and a polyacid monomer, at least one of the amino acid monomer, the polyamine monomer, and the polyacid monomer having an unsaturated aliphatic carbon-carbon bond; vi) ring-opening reaction products of cyclic amide monomers and amino acid monomers having unsaturated aliphatic carbon-carbon bonds; vii) ring-opening reaction products of cyclic amide monomers and polyacid monomers having unsaturated aliphatic carbon-carbon bonds; viii) ring-opening reaction products of cyclic amide monomers and polyamine monomers having unsaturated aliphatic carbon-carbon bonds; and ix) ring-opening reaction products of cyclic amide monomers, polyamine monomers, and polyacid monomers, wherein at least one of the polyamine monomers and the polyacid monomers has an unsaturated aliphatic carbon-carbon bond; and shearing the mixture, the shearing step comprising at least one of: cooling the mixture to below the melting point or softening temperature of the unsaturated polyamide to form particles comprising the unsaturated polyamide and the ultraviolet light absorber, forming an emulsion stabilizer coating comprised of nanoparticles disposed on an exterior surface of said particles.

12. 12. The method of claim 11, further comprising dry blending said particles with an initiator, wherein the weight ratio of said unsaturated polyamide to said initiator is from about 90:10 to about 99:

1.

13. 12. The method of claim 11, further comprising wet blending said particles with an initiator, wherein the weight ratio of said unsaturated polyamide to said initiator is from about 90:10 to about 99:

1.

14. The method of claim 13 , wherein the initiator is a photoinitiator.

15. The method of claim 13 , wherein the initiator is a thermal initiator.

16. The method of claim 11 , wherein the mixture further comprises a thermoplastic polymer that is not the unsaturated polyamide.

17. The method of claim 11 , wherein the nanoparticles are embedded in the outer surface of the particle.

18. The method of claim 11, wherein the mixture further comprises an initiator, and the weight ratio of the initiator to the unsaturated polyamide is from about 90:10 to about 99:

1.

19. The method of claim 11, wherein the particles have a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, and a D90 of about 3 μm to about 300 μm, and wherein D10<D50<D90.

20. The method of claim 11, wherein the particles have a circularity of about 0.9 to about 1.0.