Glass molding die for optical element molding, and method for producing optical element

JP2022107529A5Active Publication Date: 2024-10-10HOYA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022001429
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-01-08
Filing Date
2022-01-07
Publication Date
2024-10-10
Estimated Expiration
2042-01-07

AI Technical Summary

Technical Problem

Existing glass molds for optical elements exhibit significant temperature-dependent elasticity changes during press-molding processes, leading to variations in the shape of mass-produced optical elements.

Method used

A glass mold composition with a specific ratio of Li2O, Na2O, and K2O to MgO, ranging from 0.000 to 0.400, along with a high SiO2 and Al2O3 content, is used to minimize temperature dependence of elasticity, ensuring consistent optical element shape.

Benefits of technology

The proposed glass mold composition reduces temperature-induced shape changes, enabling stable production of optical elements with minimal variation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a glass molding die having elasticity with low temperature dependency.SOLUTION: The present invention pertains to a glass molding die for optical element molding. The glass is aluminosilicate glass. In the glass composition of the glass expressed by mol%, the total content of SiO2 and Al2O3 is 60% or more, and the molar ratio of the total content of Li2O, Na2O and K2O to the MgO content (Li2O+Na2O+K2O) / MgO is 0.000-0.400.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a glass mold for forming optical elements and a method for manufacturing optical elements. [Background technology]

[0002] A widely used method for manufacturing optical elements such as lenses is press molding of the material to be molded using a mold. Patent Document 1 discloses a glass mold that can be used in such a manufacturing method. [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 2019-127425 [Overview of the project] [Problems that the invention aims to solve]

[0004] When mass-producing optical elements by press-molding a material using a mold, typically, a single mold is used to repeatedly press-molde multiple materials. Minimizing shape variation in the optical elements produced in this way is desirable for the stable supply of optical elements with desired optical performance to the market. In this regard, the inventors have diligently studied the matter and have come to the new finding that a glass mold with low temperature dependence of elasticity is desirable. When press-molding a material, the glass mold is subjected to heating and cooling processes together with the material. If the elastic change of the glass mold is large during these processes, the shape of the molded surface of the glass mold will change significantly, resulting in variations in the surface shape of the optical elements formed by transferring this molded surface.

[0005] In view of the above, one aspect of the present invention aims to provide a glass mold with low temperature dependence of elasticity. [Means for solving the problem]

[0006] As a result of diligent research, the inventors have newly discovered that in aluminosilicate glass, setting the molar ratio of the total content of Li2O, Na2O, and K2O to the MgO content (Li2O + Na2O + K2O) / MgO in the range of 0.000 to 0.400 can suppress the large change in the elasticity of the glass with temperature, or more specifically, suppress the temperature dependence of Young's modulus.

[0007] That is, one aspect of the present invention is A glass mold for forming optical elements, The above glass is aluminosilicate glass. In the glass composition expressed in mol% of the above glass, The total content of SiO2 and Al2O3 is 60% or more, The above glass mold has a molar ratio (Li2O + Na2O + K2O) / MgO of the total content of Li2O, Na2O, and K2O relative to the MgO content, in the range of 0.000 to 0.400. Regarding.

[0008] Furthermore, one aspect of the present invention relates to a method for manufacturing an optical element, which includes press-molding a material to be molded using the glass mold described above. [Effects of the Invention]

[0009] According to one aspect of the present invention, a glass mold for forming optical elements can be provided, which has low temperature dependence of elasticity. Furthermore, according to one aspect of the present invention, a method for manufacturing optical elements using the above-mentioned glass mold can also be provided. [Brief explanation of the drawing]

[0010] [Figure 1] This is a schematic cross-sectional view showing an example of an optical element manufacturing apparatus including a glass mold. [Figure 2] This is a schematic cross-sectional view showing an example of a manufacturing apparatus for glass molding dies. [Modes for carrying out the invention]

[0011] [Glass molds for forming optical elements] The glass mold described above will be explained in more detail below. While the following explanation may refer to the drawings, the present invention is not limited to the embodiments shown in the drawings.

[0012] <Composition of glass molding die> Figure 1 is a schematic cross-sectional view of an example of an optical element manufacturing apparatus equipped with a glass mold. The optical element manufacturing apparatus 10 in Figure 1 manufactures an optical element 20 from a workpiece 21 by press molding and includes an upper mold 11 and a lower mold 12, which are glass molds. The upper mold 11 and the lower mold 12 are supported within a guide mold 13 so as to be able to move relative to each other, and the distance between them can be changed. The upper mold 11 and the lower mold 12 may both be movable molds, or one may be movable and the other fixed.

[0013] In one embodiment, the glass mold having the above composition can be an upper mold 11, and in another embodiment, it can be a lower mold 12. In yet another embodiment, both the upper mold 11 and the lower mold 12 can be glass molds having the above composition. In one embodiment, the glass constituting the upper mold 11 and the lower mold 12 can be the same glass, and in another embodiment, they can be different glass. In a preferred embodiment, both the upper mold 11 and the lower mold 12 can be glass molds having the above composition, and in a more preferred embodiment, the glass constituting the upper mold 11 and the lower mold 12 can be the same glass.

[0014] The upper mold 11 and the lower mold 12 have molding surfaces 14 and 15 on the sides facing each other. The optical element 20 is specifically a biconvex lens with aspherical surfaces on both sides, and the molding surfaces 14 and 15 are concave surfaces (aspherical surfaces) with shapes corresponding to the convex surfaces (aspherical surfaces) of the optical element 20 respectively. That is, the shapes of the molding surfaces 14 and 15 are transferred by press molding to form the convex surfaces of the optical element 20. However, the embodiment shown in FIG. 1 is an example, and the molding surfaces of the above glass molding die have a convex surface shape in one form and a concave surface shape in another form.

[0015] Coatings 16 and 17 are respectively formed on the molding surfaces 14 and 15. The coatings 16 and 17 can generally be coatings called release films, such as carbon films, etc., and can play a role in suppressing the fusion of the molded material. The coatings 16 and 17 shown in FIG. 1 have a single-layer structure, but it is also possible to provide coatings with a multi-layer structure composed of different compositions. Or, a configuration in which the molding surfaces 14 and l5 are exposed without the coatings 16 and 17 can also be selected.

[0016] A heater (not shown) is provided outside the guide mold 13. At the time of molding, the molded material 21 can be heated by the heater to the molding temperature at which it softens.

[0017] In the present invention and this specification, the "glass molding die" shall refer to the part provided with the molding surface. For example, in FIG. 1, the entire part excluding the coatings 16 and 17 of the upper mold 11 and the lower mold 12 may be made of glass. Or, only a part including the molding surfaces 14 and 15 of the upper mold 11 and the lower mold 12 may be made of glass, and a base part made of another material such as metal may be joined to the glass part to form the upper mold 11 or the lower mold 12.

[0018] Hereinafter, the glass constituting the above glass molding die will be described in more detail.

[0019] <Glass composition> In the present invention and this specification, the glass composition is expressed on an oxide basis with respect to the cationic components of the glass. Here, "glass composition on an oxide basis" means the glass composition obtained by calculating it assuming that all glass raw materials decompose during melting and exist as oxides in the glass. Unless otherwise specified, the glass composition is expressed on a molar basis (mol%, molar ratio). The various components that make up glass can be quantified using known methods, such as inductively coupled plasma atomic emission spectrometry (ICP-AES) and inductively coupled plasma mass spectrometry (ICP-MS). By dividing this elemental content (elemental mass %) by its atomic weight, the content of each element can be determined in mole percent. Furthermore, in the present invention and this specification, a component content of 0% or not present or introduced means that the component is substantially absent, and it is permissible for the component to be present at an unavoidable impurity level.

[0020] The above glass is aluminosilicate glass. In the present invention and this specification, "aluminosilicate glass" refers to glass in which the glass composition, expressed on an oxide basis for the cationic components of the glass, contains at least SiO2 and Al2O3. In the above glass, the total content of SiO2 and Al2O3 (SiO2 + Al2O3) is 60.0% or more. A total content of 60.0% or more (SiO2 + Al2O3) is considered to contribute to reducing the temperature dependence of elasticity (more specifically, the temperature dependence of Young's modulus, the same applies hereinafter). From this viewpoint, the total content (SiO2 + Al2O3) is preferably 65.0% or more, and in addition to the above viewpoint, it is preferably 66.0% or more from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature in which the press molding process is normally performed, and in addition to those viewpoints, it is preferably 68.0% or more from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and in addition to those viewpoints, it is preferably 70.0% or more from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later). On the other hand, the total content (SiO2 + Al2O3) is preferably 91.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 90.5% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, preferably 90.5% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), preferably 90.5% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later), preferably 89.5% or less from the viewpoint of improving the thermal expansion characteristics of the glass.

[0021] The molar ratio of the total content of Li2O, Na2O, and K2O to the MgO content ((Li2O+Na2O+K2O) / MgO) is preferably 0.400 or less, and more preferably 0.300 or less, from the viewpoint of reducing the temperature dependence of elasticity; preferably 0.200 or less, in addition to the above viewpoint, from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed; preferably 0.150 or less, in addition to the above viewpoint, from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature); and preferably 0.100 or less, in addition to the above viewpoint, from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later). The molar ratio ((Li2O+Na2O+K2O) / MgO) is 0.000 or more, and can be 0.000 or greater than 0.000.

[0022] The molar ratio of MgO content to the total MgO + CaO + SrO + BaO content (MgO / (MgO+CaO+SrO+BaO)) can be, for example, 1.000 or less. The molar ratio (MgO / (MgO+CaO+SrO+BaO)) is preferably 0.500 or more from the viewpoint of further reducing the temperature dependence of elasticity, preferably 0.550 or more from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, preferably 0.600 or more from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 0.650 or more from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0023] The total content of Li2O+Na2O+K2O (Li2O+Na2O+K2O) can be, for example, 0.0% or more or greater than 0.0%. Furthermore, the total content (Li2O+Na2O+K2O) can be, for example, 4.25% or less. From the viewpoint of further reducing the temperature dependence of elasticity, the total content (Li2O+Na2O+K2O) is preferably 4.0% or less; from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, in addition to the above viewpoint, it is preferably 3.0% or less; from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), in addition to the above viewpoints, it is preferably 2.0% or less; and from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later), it is preferably 1.0% or less.

[0024] The total content of Na2O and K2O (Na2O + K2O) can be, for example, 0.0% or more, or greater than 0.0%. Furthermore, the total content (Na2O + K2O) can be, for example, 4.25% or less. From the viewpoint of further reducing the temperature dependence of elasticity or avoiding excessively large thermal expansion coefficients, the total content (Na2O + K2O) can be, for example, 4.0% or less, 3.0% or less, 2.0% or less, 1.0% or less, or 0.5% or less.

[0025] The total content of MgO, CaO, SrO, and BaO (MgO + CaO + SrO + BaO) can be, for example, 35.0% or less. From the viewpoint of further reducing the temperature dependence of elasticity, the total content (MgO + CaO + SrO + BaO) is preferably 32.5% or less; from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, in addition to the above viewpoint, it is preferably 30.0% or less; from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), in addition to the above viewpoint, it is preferably 27.5% or less; and from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later), it is preferably 25.0% or less. Furthermore, the total content (MgO + CaO + SrO + BaO) can be, for example, 0.0% or more or 1.0% or more. From the viewpoint of further reducing the temperature dependence of elasticity, the total content (MgO + CaO + SrO + BaO) is preferably 8.0% or more. In addition to the above viewpoint, it is preferably 8.5% or more from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature in which the press molding process is normally performed. In addition to these viewpoints, it is preferably 9.0% or more from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature). In addition to these viewpoints, it is preferably 9.5% or more from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0026] The total content of MgO and CaO (MgO + CaO) can be, for example, 32.5% or less. From the viewpoint of further reducing the temperature dependence of elasticity, the total content (MgO + CaO) is preferably 30.0% or less; from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, in addition to the above viewpoint, it is preferably 27.5% or less; from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), in addition to the above viewpoint, it is preferably 25.0% or less; and from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later), it is preferably 22.5% or less. Furthermore, the total content (MgO + CaO) can be, for example, 0.0% or more or 1.0% or more. From the viewpoint of further reducing the temperature dependence of elasticity, the total content (MgO + CaO) is preferably 8.0% or more; from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, in addition to the above viewpoint, it is preferably 8.5% or more; from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), in addition to the above viewpoint, it is preferably 9.0% or more; and from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later), it is preferably 9.5% or more.

[0027] The total content of SiO2, Al2O3, and MgO (SiO2 + Al2O3 + MgO) can be, for example, 100.0% or less or less than 100.0%. Alternatively, the total content (SiO2 + Al2O3 + MgO) can be, for example, 80.0% or more. From the viewpoint of further reducing the temperature dependence of elasticity, the total content (SiO2 + Al2O3 + MgO) is preferably 85.0% or more. In addition to the above viewpoint, from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, it is preferably 86.0% or more. In addition to these viewpoints, from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), it is preferably 87.0% or more. In addition to these viewpoints, from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α value, as described later), it is preferably 88.0% or more.

[0028] The total content of Li2O, Na2O, K2O, SrO, and BaO (Li2O + Na2O + K2O + SrO + BaO) can be, for example, 0.0% or more or greater than 0.0%. Furthermore, the total content (Li2O + Na2O + K2O + SrO + BaO) can be, for example, 4.5% or less, preferably 3.5% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 3.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, preferably 3.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), preferably 2.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 1.0% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0029] The total content of SiO2, Al2O3, MgO, CaO, ZrO2, and TiO2 (SiO2 + Al2O3 + MgO + CaO + ZrO2 + TiO2) can be, for example, 100.0% or less or less than 100.0%. Furthermore, the total content (SiO2 + Al2O3 + MgO + CaO + ZrO2 + TiO2) can be, for example, 85.0% or more, preferably 90.0% or more from the viewpoint of further reducing the temperature dependence of elasticity, preferably 91.0% or more from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, preferably 92.0% or more from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 93.0% or more from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0030] The molar ratio of the total content of Li2O, Na2O, and K2O to the total content of MgO and CaO ((Li2O+Na2O+K2O) / (MgO+CaO)) can be, for example, 0.000 or more or greater than 0.000. Furthermore, the molar ratio ((Li2O+Na2O+K2O) / (MgO+CaO)) can be, for example, 2.000 or less, preferably 0.150 or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 0.100 or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, preferably 0.100 or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), preferably 0.050 or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 0.030 or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α as described later).

[0031] The molar ratio of the total content of Li2O+Na2O+K2O to the total content of SiO2+Al2O3+MgO ((Li2O+Na2O+K2O) / (SiO2+Al2O3+MgO)) can be, for example, 0.000 or more or greater than 0.000. Furthermore, the molar ratio ((Li2O+Na2O+K2O) / (SiO2+Al2O3+MgO)) can be, for example, 0.050 or less, preferably 0.040 or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 0.030 or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed in addition to the above viewpoint, preferably 0.030 or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature) in addition to the above viewpoints, preferably 0.020 or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 0.010 or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α as described later).

[0032] The molar ratio of the total content of Li2O+Na2O+K2O+SrO+BaO to the total content of SiO2+Al2O3+MgO+CaO+ZrO2+TiO2 ((Li2O+Na2O+K2O+SrO+BaO) / (SiO2+Al2O3+MgO+CaO+ZrO2+TiO2)) can be 0.000 or greater, or greater than 0.000. Furthermore, the molar ratio ((Li2O+Na2O+K2O+SrO+BaO) / (SiO2+Al2O3+MgO+CaO+ZrO2+TiO2)) can be, for example, 0.100 or less, preferably 0.090 or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 0.080 or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, preferably 0.080 or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), preferably 0.060 or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 0.050 or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0033] The total content of La2O3, Y2O3, Yb2O3, Ta2O5, Nb2O5, and HfO2 (La2O3+Y2O3+Yb2O3+Ta2O5+Nb2O5+HfO2) can be 0.000% or more, or greater than 0.000%. Furthermore, the total content (La2O3+Y2O3+Yb2O3+Ta2O5+Nb2O5+HfO2) can be, for example, 5.0% or less, and from the viewpoint of further reducing the temperature dependence of elasticity or not making the specific modulus too small, values ​​of 4.0% or less, 3.0% or less, 2.0% or less, and 1.0% or less are preferred in that order.

[0034] SiO2 is a skeletal component of glass and is a useful component for reducing the temperature dependence of elasticity. The SiO2 content is preferably 51.0% or more from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in glass molds, preferably 55.0% or more from the viewpoint of further reducing the temperature dependence of elasticity, preferably 56.0% or more from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, preferably 57.0% or more from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 58.0% or more from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later). Furthermore, the SiO2 content is preferably 79.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold; preferably 76.0% or less from the viewpoint of further reducing the temperature dependence of elasticity; preferably 75.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, in addition to the above viewpoints; preferably 74.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), in addition to the above viewpoints; and preferably 73.0% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0035] Al2O3 is a skeletal component of glass and is a useful component for reducing the temperature dependence of elasticity. The Al2O3 content is preferably 8.0% or more from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in glass molds, preferably 10.0% or more from the viewpoint of further reducing the temperature dependence of elasticity, preferably 11.0% or more from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed in addition to the above viewpoint, preferably 12.0% or more from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature) in addition to the above viewpoints, and preferably 12.5% ​​or more from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later). Furthermore, the Al2O3 content is preferably 24.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold; preferably 22.0% or less from the viewpoint of further reducing the temperature dependence of elasticity; preferably 21.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, in addition to the above viewpoints; preferably 20.5% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), in addition to the above viewpoints; and preferably 20.0% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0036] B2O3 is a component that can be optionally included in the glass, for example, to adjust the viscosity of the glass. The B2O3 content can be, for example, 0.0% or more or greater than 0.0%, and from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold, it can be 0.1% or more, 0.3% or more, 0.5% or more, or 1.0% or more. Furthermore, the B2O3 content is preferably 2.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, and also from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, and also from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and also from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0037] MgO is a component that can contribute to improving the Young's modulus of glass, lowering its specific gravity (and improving its specific modulus by lowering its specific gravity), and / or lowering α as described below. The MgO content can be 0.0% or more, greater than 0.0%, or 1.0% or more. From the viewpoint of suppressing the occurrence of bubbles, striations, and / or undissolved material in the glass mold, it is preferable to have 6.0% or more. From the viewpoint of further reducing the temperature dependence of elasticity, it is preferable to have 8.0% or more. In addition to the above viewpoint, from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, it is preferable to have 8.5% or more. In addition to the above viewpoint, from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), it is preferable to have 9.0% or more. In addition to the above viewpoint, from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α as described below), it is preferable to have 9.5% or more. Furthermore, the MgO content can be, for example, 30.0% or less, preferably 24.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold, preferably 22.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 21.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, preferably 20.5% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 20.0% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0038] The CaO content can be 0.0% or more, or greater than 0.0%. CaO is a component that can contribute to improving the Young's modulus of glass and lowering its specific gravity (and improving its specific modulus by lowering its specific gravity), and it is preferable to use it in combination with MgO. The CaO content can be, for example, 15.0% or less, preferably 10.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold and suppressing a decrease in the glass transition temperature, preferably 8.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 7.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed in addition to the above viewpoints, preferably 6.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature) in addition to the above viewpoints, and preferably 5.5% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α as described later).

[0039] The SrO content can be 0.0% or more, or greater than 0.0%. SrO is a component that can contribute to adjusting the fusion properties of glass, and by substituting it with an alkaline component, it can further reduce the temperature dependence of elasticity. The SrO content can be, for example, 12.0% or less, preferably 6.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold and suppressing a decrease in the Young's modulus of the glass, preferably 5.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 4.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed in addition to the above viewpoints, preferably 3.5% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature) in addition to the above viewpoints, and preferably 3.0% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α as described later).

[0040] The BaO content can be 0.0% or more, or greater than 0.0%. BaO is a component that can contribute to adjusting the meltability of the glass, and by substituting it with an alkaline component, it can further reduce the temperature dependence of the elasticity. The BaO content can be, for example, 12.0% or less, preferably 8.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold and suppressing a decrease in the Young's modulus of the glass, preferably 5.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 4.5% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed in addition to the above viewpoints, preferably 4.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature) in addition to the above viewpoints, and preferably 3.8% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α as described later).

[0041] The ZnO content can be 0.0% or more, or greater than 0.0%. Keeping the ZnO content below a certain level may contribute to suppressing a decrease in the glass transition temperature and / or a decrease in the specific modulus. The ZnO content can be, for example, 10.0% or less, preferably 5.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold and from the above viewpoint, preferably 4.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 3.5% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed in addition to the above viewpoint, preferably 3.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature) in addition to the above viewpoint, and preferably 2.5% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α as described later).

[0042] The Li2O content can be 0.0% or more, or greater than 0.0%. Keeping the Li2O content below a certain amount may contribute to further reducing the temperature dependence of elasticity, suppressing the decrease in glass transition temperature, and / or suppressing the decrease in Young's modulus. The Li2O content can be, for example, 8.0% or less, preferably 3.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold and from the above viewpoint, preferably 2.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 1.5% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed in addition to the above viewpoint, preferably 1.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature) in addition to the above viewpoint, and preferably 0.5% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α as described later).

[0043] The Na2O content can be 0.0% or more, or greater than 0.0%. Keeping the Na2O content below a certain amount may contribute to further reducing the temperature dependence of elasticity, suppressing the decrease in the glass transition temperature, and / or suppressing the decrease in Young's modulus. The Na2O content is preferably 3.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 2.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, preferably 1.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 0.5% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0044] The K2O content can be 0.0% or more, or greater than 0.0%. Keeping the K2O content below a certain amount may contribute to further reducing the temperature dependence of elasticity, suppressing the decrease in glass transition temperature, and / or suppressing the decrease in Young's modulus. The K2O content is preferably 3.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 2.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press forming process is normally performed, preferably 1.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 0.5% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0045] ZrO2 is a component that can be optionally included in the glass, for example, to improve the Young's modulus. The ZrO2 content can be, for example, 0.0% or more or greater than 0.0%. The ZrO2 content can be, for example, 10.0% or less, preferably 4.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold, preferably 2.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 2.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, preferably 1.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 0.5% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0046] TiO2 is a component that can be optionally included in the glass, for example, to improve Young's modulus and / or to suppress the formation of bubbles in the glass mold. The TiO2 content can be, for example, 0.0% or more or greater than 0.0%. From the viewpoint of suppressing the formation of bubbles, striations and / or undissolved material in the glass mold, the TiO2 content can be 0.1% or more, 0.3% or more, 0.5% or more, or 1.0% or more. Furthermore, the TiO2 content can be, for example, 6.0% or less, preferably 5.0% or less from the viewpoint of suppressing the occurrence of bubbles, striations and / or undissolved material in the glass mold, preferably 4.0% or less from the viewpoint of further reducing the temperature dependence of elasticity, preferably 3.0% or less from the viewpoint of increasing the rigidity of the glass (e.g., Young's modulus) at the temperature at which the press molding process is normally performed, preferably 2.0% or less from the viewpoint of increasing the heat resistance of the glass (e.g., glass transition temperature), and preferably 1.0% or less from the viewpoint of improving the thermal expansion characteristics of the glass (e.g., having a low α, as described later).

[0047] From the viewpoint of reducing the temperature dependence of elasticity, the La2O3 content is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. The La2O3 content can be 0.0%, 0.0% or more, or greater than 0.0%.

[0048] From the viewpoint of reducing the temperature dependence of elasticity, the Y2O3 content is preferably 4.0% or less, more preferably 3.0% or less, and preferably 2.0% or less. The Y2O3 content may also be 1.0% or less or 0.5% or less, and may also be 0.0% (i.e., not contained), 0.0% or more, or greater than 0.0%.

[0049] From the viewpoint of reducing the temperature dependence of elasticity, the Yb2O3 content is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. The Yb2O3 content may also be 1.0% or less or 0.5% or less, and may also be 0.0% (i.e., not contained), 0.0% or more, or greater than 0.0%.

[0050] From the viewpoint of reducing the temperature dependence of elasticity, the Ta2O5 content is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. The Ta2O5 content may also be 1.0% or less or 0.5% or less, and may also be 0.0% (i.e., not contained), 0.0% or more, or greater than 0.0%.

[0051] From the viewpoint of reducing the temperature dependence of elasticity, the Nb2O5 content is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. The Nb2O5 content may also be 1.0% or less or 0.5% or less, and may also be 0.0% (i.e., not contained), 0.0% or more, or greater than 0.0%.

[0052] From the viewpoint of reducing the temperature dependence of elasticity, the HfO2 content is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. The HfO2 content may also be 1.0% or less or 0.5% or less, and may also be 0.0% (i.e., not contained), 0.0% or more, or greater than 0.0%.

[0053] SnO2 is a component that can be optionally included in the glass, for example, to improve Young's modulus and / or to suppress the formation of bubbles in the glass mold. The SnO2 content can be, for example, 0.0% or more or greater than 0.0%. From the viewpoint of suppressing the formation of bubbles, striations and / or undissolved material in the glass mold, the SnO2 content can be 0.05% or more, 0.3% or more, or 0.5% or more. Furthermore, the SnO2 content is preferably 3.0% or less, preferably 2.0% or less, preferably 1.5% or less, preferably 1.0% or less, and preferably 0.5% or less, from the viewpoint of suppressing the formation of bubbles, striations and / or undissolved matter in the glass mold. The SnO2 content may also be 0.2% or less or 0.1% or less, and may also be 0.0% (i.e., not contained), 0.0% or more, or greater than 0.0%.

[0054] CeO2 is a component that can be optionally included in the glass, for example, to improve the Young's modulus and / or to suppress the formation of bubbles in the glass mold. The CeO2 content can be, for example, 0.0% or more or greater than 0.0%. From the viewpoint of suppressing the formation of bubbles, striations and / or undissolved material in the glass mold, the CeO2 content can be 0.05% or more, 0.3% or more, or 0.5% or more. Furthermore, the CeO2 content is preferably 3.0% or less, preferably 2.0% or less, preferably 1.5% or less, preferably 1.0% or less, and preferably 0.5% or less, from the viewpoint of suppressing the formation of bubbles, striations and / or undissolved matter in the glass mold. The CeO2 content may also be 0.2% or less or 0.1% or less, and may also be 0.0% (i.e., none), 0.0% or more, or greater than 0.0%.

[0055] Sb2O3 is a component that can be optionally included in the glass, for example, to improve Young's modulus and / or to suppress the formation of bubbles in the glass mold. The Sb2O3 content can be, for example, 0.0% or more or greater than 0.0%. From the viewpoint of suppressing the formation of bubbles, striations and / or undissolved material in the glass mold, the Sb2O3 content can be 0.05% or more, 0.1% or more, 0.3% or more, 0.5% or more, or 1.0% or more. Furthermore, the Sb2O3 content is preferably 3.0% or less, preferably 2.0% or less, preferably 1.5% or less, preferably 1.0% or less, and preferably 0.5% or less, from the viewpoint of suppressing the formation of bubbles, striations and / or undissolved matter in the glass mold.

[0056] Fe2O3 is a component that can be optionally included in the glass, for example, to improve Young's modulus and / or to suppress the formation of bubbles in the glass mold. The Fe2O3 content can be, for example, 0.0% or more or greater than 0.0%. From the viewpoint of suppressing the formation of bubbles, striations and / or undissolved material in the glass mold, the Fe2O3 content can be 0.05% or more, 0.3% or more, or 0.5% or more. Furthermore, the Fe2O3 content is preferably 2.0% or less, preferably 1.0% or less, preferably 0.5% or less, preferably 0.2% or less, and preferably 0.01% or less, from the viewpoint of suppressing the formation of bubbles, striations and / or undissolved matter in the glass mold.

[0057] <Glass Properties> The glass constituting the above-mentioned glass mold may, in one embodiment, possess one or more of the following glass properties.

[0058] (Glass transition temperature Tg, flexion point Ts) In the present invention and this specification, the glass transition temperature Tg and the bending point Ts of the glass constituting the glass mold described above are values ​​that can be determined by the following method. Glass samples are cut from a glass mold, or glass samples are prepared from the same material as the glass mold. For each glass sample, the thermal expansion properties are measured according to the method specified in JOGIS08-2003. Specifically, the annealing temperature is set by rounding the last digit of the glass's Tg (unit: °C) to the nearest 10°C. The glass sample is placed in an annealing furnace capable of reaching this temperature, heated from room temperature (approximately 25°C) to the set temperature in 1-2 hours, held for 2 hours, then cooled at a rate of -30°C / hour for 4 hours, and then allowed to cool in the furnace to room temperature (approximately 25°C). The glass sample is then processed into a cylindrical glass sample with a diameter of 4.0-5.0 mm and a length of 10-20 mm. A load of 98 mN is applied to this glass sample, and it is heated at a rate of 4°C / minute. The amount of elongation (unit: mm) with respect to temperature is measured every second, and a graph (so-called thermal expansion curve) is created. The temperature corresponding to the intersection of the extensions of the straight lines in the low-temperature and high-temperature regions in the graph above is defined as the glass transition point Tg, and the temperature at which expansion seemingly stops in the graph above, that is, the temperature at the inflection point where the elongation changes from increasing to decreasing with increasing temperature, is defined as the flexing point Ts. For the above glass mold to be suitable for press molding at higher temperatures, the glass transition temperature Tg of the glass is preferably 755°C or higher, more preferably 760°C or higher, even more preferably 765°C or higher, and even more preferably 770°C or higher. Furthermore, the glass transition temperature Tg of the glass can be, for example, 860°C or lower, 855°C or lower, 850°C or lower, 845°C or lower, or 840°C or lower. Furthermore, in order for the above-mentioned glass mold to be a mold suitable for press molding at higher temperatures, the bending point Ts of the glass is preferably 830°C or higher, more preferably 835°C or higher, even more preferably 840°C or higher, and even more preferably 845°C or higher. Also, the bending point Ts of the glass can be, for example, 940°C or lower, 935°C or lower, 930°C or lower, 925°C or lower, or 920°C or lower.

[0059] (Mean coefficient of linear expansion α) For example, as shown in FIG. 1, a manufacturing apparatus for an optical element can be configured by combining a glass mold with a guiding mold. From the perspective of stress control received by the glass mold in the manufacturing apparatus for an optical element when combined with a component such as the guiding mold, it is preferable to adjust the thermal expansion characteristics of the glass constituting the glass mold. In one form, the thermal expansion characteristics of the glass constituting the glass mold, as the average linear expansion coefficient α in the temperature range of 100 to 300 °C, are preferably 23.5×10 / °C or more, more preferably 24.0×10 -7 / °C or more, still more preferably 24.5×10 -7 / °C or more, even more preferably 25.0×10 -7 / °C or more. Further, the average linear expansion coefficient α of the glass is preferably 48.0×10 -7 / °C or less, more preferably 47.0×10 -7 / °C or less, still more preferably 46.0×10 -7 / °C or less, even more preferably 45.0×10 -7 / °C or less, still even more preferably 44.0×10 -7 / °C or less. The average linear expansion coefficient α is calculated by the formula: α = d / (L×T). d is the change amount (mm) of the sample length in the temperature range of 100 to 300 °C, L is the initial length (mm) of the sample, and T is the temperature difference (K)(300 °C - 100 °C = 200 °C). As a measuring device for the linear expansion coefficient, a thermomechanical analyzer (TMA; Thermomechanical Analysis) or a dilatometer can be used. The average linear expansion coefficient α can be obtained, for example, by the following method. For glass samples cut from a glass mold, or glass samples made from the same material as the glass mold, a thermomechanical analysis (TMA) is used to set the annealing temperature by rounding the glass's Tg (in °C) to the nearest 10°C and rounding to the nearest 10°C. The glass sample is then placed in an annealing furnace capable of reaching this temperature, heated from room temperature (approximately 25°C) to the set temperature in 1-2 hours, held for 2 hours, then slowly cooled at -30°C / hour for 4 hours, and finally allowed to cool to room temperature (approximately 25°C) in the furnace. This glass sample is then processed into a cylindrical glass sample with a diameter of 4.0-5.0 mm and a length of 10-20 mm. With a load of 98 mN applied to this glass sample, it is heated at a heating rate of 4°C / min, and the elongation (in mm) with respect to temperature is measured every second. The average linear expansion coefficient α can then be determined from the resulting graph (so-called thermal expansion curve).

[0060] In one embodiment, the components of a manufacturing apparatus for optical elements such as guide types can be made of silicon carbide (SiC). SiC has an average coefficient of linear thermal expansion α of 37 × 10⁻⁶. -7 The temperature is approximately / °C. -7 When the temperature is " / ℃", it is preferable that X calculated by the formula X=A-37 is a negative value from the viewpoint of suppressing the falling of the optical element during manufacturing. From this viewpoint, it is preferable that X calculated by the above formula for the glass be -13.5 or higher, more preferably -13.0 or higher, even more preferably -12.5 or higher, and even more preferably -12.0 or higher. Furthermore, X can be, for example, 11.0 or lower, 10.0 or lower, 9.0 or lower, 8.0 or lower, or 7.0 or lower, and from the above viewpoint, it is preferable that it be less than 0.0. Furthermore, from the viewpoint of suppressing stress on the glass mold from the SiC component in the manufacturing apparatus for optical elements, the absolute value of X|X| is preferably 13.0 or less, more preferably 12.5 or less, even more preferably 12.0 or less, and even more preferably 11.5 or less. Also, the absolute value of X|X| is preferably 0.0 or more, and even more preferably greater than 0.0.

[0061] (specific gravity) From the viewpoint of adjusting the specific modulus of elasticity, as described later, it is preferable for the glass to have a low specific gravity. The specific gravity of the glass is preferably 2.98 or less, more preferably 2.93 or less, even more preferably 2.88 or less, and even more preferably 2.83 or less. The specific gravity of the glass can also be, for example, 2.35 or more, 2.37 or more, 2.40 or more, or 2.43 or more, and can be lower than the values ​​exemplified here. The specific gravity of the glass can be determined by the Archimedes method for a glass sample cut from a glass mold, or for a glass sample made from the same material as the glass mold.

[0062] (Young's modulus) From the viewpoint of suppressing deformation of the glass mold described above, it is preferable that the Young's modulus of the glass constituting the glass mold is high. From this viewpoint, the Young's modulus of the glass is preferably 87 GPa or higher, more preferably 88 GPa or higher, even more preferably 89 GPa or higher, and even more preferably 90 GPa or higher. Furthermore, the Young's modulus of the glass can be, for example, 120 GPa or less, 110 GPa or less, 101 GPa or less, 100 GPa or less, 99 GPa or less, 98 GPa or less, or 97 GPa or less, or it can exceed the values ​​exemplified herein. The Young's modulus of the glass can be determined for a glass sample cut from the glass mold, or for a glass sample made of the same material as the glass mold, at a measurement temperature of 25°C ± 5°C by the ultrasonic pulse method described in JIS R1602:1995. The size of the glass sample can be appropriately set to a size greater than or equal to the minimum dimensions described in JIS R1602:1995.

[0063] For glass forming molds, it is preferable that the glass has high rigidity at the temperature at which the press molding process is normally performed. From this viewpoint, the Young's modulus of the glass at a measurement temperature of 590°C is preferably 80 GPa or higher, more preferably 85 GPa or higher, even more preferably 88 GPa or higher, even more preferably 90 GPa or higher, even more preferably 91 GPa or higher, and even more preferably 92 GPa or higher. Furthermore, the Young's modulus of the glass at a measurement temperature of 590°C can be, for example, 118 GPa or less, 107 GPa or less, 102 GPa or less, 100 GPa or less, 98 GPa or less, 97 GPa or less, or 96 GPa or less, or it can exceed the values ​​exemplified herein. Furthermore, from the above viewpoint, the Young's modulus of the glass at a measurement temperature of 650°C is preferably 80 GPa or higher, more preferably 84 GPa or higher, even more preferably 87 GPa or higher, even more preferably 89 GPa or higher, even more preferably 90 GPa or higher, and even more preferably 91 GPa or higher. In addition, the Young's modulus of the glass at a measurement temperature of 650°C can be, for example, 117 GPa or less, 106 GPa or less, 101 GPa or less, 99 GPa or less, 97 GPa or less, 96 GPa or less, or 95 GPa or less, or it can exceed the values ​​exemplified herein. The Young's modulus at a measurement temperature of 590°C or 650°C can be determined by the Young's modulus measurement method described above, except that the measurement temperature is set to 590°C or 650°C.

[0064] (Specific modulus of elasticity) The specific modulus of elasticity is the Young's modulus of glass divided by its density. Here, density is the specific gravity of the glass divided by g / cm³. 3 This can be considered as a value with the unit attached. A mold made from glass with a higher specific modulus of elasticity can be said to be a mold that is lighter and less prone to deformation. From this viewpoint, the specific modulus of elasticity of the glass is preferably 31.0 MNm / kg or more, more preferably 32.0 MNm / kg or more, even more preferably 33.0 MNm / kg or more, and even more preferably 33.5 MNm / kg or more. Furthermore, the specific modulus of elasticity of the glass can be, for example, 41.0 MNm / kg or less, 40.5 MNm / kg or less, 40.0 MNm / kg or less, 39.5 MNm / kg or less, or 39.0 MNm / kg or less, and can exceed the values ​​exemplified here.

[0065] (rigidity) The rigidity modulus of glass represents its resistance to deformation under shear force, and from the viewpoint of suppressing deformation of the glass mold, it is preferable for the glass constituting the glass mold to have a high rigidity modulus. From this viewpoint, the rigidity modulus of the glass can be 33.0 GPa or higher, and is preferably 34.0 GPa or higher, 35.0 GPa or higher, and 36.0 GPa or higher, in that order. The rigidity modulus of the glass can be, for example, 42.0 GPa or less, 41.5 GPa or less, 41.0 GPa or less, 40.5 GPa or less, or 40.0 GPa or less. The rigidity modulus of the above-mentioned glass can be determined for a measurement glass sample cut from a glass mold, or for a measurement glass sample made from the same material as the glass mold, at a measurement temperature of 25°C ± 5°C using the ultrasonic pulse method described in JIS R1602:1995. The size of the measurement glass sample can be appropriately set to a size greater than or equal to the minimum dimensions described in JIS R1602:1995.

[0066] (Poisson's ratio) The Poisson's ratio of glass is a dimensionless parameter determined from the ratio of Young's modulus to shear modulus. The Poisson's ratio of the glass can be, for example, 0.190 or higher, and is preferably 0.195 or higher, 0.200 or higher, 0.205 or higher, and 0.210 or higher, in that order. Alternatively, the Poisson's ratio of the glass can be, for example, 0.333 or lower, and is preferably 0.300 or lower, 0.290 or lower, 0.280 or lower, 0.270 or lower, and 0.260 or lower, in that order. The Poisson's ratio of the above-mentioned glass can be determined for a glass sample cut from a glass mold, or for a glass sample made from the same material as the glass mold, at a measurement temperature of 25°C ± 5°C using the ultrasonic pulse method described in JIS R1602:1995. The size of the glass sample can be appropriately set to a size greater than or equal to the minimum dimensions described in JIS R1602:1995.

[0067] (Liquidus temperature LT) The liquidus temperature LT can be cited as an indicator of the meltability of glass. From the viewpoint of improving the meltability of glass, the liquidus temperature LT of the glass constituting the glass mold is preferably 1440°C or lower, more preferably 1420°C or lower, even more preferably 1400°C or lower, even more preferably 1380°C or lower, and even more preferably 1360°C or lower. Furthermore, the liquidus temperature LT of the glass can be, for example, 1150°C or higher, 1170°C or higher, 1200°C or higher, or 1230°C or higher, and can also be lower than the values ​​exemplified here.

[0068] In the present invention and this specification, "liquid phase temperature" is determined for a glass sample cut from a glass mold, or for a glass sample made from the same material as the glass mold, by the following method. Approximately 20cc of glass (for example, 50g of glass with a specific gravity of 2.5g / cc) is placed in a platinum crucible and heated in a furnace with an ambient temperature of 1400°C to 1600°C for 15 to 30 minutes until molten. Then, it is cooled to below the glass transition temperature Tg. The cooled glass is moved to a furnace with an ambient temperature T and held in the furnace for 16 hours. After that, the presence or absence of crystal precipitation is determined by observation with an optical microscope (magnification 100x). For each different temperature T (in 10°C increments), the presence or absence of crystal precipitation is determined using the method described above. The lowest temperature T at which no crystal precipitation is observed is defined as the liquidus temperature.

[0069] <Method for manufacturing glass molding dies> The above-mentioned glass molding die can be manufactured as a glass molding die having a concave or convex molding surface by pressing a glass material for glass molding dies with a master die.

[0070] Figure 2 is a schematic cross-sectional view of an example of a glass mold manufacturing apparatus (hereinafter also referred to as "mold manufacturing apparatus"). The mold manufacturing apparatus in Figure 2 includes an upper mold (master mold) 31 having a convex molding surface 34, a lower mold 32, and a guide mold 33. A glass material 41 is pressed between the upper mold 31 and the lower mold 32, and the surface shape of the molding surface 34 of the upper mold is transferred to the glass material 41, thereby obtaining a glass mold having a concave molding surface. The surface shape of the lower mold 32 may be planar, convex, or concave, and is not particularly limited. In addition, in the mold manufacturing apparatus in Figure 2, the master mold for transferring the surface shape to the glass material and forming the molding surface of the glass mold is the upper mold, but such a master mold can also be arranged as the lower mold.

[0071] The upper mold 31 and the lower mold 32 are supported within a guide mold (also commonly called a "sleeve") 33 so as to be able to move relative to each other, and the distance between them can be changed. Both the upper mold 31 and the lower mold 32 may be movable, or one may be movable and the other fixed.

[0072] A heater (not shown) is provided on the outside of the guide mold 33. During molding, the glass material 41 can be heated by the heater to a molding temperature Ta at which it softens. Ta can be set according to the type of glass material, for example, in the range of 700 to 1000°C, preferably in the range of 750 to 950°C. In one embodiment, Ta can be set to Ta = Ts ± 50°C. In the mold manufacturing apparatus of Figure 2, the upper mold, lower mold, and guide mold are heated together with the glass material by the heater provided on the outside of the guide mold 33.

[0073] The glass material, heated to temperature Ta, is pressed against the master mold surface (the molding surface 34 of the upper mold 31 in Figure 2). The glass material 41 can be pressed by applying a pressing load to it via the upper mold 31 and / or the lower mold 32.

[0074] Subsequently, the glass material 41 is cooled in contact with the master mold surface. The cooling rate C in this cooling process is the average cooling rate from Ta to Tb (described later), and from the viewpoint of increasing the productivity of the glass mold and / or suppressing thermal degradation of the master mold, it is -0.1°C / min or higher, -0.3°C / min or higher, -0.5°C / min or higher, -1.0°C / min or higher, -3.0°C / min or higher, -5.0°C / min or higher, -10.0°C / min or higher, or -15.0°C / min. It can be above -100.0°C / min or lower, -50.0°C / min or lower, -30.0°C / min or lower, -25.0°C / min or lower, -20.0°C / min or lower, -18.0°C / min or lower, -16.0°C / min or lower, -14.0°C / min or lower, -12.0°C / min or lower, -10.0°C / min or lower, -5.0°C / min or lower, -3.0°C / min or lower, or -1.0°C / min or lower. In one configuration, from the viewpoint of increasing productivity, the press load and / or cooling rate may be switched at temperatures Tm above Tb and below Ta. The cooling rate C in this case is determined from the cooling rate Ca (unit: °C / min) from Ta to Tm and the cooling rate Cb (unit: °C / min) from Tm to Tb. C (unit: °C / min) = (Ta - Tb) / {(Ta - Tm) / Ca + (Tm - Tb) / Cb} It can be calculated as follows.

[0075] After the above cooling, the contact state with the master mold surface is released. In this way, the glass material 41 is press-molded, and a glass mold can be obtained having a concave molding surface formed by transferring the surface shape of the master mold surface (molding surface 34 of the upper mold 31 in Figure 2). The above release of the contact state can be performed at a temperature Tb in which the hardening of the glass has progressed sufficiently. Tb can be, for example, a temperature around or below Tg. Preferably, Tb is well below the strain point of the glass, and from this viewpoint, it can be, for example, Tg-150°C or below, preferably Tg-160°C or below, more preferably Tg-180°C or below, and even more preferably Tg-200°C or below. From the viewpoint of making it easier for the temperature of the glass mold and / or master mold to follow the cooling rate, Tb can be, for example, 20°C or higher, 50°C or higher, 70°C or higher, 100°C or higher, 150°C or higher, 200°C or higher, 250°C or higher, 300°C or higher, 350°C or higher, or 400°C or higher. Furthermore, it is preferable that Tb be well below the Tg of the glass mold, and from this viewpoint, it can be, for example, 900°C or lower, 800°C or lower, 700°C or lower, 600°C or lower, 550°C or lower, 500°C or lower, 400°C or lower, 350°C or lower, or 300°C or lower. During cooling from Ta to Tb, a pressing load may be continuously applied to the glass material 41 via the upper mold 31 and / or lower mold 32 as appropriate, or the load may be only the weight of the mold itself.

[0076] According to the mold molding apparatus shown in Figure 2, a glass mold having a concave molding surface can be obtained. On the other hand, if the surface shape of the molding surface of the master mold is concave, the concave shape can be transferred to the glass material, thereby obtaining a glass mold having a convex molding surface. The glass mold removed from the mold molding apparatus can be subjected to one or more known post-processes, such as annealing and coating formation.

[0077] The material of the master mold is not particularly limited. From the viewpoint of heat resistance, durability, etc., master molds made of silicon carbide (SiC) or glass are preferred. The master mold can be manufactured by known methods.

[0078] [Manufacturing method for optical elements] One aspect of the present invention relates to a method for manufacturing an optical element, which includes press molding a material to be molded using the glass mold described above.

[0079] Regarding the manufacturing method of the optical element described above, prior art for manufacturing optical elements by press molding can be applied, except for the use of the glass mold described earlier. An example of an optical element manufacturing apparatus that can be used for press molding is the optical element manufacturing apparatus shown in Figure 1, which was described earlier.

[0080] Examples of optical elements include various lenses such as spherical lenses, aspherical lenses, and microlenses, as well as prisms. Furthermore, the material to be molded can be glass, and the optical elements can be glass optical elements.

[0081] For example, using the above-mentioned glass mold, a glass block processed for press molding (hereinafter referred to as "press-molding glass material") can be press-molded. Examples of press-molding glass materials include glass blocks having a mass equivalent to the mass of a press-molded product, such as a preform for precision press molding or a glass material for obtaining an optical element blank by press molding (press-molding glass gob). Press-molding glass materials are produced through a process of processing a glass molded body. A glass molded body can be produced by heating and melting glass raw materials and molding the resulting molten glass. Examples of processing methods for glass molded bodies include cutting, grinding, and polishing. An optical element blank is a glass molded body having a shape that approximates the shape of the optical element to be manufactured. An optical element blank can be produced by a method such as molding glass to a shape that includes the processing allowance to be removed by processing, in addition to the shape of the optical element to be manufactured. For example, optical element blanks can be manufactured by methods such as the reheat press method, which involves heating and softening a glass material for press molding, or the direct press method, which involves supplying a molten glass mass to a press mold using a known method and then press molding it.

[0082] For example, the shape accuracy of the molding surface of a mold for precision press forming requires several times the shape accuracy required for optical elements. According to the glass mold manufacturing method described above, a glass mold can be manufactured by transferring the surface shape of a master mold with high precision. The glass mold thus obtained is suitable as a mold for precision press forming. However, since excellent shape accuracy of the molding surface is desirable in various press forming processes, the glass mold manufactured by the above manufacturing method is not limited to molds for precision press forming, but is suitable as a mold for various press forming processes.

[0083] The following describes a specific example of a method for obtaining glass optical elements by press molding. A carbon film is coated as a release film on the molding surface of a glass mold and placed inside the optical element manufacturing apparatus. After supplying the press-molded glass material (glass material to be molded) into the optical element manufacturing apparatus, the viscosity of the glass material to be molded is 10 8 dPa·s~10 12 The glass is heated and softened to a temperature equivalent to a viscosity of dPa·s, and then pressed with a mold to transfer the molding surface of the glass mold to the glass material to be molded. The temperature set in the apparatus at this time is called the press temperature. To prevent oxidation of the molding surface, it is preferable to use a non-oxidizing atmosphere during molding. After this, the glass mold and the glass material to be molded are cooled to near the glass transition temperature of the glass constituting the glass material to be molded, while maintaining close contact between the molding surface and the glass element to be molded, while applying an appropriate load application schedule (for example, -50°C / min). After that, the optical element manufacturing apparatus can be opened (disassembled) and the molded body (optical element) can be removed. [Examples]

[0084] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the embodiments shown in the examples.

[0085] [Examples 1-20, Comparative Example 1] <Glass material for glass molding dies> Glass materials having the glass composition shown in Table 1 were prepared by the following method. To obtain the glass composition shown in Table 1, various oxides, boric acid, carbonates, and sulfates were used as raw materials to introduce each component. The raw materials were weighed and thoroughly mixed to form the blended raw materials. At this time, a total of 200g of each raw material in terms of oxide equivalent was used. The crucible containing the blended raw materials was placed in a glass melting furnace, and the glass was melted, clarified, and homogenized at 1600°C for 3 hours. The molten glass was then poured from the crucible into a preheated mold and shaped. Next, the shaped glass was removed from the mold and placed in an annealing furnace set to a furnace temperature of 750°C, and annealed at a slow cooling rate of -30°C / hour to obtain the glass material.

[0086] [Table 1-1]

[0087] [Table 1-2]

[0088] <Master type> A SiC master mold was prepared as the master mold.

[0089] <Fabrication of glass molds by press molding> For each glass material, press molding was performed using the mold manufacturing apparatus configured as shown in Figure 2, according to the method described above. The glass material was pressed by applying a load while in contact with the master mold surface at a temperature Ta in the range of 780°C to 900°C, the temperature Tb was set to a temperature in the range of 450°C to 650°C, and the cooling rate C (average cooling rate from temperature Ta to Tb) was set to a range of -5.0°C / min to -30.0°C / min. After that, the glass was allowed to cool to approximately room temperature within the mold manufacturing apparatus, the contact with the master mold was released, and the glass mold with the surface shape of the master mold transferred to form the molded surface was removed from the mold manufacturing apparatus. In this way, a glass mold having a concave molding surface was fabricated.

[0090] [Evaluation of glass molding dies] <Glass Properties> For each glass mold used in Examples 1-20 and Comparative Example 1, the various glass properties shown in Table 3 were determined using the previously exemplified method and are shown in Table 2. The Young's modulus shown in Table 2 is the Young's modulus at a measurement temperature of 25°C ± 5°C. [Table 2]

[0091] <Evaluation of the temperature dependence of elasticity (Young's modulus)> For each glass mold used in Examples 1 to 20, the Young's modulus was measured at 590°C, 650°C, 700°C, and 750°C using the method described above. For the glass mold of Comparative Example 1, the Young's modulus at measurement temperatures of 590°C and 650°C was measured using the method exemplified earlier. In Table 3, E(590), E(650), E(700), and E(750) represent the Young's modulus at the measurement temperature, respectively. The unit is "GPa". From the measurement results, an approximate straight line was created using the least squares method with Young's modulus on the vertical axis and the measured temperature on the horizontal axis. The slope of this approximate straight line is shown in Table 3 as the "slope of Young's modulus." The unit of the slope of Young's modulus is "GPa / °C." The smaller the absolute value of the slope of the Young's modulus obtained in this way, the smaller the temperature dependence of the Young's modulus of the glass mold. From the results shown in Table 3, it can be confirmed that the glass molds of Examples 1 to 20 have less temperature dependence of Young's modulus compared to the glass mold of Comparative Example 1. In one embodiment, the slope of the Young's modulus calculated as described above from the Young's modulus at four measurement temperatures of 590°C, 650°C, 700°C, and 750°C is preferably -0.0100 GPa / °C or higher, more preferably -0.0090 GPa / °C or higher, even more preferably -0.0080 GPa / °C or higher, even more preferably -0.0070 GPa / °C or higher, even more preferably -0.0060 GPa / °C or higher, even more preferably -0.0050 GPa / °C or higher, even more preferably -0.0045 GPa / °C or higher, and even more preferably -0.0040 GPa / °C or higher. The slope of the above Young's modulus can be, for example, -0.0010 GPa / °C or less, or -0.0020 GPa / °C or less, or it can exceed the values ​​exemplified here.

[0092] [Table 3]

[0093] [Manufacturing and evaluation of optical elements] When mass-producing optical elements by press molding, the less the shape of the molding surface of the glass mold changes, the more effectively the shape variations of the optical elements can be suppressed. The degree of change in the shape of the molding surface of the glass mold when mass-producing optical elements by press molding can be evaluated by the following method. During a single lens molding cycle, a glass mold is exposed to the press temperature environment, heated, and then cooled to near its glass transition temperature. The shape change of the molded surface of the glass mold primarily occurs at the higher press temperature during a single lens molding cycle, and this change is expected to increase with the number of presses. The number of Newton lines is calculated from the shape of the glass mold used for lens molding for a certain number of times (shots) X or more (e.g., 50 shots or more) at a certain press temperature, compared to its shape before use. The number of Newtons can be determined by the following method. The shape of the molded surface of a glass mold is measured at room temperature (approximately 25°C) using a shape measuring instrument. Examples of shape measuring instruments include interferometers and three-dimensional measuring machines (e.g., Panasonic Production Engineering Co., Ltd. UA3P). In this study, Panasonic Production Engineering Co., Ltd. UA3P was used. From the radius of curvature R of the molded surface measured by the shape measurement (paraxial R for aspherical molded surfaces), the number of Newton's rings is calculated when the measurement wavelength is 546.1 nm. The difference in the number of Newtons D (after use - before use) before and after use is divided by the number of shots X to obtain the value D / X, which is the change in Newtons per shot ΔN. Multiplying this by 100 gives the change in Newtons per 100 shots, 100D / X. The lower limit of the number of presses X used to determine ΔN should be 50 or more, taking into account the measurement error of ΔN. The upper limit of X should be 100 or less, more preferably 80 or less, and even more preferably 60 or less, because if X is increased to the point where no change in the shape of the glass mold occurs, the apparent ΔN will become small and may not be suitable for evaluation. For example, the Newton change ΔN per shot at 590°C can be calculated by determining the number of Newtons from the shape of the glass mold used for lens molding a certain number of times X (50 ≤ X ≤ 100) at a press temperature of 590°C, and the shape before use, using the method described above. Then, the difference in the number of Newtons before and after lens molding, D (after use - before use), is divided by the number of shots X to obtain the value D / X, which is the "Newton change ΔN per shot at 590°C". The smaller this value, the less change in the shape of the molding surface of the glass mold can be evaluated when mass-producing optical elements by press molding. For Examples 7, 11, 12 and Comparative Example 1, the glass molds having the concave shape described above were used as the upper and lower molds, and precision press molding of glass materials to be molded was performed in the optical element manufacturing apparatus configured as shown in Figure 1, according to the method of the specific example described above, to produce glass optical elements (biconvex lenses). This process was repeated at a press temperature of 590°C, with X being the number of shots (50 ≤ X ≤ 60). Subsequently, ΔN = D / X obtained by the above method was multiplied by 100 to calculate 100D / X, which is shown in Table 4 as "the value obtained by multiplying the Newton change amount ΔN per shot at 590°C by 100". The value obtained by multiplying the Newton change ΔN per shot at 590°C by 100 can be 0.00 or greater, and preferably 1.00 or less, in the order of 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, and 0.30 or less. In Comparative Example 1, the change in the molding surface shape of the mold was large, and press molding could not be performed up to the number of shots X, so it is indicated as "Pressing not possible" in Table 4.

[0094] [Table 4]

[0095] As shown in Table 3, the glass molds of the examples, which are made from glass having the composition described above, exhibit little temperature dependence of Young's modulus. The results shown in Table 4 indicate that glass molds with such little temperature dependence of Young's modulus undergo little change in the shape of the molded surface when mass-producing optical elements by press molding.

[0096] Finally, we will summarize each of the aforementioned aspects.

[0097] According to one embodiment, a glass mold for forming optical elements is provided, wherein the glass is aluminosilicate glass, and in the glass composition expressed in molar percentage, the total content of SiO2 and Al2O3 is 60% or more, and the molar ratio of the total content of Li2O, Na2O, and K2O to the MgO content (Li2O+Na2O+K2O) / MgO is in the range of 0.000 to 0.400.

[0098] The above-mentioned glass mold is a glass mold for optical elements and can be a glass mold with low temperature dependence of elasticity.

[0099] In one embodiment, in the glass composition expressed in mol% of the above glass, the molar ratio of MgO to the total content of MgO, CaO, SrO, and BaO (MgO / (MgO+CaO+SrO+BaO)) can be 0.500 or more.

[0100] In one embodiment, in the glass composition expressed in mol% of the above glass, the molar ratio of the total content of Li2O, Na2O, K2O, SrO, and BaO to the total content of SiO2, Al2O3, MgO, CaO, ZrO2, and TiO2 ((Li2O+Na2O+K2O+SrO+BaO) / (SiO2+Al2O3+MgO+CaO+ZrO2+TiO2)) can be in the range of 0.000 to 0.100.

[0101] In one embodiment, the glass composition expressed in molar percentages of the above glass may include: MgO content of 1.0-30.0%, CaO content of 0.0-15.0%, SrO content of 0.0-12.0%, BaO content of 0.0-12.0%, ZnO content of 0.0-10.0%, Li2O content of 0.0-8.0%, total content of Na2O and K2O of 0.0-4.25%, ZrO2 content of 0.0-10.0%, TiO2 content of 0.0-6.0%, and total content of La2O3, Y2O3, Yb2O3, Ta2O5, Nb2O5, and HfO2 of 0.0-4.0%.

[0102] In one embodiment, the Young's modulus of the glass at a measurement temperature of 590°C can be 80 GPa or higher.

[0103] In one embodiment, the Young's modulus of the glass at a measurement temperature of 650°C can be 80 GPa or higher.

[0104] According to one embodiment, a method for manufacturing an optical element is provided, which includes press-molding a material to be molded using the glass mold described above.

[0105] In one embodiment, the optical element can be a glass optical element.

[0106] The embodiments disclosed herein should be considered in all respects to be illustrative and not restrictive. The scope of the present invention is indicated by the claims rather than by the foregoing description, and all modifications within the meaning and scope equivalent to the claims are intended to be included. For example, it is certainly possible to arbitrarily combine two or more of the forms described in the specification as examples or preferred scopes.

Claims

1. A glass mold for molding optical elements, comprising: the glass is an aluminosilicate glass, In the glass composition expressed in mol %, SiO 2 and Al 2 O 3 The total content is 60% or more, and Li relative to MgO content 2 O, Na 2 O and K 2 Molar ratio of the total content of O (Li 2 O+Na 2 O+K 2 The glass molding die, wherein the ratio of MgO to MgO is in the range of 0.000 to 0.

400.

2. In the glass composition expressed in mol %, 2. The glass molding die according to claim 1, wherein a molar ratio of MgO to the total content of MgO, CaO, SrO and BaO (MgO / (MgO+CaO+SrO+BaO)) is 0.500 or more.

3. In the glass composition expressed in mol %, SiO 2 , Al 2 O 3 , MgO, CaO, ZrO 2 and TiO 2 Li relative to the total content 2 O, Na 2 O.K. 2 The molar ratio of the total content of O, SrO and BaO ((Li 2 O+Na 2 O+K 2 O+SrO+BaO) / (SiO 2 +Al 2 O 3 +MgO+CaO+ZrO 2 + TiO 2 3. The glass molding die according to claim 1, wherein the ratio of the stoichiometric ratio of the polyimide to the stoichiometric ratio of the glass is 0.000 to 0.

100.

4. In the glass composition expressed in mol %, MgO content is 1.0 to 30.0%, CaO content: 0.0 to 15.0%, The SrO content is 0.0 to 12.0%, BaO content is 0.0 to 12.0%, ZnO content: 0.0-10.0%; Li 2 O content: 0.0 to 8.0%; Na 2 O and K 2 The total content with O is 0.0 to 4.25%, ZrO 2 Content is 0.0-10.0%, TiO 2 The content is 0.0 to 6.0%, and La 2 O 3 , Y 2 O 3 , Yb 2 O 3 , Ta 2 O 5 , Nb 2 O 5 and HfO 2 The total content is 0.0 to 4.0%, The glass molding die according to any one of claims 1 to 3,

5. The glass composition, expressed in mole percent, of the glass, The glass molding die according to any one of claims 1 to 4, wherein the Al 2 O 3 content is 12.5% ​​to 24.0%.

6. The glass composition, expressed in mole percent, of the glass comprises 6. The glass molding die according to claim 1, wherein a molar ratio of the MgO content to the total content of MgO + CaO + SrO + BaO (MgO / (MgO + CaO + SrO + BaO)) is 0.600 or more and 1.000 or less.

7. The glass composition, expressed in mole percent, of the glass, The glass molding die according to any one of claims 1 to 6, wherein the B 2 O 3 content is 0.0% to 2.0%.

8. 8. The glass molding die according to claim 1, wherein the glass has a Young's modulus of 80 GPa or more at a measurement temperature of 590°C.

9. 9. The glass molding die according to claim 1, wherein the glass has a Young's modulus of 80 GPa or more at a measurement temperature of 650°C.

10. Press molding a material to be molded using the glass mold according to any one of claims 1 to 9; A method for manufacturing an optical element, comprising:

11. The method for producing an optical element according to claim 10 , wherein the optical element is a glass optical element.